A method for recycling the positive electrode sheet of retired lithium-ion batteries

By treating lithium-ion battery cathode sheets with an eluent containing hydrogen bond disruptors and current collector interface modifiers at room temperature, the problems of high energy consumption and structural damage in existing technologies are solved. This achieves efficient and environmentally friendly separation of current collectors and cathode materials, resulting in directly recyclable aluminum foil and cathode materials.

CN123120950APending Publication Date: 2026-11-17GUANGXI ACAD OF SCI +3
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611260783.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for recycling lithium-ion battery cathode sheets suffer from high energy consumption, significant impact on the structure of current collectors and cathode materials, and poor separation selectivity and purity, making it difficult to achieve efficient and environmentally friendly selective separation of current collectors and cathode materials.

Method used

The positive electrode sheet is immersed in an eluent at room temperature. A hydrogen bond disruptor is used to break the hydrogen bonds between the binder and the aluminum foil. The current collector is separated from the positive electrode material by reacting with the aluminum foil oxide layer through an interface regulator. The morphology and structural integrity of the material are maintained during the separation process.

Benefits of technology

This technology enables low-energy, environmentally friendly separation of current collectors and cathode materials. The resulting aluminum foil and cathode materials can be directly recycled, simplifying subsequent processing and improving the economic value and purity of the separated and recycled materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120950A_ABST
    Figure CN123120950A_ABST
Patent Text Reader

Abstract

This invention discloses a method for recycling the positive electrode sheet of retired lithium-ion batteries, belonging to the field of lithium-ion battery recycling technology. The invention includes: (1) drying the positive electrode sheet under negative pressure air or vacuum to obtain a dry positive electrode sheet; (2) immersing the dry positive electrode sheet obtained in step (1) in an eluent to separate the current collector and positive electrode material, obtaining a complete current collector and positive electrode material; (3) washing and drying the current collector and positive electrode material obtained in step (2) to complete the positive electrode sheet recycling. This invention can ensure the separation of the current collector and positive electrode material while maintaining the morphology and structure of the aluminum foil and positive electrode material without change, obtaining directly usable aluminum foil and positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery recycling technology, specifically relating to a method for recycling the positive electrode sheet of retired lithium-ion batteries. Background Technology

[0002] Lithium-ion batteries have been widely adopted due to their significant advantages such as high energy density, long lifespan, and low self-discharge rate. This large-scale application inevitably generates and accumulates a large number of retired lithium-ion batteries. Since the positive electrode sheets of these retired batteries are rich in key metals such as iron, cobalt, nickel, manganese, and lithium, improper disposal not only leads to the loss of these key metals and resource waste but also easily causes heavy metal pollution. Therefore, recycling lithium-ion battery positive electrode sheets is beneficial for resource reuse, environmental protection, and supply chain stability.

[0003] Currently, the main regeneration methods for lithium-ion battery cathode sheets fall into three categories: pyrometallurgical regeneration, wet regeneration, and direct repair regeneration. Regardless of the method used, retired lithium-ion battery cathode sheets typically require separation and recycling to recover the current collector and cathode material, obtaining cathode powder that can be further smelted, leached, or repaired and regenerated. Therefore, the effective separation of the current collector and active material in the cathode sheet, as well as the quality of the separated current collector and cathode material, are crucial factors affecting the economic value of the current collector after separation and recycling, and the quality of the regenerated retired lithium-ion battery cathode material. Especially for the direct repair regeneration route, the particle morphology, crystal structure, impurity content, and current collector residue of the separated and recycled cathode powder directly affect the subsequent repair and regeneration effect. Therefore, achieving selective separation of the current collector and cathode active material while minimizing damage to the aluminum foil current collector, maintaining the structural integrity of the cathode material, and reducing the introduction of impurities is of great significance.

[0004] The positive electrode sheet of a retired lithium-ion battery typically includes an aluminum foil current collector and a positive electrode active material layer coated on the surface of the aluminum foil. The positive electrode active material layer generally contains components such as positive electrode active material, conductive agent, and binder. Among them, the binder forms a strong bond between the active material particles and between the active material layer and the aluminum foil current collector, making it quite difficult to completely detach the positive electrode active material from the surface of the aluminum foil current collector while ensuring the morphology and crystal structure of the positive electrode active material.

[0005] Existing methods for separating and recycling positive electrode sheets mainly include mechanical crushing and sorting, organic solvent leaching, alkaline dissolution, and thermal decomposition. Mechanical crushing and sorting typically involves crushing the entire electrode sheet before sorting to achieve preliminary separation of different components. It has advantages such as simple process and large throughput, but it easily causes breakage of the aluminum foil current collector, damage to positive electrode material particles, and the mixing of aluminum impurities into the positive electrode powder, resulting in poor separation selectivity, product purity, and structural integrity. Organic solvent leaching typically uses organic solvents to leach the metals of the positive electrode active material in ionic form while maintaining the current collector in a solid phase, thus achieving separation between the current collector and the positive electrode active material. However, during organic solvent leaching, the metal resources in the positive electrode active material change from a solid phase to an ionic liquid phase, damaging its material morphology and inherent crystal structure, making it unsuitable for direct regeneration. Multiple subsequent processing steps are required, and the current collector tends to adhere to a large amount of binder, necessitating further purification to improve its economic value for sale. Alkaline dissolution typically uses alkaline solutions to break down or dissolve the aluminum foil current collector to release the positive electrode material, but this results in aluminum foil loss and makes complete recovery of the current collector difficult. Thermal decomposition uses high-temperature treatment to decompose and degrade the binder, thereby separating the positive electrode material from the current collector. However, this method is energy-intensive, and the high-temperature environment can easily affect the particle morphology, surface chemical state, or crystal structure of the positive electrode material, hindering the subsequent direct repair and recycling of the separated and recovered positive electrode active material. For example, patent CN118213656A discloses a method and application for processing waste lithium battery positive electrode sheets. This method involves rapidly heating the positive electrode sheet and continuously rinsing it with an acidic rinsing solution to separate the current collector (aluminum foil) from the positive electrode material for recycling. This method requires heating, has high energy consumption, and the separation time is long.

[0006] Therefore, it is necessary to provide a method for recycling the cathode sheet of retired lithium-ion batteries, which simplifies the process complexity, reduces energy consumption, improves the environmental friendliness of recycling, and avoids the recycling process from affecting the current collector and the structure and morphology of the cathode material, thereby obtaining a current collector that can be sold directly and a cathode material that can be used directly for subsequent regeneration. Summary of the Invention

[0007] To overcome the problems in the prior art, the present invention immerses the positive electrode sheet in an eluent. The eluent selectively acts on the interface and binder between the current collector and the positive electrode material at room temperature, thereby destroying the interface and causing the binder to fail. This allows the current collector and the positive electrode material to be separated while maintaining their original morphology and structure. Both the current collector and the positive electrode material are solid after separation. The current collector and the positive electrode material can be separated by filtration and sieving to obtain a current collector that can be sold directly and a positive electrode material that can be used for subsequent regeneration.

[0008] To achieve the above objectives, the present invention is implemented through the following technical solution: This invention provides a method for recycling the positive electrode sheet of a retired lithium-ion battery, the method comprising the following steps: (1) Dry the positive electrode sheet under negative pressure air or vacuum environment to obtain a dry positive electrode sheet.

[0009] (2) The dried positive electrode obtained in step (1) is immersed in the eluent to separate the current collector and the positive electrode material, thereby obtaining the complete current collector and positive electrode material.

[0010] (3) The current collector and positive electrode material obtained in step (2) are washed and dried respectively to complete the positive electrode recycling.

[0011] Preferably, in step (1), the drying temperature is 60~100℃ and the drying time is 4~12h.

[0012] Preferably, in step (1), the negative pressure air pressure is 0.01~0.05MPa.

[0013] Negative pressure refers to a gas pressure state below normal pressure, which is characterized by an absolute pressure lower than atmospheric pressure or a negative relative pressure. The pressure of standard atmosphere is 101325 Pa, which is about 0.1 MPa. A pressure of 0.01~0.05 MPa is lower than 0.1 MPa and is considered a negative pressure condition.

[0014] Preferably, in step (2), the eluent is an aqueous solution of an active substance, which includes a hydrogen bond disruptor and a current collector interface modifier.

[0015] Preferably, the mass ratio of the current collector interface modifier to the hydrogen bond disruptor is current collector interface modifier: hydrogen bond disruptor = 1:2~1:19.

[0016] Preferably, the eluent contains 30% to 70% by mass of active substances, with the remainder being water.

[0017] Preferably, the hydrogen bond disruptor includes at least one of urea, thiourea, formamide, methanol, ethanol, acetone, and isopropanol; and the current collector interface modifier includes at least one of malic acid, tartaric acid, and oxalic acid.

[0018] When the hydrogen bond disruptor is a mixture of two or more substances, the substances in the hydrogen bond disruptor are mixed in any mass ratio.

[0019] When the current collector interface modifier is a mixture of two or more substances, the substances in the current collector interface modifier are mixed in any mass ratio.

[0020] Preferably, in step (2), the soaking temperature is room temperature to 60°C and the soaking time is 5 to 16 minutes.

[0021] Preferably, in step (3), the drying temperature is 80~120℃ and the drying time is 6~12h.

[0022] Preferably, in step (2), the eluent is stirred during soaking. More preferably, the stirring speed does not exceed 400 r / min.

[0023] Preferably, in step (3), the current collector debris is removed by filtration before washing the positive electrode material. More preferably, a 200-400 mesh sieve is used to filter the positive electrode material.

[0024] As a preferred method, the washing method for the current collector and the positive electrode material is as follows: soak the current collector or the positive electrode material in deionized water and ethanol for 5-10 minutes respectively.

[0025] The beneficial effects of this invention are: 1. The positive electrode sheet of a retired lithium-ion battery is usually formed by bonding a positive electrode material and a current collector with an adhesive. The current collector is usually aluminum foil, and the adhesive is usually polyvinylidene fluoride (PVDF). This invention uses a hydrogen bond disruptor in the eluent to break the hydrogen bonds formed between PVDF and aluminum foil, and further degrades PVDF into small molecule organic matter. This allows the current collector interface regulator to react rapidly with the aluminum foil oxide layer, breaking the connection between the aluminum foil and the positive electrode material and generating a dense complex passivation layer. This effectively promotes the failure of PVDF while preventing further damage to the aluminum foil and the positive electrode material. By promoting the failure of PVDF and protecting the aluminum foil and the positive electrode material, the effective separation of the aluminum foil and the positive electrode material is ensured, while maintaining the morphology and structure of the aluminum foil and the positive electrode material, resulting in usable aluminum foil and positive electrode material.

[0026] 2. The hydrogen bond disruptor and current collector interface modifier used in this invention are not highly corrosive and have high environmental friendliness. Furthermore, PVDF is degraded into small molecule organic matter, which can reduce the pollution of PVDF.

[0027] 3. The separation process of this invention only involves low-temperature drying and soaking, without the need for complex equipment or continuous high-temperature heating. It has low energy consumption, simple operation, strong process controllability, good separation and recovery effect of aluminum foil and positive electrode material, high quality and few impurities. Apart from simple operations such as filtration, no other operations are required. The separated and recovered positive electrode material can be directly used for regeneration (both pyrometallurgical and hydrometallurgical methods are acceptable, and it is especially suitable for direct repair and regeneration), without the need for cumbersome impurity removal and extraction processes. The separated and recovered aluminum foil has high economic value and can be sold directly, making it suitable for industrial promotion and application. Attached Figure Description

[0028] Figure 1 This is a photograph of a positive electrode sheet disassembled from a retired lithium-ion battery. Figure 2 This is a diagram showing the separation of the current collector and the positive electrode material during the elution process of the positive electrode sheet in Example 1 of the present invention; Figure 3 This is a photograph of the aluminum foil recovered in Example 1 of the present invention; Figure 4 This is a photograph of the positive electrode material recovered in Example 1 of the present invention; Figure 5 The image shows the X-ray diffraction results of the cathode material before separation (d-NCM) and the cathode material after separation (s-NCM) in Example 1 of the present invention. Figure 6 This is a scanning electron microscope image of the positive electrode material before separation in Example 1 of the present invention; Figure 7 This is a scanning electron microscope image of the positive electrode material recovered in Example 1 of the present invention; Figure 8 The images shown are X-ray photoelectron spectroscopy (XPS) analyses of the cathode material before and after separation in Example 1 of this invention. Figure 8 (a) is the Al 2p diagram of the cathode material before separation. Figure 8 (b) is the C 1s plot of the cathode material before separation. Figure 8 (c) is the F 1s plot of the cathode material before separation. Figure 8 (d) is the Al 2p diagram of the separated cathode material. Figure 8 (e) is the C 1s plot of the separated cathode material. Figure 8 (f) is the F 1s plot of the separated cathode material; Figure 9 This is a photograph of the aluminum foil recovered in Example 2 of the present invention. Figure 10 This is a photograph of the aluminum foil recovered in Example 3 of the present invention. Figure 11 This is a photograph of the aluminum foil recovered in Example 5 of the present invention. Figure 12 This is a photograph of the positive electrode material recovered in Example 5 of the present invention. Figure 13 The X-ray diffraction curves of the cathode material before separation (d-LFP) and the cathode material after separation (s-LFP) in Example 5 of the present invention are shown. Figure 14 This is a scanning electron microscope image of the positive electrode material before separation in Example 5 of the present invention; Figure 15 This is a scanning electron microscope image of the positive electrode active material recovered in Example 5 of the present invention; Figure 16 This is a graph showing the results of the number of cycles of the eluent versus the separation time / separation rate in Example 1 of the present invention. Figure 17 This is a capacity-voltage diagram of the positive electrode material obtained from the recycling of Example 4 and Comparative Example 2 of the present invention after direct regeneration.

[0029] Figure 18 This is a photograph of the aluminum foil recovered in Comparative Example 3 of this invention. Figure 19 This is a photograph of the aluminum foil recovered in Comparative Example 4 of the present invention. Detailed Implementation

[0030] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments, but the scope of protection of the present invention is not limited to the content described.

[0031] The positive electrode sheets used in the embodiments and comparative examples of this invention were all disassembled from retired lithium-ion batteries. Unless otherwise specified, all chemical reagents used in the embodiments and comparative examples were commercially available analytical grade reagents.

[0032] Example 1 This embodiment uses the following method to separate and recycle the positive electrode sheet: (1) Discharge the retired lithium-ion ternary power battery, disassemble the retired lithium-ion power battery to obtain the positive electrode sheet, dry the positive electrode sheet under a negative pressure of 0.01MPa, dry at a temperature of 80℃ for 10h, remove the electrolyte remaining on the positive electrode sheet, and obtain the dried positive electrode sheet (e.g. Figure 1 (As shown).

[0033] (2) At room temperature, the dry positive electrode sheet was immersed in the eluent for 10 minutes. The aluminum foil and the positive electrode material were separated in the eluent. Then, the positive electrode sheet was removed from the eluent, and the positive electrode material was removed from the aluminum foil with tweezers to obtain the complete aluminum foil and the positive electrode material. The active substance in the eluent was a mixture of oxalic acid and urea. The mass percentage of the active substance in the eluent was 30%, and the mass ratio of oxalic acid to urea was 1:4.

[0034] (3) Filter the positive electrode material using a 200-400 mesh sieve, and wash the filtered positive electrode material and aluminum foil by immersing them in deionized water and ethanol for 10 minutes respectively. Then, place the aluminum foil and positive electrode material in a forced-air drying oven and dry them at 100°C for 10 hours to obtain dried aluminum foil (e.g. Figure 3 (as shown) and positive electrode materials (such as Figure 4 (As shown).

[0035] pass Figure 2It can be seen that during the elution process, after 6 minutes, slight cracks appeared at the interface between the aluminum foil and the positive electrode material, and after 10 minutes, obvious cracks appeared at the interface between the aluminum foil and the positive electrode material. Furthermore, the eluent remained white and transparent throughout the entire separation process, which fully demonstrates that the eluent of the present invention selectively acts on the interface between the positive electrode material and the current collector and the PVDF, rather than dissolving the positive electrode material. Almost no metal ions were dissolved during the elution process.

[0036] pass Figure 3 and Figure 1 The comparison shows that after separation and recycling, the aluminum foil is intact and there is no residue of positive electrode active material.

[0037] pass Figure 4 It can be seen that after separation and recycling, the cathode material has a good morphology and no current collector adhesion.

[0038] Inductively coupled plasma optical emission spectroscopy (ICP-OES) was performed on the eluent, and the results showed that the metal leaching rate of the cathode material during the recovery process was ≤0.8%, indicating that there was basically no metal ion leaching during the elution process, and the damage to the morphology and structure of the cathode material was minimal.

[0039] pass Figure 5 , 6 As can be seen from 7, the separated and recovered cathode material basically maintains its original crystal structure and microstructure, which further illustrates that the main principle of the processing and recycling process of the present invention is to cause the binder to fail, without damaging the cathode material, and to recover cathode material that can be directly used as a regenerated raw material.

[0040] pass Figure 8 It can be seen that the disappearance of the Al-O peak after elution indicates that the current collector interface modifier in the eluent can undergo a complexation reaction with the alumina / alumina hydroxyl layer on the aluminum foil surface, causing the original Al-O structure to be destroyed, dissolved, or transformed. This weakens the interfacial connection between the aluminum foil current collector and the positive electrode active material layer, promoting the detachment of the positive electrode active material layer from the aluminum foil surface. Simultaneously, the aluminum-oxalate complex or surface adsorption layer formed by the current collector interface modifier and aluminum species can provide a certain degree of corrosion inhibition protection to the newly exposed aluminum foil surface, reducing the continuous corrosion of the aluminum foil current collector by the eluent (ICP-OES results show that the Al loss rate is less than 2 wt.%), thus achieving a synergistic effect of interfacial stripping and current collector protection. Furthermore, the C=O peak appearing after elution indicates the formation of a new oxalate protective layer on the positive electrode material surface, which can also prevent further leaching of metal elements from the positive electrode material. The decrease in the LiF peak value indicates that most of the electrolyte residue was removed during drying and separation.

[0041] Example 2 This embodiment uses the following method to separate and recycle the positive electrode sheet: (1) Discharge the retired lithium-ion ternary power battery, disassemble the retired lithium-ion power battery to obtain the positive electrode sheet, dry the positive electrode sheet under a negative pressure of 0.01MPa, the drying temperature is 60℃, the drying time is 12h, remove the electrolyte remaining on the positive electrode sheet, and obtain the dry positive electrode sheet.

[0042] (2) At room temperature, the dry positive electrode sheet was immersed in the eluent for 15 minutes. The aluminum foil and the positive electrode material were separated in the eluent. Then, the positive electrode sheet was removed from the eluent, and the positive electrode material was removed from the aluminum foil with tweezers to obtain the complete aluminum foil and the positive electrode material. The active material in the eluent was a mixture of malic acid and thiourea. The mass percentage of the active material in the eluent was 60%, and the mass ratio of malic acid to thiourea was 1:10.

[0043] (3) Filter the positive electrode material using a 200-400 mesh sieve, and wash the filtered positive electrode material and aluminum foil by immersing them in deionized water and ethanol for 10 minutes respectively. Then, place the aluminum foil and positive electrode material in a forced-air drying oven and dry them at 100°C for 10 hours to obtain dried aluminum foil (e.g. Figure 9 (as shown) and the positive electrode material.

[0044] pass Figure 9 As can be seen, the aluminum foil recovered in this embodiment is intact and has no residue of positive electrode active material.

[0045] The recycling process and the morphological structure of the recovered cathode material in this embodiment are basically the same as those in Embodiment 1, indicating that the recycling process will not damage the cathode material.

[0046] Example 3 This embodiment uses the following method to separate and recycle the positive electrode sheet: (1) Discharge the retired lithium-ion ternary power battery, disassemble the retired lithium-ion power battery to obtain the positive electrode sheet, dry the positive electrode sheet under a negative pressure of 0.05MPa, the drying temperature is 100℃, the drying time is 4h, remove the electrolyte remaining on the positive electrode sheet, and obtain the dry positive electrode sheet.

[0047] (2) At room temperature, the dry positive electrode sheet was immersed in the eluent for 16 minutes. The aluminum foil and the positive electrode material were separated in the eluent. Then, the positive electrode sheet was removed from the eluent, and the positive electrode material was removed from the aluminum foil with tweezers to obtain a complete aluminum foil and positive electrode material. The active substance in the eluent was a mixture of tartaric acid and formamide. The mass percentage of the active substance in the eluent was 70%, and the mass ratio of tartaric acid to formamide was 1:19.

[0048] (3) Filter the positive electrode material using a 200-400 mesh sieve, and wash the filtered positive electrode material and aluminum foil by immersing them in deionized water and ethanol for 10 minutes respectively. Then, place the aluminum foil and positive electrode material in a forced-air drying oven and dry them at 80°C for 12 hours to obtain dried aluminum foil (e.g. Figure 10 (as shown) and the positive electrode material.

[0049] pass Figure 10 It can be seen that the separated and recycled aluminum foil is intact and has no residue of positive electrode active material.

[0050] The recycling process and the morphological structure of the recovered cathode material in this embodiment are basically the same as those in Embodiment 1, indicating that the recycling process will not damage the cathode material.

[0051] Example 4 This embodiment uses the following method to separate and recycle the positive electrode sheet: (1) Discharge the retired lithium-ion ternary power battery, disassemble the retired lithium-ion power battery to obtain the positive electrode sheet, dry the positive electrode sheet under a negative pressure of 0.03MPa, the drying temperature is 90℃, the drying time is 8h, remove the electrolyte remaining on the positive electrode sheet, and obtain the dry positive electrode sheet.

[0052] (2) At 45℃, the dried positive electrode sheet was immersed in the eluent for 9 minutes. During the immersion process, the eluent was stirred at 300 r / min. The aluminum foil and the positive electrode material were separated in the eluent. Then, the positive electrode sheet was removed from the eluent, and the positive electrode material was removed from the aluminum foil using tweezers to obtain a complete aluminum foil and positive electrode material. The active substance in the eluent was a mixture of oxalic acid and methanol, with a mass percentage of 60% and a mass ratio of oxalic acid to methanol of 3:7.

[0053] (3) Use a 200~400 mesh screen to filter the positive electrode material, and soak the filtered positive electrode material and aluminum foil in deionized water and ethanol for 10 min respectively for washing. Then place the aluminum foil and positive electrode material in a forced-air drying oven and dry at 120℃ for 6 h to obtain dried aluminum foil and positive electrode material.

[0054] The positive electrode sheet in this embodiment is the same as that in Embodiment 1. The recycled aluminum foil and positive electrode material are basically the same as those in Embodiment 1. The aluminum foil is intact and there is no residue of positive electrode material. The morphology and structure of the positive electrode material are basically maintained in the state before separation.

[0055] Example 5 This embodiment uses the following method to separate and recycle the positive electrode sheet: (1) Discharge the retired lithium iron phosphate battery, disassemble the battery to obtain lithium iron phosphate positive electrode sheet, dry the positive electrode sheet in a vacuum environment at a temperature of 100°C for 4 hours, remove the electrolyte remaining on the positive electrode sheet, and obtain the dried positive electrode sheet.

[0056] (2) At 60℃, the dried positive electrode sheet was immersed in the eluent for 5 minutes. During the immersion process, the eluent was stirred at 400 r / min. The aluminum foil and the positive electrode material were separated in the eluent. Then, the positive electrode sheet was removed from the eluent, and the positive electrode material was removed from the aluminum foil using tweezers to obtain a complete aluminum foil and positive electrode material. The active material in the eluent was a mixture of malic acid and acetone, with a mass percentage of 40% and a mass ratio of malic acid to acetone of 3:7.

[0057] (3) Filter the positive electrode material using a 200-400 mesh sieve, and wash the filtered positive electrode material and aluminum foil by immersing them in deionized water and ethanol for 5 minutes respectively. Then, place the aluminum foil and positive electrode material in a forced-air drying oven and dry them at 80°C for 10 hours to obtain dried aluminum foil (e.g. Figure 11 (as shown) and positive electrode materials (such as Figure 12 (As shown).

[0058] pass Figure 11 As can be seen, the aluminum foil in this embodiment is intact and there is no residue of positive electrode material.

[0059] pass Figure 12 As can be seen, the positive electrode active material separated and recovered in this embodiment has a good morphology and no current collector adhesion.

[0060] pass Figure 13 , 14 As can be seen from 15, the cathode material after separation and recycling in this embodiment basically maintains its original crystal structure and micromorphology, indicating that the processing and recycling process of the present invention will not damage the cathode material.

[0061] This embodiment demonstrates that the method of the present invention has wide applicability and excellent applicability to lithium iron phosphate battery cathode sheets.

[0062] Example 6 This embodiment uses the same method as in Example 1 to separate and recover the same positive electrode sheet. The difference is that in the active material of the eluent in this embodiment, the hydrogen bond disruptor is a mixture of urea, thiourea, formamide, methanol, ethanol, acetone and isopropanol in any mass ratio, and the current collector interface regulator is a mixture of malic acid, tartaric acid and oxalic acid in any mass ratio.

[0063] In this embodiment, the overall recovery rate of the positive electrode material and aluminum foil fluctuated slightly compared with that of Example 1, but the morphological integrity of the aluminum foil and positive electrode material was similar to that of Example 1.

[0064] Calculations show that in Examples 1-4, the overall recovery rate of the cathode material and aluminum foil is ≥98%, and the Al impurity content in the cathode material is ≤0.8%, indicating excellent recovery performance.

[0065] For the lithium iron phosphate battery cathode sheet of Example 5, the overall recovery rate of the cathode material and aluminum foil is ≥95%, and the Al impurity content of the cathode material is less than 1%. This indicates that the present invention has a wide range of applications and also has a better cathode sheet separation and recovery effect for ternary lithium batteries.

[0066] Example of effect This example demonstrates the recycling of the eluent already used in Example 1, yielding the following results: Figure 16 As shown.

[0067] pass Figure 16 As can be seen, the eluent of this invention can be recycled 40 times, and the separation time can still be maintained at about 15 minutes, and the separation recovery rate can be maintained at over 95%. This proves that the eluent of this invention can be recycled multiple times, with low usage cost and excellent economic benefits.

[0068] Comparative Example 1 This comparative example uses the same method as Example 1 to separate and recover the same positive electrode sheet. The difference is that the eluent in this example is an aqueous solution of oxalic acid, and the active material does not contain urea.

[0069] This comparative example requires soaking for more than 60 minutes for the aluminum foil and the positive electrode material to be completely separated. A comparison between Comparative Example 1 and Example 1 confirms that after adding the hydrogen bond disruptor, it can break the hydrogen bonds between the adhesive and the aluminum foil through its own hydroxyl groups, thereby accelerating the separation process.

[0070] Comparative Example 2 This comparative example uses the same method as Example 4 to separate and recover the same positive electrode, the difference being that the eluent in this comparative example is an aqueous solution of oxalic acid.

[0071] The separation time required for this comparative example is >90 min. Compared with Example 1, it can be seen that the addition of a hydrogen bond disruptor in this invention can promote the separation process.

[0072] pass Figure 17 It can be seen that the cathode material in Example 4, after direct repair and regeneration, exhibits an initial discharge specific capacity of 153 mAh·g at 1C. -1 Meanwhile, the cathode material in Comparative Example 2, after direct repair and regeneration, exhibited an initial discharge specific capacity of 119 mAh·g at 1C.-1 It can be seen that, due to the absence of hydrogen bond disruptors in the separation process, the separation time is too long, resulting in severe damage to the cathode material. Consequently, when it is used as a raw material for direct repair and regeneration, the performance of the repaired and regenerated cathode material deteriorates.

[0073] Comparative Example 3 This comparative example uses the same method as Example 4 to separate and recover the same positive electrode, the difference being that the eluent in this comparative example is pure methanol.

[0074] First, the separation process in this comparative example requires a time of at least 90 minutes. Second, the separation and recovery process in this comparative example requires a temperature of at least 80°C. Finally, the separated and recovered aluminum foil should be... Figure 18 As shown.

[0075] pass Figure 18 It can be seen that although pure methanol solution can separate the current collector aluminum foil from the cathode material at higher temperatures, a large amount of cathode material remains on the aluminum foil surface, making it almost impossible to reuse directly, and the cathode material recovery rate is reduced.

[0076] Comparative Example 4 This comparative example uses the same method as Example 4 to separate and recover the same positive electrode, the difference being that the eluent in this comparative example is a methanol aqueous solution with a methanol mass percentage of 60%.

[0077] pass Figure 19 It can be seen that the positive electrode in this comparative example did not show any significant changes, indicating that a 60% methanol aqueous solution is basically unable to achieve effective separation between the current collector aluminum foil and the positive electrode material.

[0078] Comparative Example 5 This comparative example uses the same method as Example 4 to separate and recover the same positive electrode sheet. The difference is that the eluent in this comparative example is a mixture of oxalic acid and methanol, and there is no water in the eluent.

[0079] In this comparative example, the eluent became turbid during the separation process, indicating that the metal in the cathode material leached into the eluent in ionic form. The target of the eluent in this comparative example has shifted from PVDF to the metal in the cathode material. The eluent reacts with the metal to generate metal ions, causing the metal to leach out in ionic form, thus achieving the separation of the cathode material from the aluminum foil. However, this comparative example has damaged the microstructure and morphology of the metal in the cathode material during the separation process, making it unsuitable for direct use as a regeneration and repair material. Furthermore, the metal ions obtained in this comparative example require subsequent extraction and reduction processes for recycling before they can be used as regeneration materials, complicating the cathode material recycling process and increasing the investment cost for cathode material recycling and regeneration.

[0080] In summary, the eluent of this invention selectively acts on PVDF through a hydrogen bond disruptor, causing PVDF to rapidly degrade and fail through a synergistic effect. Simultaneously, the current collector interface regulator rapidly reacts with the aluminum foil oxide layer, disrupting the connection between the aluminum foil and the cathode material, and providing protection for both the aluminum foil and the cathode material. This achieves high integrity and high recovery rate separation and recycling of the aluminum foil and cathode material while maintaining their basic morphology and structure. The resulting aluminum foil and cathode material can be directly reused. The method is environmentally friendly, simple to operate, highly controllable, and requires no complex equipment.

[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A method for recycling the positive electrode sheet of a retired lithium-ion battery, characterized in that: The positive electrode recycling method includes the following steps: (1) Dry the positive electrode sheet under negative pressure air or vacuum environment to obtain a dry positive electrode sheet; (2) Immerse the dried positive electrode sheet obtained in step (1) in the eluent to separate the current collector and positive electrode material of the positive electrode sheet, and obtain the complete current collector and positive electrode material; (3) The current collector and positive electrode material obtained in step (2) are washed and dried respectively to complete the positive electrode recycling.

2. The positive electrode recycling method according to claim 1, characterized in that: In step (1), the drying temperature is 60~100℃ and the drying time is 4~12h.

3. The positive electrode recycling method according to claim 1, characterized in that: In step (1), the negative pressure air pressure is 0.01~0.05MPa.

4. The positive electrode recycling method according to claim 1, characterized in that: In step (2), the eluent is an aqueous solution of an active substance, which includes a hydrogen bond disruptor and a current collector interface modifier.

5. The positive electrode recycling method according to claim 4, characterized in that: The mass ratio of the current collector interface modifier to the hydrogen bond disruptor is 1:2 to 1:

19.

6. The positive electrode recycling method according to claim 4, characterized in that: The eluent contains 30% to 70% active substances by mass, with the remainder being water.

7. The positive electrode recycling method according to claim 4, characterized in that: The hydrogen bond disruptor includes at least one of urea, thiourea, formamide, methanol, ethanol, acetone, and isopropanol; the current collector interface modifier includes at least one of malic acid, tartaric acid, and oxalic acid.

8. The positive electrode recycling method according to claim 1, characterized in that: In step (2), the soaking temperature is room temperature to 60°C, and the soaking time is 5 to 16 minutes.

9. The positive electrode recycling method according to claim 1, characterized in that: In step (3), the drying temperature is 80~120℃ and the drying time is 6~12h.

10. The positive electrode recycling method according to claim 1, characterized in that: In step (2), the eluent is stirred during soaking.

Citation Information

Patent Citations

  • Positive plate recovery method suitable for retired lithium ion power battery

    CN118213656A