A flame-retardant self-healing composite separator for lithium-ion batteries and its preparation method
By employing a layered configuration of PI/PMMA blended nanofiber framework, dynamic disulfide bond network self-healing layer, and covalent DOPO phosphorus-containing flame retardant layer in lithium-ion battery separators, the problems of coating delamination and flame retardant migration during thermo-mechanical cycling of lithium-ion battery separators are solved, thereby improving the thermal stability and self-healing ability of the separators.
Patent Information
- Application Number
- CN202611492717.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-17
AI Technical Summary
Existing lithium-ion battery separators are prone to problems such as coating delamination, microcracks that are difficult to repair, flame retardant migration, and flame retardant filler blockage during thermo-mechanical cycling. Traditional composite separators are difficult to solve these problems without significantly sacrificing lithium-ion transport performance.
PI/PMMA blended nanofibers are used as a porous support framework. A stable interface is constructed through fiber surface activation and silane coupling. An inner self-healing layer mainly composed of dynamic disulfide bond network and an outer flame-retardant layer mainly composed of covalent DOPO phosphorus-containing units and nano-aluminum hydroxide are formed on the surface to achieve functional layered configuration.
Without significantly affecting lithium-ion transport performance, the membrane's thermal stability, interfacial stability, flame retardancy, and self-healing ability after damage are improved, while reducing the risk of flame retardant migration and coating delamination.
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery separator technology, and in particular to a flame-retardant self-healing composite separator for lithium-ion batteries and its preparation method. Background Technology
[0002] A lithium-ion battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator disposed between the positive and negative electrodes. The separator prevents the positive and negative electrodes from directly contacting each other and causing an internal short circuit, while allowing lithium ions in the electrolyte to migrate between the positive and negative electrodes. Therefore, the thermal stability, mechanical properties, pore structure, electrolyte wetting properties, and interfacial stability of the separator directly affect the safety and cycle performance of the lithium-ion battery.
[0003] Existing commercial lithium-ion battery separators primarily use polyolefin materials such as polyethylene and polypropylene. These separators offer advantages such as light weight, good chemical stability, and mature manufacturing processes, but their heat resistance is relatively limited. Under abnormal battery temperature conditions, polyolefin separators are prone to significant thermal shrinkage or even melting, thereby increasing the risk of direct contact between the positive and negative electrodes and thermal runaway.
[0004] Polyimide materials possess high heat resistance and good mechanical properties; therefore, constructing high-temperature resistant separators using polyimide nanofibers has become one of the technical approaches to improve the safety of lithium-ion batteries. However, pure polyimide nanofiber separators still suffer from limited surface functionality and unstable interfacial bonding between the coating and the fiber skeleton after further functionalization.
[0005] To impart flame-retardant properties to diaphragms, existing technologies typically incorporate phosphorus-based flame retardants, metal hydroxides, silicon-containing flame retardants, or other inorganic flame retardants into the diaphragm substrate or surface coating. Among these, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) exhibits good phosphorus-containing flame-retardant properties; aluminum hydroxide can absorb heat and release moisture during heating, while simultaneously providing an inorganic barrier effect. Therefore, both DOPO and aluminum hydroxide can be used to improve the flame-retardant properties of polymer materials.
[0006] However, adding flame retardants to polymer coatings through simple physical blending often presents the following problems: On the one hand, flame retardants, especially low-molecular-weight phosphorus-containing flame retardants, may migrate or precipitate during long-term electrolyte wetting, causing flame retardant performance to decrease over time and potentially adversely affecting the battery interface; on the other hand, when a large amount of inorganic flame retardant particles are added, particle agglomeration is likely to occur, which may also block the membrane pores, reducing the membrane porosity, electrolyte absorption performance, and ion transport performance. Furthermore, the functional coating and the porous fiber skeleton are usually connected primarily through physical adsorption, mechanical interlocking, or ordinary adhesives. Under battery winding, charge-discharge cycles, thermal shock, or external mechanical stress, the flame retardant coating is prone to microcracks, and in severe cases, local delamination may occur. Traditional flame retardant coatings typically lack the ability to actively repair existing microcracks. Once the coating continuity is disrupted, its flame retardant, interface protection, and thermal stability effects may all decrease.
[0007] Therefore, there is a need to provide a new lithium-ion battery separator structure that can solve the problems that traditional composite separators are prone to during thermo-mechanical cycling, such as coating delamination, difficulty in repairing microcracks, flame retardant migration, and flame retardant filler blockage, without significantly sacrificing lithium-ion transport performance. Summary of the Invention
[0008] This invention aims to solve the above-mentioned problems by providing a flame-retardant self-healing composite separator for lithium-ion batteries and its preparation method. PI / PMMA blended nanofibers serve as a porous support framework. A stable interface is constructed through fiber surface activation and silane coupling. An inner self-healing layer, primarily composed of a dynamic disulfide bond network, and an outer flame-retardant layer, primarily composed of covalent DOPO phosphorus-containing units and nano-aluminum hydroxide, are sequentially formed on the surface. This allows for layered configuration of different functions along the thickness direction, thereby achieving a balance between thermal stability, interface stability, flame retardancy, ion transport performance, and self-healing capability after damage.
[0009] The technical solution to the problem solved by this invention is:
[0010] First, a composite lithium-ion battery separator with self-healing and flame-retardant functions is provided, comprising: a PI / PMMA blended nanofiber skeleton, a silane interface structure formed on the surface of the PI / PMMA blended nanofiber skeleton, and a PMMA-based functional coating formed on the outside of the silane interface structure.
[0011] The surface of the PI / PMMA blended nanofiber skeleton has oxygen-containing active groups, and the silane coupling agent in the silane interface structure forms a chemical connection with the fiber surface having the oxygen-containing active groups after hydrolysis and condensation.
[0012] The PMMA-based functional coating comprises a polymer network and nano-Al(OH)3 dispersed in the polymer network;
[0013] The polymer network is formed by co-polymerization of methyl methacrylate and at least one functional polymerizable monomer, and includes methyl methacrylate-derived structural units, interfacial reaction units, dynamic disulfide bond crosslinking nodes, and phosphorus-containing units.
[0014] The functional polymerizable monomer includes at least an interfacial reactive monomer for forming the interfacial reactive unit, a disulfide-containing multifunctional polymerizable monomer for forming the dynamic disulfide bond crosslinking node, and a DOPO derivative having polymerizable unsaturated groups for forming the phosphorus-containing unit.
[0015] The interfacial reaction unit forms a chemical connection with the organic functional groups of the silane coupling agent;
[0016] The PMMA-based functional coating includes at least a self-healing layer and a flame-retardant layer in sequence along the direction away from the PI / PMMA blended nanofiber skeleton. The content of dynamic disulfide bond crosslinking nodes and interfacial reaction units in the self-healing layer is higher than the corresponding content in the flame-retardant layer. The content of phosphorus-containing units and nano-Al(OH)3 in the flame-retardant layer is higher than the corresponding content in the self-healing layer.
[0017] PI / PMMA blended nanofiber framework
[0018] The PI / PMMA blended nanofiber framework serves as the porous support for the entire composite membrane, formed by the interlocking stacking of PI / PMMA blended nanofibers. In the preparation process, polyamic acid (PAA) and PMMA are first blended in the same spinning solution. The resulting blended spinning solution is then electrospun to form PAA / PMMA blended nanofibers, followed by gradient thermal imidization to at least partially convert PAA into PI. This process retains both PI and PMMA components in the resulting blended nanofibers. The PI component primarily provides heat resistance, mechanical support, and resistance to heat shrinkage; the PMMA component enhances the material compatibility between the blended nanofibers and subsequent PMMA-based functional coatings, and improves electrolyte wetting and ion transport properties.
[0019] Preferably, the thickness of the PI / PMMA blended nanofiber framework is 5–40 μm; more preferably 10–25 μm; and even more preferably 12–20 μm. Before the formation of subsequent coatings, the porosity of the PI / PMMA blended nanofiber framework is 55%–80%; preferably 60%–75%; and even more preferably 65%–75%. These thickness and porosity ranges facilitate a balance between mechanical support, high-temperature dimensional stability, electrolyte retention, and lithium-ion transport within the blended nanofiber framework.
[0020] As a preferred embodiment of the present invention, the mass ratio of PI to PMMA is 4:1 to 1:1, based on the theoretical PI mass corresponding to complete imidization of PAA. In some preferred embodiments, PMMA accounts for 20% to 30% of the total mass of theoretical PI and PMMA. An appropriate amount of PMMA can improve the wetting and holding capacity of the blended nanofibers to the electrolyte and improve their compatibility with the PMMA-based functional coating; a higher PI proportion is beneficial for maintaining the heat resistance and high-temperature dimensional stability of the composite nanofiber skeleton. The above ratio is uniformly converted using the theoretical PI mass corresponding to complete imidization of PAA, and it is not required that the actual heat treatment achieves 100% imidization.
[0021] As a preferred embodiment of the present invention, the average diameter of the PI / PMMA blended nanofibers is 100–500 nm; preferably 150–350 nm; and more preferably 180–300 nm. If the blended nanofibers are too fine, the framework may become too dense and increase ion transport resistance; if they are too coarse, the specific surface area per unit mass and the effective working area of the subsequent silane interface structure may be reduced.
[0022] In the PI / PMMA blended nanofibers, the PI and PMMA components coexist within the blended fibers; they can form a microscopic blend structure or local phase regions, but are not required to be distributed in a completely uniform proportion in each fiber, nor are they required to form a homogeneous mixture at the molecular scale. Through blend spinning, the PMMA component is distributed within the blended nanofiber framework, rather than forming independent PMMA fiber layers only on the surface of the framework, thereby reducing the possibility of new weak interfaces forming between different fiber layers.
[0023] The blended nanofiber structure enables the composite of a heat-resistant PI component and a PMMA component with good interfacial compatibility at the fiber scale: the PI component provides the heat-resistant load-bearing foundation, while the PMMA component helps to mitigate the abrupt changes in material properties between the blended nanofiber skeleton and the outer PMMA-based functional coating, and can improve the coating bonding stability through limited swelling, segment compatibility, and interfacial interdiffusion. The maximum temperature of gradient thermal imidization is preferably controlled within a range that does not significantly cause thermal degradation of PMMA, so as to balance the imidization conversion of PAA and the retention of PMMA component.
[0024] As a preferred embodiment of the present invention, the PI / PMMA blended nanofiber skeleton is subjected to surface activation treatment, so that oxygen-containing active groups are formed on the fiber surface exposed on the surface of the composite skeleton and the near-surface region, providing reaction sites for the subsequent formation of silane interface structures.
[0025] Silane interface structure
[0026] Silane interface structures are mainly used to establish stable cross-interfacial chemical connections between the PI / PMMA blended nanofiber framework and the outer PMMA-based functional coating.
[0027] The silane interface structure is primarily formed based on a silane coupling agent. This silane coupling agent is a bifunctional silane coupling agent having a hydrolyzable silane group and an organic functional group capable of reacting with interfacial reactive units in a subsequent PMMA-based functional coating. For example, the silane coupling agent may be selected from at least one of aminosilanes, epoxysilanes, mercaptosilanes, and silanes containing unsaturated double bonds.
[0028] As a preferred embodiment of the present invention, the silane coupling agent is an aminosilane coupling agent; for example, it may be selected from at least one of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane; preferably γ-aminopropyltriethoxysilane (KH-550). When KH-550 is used, its alkoxysilane end first undergoes hydrolysis in an aqueous system to form a silanol structure, which then forms a silicon-oxygen-containing coupling interface on the surface of the PI / PMMA blend nanofiber skeleton through condensation, self-condensation, and interfacial reaction with the surface-activated fiber surface. The organic side-chain amino group of KH-550 is retained on the outside of the coupling interface for further chemical connection with the interfacial reaction units in the subsequent PMMA-based functional coating.
[0029] PMMA-based functional coatings
[0030] A PMMA-based functional coating is formed on the outer side of the silane interface structure, with a polymer network formed by the co-polymerization of methyl methacrylate and at least one functional polymerizable monomer as the continuous organic phase, while also containing nano-Al(OH)3 inorganic flame-retardant components dispersed in the polymer network. By involving multiple functional polymerizable monomers in the formation of the PMMA-based polymer network, interfacial bonding, dynamic covalent cross-linking, and at least some flame-retardant functions are directly constructed within the same continuous polymer network.
[0031] As a preferred embodiment of the present invention, the total thickness of the PMMA-based functional coating is 1–6 μm; preferably 2–4 μm; and more preferably 2–3 μm. If the coating thickness is too small, it may be difficult to form a continuous and complete flame-retardant and self-healing functional layer; if the coating thickness is too large, it may increase lithium-ion transport resistance, reduce membrane porosity, and increase internal stress within the coating.
[0032] Polymer Network
[0033] Polymer networks are polymer networks that use methyl methacrylate-derived structural units as the main polymer chain structural units and further include one or more functional polymerizable monomers.
[0034] Methyl methacrylate (MDMA) is the monomer-derived structural unit that constitutes the largest proportion of the polymer network. Unless otherwise stated, when this specification refers to the mass fraction range of each polymerizable organic component in a PMMA-based functional coating, it refers to the overall composition calculated by combining the polymerizable organic components in the self-healing layer and the flame-retardant layer according to their actual usage.
[0035] As a preferred embodiment of the present invention, based on 100 parts by mass of all polymerizable organic components forming the polymer network in the PMMA-based functional coating, the methyl methacrylate comprises 60-75 parts; preferably 62-72 parts; and more preferably 65-70 parts. The local composition of each functional layer can be adjusted according to its dominant function.
[0036] The functional polymerizable monomers include at least an interfacial reactive monomer for forming the interfacial reactive unit, a disulfide-containing polyfunctional polymerizable monomer for forming the dynamic disulfide crosslinking node, and a DOPO derivative having polymerizable unsaturated groups for forming the phosphorus-containing unit. These functional polymerizable monomers participate in polymerization with methyl methacrylate, making the interfacial reactive unit, dynamic disulfide crosslinking node, and phosphorus-containing unit integral parts of the polymer network.
[0037] Interface reaction unit
[0038] The interfacial reaction unit, as an interfacial connecting functional structure in the polymer network, is used to form a chemical connection with the organic functional groups of the silane coupling agent in the silane interfacial structure, thereby enabling the polymer network to establish a cross-interfacial chemical bridge with the PI / PMMA blended nanofiber skeleton through the silane coupling interface.
[0039] As a preferred embodiment of the present invention, when the silane coupling agent is an amino-containing silane coupling agent, the interfacial reaction monomer used to form the interfacial reaction unit is a polymerizable monomer containing an epoxy group; preferably, glycidyl methacrylate. The polymerizable double bond in glycidyl methacrylate can participate in free radical polymerization with methyl methacrylate and other functional polymerizable monomers to form the interfacial reaction unit. Its epoxy group can undergo a ring-opening reaction with the amino group of the amino-containing silane coupling agent, thereby forming a stable chemical connection between the silane coupling interface and the polymer network.
[0040] As a preferred embodiment of the present invention, based on 100 parts by mass of all polymerizable organic components forming the polymer network in the PMMA-based functional coating, the overall average addition amount of the interfacial reactive monomer is 3 to 8 parts, preferably 4 to 7 parts. The self-healing layer is close to the silane interface structure, and its local content of the interfacial reactive monomer can be higher than the aforementioned overall average content; the content of the interfacial reactive monomer in the flame-retardant layer can be relatively reduced. If the content of the interfacial reactive monomer is too low, the number of reaction sites available for forming chemical connections with the silane coupling interface may be insufficient; if the content is too high, it may alter the polarity, crosslinking state, and chain segment mobility of the polymer network.
[0041] Dynamic disulfide bond crosslinking nodes
[0042] Dynamic disulfide bond crosslinking nodes are formed inside the polymer network to establish reversible dynamic covalent connections containing disulfide bonds between different polymer chains. This allows PMMA-based functional coatings to reconnect local network structures through dynamic covalent bond exchange and polymer chain rearrangement after microcracks are generated under thermo-mechanical conditions.
[0043] The dynamic disulfide bond crosslinking nodes are formed by the polymerization of disulfide-bonded multifunctional polymerizable monomers, methyl methacrylate, and other functional polymerizable monomers. Each disulfide-bonded multifunctional polymerizable monomer possesses at least two polymerizable groups capable of participating in free radical polymerization and at least one disulfide bond structure, allowing it to be incorporated into different polymer chains during polymerization. This makes the disulfide bond a network crosslinking node connecting different polymer chains.
[0044] Preferably, the disulfide-bonded polyfunctional polymerizable monomer is a difunctional (meth)acrylate monomer containing disulfide bonds, wherein the two polymerizable (meth)acrylate groups are located on both sides of the disulfide bond structure. For example, in some embodiments, the disulfide-bonded polyfunctional polymerizable monomer is a dimethacrylate compound containing disulfide bonds. In other embodiments, the disulfide-bonded polyfunctional polymerizable monomer comprises an aromatic disulfide bond structure, with acrylate or methacrylate groups capable of participating in polymer network formation attached to both sides of the aromatic disulfide bond. An organic linker group formed by alkylene, ether, ester, carbamate, or combinations thereof may be further provided between the disulfide bond and the polymerizable group to adjust the segment flexibility, monomer compatibility, and network mechanical properties around the dynamic crosslinking nodes. Preferably, the disulfide-bonded polyfunctional polymerizable monomer is bis(4-methacryloyloxyphenyl)disulfide.
[0045] Its self-healing principle is as follows: After microcracks are generated in the coating, an appropriate temperature is applied to the composite membrane, which enhances the chain segment mobility of the polymer network on both sides of the crack and brings the dynamic disulfide bond structures closer together. Based on this, the original network connections are recombined through disulfide bond exchange reactions, and cross-chain dynamic covalent connections are re-established at the crack interface, thereby promoting the restoration of network continuity in the crack region. The self-healing process is jointly controlled by the dynamic disulfide bond exchange capacity and the polymer chain segment mobility.
[0046] As a preferred embodiment of the present invention, based on 100 parts by mass of all polymerizable organic components forming the polymer network in the PMMA-based functional coating, the average total amount of the disulfide-bonded polyfunctional polymerizable monomer is 2-5 parts, preferably 3-4 parts. The content of the disulfide-bonded polyfunctional polymerizable monomer in the self-healing layer can be higher than that in the flame-retardant layer to improve the dynamic network reconstruction capability near the skeleton region. If the content is too low, the number of dynamically formed disulfide bond crosslinking nodes may be insufficient; if the content is too high, it may lead to excessively high polymer network crosslinking density and restrict chain segment movement, thus hindering dynamic repair.
[0047] Phosphorus-containing units
[0048] The phosphorus-containing unit is a flame-retardant functional structure in the polymer network. It is formed by the polymerization of DOPO derivatives with polymerizable unsaturated groups, methyl methacrylate, and other functional polymerizable monomers, and is covalently bound to the polymer network. This reduces the possibility of migration, precipitation, or loss of free phosphorus-containing flame retardants during storage, electrolyte immersion, and battery operation. The phosphorus-containing unit, together with nano-Al(OH)3 dispersed in the polymer network as inorganic particles, constitutes an organic-inorganic composite flame-retardant system.
[0049] Preferably, in the DOPO derivative having polymerizable unsaturated groups, the polymerizable unsaturated groups can participate in free radical polymerization and can be selected from acrylate groups, methacrylate groups, or other vinyl unsaturated groups capable of copolymerizing with methyl methacrylate. The DOPO derivative participates in the construction of the polymer network through its polymerizable unsaturated groups, while the phosphorus-containing structure derived from DOPO is retained in the polymer chain or network structure formed after polymerization, thereby forming phosphorus-containing units covalently bonded in the polymer network. Preferably, the DOPO derivative having polymerizable unsaturated groups is a DOPO-based methacrylate monomer (the DOPO side group is connected to the methacrylate group via a methylene or aliphatic spacer group).
[0050] As a preferred embodiment of the present invention, based on 100 parts by mass of all polymerizable organic components forming the polymer network in the PMMA-based functional coating, the average total amount of the DOPO derivative with polymerizable unsaturated groups added is 10-20 parts, preferably 12-18 parts, and more preferably 14-18 parts. The local content of the DOPO derivative in the flame-retardant layer is preferably higher than that in the self-healing layer, so that the phosphorus-containing flame-retardant structure is mainly concentrated in the outer flame-retardant region. If the overall content of the DOPO derivative is too low, the improvement in flame-retardant performance is limited; if the content is too high, it may affect the polymerization reaction, network rigidity, chain segment mobility, and coating film-forming properties.
[0051] Nano Al(OH)3
[0052] Nano-Al(OH)3, as an inorganic flame retardant component in PMMA-based functional coatings, is dispersed in the polymer network in the form of inorganic particulate phases, and together with phosphorus-containing units formed by polymerization of DOPO derivatives with polymerizable unsaturated groups, it constitutes an organic-inorganic composite flame retardant system.
[0053] As a preferred embodiment of the present invention, the median particle size D50 of the nano-Al(OH)3 is 50–200 nm, preferably 50–150 nm, and more preferably 70–120 nm. Using nanoscale Al(OH)3 that matches the thickness of the PMMA-based functional coating facilitates the uniform dispersion of inorganic particles in the micron-scale functional coating and reduces localized protrusions, coating discontinuities, stress concentrations, and pore blockages caused by large-sized particles. Furthermore, if the nano-Al(OH)3 particle size is too small, its specific surface area and surface energy increase, potentially leading to increased particle agglomeration and a corresponding increase in the viscosity of the coating precursor solution. Therefore, it is preferable to select an appropriate particle size range that balances particle dispersibility, thin-film formation, and flame-retardant properties.
[0054] As a preferred embodiment of the present invention, based on 100 parts by mass of all polymerizable organic components forming the polymer network in the PMMA-based functional coating, the average total amount of nano-Al(OH)3 added is 3-8 parts, preferably 4-6 parts by mass. The nano-Al(OH)3 is preferably mainly distributed in the flame-retardant layer. The self-healing layer may not contain or may only contain a low amount of nano-Al(OH)3 to reduce the accumulation of inorganic particles near the porous framework. If the overall content of nano-Al(OH)3 is too low, its contribution to the composite flame-retardant system may be limited; if the content is too high, it can easily increase particle agglomeration, pore blockage, and adversely affect the movement of dynamic network segments.
[0055] As a preferred embodiment of the present invention, the nano-Al(OH)3 can be surface-organized to improve its dispersion stability in the PMMA-based functional coating precursor solution and the interfacial bonding between inorganic particles and the organic network. The surface modifier can be a silane coupling agent with polymerizable unsaturated groups; preferably, a silane coupling agent containing (meth)acryloyloxy; more preferably, γ-methacryloyloxypropyltrimethoxysilane, which forms an interfacial bond with the hydroxyl structure on the surface of nano-Al(OH)3 through its hydrolyzable silane end, and retains the polymerizable unsaturated groups on the outer side of the particles. During the formation of the polymer network, the polymerizable unsaturated groups on the particle surface can further participate in free radical polymerization, thereby enhancing the interfacial bonding between nano-Al(OH)3 and the polymer network and the particle fixation stability.
[0056] Optional flexible copolymer unit
[0057] The dynamic self-healing mechanism of this invention does not solely depend on the presence of dynamic disulfide bond crosslinking nodes. After microcracks form in the coating, the exchange of dynamic disulfide bonds and network reconstruction also require a certain degree of movement, contact, and rearrangement of polymer segments on both sides of the crack. When the chain segment mobility of the polymer network is insufficient, even if dynamic disulfide bond crosslinking nodes exist in the network, network reconnection in the crack region may still be limited. Therefore, in some preferred embodiments, the chain segment mobility of the polymer network is adjusted by introducing an appropriate amount of flexible copolymer units. This is mainly used to regulate the glass transition behavior of the polymer network, local chain segment flexibility, and chain segment mobility at a predetermined self-healing temperature, thereby providing favorable conditions for contact, rearrangement, and network reconnection after dynamic disulfide bond exchange at the crack interface.
[0058] As a preferred embodiment of the present invention, the flexible copolymer unit is formed from a polymerizable monomer capable of co-participating in free radical polymerization with methyl methacrylate and whose homopolymer has a relatively low glass transition temperature. For example, the flexible comonomer may be selected from at least one of ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate, preferably butyl acrylate.
[0059] As a preferred embodiment of the present invention, based on 100 parts by mass of all polymerizable organic components forming the polymer network in the PMMA-based functional coating, the amount of the flexible comonomer added is 2 to 20 parts, preferably 5 to 15 parts, and more preferably 8 to 12 parts. Excessive content of the flexible comonomer may reduce the polymer network modulus and high-temperature dimensional stability, and may increase the swelling tendency in the electrolyte environment, thereby negatively impacting the mechanical stability of the composite membrane and the integrity of the coating structure.
[0060] Self-healing layer and flame-retardant layer
[0061] The PMMA-based functional coating includes at least a self-healing layer and a flame-retardant layer in sequence along the direction away from the PI / PMMA blended nanofiber skeleton, so that the dynamic repair function and the flame-retardant function are configured in layers in the thickness direction.
[0062] The self-healing layer is located near the silane interface structure and is mainly used to restore network continuity through dynamic disulfide bond exchange and polymer segment rearrangement after microcracks or localized damage occur in the coating. The self-healing layer preferably has a relatively high content of dynamic disulfide bond crosslinking nodes and interfacial reactive units, and a relatively low content of phosphorus-containing units and nano-Al(OH)3. Thus, the self-healing layer can, on the one hand, improve the network reconstruction capability of the crack region by utilizing a high density of dynamic disulfide bonds, and on the other hand, form a stable cross-interfacial connection with the silane interface structure through a high content of interfacial reactive units.
[0063] As a preferred embodiment of the present invention, the thickness of the self-healing layer is 0.2–1.0 μm, preferably 0.3–0.8 μm.
[0064] The flame-retardant layer is located on the side of the self-healing layer away from the PI / PMMA blended nanofiber skeleton, and mainly serves to provide phosphorus-containing and inorganic flame-retardant functions. The content of phosphorus-containing units and nano-Al(OH)3 in the flame-retardant layer is higher than the corresponding content in the self-healing layer; at the same time, the flame-retardant layer may still contain a certain amount of dynamic disulfide bond crosslinking nodes to maintain the structural integrity of the outer functional layer after damage, but its content of dynamic disulfide bond crosslinking nodes is preferably lower than that of the self-healing layer.
[0065] As a preferred embodiment of the present invention, the thickness of the flame-retardant layer is 1.0–4.0 μm, preferably 1.2–3.0 μm. The thickness ratio of the self-healing layer to the flame-retardant layer is 1:3 to 1:5.
[0066] The self-healing layer and the flame-retardant layer are two adjacent functional layers with different dominant functions in the PMMA-based functional coating. They can form a identifiable compositional layering, but preferably, the polymer network remains continuous between the layers, and a transition interface can be formed through monomer diffusion, cross-layer copolymerization, or segment interdiffusion to avoid the formation of a new weak interface between the self-healing layer and the flame-retardant layer.
[0067] Secondly, another objective of this invention is to provide a method for preparing the composite lithium-ion battery separator with self-healing and flame-retardant functions, comprising the following steps:
[0068] S1. Polyamic acid and PMMA are blended and electrospun, and then subjected to gradient thermal imidization at a maximum processing temperature not exceeding 220°C, so that the polyamic acid is at least partially imidized to form PI component, thereby obtaining PI / PMMA blended nanofiber skeleton; subsequently, the PI / PMMA blended nanofiber skeleton is subjected to surface activation treatment to form oxygen-containing active groups on the fiber surface.
[0069] S2. The surface-activated PI / PMMA blended nanofiber framework is brought into contact with a hydrolyzed silane coupling agent and then dried to form the silane interface structure;
[0070] S3. A self-healing layer precursor liquid and a flame-retardant layer precursor liquid are sequentially applied to the surface of the PI / PMMA blended nanofiber skeleton treated with a silane coupling agent to form a coating precursor structure with a self-healing layer and a flame-retardant layer; then polymerization curing and heat post-treatment are performed.
[0071] Step S1
[0072] As a preferred embodiment of the present invention, pyromellitic dianhydride (PMDA) and 4,4'-diaminodiphenyl ether (ODA) are used as PI monomers, with their molar ratio controlled at approximately 1:1. A polyamic acid (PAA) precursor is synthesized in N,N-dimethylacetamide (DMAc) under dry nitrogen protection. Preferably, ODA is first dissolved in DMAc, and PMDA is added in batches at 0–5°C and reacted for 1–3 h. The reaction is then continued at room temperature for 6–18 h to obtain a PAA precursor with a solid content of approximately 12–18 wt%. PMMA with a weight-average molecular weight of 80,000–150,000 Da is added to the PAA precursor, and the mass ratio of PI to PMMA is adjusted to 4:1–1:1 based on the theoretical PI mass corresponding to complete imidization of PAA. DMAc is added as needed to bring the total polymer solid content of the blend spinning solution to 12–18 wt%. The blended spinning solution is electrospun, preferably at a spinning voltage of 18–20 kV, a receiving distance of approximately 18 cm, and a push rate of 0.8–1.0 mL / h, to obtain a PAA / PMMA blended nanofiber framework substrate. The blended nanofiber framework substrate is preferably first vacuum-dried at 50–70 °C for 4–8 h to remove residual DMAc, and then subjected to gradient thermal imidization under nitrogen protection. To balance PAA imidization with PMMA component retention, the maximum temperature for gradient thermal imidization is preferably 180–220 °C; in one specific method, the temperature is sequentially increased to 80 °C for 1 h, 120 °C for 1 h, 160 °C for 1 h, and 200 °C for 2 h at a heating rate of approximately 2 °C / min, followed by cooling to room temperature under nitrogen protection. This gradient heat treatment causes PAA to gradually dehydrate and cyclize to form the PI component, while limiting the maximum temperature reduces the possibility of significant thermal degradation of PMMA. The formation of characteristic absorption peaks of the imide ring and the weakening of PAA amide-related absorption peaks can be observed by infrared spectroscopy to confirm the iminoization conversion.
[0073] Surface activation methods can be varied, as long as they can increase oxygen-containing active groups on the fiber surface without significantly damaging the main structure of the nanofibers. For example, at least one of oxygen plasma treatment, air plasma treatment, UV / O3 treatment, and mild chemical oxidation treatment can be used. In some embodiments, oxygen plasma treatment is employed. The oxygen plasma treatment power is 20–150 W; preferably 30–80 W. The treatment time is 20–300 s; preferably 60–180 s. This controls the degree of surface activation, enabling the increase of silane reaction sites while avoiding over-activation that would lead to a significant decrease in fiber strength.
[0074] Step S2
[0075] As a preferred embodiment of the present invention, the silane coupling agent is added to an aqueous alcohol mixture for pre-hydrolysis, so that the surface-activated PI / PMMA blended nanofiber skeleton comes into contact with the pre-hydrolyzed silane coupling agent, so that the silane coupling agent is at least distributed and anchored on the surface and near-surface region of the composite nanofiber skeleton; then drying is performed, so that the silane coupling agent is hydrolyzed and condensed to form a stable silane interface structure.
[0076] The aqueous alcohol mixture is preferably an ethanol / water mixture with a volume ratio of ethanol to water of 80:20–98:2, preferably 90:10–95:5; the concentration of the silane coupling agent is 0.2–5 wt%, preferably 0.5–2 wt%; and the pH of the treatment solution is 4.0–6.0. The silane coupling agent is preferably pre-hydrolyzed for 10–60 min and then contacted with the PI / PMMA blended nanofiber framework for 3–30 min; after contact, it is preferably dried at 40–100°C.
[0077] Step S3
[0078] As a preferred embodiment of the present invention, a self-healing layer precursor liquid is first applied to the surface of a PI / PMMA blended nanofiber skeleton treated with silane coupling, and then partially prepolymerized or precured to form an inner self-healing layer while maintaining a certain level of reactivity; subsequently, a flame-retardant layer precursor liquid is applied, and then integrally polymerized and post-cured to form a continuous or transitional PMMA-based polymer network between the self-healing layer and the flame-retardant layer.
[0079] The self-healing layer precursor solution comprises at least methyl methacrylate, a polyfunctional polymerizable monomer containing disulfide bonds, and an interfacial reactive monomer, and may further comprise a flexible comonomer and a DOPO derivative having polymerizable unsaturated groups. The solid content of the self-healing layer precursor solution is preferably 5–10 wt%, and the thickness of the formed self-healing layer is preferably 0.3–0.8 μm.
[0080] The flame-retardant layer precursor liquid includes at least methyl methacrylate, a DOPO derivative with polymerizable unsaturated groups, and nano-Al(OH)3, and may further include polyfunctional polymerizable monomers containing disulfide bonds, flexible comonomers, and interfacial reactive monomers. The solid content of the flame-retardant layer precursor liquid is preferably 10–20 wt%, and the thickness of the formed flame-retardant layer is preferably 1.2–3.0 μm.
[0081] The polymerization is a free radical polymerization in which methyl methacrylate, interfacial reactive monomers, polyfunctional polymerizable monomers containing disulfide bonds, DOPO derivatives with polymerizable unsaturated groups, and optional flexible comonomers participate in the polymerization, and the self-healing layer and flame retardant layer form polymer networks and maintain chemical or physical continuity between the layers.
[0082] As a preferred embodiment of the present invention, the free radical polymerization can be carried out by photoinitiation, thermal initiation, or a combination of photoinitiation and thermal initiation. Photoinitiation is preferred for initial polymerization and structural fixation, followed by heat treatment to further complete the polymerization reaction and stabilize the chemical bonds between the silane interface structure and the interfacial reaction units.
[0083] The photopolymerization is preferably carried out using 365–405 nm ultraviolet or near-ultraviolet light; the amount of photoinitiator added is preferably 0.5–1.5 wt% of the total mass of the polymerizable organic components. The heat treatment temperature is preferably 70–130 °C, more preferably 90–110 °C, and the treatment time is preferably 15–30 min. During the polymerization curing and heat treatment, it is preferable not to apply pressure or only apply a slight pressure of 0–0.5 MPa to reduce the compaction of the pore structure of the PI / PMMA blended nanofiber framework. After the polymerization curing is completed, it is preferable to further dry under vacuum conditions at 60–80 °C for 6–12 h to remove residual solvent, moisture and unreacted small molecule components, thereby obtaining the composite lithium-ion battery separator with self-healing and flame-retardant functions.
[0084] The beneficial effects of this invention are:
[0085] In this invention, the PI / PMMA blended nanofiber framework is constructed by gradient thermal imidization of PAA and PMMA after blending and spinning, while maintaining the thermal stability of PMMA. This allows the PI and PMMA components formed by PAA imidization to coexist within the blended nanofiber framework, thus avoiding the formation of new interlayer interfaces caused by the superposition of independent PI and PMMA fiber layers. The PI component provides heat resistance and resistance to heat shrinkage, while the PMMA component improves electrolyte wetting and material compatibility with PMMA-based functional coatings. The oxygen-containing active groups on the fiber surface provide an anchoring basis for the silane coupling agent, which further reacts with the interfacial reaction units in the polymer network through its organic functional groups, thereby establishing a stable cross-interfacial chemical bond between the blended nanofiber framework and the PMMA-based functional coating.
[0086] Based on this, the present invention sequentially sets a self-healing layer and a flame-retardant layer along the direction away from the blended nanofiber skeleton. The inner self-healing layer increases the content of dynamic disulfide bond crosslinking nodes and interfacial reaction units, making it mainly responsible for repairing internal damage and stabilizing the interface of the coating; the outer flame-retardant layer increases the content of covalent DOPO phosphorus-containing units and nano-Al(OH)3, so that the flame-retardant components are concentrated in the outer thermal protection area, while reducing the possibility of high-content inorganic flame-retardant particles accumulating near the porous skeleton and blocking ion transport channels. Detailed Implementation
[0087] The following are specific embodiments of the present invention, and the technical solutions of the present invention will be further described, but the present invention is not limited to these embodiments.
[0088] DOPO derivatives (DOPO-propyl methacrylate) containing polymerizable unsaturated groups.
[0089] The DOPO-based propyl methacrylates involved in the following examples and comparative examples were prepared by the following method:
[0090] Under nitrogen protection, 1 mol of DOPO, 1.2 mol of allyl alcohol, and azobisisobutyronitrile (AIBN) were added to a reaction vessel, with the amount of AIBN being 0.8 wt% of the DOPO mass. The reaction system was heated to 70 °C and reacted for 12 h under stirring, allowing the PH group in DOPO to undergo a free radical addition reaction with the carbon-carbon double bond in allyl alcohol, generating a DOPO-propanol intermediate containing terminal hydroxyl groups. After the reaction, excess allyl alcohol and other volatile components were removed under reduced pressure. The crude product was purified by silica gel column chromatography using a petroleum ether / ethyl acetate mixture as the eluent to obtain the DOPO-propanol intermediate. 1 mol of the obtained DOPO-propanol intermediate was dissolved in anhydrous dichloromethane, and 1.3 mol of triethylamine and approximately 200 ppm of hydroquinone monomethyl ether relative to the total mass of the DOPO-propanol intermediate and methacryloyl chloride were added as a polymerization inhibitor. 1.2 mol of methacryloyl chloride was slowly added dropwise under nitrogen protection and at 0–5 °C. After the addition was complete, the reaction was continued at room temperature for 12 h. After the reaction was completed, the salt precipitate formed during the reaction was removed by filtration. The resulting filtrate was washed successively with saturated sodium bicarbonate aqueous solution, deionized water, and saturated sodium chloride aqueous solution. The organic phase was dried over anhydrous magnesium sulfate, filtered, and dichloromethane was removed under reduced pressure. The crude product was purified by silica gel column chromatography to obtain DOPO-propyl methacrylate.
[0091] Polymerizable monomer containing disulfide bonds [bis(4-methacryloyloxyphenyl)disulfide]
[0092] The bis(4-methacryloyloxyphenyl) disulfide involved in the following examples and comparative examples was prepared by the following method:
[0093] 1.00 g of bis(4-hydroxyphenyl) disulfide and 1.62 g of triethylamine were added to 20 mL of anhydrous acetonitrile and stirred under nitrogen protection to ensure complete dispersion or dissolution. The reaction system was cooled to approximately 0°C in an ice bath, and 1.67 g of methacryloyl chloride was slowly added dropwise with continuous stirring. After the addition was complete, the reaction system was heated to approximately 30°C and the reaction was continued for 24 h. After the reaction was completed, the acetonitrile was removed under reduced pressure, and the resulting residue was dissolved in chloroform and washed three times with 0.10 mol / L potassium carbonate aqueous solution, followed by three washes with deionized water. The resulting organic phase was dried over anhydrous magnesium sulfate, filtered, and the organic solvent was removed under reduced pressure. The crude product was recrystallized from ethanol and then dried under vacuum at 80°C for 24 h to obtain bis(4-methacryloyloxyphenyl) disulfide.
[0094] Example 1
[0095] A flame-retardant self-healing composite separator for lithium-ion batteries is prepared through the following steps:
[0096] S1. PAA precursors were prepared in DMAc using PMDA and ODA as PI monomers at a molar ratio of approximately 1:1. Specifically, ODA was dissolved in DMAc under nitrogen protection, and equimolar amounts of PMDA were added in batches at 0–5°C. After reacting at low temperature for 2 h, the reaction was continued at room temperature for 12 h to obtain a PAA precursor with a solid content of approximately 15 wt%. PMMA with a weight-average molecular weight of approximately 100,000 Da was used, and the ratio of the theoretical PI mass to PMMA mass corresponding to complete imidization of PAA was 70:30. PMMA was added to the PAA precursor and thoroughly stirred and blended. The total polymer solid content of the blending spinning solution was adjusted to approximately 15 wt% using DMAc. PAA / PMMA blended nanofiber framework substrates were prepared by electrospinning, with a spinning voltage of 19 kV, a receiving distance of 18 cm, and a liquid pushing rate of 0.9 mL / h. The resulting scaffold substrate was first vacuum-dried at 60 °C for 6 h, followed by gradient thermal imidization under nitrogen protection: the temperature was increased to 80 °C at a rate of approximately 2 °C / min and held for 1 h, then successively increased to 120 °C and held for 1 h, 160 °C and held for 1 h, and finally increased to 200 °C and held for 2 h, after which it was naturally cooled to room temperature under nitrogen protection. This gradient heat treatment imidized PAA and formed the PI component, while reducing the possibility of significant thermal degradation of PMMA at high temperatures, resulting in a PI / PMMA blended nanofiber scaffold. The obtained PI / PMMA blended nanofibers had an average diameter of approximately 250 nm, a total scaffold thickness of approximately 18 μm, and a porosity of approximately 70%.
[0097] The obtained PI / PMMA blended nanofiber framework was placed in an oxygen plasma treatment device and subjected to oxygen plasma treatment for 90 s at a power of 60 W to form oxygen-containing active groups on the surface of the blended nanofibers. Step S2 was performed immediately after the treatment to reduce the aging decay of the activated surface.
[0098] S2. Prepare a mixed solvent according to the volume ratio of ethanol:deionized water = 90:10, and add γ-aminopropyltriethoxysilane (KH-550) to the mixed solvent to make the concentration of KH-550 1.0 wt.
[0099] The pH of the resulting solution was adjusted to approximately 5.0 using acetic acid, and the solution was stirred at room temperature for 20 min to allow KH-550 to be pre-hydrolyzed.
[0100] The PI / PMMA blended nanofiber skeleton, which has been activated by oxygen plasma, was immersed in the above-mentioned KH-550 solution for 10 min. After being removed, excess liquid on the surface was removed, and the fiber was dried under vacuum at 70°C for 30 min. This allowed the hydrolyzed silane coupling agent to further condense and form a silane interface structure on the fiber surface.
[0101] S3. Based on 100 parts by mass of polymerizable organic components: 69 parts MMA, 12 parts BA, 8 parts GMA, 5 parts bis(4-methacryloyloxyphenyl) disulfide, and 6 parts DOPO-propyl methacrylate were mixed, and 0.8 wt% TPO-L was added as a photoinitiator relative to the above polymerizable organic components. A self-healing layer coating solution with a solid content of 8 wt% was prepared using THF. The obtained self-healing layer coating solution was applied to both sides of the KH-550-treated PI / PMMA blended nanofiber framework using a rapid blade coating method. THF was immediately and rapidly evaporated after coating to reduce excessive swelling of the PMMA component in the blended nanofibers by THF. The thickness of the resulting self-healing layer dry film on one side was controlled to be approximately 0.5 μm.
[0102] Under nitrogen protection conditions, an irradiation with a center wavelength of approximately 395 nm and an irradiation intensity of approximately 50 mW / cm² was used. 2 Irradiation with an LED light source for 3 seconds causes partial prepolymerization of the self-healing layer, while retaining some unreacted unsaturated groups to facilitate the formation of a continuous polymer network with the subsequent flame-retardant layer.
[0103] Based on 100 parts by mass of polymerizable organic components: 70 parts MMA, 6 parts BA, 2 parts GMA, 2 parts bis(4-methacryloyloxyphenyl) disulfide, and 20 parts DOPO-propyl methacrylate were mixed. Additionally, 6 parts of nano-Al(OH)3 (with a D50 of approximately 100 nm) relative to 100 parts by mass of the above organic components were added. 0.8 wt% TPO-L was added as a photoinitiator relative to the total mass of the polymerizable organic components, and THF was added to adjust the solid content of the coating solution to 15 wt%. The mixture was first dispersed using a high-speed shear disperser at approximately 6000 r / min for 10 min, followed by ultrasonic dispersion for 20 min to ensure uniform dispersion of the nano-Al(OH)3 in the coating solution. The resulting flame-retardant coating solution was applied to the outside of the pre-polymerized self-healing layer using a rapid blade coating method, and the THF was promptly evaporated and removed. The thickness of the dry film on one side of the resulting flame-retardant layer was controlled to be approximately 2.0 μm. The thickness ratio of the self-healing layer to the flame-retardant layer is approximately 1:4, and the total thickness of the two functional layers on one side is approximately 2.5 μm.
[0104] Under nitrogen protection conditions, an irradiation with a center wavelength of approximately 395 nm and an irradiation intensity of approximately 50 mW / cm² was used. 2 Irradiation with an LED light source for 60 seconds causes the methacrylate and acrylate unsaturated groups in the coating to undergo free radical polymerization, forming a continuous polymer network.
[0105] After photocuring, the resulting separator was subjected to heat treatment at 100°C for 20 min. During the heat treatment, a light pressure of approximately 0.1 MPa was applied to promote interfacial contact between the coating and the fiber skeleton and subsequent interfacial reactions, while avoiding over-compacting the fiber channels. Subsequently, it was dried under vacuum at 70°C for 8 h to obtain a flame-retardant self-healing composite separator for lithium-ion batteries.
[0106] Example 2
[0107] This embodiment is basically the same as that of Example 1, except that: bis(2-methacryloyloxyethyl) disulfide (DSDMA) of equal mass is used to replace bis(4-methacryloyloxyphenyl) disulfide in the self-healing layer and flame retardant layer of Example 1.
[0108] The composition, amount and preparation conditions of the remaining raw materials are the same as those in Example 1.
[0109] Example 3
[0110] This embodiment is basically the same as Embodiment 1, except that the nano-Al(OH)3 with added flame retardant layer is pre-modified with organic matter.
[0111] Specifically: 10 g of nano-Al(OH)3 was added to 200 mL of an ethanol / deionized water mixture, wherein the volume ratio of ethanol to deionized water was 90:10. The mixture was ultrasonically treated for 20 min to ensure thorough dispersion of the nano-Al(OH)3. 0.30 g of γ-methacryloyloxypropyltrimethoxysilane (KH-570) was added, and the pH of the system was adjusted to approximately 4.5–5.0 using acetic acid. The mixture was stirred at 50 °C for 2 h. After the reaction was complete, the solid product was separated by centrifugation or filtration, washed sequentially with ethanol and deionized water, and then dried under vacuum at 80 °C for 12 h to obtain KH-570 surface-modified organic nano-Al(OH)3. The obtained surface-modified nano-Al(OH)3 was used to replace the unmodified nano-Al(OH)3 in Example 1 by the same mass.
[0112] The composition, amount and preparation conditions of the remaining raw materials are the same as those in Example 1.
[0113] Example 4
[0114] This embodiment is basically the same as Embodiment 1, except that in step S1, the mass ratio of PI to PMMA is adjusted to 60:40 based on the theoretical PI mass corresponding to the complete imidization of PAA.
[0115] The composition, amount and preparation conditions of the remaining raw materials are the same as those in Example 1.
[0116] Example 5
[0117] This embodiment is basically the same as Embodiment 1, except that in step S1, the mass ratio of PI to PMMA is adjusted to 80:20 based on the theoretical PI mass corresponding to the complete imidization of PAA.
[0118] The composition, amount and preparation conditions of the remaining raw materials are the same as those in Example 1.
[0119] Comparative Example 1
[0120] This comparative example is basically the same as Example 1, except that: after oxygen plasma treatment in step S1, the KH-550 treatment in step S2 is not performed, and the coating preparation in step S3 is carried out directly.
[0121] The composition, amount and preparation conditions of the remaining raw materials are the same as those in Example 1.
[0122] Comparative Example 2
[0123] This comparative example is basically the same as Example 1, except that in the self-healing layer and flame retardant layer formulations in step S3, MMA of equal mass is used to replace GMA.
[0124] Specifically: the self-healing layer consists of 77 parts MMA, 12 parts BA, 5 parts bis(4-methacryloyloxyphenyl) disulfide and 6 parts DOPO propyl methacrylate; the flame retardant layer consists of 72 parts MMA, 6 parts BA, 2 parts bis(4-methacryloyloxyphenyl) disulfide and 20 parts DOPO propyl methacrylate.
[0125] The composition, amount and preparation conditions of the remaining raw materials are the same as those in Example 1.
[0126] Comparative Example 3
[0127] This comparative example is basically the same as Example 1, except that in the self-healing layer and flame-retardant layer formulations in step S3, ethylene glycol dimethacrylate (EGDMA) is used instead of bis(4-methacryloyloxyphenyl) disulfide.
[0128] Specifically: the self-healing layer uses 5 parts EGDMA instead of 5 parts bis(4-methacryloyloxyphenyl) disulfide; the flame retardant layer uses 2 parts EGDMA instead of 2 parts bis(4-methacryloyloxyphenyl) disulfide.
[0129] The composition, amount and preparation conditions of the remaining raw materials are the same as those in Example 1.
[0130] Comparative Example 4
[0131] This comparative example is basically the same as Example 1, except that in step S3, ordinary free DOPO is used instead of DOPO-propyl methacrylate, and the theoretical mass of phosphorus introduced into the two systems is basically the same.
[0132] Specifically: in Example 1, 6 parts of DOPO-based propyl methacrylate in the self-healing layer were replaced with 3.79 parts of ordinary free DOPO; in Example 1, 20 parts of DOPO-based propyl methacrylate in the flame-retardant layer were replaced with approximately 12.63 parts of ordinary free DOPO. To maintain a consistent total mass of organic components in each functional layer, the remaining mass was supplemented by MMA.
[0133] Therefore, the self-healing layer, based on 100 parts by weight of total organic components, includes: 71.21 parts MMA, 12 parts BA, 8 parts GMA, 5 parts bis(4-methacryloyloxyphenyl) disulfide, and 3.79 parts free DOPO; the flame-retardant layer, based on 100 parts by weight of total organic components, includes: 77.37 parts MMA, 6 parts BA, 2 parts GMA, 2 parts bis(4-methacryloyloxyphenyl) disulfide, and 12.63 parts free DOPO, with an additional 6 parts nano-Al(OH)3.
[0134] The composition, amount and preparation conditions of the remaining raw materials are the same as those in Example 1.
[0135] Comparative Example 5
[0136] This comparative example is basically the same as Example 1, except that: it does not form a functional layer of self-healing layer and flame retardant layer, but adopts a single PMMA-based functional coating with uniform overall composition.
[0137] Specifically, to ensure the overall composition of the uniform coating remains as consistent as possible with Example 1, the polymerizable organic components were weighted according to the target dry film thickness ratio of approximately 1:4 between the self-healing layer and the flame-retardant layer in Example 1. Based on 100 parts by mass of the total polymerizable organic components, 69.8 parts of MMA, 7.2 parts of BA, 3.2 parts of GMA, 2.6 parts of bis(4-methacryloyloxyphenyl) disulfide, and 17.2 parts of DOPO-propyl methacrylate were mixed; additionally, 4.8 parts of nano-Al(OH)3 relative to the above 100 parts by mass of polymerizable organic components were added, along with 0.8 wt% of TPO-L as a photoinitiator relative to the polymerizable organic components. The coating liquid-solid content was adjusted to 12 wt% using THF, and the nano-Al(OH)3 was subjected to high-speed shearing and ultrasonic dispersion using the same method as in Example 1.
[0138] The uniformly composed coating solution was rapidly coated onto both sides of the PI / PMMA blend nanofiber framework treated with KH-550 in a single application, and THF was promptly evaporated to remove it. The total thickness of the dry film on each side was controlled to be approximately 2.5 μm.
[0139] Under nitrogen protection conditions, the center wavelength was approximately 395 nm and the irradiation intensity was approximately 50 mW / cm². 2 Irradiated with an LED light source for 60 s, followed by heat treatment at 100℃ for 20 min, and dried under vacuum at 70℃ for 8 h to obtain a uniform PMMA-based functional coating composite membrane without thickness gradient.
[0140] Performance testing
[0141] Self-repair
[0142] The diaphragms obtained in the examples and comparative examples were cut into 20 mm × 20 mm samples. Artificial micro-scratches were prepared on the surface of the PMMA-based functional coating using a micro-scratcher. To enable the test to evaluate the effect of the inner self-healing layer on the overall crack recovery, the scratch load was calibrated through a pre-experiment, so that the scratch extended from the outer flame-retardant layer inward and into the self-healing layer, but did not penetrate the PMMA-based functional coating and damage the PI / PMMA blend nanofiber skeleton. For the sample with a total thickness of approximately 2.5 μm for one side of the functional coating in Example 1, the scratch depth was controlled to be approximately 2.1–2.3 μm, the scratch speed to be approximately 1 mm / s, and the scratch length to be approximately 5 mm. The scratch depth was confirmed and the scratch area before repair was recorded using a laser confocal microscope. The scratch area was measured using image analysis software and recorded as A0. Subsequently, the sample was placed in an 80°C oven and treated for 12 h without external mechanical load. After treatment, it was cooled to room temperature, and the scratch area was re-observed at the same position and magnification. The repaired scratch area was measured and recorded as At. The self-repair rate η is calculated according to the following formula: η=(A0-At) / A0×100%.
[0143] Interface adhesion (tape-assisted 180° peel)
[0144] A tape-assisted 180° peel test was used. The composite diaphragm to be tested was cut into strips 15 mm wide and 100 mm long. The diaphragm was fixed on a clean glass plate with the PMMA functional coating to be tested facing upwards. A standard pressure-sensitive tape with the same width as the diaphragm was pasted onto the coating surface, and a 2 kg roller was used to roll it back and forth three times along the tape direction. The free end of the tape was fixed to the upper clamp of a universal testing machine, and the test was conducted in a 180° peel direction with a peel speed set at 20 mm / min. The unstable region at the beginning of the peel was discarded, and the average peel force F in the intermediate stable peel range was recorded. The apparent peel strength per unit width was calculated according to P=F / b, where P is in N / m, F is the average peel force, and b is the effective width of the sample. After the test, the failure location was observed to confirm the differences in coating adhesion between different samples under the same test conditions.
[0145] Ion transport
[0146] The apparent ionic conductivity of the composite membrane under electrolyte-wetting conditions was determined using AC impedance spectroscopy. The membrane was cut into discs with a diameter of approximately 15.9 mm, and its actual thickness L was measured. A 1.0 mol / L LiPF6 EC / DMC mixed electrolyte was used as the test electrolyte, with a volume ratio of EC to DMC of 1:1. The membrane discs were immersed in the electrolyte for 30 min in an argon-protected glove box to ensure thorough wetting. The wetted membrane was then sandwiched between two stainless steel electrodes and assembled into a CR2032 type SS / membrane / SS barrier symmetric cell. AC impedance spectroscopy was performed at 25 °C using an electrochemical workstation, with a test frequency range of 1 MHz to 1 Hz and an AC perturbation voltage of 10 mV. The bulk resistance Rb of the membrane / electrolyte system was determined by the intersection of the high-frequency region and the real axis of the obtained Nyquist curve. The apparent ionic conductivity σ of the diaphragm is calculated using the following formula: σ = L / (Rb × A). Where: σ is the ionic conductivity, in S / cm; L is the diaphragm thickness, in cm; Rb is the bulk resistance, in Ω; and A is the effective contact area between the stainless steel electrode and the diaphragm, in cm². 2 .
[0147] Flame retardant
[0148] The flame-retardant properties of composite membranes were evaluated using the limiting oxygen index (LOI) method. The membranes to be tested were cut into strips 20 mm wide and 200 mm long. Multiple layers of identical samples were neatly stacked to achieve a total thickness of approximately 0.10 mm, and the stacked samples were then rolled into rolls suitable for the limiting oxygen index test. The resulting samples were mounted in a limiting oxygen index tester and subjected to combustion tests in a mixed atmosphere of oxygen and nitrogen. By gradually adjusting the oxygen volume fraction, the minimum oxygen concentration at which the sample could maintain the specified combustion behavior was determined, and this minimum oxygen volume fraction was recorded as the limiting oxygen index (LOI), expressed as a volume percentage.
[0149] The diaphragm was immersed in the aforementioned 1 mol / L LiPF6 / EC:DMC=1:1 electrolyte and soaked at 25°C for 24 h. After removal, the surface was quickly rinsed with DMC and vacuum dried at 60°C for 12 h. The LOI was then measured using the same method.
[0150] Heat shrinkage
[0151] The diaphragm to be tested was cut into 50 mm × 100 mm rectangular specimens, and the test directions were marked along the longitudinal (MD) and transverse (TD) directions, respectively. The initial length LMD,0 and initial length LTD,0 of the specimens in the MD direction were measured before heat treatment. The specimens were placed flat on a heat-resistant substrate without tension and placed in a preheated oven at 150°C for 1 h. After heat treatment, the specimens were removed and allowed to cool naturally at room temperature for 30 min. The lengths LMD,1 and LTD,1 in the MD and TD directions were measured again. The heat shrinkage rate SMD in the MD direction was calculated using the following formula: SMD = (LMD,0 - LMD,1) / LMD,0 × 100%. The heat shrinkage rate STD in the TD direction was calculated using the following formula: STD = (LTD,0 - LTD,1) / LTD,0 × 100%.
[0152] The test results are shown in Table 1 below:
[0153] sample Self-repair rate / % Peel strength (N / m) Initial LOI / % LOI / % after soaking Ionic conductivity (mS / cm) 150℃×1 h heat shrinkage rate MD / TD / % Example 1 92 275 30.8 30.1 1.48 1.4 / 1.2 Example 2 87 268 30.6 29.9 1.50 1.4 / 1.2 Example 3 90 286 31.7 31.0 1.55 1.3 / 1.1 Example 4 90 278 29.8 29.1 1.62 1.9 / 1.6 Example 5 91 270 31.2 30.5 1.20 1.1 / 0.9 Comparative Example 1 91 118 30.5 29.8 1.50 1.5 / 1.3 Comparative Example 2 90 165 30.4 29.7 1.52 1.5 / 1.3 Comparative Example 3 12 271 30.5 29.8 1.44 1.4 / 1.2 Comparative Example 4 91 267 30.3 26.2 1.43 1.5 / 1.3 Comparative Example 5 87 218 30.4 29.7 1.08 1.5 / 1.3
[0154] Based on the above test results, it is evident that the functional structures of this invention have a clear division of labor and synergistic relationship. Examples 1 and 2 both used dynamic crosslinking agents containing disulfide bonds, and their self-healing rates were both higher than 85%. However, Comparative Example 3, which used the common permanent crosslinking agent EGDMA, showed a significantly lower self-healing rate, indicating that the dynamic disulfide bond crosslinking nodes are key to the coating's thermally induced damage repair. Example 1, using an aromatic disulfide bond crosslinking agent, exhibited a relatively higher self-healing rate. The apparent peel strength of Example 1 was significantly higher than that of Comparative Example 1 without KH-550 and Comparative Example 2 without GMA, indicating that the silane interface structure and interface reaction units together improved the interfacial stability between the blended nanofiber skeleton and the PMMA-based functional coating. Example 1 and Comparative Example 4, which used free DOPO, showed relatively limited differences in initial LOI, but Example 1 maintained a higher LOI after electrolyte immersion, indicating that covalently introducing DOPO into the network as a polymerizable monomer is beneficial for reducing the migration or loss of phosphorus-containing flame-retardant components and improving the retention of flame-retardant function. Compared to Comparative Example 5, which has a similar overall composition but lacks functional stratification, Example 1 exhibits higher apparent peel strength and ionic conductivity while maintaining a similar initial flame retardant level. This indicates that primarily configuring dynamic disulfide bonds and interfacial reaction units in the inner self-healing layer, and primarily configuring DOPO and nano-Al(OH)3 in the outer flame-retardant layer, helps reduce the enrichment of high-content flame-retardant fillers near the porous framework and achieves a better overall balance between interfacial stability, self-healing, flame retardancy, and ion transport. Examples 4 and 5 further demonstrate that increasing the PMMA ratio improves ion transport performance, while increasing the PI ratio improves high-temperature dimensional stability; a 70:30 PI / PMMA ratio achieves better overall performance.
[0155] The specific embodiments described herein are merely illustrative of the spirit of the invention. Those skilled in the art to which this invention pertains may make various modifications or additions to the described specific embodiments or use similar methods to substitute them, without departing from the spirit of the invention or exceeding the scope defined by the appended claims.
Claims
1. A flame-retardant self-healing composite separator for lithium-ion batteries, characterized in that: It includes a PI / PMMA blended nanofiber framework, a silane interface structure formed on the surface of the PI / PMMA blended nanofiber framework, and a PMMA-based functional coating formed on the outside of the silane interface structure. The surface of the PI / PMMA blended nanofiber skeleton has oxygen-containing active groups, and the silane coupling agent in the silane interface structure forms a chemical connection with the fiber surface having the oxygen-containing active groups after hydrolysis and condensation. The PMMA-based functional coating comprises a polymer network and nano-Al(OH)3 dispersed in the polymer network; The polymer network is formed by co-polymerization of methyl methacrylate and at least one functional polymerizable monomer, and includes methyl methacrylate-derived structural units, interfacial reaction units, dynamic disulfide bond crosslinking nodes, and phosphorus-containing units. The functional polymerizable monomer includes at least an interfacial reactive monomer for forming the interfacial reactive unit, a disulfide-containing multifunctional polymerizable monomer for forming the dynamic disulfide bond crosslinking node, and a DOPO derivative having polymerizable unsaturated groups for forming the phosphorus-containing unit. The interfacial reaction unit forms a chemical connection with the organic functional groups of the silane coupling agent; The PMMA-based functional coating includes at least a self-healing layer and a flame-retardant layer in sequence along the direction away from the PI / PMMA blended nanofiber skeleton. The content of dynamic disulfide bond crosslinking nodes and interfacial reaction units in the self-healing layer is higher than the corresponding content in the flame-retardant layer. The content of phosphorus-containing units and nano-Al(OH)3 in the flame-retardant layer is higher than the corresponding content in the self-healing layer.
2. The flame-retardant self-healing composite separator for lithium-ion batteries according to claim 1, characterized in that: The PI / PMMA blended nanofiber skeleton is formed by the interleaved stacking of PI / PMMA blended nanofibers formed by electrospinning and imidization of a blended spinning solution containing polyamic acid and PMMA. The PI / PMMA blended nanofibers contain both PI and PMMA components formed by imidization of polyamic acid. Based on the theoretical PI mass corresponding to the complete imidization of polyamic acid, the mass ratio of PI to PMMA is 4:1 to 1:
1.
3. The flame-retardant self-healing composite separator for lithium-ion batteries according to claim 2, characterized in that: The average diameter of the PI / PMMA blended nanofibers is 100–500 nm.
4. The flame-retardant self-healing composite separator for lithium-ion batteries according to claim 1, characterized in that: The silane coupling agent in the silane interface structure is an aminosilane coupling agent; the interface reaction monomer used to form the interface reaction unit is a polymerizable monomer containing an epoxy group.
5. The flame-retardant self-healing composite separator for lithium-ion batteries according to claim 4, characterized in that: The aminosilane coupling agent is γ-aminopropyltriethoxysilane; the epoxy-containing polymerizable monomer is glycidyl methacrylate.
6. The flame-retardant self-healing composite separator for lithium-ion batteries according to claim 1, characterized in that: Based on 100 parts by mass of all polymerizable organic components forming the polymer network in the PMMA-based functional coating, the composition includes: 60-75 parts of methyl methacrylate, 3-8 parts of interfacial reactive monomers, 2-5 parts of polyfunctional polymerizable monomers containing disulfide bonds, 10-20 parts of DOPO derivatives with polymerizable unsaturated groups, and the remainder being other polymerizable organic components; and based on the 100 parts by mass of polymerizable organic components, nano-Al(OH)3 comprises 3-8 parts.
7. The flame-retardant self-healing composite separator for lithium-ion batteries according to claim 6, characterized in that: The other polymerizable organic components include butyl acrylate.
8. A flame-retardant self-healing composite separator for lithium-ion batteries according to claim 1 or 6, characterized in that: The disulfide-containing polyfunctional polymerizable monomer is bis(4-methacryloyloxyphenyl) disulfide.
9. The flame-retardant self-healing composite separator for lithium-ion batteries according to claim 1, characterized in that: The thickness ratio of the self-healing layer to the flame-retardant layer is 1:3 to 1:5; the total thickness of the PMMA-based functional coating is 2 to 4 μm.
10. A method for preparing a flame-retardant self-healing composite separator for lithium-ion batteries as described in any one of claims 1 to 9, characterized in that, Includes the following steps: S1. Polyamic acid and PMMA are blended and electrospun, and then subjected to gradient thermal imidization at a maximum processing temperature not exceeding 220°C, so that the polyamic acid is at least partially imidized to form PI component, thereby obtaining PI / PMMA blended nanofiber skeleton; subsequently, the PI / PMMA blended nanofiber skeleton is subjected to surface activation treatment to form oxygen-containing active groups on the fiber surface. S2. The surface-activated PI / PMMA blended nanofiber framework is brought into contact with a hydrolyzed silane coupling agent and then dried to form the silane interface structure; S3. A self-healing layer precursor liquid and a flame retardant layer precursor liquid are sequentially applied to the surface of the PI / PMMA blended nanofiber skeleton treated with silane coupling agent to form a coating precursor structure that sequentially includes a self-healing layer and a flame retardant layer. Then, polymerization, curing, and post-heat treatment are carried out.