A type of aluminum-plastic composite film for soft-pack battery cells whose quality can be easily judged visually during the stamping process.
By introducing a double-layer color-developing PP functional component into the aluminum-plastic composite film, and using color contrast to identify stamping defects, the problem of difficulty in quickly identifying defects in the rounded corner area of the aluminum-plastic composite film in the existing technology is solved, and efficient and low-cost online quality control is achieved.
Patent Information
- Application Number
- CN202611600899.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing aluminum-plastic composite films are difficult to quickly, directly, and non-destructively identify minute cracks and defects in rounded corner areas during the stamping process, resulting in a high rate of missed detections and increasing the risk of cell leakage and safety.
The system employs a dual-layer color-detecting PP functional component, consisting of a continuous colored masking PP sublayer and a local warning PP sublayer. The molding quality is directly determined by the color contrast. The local warning PP sublayer is only set in the rounded corner area, sandwiched between the continuous colored masking PP layer and the first polyurethane adhesive layer, forming a clear color difference to identify defects.
It improves the visual identifiability of stamping defects and the efficiency of online quality assessment, reduces inspection costs and the risk of misjudgment, and keeps the performance of aluminum-plastic composite film unaffected.
Smart Images

Figure CN123121007A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery packaging materials technology, specifically to a soft-pack battery cell aluminum-plastic composite film that allows for direct visual judgment of its quality during the stamping and forming process. Background Technology
[0002] Soft-pack lithium-ion cells commonly use aluminum-plastic composite film as the outer casing material. During cell manufacturing, the aluminum-plastic composite film needs to be stamped to form recesses with accommodating space to accommodate the cell electrode assembly. During stamping, the aluminum-plastic composite film undergoes significant plastic deformation under the action of the stamping die, especially in the four rounded corner areas of the recess. Due to the multi-directional stretching and bending of the material, stress is highly concentrated, making it prone to microcracks, pinholes, delamination, and even localized penetrating damage. These defects are often tiny and covered by the outer material, making them difficult to detect with the naked eye under natural light or conventional workshop lighting conditions.
[0003] Currently, the industry mainly relies on strong light visual inspection, dye penetration testing, or offline optical inspection equipment to inspect the quality of aluminum-plastic film stamping. Strong light visual inspection is not sensitive enough to micro-cracks and is prone to missing them; dye penetration testing is a destructive sampling inspection and cannot achieve full online inspection; offline optical inspection equipment is expensive and has a slow inspection cycle, making it difficult to meet the needs of high-speed continuous production. Therefore, existing aluminum-plastic composite film stamping processes lack a fast, direct, and non-destructive online visual judgment method, which makes defective stamped parts easy to flow into subsequent packaging processes, increasing the risk of cell leakage, gas expansion, and even safety failure.
[0004] To reduce the missed detection rate of defects in rounded corner areas during stamping, the industry has attempted to add functional layers to the outer layer of the aluminum-plastic film to improve inspection convenience, such as using a uniform colored outer layer and adding easily identifiable markings. However, a uniform colored outer layer cannot provide selective warnings for specific high-risk areas (such as rounded corners), and the difference in appearance before and after damage is not obvious, making direct judgment difficult. The additional marking layers are mostly integral coatings, which cannot accurately match the deformation area of the stamping mold, and also have problems such as increasing film thickness, affecting molding performance, and increasing material costs.
[0005] Therefore, providing an aluminum-plastic composite film that can quickly determine whether the forming quality of the rounded corner area is qualified by direct visual observation without the need for auxiliary equipment during the stamping process is an urgent technical problem to be solved in the field of soft-pack battery packaging. Summary of the Invention
[0006] The purpose of this invention is to provide a flexible battery cell aluminum-plastic composite film that allows for direct visual judgment of its quality during the stamping process. Existing flexible battery cell aluminum-plastic composite films, after stamping, suffer from defects such as through-cracks, tears, or localized breaks in the rounded corner areas due to the uniform color of the protective layer. These defects are difficult to identify directly and quickly visually, resulting in high missed rates during manual visual inspection and high costs and susceptibility to environmental interference during machine vision inspection. The aluminum-plastic composite film provided by this invention allows for direct and intuitive judgment of quality by observing the color contrast of the rounded corner areas after stamping, thereby effectively improving the efficiency and accuracy of online quality judgment and reducing the risk of defective products flowing into subsequent processes.
[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows: This invention provides a flexible battery cell aluminum-plastic composite film, comprising, from the outside to the inside, a double-layer color-developing and waste-detecting PP functional component, a first polyurethane adhesive layer, an aluminum foil, a second polyurethane adhesive layer, and an inner heat-sealing PP layer. The double-layer color-developing and waste-detecting PP functional component includes a continuous colored masking PP sub-layer on the outer surface and four local warning PP sub-layers disposed on the side of the continuous colored masking PP sub-layer facing the aluminum foil. The four local warning PP sub-layers are respectively disposed at positions corresponding to the four rounded corners of the flexible battery cell's stamping area, and each forms a rounded L-shaped warning area consistent with the extension direction of the corresponding rounded corner. The local warning PP sub-layers are a different color from the continuous colored masking PP sub-layer, and are sandwiched between the continuous colored masking PP sub-layer and the first polyurethane adhesive layer. The four local warning PP sub-layers are spaced apart from each other and are not interconnected. When the continuous colored masking PP sub-layer remains intact, it covers the local warning PP sub-layers, so that the local warning PP sub-layers are not directly exposed to the outer surface of the flexible battery cell aluminum-plastic composite film.
[0008] like Figure 1 and Figure 2 As shown, Figure 1 The positional relationship between the local warning PP sublayer and the predetermined stamping forming area of the present invention is shown. The four rounded L-shaped local warning areas are respectively set at the four rounded corner positions of the predetermined stamping forming area and are arranged along the extension direction on both sides of the corresponding rounded corners to cover the high-risk areas that are prone to stress concentration and cracking during the stamping process. Figure 2The layered structure at the transverse termination edge of the local warning PP sublayer is shown. The composite film, from the outside to the inside, includes a continuous colored masking PP sublayer, a local warning PP sublayer, a first polyurethane adhesive layer, an aluminum foil, a second polyurethane adhesive layer, and an inner heat-sealed PP layer. The local warning PP sublayer is only provided in the rounded L-shaped warning area and sandwiched between the continuous colored masking PP sublayer and the first polyurethane adhesive layer. The non-warning area does not have a local warning PP sublayer. Therefore, when the continuous colored masking PP sublayer remains intact, the local warning PP sublayer is not directly exposed on the outer surface of the composite film. When the stamping process causes the continuous colored masking PP sublayer in the corresponding rounded corner area to have a through crack, tear, or partial breakage, the underlying local warning PP sublayer can be exposed from the damaged position, thereby using color contrast to achieve direct visual judgment of stamping defects.
[0009] The continuous colored masking PP sublayer and the local warning PP sublayer are each independently measured in 100 parts by weight of their respective PP base material. Taking the PP base material in the continuous colored masking PP sublayer as 100 parts by weight, this sublayer contains 100 parts of PP base material, 5-10 parts of the first-color PP masterbatch, 5-10 parts of titanium dioxide PP masterbatch, and 0-3 parts of maleic anhydride-grafted PP. Taking the PP base material in the local warning PP sublayer as 100 parts by weight, this sublayer contains 100 parts of PP base material, 10-30 parts of the second-color PP masterbatch, and 6-15 parts of maleic anhydride-grafted PP. The above weight percentages are used to define the raw material ratio of each sublayer and do not represent the total weight distribution ratio of the two sublayers in the final composite film. The actual amount of the local warning PP sublayer in the final composite film is determined by the area of the rounded L-shaped warning area and the thickness of the local warning PP sublayer. Both the first color PP masterbatch and the second color PP masterbatch can be colored masterbatches with PP as the carrier, and the two have different colors and form a recognizable color contrast; among them, phthalocyanine blue masterbatch and quinacridone red masterbatch with PP as the carrier are preferred combinations of the first color PP masterbatch and the second color PP masterbatch, respectively.
[0010] To balance masking effect and warning color contrast, the thickness of the continuous colored masking PP sublayer can be controlled to be 20–38 μm, more preferably 24–32 μm; the thickness of the local warning PP sublayer can be controlled to be 4–10 μm, more preferably 5–8 μm. The strip width of each rounded L-shaped warning area can be 3–8 mm, preferably 4–6 mm, the length of the two arms is 10–25 mm, preferably 12–20 mm, and the inner corner radius is 3–12 mm, preferably 5–10 mm. By setting the size of the rounded L-shaped warning area within the above range, it can be ensured that the warning area covers the rounded deformation area at which cracking is likely to occur due to stress concentration during the stamping process. Based on 100 parts of PP base material in each sublayer, the amount of the first color PP masterbatch added to the continuous colored masking PP sublayer is preferably 6–10 parts, and the amount of titanium dioxide PP masterbatch added is preferably 6–10 parts; the amount of the second color PP masterbatch added to the local warning PP sublayer is preferably 12–28 parts. The introduction of titanium dioxide PP masterbatch can improve the hiding power of continuous colored masking PP sublayer, making the blue color on the outer surface more uniform and saturated.
[0011] The maleic anhydride grafting rate of maleic anhydride-grafted PP can be 0.6–1.5 wt%. Based on 100 parts of PP base material in each sublayer, the amount of maleic anhydride-grafted PP added to the continuous colored masking PP sublayer is 0–3 parts, and the amount added to the local warning PP sublayer is 6–15 parts, resulting in a relatively high maleic anhydride-grafted PP content in the local warning PP sublayer. The presence of maleic anhydride-grafted PP enhances the interfacial bonding force between PP sublayers and between PP sublayers and adjacent adhesive layers. This helps the relatively thin local warning PP sublayer adhere firmly to the side of the continuous colored masking PP sublayer facing the aluminum foil, preventing displacement or failure of the local warning PP sublayer due to interlayer peeling during stamping.
[0012] The aluminum foil thickness is typically 30–50 μm. The inner heat-sealed PP layer uses cast polypropylene film, typically 50–80 μm thick. The first and second polyurethane adhesive layers are formed by drying and curing a two-component polyurethane composite adhesive solution; by weight, the two-component polyurethane composite adhesive solution comprises 100 parts of polyurethane main agent, 10 parts of curing agent, and 173 parts of ethyl acetate, wherein the polyurethane main agent has a solid content of 75 wt%. In the embodiment, the polyurethane main agent is YH-501, and the curing agent is YH-10. The dry adhesive coating amount of the first polyurethane adhesive layer is controlled to be 2.0–4.5 g / m². 2 The dry adhesive coating amount of the second polyurethane adhesive layer is controlled to be 2.0–4.5 g / m². 2Four rounded L-shaped warning areas are respectively set on the outer sides of the four rounded corners of the predetermined stamping shell outline. The planar position deviation between the inner rounded corner center of each rounded L-shaped warning area and the corresponding predetermined stamping shell rounded corner center is no more than 2.0 mm, preferably controlled within 0 to 2.0 mm. The above positioning ensures that the local warning PP sub-layer only covers the area around the rounded corner where the stamping shell deformation is most severe. Once the continuous colored masking PP sub-layer develops a through crack, tear, or local breakage at this location, the red warning layer below the damaged area will be exposed, forming a sharp color contrast. The PP base material used for the continuous colored masking PP sub-layer can be selected with a melt flow rate in the range of 2 to 8 g / 10 min (230℃, 2.16 kg); the polypropylene resin used for the cast polypropylene film layer can be selected with a melt flow rate in the range of 3 to 10 g / 10 min, to facilitate extrusion casting and obtain a product with uniform thickness.
[0013] This invention also provides a method for preparing the above-mentioned soft-pack battery cell aluminum-plastic composite film, the steps of which are as follows: taking 100 parts of PP base material in the continuous colored masking PP sublayer as 100 parts, 100 parts of PP base material, 5-10 parts of first color PP masterbatch, 5-10 parts of titanium dioxide PP masterbatch, and 0-3 parts of maleic anhydride grafted PP are mixed, melt-extruded at 180-215℃ and cooled to form a film, to obtain a continuous colored masking PP film with a thickness of 20-38 μm; taking the local color masking PP sublayer as 100 parts of PP base material in the continuous colored ... The red warning PP film, with a thickness of 4-10 μm, is prepared by mixing 100 parts of PP base material, 10-30 parts of second-color PP masterbatch, and 6-15 parts of maleic anhydride-grafted PP. The mixture is then melt-extruded at 180-215°C and cooled to form a film. The red warning PP film is then cut into four rounded L-shaped warning strips. Each strip has a strip width of 3-8 mm and two arms with lengths of 10-25 mm. The inner corner radius is 3-12mm; the positions of the four rounded corners of the punching shell are determined according to the predetermined punching shell forming contour, and the four rounded L-shaped warning pieces are respectively positioned on the side of the continuous colored masking PP film facing the aluminum foil, so that the position of each warning piece corresponds to the corresponding rounded corner of the punching shell, and the positional deviation between the center of the inner corner of each warning piece and the center of the corresponding predetermined rounded corner of the punching shell is controlled within 0-2.0mm. The film is hot-pressed for 3-12s at 120-150℃ and 0.2-0.6MPa to fix the rounded L-shaped warning pieces to the continuous colored masking PP film, thus obtaining a double-layer color-developing waste-judgment PP functional film; a two-component polyurethane composite adhesive is prepared by mixing 100 parts of polyurethane main agent, 10 parts of curing agent, and 173 parts of ethyl acetate according to mass, wherein the solid content of the polyurethane main agent is 75wt%; the adhesive is applied to the side of the double-layer color-developing waste-judgment PP functional film with the rounded L-shaped warning pieces, and the dry adhesive coating amount is controlled to be 2.0-4.5g / m³. 2The first composite film was obtained by laminating the aluminum foil with a thickness of 30–50 μm at 55–85℃ and 0.20–0.50 MPa. A two-component polyurethane composite adhesive with the same formulation was then coated on the side of the aluminum foil opposite to the double-layer color-developing and waste-judging PP functional film, with the dry adhesive coating amount controlled at 2.0–4.5 g / m². 2 The film is laminated with a cast polypropylene film with a thickness of 50–80 μm at 55–85℃ and 0.20–0.50 MPa. The resulting composite film is then cured at 40–60℃ for 24–72 hours to obtain a soft-pack battery cell aluminum-plastic composite film. Both types of PP films can be continuously prepared according to their respective formulations. Only the rounded L-shaped warning pieces obtained from cutting the red warning PP film are used in the final lamination; the uncut red warning PP film is not included in the actual amount of local warning PP sublayers used in the final composite film.
[0014] When using the aluminum-plastic composite film of the soft-pack battery cell for stamping, visual quality can be judged as follows: Position the aluminum-plastic composite film of the soft-pack battery cell according to the predetermined stamping outline, so that the four local warning PP sub-layers correspond to the four rounded corner positions of the stamping area; after the stamping is completed, observe the four rounded corner areas from the side where the double-layer color-coded rejection PP functional components are located; if no color of the local warning PP sub-layer is exposed through the opening of the continuous colored masking PP sub-layer in any of the four rounded corner areas, the stamped part is judged to pass this appearance judgment; if the color of the local warning PP sub-layer is exposed due to the through crack, tear, or partial breakage of the continuous colored masking PP sub-layer in any rounded corner area, the stamped part is judged to fail this appearance judgment. This visual judgment targets rounded corner forming defects that can cause through cracks, tears, or partial breaks in the continuous colored masking PP sub-layer and expose the warning color below, and does not consider internal defects that do not cause the above-mentioned outer layer openings as the direct detection object of this visual judgment.
[0015] As a technological derivative based on the aforementioned color contrast rejection principle, the color-displaying structure can also employ a single-layer colored PP / aluminum foil composite structure. This means that no local warning PP sub-layer is provided; only the PP layer laminated to the outer surface of the aluminum foil is colored. The colored PP layer is made from a PP base material with a certain degree of light transmittance and transparent colored masterbatch. By controlling the amount of colored masterbatch added and the initial thickness of the colored PP layer, the un-punched area is uniformly colored, thus masking the silvery-white aluminum foil. When excessive bidirectional stretching occurs at the punched corners, the colored PP layer locally thins, simultaneously reducing the amount of colorant and the optical path per unit area, increasing light transmittance. This allows the light color or silvery-white of the underlying aluminum foil to be displayed, creating a recognizable color contrast with the surrounding areas that are not excessively thinned.
[0016] As another technological development, the PP layer and the first polyurethane adhesive layer laminated on the outside of the aluminum foil can be kept transparent or have low haze, and a colored treatment can be applied to the surface of the aluminum foil facing the PP layer. This colored treatment can involve forming a colored conversion layer or colored coating containing a trace amount of colorant on the aluminum foil surface. The amount of colorant added and the coating thickness are determined so that the normal area exhibits a continuous, uniform light color without significantly affecting the barrier properties and composite strength of the aluminum foil. When the aluminum foil and its surface colored layer at the rounded corners of the stamped shell undergo excessive stretching, the colorant content per unit area of the colored layer decreases, or microcracks appear in the colored layer, locally exposing the silvery-white color of the aluminum foil itself. This causes the area to appear lighter in color, with enhanced silvery-white, or to show light-colored streaks or spots; these changes can be observed through the transparent or low-haze PP layer.
[0017] When employing any of the above-mentioned derivative solutions, the undeformed planar area of the stamped shell can be used as a reference under a unified light source to visually observe the four rounded corner areas, or the L*, a*, and b* values of the rounded corner areas and the reference area can be collected by a visual inspection system and the color difference ΔE can be calculated. When the rounded corner area shows a visible light-colored or silvery-white aluminum foil, a significant color fading, or the color difference between it and the reference area reaches the rejection threshold pre-calibrated using qualified samples and excessively deep-stamped samples, it is determined that the rounded corner area has a risk of excessive thinning. Thus, the rejection method of "exposing warning color after outer layer opening" of this invention can be extended to a rejection method of "comprehensive color change caused by local excessive thinning or color layer rupture". The above-mentioned derivative solutions can be used alone or in combination with the aforementioned dual-layer color-display rejection PP functional component.
[0018] Compared with the prior art, the beneficial effects of the present invention are: 1. The visual identifiability of defects in the stamping process is significantly improved. When the continuous colored masking PP sublayer experiences through-cracks, breaks, or local fractures at the rounded corners during the stamping process, the color of the underlying local warning PP sublayer is exposed from the damaged area, creating a strong contrast with the color of the surrounding intact masking layer. Operators can quickly identify defects directly with the naked eye without relying on complex vision equipment, effectively reducing the risk of missing minute cracks in the rounded corner area.
[0019] 2. Improved efficiency and reduced inspection costs in online quality assessment. Defect identification can be achieved simply by comparing the color between the outer layer and the warning layer. Conventional visual inspection or simple photoelectric detection can replace high-resolution machine vision systems and their algorithms, reducing sensitivity to ambient light and film surface reflection. This results in faster inspection cycles and significantly reduced equipment investment and maintenance costs.
[0020] 3. Precise defect location, reducing the likelihood of misjudgment. The four local warning PP sub-layers are independent and only cover the high-risk areas corresponding to the rounded corners of the stamped shell. The warning color exposed after damage directly indicates the specific rounded corner location of the defect, facilitating the rapid rejection of defective products. In intact areas, the red warning layer is completely covered, and the overall appearance of the composite film is uniform, preventing incorrect judgment of non-rounded corner areas.
[0021] 4. The structural design is reliable and does not compromise the intrinsic properties of the aluminum-plastic composite film. The localized warning PP sublayer is sandwiched between a continuous colored masking PP sublayer and the first polyurethane adhesive layer, with maleic anhydride-grafted PP used to strengthen the interlayer bonding. During normal use, the warning layer is not exposed, and the film surface maintains a consistent blue appearance. The reasonable combination of the thickness and size of each functional layer ensures that the aluminum-plastic composite film still possesses good barrier properties, electrolyte resistance, and die-casting adaptability, without weakening the core performance of battery encapsulation due to the addition of the color-developing structure.
[0022] 5. The manufacturing process is highly adaptable and easy to promote on existing production lines. The preparation of the double-layer color-developing waste-detecting PP functional film, the positioning of the warning sheet, and the hot-press lamination can all be achieved by adding simple workstations using conventional dry lamination equipment. No major modifications to existing stamping molds are required. The material formula and process parameters are compatible with the existing aluminum-plastic composite film production system, requiring minimal equipment modification and facilitating industrialization. Attached Figure Description
[0023] Figure 1 This is a schematic diagram showing the positional relationship between the local warning PP sublayer and the predetermined stamping area described in this invention; Among them, ①-four rounded L-shaped local warning areas, ②-pre-determined shell forming area.
[0024] Figure 2 This is a schematic cross-sectional view of the layered structure at the lateral termination edge of the local warning PP sublayer of the present invention; Among them, ①- Continuous colored masking PP sub-layer (covering the entire outer surface, continuously present), ②- Local warning PP sub-layer (only present in the rounded L-shaped area, sandwiched between ① and ③), ③- First polyurethane adhesive layer (thin layer), ④- Aluminum foil (barrier layer, relatively thick and dense layer), ⑤- Second polyurethane adhesive layer (thin layer), ⑥- Inner heat-sealing PP layer (facing the inner side of the cell, heat-sealing layer).
[0025] Figure 3 This is a scanning electron microscope cross-sectional morphology image of the aluminum-plastic composite film for the soft-pack battery cell prepared in Example 1 of the present invention.
[0026] Figure 4 This is a super depth-of-field microscope image of the rounded corner area sample of the soft-pack battery cell aluminum-plastic composite film prepared in Example 1 of the present invention after being formed by punching. Detailed Implementation
[0027] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are merely some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0028] Manufacturer model and property information of the raw materials involved in the embodiments / comparative examples of this invention: The melt flow rate of the PP base material is 3.0 g / 10 min; The first color PP masterbatch uses PP as a carrier and contains 40wt% phthalocyanine blue pigment.
[0029] Titanium dioxide PP masterbatch is a white masterbatch of PP / TiO2-60, with PP as the carrier and TiO2 content of 60wt%.
[0030] The second color PP masterbatch is a PP quinacridone red masterbatch, with PP as the carrier and a quinacridone red pigment content of 30wt%.
[0031] Maleic anhydride grafted onto PP, wherein the maleic anhydride grafting rate is 0.8–1.2 wt%.
[0032] The aluminum foil is 8011-O soft aluminum foil.
[0033] The polyurethane main component of the two-component polyurethane composite adhesive is YH-501 (solid content 75wt%), and the curing agent is YH-10.
[0034] The inner heat-sealed cast polypropylene film is a CPP-L11 type CPP composite film.
[0035] The polyurethane composite adhesive is prepared by weight of 100 parts YH-501 main agent, 10 parts YH-10 curing agent and 173 parts ethyl acetate. YH-10 is used as supplied by the manufacturer.
[0036] The cast polypropylene (CPP) film is Kelly CPP-L11.
[0037] Example 1
[0038] Preparation of an aluminum-plastic composite film for soft-pack battery cells 1. Preparation of a double-layer colorimetric waste detection PP functional film 1.1 Independent formulation for each sublayer The continuous colored masking PP sublayer and the local warning PP sublayer were each independently measured in 100 parts by weight of their respective PP base material. The formulations of each sublayer in Example 1 are as follows: The formulation for continuous colored masking PP sublayer is as follows: 100 parts PP base material, 8 parts first color PP masterbatch, 8 parts titanium dioxide PP masterbatch, and 1.6 parts maleic anhydride grafted PP. The formulation for the local warning PP sublayer is as follows: 100 parts PP base material, 16 parts second color PP masterbatch, and 7.2 parts maleic anhydride grafted PP.
[0039] Note: The mass fractions of the continuous colored masking PP sublayer and the local warning PP sublayer mentioned above are the formulation basis within their respective sublayers. The kg-level weighings in S1 and S2 are used for film-making batches of the continuous blue PP film and the red warning PP film, respectively; only the four rounded L-shaped warning pieces cut from the red warning PP film are included in the final single-sheet composite film, and the unused portion is not included in the mass of the local warning PP sublayer of the final product.
[0040] 1.2 Preparation method S1. Weigh 75 kg of PP base material (melt flow rate 3.0 g / 10 min), 6 kg of first-color PP masterbatch, 6 kg of titanium dioxide PP masterbatch, and 1.2 kg of maleic anhydride-grafted PP according to the continuous colored masking PP sublayer formula. Put them into a high-speed mixer and mix at 300 r / min for 10 min to obtain a premix. Add the premix to a single-screw extruder. Set the temperatures of each section of the extruder to 190℃, 200℃, 205℃, and 200℃ (from the feed port to the die), with a die temperature of 195℃ and a screw speed of 40 r / min. After melt extrusion, cool and shape the film by a cooling roller (cooling water temperature 20℃), and then traction and wind it to obtain a continuous colored masking PP film with a thickness of 28 μm.
[0041] S2. Weigh 25 kg of PP base material (same as S1), 4 kg of second-color PP masterbatch, and 1.8 kg of maleic anhydride-grafted PP according to the local warning PP sublayer formula. Put them into a high-speed mixer and mix at 300 r / min for 10 min to obtain a premix. Add the premix to another single-screw extruder. The temperature of each section of the extruder is the same as in S1, the die temperature is 195℃, and the screw speed is 30 r / min. After melt extrusion, it is cooled and shaped by cooling rollers (cooling water 20℃), and then pulled and wound to obtain a red warning PP film with a thickness of 6 μm.
[0042] S3. Lay the red warning PP film obtained in step S2 flat on the die-cutting machine table, and use a die of a predetermined shape to cut it to obtain four rounded L-shaped warning pieces. The strip width of each rounded L-shaped warning piece is 5mm, the length of each arm is 15mm, and the inner radius of the rounded corner is 7mm.
[0043] S4. On the side of the continuous colored masking PP film facing the aluminum foil, positioning marks are made at the four rounded corners corresponding to the predetermined punching outline using a printing method. Using a tooling template with positioning pins, the four rounded L-shaped warning pieces are placed at each marked position, ensuring that the planar positional deviation between the center of the inner rounded corner of each warning piece and the center of the corresponding predetermined punching corner does not exceed 1.5mm. The stacked films are placed in a flatbed hot press and hot-pressed at 135℃ and 0.4MPa for 8s to fix the rounded L-shaped warning pieces onto the continuous colored masking PP film. After cooling, they are removed to obtain a double-layer color-developing waste-judgment PP functional film.
[0044] 2. Preparation of aluminum-plastic composite film for soft-pack battery cells 2.1 Layer Structure Parameters Example 1 uses 40μm thick 8011-O flexible aluminum foil; the continuous colored masking PP sublayer has a thickness of 28μm, and the local warning PP sublayer has a thickness of 6μm; the dry adhesive coating weight of both the first and second polyurethane adhesive layers is 3.0g / m². 2 The inner heat-sealed PP layer uses a 60μm thick cast polypropylene film. The local warning PP sublayer exists only in the four rounded L-shaped warning areas, and its actual mass in the final composite film is determined by the local coverage area and the 6μm thickness, not by the total batch mass of the red warning PP film.
[0045] 2.2 Preparation method S5. Take a 40μm thick 8011-O soft aluminum foil. Prepare the polyurethane composite adhesive: Mix 10.0kg of main agent YH-501 (75% solid content) with 1.0kg of curing agent YH-10, add 17.3kg of ethyl acetate (the mass ratio of main agent, curing agent, and ethyl acetate is 100:10:173), and stir at 200r / min for 30min to obtain a uniform polyurethane composite adhesive. Apply the adhesive to one surface of the aluminum foil using a 200-line anilox roller at a coating speed of 30m / min, and dry in an 80℃ oven to obtain a dry adhesive coating weight of 3.0g / m². 2 The first polyurethane adhesive layer. The side of the double-layer color-developing waste-judgment PP functional film obtained in step S4, which has a rounded L-shaped warning piece, is bonded to the adhesive surface, and then laminated by a composite roller at 75°C and 0.35MPa linear pressure to obtain the first composite film.
[0046] S6. On the other side of the aluminum foil of the first composite film, apply the same adhesive and coating method as in S5, controlling the dry adhesive coating amount to 3.0 g / m². 2 A second polyurethane adhesive layer is formed. Subsequently, a 60μm thick cast polypropylene film is bonded to the adhesive-coated surface and laminated by a composite roller at 75°C and 0.35MPa linear pressure to obtain a second composite film.
[0047] S7. Place the composite film roll obtained in step S6 in a constant temperature drying room and cure it at 50°C for 48 hours. Take it out and cool it to room temperature to obtain the soft-pack battery cell aluminum-plastic composite film.
[0048] The outer surface of the composite film is uniformly blue, and the local warning PP sublayer is completely covered by a continuous colored masking PP sublayer, making it invisible from the outside.
[0049] like Figure 3 The image shown is a scanning electron microscope cross-sectional morphology image of the aluminum-plastic composite film for the soft-pack battery cell prepared in Example 1. The cross-sectional sampling location is located inside the rounded L-shaped local warning area. Figure 3 It can be seen that the obtained composite film cross-section exhibits a relatively clear multilayer composite structure, with each layer continuously distributed along the thickness direction. The interlayer interfaces are generally smooth, and no obvious large-area pores, delamination, or interface separation phenomena were observed. Among them, the dense and grayish area in the middle corresponds to the aluminum foil layer, and the aluminum foil forms a stable composite structure with the polymer functional layer and the inner heat-sealed PP layer on both sides, respectively. Based on the preparation record of Example 1, the thickness of the outer continuous colored masking PP film is 28 μm, the thickness of the local warning PP film is 6 μm, the thickness of the aluminum foil is 40 μm, and the thickness of the inner heat-sealed PP layer is 60 μm. Figure 3 It is mainly used to verify the hierarchical order, continuity and interface bonding of each functional layer. The thickness value is based on the preparation control parameters and cross-sectional measurement records of the embodiment.
[0050] like Figure 4 The image shown is a deep-field microscope photograph of the rounded corner area of the aluminum-plastic composite film for the soft-pack battery cell prepared in Example 1 after it has been formed by punching. Figure 4 It can be seen that after stamping, the composite film exhibits significant bending and stretching deformation in the rounded corner transition area. The overall outer surface remains blue, but in areas of high deformation, cracks are observed in the continuous colored masking PP sublayer, exposing the underlying red local warning PP sublayer at the crack location. This creates a clear color contrast between the cracked area and the surrounding blue surface. This phenomenon aligns with the color-based defect detection principle of this invention: when the continuous colored masking PP sublayer remains intact, the red local warning PP sublayer is masked and invisible; when a through-crack, tear, or partial fracture occurs in the rounded corner area during stamping, the red local warning PP sublayer is exposed at the damaged point. This allows for direct visual identification of the molding defect in the rounded corner area, enabling the judgment of the appearance quality of the stamped part.
[0051] Example 2
[0052] The preparation of a soft-pack battery cell aluminum-plastic composite film differs from that in Example 1 in that: In the preparation of the double-layer colorimetric waste detection PP functional film, each sublayer is calculated based on 100 parts of its own PP base material: the continuous colored masking PP sublayer formula consists of 100 parts of PP base material, 5.7 parts of first-color PP masterbatch, and 5.7 parts of titanium dioxide PP masterbatch, without maleic anhydride-grafted PP; the local warning PP sublayer formula consists of 100 parts of PP base material, 10 parts of second-color PP masterbatch, and 6.7 parts of maleic anhydride-grafted PP. The thickness of the continuous colored masking PP film obtained in S1 is 20 μm; the thickness of the red warning PP film obtained in S2 is 4 μm; the strip width of the rounded L-shaped warning strip in S3 is 3 mm, the length of both arms is 10 mm, and the inner corner radius is 3 mm; the hot pressing conditions in S4 are 120℃, 0.2 MPa, and 12 s, and the positioning method and position deviation are the same as in Example 1.
[0053] In the preparation of the aluminum-plastic composite film for soft-pack battery cells, the aluminum foil thickness in S5 is 30 μm, and the dry adhesive coating amount of the first polyurethane adhesive layer is 2.0 g / m³. 2 The thickness of the cast polypropylene film in S6 is 50 μm, and the dry adhesive coating amount of the second polyurethane adhesive layer is 2.0 g / m³. 2 The localized warning PP sublayer is still only set in the four rounded L-shaped warning areas. All other raw materials, process steps, and parameters not mentioned are the same as in Example 1.
[0054] Example 3
[0055] The preparation of a soft-pack battery cell aluminum-plastic composite film differs from that in Example 1 in that: In the preparation of the double-layer color-detecting waste-judgment PP functional film, each sublayer is calculated based on 100 parts of its own PP base material: the continuous colored masking PP sublayer formula consists of 100 parts of PP base material, 10 parts of the first color PP masterbatch, 10 parts of titanium dioxide PP masterbatch, and 2.5 parts of maleic anhydride-grafted PP; the local warning PP sublayer formula consists of 100 parts of PP base material, 30 parts of the second color PP masterbatch, and 15 parts of maleic anhydride-grafted PP. The thickness of the continuous colored masking PP film obtained in S1 is 38 μm; the thickness of the red warning PP film obtained in S2 is 10 μm; the strip width of the rounded L-shaped warning strip in S3 is 8 mm, the length of both arms is 25 mm, and the inner corner radius is 12 mm; the hot-pressing conditions in S4 are 150℃, 0.6 MPa, and 3 s, and the positioning method and position deviation are the same as in Example 1.
[0056] In the preparation of the aluminum-plastic composite film for soft-pack battery cells, the aluminum foil thickness in S5 is 50 μm, and the dry adhesive coating amount of the first polyurethane adhesive layer is 4.5 g / m. 2 The thickness of the cast polypropylene film in S6 is 80 μm, and the dry adhesive coating amount of the second polyurethane adhesive layer is 4.5 g / m³. 2The localized warning PP sublayer is still only set in the four rounded L-shaped warning areas. All other raw materials, process steps, and parameters not mentioned are the same as in Example 1.
[0057] Comparative Example 1 Referring to Example 1, the difference is that maleic anhydride-grafted PP is not added at all in the preparation of the double-layer color-detecting waste PP functional film. Specifically, based on 100 parts of the PP base material of each sublayer, the raw material composition of the continuous colored masking PP sublayer is 100 parts of PP base material, 8 parts of the first color PP masterbatch, and 8 parts of titanium dioxide PP masterbatch, excluding maleic anhydride-grafted PP; the raw material composition of the partial warning PP sublayer is 100 parts of PP base material and 16 parts of the second color PP masterbatch, excluding maleic anhydride-grafted PP. The other raw material types, the thickness and extrusion parameters of the continuous colored masking PP film, the thickness and extrusion parameters of the red warning PP film, the cutting size of the rounded L-shaped warning film, the positioning method, the hot pressing conditions, the adhesive layer coating amount and composite process, the specifications of the cast polypropylene film, and the curing conditions are all exactly the same as in Example 1.
[0058] Comparative Example 2 Referring to Example 1, the difference is that, based on 100 parts of PP base material in the continuous colored masking PP sublayer, the amount of the first color PP masterbatch added is adjusted from 8 parts to 2.7 parts. Correspondingly, the raw material composition of the continuous colored masking PP sublayer is 100 parts of PP base material, 2.7 parts of the first color PP masterbatch, 8 parts of titanium dioxide PP masterbatch, and 1.6 parts of maleic anhydride-grafted PP. The other raw material types, amounts, thickness and extrusion parameters of the continuous colored masking PP film, the complete composition and preparation of the red warning PP film, cutting dimensions, positioning method, hot pressing conditions, adhesive layer coating amount and composite process, cast polypropylene film specifications, curing conditions, etc., are completely the same as in Example 1.
[0059] Comparative Example 3 Referring to Example 1, the difference is that the thickness of the red warning PP film in step S2 is adjusted from 6 μm to 2 μm, and this thickness is achieved by adjusting the extrusion rate and traction speed. Correspondingly, the thickness of the rounded L-shaped warning sheet obtained in step S3 is 2 μm. The remaining raw material composition and dosage, the complete composition and preparation of the continuous colored masking PP film, the cutting size, the positioning method, the hot pressing conditions, the amount of adhesive coating and the composite process, the aluminum foil thickness, the specifications of the cast polypropylene film, and the curing conditions are all exactly the same as in Example 1.
[0060] Comparative Example 4 Referring to Example 1, the only difference is that the hot-pressing temperature in step S4 is adjusted from 135℃ to 100℃. The hot-pressing pressure remains unchanged at 0.4MPa, and the hot-pressing time remains unchanged at 8s. The remaining raw material composition and dosage, the entire preparation process of the double-layer color-developing waste-judgment PP functional film, the cutting size and positioning of the rounded L-shaped warning sheet, the amount of adhesive coating and the composite process, the specifications of the cast polypropylene film, and the curing conditions are all exactly the same as in Example 1.
[0061] Comparative Example 5 Referring to Example 1, the difference is that in step S4, the planar position deviation between the inner rounded corner center of the four rounded L-shaped warning pieces and the corresponding predetermined stamped shell forming rounded corner center is adjusted from no more than 1.5mm to 4.0mm. That is, by manually offsetting the positioning, some of the rounded L-shaped warning pieces are deviated from the high-stress deformation area of the corresponding stamped shell forming rounded corner. The remaining raw material composition and dosage, the preparation and cutting size of each film, the hot pressing temperature and pressure time, the adhesive layer coating amount and composite process, the specifications of the cast polypropylene film, and the curing conditions are all exactly the same as in Example 1.
[0062] Comparative Example 6 Referring to Example 1, the difference is that after the composite process in step S6, the curing treatment described in step S7 is not performed. That is, the resulting composite film roll is placed at room temperature for 48 hours and then used directly as a finished product. The composition and dosage of other raw materials, the entire preparation, cutting and positioning of the double-layer color-developing waste-judgment PP functional film, the amount of adhesive coating and the composite process, and the specifications of the aluminum foil and the cast polypropylene film are all exactly the same as in Example 1.
[0063] Performance testing: In this invention, the performance of the prepared aluminum-plastic composite film for flexible battery cells is evaluated using the following test methods. The samples, instruments, conditions, and evaluation indicators used in each test method are described below.
[0064] 1. Visual Judgment Test for Stamping Shell Forming (1) Sample preparation: Several rectangular samples with a length of 150 mm and a width of 100 mm were cut from the soft-pack battery cell aluminum-plastic composite film roll obtained in the examples or comparative examples. It was ensured that each sample completely included four rounded L-shaped warning areas, and the planar deviation of each warning area relative to the rounded corner position of the punching mold met the predetermined requirements. The samples were placed in an environment with a temperature of 23℃±2℃ and a relative humidity of 50%±5% for no less than 4 hours.
[0065] (2) Instruments and equipment: Stamping mold: The shape and size of the mold cavity are consistent with the predetermined stamping profile corresponding to the aluminum-plastic composite film of the soft-pack battery cell; in the test examples and comparative samples, the mold cavity used is rectangular, with a length of 80mm, a width of 50mm, a radius of 7mm for the four rounded corners of the cavity, and a forming depth of 4.0mm; the matching punch is matched with the cavity. Stamping is carried out on a servo press or hydraulic press, and the stamping speed is adjustable.
[0066] (3) Test conditions: The test environment temperature is 23℃±2℃, and the relative humidity is 50%±5%. The mold is used at room temperature without heating. The stamping speed is controlled within the range of 10mm / s to 30mm / s. At least 3 samples are tested under each condition.
[0067] (4) Test procedure: Place the sample flat on the lower die of the stamping mold, aligning the four rounded L-shaped warning areas with the four rounded corners of the mold cavity. Use the positioning marks on the lower die to control the planar position deviation within the range of 0-1.0 mm. Start the stamping machine and complete the stamping at a constant speed. After forming, hold the pressure for 1 second, demold and remove the stamped part. Under a standard light source box, at least three inspectors with normal vision (or corrected to normal) and who have been trained should independently observe the four rounded corner areas from the side where the double-layer color-coded rejection PP functional components are located. The inspectors will judge based solely on whether red is exposed through the opening of the continuously colored PP sublayer: if no visible red appears in any of the four rounded corner areas, it is judged as "pass"; if any rounded corner area shows dotted, linear, or patchy red, it is judged as "fail". The judgment will be locked and recorded after the judgment. After visual inspection, testers not involved in the visual inspection used an image measuring instrument or stereomicroscope to re-examine each of the four rounded corner areas, checking for through cracks, breaks, or local fractures in the continuous colored PP sublayer. The presence of exposed red was not used as a criterion for determining actual damage during the re-examination. Samples confirmed by this independent re-examination to have the aforementioned outer layer through-defects were defined as "actually damaged samples," thus corroborating the visual inspection results with the actual damage condition.
[0068] (5) Evaluation indicators: The first-pass yield, visual correct identification rate, and number of false positives without breakage are statistically analyzed. The visual correct identification rate is calculated as "the number of samples visually judged as failing and confirmed as actually broken after independent review / the total number of samples confirmed as actually broken after independent review × 100%"; the number of false positives without breakage is the number of samples that were confirmed as not having the above-mentioned penetrating defects after independent review but were visually judged as "failing". At the same time, the specific rounded corner position of the red warning area is recorded to evaluate the correspondence of the local warning PP sublayer positioning.
[0069] 2. Interlayer peel strength test: (1) Sample preparation: For the interfacial peel strength between the continuous colored masking PP sublayer and the local warning PP sublayer, interfacial witness samples were prepared simultaneously when preparing the double-layer color-detecting waste PP functional film of each embodiment or comparative example: Take the continuous colored masking PP film and the red warning PP film with the same formula and thickness as the corresponding group, continuously lay the red warning PP film strip with a width of not less than 25 mm on the continuous colored masking PP film, and perform hot pressing with the same hot pressing temperature, pressure and time as step S4 of the corresponding group. After cooling, cut strip samples with a width of 15 mm and a length of about 150 mm along the overlapping area. For the peel strength between the entire double-layer color-detecting waste PP functional component and the aluminum foil, cut strip samples with a width of 15 mm and a length of about 150 mm from the corresponding final composite film. Take no less than 5 parallel samples for each group, and place the samples at a temperature of 23℃±2℃ and a relative humidity of 50%±5% for no less than 4 h.
[0070] (2) Instruments and equipment: Electronic universal testing machine (the range of the force sensor should be between 15% and 85% of its range, and the accuracy should be better than level 1), peeling fixture, cutting tool.
[0071] (3) Test conditions: Refer to GB / T8808-1988 "Peel Test Method for Flexible Composite Plastic Materials". The test speed is 300 mm / min ± 10 mm / min, and the initial clamping distance is 50 mm. The test ambient temperature is 23℃ ± 2℃.
[0072] (4) Test Procedure: For the peel strength between the continuous colored masking PP sublayer and the local warning PP sublayer, the aforementioned interface witness sample was used. A peel opening of approximately 20 mm was pre-separated from one end of the sample between the two PP film layers. For the peel strength between the entire double-layer color-detecting waste PP functional component and the aluminum foil, a peel opening of approximately 20 mm was pre-separated from the aluminum foil at one end of the final composite film strip sample. Both ends of the peel opening were clamped in the upper and lower clamps of the testing machine, ensuring the peel direction remained as close to 180° as possible. The testing machine was started, and the peel force curve was recorded. The average force value of the relatively stable section in the middle of the curve was taken as the peel strength, and the result was expressed in N / 15 mm.
[0073] (5) Evaluation index: Calculate the average value and standard deviation of the peel strength of each group of samples to evaluate the bonding strength between each layer.
[0074] 3. Electrolyte resistance test: (1) Sample preparation: Cut a 100mm×50mm sample from the aluminum-plastic composite film of the soft-pack battery cell prepared in the example or comparative example, and seal the four sides of the cross-section with heat sealing or paraffin to prevent electrolyte from seeping in from the edges.
[0075] (2) Electrolyte for testing: The electrolyte commonly used in lithium-ion batteries is used: 1 mol / L LiPF6 dissolved in a mixed solvent of ethylene carbonate (EC) and dimethyl carbonate (DMC) in a volume ratio of 1:1, with a water content ≤20 ppm. The electrolyte is prepared and stored in a dry, inert atmosphere glove box.
[0076] (3) Instruments and equipment: inert atmosphere glove box (H2O < 1ppm, O2 < 1ppm), constant temperature drying oven, weighing balance (sensitivity 0.1mg), polytetrafluoroethylene sealed container.
[0077] (4) Test conditions: Test temperature 60℃±2℃, soaking time 72h.
[0078] (5) Test Procedure: Immerse the sample completely in a polytetrafluoroethylene bottle containing electrolyte in a glove box, seal it, and place it in a 60℃ constant temperature drying oven. After 72 hours, remove the sample from the glove box, rinse the surface with clean dimethyl carbonate, and air dry at room temperature in the glove box. Visually inspect each layer of the sample for any abnormalities such as delamination, blistering, or discoloration. At the same time, referring to the aforementioned peel strength test method, test the peel strength between the sample and the double-layer color-developing waste PP functional component and aluminum foil before and after immersion, and calculate the peel strength retention rate.
[0079] (6) Evaluation indicators: Record the changes in appearance and peel strength retention rate of the sample after immersion. The higher the retention rate and the less abnormal the appearance, the better the electrolyte resistance.
[0080] 4. Color contrast test: (1) Sample preparation: Cut a sample containing the complete and continuous colored masking PP sublayer outer surface (blue) from the soft-pack battery cell aluminum-plastic composite film prepared in the examples or comparative examples. At the same time, prepare a reference sample that only exposes the local warning PP sublayer surface (red), or directly obtain the red area exposed after punching.
[0081] (2) Instruments and equipment: colorimeter, standard white board.
[0082] (3) Test conditions: Refer to GB / T3979. The ambient temperature is 23℃±2℃, and the sample is placed against the same black background.
[0083] (4) Test procedure: Use a standard white plate to calibrate the colorimeter, randomly select no less than 5 measurement points on the blue and red areas of the sample respectively, record the L, a, and b values of each point, and calculate the result according to the formula ΔE = [(ΔL)]. 2 +(Δa) 2 +(Δb) 2 ]1 / 2 Calculate the color difference value between the two.
[0084] (5) Evaluation index: The larger the color difference value ΔE, the greater the visual contrast between blue and red, and the easier it is for the naked eye to recognize.
[0085] 5. Positioning accuracy test: (1) Sample preparation: Extract at least 10 samples of the double-layer colorimetric waste PP functional film or final composite film product obtained in step S4, each sample containing four rounded L-shaped warning areas.
[0086] (2) Instruments and equipment; image measuring instrument (measuring accuracy ≤ 0.01 mm) or stereomicroscope with measuring function.
[0087] (3) Test procedure: Lay the sample flat on the measuring table, and take the center of the rounded corner of the predetermined stamping shell forming contour as the reference, measure the planar position deviation between the center of the inner rounded corner of each rounded L-shaped warning area and the corresponding reference. At the same time, check the consistency between the extension direction of the two arms of the rounded L-shaped warning area and the extension direction of the straight segments on both sides of the rounded corner of the stamping shell forming.
[0088] (4) Evaluation indicators: Calculate the average and maximum values of the positional deviation of all test points, evaluate whether the requirement of not exceeding 2.0 mm is met, and check the consistency of the extension direction.
[0089] The performance of the aluminum-plastic composite films for soft-pack battery cells prepared in Examples 1-3 and Comparative Examples 1-6 was tested according to the performance testing methods described above in this specification, and the results are as follows.
[0090] 1. Visual judgment test results of stamping shell forming: The aforementioned visual judgment test method for stamping and forming was used, with 30 samples tested in each group. First, three inspectors independently made a visual judgment of "pass" or "fail" based on the red warning indications and locked in the results. Then, testers who did not participate in the visual judgment independently verified whether there were through cracks, breaks, or local fractures in the continuous colored masking PP sublayer using an image measuring instrument or stereomicroscope, and determined the "actual number of damaged samples" accordingly. The visual correct identification rate was calculated as the proportion of the actual number of damaged samples correctly detected by visual inspection to the total number of actual damaged samples.
[0091]
[0092] Note: In Comparative Example 2, the amount of the first-color PP masterbatch added was insufficient, resulting in a lighter blue color in the continuously colored masking PP sublayer. This reduced the contrast between the exposed red and the blue, leading to the inspector's missed detection. In Comparative Example 3, the thickness of the local warning PP sublayer was too thin, reducing the red saturation and making the exposed red area of some minor breaks difficult to distinguish. In Comparative Example 5, the positioning deviation of the rounded L-shaped warning area exceeded 2.0 mm. Of the five actually damaged samples independently verified, three had damage outside the warning area. Therefore, although the continuously colored masking PP sublayer had penetrating defects, there was no red warning layer below the corresponding location, making identification by red exposure impossible, resulting in a low visual recognition rate. In the other groups, when the actual damage occurred within the warning area, the contrast between red and blue was more obvious, and the inspectors were able to identify it correctly.
[0093] 2. Results of interlayer peel strength test: According to the interlayer peel strength test method described above, the interfacial peel strength between the continuous colored masking PP sublayer and the local warning PP sublayer was tested using the interface witness test sample prepared under the same conditions as step S4 of each group. The peel strength between the entire double-layer color-developing waste PP functional component and the aluminum foil (first polyurethane adhesive layer) was tested using the final composite film sample. The results are all expressed as N / 15mm, and the average value of 5 samples is taken for each group.
[0094]
[0095] Note: In Comparative Example 1, without the addition of maleic anhydride-grafted PP, the peel strength between the continuous colored masking PP sublayer and the local warning PP sublayer was significantly lower. In Comparative Example 4, the hot-pressing temperature was insufficient, resulting in incomplete fusion at the interface and a significant decrease in peel strength. In Comparative Example 6, no curing was performed, leading to incomplete curing of the first polyurethane adhesive layer and a significant reduction in peel strength between the double-layer colored waste-judgment PP functional component and the aluminum foil. Changes in the amount of color masterbatch (Comparative Example 2) and the thickness of the local warning PP sublayer (Comparative Example 3) had no substantial impact on interlayer adhesion.
[0096] 3. Electrolyte resistance test: After soaking in 60℃ electrolyte for 72 hours, the appearance of the sample was checked, and the peel strength between the double-layer color-developing waste PP functional component and the aluminum foil was tested. The peel strength retention rate was calculated, and the average value of the results of 3 samples in each group was taken.
[0097]
[0098] Note: Comparative Example 6 was not cured, resulting in insufficient curing of the polyurethane adhesive layer, significantly reduced resistance to electrolyte erosion, blistering, and a substantial decrease in peel strength. Comparative Example 1, lacking maleic anhydride-grafted PP, showed localized weak interfacial bonding of the PP sublayer, leading to localized delamination after immersion. Examples 1-3 all exhibited good electrolyte resistance.
[0099] 4. Color contrast test: The L, a, and b values of the outer blue region and the inner red region of the composite film were measured using a colorimeter, and the color difference ΔE between them was calculated. The average value of 5 measurement points was taken for each group.
[0100]
[0101] Note: According to the formula given in this manual, ΔE = [(ΔL)] 2 +(Δa) 2 +(Δb) 2 The color difference was recalculated using the 1 / 2 formula, based on the average values of L, a, and b in the table. The ΔE of Comparative Example 2 was 61.3, lower than the 65.1–77.0 of Examples 1–3, indicating that the color contrast decreased after reducing the amount of blue masterbatch, but still maintained a discernible difference. The ΔE of Comparative Example 3 was 55.0, the lowest value among all groups, approximately 23.8% lower than the 72.1 of Example 1. Combined with its local warning that the PP sublayer thickness was only 2 μm and the actual exposed area at the micro-tears was limited, visual identification became more difficult. Except for Comparative Examples 2 and 3, the ΔE of all other groups was not lower than 71.8, indicating a relatively clear blue-red contrast.
[0102] 5. Positioning accuracy test: The planar position deviation between the center of the rounded corner and the corresponding predetermined rounded corner of the blanking shell in each of the samples taken in the examples and comparative examples was tested. The maximum and average deviation values of 10 samples (including 40 rounded corner warning areas) were statistically analyzed.
[0103]
[0104] Note: In Comparative Example 4, due to the low hot-pressing temperature, some rounded L-shaped warning pieces experienced slight slippage during subsequent operations, resulting in a maximum deviation exceeding 2.0 mm. In Comparative Example 5, the positioning deviation was artificially increased, with a maximum deviation reaching 4.2 mm, and the warning area did not correspond to the rounded corner of the stamped shell. The positioning accuracy of all other groups met the requirement of not exceeding 2.0 mm.
[0105] The performance test results show that adding a higher proportion of maleic anhydride-grafted PP to the local warning PP sublayer, based on the PP base material quality of each sublayer, helps to enhance the interfacial adhesion between the continuous colored masking PP sublayer and the local warning PP sublayer, as well as between the PP sublayer and the first polyurethane adhesive layer. This improves the interlayer peel strength and the ability to maintain interlayer integrity after immersion in electrolyte. When maleic anhydride-grafted PP is missing or the hot-pressing temperature is too low, the degree of fusion between PP sublayers weakens, the interfacial peel strength decreases, and local delamination is more likely to occur under the action of electrolyte. The amount of first-color PP masterbatch and titanium dioxide PP masterbatch added to the continuous colored masking PP sublayer affects the blue saturation and hiding power of the sublayer. In Comparative Example 2, after the blue masterbatch was reduced, the ΔE calculated according to the L, a, and b values in the table decreased from 72.1 in Example 1 to 61.3, accompanied by a decrease in the visual correct recognition rate. A thin PP sublayer in localized warnings reduces the effective visibility of the red color at the tear. Comparative Example 3 has a ΔE of 55.0, the lowest among all groups, and a visual correct recognition rate of 66.7%, indicating that color contrast and visible area jointly affect the reliability of defect identification. The positioning accuracy of the rounded L-shaped warning area directly impacts the effectiveness of visual judgment. When the positional deviation between the warning area and the predetermined rounded corner of the punched shell is too large, through-cracks, tears, or localized fractures may occur outside the warning area's coverage. In this case, even if the PP sublayer is continuously masked by color and damaged, the underlying red color cannot be exposed, increasing the risk of missed detection. A stable composite interface can be formed after the polyurethane adhesive layer is prepared with 100 parts of main agent, 10 parts of curing agent, and 173 parts of ethyl acetate and fully cured. Comparative Example 6, without curing, exhibits blistering at the aluminum foil / adhesive layer interface and a significantly reduced peel strength retention rate, indicating that the curing step plays a crucial role in the stability of the adhesive layer interface.
[0106] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A soft-pack battery cell aluminum-plastic composite film whose quality can be directly judged visually during the stamping process, characterized in that, From the outside to the inside, it includes a double-layer color-developing and waste-judging PP functional component, a first polyurethane adhesive layer, an aluminum foil, a second polyurethane adhesive layer, and an inner heat-sealing PP layer. The dual-layer color-detecting waste PP functional component includes a continuous colored masking PP sub-layer on the outer surface and four local warning PP sub-layers disposed on the side of the continuous colored masking PP sub-layer facing the aluminum foil. The four local warning PP sub-layers are respectively disposed at positions corresponding to the four rounded corners of the soft-pack battery cell stamping area, and respectively form rounded L-shaped warning areas consistent with the extension direction of the corresponding rounded corners. The local warning PP sub-layers are different in color from the continuous colored masking PP sub-layers, and the local warning PP sub-layers are sandwiched between the continuous colored masking PP sub-layers and the first polyurethane adhesive layer. The four local warning PP sub-layers are spaced apart from each other and are not interconnected. When the continuous colored masking PP sub-layers are intact, they cover the local warning PP sub-layers. The local warning PP sub-layers are not directly exposed on the outer surface of the soft-pack battery cell aluminum-plastic composite film. Based on 100 parts of PP base material in the continuous colored masking PP sublayer, the continuous colored masking PP sublayer contains 100 parts of PP base material, 5-10 parts of first color PP masterbatch, 5-10 parts of titanium dioxide PP masterbatch, and 0-3 parts of maleic anhydride grafted PP. Based on 100 parts of PP base material in the local warning PP sublayer, the local warning PP sublayer contains 100 parts of PP base material, 10-30 parts of second color PP masterbatch, and 6-15 parts of maleic anhydride grafted PP. The continuous colored masking PP sublayer and the local warning PP sublayer are each measured independently according to their respective PP base material mass. The actual amount of the local warning PP sublayer in the final composite film is determined by the area of the rounded L-shaped warning area and the thickness of the local warning PP sublayer. Both the first color PP masterbatch and the second color PP masterbatch are colored masterbatches with PP as the carrier, and the two have different colors and can form a color contrast that can be recognized by the naked eye.
2. The aluminum-plastic composite film for soft-pack battery cells according to claim 1, which is easy to visually judge whether it is qualified or not during the stamping process, wherein the thickness of the continuous colored masking PP sub-layer is 20-38 μm, and the thickness of the local warning PP sub-layer is 4-10 μm.
3. The soft-pack battery cell aluminum-plastic composite film according to claim 1, which is easy to visually judge whether it is qualified or not during the stamping process, wherein the strip width of each of the rounded L-shaped warning areas is 3-8mm, the length of the two arms is 10-25mm respectively, and the inner rounded corner radius is 3-12mm.
4. The soft-pack battery cell aluminum-plastic composite film according to claim 1, which is easy to visually judge whether it is qualified or not during the stamping process, wherein the maleic anhydride grafting rate of the maleic anhydride grafted PP is 0.6 to 1.5 wt%.
5. The aluminum-plastic composite film for soft-pack battery cells according to claim 1, which is easy to visually judge whether it is qualified or not during the stamping process, wherein the thickness of the aluminum foil is 30-50 μm, and the inner heat-sealing PP layer is a cast polypropylene film with a thickness of 50-80 μm.
6. The soft-pack battery cell aluminum-plastic composite film according to claim 1, which allows for direct visual judgment of its quality during the stamping process, wherein the first polyurethane adhesive layer and the second polyurethane adhesive layer are respectively formed by drying and curing a two-component polyurethane composite adhesive; by weight, the two-component polyurethane composite adhesive comprises 100 parts of polyurethane main agent, 10 parts of curing agent, and 173 parts of ethyl acetate, wherein the solid content of the polyurethane main agent is 75 wt%; the dry adhesive coating amount of the first polyurethane adhesive layer is 2.0–4.5 g / m³. 2 The dry adhesive coating amount of the second polyurethane adhesive layer is 2.0–4.5 g / m². 2 .
7. The soft-pack battery cell aluminum-plastic composite film according to claim 1, which is easy to visually judge whether it is qualified or not during the stamping process, wherein the four rounded L-shaped warning areas are respectively set in the corresponding areas on the outside of the four rounded corners of the predetermined stamping outline, and the planar position deviation between the inner rounded corner center of each rounded L-shaped warning area and the corresponding predetermined stamping rounded corner center is not greater than 2.0mm.
8. The soft-pack battery cell aluminum-plastic composite film according to claim 1, which is easy to visually judge whether it is qualified or not during the stamping process, wherein, based on 100 parts of PP base material in each sub-layer, the amount of first color PP masterbatch added in the continuous colored masking PP sub-layer is 6-10 parts, the amount of titanium dioxide PP masterbatch added is 6-10 parts, and the amount of second color PP masterbatch added in the local warning PP sub-layer is 12-28 parts.
9. A method for preparing a soft-pack battery cell aluminum-plastic composite film as described in any one of claims 1 to 8, which is easily visually judged for its quality during the stamping process, characterized in that, Includes the following steps: S1. Taking 100 parts of PP base material in the continuous colored masking PP sublayer as 100 parts, mix 100 parts of PP base material, 5-10 parts of first color PP masterbatch, 5-10 parts of titanium dioxide PP masterbatch and 0-3 parts of maleic anhydride grafted PP, melt extrude at 180-215℃ and cool to form a film to obtain a continuous colored masking PP film with a thickness of 20-38μm. S2. Taking 100 parts of PP base material in the local warning PP sublayer as 100 parts, mix 100 parts of PP base material, 10-30 parts of second color PP masterbatch and 6-15 parts of maleic anhydride grafted PP, melt extrude at 180-215℃ and cool to form a film to obtain a red warning PP film with a thickness of 4-10 μm. S3. Cut the red warning PP film into four rounded L-shaped warning pieces. The strip width of each rounded L-shaped warning piece is 3-8mm, the length of each arm is 10-25mm, and the inner rounded corner radius is 3-12mm. S4. Determine the positions of the four rounded corners of the punched shell according to the predetermined punched shell forming contour, and position the four rounded L-shaped warning pieces on the side of the continuous colored masking PP film facing the aluminum foil, so that each rounded L-shaped warning piece corresponds to the position of the corresponding punched shell forming rounded corner, and the positional deviation between the center of the inner rounded corner of each rounded L-shaped warning piece and the center of the corresponding predetermined punched shell forming rounded corner is controlled within 0 to 2.0 mm. Hot press for 3 to 12 seconds at 120 to 150°C and 0.2 to 0.6 MPa to fix the rounded L-shaped warning pieces to the continuous colored masking PP film, and obtain a double-layer color-developing waste judgment PP functional film; S5. Prepare a two-component polyurethane composite adhesive by mixing 100 parts by weight of polyurethane main agent, 10 parts by weight of curing agent and 173 parts by weight of ethyl acetate, wherein the solid content of the polyurethane main agent is 75 wt%; apply the two-component polyurethane composite adhesive to one side of the double-layer color-developing waste-judging PP functional membrane with the rounded L-shaped warning sheet, controlling the dry adhesive coating amount to be 2.0-4.5 g / m³. 2 The first composite film was obtained by combining it with an aluminum foil with a thickness of 30-50 μm under conditions of 55-85℃ and 0.20-0.50 MPa. S6. Coat the side of the aluminum foil opposite to the double-layer color-developing and waste-judging PP functional film with a two-component polyurethane composite adhesive with the same formulation as in step S5, controlling the dry adhesive coating amount to be 2.0–4.5 g / m³. 2 It is composited with a cast polypropylene film with a thickness of 50-80 μm under conditions of 55-85℃ and 0.20-0.50MPa. S7. The composite film obtained in step S6 is aged at 40-60°C for 24-72 hours to obtain the soft-pack battery cell aluminum-plastic composite film that can be directly visually judged as qualified or not in the stamping process.
10. A method for visually judging the quality of punching and forming of soft-pack battery cells using the aluminum-plastic composite film of any one of claims 1 to 8, which is easily visually judged for its pass / fail status during the punching and forming process, characterized in that, The aluminum-plastic composite film of the soft-pack battery cell is positioned according to the predetermined stamping outline, so that the four local warning PP sub-layers correspond to the four rounded corner positions of the stamping area. After the stamping is completed, the four rounded corner areas are observed from the side where the double-layer color-coded waste PP functional components are located. If the color of the local warning PP sub-layer exposed by the opening of the continuous colored masking PP sub-layer appears in any of the four rounded corner areas, the stamped part is determined to pass the appearance judgment. If the color of the local warning PP sub-layer exposed by the through crack, tear or partial break of the continuous colored masking PP sub-layer appears in any rounded corner area, the stamped part is determined to fail the appearance judgment.