A method for directly regenerating single-crystal ternary cathode materials from waste cathode materials
By using waste ternary cathode materials as seed crystals and mixing them with precursors at low temperatures to form single-crystal ternary cathode materials, the problems of low recycling efficiency of waste materials and high cost of single-crystal preparation are solved, realizing an efficient and simplified regeneration process and high-quality single-crystal material production.
Patent Information
- Application Number
- CN202611520898.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, the recycling efficiency of waste ternary cathode materials is low, polycrystalline ternary particles are prone to cracking and corrosion, have rapid capacity decay and poor thermal stability, and the preparation cost of single-crystal ternary materials is high and difficult to scale up. Furthermore, waste materials cannot be directly used as seed crystals and roasted together with precursors.
Waste ternary cathode material is used as seed crystal, mixed with ternary cathode material precursor and lithium source at a lower temperature than conventional single crystal sintering temperature, and epitaxially grown by high-temperature calcination to form single-crystal ternary cathode material, retaining the original layered crystal structure and avoiding complex acid leaching and extraction processes.
It achieves efficient recycling of waste materials, improves crystal integrity and crystal quality, simplifies the process, reduces resource consumption, and is suitable for industrial production of various ternary cathode materials.
Smart Images

Figure CN123120955A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for directly regenerating single-crystal ternary cathode materials from waste cathode materials, belonging to the field of lithium-ion batteries. Background Technology
[0002] Lithium-ion batteries are the core energy storage carriers for portable electronic devices, new energy vehicles, and large-scale static energy storage devices. The improvement of the overall performance of batteries is highly dependent on the selection and modification of the cathode material system. Cathode materials are not only the core component that determines the energy density of the cell, but also the safety performance and manufacturing cost of the battery. At present, the core goal of the industry and scientific research is to overcome the technical barriers to improving energy density while taking into account both material safety and industrialization economics.
[0003] Ternary cathode materials have become the mainstream cathode material for power batteries and consumer lithium batteries due to their high specific capacity, adjustable composition, and ease of mass production. However, current issues include low recycling efficiency of waste ternary materials and low overall recycling efficiency. Furthermore, polycrystalline ternary particles, due to their numerous grain boundaries, suffer from drawbacks such as easy cracking and corrosion during cycling, rapid capacity decay, and poor thermal stability. In contrast, monocrystalline ternary particles have complete grains, fewer grain boundaries, and a stable structure, which can mitigate metal dissolution and side reactions, resulting in superior cycle and safety performance, and suitability for high voltages to improve energy density. However, monocrystalline preparation relies on high-temperature sintering, which also presents challenges such as lithium volatilization, difficulty in controlling particle size, high energy consumption, and high production costs, limiting its large-scale promotion.
[0004] In the prior art, such as application publication number CN115744875A, there is a method for in-situ preparation of cathode materials using seed crystals. This invention first prepares cathode material seed crystals through a hydrothermal reaction, then adds a mixed slurry, freeze-dries it to generate a cathode precursor, and finally adds a carbon source to the cathode material precursor, dries it, and sinters to obtain the cathode material. This invention prepares the precursor using pure seed crystals and finally obtains the cathode material. In other words, there is no existing technology that allows waste cathode material to be used as a seed crystal and calcined together with the precursor.
[0005] The authorized publication number CN111129487B discloses a hydrothermal lithium replenishment-spray remodeling method for regenerating waste ternary cathode materials. The method involves deep discharging and separating waste ternary lithium batteries; placing cathode aluminum foil in a sodium hydroxide solution; drying, calcining, and grinding the detached waste ternary lithium battery cathode material to obtain powder; adding the powder to an organic acid for surface activation; then adding a lithium salt solution for hydrothermal treatment; subsequently, using the powder as a seed crystal and mixing it with nickel, manganese, and cobalt sources to obtain a homogeneous suspension; spray granulation and remodeling of the suspension to obtain an NCM precursor; and then performing a two-stage sintering process using oxygen to obtain the regenerated ternary cathode material. This invention still involves grinding the waste ternary cathode material into powder and adding it to a lithium salt solution, and still requires leaching the waste ternary cathode material to an ionic state. Summary of the Invention
[0006] To address the problems and shortcomings of the existing technology, this invention provides a method for directly regenerating single-crystal ternary cathode materials from waste cathode materials. One objective of this invention is to utilize waste ternary cathode materials as seed crystals to complete the sintering of single-crystal ternary cathode materials at a temperature lower than that of conventional single-crystal sintering.
[0007] This invention is achieved through the following technical solution: A method for directly regenerating single-crystal ternary cathode materials from waste cathode materials includes the following steps: Waste lithium-ion battery ternary cathode materials are recycled and processed to remove current collectors, binders and conductive agents, and waste ternary cathode active materials are obtained. The waste ternary cathode active material is pulverized by ball milling, sand milling or air jet milling to obtain seed particles with an average particle size of 0.1 to 2 μm; the pulverization time can be 0.5 to 24 h; the pulverization speed can be 100 to 800 r / min. According to the target single-crystal ternary cathode material composition, the seed particles are mixed with the ternary cathode material precursor and lithium source, and the mixture is thoroughly and uniformly mixed. The resulting mixture was calcined at high temperature to induce a solid-state reaction in the precursor, and epitaxial growth was performed using the seed particles as growth cores to obtain a single-crystal ternary cathode material. After cooling, a regenerated single-crystal ternary cathode material is obtained.
[0008] The ternary cathode material of the spent lithium-ion batteries includes LiNi. x Co y Mn 1-x-y One or more of the O2 materials, including NCM111, NCM523, NCM622, NCM811, NCA or any mixture thereof in any proportion.
[0009] The recycling and processing of waste lithium-ion battery ternary cathode materials involves heat treatment or dispersion and cleaning with weak acidic solvents, including acetic acid, formic acid, hypochlorous acid, nitrous acid, or citric acid.
[0010] The pulverized seed crystal particles have a D50 particle size of 0.1–2 μm; the seed crystal particles are tempered to remove organic impurities; the amount of seed crystal particles added is 0.1–30 wt% of the total mass of the final mixture.
[0011] The chemical formula of the ternary cathode material precursor is Ni. x Co y Mn 1-x-y (OH)2; the lithium source includes one or more of LiOH, LiOH·H2O, and Li2CO3 in any proportion; the molar ratio of lithium to transition metal element can be 1.00 to 1.10:1, and the transition metal element is (Ni+Co+Mn).
[0012] The high-temperature calcination is at 400°C. o C~1000 o C, keep warm for 5–30 hours, with a heating rate of 2–10. o C / min; the atmosphere is air, oxygen, or a mixture of oxygen and air in any ratio, wherein the volume fraction of oxygen can be 20% to 100%.
[0013] During the mixing process of the seed crystal particles with the ternary cathode material precursor and lithium source, one or more metal dopants selected from Al, Mg, Ti, Zr, Mo, W, Nb, Y, and B can also be added.
[0014] The cooling process can be achieved through furnace cooling, natural cooling, or programmed cooling. The cooled product can then undergo sieving, demagnetization, light pulverization, or surface coating treatment. The programmed cooling rate can range from 0.5 to 10. o C / min, until cooled to room temperature.
[0015] A regenerated single-crystal ternary cathode material is prepared by directly regenerating single-crystal ternary cathode material from the above-mentioned waste cathode material. The primary particle size of the regenerated single-crystal ternary cathode material is 2-6 μm, the secondary particle agglomeration degree is low, and the number of grain boundaries is reduced.
[0016] A regenerated single-crystal ternary cathode material can be used as a ternary cathode material for lithium-ion batteries.
[0017] The above-mentioned recycling and processing of ternary cathode materials from waste lithium-ion batteries includes mechanically crushing the recycled waste lithium-ion battery cathode sheets to separate the cathode active material from the aluminum foil current collector, then removing the binder, conductive agent, and residual electrolyte using at least one of the following methods: heat treatment, organic solvent cleaning, and ultrasonic cleaning, followed by washing with deionized water or organic solvent, and then rinsing at 60-150°C. o Drying at C for 2–24 hours yields waste ternary cathode material.
[0018] In the above-mentioned crushing process, it is preferable to retain the original layered crystal structure of the waste cathode material, so that the resulting seed crystals have a high degree of crystallinity and can serve as heterogeneous nucleation cores for the subsequent growth of single-crystal materials. During the sintering process, the waste cathode material seed crystals act as nucleation centers, inducing the active components after the precursor decomposition to grow epitaxially along the seed crystal surface, thereby forming a ternary cathode material with a single-crystal structure.
[0019] The beneficial effects of this invention are: (1) The present invention does not require the waste cathode material to be completely leached to the ionic state, thus avoiding complex acid leaching, extraction, precipitation and other processes, and significantly shortening the process flow.
[0020] (2) The present invention uses the crushed waste cathode material as seed crystals to induce single crystal directional epitaxial growth during high-temperature sintering, thereby improving crystal integrity and crystal quality.
[0021] (3) The present invention utilizes waste cathode material for crushing treatment. Since the recycled cathode material itself has microcracks, it is easier to crush into tiny particles, thereby improving the efficiency of seed preparation.
[0022] (4) This invention realizes the direct inheritance of some crystal structures in waste cathode materials, improves atom utilization and material utilization efficiency, and reduces resource consumption.
[0023] (5) The process of this invention is simple and easy to industrialize and produce continuously. It can be applied to the direct regeneration of ternary cathode materials with different compositions, such as NCM111, NCM523, NCM622, NCM811 and others. Attached Figure Description
[0024] Figure 1 This is an XRD characterization image of the cathode material prepared in Example 1 of the present invention.
[0025] Figure 2 This is a SEM image of the cathode material prepared in Example 1 of the present invention.
[0026] Figure 3 This is a cycle performance image of the cathode material prepared in Example 1 of the present invention. Detailed Implementation
[0027] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0028] One aspect of the present invention provides a method for directly regenerating single-crystal ternary cathode materials from waste cathode materials. In some embodiments, the method may include the following steps: Step (1): Collect ternary cathode materials from waste lithium-ion batteries. The ternary cathode materials include, but are not limited to, NCM111, NCM523, NCM622, NCM811, NCA and their mixed systems.
[0029] Step (2): Heat-treat the waste lithium-ion battery ternary cathode material at 300-600℃ for 1-10 hours in an oxygen or air atmosphere to repair the surface defects formed, or use a weak acid solvent for dispersion treatment, including acetic acid, formic acid, hypochlorous acid, nitrous acid or citric acid; remove the current collector, binder and conductive agent to obtain the waste ternary cathode active material. Step (3): Place the waste ternary cathode active material in a ball mill, sand mill, air jet mill or other pulverizing equipment for pulverization to reduce its particle size to 0.1-2 μm, and use it as seed crystals for later use; Step (4): According to the composition of the target single crystal ternary cathode material, weigh the corresponding hydroxide precursor, and then add the lithium source according to the molar ratio of Li / (Ni+Co+Mn)=1.02~1.10. After uniform mixing, it is ready for use.
[0030] Step (5): Add the seed crystals obtained in step (2) or (3) to the above-mentioned mixing system. The amount of seed crystals added is preferably 0.1 to 30 wt% of the final mixed powder mass.
[0031] Step (6): In order to improve the sintering uniformity, the mixed powder can be added to an appropriate amount of deionized water or ethanol to make a slurry, which can then be granulated by spraying, roller granulation or pressing to form mixed particles with uniform particle size.
[0032] Step (7): The mixed powder or granulated particles are placed in an oxygen, oxygen-enriched air or air atmosphere for high-temperature sintering.
[0033] Step (8): After sintering, the material is cooled to room temperature by furnace cooling, controlled-speed cooling or natural cooling to obtain regenerated single-crystal ternary cathode material.
[0034] In some implementation schemes, collecting waste ternary cathode materials may include: separating the cathode active material from the aluminum foil current collector by mechanical peeling or crushing; subsequently removing the binder (PVDF), conductive agent, and residual electrolyte by heat treatment, solvent cleaning, or a combination of both; and finally washing and filtering with deionized water or organic solvent at 60–150 °C. oDrying at C for 2–24 hours; in specific embodiments, drying can be achieved at 60°C. o C, 100 o C, 120 o C or 150 o Clean waste ternary cathode material was obtained by drying under C conditions for 2h, 8h, 10h, 12h, 14h, 16h or 24h.
[0035] In some implementations, seed crystal preparation may include: pulverizing waste ternary cathode material using one or more of a ball mill, sand mill, air jet mill, or other pulverizing equipment to reduce its particle size to 0.1–2 μm. During pulverization, the original layered crystal structure of the waste material should be preserved as much as possible to ensure the resulting seed crystals have high crystal integrity, serving as heterogeneous nucleation cores for subsequent single crystal growth. If necessary, sieving or grading equipment can be used to classify the seed crystals by particle size to improve the uniformity of the seed crystal particle size distribution.
[0036] In some implementations, weighing the corresponding hydroxide precursor may include: the hydroxide precursor having the chemical formula Ni x Co y Mn 1-x-y (OH)₂, where x = 0.3–0.95, y = 0.02–0.4. The added lithium source may include LiOH, LiOH·H₂O, Li₂CO₃, or a combination thereof.
[0037] In some implementations, the mixing method may include: V-type mixing, double cone mixing, planetary mixing, high-speed mixing, wet ball milling, etc., with a mixing time of 0.5 to 12 hours. In some specific embodiments, the mixing time may be 0.5 hours, 1 hour, 5 hours, 10 hours or 12 hours, so that the seed crystals are uniformly dispersed between the precursor and the lithium source.
[0038] In some implementation schemes, the specific mechanism of high-temperature sintering includes: first, in an oxygen, oxygen-enriched air, or air atmosphere, at a temperature of 2–5... o Increase the temperature by C / min to 450-550 o C, keep warm for 2-6 hours to remove residual moisture and promote lithium source decomposition. In some specific embodiments, it can first be done at 2 o C / min, 3 o C / min or 5 o Heat to 450 °C / min o C, 500 o C or 550 o C, keep warm for 2, 4, or 6 hours; then continue at 2-5 degrees Celsius. o Increase the temperature by C / min to 700–950 oC, keep warm for 5-30 hours to allow the precursor to undergo a solid-phase reaction; in some specific embodiments, it can be continued at 2 o C / min, 3 o C / min, 4 o C / min or 5 o Temperature increased to 700 °C / min o C, 800 o C, 850 o C or 950 o C, heat treatment for 5h, 10h, 15h or 30h. During the sintering process, the waste cathode material seed crystals serve as heterogeneous nucleation centers, and the retained layered lattice provides a crystal growth template for the newly generated layered structure, inducing the precursor to undergo directional epitaxial growth, thereby forming a single-crystal ternary cathode material with complete grains and few grain boundaries.
[0039] In some implementations, cooling and post-processing may include furnace cooling, controlled-rate cooling, or natural cooling to room temperature. The sintered product is then lightly pulverized and sieved, and demagnetized if necessary to remove any introduced metallic impurities. Further surface coating treatment may be performed as needed, such as using coating materials like Li3PO4, LiNbO3, Li2ZrO3, or Al2O3, to further improve the material's cycle stability and interfacial stability. The final product is a regenerated single-crystal ternary cathode material. Example 1
[0040] The method for directly regenerating single-crystal NCM811 ternary cathode material from waste NCM811 cathode material specifically includes the following steps: Step 1, collect waste LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) cathode material, using 500 o Heat treatment in air at 120°C for 5 hours to remove polyvinylidene fluoride binder and conductive carbon black, followed by washing with deionized water three times, and then at 120°C. o Vacuum drying at C for 12 hours yields clean waste cathode material.
[0041] Step 2: Add the waste cathode material obtained in Step 1 to a planetary ball mill for crushing. The ball-to-material ratio is 10:1, the ball milling speed is 400 r / min, and the ball milling time is 8 h to obtain waste cathode material seed crystals with an average particle size of about 0.8 μm.
[0042] Step 3, weigh 100g LiNi 0.8 Co 0.1 Mn 0.1(OH)2 precursor, LiOH·H2O is added as lithium source, wherein the molar ratio of Li to transition metal element is 1.05:1, and 5g of seed crystals obtained in step 2 are added. The mixture is mixed for 4 hours using a slant mixer to make the seed crystals uniformly dispersed in the precursor and lithium source.
[0043] Step 4: The mixed powder obtained in Step 3 is loaded into a crucible and placed in a tube furnace for sintering in a pure oxygen atmosphere at 3... o Heat up to 500 °C / min o C, keep warm for 5 hours, then continue at 3 o Temperature increased to 780 °C / min o C, heat for 15 hours to allow the precursor to undergo a solid-state reaction, and use waste cathode material seed crystals as heterogeneous nucleation centers to induce single crystal growth.
[0044] Step 5: After sintering, the furnace is cooled to room temperature. The sintered product is then lightly crushed and sieved to obtain the regenerated single-crystal NCM811 cathode material.
[0045] The XRD image of the regenerated single-crystal NCM811 cathode material prepared in this embodiment is as follows: Figure 1 As shown in the figure, the material exhibits typical α-NaFeO2 layered structure characteristics (R-3m space group), and no obvious impurity phase peaks were detected; the SEM image is shown below. Figure 2 As shown, it exhibits obvious characteristics of a single-crystal material; the results of the cyclic charge-discharge test are as follows: Figure 3 As shown, from Figure 3 It can be seen that the regenerated single-crystal ternary cathode material has good initial specific capacity and capacity retention. Example 2
[0046] The method for directly regenerating single-crystal NCM523 ternary cathode material from waste NCM523 cathode material specifically includes the following steps: Step 1, collect waste LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523) cathode material, after 450 o Heat treatment at 100°C for 6 hours removes polyvinylidene fluoride binder and conductive carbon black, followed by washing three times with deionized water. o Dry at C for 10 hours.
[0047] Step 2: Place the waste cathode material in a sand mill and crush it for 4 hours to obtain seed crystals with an average particle size of about 0.5 μm.
[0048] Step 3, weigh LiNi 0.5 Co 0.2 Mn 0.3100g of (OH)2 precursor was added to Li2CO3 as a lithium source, wherein the molar ratio of Li to transition metal element was 1.04:1. Then, 8g of seed crystals obtained in step 2 were added, and the mixture was mixed for 3 hours using a high-speed mixer.
[0049] Step 4: Place the mixture obtained in Step 3 into a crucible and put it in a muffle furnace, then heat it in air at 5°C. o Heat up to 800 °C / min o C, keep warm for 12 hours.
[0050] Step 5: After sintering, the furnace is cooled to room temperature. The sintered product is then lightly crushed and sieved to obtain regenerated single-crystal NCM523 cathode material.
[0051] Step 6: Weigh the regenerated single-crystal NCM523 cathode material obtained in Step 5 and add it to a 0.05 mol / L aluminum nitrate nonahydrate solution. Mix thoroughly by magnetic stirring, then rinse three times with deionized water. Finally, heat at 80°C... o Dry at C for 6 hours.
[0052] Step 7: After grinding the material obtained in Step 6, place it in a tube furnace and heat it at 3... o Heat up to 500 °C / min o C, heat preservation for 3 hours to obtain aluminum-coated recycled single crystal NCM523 cathode material. Example 3
[0053] The method for directly regenerating single-crystal NCM111 ternary cathode material from waste NCM111 cathode material specifically includes the following steps: Step 1, collect waste LiNi 0.33 Co 0.33 Mn 0.33 O2 (NCM111) cathode material, after 500 o Heat treatment at 100°C for 6 hours removes polyvinylidene fluoride binder and conductive carbon black, followed by washing three times with deionized water. o Dry at C for 10 hours.
[0054] Step 2: Place the waste cathode material in an air jet mill and pulverize for 4 hours to obtain seed crystals with an average particle size of about 0.3 μm.
[0055] Step 3, weigh 100 g Ni 0.33 Co 0.33 Mn 0.33 (OH)2 precursor, LiOH·H2O is added as lithium source, the molar ratio of Li to transition metal element is 1.05:1, 10 g of seed crystals obtained in step 2 and molybdenum oxide with a doping amount of 0.5 mol% are added at the same time, and the mixture is mixed for 5 h using a double cone mixer.
[0056] Step 4: Place the mixed powder obtained in Step 3 under an oxygen atmosphere, at 2... o Heat up to 500 °C / min o Keep warm at 4°C for 4 hours, then raise the temperature to 800°C. o Keep warm at C for 12 hours.
[0057] Step 5: After sintering, use a programmed cooling method (cooling rate of 5). o Cool to room temperature (C / min) to obtain Mo-doped regenerated single-crystal NCM111 ternary cathode material.
[0058] The specific embodiments of the present invention have been described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention.
Claims
1. A method for directly regenerating single-crystal ternary cathode materials from waste cathode materials, characterized in that... Includes the following steps: Waste lithium-ion battery ternary cathode materials are recycled and processed to remove current collectors, binders and conductive agents, and waste ternary cathode active materials are obtained. The waste ternary cathode active material is pulverized by ball milling, sand milling or air jet milling to obtain seed particles with an average particle size of 0.1 to 2 μm; According to the target single-crystal ternary cathode material composition, the seed particles are mixed with the ternary cathode material precursor and lithium source, and the mixture is thoroughly and uniformly mixed. The resulting mixture was calcined at high temperature to induce a solid-state reaction in the precursor, and epitaxial growth was performed using the seed particles as growth cores to obtain a single-crystal ternary cathode material. After cooling, a regenerated single-crystal ternary cathode material is obtained.
2. The method for directly regenerating single-crystal ternary cathode material from waste cathode material according to claim 1, characterized in that: The ternary cathode material of the spent lithium-ion batteries includes LiNi. x Co y Mn 1-x-y One or more of the O2 materials, including NCM111, NCM523, NCM622, NCM811, NCA or any mixture thereof in any proportion.
3. The method for directly regenerating single-crystal ternary cathode material from waste cathode material according to claim 1, characterized in that: The recycling and processing of waste lithium-ion battery ternary cathode materials involves heat treatment or dispersion and cleaning with weak acidic solvents, including acetic acid, formic acid, hypochlorous acid, nitrous acid, or citric acid.
4. The method for directly regenerating single-crystal ternary cathode material from waste cathode material according to claim 1, characterized in that: The pulverized seed crystal particles D50 have a particle size of 0.1 to 2 μm; the seed crystal particles are subjected to tempering treatment; the amount of seed crystal particles added is 0.1 to 30 wt% of the total mass of the final mixture.
5. The method for directly regenerating single-crystal ternary cathode material from waste cathode material according to claim 1, characterized in that: The chemical formula of the ternary cathode material precursor is Ni. x Co y Mn 1-x-y (OH)2; the lithium source includes one or more of LiOH, LiOH·H2O, and Li2CO3 in any proportion.
6. The method for directly regenerating single-crystal ternary cathode material from waste cathode material according to claim 1, characterized in that: The high-temperature calcination is at 400°C. o C~1000 o C, keep warm for 5-30 hours; the atmosphere is air, oxygen, or a mixture of oxygen and air in any ratio.
7. The method for directly regenerating single-crystal ternary cathode material from waste cathode material according to claim 1, characterized in that: During the mixing process of the seed crystal particles with the ternary cathode material precursor and lithium source, one or more metal dopants selected from Al, Mg, Ti, Zr, Mo, W, Nb, Y, and B can also be added.
8. The method for directly regenerating single-crystal ternary cathode material from waste cathode material according to claim 1, characterized in that: The cooling is carried out by furnace cooling, natural cooling, or programmed cooling; the cooled product can also be screened, demagnetized, lightly crushed, or surface coated.
9. A regenerated single-crystal ternary cathode material, characterized in that: The method for directly regenerating single-crystal ternary cathode material from waste cathode material as described in any one of claims 1 to 8 is used to prepare the regenerated single-crystal ternary cathode material. The primary particle size of the regenerated single-crystal ternary cathode material is 2 to 6 μm, the secondary particle agglomeration degree is low, and the number of grain boundaries is reduced.
10. A regenerated single-crystal ternary cathode material according to claim 9 can be used as a ternary cathode material for lithium-ion batteries.
Citation Information
Patent Citations
A hydrothermal lithium replenishment-spray remodeling method for waste ternary cathode materials
CN111129487B
Method for in-situ preparation of positive electrode material from seed crystal
CN115744875A