Batteries, battery packs, battery modules and electrical devices

By adjusting the welding direction and distance, the problem of insulation film warping between the battery casing and the cover plate was solved, improving the battery's insulation and welding strength, and ensuring the battery's safety and reliability.

CN123121024APending Publication Date: 2026-11-17CALB GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611149948.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, the insulating film of the battery casing and cover is prone to warping, which can lead to insulation failure and affect the safety of battery use.

Method used

By adjusting the welding direction, the angle between the weld line's penetration direction and the cover plate is set to 0°-10°. The relationship between the distance D mm between the deepest point of the weld line and the surface of the cover plate and the width L mm of the insulating film flange structure is controlled to satisfy 0.66≤D×L≤9.08, ensuring the reliability of the connection between the insulating film and the cover plate.

Benefits of technology

The insulation and welding strength of the battery casing have been improved, avoiding the risk of cracking at the weld and ensuring the safety and reliability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123121024A_ABST
    Figure CN123121024A_ABST
Patent Text Reader

Abstract

This application provides a battery, battery pack, battery assembly, and power device, relating to the field of battery technology. The battery includes a cell, a casing assembly, and an insulating film. The casing assembly includes a housing and a cover plate. The housing includes a first side surface surrounding an opening. The cover plate covers the opening and is welded to the opening to form a weld line. The cover plate has a first surface facing away from the housing. The angle between the weld line's penetration direction and the first surface is 0°–10°. At least a portion of the weld line protrudes from the casing assembly to form a raised area. Along a direction perpendicular to the first surface, the distance between the deepest point of the weld line and the first surface is D mm. The insulating film covers at least a portion of the first side surface of the housing and extends to the first surface of the cover plate to form a flanged structure. The insulating film covers at least a portion of the raised area. The width of the flanged structure is L mm, satisfying: 0.66 ≤ D × L ≤ 9.08. This makes the flanged structure less prone to warping and improves the welding strength between the housing and the cover plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and in particular to a battery, battery pack, battery module, and electrical device. Background Technology

[0002] In related technologies, to ensure insulation between two adjacent battery casings, an insulating film needs to be covered on the surface of the battery casing. The insulating film typically extends to the surface of the battery cover and forms a flange. However, during battery production and use, it has been found that the flange extending to the battery cover surface can warp or even detach from the cover surface, causing insulation failure in the battery casing and affecting battery safety. Summary of the Invention

[0003] The purpose of this application is to provide a battery, battery pack, battery module, and power supply device to solve the technical problem that the insulating film in batteries in the prior art is prone to warping.

[0004] To achieve the above objectives, the technical solution adopted in this application is as follows: In a first aspect, this application provides a battery, comprising: a battery cell, a casing assembly, and an insulating film. The battery cell is disposed within the casing assembly, which includes a housing and a cover plate. At least one side of the housing has an opening. The housing includes a first side surface surrounding the opening. The cover plate covers the opening and is welded to the opening to form a weld line. The cover plate has a first surface facing away from the housing. The angle between the weld line's melting depth direction and the first surface is 0°-10°. At least a portion of the weld line protrudes from the casing assembly, forming a raised area. The distance between the deepest melting point of the weld line and the first surface is D mm along a direction perpendicular to the first surface. The insulating film covers at least a portion of the first side surface of the housing and extends to the first surface of the cover plate, forming a flanged structure. The insulating film covers at least a portion of the raised area. The width of the flanged structure is L mm, satisfying: 0.66 ≤ D × L ≤ 9.08.

[0005] The above technical solution has at least the following beneficial technical effects: In the battery provided in this application embodiment, the casing and cover plate are welded along a direction approximately perpendicular to the first side of the casing, i.e., the angle between the weld line's penetration direction and the first surface of the cover plate is 0°-10°. In this case, the raised area of ​​the weld line protrudes more from the first side of the casing, preventing the weld pool from protruding excessively from the first surface of the cover plate. This reduces the impact of the weld line's protrusion on the bonding strength between the insulating film's flange structure and the first surface of the cover plate, ensuring reliable connection between the insulating film and the cover plate. Further adjustments are made to the distance D mm between the deepest point of the weld line and the first surface of the cover plate, and the width L mm of the flange structure formed by the insulating film on the first surface of the cover plate, satisfying: 0.66 ≤ D × L ≤ 9.08. When D × L is less than 0.66, the weld line's protrusion on the first surface of the cover plate is excessive, the flange structure of the insulating film is too narrow, increasing the risk of the insulating film warping and thus increasing the risk of localized insulation failure in the battery. When D×L is greater than 9.08, the strength of the weld between the cover plate and the shell is insufficient, resulting in poor welding performance and a high risk of cracking at the connection. Therefore, D and L need to be considered comprehensively, limiting D×L to the range of 0.66~9.08. This prevents the flange structure of the insulating film on the cover plate from warping, ensuring the insulation of the battery shell, while simultaneously improving the welding strength and effect between the shell and the cover plate. This avoids the problem of excessive risk of cracking at the weld line due to insufficient weld strength between the shell and the cover plate.

[0006] Secondly, this application provides a battery pack including at least one battery as described in the first aspect.

[0007] The above technical solution has at least the following beneficial technical effects: The battery pack provided in this application embodiment can improve the insulation between batteries in the entire battery pack and improve the safety of the battery pack by setting at least one battery of the first aspect.

[0008] Thirdly, this application provides a battery pack including the battery pack described in the second aspect.

[0009] Fourthly, this application provides an electrical device including the battery pack described in the third aspect. Attached Figure Description

[0010] To more clearly illustrate the technical solutions in the embodiments of this application, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0011] Figure 1 This is a three-dimensional structural diagram of the battery provided in the embodiments of this application.

[0012] Figure 2 This is a schematic diagram of the exploded decomposition structure of the battery provided in the embodiment of this application.

[0013] Figure 3 This is a three-dimensional structural diagram of a battery with the insulating sheet omitted, provided in an embodiment of this application.

[0014] Figure 4 This is a top view of the battery structure provided in the embodiment of this application, omitting the insulating sheet.

[0015] Figure 5 This is a top view of a battery structure with the insulating sheet omitted, provided in another embodiment of this application.

[0016] Figure 6 This is a schematic diagram of a partial cross-sectional structure of the battery provided in an embodiment of this application.

[0017] Figure 7 This is a schematic diagram of the welded joint structure of the battery casing and cover plate provided in the embodiments of this application.

[0018] Figure 8 This is a three-dimensional structural diagram of a battery with the insulating sheet omitted, provided in another embodiment of this application.

[0019] Figure 9 This is a three-dimensional structural diagram of a battery with an insulating sheet omitted, provided in another embodiment of this application.

[0020] Figure 10 This is a side view of the battery provided in an embodiment of this application.

[0021] In the diagram: 10-insulating sheet; 20-cover plate; 30-shell; 40-insulating film; 50-welding wire; 60-cell; 70-terminal post; 201-first surface; 202-first side; 203-second side; 204-second surface; 300-shell body; 301-opening; 302-first side; 303-reinforcing protrusion; 3021-first sub-side; 3022-second sub-side; 401-flanged structure; 4011-first flanged structure; 4012-second flanged structure; 402-overlapping area; 403-hollowed-out part; 501-protruding area; 502-first end; 503-second end; 5011-first protrusion; 5012-second protrusion. Detailed Implementation

[0022] To make the technical problems, technical solutions, and beneficial effects to be solved by this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and are not intended to limit the scope of this application.

[0023] It should be noted that when a component is referred to as being "fixed to" or "set on" another component, it can be directly on or indirectly on that other component. When a component is referred to as being "connected to" another component, it can be directly connected to or indirectly connected to that other component.

[0024] It should be understood that the terms "length", "width", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.

[0025] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.

[0026] Research has found that when the battery casing and cover are welded together, the weld lines formed at the weld joints protrude from the surface of the casing and / or the cover. When the insulating film covers the weld line area, its thickness and stiffness cause uneven adhesion between the film and the protruding weld line, weakening the bond strength. Furthermore, the flanged structure of the insulating film covering the cover surface is typically narrow, and the weld line protrusion is close to this flanged structure, making the flanged area more prone to detaching from the cover surface and warping. This can lead to localized insulation failure in the battery casing.

[0027] Based on the above considerations, in order to solve the technical problem that the insulating film in existing batteries is prone to warping, this application provides a battery, a battery pack, a battery module, and an electrical device. In the battery, because the flanged structure of the insulating film covers the first surface of the cover plate, the width of the flanged structure is relatively small, and the adhesion width with the first surface of the cover plate is also small. Moreover, the starting point of the flanged structure is the junction between the cover plate and the shell, where the insulating film will bend. Therefore, after the flanged structure covers the first surface of the cover plate, it tends to return to its straightness. The flanged structure itself is more prone to warping. If more weld line protrusions are formed on the first surface of the cover plate, this will further exacerbate the tendency of the flanged structure to warp. Therefore, in the battery of this application embodiment, by welding the shell and the cover plate in a direction approximately perpendicular to the first side of the shell, that is, the angle between the weld line penetration direction and the first surface of the cover plate is 0°-10°, the weld line protrusion area will protrude more from the first side of the shell. This avoids excessive protrusion of the weld pool from the first surface of the cover plate, thus making the adhesion strength between the flange structure of the insulating film and the first surface of the cover plate less affected by the weld line protrusion area, ensuring the reliability of the connection between the insulating film and the cover plate. Further adjusting the relationship between the distance D mm between the deepest point of the weld line and the first surface of the cover plate and the width L mm of the flange structure formed by the insulating film on the first surface of the cover plate satisfies: 0.66≤D×L≤9.08. This makes the flange structure of the insulating film on the cover plate less prone to warping, ensuring the insulation of the battery shell, while improving the welding strength and welding effect between the shell and the cover plate, avoiding the problem of insufficient weld line strength leading to excessive risk of cracking at the weld line.

[0028] The battery described in this application is applicable to electrical devices that use batteries as a power source. The electrical devices disclosed in the embodiments of this application can be vehicles, mobile phones, portable devices, laptops, ships, spacecraft, electric toys, power tools, energy storage devices, amusement equipment, elevators, and lifting equipment, etc. Electric toys include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, or electric airplane toys, etc.; power tools include metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers, etc.; energy storage devices can be energy storage walls, base station energy storage, container energy storage, etc.; amusement equipment can be carousels, drop towers, etc.

[0029] This application describes an electrical device using a vehicle as an example. The vehicle can be a gasoline-powered vehicle, a natural gas-powered vehicle, or a new energy vehicle. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A battery is installed inside the vehicle, and the battery can be located at the bottom, front, or rear of the vehicle. The battery can be used to power the vehicle; for example, it can serve as the vehicle's operating power source. The vehicle may also include a controller and a motor. The controller controls the battery to supply power to the motor, for example, to meet the power needs of starting, navigation, and driving the vehicle. The battery can not only serve as the vehicle's operating power source but also as its driving power source, replacing or partially replacing gasoline or natural gas to provide driving power to the vehicle.

[0030] In one embodiment of this application, the battery pack includes a battery management system (BMS), a thermal management system, an electrical connection system (high-voltage / low-voltage connectors, wiring harnesses, etc.), structural components (shell, brackets, etc.), and protective components, etc., and the above components are placed in a box and sealed with a cover plate to form a complete functional unit that can directly output electrical energy.

[0031] This application provides a battery pack in which multiple batteries of similar capacity and internal resistance are connected in series or parallel. The battery can store chemical energy and controllably convert it into electrical energy. In recyclable batteries, the active materials can be activated by charging after discharge for continued use. The battery includes a casing assembly and battery cells 60 disposed within the casing assembly. There can be one or more battery cells 60. The battery cell 60 is the component in the battery where electrochemical reactions occur; it is the smallest unit in the battery capable of electrochemical reactions such as charging / discharging. The battery cell 60 is the basic unit in the battery. The battery cell can be a wound core or a stacked core. The battery cell 60 typically includes a positive electrode, a negative electrode, and a separator. Lithium-ion battery cells mainly rely on the insertion and extraction of lithium ions between the positive and negative electrode plates to operate. Among them, a cylindrical cell is an electrode assembly in which three layers of materials, namely a positive electrode, a negative electrode, and a separator, are wound into a cylindrical shape, while a cuboid cell is an electrode assembly in which the positive electrode, a negative electrode, and a separator are wound or stacked into a roughly cuboid shape. The technical solution of this application will be described in detail below with reference to the accompanying drawings.

[0032] Please refer to Figure 1 and Figure 2This application provides a battery, including a battery cell 60 and a casing assembly. The battery cell 60 is disposed within the casing assembly, which includes a housing 30 and a cover plate 20. The housing 30 is a component that provides a receiving space to house the battery cell 60 and other components, isolating them from the outside environment. At least one side of the housing 30 has an opening 301, which can be closed by the cover plate 20 to seal and isolate the internal environment of the battery from the external environment. The material of the housing 30 can be various, including but not limited to copper, iron, aluminum, stainless steel, aluminum alloy, titanium alloy, etc., and this application does not impose any special limitations on this. The cover plate 20 is a component that covers the opening 301 of the housing 30 to isolate the internal environment of the battery from the external environment. The shape of the cover plate 20 can be adapted to the shape of the housing 30 to fit the housing 30. In some embodiments, the cover plate 20 may be made of a material with a certain hardness and strength (such as aluminum alloy), so that the cover plate 20 is not easily deformed when subjected to compression and impact, enabling the battery to have higher structural strength and improving safety performance. The material of the cover plate 20 may also be various, including but not limited to copper, iron, aluminum, stainless steel, aluminum alloy, titanium alloy, etc., and this application embodiment does not impose any special limitations on this.

[0033] Please refer to Figure 2The housing 30 includes a first side surface 302 surrounding the opening 301. The first side surface 302 can be understood as the outer peripheral surface of the housing 30 located circumferentially around the opening 301 and facing away from the interior of the housing 30, i.e., the four sides of the housing 30 adjacent to the cover plate 20. The cover plate 20 covers the opening 301 and is welded to the opening 301 to form a weld line 50. The weld line 50 can be a connection structure that fixes and seals the cover plate 20 and the opening 301 of the housing 30 through a welding process. In some embodiments, the weld line 50 can be a continuous weld formed by laser welding or the like. The material of the weld line 50 is usually a fusion of the base materials of the cover plate 20 and the housing 30. The cross-sectional shape of the weld line 50 can be any regular or irregular shape. The cover plate 20 has a first surface 201 facing away from the housing 30. The first surface 201 can be understood as the outer surface of the cover plate 20 facing away from the interior of the housing 30 and towards the external environment of the battery. In this embodiment, the angle between the penetration direction of the welding wire 50 and the first surface 201 is 0°-10°. The penetration direction of the welding wire 50 can be understood as the penetration direction of the high-energy beam (e.g., a laser beam) during welding. Therefore, the angle between the penetration direction of the welding wire 50 and the first surface 201 is 0°-10°, which can be understood as follows: In some embodiments, the angle between the penetration direction of the welding wire 50 and the first surface 201 can be 0°, in which case the penetration direction of the welding wire 50 is parallel to the first surface 201. Of course, in other embodiments, the angle between the penetration direction of the welding wire 50 and the first surface 201 can also be greater than 0° and less than or equal to 10°, that is, there is an angle less than or equal to 10° between the penetration direction of the high-energy beam during welding and the first surface 201 of the cover plate 20. In this embodiment, the connection surface of the opening 301 of the cover plate 20 and the housing 30 is parallel to the first surface 201 of the cover plate 20, such as... Figure 6 As shown.

[0034] Please refer to Figure 7 At least a portion of the weld wire 50 protrudes from the housing assembly, forming a raised area 501. The raised area 501 refers to the raised region formed on the surface of the housing assembly after the weld pool solidifies during welding. The distance between the deepest point of the weld wire 50 and the first surface 201 along a direction perpendicular to the first surface 201 is D mm. The deepest point of the weld wire 50 refers to the point on a cross-section perpendicular to the first surface 201 where the boundary of the weld pool is furthest from the first side surface 302 of the housing 30 along the weld depth direction.

[0035] An insulating film 40, having a certain thickness and stiffness, is used to cover the outer surface of the battery casing assembly to improve the insulation performance of the battery's outer surface. The insulating film 40 covers at least a portion of the first side 302 of the housing 30 and extends to the first surface 201 of the cover plate 20, forming a flange structure 401. The flange structure 401 can be understood as the portion of the insulating film 40 that bends from the connection between the housing 30 and the cover plate 20 and extends to the first surface 201 of the cover plate 20 for adhesive fixation. The insulating film 40 covers at least a portion of the raised area 501, and the width of the flange structure 401 is L mm. Figure 4 , Figure 5 and Figure 6 As shown. It can be understood that the width of the flange structure 401 refers to the width dimension of the insulating film 40 covering the first surface 201 in the direction from the edge of the cover plate 20 to the center of the cover plate 20, and among all flange structures 401, the minimum width dimension is taken as the width of the flange structure 401.

[0036] The relationship between the distance D mm between the deepest penetration point of the weld wire 50 and the first surface 201 of the cover plate 20 and the width L mm of the flange structure 401 formed by the insulating film 40 on the first surface 201 of the cover plate 20 satisfies: 0.66 ≤ D × L ≤ 9.08. For example, D × L can be 0.66, 0.82, 1.48, 2.17, 2.72, 3.14, 4.03, 4.75, 5.76, 6.76, 7.70, 8.80, 9.08, etc., or any value between any two adjacent values ​​mentioned above.

[0037] In the battery provided in this application embodiment, since the flanged structure 401 of the insulating film 40 covers the first surface 201 of the cover plate 20, the width of the flanged structure 401 is relatively small, and the bonding width with the first surface 201 of the cover plate 20 is also small. Moreover, the starting point of the flanged structure 401 is the junction of the cover plate 20 and the shell 30, where the insulating film 40 will bend. Therefore, after the flanged structure 401 covers the first surface 201 of the cover plate 20, it tends to return to a straight position. The flanged structure 401 itself is more prone to warping. If more molten pool protrusions are formed on the first surface 201 of the cover plate 20, this will further exacerbate the tendency of the flanged structure 201 to warp. Therefore, this application welds the housing 30 and the cover plate 20 along a direction approximately perpendicular to the first side 302 of the housing 30, that is, the angle between the weld line 50 and the first surface 201 is 0°-10°. At this time, the weld line protrusion area will protrude more from the first side 301 of the housing 30, which can avoid the weld pool protruding too much from the first surface 201 of the cover plate 20. This makes the bonding strength between the flange structure 401 and the first surface 201 of the cover plate 20 less affected by the weld line protrusion area, and ensures the reliability of the connection between the insulating film 40 and the cover plate 20.

[0038] During the welding process, the deepest point of the weld line 50 can be used as the starting point of the molten pool. The distance D mm between the deepest point of the weld line 50 and the first surface 201 of the cover plate 20 can be used as the distance between the laser focus point and the first surface 201 of the cover plate 20 during laser welding. When the value of D is smaller, that is, along the direction perpendicular to the first surface 201, the distance between the deepest point of the weld line 50 and the first surface 201 is smaller. Then, the area of ​​the protrusion 501 of the weld pool protruding from the first surface 201 is larger, resulting in a more uneven adhesion of the flange structure 401 of the insulating film 40 at the protrusion 501. The bonding strength of the flange structure 401 of the insulating film 40 is weakened, and the risk of the flange structure 401 lifting is greater, which increases the risk of local insulation failure of the battery. When the D value is larger, that is, along the direction perpendicular to the first surface 201, the distance between the deepest point of the weld line 50 and the first surface 201 is larger. This leads to a reduction in the welding area of ​​the cover plate 20, a poorer welding effect between the cover plate 20 and the housing 30, and a higher likelihood of cracking at the weld joint. When the L value is larger, that is, the width of the flange structure 401 of the insulating film 40 is larger. The flange structure 401 is more likely to interfere with other functional components (such as terminals) on the cover plate 20, affecting the installation of other functional components. When the L value is smaller, that is, the width of the flange structure 401 of the insulating film 40 is smaller. This increases the risk of the flange structure 401 warping at the protrusion area 501, leading to an increased risk of local insulation failure of the battery. The values ​​D and L can be comprehensively adjusted. When D is small, the risk of warping of the insulating film 40 is high. In this case, the value L can be adjusted to be slightly larger, resulting in a wider flange structure 401 formed by the insulating film 40 on the first surface 201 of the cover plate 20. This increases the bonding area and strength between the flange structure 401 and the first surface 201 of the cover plate 20, making the insulating film 40 less prone to warping. When D is large, the risk of warping of the insulating film 40 is relatively reduced. In this case, the value L can be adjusted to be slightly smaller, avoiding interference between the flange structure 401 and other functional components on the cover plate 20. Further adjustment of the relationship between the distance D mm between the deepest weld point of the bonding wire 50 and the first surface 201 of the cover plate 20 and the width L mm of the flange structure 401 formed by the insulating film 40 on the first surface 201 of the cover plate 20 satisfies: 0.66 ≤ D × L ≤ 9.08. When D×L is less than 0.66, the raised area 501 of the welding line 50 protrudes excessively from the first surface 201 of the cover plate 20, and the width of the flange structure 401 of the insulating film 40 is too small, increasing the risk of the insulating film 40 warping and thus increasing the risk of local insulation failure of the battery. When D×L is greater than 9.08, the strength of the weld between the cover plate 20 and the shell 30 is insufficient, the welding effect between the cover plate 20 and the shell 30 is poor, and the connection between the cover plate 20 and the shell 30 is prone to cracking.Therefore, D and L need to be considered comprehensively, and D×L should be limited to the range of 0.66~9.08. This makes it less likely for the flange structure 401 of the insulating film 40 on the cover plate 20 to warp, ensuring the insulation of the battery casing 30. At the same time, it improves the welding strength and welding effect between the casing 30 and the cover plate 20, avoiding the problem of excessive risk of cracking at the weld line due to insufficient weld line strength between the casing 30 and the cover plate 20.

[0039] In some embodiments, to further reduce the risk of the insulating film 40 warping and to further improve the strength of the bonding wire 50 and the welding effect between the cover plate 20 and the housing 30, the following condition is further defined: 2.17 ≤ D×L ≤ 7.70. For example, D×L can be 2.17, 2.72, 3.14, 4.03, 4.75, 5.76, 6.76, 7.70, etc., or any value between any two adjacent values ​​mentioned above. By limiting D×L to the range of 2.17 to 7.7, the flange structure 401 of the insulating film 40 on the cover plate 20 is less prone to warping, ensuring the insulation of the battery housing 30, and further improving the welding strength and welding effect between the housing 30 and the cover plate 20. When D×L is less than 2.17, the risk of the insulating film 40 warping increases, leading to an increased risk of local insulation failure in the battery. When D×L is greater than 7.7, the welding effect between the cover plate 20 and the shell 30 is relatively poor, which makes the connection between the cover plate 20 and the shell 30 prone to cracking.

[0040] In some embodiments, the distance between the deepest penetration point of the weld wire 50 and the first surface 201 of the cover plate 20 satisfies: 0.30 mm ≤ D mm ≤ 1.21 mm; for example, D mm can be 0.30 mm, 0.41 mm, 0.53 mm, 0.62 mm, 0.68 mm, 0.73 mm, 0.84 mm, 0.88 mm, 0.96 mm, 1.04 mm, 1.07 mm, 1.10 mm, 1.21 mm, etc., or any value between any two adjacent values ​​mentioned above. By limiting the distance between the deepest point of the weld line 50 and the first surface 201 of the cover plate 20 to within the range of 0.30 mm to 1.21 mm, the flange structure 401 of the insulating film 40 on the cover plate 20 is less prone to warping, ensuring the insulation of the battery casing 30. Simultaneously, it improves the welding strength and effect between the casing 30 and the cover plate 20, avoiding the problem of excessive risk of cracking at the weld line due to insufficient weld line strength between the casing 30 and the cover plate 20. When D mm is less than 0.30 mm, that is, along the direction perpendicular to the first surface 201, the distance between the deepest point of the weld line 50 and the first surface 201 is too small. This results in an excessively large area of ​​the weld pool protruding from the first surface 201, causing the flange structure 401 of the insulating film 40 to adhere more unevenly at the protrusion area 501. The adhesive strength of the flange structure 401 of the insulating film 40 weakens, increasing the risk of warping and thus increasing the risk of localized insulation failure in the battery. When D mm is greater than 1.21 mm, that is, along the direction perpendicular to the first surface 201, the greater the distance between the deepest melting point of the weld line 50 and the first surface 201, the smaller the welding area of ​​the cover plate 20 will be, the poorer the welding effect between the cover plate 20 and the shell 30 will be, and cracks will easily occur at the weld between the cover plate 20 and the shell 30.

[0041] In some embodiments, the width of the flange structure 401 satisfies the following condition: 2.0 mm ≤ L mm ≤ 8.0 mm. For example, L mm can be 2.0 mm, 2.2 mm, 2.8 mm, 3.5 mm, 4.0 mm, 4.3 mm, 4.8 mm, 5.0 mm, 5.4 mm, 6.0 mm, 6.5 mm, 7.2 mm, 7.5 mm, 8.0 mm, etc., or any value between any two adjacent values ​​mentioned above. By limiting the width of the flange structure 401 to the range of 2.0 mm to 8.0 mm, the flange structure 401 on the cover plate 20 is less prone to warping, ensuring the insulation of the battery casing 30, while preventing the flange structure 401 from interfering with other functional components on the cover plate 20 and affecting the installation of other functional components. When L mm is less than 2.0 mm, the width of the flange structure 401 of the insulating film 40 is too small, which increases the risk of the flange structure 401 warping at the raised area 501, thus increasing the risk of local insulation failure of the battery. When L mm is greater than 8.0 mm, the width of the flange structure 401 of the insulating film 40 is too large, and the flange structure 401 is prone to interfering with other functional components (such as terminals) on the cover plate 20, affecting the installation of other functional components.

[0042] In some embodiments, the flange structure 401 covers at least a portion of the raised area 501 of the weld line 50. That is, on a plane parallel to the first surface 201, the orthographic projection of the raised area 501 at least partially overlaps with the orthographic projection of the flange structure 401. Thus, the flange structure 401 is more prone to uneven adhesion at the raised area 501, leading to weakened bond strength. Therefore, in this embodiment, to further improve the bond strength of the flange structure 401, please refer to... Figure 7The minimum length by which the edge of the flange structure 401 extends beyond the raised area 501 is controlled to be L1 mm, satisfying the condition: 1 mm ≤ L1 mm ≤ 7.9 mm. For example, L1 mm can be 1 mm, 1.6 mm, 2.2 mm, 2.8 mm, 3.1 mm, 3.6 mm, 3.9 mm, 4.8 mm, 5.6 mm, 6.4 mm, 7.2 mm, 7.9 mm, etc., or any value between any two adjacent values ​​mentioned above. It can be understood that the minimum length by which the edge of the flange structure 401 extends beyond the raised area 501 is the minimum distance between the edge of the flange structure 401 and the raised area 501. This increases the bonding strength of the flange structure 401 in the raised area 501, reduces the risk of the flange structure 401 warping, and avoids interference between the flange structure 401 and other functional components on the cover plate 20, thus preventing them from being installed. When L1 mm is less than 1 mm, the edge of the flange structure 401 extends too little beyond the minimum length of the raised area 501, resulting in uneven adhesion of the flange structure 401 at the raised area 501. This weakens the bonding strength and increases the risk of the flange structure 401 lifting off the edge, thereby increasing the risk of local insulation failure of the battery. When L1 mm is greater than 7.9 mm, the edge of the flange structure 401 extends too much beyond the minimum length of the raised area 501. The flange structure 401 is prone to interfering with other functional components (such as terminals) on the cover plate 20, affecting the installation of other functional components.

[0043] In some embodiments, please refer to Figure 4The cover plate 20 is provided with terminals 70, which are used to electrically connect the battery cell 60 located inside the housing 30 and the device (adjacent battery or other electrical equipment) located outside the housing 30. The battery can discharge to the external device through the output terminal (tab) of the battery cell and the output terminal (terminal) of the external device. The external power supply can charge the battery through the terminal and the tab. The terminal 70 can be directly electrically connected to the battery cell tab or electrically connected to the tab through a metal adapter. The terminal 70 is made of metal materials including but not limited to copper, aluminum, aluminum alloy, and copper-aluminum alloy. In order to meet the requirements of fast charging performance, the size of the battery terminal 70 is usually designed to be large to accommodate the overcurrent requirement. Therefore, on the plane parallel to the first surface 201 of the cover plate 20, the distance between the terminal 70 and the side of the cover plate 20, especially the first side 202, is relatively short. In order to avoid the terminal 70 affecting the flange structure 401, the minimum distance between the flange structure 401 and the terminal 70 is further limited to L2 mm, which satisfies: 2 mm ≤ L2 mm ≤ 10 mm. For example, L2 mm can be 2 mm, 2.2 mm, 2.8 mm, 3.1 mm, 3.4 mm, 3.9 mm, 4.8 mm, 5.6 mm, 6.5 mm, 7.2 mm, 7.5 mm, 8.8 mm, 9.2 mm, 10 mm, etc., or any value between any two adjacent values ​​mentioned above. This improves the bonding strength of the flanged structure 401, reduces the risk of warping, and prevents the terminal 70 from affecting the flanged structure 401 during overcurrent. When L2 mm is less than 2 mm, the minimum distance between the flanged structure 401 and the terminal 70 is too small, and the heat generated by the terminal 70 can easily damage the flanged structure 401, affecting the insulation between the battery casings. When L2 mm is greater than 10 mm, the minimum distance between the flanged structure 401 and the terminal 70 is too large, increasing the risk of warping and potentially leading to localized insulation failure in the battery.

[0044] Please refer to Figure 2 The cover plate 20 includes two opposing first sides 202 and two opposing second sides 203, wherein the length of the first side 202 is greater than the length of the second side 203. Please refer to... Figure 3 The flange structure 401 includes a first flange structure 4011 disposed along the first side 202 and a second flange structure 4012 disposed along the second side 203. It can be understood that the cover plate 20 is rectangular in shape. The first flange structure 4011 is disposed on the first surface 201 of the cover plate 20 along the length direction of the first side 202, that is, the length direction of the first flange structure 4011 is parallel to the length direction of the first side 202. The second flange structure 4012 is disposed on the first surface 201 of the cover plate 20 along the length direction of the second side 203, that is, the length direction of the second flange structure 4012 is parallel to the length direction of the second side 203.

[0045] In some embodiments, please refer to Figure 5 The first flange structure 4011 and the second flange structure 4012 form an overlapping area 402 at the corner of the cover plate 20, and the overlapping area 402 covers the first flange structure 4011 located on the first side 202. It is understood that the overlapping area 402 includes at least two layers of insulating film 40. Since the distance between the two opposing first sides 202 and the terminal post 70 is small, the first flange structure 4011 is more prone to warping than the second flange structure 4012. Covering the first flange structure 4011 on the first side 202 with the overlapping area 402 can improve the adhesive strength of the first flange structure 4011 located on the first side 202, making it less prone to warping, thereby improving the insulation between battery casings. In this embodiment, to avoid warping of the flange structure 401, the width L mm of the flange structure 401 is further limited to satisfy: 2.5 mm ≤ L mm ≤ 8 mm. For example, L mm can be 2.5mm, 2.8mm, 3.1mm, 3.4mm, 3.9mm, 4.8mm, 5.6mm, 6.5mm, 7.2mm, 7.5mm, 8mm, etc., or any value between any two adjacent values ​​mentioned above. The width of the flange structure 401 can be designed to be appropriately large to avoid the overlapping area 402 being prone to warping if the width of the flange structure 401 of the insulating film 40 is too small.

[0046] In some embodiments, since the space between the two oppositely arranged second sides 203 is larger than the space between the two oppositely arranged first sides 202, the width of the second flange structure 4012 is greater than the width of the first flange structure 4011. This avoids the flange structure 401 on the first side 202 being too wide and interfering with functional components installed along the battery thickness direction. At the same time, the wider second flange structure 4012 can further ensure the bonding strength between the flange structure 401 and the cover plate 20, making it less prone to warping.

[0047] In some embodiments, please refer to Figure 3 , Figure 4 , Figure 5 The first flange structure 4011 continuously covers the first side 202 along its length, and the second flange structure 4012 continuously covers the second side 203 along its length. That is, both the first flange structure 4011 and the second flange structure 4012 are continuous and uninterrupted structures, which can improve the bonding strength between the first flange structure 4011 and the second flange structure 4012 and the first surface 201 of the cover plate 20, making it less prone to warping.

[0048] In other embodiments, please refer to Figure 9The first flange structure 4011 continuously covers the first side 202 along its length direction, while the second flange structure 4012 intermittently covers the second side 203 along its length direction; that is, the second flange structure 4012 is a discontinuous structure. This improves the coating efficiency of the insulating film 40 and avoids wrinkles in the insulating film 40. In this embodiment, to improve the adhesive strength of the second flange structure 4012 and prevent warping, the ratio of the total length of the second flange structure 4012 to the length of the second side 203 along its length direction is further defined as 'a', satisfying a ≥ 0.2. For example, a can be 0.2, 0.3, 0.4, 0.5, 0.6, etc., or any value between any two adjacent values ​​mentioned above.

[0049] By limiting the ratio 'a' of the total length of the second flange structure 4012 to the length of the second side 203 to greater than or equal to 0.2, the adhesive strength of the second flange structure 4012 can be improved, making it less prone to warping. When 'a' is less than 0.2, the ratio of the total length of the second flange structure 4012 to the length of the second side 203 is too small, resulting in weak adhesive strength of the second flange structure 4012, increasing the risk of warping and affecting the insulation of the battery casing.

[0050] In some embodiments, please refer to Figure 2 The first side surface 302 of the housing 30 includes two opposing first sub-side surfaces 3021 and two opposing second sub-side surfaces 3022, wherein the area of ​​the first sub-side surface 3021 is larger than the area of ​​the second sub-side surface 3022. For example... Figure 3 As shown, the insulating film 40 simultaneously covers both first sub-sides 3021 and both second sub-sides 3022. Thus, by simultaneously covering both first sub-sides 3021 and both second sub-sides 3022 with the insulating film 40, the first side 302 of the casing 30 is completely covered, improving the insulation of the battery casing 30.

[0051] In other embodiments, please refer to Figure 8 The insulating film 40 includes a cutout portion 403, which is used to expose the housing 30. The cutout portion 403 can be understood as a pre-reserved gap on the insulating film 40. When the insulating film 40 covers the battery housing 30, the housing 30 is exposed at the cutout portion 403 so that it can be directly fixed to the adjacent battery housing 30 or the battery housing 30 to other structural components in the battery pack, thereby improving the structural strength of the battery in the battery pack.

[0052] In some embodiments, the cutout portion 403 is provided on the first side surface 302 of the housing 30. Therefore, the provision of the cutout portion 403 will cause the width of the insulating film 40 near the cover plate 20 from the first surface 201 of the cover plate 20 to be shorter, making the insulating film 40 prone to warping. To avoid the insulating film 40 warping, further limitation is made: Please refer to Figure 10 Along the direction perpendicular to the first surface 201 of the cover plate 20, the minimum distance between the perforated portion 403 and the first surface 201 is L3 mm, satisfying: L3 mm ≥ 5 mm. For example, L3 can be 5 mm, 5.5 mm, 6 mm, 6.5 mm, 7 mm, 7.5 mm, 8 mm, 8.5 mm, etc., or any value between any two adjacent values ​​mentioned above. This avoids the insulating film 40 located above the perforated portion 403 from easily warping, while ensuring that the perforated portion 403 has sufficient size to improve the fixing firmness between two adjacent battery casings or between the battery casing and other structural components. When L3 mm is less than 5 mm, the minimum distance between the perforated portion 403 and the first surface 201 is too small, and the width of the insulating film 40 covering the area from the top of the perforated portion 403 to the first surface 201 is too short, making the insulating film 40 at this location prone to warping, affecting the insulation of the battery casing 30.

[0053] To further improve the insulation of the battery casing, please refer to... Figure 8 The cutout portion 403 is located on the second sub-side surface 3022. It is understandable that, since the width of the first flange structure 4011 along the first side 202 is relatively small, when the cutout portion 403 is located on the larger first sub-side surface 3021 of the housing 30, the first flange structure 4011 is more prone to warping. Therefore, by placing the cutout portion 403 on the smaller second sub-side surface 3022 of the housing 30, it is possible to ensure that the first side surface 302 of the battery housing 30 has sufficient coverage area of ​​the insulating film 40, thereby improving the adhesion strength of the insulating film 40 and the insulation of the battery housing 30. Simultaneously, the cutout portion 403 can be used to directly fix the battery housing 30 to adjacent battery housings, improving the structural strength of the battery within the battery pack.

[0054] In some embodiments, please refer to Figure 7The raised area 501 includes a first protrusion 5011, which protrudes from the first side surface 302 of the housing 30. On the plane of the first side surface 302, the orthographic projection of the cutout portion 403 of the insulating film 40 does not overlap with the orthographic projection of the first protrusion 5011. It can be understood that the first protrusion 5011 can be a raised structure protruding from the first side surface 302 of the housing 30, and the area of ​​the cutout portion 403 can avoid the position of the first protrusion 5011, ensuring that the first protrusion 5011 of the bonding wire 50 is covered by the insulating film 40, thereby improving the insulation of the battery housing 30.

[0055] In some embodiments, please refer to Figure 7 The raised area 501 includes a second protrusion 5012, which protrudes from the first surface 201 of the cover plate 20. The second protrusion 5012 can be a raised structure protruding from the first surface 201 of the cover plate 20. To avoid the protrusion height of the second protrusion 5012 affecting the bonding strength of the flange structure 401 of the insulating film 40, it is further defined that the maximum dimension of the second protrusion 5012 protruding from the first surface 201 of the cover plate 20 is H1 mm, satisfying: 0.01 mm ≤ H1 mm ≤ 0.5 mm. For example, H1 can be 0.01 mm, 0.08 mm, 0.12 mm, 0.16 mm, 0.18 mm, 0.25 mm, 0.28 mm, 0.34 mm, 0.39 mm, 0.48 mm, 0.5 mm, etc., or any value between any two adjacent values ​​mentioned above. By limiting the maximum dimension H1 mm of the second protrusion 5012 protruding from the first surface 201 of the cover plate 20 to the range of 0.01 mm to 0.5 mm, the connection between the insulating film 40 and the cover plate 20 is made smoother, and the insulating film 40 is less likely to warp on the first surface 201 of the cover plate 20, thus ensuring the insulation of the battery casing and also ensuring the welding strength between the casing 30 and the cover plate 20. When H1 mm is less than 0.01 mm, the maximum dimension of the second protrusion 5012 protruding from the first surface 201 of the cover plate 20 is too small, resulting in poor welding strength between the casing 30 and the cover plate 20, and a risk of cracking of the weld line 50. When H1 mm is greater than 0.5 mm, that is, the maximum dimension H1 of the second protrusion 5012 protruding from the first surface 201 of the cover plate 20 is too large, the second protrusion 5012 will affect the flatness of the insulating film 40 covering, causing the flange structure 401 of the insulating film 40 to warp easily, resulting in insulation failure in some areas of the battery casing.

[0056] It should be noted that the measurement method for the maximum dimension H1 mm of the second protrusion 5012 protruding from the first surface 201 of the cover plate 20 described in this application can be as follows: taking the intersection point of the length center of the weld line 50 and a first sub-side surface 3021 as the starting point, and along the extension direction of the weld line 50, take a measurement point every 20 mm, and perform the following operations for each measurement point: 1. Sampling: For each measurement point, use a cutting machine (e.g., Beta-300Pro) with a SiC cutting disc to cut a sample containing the complete weld line from the welded battery casing along the direction perpendicular to the weld line, in a low-speed pulse mode (6A, 0.6mm / s, 2200rpm) to avoid deformation of the heat-affected zone of the weld line. 2. Mounting: TJ2210 acrylic resin or TJ2568 epoxy resin is preferred. Apply 0.3MPa pressure for 15 minutes in a pressure cold mounting machine (e.g., Theta Mount pressure cold mounting machine) to avoid thermal stress damaging the microstructure of the weld line. 3. Grinding and Polishing: Use a grinding and polishing machine (such as GP-2000A) to grind step by step with graded sandpaper (P400 grit → 800 grit → 1200 grit → 2500 grit), and finally use 0.05μm alumina polishing liquid to obtain a mirror finish, ensuring that the weld line interface is clearly visible. 4. Etching: Soak in 0.01-0.5mol / L NaOH solution for 30 minutes, or use a 10% ammonium persulfate aqueous solution for chemical etching, to create a clear contrast between the welded area and the heat-affected zone. 5. Observation and Measurement: Observe the cross-section using a stereomicroscope or metallographic microscope, and measure the maximum dimension H1n of the second protrusion 5012 protruding from the first surface 201 of the cover plate 20 at each measurement point using professional image analysis software. Take the average value of the distance H1n at all measurement points as the value of H1.

[0057] In some embodiments, please refer to Figure 7The raised area 501 includes a first protrusion 5011, which protrudes from the first side surface 302 of the housing 30. The first protrusion 5011 can be a raised structure protruding from the first side surface 302 of the housing 30. In this embodiment, the maximum dimension of the first protrusion 5011 protruding from the first side surface 302 of the housing 30 is H2 mm, satisfying: 0.1 mm ≤ H2 mm ≤ 0.5 mm. For example, H2 mm can be 0.1 mm, 0.16 mm, 0.18 mm, 0.25 mm, 0.28 mm, 0.34 mm, 0.39 mm, 0.48 mm, 0.5 mm, etc., or any value between any two adjacent values ​​mentioned above. Thus, by limiting the maximum size of the first protrusion 5011 protruding from the first side surface 302 of the housing 30 to within the range of 0.1 mm to 0.5 mm, the insulating film 40 is made flatter at the first protrusion 5011, making it less prone to curling at the first surface 201 of the cover plate 20, ensuring the insulation of the battery housing, and also ensuring the welding strength between the housing 30 and the cover plate 20. When H2 mm is less than 0.1 mm, the maximum size of the first protrusion 5011 protruding from the first side surface 302 of the housing 30 is too small, resulting in poor welding strength between the housing 30 and the cover plate 20, and a risk of cracking of the weld line 50. When H2 mm is greater than 0.5 mm, that is, the maximum size of the first protrusion 5011 protruding from the first side surface 302 of the housing 30 is too large, the first protrusion 5011 will affect the flatness of the insulating film 40 covering, causing the flange structure 401 of the insulating film 40 to easily curl, resulting in insulation failure in some areas of the battery housing.

[0058] It should be noted that the measurement method for the maximum dimension H2 mm of the first protrusion 5011 protruding from the first side surface 302 of the housing 30 described in this application can be as follows: taking the intersection point of the length center of the welding line 50 and a first sub-side surface 3021 as the starting point, and along the extension direction of the welding line 50, take a measurement point every 20 mm, and perform the following operations for each measurement point: 1. Sampling: For each measurement point, use a cutting machine (e.g., Beta-300Pro) with a SiC cutting disc to cut a sample containing the complete welding line from the welded battery housing along the direction perpendicular to the welding line, in a low-speed pulse mode (6A, 0.6mm / s, 2200rpm) to avoid deformation of the heat-affected zone of the welding line. 2. Mounting: TJ2210 acrylic resin or TJ2568 epoxy resin is preferred. Apply a pressure of 0.3MPa for 15 minutes in a pressure cold mounting machine (e.g., Theta Mount pressure cold mounting machine) to avoid thermal stress damaging the microstructure of the welding line. 3. Grinding and Polishing: Use a grinding and polishing machine (such as GP-2000A) to grind step by step with graded sandpaper (P400 grit → 800 grit → 1200 grit → 2500 grit), and finally use 0.05μm alumina polishing liquid to obtain a mirror finish, ensuring that the weld line interface is clearly visible. 4. Etching: Immerse in 0.01-0.5mol / L NaOH solution for 30 minutes, or use 10% ammonium persulfate aqueous solution for chemical etching, to create a clear contrast between the welded area and the heat-affected zone. 5. Observation and Measurement: Observe the cross-section using a stereomicroscope or metallographic microscope, and measure the maximum dimension H2n of the first protrusion 5011 protruding from the first side surface 302 of the shell 30 at each measurement point using professional image analysis software. Take the average value of the distance H2n at all measurement points as the value of H2.

[0059] In some embodiments, please refer to Figure 7 Along a direction perpendicular to the first surface 201, the bonding wire 50 includes a first end 502 near the first surface 201 and a second end 503 away from the first surface 201. The first end 502 can be understood as having the boundary of the bonding wire molten pool at the highest point in a cross-section perpendicular to the first surface 201, and the second end 503 having the boundary of the bonding wire molten pool at the lowest point in a cross-section perpendicular to the first surface 201. The distance between the deepest point of the bonding wire 50 and the plane containing the first end 502 is less than the distance between the deepest point of the bonding wire 50 and the plane containing the second end 503. This reduces the protruding area of ​​the protrusion region 501 of the bonding wire 50 on the first surface 201, improves the adhesion strength of the flange structure 401 of the insulating film 40 at the protruding area 501, and simultaneously ensures the welding strength of the bonding wire 50, thereby improving the welding strength between the housing 30 and the cover plate 20.

[0060] In some embodiments, such as Figure 7 As shown, the cover plate 20 also includes a second surface 204 disposed opposite to the first surface 201. In order to make the distance between the deepest melting point of the bonding wire 50 and the plane where the first end 502 is located less than the distance between the deepest melting point of the bonding wire 50 and the plane where the second end 503 is located, the distance between the deepest melting point of the bonding wire 50 and the first surface 201 of the cover plate 20 in the direction perpendicular to the first surface 201 is greater than the distance between the deepest melting point of the bonding wire 50 and the second surface 204, so that the deepest melting point of the bonding wire 50 is more biased towards the second surface 204 of the cover plate. This can reduce the protrusion area of ​​the protrusion area 501 of the bonding wire 50 on the first surface 201, improve the bonding strength of the flange structure 401 of the insulating film 40 at the protrusion area 501, and at the same time ensure the welding strength of the bonding wire 50, so as to improve the welding strength between the housing 30 and the cover plate 20.

[0061] It should be noted that the test method for the weld depth and width of the weld pool in this application can be carried out by metallographic analysis. By preparing a cross-sectional sample of the weld wire, the weld depth and width can be directly observed and quantified under an optical microscope. The measurement method and implementation process are as follows: 1. Sampling: From the welded battery casing, along the direction perpendicular to the weld, use a cutting machine (e.g., Beta-300Pro) with a SiC cutting disc to cut a sample containing the complete weld in a low-speed pulse mode (6A, 0.6mm / s, 2200rpm) to avoid deformation of the heat-affected zone. 2. Mounting: TJ2210 acrylic resin or TJ2568 epoxy resin is preferred. Apply a pressure of 0.3MPa for 15 minutes in a pressure cold mounting machine (e.g., Theta Mount pressure cold mounting machine) to avoid thermal stress damaging the weld microstructure. 3. Grinding and Polishing: Use a grinding and polishing machine (such as GP-2000A) to grind in a gradient sandpaper sequence (P400 grit → 800 grit → 1200 grit → 2500 grit), finally achieving a mirror finish with 0.05μm alumina polishing solution to ensure a clearly discernible weld interface. 4. Corrosion: Immerse in a 0.01-0.5mol / L NaOH solution for 30 minutes, or perform chemical corrosion using a 10% ammonium persulfate aqueous solution to create a clear contrast between the welded area and the heat-affected zone. 5. Observation and Measurement: Observe the cross-section using a stereomicroscope or metallographic microscope, and measure the weld penetration and weld width using professional image analysis software. Weld penetration refers to the vertical distance from the base material surface to the deepest melting point of the weld line. Weld width refers to the horizontal width of the base material melting boundary on both sides of the weld line.

[0062] The weld penetration and weld width can be controlled by adjusting the welding process, the materials of the shell 30 and cover plate 20, and the thickness of the weld joint. For example, when using laser welding, the welding process can be controlled by adjusting the laser power (range: 1000W to 6000W), welding speed (range: 200–400mm / s), defocusing amount (positive defocusing range: +0.5mm to +4mm, negative defocusing range: -0.5mm to -3mm), pulse waveform (sharp wave or double peak wave), and laser oscillation mode (using a "figure-eight" or "elliptical" trajectory). When the shell 30 is made of steel, aluminum, titanium, etc., the proportion of trace doping elements in the shell material, such as Mg, Cu, Cr, Fe, Mn, Zn, C, Si, N, etc., can be adjusted.

[0063] In some embodiments, please refer to Figure 7 The housing 30 includes a housing body 300 and a reinforcing protrusion 303, which is located near the opening 301. The reinforcing protrusion 303 is located on the side of the housing body 300 facing the battery cell 60. The reinforcing protrusion 303 increases the thickness of the housing body 300 near the opening 301, thereby improving the welding strength between the cover plate 20 and the housing 30. However, the reinforcing protrusion 303 increases the thickness of the housing 30 at the welding position, resulting in higher welding energy during welding. This makes it easier to form a raised area 501 on the surface of the housing assembly, meaning the weld line 50 is more likely to protrude from the housing assembly and form a raised area. In this embodiment, the following condition is further defined: 2.17 ≤ D×L ≤ 9.08. For example, D×L can be 2.17, 2.72, 3.14, 4.03, 4.75, 5.76, 6.76, 7.70, 8.8, 9.08, etc., or any value between any two adjacent values ​​mentioned above. The D×L value is made slightly larger to avoid the insulation film 40 being too narrow in this embodiment, which would make it prone to curling and cause local insulation failure of the battery.

[0064] It is understood that the reinforcing protrusion 303 can be integrally formed with the housing body 300, such that the total thickness of the housing body 300 and the reinforcing protrusion 303 is greater than the thickness of other housing bodies 300 without the reinforcing protrusion 303 near its opening 301. In some embodiments, the reinforcing protrusion 303 is connected to the housing body 300 in a gradually decreasing thickness along a direction perpendicular to the first surface 201, thereby improving the structural strength of the housing 30.

[0065] In some embodiments, along a direction perpendicular to the first side surface 302, the reinforcing protrusion 303 protrudes from the housing body 300 by a thickness of E mm, satisfying: 0.05 mm ≤ E mm ≤ 1.5 mm. For example, E mm can be 0.05 mm, 0.15 mm, 0.25 mm, 0.35 mm, 0.45 mm, 0.55 mm, 0.65 mm, 0.75 mm, 0.85 mm, 0.95 mm, 1.15 mm, 1.35 mm, 1.45 mm, 1.5 mm, etc., or any value between any two adjacent values ​​mentioned above. It is understood that the thickness of the reinforcing protrusion 303 protruding from the housing body 300 is the distance between the surface of the reinforcing protrusion 303 facing the interior of the housing 300 and the surface of the housing body 300 facing the interior of the housing 300. This improves the welding strength between the cover plate 20 and the housing 30 while reducing the risk of the insulating film warping. When E mm is less than 0.05 mm, the thickness of the reinforcing protrusion 303 protruding from the housing body 300 is too small, reducing the welding strength between the cover plate 20 and the housing 30. When E mm is greater than 1.5 mm, the thickness of the reinforcing protrusion 303 protruding from the housing body 300 is too large, which makes it easier for a raised area 501 to form on the surface of the housing assembly. The excessive protrusion height of the raised area 501 makes the insulating film prone to peeling, leading to local insulation failure of the battery.

[0066] In some embodiments, please refer to Figure 2 and Figure 6 The battery also includes an insulating sheet 10, which is connected to the first surface 201 of the cover plate 20. The insulating sheet 10 thus provides insulation to the cover plate 20. The insulating sheet 10 is disposed on the outer surface of the cover plate 20, insulating the surface of the cover plate 20 not protected by the insulating film 40, thereby improving the insulation performance of the battery's outer surface. The insulating sheet 10 is typically adhered to the first surface 201 of the cover plate 20 with adhesive. The material of the insulating sheet 10 can be polyimide (PI), polypropylene (PP), polyphenylene sulfide (PPS), polyethylene (PE), epoxy resin (FR4), etc.

[0067] In some embodiments, please refer to Figure 6 On a plane parallel to the first surface 201, the orthographic projection of the insulating sheet 10 at least partially overlaps with the orthographic projection of the flange structure 401 of the insulating film 40, with the insulating sheet 10 disposed on the side of the flange structure 401 facing away from the cover plate 20. In this way, the flange structure 401 can be fixed by the insulating sheet 10, further preventing the flange structure 401 from warping.

[0068] In some embodiments, the insulating sheet 10 is bonded to the flange structure 401, thus fixing the flange structure 401 with the insulating sheet 10. In this embodiment, because the flange structure 401 is less prone to warping under the pressing action of the insulating sheet 10, it can be further defined that the distance D mm between the deepest point of the weld line 50 and the first surface 201 in the direction perpendicular to the first surface 201 satisfies: 0.30 mm ≤ D mm ≤ 1.07 mm. For example, D mm can be 0.30 mm, 0.50 mm, 0.62 mm, 0.74 mm, 0.82 mm, 0.90 mm, 1.0 mm, 1.07 mm, etc., or any value between any two adjacent values ​​mentioned above. This allows the value of D to be appropriately small, increasing the welding area of ​​the cover plate 20, thereby improving the welding strength between the cover plate 20 and the housing 30.

[0069] In some embodiments, the flanged structure 401 is bonded to the first surface 201 of the cover plate 20 by an adhesive layer. For example, the insulating film 40 can be polyester film (PET, Polyethylene Terephthalate), polyimide (PI), polypropylene (PP), polyphenylene sulfide (PPS), or polyethylene (PE), etc., thereby improving the bonding strength between the flanged structure 401 of the insulating film 40 and the cover plate 20, and further reducing the risk of the insulating film 40 detaching from the cover plate 20 and warping. In other embodiments, the insulating film 40 is bonded to the housing 30, for example, the insulating film 40 itself may have an adhesive layer, and the insulating film 40 and the housing 30 can be bonded together by the adhesive layer, thereby improving the bonding strength between the insulating film 40 and the housing 30.

[0070] In some embodiments, the shear strength of the insulating film 40 is 0.2 MPa to 15 MPa. For example, it can be 0.2 MPa, 1.5 MPa, 5 MPa, 8 MPa, 12 MPa, 15 MPa, or any value between any two adjacent values ​​mentioned above. This improves the adhesive strength of the insulating film 40 while ensuring that it can be easily peeled from the housing 30 or the cover plate 20, facilitating battery repair. It is understood that the insulating film 40 includes a base film layer and an adhesive layer, with the base film layer bonded to the housing 30 and the cover plate 20 via the adhesive layer. The shear strength of the insulating film 40 described in this application refers to the shear strength of the base film layer.

[0071] It should be noted that the method for measuring the distance Dmm between the deepest point of the weld wire 50 and the first surface 201 described in this application can be referred to as follows: taking the intersection point of the length center of the weld wire 50 and a first sub-side surface 3021 as the starting point, along the extension direction of the weld wire 50, take a measurement point every 20mm, and perform the following operation for each measurement point.

[0072] 1. Sampling: For each measurement point, use a cutting machine (e.g., Beta-300Pro) with a SiC cutting disc along the direction perpendicular to the weld on the welded battery casing to cut a sample containing the complete weld line in low-speed pulse mode (6A, 0.6mm / s, 2200rpm) to avoid deformation of the heat-affected zone of the weld line.

[0073] 2. Embedding: TJ2210 acrylic resin or TJ2568 epoxy resin are preferred. Apply 0.3MPa pressure for 15 minutes in a pressure cold embedding machine (e.g., Theta Mount pressure cold embedding machine) to avoid thermal stress damaging the microstructure of the bonding wire.

[0074] 3. Grinding and polishing: Use a grinding and polishing machine (such as GP-2000A) to grind step by step in the order of gradient sandpaper (P400 mesh → 800 mesh → 1200 mesh → 2500 mesh), and finally use 0.05μm alumina polishing liquid to obtain a mirror surface, ensuring that the weld interface is clearly visible.

[0075] 4. Corrosion: Soak in 0.01-0.5 mol / L NaOH solution for 30 minutes, or use 10% ammonium persulfate aqueous solution for chemical corrosion to create a clear contrast between the welded area and the heat-affected zone.

[0076] 5. Observation and Measurement: Observe the cross-section using a stereomicroscope or metallographic microscope. Measure the distance Dn between the deepest point of the weld wire 50 and the first surface 201 at each measurement point using professional image analysis software. Take the average of the distances Dn at all measurement points as the value of D.

[0077] The distance D mm between the deepest point of the weld line 50 and the first surface 201 can be adjusted by adjusting the laser focusing position, laser power (range: 1000W to 6000W), welding speed (range: 200–400mm / s), defocusing amount (positive defocusing range: +0.5mm to +4mm, negative defocusing range: -0.5mm to -3mm), pulse waveform (peak wave or double peak wave), and laser oscillation mode (using a "figure-eight" or "elliptical" trajectory) during laser welding.

[0078] The method for measuring the width L of the flange structure 401 in this application can be as follows: measure the width of the flange structure 401 extending beyond the two first edges 202 and the two second edges 203 on the first surface 201 of the cover plate 20 of the battery in sequence, and take the smallest value as the value of the width L of the flange structure 401 in the battery.

[0079] The battery provided in this application will be described in detail below through specific embodiments.

[0080] It should be noted that the dimensions and area of ​​this application can be measured using measuring instruments such as micrometers or calipers, measuring parameters such as length, width, distance, and thickness. The area is calculated from the measured parameters such as length, width, distance, and thickness.

[0081] Battery manufacturing: (1) Preparation of positive electrode sheet.

[0082] The prepared positive electrode active material, conductive agent (e.g., acetylene black), and binder (e.g., PVDF) are mixed, and solvent NMP is added. The mixture is stirred under vacuum until the system is homogeneous to obtain a positive electrode slurry. The positive electrode slurry is uniformly coated on both surfaces of the positive electrode current collector foil, dried at room temperature, and then transferred to an oven for further drying. The positive electrode sheet is then obtained by rolling and slitting.

[0083] Specifically, the mass ratio of positive electrode active material: conductive agent: binder satisfies (92~98): (4~1): (4~1).

[0084] (2) Preparation of negative electrode sheet.

[0085] The negative electrode active material, conductive agent (e.g., acetylene black), thickener (e.g., carboxymethyl cellulose (CMC)), and binder (e.g., styrene-butadiene rubber (SBR)) are mixed, and deionized water is added as a solvent. The mixture is stirred under vacuum until the system is homogeneous to obtain a negative electrode slurry. The negative electrode slurry is uniformly coated on both surfaces of the negative electrode current collector foil, air-dried at room temperature, and then transferred to an oven for further drying. Finally, the negative electrode sheet is obtained by rolling and slitting.

[0086] Specifically, the ratio of negative electrode active material: conductive agent: thickener: binder satisfies (90~96): (4~2): (2~1): (4~1).

[0087] (3) Preparation of electrolyte.

[0088] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to obtain an organic solvent. Then, fully dried lithium salt LiPF6 was dissolved in the mixed organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0089] (4) Preparation of the diaphragm: Polyethylene film is selected as the diaphragm.

[0090] (5) Preparation of lithium-ion batteries.

[0091] The positive electrode, separator, and negative electrode are stacked in sequence and formed into a bare cell by winding or stacking. The bare cell is then placed in a battery casing, which is a prismatic casing. The battery is dried, injected with electrolyte, and then packaged, allowed to stand, formed, and calibrated to obtain a lithium-ion battery.

[0092] (6) Applying the insulating film.

[0093] An insulating film is adhered to the first side of the lithium-ion battery casing, with the top of the insulating film extending beyond the first side. The excess portion is bent towards the cover plate and bonded to the first surface of the cover plate, forming a flanged structure. The insulating film is selected from polyester film (PET, Polyethylene Terephthalate), polyimide (PI), polypropylene (PP), polyphenylene sulfide (PPS), or polyethylene (PE), etc., and the adhesive layer is selected from acrylic adhesive, epoxy resin adhesive, polyurethane adhesive, etc.

[0094] In the selection of materials for the battery, this application may also select other materials, not limited to the materials limited by the above preparation method. The positive electrode active material may be selected from one or more lithium-containing positive electrode active materials, including lithium iron phosphate, ternary materials containing nickel, cobalt and manganese, and lithium manganese iron phosphate; the negative electrode active material may be selected from one or more negative electrode active main materials, such as artificial graphite, natural graphite, silicon carbide, silicon oxide, and lithium titanate.

[0095] The conductive agent includes, but is not limited to, one or more combinations of graphite, superconducting carbon, carbon black (such as acetylene black, Ketjen black, Super P, etc.), carbon nanotubes, graphene, and carbon nanofibers. The binder includes, but is not limited to, one or more combinations of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, fluorinated acrylate resin, styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, carboxymethyl chitosan, etc.

[0096] The solvent can be deionized water, NMP (N-methylpyrrolidone), alcohol, ether, ketone or other types of pyrrolidone, etc.

[0097] The positive electrode current collector foil can be a metal foil or a composite current collector. For example, as a metal foil, it can be made of stainless steel, copper, aluminum, nickel, carbon electrode, carbon, nickel, or titanium with a silver-plated surface. The composite current collector may include a polymer material base layer and a metal layer. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.). The negative electrode current collector foil can be a metal foil or a composite current collector. For example, as a metal foil, it can be made of stainless steel, copper, aluminum, nickel, carbon electrodes, or titanium with a silver-plated surface. The composite current collector may include a polymer material base layer and a metal layer. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloy, copper, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).

[0098] Performance tests are as follows: Performance Test 1: Warpage ratio of the insulating film flange structure.

[0099] Following the battery fabrication method described above, 200 batteries were prepared for each embodiment and comparative example. The bottom of each battery was adhered to a flat metal base plate using structural adhesive, serving as the test object. Epoxy resin structural adhesive was used. All other test conditions remained consistent.

[0100] Then, according to the requirements of GB / T2423.43, the test object is mounted on the vibration table. The test procedure is carried out according to the provisions of GB / T2423.56. Random and fixed-frequency vibration loads are applied in each direction respectively. The loading sequence should preferably be random z-axis, fixed-frequency z-axis, random y-axis, fixed-frequency y-axis, random x-axis, fixed-frequency x-axis (the direction of the line connecting the front and rear of the battery pack is the x-axis direction, and the other horizontal direction perpendicular to the x-axis direction is the y-axis direction). The vibration frequency, power spectral density (PSD), vibration time, etc. are shown in Table 1 below.

[0101] Table 1 After vibration, remove the batteries and observe whether the insulating film flange structure in the battery pack has warped. Count the number of batteries whose flange structure has detached from the first surface of the cover plate, and calculate the percentage of batteries with warped insulating film flange structures. If the percentage of batteries with warped insulating film flange structures is less than or equal to 3%, it is considered good; if the percentage is less than or equal to 5% but greater than 3%, it is considered acceptable; if the percentage is greater than 5%, it is considered unacceptable.

[0102] Performance Test 2: Bond Wire Cracking Rate.

[0103] Following the battery fabrication method described above, 200 batteries were prepared for each embodiment and comparative example. The bottom of each battery was adhered to a flat metal base plate using structural adhesive, and the terminals of each battery were connected in series via a busbar. These batteries served as test subjects. Epoxy resin structural adhesive was used. All other test conditions remained consistent.

[0104] Then, according to the requirements of GB / T2423.43, the test object is mounted on the vibration table. The test procedure is carried out according to the provisions of GB / T2423.56. Random and fixed-frequency vibration loads are applied in each direction respectively. The loading sequence should preferably be random z-axis, fixed-frequency z-axis, random y-axis, fixed-frequency y-axis, random x-axis, fixed-frequency x-axis (the direction of the line connecting the front and rear of the battery pack is the x-axis direction, and the other horizontal direction perpendicular to the x-axis direction is the y-axis direction). The vibration frequency, power spectral density (PSD), vibration time, etc. are shown in Table 2 below.

[0105] Table 2 After vibration, the battery pack was subjected to 50 charge-discharge cycles at room temperature (20℃). The charge-discharge cycle conditions were as follows: constant current charging at a rate of 1C until the battery voltage reached the upper limit voltage, then switching to constant voltage charging until the battery current dropped to 0.05C, resting for 30 minutes, and then discharging at a rate of 1C until the lower limit voltage was reached, resting for 30 minutes before starting the next cycle. The upper and lower limit voltages of individual batteries need to be adjusted accordingly for different systems: Lithium iron phosphate (LFP) - upper limit voltage 3.65V, lower limit voltage 2.5V; Nickel-cobalt-manganese ternary NCM - upper limit voltage 4.25V, lower limit voltage 2.5V; Lithium manganese iron phosphate (LFMP) - upper limit voltage 4.25V, lower limit voltage 2.5V; Lithium nickel manganese oxide - upper limit voltage 4.8V, lower limit voltage 3.5V.

[0106] After the cycle is completed, remove the battery and observe whether the solder joint between the cover plate and the shell is cracked. Calculate the proportion of batteries with cracked solder joints. If the proportion of batteries with cracked solder joints is less than or equal to 1.5%, it is considered good; if the proportion of batteries with cracked solder joints is less than or equal to 3% but greater than 1.5%, it is considered qualified; if the proportion of batteries with cracked solder joints is greater than 3%, it is considered unqualified.

[0107] The positive electrode active material used in this test was selected from LiNi. 0.6 Co 0.2 Mn 0.2Taking O2 as an example, all other positive electrode materials meet the above test requirements, and the mass ratio of positive electrode active material: conductive agent: binder is 96:2:2; the negative electrode active material is selected from artificial graphite, and the ratio of negative electrode active material: conductive agent: thickener: binder is 95:2:1:2.

[0108] The test parameters and performance test results of each example and comparative example are shown in Table 3.

[0109] Table 3 Test parameters and results of Examples 1 to 15 and Comparative Examples 1 to 3 It can be seen from the above Table 3 that, compared with Comparative Examples 1 to 3, in Examples 1 to 15 where 0.66≤D×L≤9.08 is satisfied, the proportion of batteries with warped flanged structure of the insulating film is all less than or equal to 5%, Performance Test 1 shows qualified or good, the proportion of batteries with cracked welding lines is all less than or equal to 3%, and Performance Test 2 shows qualified or good. In Comparative Example 1, the D×L value is less than 0.66, the D×L value is too small, which increases the risk of warpage of the flanged structure of the insulating film. In Performance Test 1, the proportion of batteries with warped flanged structure of the insulating film is greater than 5%, so Performance Test 1 shows unqualified. In Comparative Example 2, the D value is greater than 1.21, resulting in the D×L value being greater than 9.08. The D×L value is too large, which leads to insufficient strength at the welding position of the cover plate and the housing. In Performance Test 2, the proportion of batteries with cracked welding lines is greater than 3%, and Performance Test 2 shows unqualified. In Comparative Example 3, the L value is less than 2.0, resulting in the D×L value being less than 0.66. The D×L value is too small, which increases the risk of warpage of the flanged structure of the insulating film. In Performance Test 1, the proportion of batteries with warped flanged structure of the insulating film is greater than 5%, so Performance Test 1 shows unqualified.

[0110] Compared with Examples 4 to 11, although Examples 1 to 3 satisfy 0.66≤D×L≤9.08, their D×L values are less than 2.17, the D×L values are relatively small, the risk of warpage of the flanged structure of the insulating film is relatively high, and the proportion of batteries with warped flanged structure of the insulating film in Performance Test 1 is greater than 3% but less than or equal to 5%, so Performance Test 1 shows qualified. While in Examples 4 to 11, the D×L values satisfy 2.17≤D×L≤7.70, which can reduce the risk of warpage of the flanged structure of the insulating film. The proportion of batteries with warped flanged structure of the insulating film in Performance Test 1 is less than or equal to 3%, and Performance Test 2 shows good.

[0111] Compared with Examples 4 to 11, in Examples 12 and 13, although the D×L value satisfies 0.66≤D×L≤9.08, the D×L value is greater than 7.70, the D×L value is relatively large, the strength of the welded joint between the cover plate and the housing is relatively weak, the proportion of batteries with cracked welding lines in Performance Test 2 is greater than 1.5% but less than or equal to 3%, and Performance Test 2 is qualified. While in Examples 4 to 11, the D×L value satisfies 2.17≤D×L≤7.70, the strength of the welded joint between the cover plate and the housing is increased, the proportion of batteries with cracked welding lines in Performance Test 2 is all less than or equal to 1.5%, and Performance Test 2 shows a good result.

[0112] Compared with Examples 4 to 11, in Example 14, the D value is less than 0.30, so that although the D×L value satisfies 0.66≤D×L≤9.08, the D×L value is less than 2.17, the D×L value is relatively small, the proportion of batteries with warped flanged structure of the insulating film in Performance Test 1 is greater than 3% but less than or equal to 5%, so Performance Test 1 is qualified. While in Examples 4 to 11, the D×L value satisfies 2.17≤D×L≤7.70, which can reduce the risk of warpage of the flanged structure of the insulating film, the proportion of batteries with warped flanged structure of the insulating film in Performance Test 1 is less than or equal to 3%, and Performance Test 1 shows a good result.

[0113] In Example 15, although the L value is greater than 8.0, the D×L value satisfies 2.17≤D×L≤7.70, the proportion of batteries with warped flanged structure of the insulating film in Performance Test 1 is less than or equal to 3%, and Performance Test 1 shows a good result. The proportion of batteries with cracked welding lines in Performance Test 2 is all less than or equal to 1.5%, and Performance Test 2 shows a good result.

[0114] The foregoing description is merely preferred embodiments of the present application, and is not intended to limit the present application. Any modifications, equivalent replacements, improvements and the like made within the spirit and principle of the present application shall all be included in the protection scope of the present application.

Claims

1. A battery, characterized in that, include: Battery cell (60); A housing assembly, wherein the battery cell (60) is disposed within the housing assembly, the housing assembly includes a housing (30) and a cover plate (20), the housing (30) has an opening (301) on at least one side, the housing (30) includes a first side surface (302) surrounding the opening (301), the cover plate (20) covers the opening (301) and is welded to the opening (301) to form a weld line (50), the cover plate (20) has a first surface (201) facing away from the housing (30), wherein the angle between the melting depth direction of the weld line (50) and the first surface (201) is 0°-10°, at least a portion of the weld line (50) protrudes from the housing assembly to form a protrusion area (501); along a direction perpendicular to the first surface (201), the distance between the deepest melting point of the weld line (50) and the first surface (201) is D mm; An insulating film (40) covers at least a portion of the first side surface (302) of the housing (30) and extends to the first surface (201) of the cover plate (20) to form a flange structure (401). The insulating film (40) covers at least a portion of the raised area (501). The width of the flange structure (401) is L mm, satisfying: 0.66≤D×L≤9.

08.

2. The battery according to claim 1, characterized in that, The flange structure (401) covers at least a portion of the raised area (501) of the weld line (50).

3. The battery according to claim 2, characterized in that, The minimum length of the edge of the flange structure (401) extending beyond the protrusion area (501) is L1 mm, satisfying: 1.0 mm ≤ L1 mm ≤ 7.9 mm.

4. The battery according to claim 1, characterized in that, The cover plate (20) is provided with a pole post (70), and the minimum distance between the flange structure (401) and the pole post (70) is L2 mm, which satisfies: 2 mm ≤ L2 mm ≤ 10 mm.

5. The battery according to claim 1, characterized in that, The cover plate (20) includes two oppositely arranged first sides (202) and two oppositely arranged second sides (203), the length of the first side (202) is greater than the length of the second side (203), and the flange structure (401) includes a first flange structure (4011) arranged along the first side (202) and a second flange structure (4012) arranged along the second side (203).

6. The battery according to claim 5, characterized in that, The first flange structure (4011) and the second flange structure (4012) form an overlapping area (402) at the corner of the cover plate (20), and the overlapping area (402) covers the first flange structure (4011) located on the first side (202).

7. The battery according to claim 6, characterized in that, The width L mm of the flange structure (401) satisfies: 2.5 mm ≤ L mm ≤ 8 mm.

8. The battery according to claim 5, characterized in that, The width of the second flange structure (4012) is greater than the width of the first flange structure (4011).

9. The battery according to claim 5, characterized in that, The first flange structure (4011) continuously covers the first side (202) along the length direction of the first side (202), and the second flange structure (4012) covers the second side (203) at intervals along the length direction of the second side (203). The ratio of the total length of the second flange structure (4012) along the length direction of the second side (203) to the length of the second side (203) is a, which satisfies: a≥0.

2.

10. The battery according to any one of claims 1 to 9, characterized in that, The first side (302) of the housing (30) includes two oppositely arranged first sub-sides (3021) and two oppositely arranged second sub-sides (3022), the area of ​​the first sub-side (3021) is larger than the area of ​​the second sub-side (3022), and the insulating film (40) covers both the first sub-sides (3021) and the two second sub-sides (3022).

11. The battery according to any one of claims 1 to 9, characterized in that, The insulating film (40) includes a cutout portion (403) for exposing the housing (30). The cutout portion (403) is located on the first side (302) of the housing (30). Along the direction perpendicular to the first surface (201) of the cover plate (20), the minimum distance between the cutout portion (403) and the first surface (201) is L3 mm, satisfying: L3 mm ≥ 5 mm.

12. The battery according to claim 11, characterized in that, The first side (302) of the housing (30) includes two oppositely arranged first sub-sides (3021) and two oppositely arranged second sub-sides (3022), the area of ​​the first sub-side (3021) is larger than the area of ​​the second sub-side (3022), and the hollow part (403) is provided on the second sub-side (3022).

13. The battery according to claim 11, characterized in that, The raised area (501) includes a first protrusion (5011), which protrudes from the first side surface (302) of the housing (30). On the plane where the first side surface (302) is located, the orthographic projection of the hollow portion (403) of the insulating film (40) does not overlap with the orthographic projection of the first protrusion (5011).

14. The battery according to any one of claims 1 to 9, characterized in that, The raised area (501) includes a second protrusion (5012), which protrudes from the first surface (201) of the cover plate (20). The maximum size of the second protrusion (5012) protruding from the first surface (201) of the cover plate (20) is H1 mm, satisfying: 0.01 mm ≤ H1 mm ≤ 0.5 mm.

15. The battery according to any one of claims 1 to 9, characterized in that, The raised area (501) includes a first protrusion (5011) that protrudes from the first side surface (302) of the housing (30).

16. The battery according to claim 15, characterized in that, The first protrusion (5011) protrudes from the first side (302) of the housing (30) with a maximum dimension of H2 mm, satisfying: 0.1 mm ≤ H2 mm ≤ 0.5 mm.

17. The battery according to any one of claims 1 to 9, characterized in that, Along a direction perpendicular to the first surface (201), the bonding wire (50) includes a first end (502) near the first surface (201) and a second end (503) away from the first surface (201), wherein the distance between the deepest point of the bonding wire (50) and the plane where the first end (502) is located is less than the distance between the deepest point of the bonding wire (50) and the plane where the second end (503) is located.

18. The battery according to any one of claims 1 to 9, characterized in that, The housing (30) includes a housing body (300) and a reinforcing protrusion (303). The reinforcing protrusion (303) is disposed near the opening (301). The reinforcing protrusion (303) is disposed on the side of the housing body (300) facing the battery cell (60) and satisfies: 2.17≤D×L≤9.

08.

19. The battery according to claim 18, characterized in that, Along the direction perpendicular to the first side surface (302), the reinforcing protrusion (303) protrudes from the housing body (300) with a thickness of E mm, satisfying: 0.05 mm ≤ E mm ≤ 1.5 mm.

20. The battery according to any one of claims 1 to 9, characterized in that, Also includes: An insulating sheet (10) is connected to the first surface (201) of the cover plate (20).

21. The battery according to claim 20, characterized in that, On a plane parallel to the first surface (201), the orthographic projection of the insulating sheet (10) at least partially overlaps with the orthographic projection of the flange structure (401) of the insulating film (40), and the insulating sheet (10) is disposed on the side of the flange structure (401) away from the cover plate (20).

22. The battery according to claim 21, characterized in that, The insulating sheet (10) is bonded to the flange structure (401). Along the direction perpendicular to the first surface (201), the distance D mm between the deepest melting point of the welding line (50) and the first surface (201) satisfies: 0.30 mm ≤ D mm ≤ 1.07 mm.

23. The battery according to any one of claims 1 to 9, characterized in that, The flange structure (401) is bonded to the first surface (201) of the cover plate (20) by an adhesive layer.

24. The battery according to any one of claims 1 to 9, characterized in that, It must satisfy: 0.30 mm ≤ D mm ≤ 1.21 mm; and / or, 2.0 mm ≤ L mm ≤ 8.0 mm.

25. A battery pack comprising at least one battery as described in any one of claims 1 to 24.

26. A battery pack comprising the battery pack of claim 25.

27. An electrical device comprising the battery pack of claim 26.