A high-power device and its fabrication method
By employing a dual-channel structure and an arrayed nanochannel structure in high-power radio frequency devices, and utilizing a high thermal conductivity material layer to achieve rapid heat dissipation, the problem of internal heat accumulation in the device is solved, current density and output power are improved, and the reliability and current collapse characteristics of the device are ensured.
Patent Information
- Application Number
- CN202611610898.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-17
AI Technical Summary
While increasing current density, existing high-power radio frequency devices struggle to effectively address the issue of internal heat accumulation, thus hindering performance improvement.
By employing a dual-layer channel structure and an arrayed nanochannel structure, and filling the space between the nanochannels with a layer of high thermal conductivity material, a high thermal conductivity material layer is formed to make close contact with the conductive channel, thereby achieving rapid heat dissipation and increasing the current density without affecting the passivation effect.
It significantly improves the current density and heat dissipation performance of the device, reduces the operating junction temperature, and enhances the output power and reliability of the device, while taking into account both current collapse characteristics and stability under high power conditions.
Smart Images

Figure CN123124393A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of microelectronics technology, specifically relating to a high-power device and its fabrication method. Background Technology
[0002] Gallium nitride (GaN) semiconductors, with their wide bandgap characteristics such as high breakdown electric field and high electron mobility, have shown great application potential in high-power radio frequency devices and have therefore attracted widespread attention. However, as GaN materials and device processes mature and device output power continues to increase, the problem of internal heat accumulation becomes increasingly prominent, limiting further performance improvements.
[0003] In recent years, thermal management of high-power radio frequency (RF) devices has received considerable attention. A series of technologies, including high thermal conductivity heat sink materials, heterogeneous integration of high thermal conductivity substrates, heteroepitaxial growth of high thermal conductivity substrates, and passivation of high thermal conductivity materials, have been proposed to address the rapid heat dissipation problem of high-power RF devices. Research shows that high thermal conductivity heat sinks and heterogeneous integration of high thermal conductivity substrates can improve the steady-state heat dissipation performance of devices, but the heat transfer path is relatively long, limiting the improvement effect on instantaneous heat transfer within the device. Heteroepitaxial growth of high thermal conductivity substrates requires high substrate crystal quality and orientation, and this technology is limited by existing high thermal conductivity substrate growth techniques, making large-scale application difficult in the short term. Direct contact between the high thermal conductivity passivation layer material and the barrier layer results in poor passivation of dangling bonds on the barrier layer surface, affecting the current collapse characteristics of the device. Typically, a conventional passivation layer needs to be inserted between the high thermal conductivity passivation layer and the barrier layer, resulting in a large distance between the high thermal conductivity passivation layer and the conductive channel, leading to a large thermal resistance in the transmission path and affecting heat transfer efficiency.
[0004] For high-power devices, how to increase current density while not affecting the device passivation effect and current collapse characteristics, and solve the more serious heat accumulation problem caused by high power density, is a technical problem that has not yet been properly solved in the existing technology. Summary of the Invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.
[0006] Therefore, a first aspect of the present invention provides a high-power device.
[0007] A second aspect of the present invention provides a method for fabricating a high-power device.
[0008] In view of this, a high-power device is provided according to a first aspect of the embodiments of this application, comprising: The substrate layer, nucleation layer, buffer layer, second channel layer, second barrier layer, first channel layer, first barrier layer, cap layer and passivation layer are stacked in sequence. First n +Material layer, first n + The material layer penetrates the cap layer, the first barrier layer, the first channel layer, and the second barrier layer, the first n + The bottom of the material layer extends below the channel of the second channel layer; Source electrode, the source electrode is located at the first n + Above the material layer; Second n + Material layer, second n + The material layer penetrates the cap layer, the first barrier layer, the first channel layer, and the second barrier layer, and the second n + The bottom of the material layer extends below the channel of the second channel layer; Drain electrode, the drain electrode is located at the second n + Above the material layer; Arrayed nanochannel structures, the arrayed nanochannel structures are composed of a first n + Material layer and the second n + It consists of a second channel layer, a second barrier layer, a first channel layer, a first barrier layer, and a cap layer between material layers; A high thermal conductivity material layer is filled in the channel grooves of an arrayed nanochannel structure; Gate electrode, the gate electrode is located at the first n + Material layer and the second n + Between the material layers, the gate electrode is located above the arrayed nanochannel structure and the high thermal conductivity material layer.
[0009] In one feasible implementation, the material of the first barrier layer includes at least one selected from aluminum nitride (AlN), indium aluminum nitride (InAlN), scandium aluminum nitride (ScAlN), aluminum gallium nitride (AlGaN), and indium aluminum gallium nitride (InAlGaN); The material of the second barrier layer includes at least one of aluminum nitride (AlN), indium aluminum nitride (InAlN), scandium aluminum nitride (ScAlN), aluminum gallium nitride (AlGaN), and indium aluminum gallium nitride (InAlGaN).
[0010] In one feasible implementation, the arrayed nanochannel structure includes nanochannels that are uniformly distributed along the gate width direction of the gate electrode, and a channel groove is formed between two adjacent nanochannels.
[0011] In one feasible implementation, the width of the nanochannel is 20 nm to 20000 nm; the spacing between two adjacent nanochannels is 20 nm to 2000 nm.
[0012] In one feasible implementation, the thickness of the first channel layer is 10nm~60nm; the thickness of the second channel layer is 50nm~500nm.
[0013] According to a second aspect of the embodiments of this application, a method for fabricating a high-power device is provided, for fabricating a high-power device as described in any of the above technical solutions. The method for fabricating the high-power device includes: S1. A double-channel heterojunction material substrate is provided, the double-channel heterojunction material substrate comprising a substrate layer, a nucleation layer, a buffer layer, a second channel layer, a second barrier layer, a first channel layer, a first barrier layer and a cap layer stacked sequentially; a first mask layer is grown on the cap layer; S2. Define the ohmic regrowth region pattern on the first mask layer, etch the cap layer, the first barrier layer, the first channel layer, the second barrier layer and part of the second channel layer to form a first groove located in the source electrode region and a second groove located in the drain electrode region. S3, growing n in the first and second grooves + Material layer; S4. Remove the first mask layer to remove n outside the first and second grooves. + Material layer, retaining n in the first and second grooves + Material layer, forming the first n + Material layer and second n + Material layer; S5, Deposited passivation layer; S6, Remove the first n + Material layer and second n + A passivation layer covering the material layer; S7, Deposit the second mask layer; S8. Define a nanochannel pattern on the second mask layer, and etch the second mask layer, passivation layer, cap layer, first barrier layer, first channel layer, second barrier layer, and part of the second channel layer to form a nanochannel pattern located on the first n-channel layer. + Material layer and second n + Arrayed nanochannel structures between material layers; S9. Deposit a high thermal conductivity material layer, so that the high thermal conductivity material layer fills the channel groove of the arrayed nanochannel structure and covers the second mask layer. S10. Remove the second mask layer and the high thermal conductivity material layer covering the second mask layer, while retaining the high thermal conductivity material layer in the channel groove; S11, in the first n + The source electrode is fabricated on the material layer, and in the second n + Drain electrodes are fabricated on the material layer; S12. Define the gate electrode groove region pattern, etch the passivation layer, and form the gate electrode groove located between the source electrode and the drain electrode. S13. Fabricate a gate electrode at the gate electrode groove, so that the gate electrode is located at the first n + Material layer and second n +Between the material layers, and with the gate electrode positioned above the arrayed nanochannel structure and the high thermal conductivity material layer.
[0014] In one feasible implementation, when etching the second channel layer, the etching extends through the interface between the second barrier layer and the second channel layer, and below the depth where the channel of the second channel layer is located, so as to expose the channel of the second channel layer on the sidewall of the channel recess.
[0015] In one feasible implementation, a high thermal conductivity material layer is filled in the channel groove, the high thermal conductivity material layer is in direct contact with the sidewall of the arrayed nanochannel structure, and the high thermal conductivity material layer is adjacent to the channel of the second channel layer.
[0016] In one feasible implementation, the high thermal conductivity material layer and the passivation layer within the channel groove do not overlap in the vertical direction.
[0017] In one feasible implementation, a high thermal conductivity material layer is deposited within the trench and above the second mask layer. By removing the second mask layer, the high thermal conductivity material layer above the second mask layer is simultaneously peeled off, thereby retaining the high thermal conductivity material layer filling the trench.
[0018] The high-power device and its fabrication method disclosed in this application have the following advantages compared with the prior art: The high-power device provided in this application includes a substrate layer, a nucleation layer, a buffer layer, a second channel layer, a second barrier layer, a first channel layer, a first barrier layer, a cap layer, and a passivation layer, forming a double-channel heterojunction structure. High-concentration two-dimensional electron gases are formed at the interfaces of the two heterojunction layers, significantly increasing the total carrier density of the device and thus achieving a higher current density to meet high-power output requirements. + Material layer and second n + The material layers penetrate the cap layer, the first barrier layer, the first channel layer, and the second barrier layer, respectively, and extend to the bottom below the channel of the second channel layer. The source electrode and the drain electrode are located at the first n... + Material layer and second n + Above the material layer. The first n + Material layer and second n + The material layer is n +Heavily doped materials form low-resistance ohmic contacts with the second channel layer, effectively reducing the contact resistance between the source and drain electrodes and improving the device's conduction performance. The arrayed nanochannel structure composed of a double-layer channel structure can achieve high current density. By filling the arrayed nanochannel structure with a high thermal conductivity layer, the heat accumulated near the channel due to the high current density can be dissipated through the high thermal conductivity layer to other areas, effectively reducing the device's operating junction temperature and improving output power and efficiency. Furthermore, the high thermal conductivity layer fills the channel recesses of the arrayed nanochannel structure, with the gate electrode located in the first n... + Material layer and the second n + The material layers, located between the arrayed nanochannel structure and above the high thermal conductivity material layer, serve as continuous heat conduction channels, continuously dissipating heat outwards and diffusing it throughout the area covered by the high thermal conductivity material layer. This prevents heat accumulation in localized areas, achieving steady-state heat dissipation, reducing device operating temperature, and improving device reliability and output efficiency under high power conditions. This application improves current density through a dual-channel structure while simultaneously addressing the more severe heat accumulation problem caused by high power density by utilizing a high thermal conductivity material layer filled within the channel grooves of the arrayed nanochannel structure. This allows for synergistic optimization of heat dissipation and electrical performance, thereby comprehensively improving the device's output power, efficiency, and operational reliability under high power conditions. Furthermore, the high thermal conductivity material layer is selectively grown within the channel grooves between the nanochannels, without spatial overlap with the passivation layer. This significantly preserves the freedom in the passivation process above the barrier layer, facilitating excellent current collapse performance of the device. Attached Figure Description
[0019] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings: Figure 1 A schematic structural diagram of a high-power device from the first angle according to an embodiment of this application; Figure 2 for Figure 1 A schematic structural diagram of the AA surface; Figure 3 for Figure 1 A schematic structural diagram of the BB side; Figure 4 for Figure 1 A schematic structural diagram of the C-plane; Figure 5 A schematic flowchart illustrating the steps of a method for fabricating a high-power device according to an embodiment of this application; Figure 6a This is a schematic structural diagram of the double-channel heterojunction material substrate provided in S1' of Embodiment 1 of this application; Figure 6b This is a schematic structural diagram of growing a first mask layer on the cap layer in S1' of Embodiment 1 of this application; Figure 6c This is a schematic structural diagram of the etching of the first groove and the second groove in S2' of Embodiment 1 of this application; Figure 6d In embodiment S3' of this application, n is grown in the first groove and the second groove. + A schematic diagram of the material layer structure; Figure 6e To form the first n in S4' of Embodiment 1 of this application + Material layer and second n + A schematic diagram of the material layer structure; Figure 6f This is a schematic structural diagram of the passivation layer deposited in S5' of Embodiment 1 of this application; Figure 6g To remove the first n in S6' of Embodiment 1 of this application + Material layer and second n + A schematic structural diagram of the passivation layer covering the material layer; Figure 6h This is a schematic structural diagram of the deposition of the second mask layer in S7' of Embodiment 1 of this application; Figure 6i-1 This is a top view after defining the nanochannel pattern in S8' of Embodiment 1 of this application; Figure 6i-2 This is a cross-sectional view of BB after etching in S8' of Embodiment 1 of this application; Figure 6i-3 This is a cross-sectional view of the CC after etching in S8' of Embodiment 1 of this application; Figure 6j-1 This is a cross-sectional view of section AA after depositing a high thermal conductivity material layer in S9' of Example 1 of this application; Figure 6j-2 This is a cross-sectional view of BB after depositing a high thermal conductivity material layer in S9' of Embodiment 1 of this application; Figure 6j-3 This is a cross-sectional view of the C-section after depositing a high thermal conductivity material layer in S9' of Embodiment 1 of this application; Figure 6k-1 This is a cross-sectional view of AA after peeling in S10' of Embodiment 1 of this application; Figure 6k-2 This is a cross-sectional view of BB after peeling in S10' of Embodiment 1 of this application; Figure 6k-3This is a cross-sectional view of CC after peeling in S10' of Embodiment 1 of this application; Figure 6l-1 This is a top view of the source electrode and drain electrode after fabrication in S11' of Embodiment 1 of this application; Figure 6l-2 This is a cross-sectional view of the source electrode and drain electrode after fabrication in S11' of Example 1 of this application; Figure 6m-1 This is a top view after defining the gate electrode recess region in S12' of Embodiment 1 of this application; Figure 6m-2 This is a cross-sectional view of the gate electrode groove after etching in S12' of Embodiment 1 of this application; Figure 6m-3 This is a cross-sectional view of the gate electrode groove after etching in S12' of Embodiment 1 of this application; Figure 6n-1 This is a cross-sectional view of section AA after the gate electrode is fabricated in S13' of Example 1 of this application; Figure 6n-2 This is a cross-sectional view of BB after the gate electrode is fabricated in S13' of Example 1 of this application; Figure 6n-3 This is a cross-sectional view of the gate electrode after it has been fabricated in S13' of Example 1 of this application; in, Figures 1-4 , Figures 6a to 6n-3 The correspondence between the reference numerals and component names in the attached drawings is as follows: 1. Substrate layer; 2. Nucleation layer; 3. Buffer layer; 4. Second channel layer; 5. Second barrier layer; 6. First channel layer; 7. First barrier layer; 8. Cap layer; 9. First n + Material layer; 10, the second n + 11. Material layer; 12. Passivation layer; 13. High thermal conductivity material layer; 14. Source electrode; 15. Drain electrode; 16. Gate electrode; 80. First mask layer; 90. First groove; 100. Second groove; 101. Second mask layer; 103. Gate electrode groove; 111. Nanochannel; 112. Region between nanochannel patterns (channel groove); 123. Gate electrode groove region pattern. Detailed Implementation
[0020] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.
[0021] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.
[0022] In this application, unless otherwise expressly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.
[0023] The preferred embodiments of this application are described below with reference to the accompanying drawings. It should be understood that the preferred embodiments described herein are for illustration and explanation only and are not intended to limit this application.
[0024] like Figures 1 to 4 As shown, according to a first aspect of the embodiments of this application, a high-power device is proposed, comprising: a substrate layer 1, a nucleation layer 2, a buffer layer 3, a second channel layer 4, a second barrier layer 5, a first channel layer 6, a first barrier layer 7, a cap layer 8, and a passivation layer 11, sequentially stacked, and a first n + Material layer 9, source electrode 13, second n + Material layer 10, drain electrode 14, arrayed nanochannel structure 111, high thermal conductivity material layer 12, gate electrode 15; first n + Material layer 9 penetrates cap layer 8, first barrier layer 7, first channel layer 6, and second barrier layer 5, first n + The bottom of material layer 9 extends below the channel of the second channel layer 4; the source electrode 13 is located in the first n + Above material layer 9; the second n +Material layer 10 penetrates cap layer 8, first barrier layer 7, first channel layer 6, and second barrier layer 5, second n + The bottom of material layer 10 extends below the channel of the second channel layer 4; the drain electrode 14 is located in the second n + Above material layer 10; the arrayed nanochannel 111 structure consists of the first n + Material layer 9 and the second n + The material layers 10 are composed of a second channel layer 4, a second barrier layer 5, a first channel layer 6, a first barrier layer 7, and a cap layer 8; a high thermal conductivity material layer 12 is filled in the channel groove 112 of the arrayed nanochannel 111 structure; the gate electrode 15 is located in the first n + Material layer 9 and the second n + Between the material layers 10, and the gate electrode 15 is located above the arrayed nanochannel 111 structure and the high thermal conductivity material layer 12.
[0025] The high-power device provided in this application embodiment includes a substrate layer 1, a nucleation layer 2, a buffer layer 3, a second channel layer 4, a second barrier layer 5, a first channel layer 6, a first barrier layer 7, a cap layer 8, and a passivation layer 11, forming a double-channel heterojunction structure. High-concentration two-dimensional electron gases are formed at the interfaces of the two heterojunction layers, significantly increasing the total carrier density of the device and thus achieving a higher current density to meet high-power output requirements. + Material layer 9 and the second n + Material layer 10 penetrates cap layer 8, first barrier layer 7, first channel layer 6, and second barrier layer 5 respectively, and extends to the bottom below the channel of second channel layer 4. Source electrode 13 and drain electrode 14 are located at the first n + Material layer 9 and the second n + Above material layer 10. First n + Material layer 9 and the second n + Material layer 10 is n + Heavily doped material forms a low-resistance ohmic contact with the second channel layer 4, effectively reducing the contact resistance between the source electrode 13 and the drain electrode 14, and improving the device's conduction performance. The arrayed nanochannel 111 structure composed of a double-layer channel structure can achieve a high current density. By filling the arrayed nanochannel 111 structure with a high thermal conductivity material layer 12, the heat accumulated near the channel due to the high current density can be dissipated through the high thermal conductivity material layer 12 and diffused to other areas, effectively reducing the device's operating junction temperature and improving the device's output power and efficiency. Furthermore, the high thermal conductivity material layer 12 fills the channel recesses 112 of the arrayed nanochannel 111 structure, and the gate electrode 15 is located in the first n... + Material layer 9 and the second n +The material layers 10, located between the arrayed nanochannel 111 structure and above the high thermal conductivity material layer 12, serve as continuous heat conduction channels. They continuously conduct heat outwards and diffuse it throughout the area covered by the high thermal conductivity material layer 12, preventing localized heat accumulation, achieving steady-state heat dissipation, reducing device operating temperature, and improving device reliability and output efficiency under high power conditions. This application improves current density through a dual-channel structure while simultaneously addressing the more severe heat accumulation problem caused by high power density by utilizing the high thermal conductivity material layer 12 filled within the channel grooves 112 of the arrayed nanochannel 111 structure. This allows for synergistic optimization of heat dissipation and electrical performance, thereby comprehensively improving the device's output power, efficiency, and operational reliability under high power conditions.
[0026] The inventors discovered that in the prior art, high thermal conductivity material layers are typically disposed at the bottom of the device (e.g., on a high thermal conductivity substrate) or covered on the device surface (e.g., on a high thermal conductivity passivation layer). When the high thermal conductivity material layer is disposed at the bottom of the device, it is separated from the conductive channel (two-dimensional electron gas at the heterojunction interface) by multiple layers such as buffer layers and nucleation layers, resulting in a long heat transfer path and high thermal resistance. When the high thermal conductivity material layer is covered on the device surface, although it is close to the channel, direct contact with the barrier layer will affect the surface state passivation effect and deteriorate the current collapse characteristics. This application achieves close contact between the high thermal conductivity material layer 12 and the conductive channel by disposing of the high thermal conductivity material layer 12 within the channel groove 112 between the nanochannels 111, while avoiding direct contact with the surface of the barrier layer, thus balancing heat dissipation and passivation.
[0027] In one feasible implementation, the material of the first barrier layer 7 includes at least one of aluminum nitride (AlN), indium aluminum nitride (InAlN), scandium aluminum nitride (ScAlN), aluminum gallium nitride (AlGaN), and indium aluminum gallium nitride (InAlGaN); the material of the second barrier layer 5 includes at least one of aluminum nitride (AlN), indium aluminum nitride (InAlN), scandium aluminum nitride (ScAlN), aluminum gallium nitride (AlGaN), and indium aluminum gallium nitride (InAlGaN).
[0028] In this technical solution, heterojunctions are formed between the first barrier layer 7 and the first channel layer 6, and between the second barrier layer 5 and the second channel layer 4, respectively. High-concentration, high-mobility two-dimensional electron gas is generated at the interface of the two heterojunctions through polarization effects, serving as the conductive channel of the device. At least one of aluminum nitride (AlN), indium aluminum nitride (InAlN), scandium aluminum nitride (ScAlN), aluminum gallium nitride (AlGaN), and indium aluminum gallium nitride (InAlGaN) is selected as the barrier layer material to give the barrier layer a large bandgap and a strong polarization effect, thereby effectively improving the areal density and mobility of the two-dimensional electron gas, and thus enhancing the current density and output power of the device. Meanwhile, materials such as indium aluminum nitride (InAlN), scandium aluminum nitride (ScAlN), and indium aluminum gallium nitride (InAlGaN) are selected as barrier layer materials. The good lattice matching between the barrier layer and the corresponding channel layer is beneficial to reducing the interface defect density and carrier scattering, thereby improving the conduction characteristics and high-frequency performance of the device. Furthermore, the double-layer barrier structure can further improve the confinement effect on the two-dimensional electron gas, thereby enhancing the frequency and power characteristics of the device.
[0029] like Figure 1 As shown, in one feasible embodiment, the arrayed nanochannel 111 structure includes nanochannels 111, which are uniformly distributed along the gate width direction of the gate electrode 15, and a channel groove 112 is formed between two adjacent nanochannels 111.
[0030] In this technical solution, the arrayed nanochannel 111 structure, composed of a double-layer channel structure, forms a high-concentration two-dimensional electron gas at the interface of the two heterojunction layers through polarization effects, significantly increasing the total carrier density of the device and achieving a higher current density. Simultaneously, the channel grooves 112 between the nanochannels 111 provide filling space for high thermal conductivity material, allowing the material to be close to the conductive channel, thereby rapidly dissipating heat from the channel. Uniform distribution of the nanochannel 111 structure improves the uniformity of current density and heat distribution, avoiding localized current concentration and heat accumulation, thus enhancing the stability and reliability of the device under high-current operating conditions. By arranging multiple nanochannels 111 in parallel, with each channel sidewall surrounded by high thermal conductivity material, heat is simultaneously dissipated from multiple hot spots, rapidly diffusing and homogenizing laterally within the high thermal conductivity material layer 12 in the channel grooves 112, preventing overheating of any single channel and achieving rapid heat homogenization.
[0031] In one feasible implementation, the width W of the nanochannel 111 ch =20nm~20000nm; the spacing between two adjacent nanochannels 111 is 20nm~2000nm.
[0032] In this technical solution, the dual-channel structure generates a high-concentration two-dimensional electron gas at the interface of the two heterojunctions through polarization effects, significantly improving the total carrier density of the device and achieving a higher current density. Based on this, by controlling the width of the nanochannels 111 within the range of 20 nm to 20000 nm, and the spacing between adjacent nanochannels 111 within the range of 20 nm to 2000 nm, i.e., controlling the width of the channel recesses 112 within the range of 20 nm to 2000 nm, the size of the nanochannels 111 is optimized within the nanometer to micrometer range. When the width and spacing of the nanochannels 111 are within the above range, it ensures that multiple nanochannels 111 connected in parallel provide sufficient current conduction capability, fully leveraging the high carrier density advantage of the dual-channel structure 111, while also providing sufficient filling space and contact area with the channel sidewalls for the high thermal conductivity material within the channel recesses 112, achieving efficient heat dissipation. Meanwhile, the size ratio of the nanochannel 111 to the channel groove 112 is appropriate, which can suppress the short-channel effect, improve the breakdown characteristics and threshold voltage stability of the device, and enable the device to meet the power application requirements of high current density and high withstand voltage.
[0033] In one feasible implementation, the thickness of the first channel layer 6 is 10nm~60nm; the thickness of the second channel layer 4 is 50nm~500nm.
[0034] In this technical solution, by controlling the thickness of the first channel layer 6 within the range of 10nm to 60nm, the first channel layer 6 can serve as both a stress buffer layer 3 between the second barrier layer 5 and the first barrier layer 7, and effectively transmit the polarization effect generated between the first barrier layer 7 and the second barrier layer 5. When the thickness of the first channel layer 6 is within this range, the polarization electric fields generated by the upper and lower barrier layers can work synergistically to simultaneously form a high-concentration two-dimensional electron gas at the interfaces of the second channel layer 4 and the second barrier layer 5, and at the interfaces of the first channel layer 6 and the first barrier layer 7. This increases the total carrier density of the device, allowing the high current density advantage of the double-layer nanochannel 111 structure to be fully utilized. Simultaneously, controlling the thickness of the first channel layer 6 within the range of 10nm to 60nm enables the device to achieve higher current density and better frequency characteristics, providing a structural basis for high-power, high-frequency applications. Based on this, by controlling the thickness of the second channel layer 4 within the range of 50nm to 500nm, the second channel layer 4 provides sufficient migration space for the underlying two-dimensional electron gas while possessing a good thermal conductivity path. This facilitates the rapid vertical conduction of heat generated in the upper channel to the buffer layer 3 and the substrate, preventing heat accumulation in the channel region. Simultaneously, the thickness of the second channel layer 4 within the 50nm to 500nm range is compatible with the subsequent etching process for forming the arrayed nanochannel 111 structure. This ensures that the etching depth precisely penetrates the interface between the second barrier layer 5 and the second channel layer 4, exposing the underlying channel. This allows the subsequently filled high thermal conductivity material layer 12 to directly contact the hotspot region of the channel where heat is most concentrated, thereby fully utilizing the heat dissipation effect of the high thermal conductivity material layer 12. Furthermore, this helps maintain the overall mechanical stability and process compatibility of the device structure, preventing insufficient structural strength due to an excessively thin channel layer or increased process difficulty due to an excessively thick channel layer, thus ensuring high reliability and large-scale manufacturing of the device.
[0035] In one feasible implementation, the high thermal conductivity material layer 12 is non-conductive, and the material of the high thermal conductivity material layer 12 includes at least one of diamond, diamond-like carbon, aluminum nitride, and cubic boron nitride.
[0036] In this technical solution, the high thermal conductivity material layer 12 is non-conductive. When it fills the channel groove 112 between adjacent nanochannels 111, it will not cause an electrical short circuit between the source electrode 13, drain electrode 14, or gate electrode 15, ensuring the electrical isolation and normal operation of the device. Materials such as diamond, diamond-like carbon, aluminum nitride, and cubic boron nitride have extremely high thermal conductivity, which can rapidly conduct the heat generated by the conductive channel laterally, significantly shortening the heat transfer path. At the same time, materials such as diamond, diamond-like carbon, aluminum nitride, and cubic boron nitride have excellent chemical and thermal stability, which can maintain stable performance under high-temperature operating conditions, thereby suppressing the channel temperature rise caused by self-heating effect and improving the output power density and long-term operational reliability of the device.
[0037] like Figure 5 As shown, according to a second aspect of this application, a method for fabricating a high-power device is proposed, used to fabricate a high-power device as described in any of the above technical solutions, comprising: S1. A double-channel heterojunction material substrate is provided, the double-channel heterojunction material substrate comprising a substrate layer 1, a nucleation layer 2, a buffer layer 3, a second channel layer 4, a second barrier layer 5, a first channel layer 6, a first barrier layer 7 and a cap layer 8 stacked sequentially; a first mask layer 80 is grown on the cap layer 8. S2. Define the ohmic regrowth region pattern on the first mask layer 80, etch the cap layer 8, the first barrier layer 7, the first channel layer 6, the second barrier layer 5 and part of the second channel layer 4 to form the first groove 90 located in the source electrode 13 region and the second groove 100 located in the drain electrode 14 region. S3, growing n in the first groove 90 and the second groove 100 + Material layer; S4. Remove the first mask layer 80 to remove n outside the first groove 90 and the second groove 100. + Material layer, retaining n within the first groove 90 and the second groove 100 + Material layer, forming the first n + Material layer 9 and the second n + Material layer 10; S5, Deposited passivation layer 11; S6, Remove the first n + Material layer 9 and the second n + A passivation layer 11 covers the material layer 10; S7, Deposit the second mask layer 101; S8. Define a nanochannel 111 pattern on the second mask layer 101, and etch the second mask layer 101, passivation layer 11, cap layer 8, first barrier layer 7, first channel layer 6, second barrier layer 5, and part of the second channel layer 4 to form a nanochannel 111 pattern located on the first n + Material layer 9 and the second n+ The arrayed nanochannel 111 structure between material layers 10; S9. Deposit a high thermal conductivity material layer 12, so that the high thermal conductivity material layer 12 fills the channel groove 112 of the arrayed nanochannel 111 structure and covers the second mask layer 101. S10, Remove the second mask layer 101 and the high thermal conductivity material layer 12 covering the second mask layer 101, and retain the high thermal conductivity material layer 12 in the channel groove 112; S11, in the first n + Source electrode 13 is fabricated on material layer 9, and in the second n + A drain electrode 14 is fabricated on the material layer 10; S12. Define the groove region pattern 123 of the gate electrode 15, etch the passivation layer 11, and form the groove 103 of the gate electrode 15 located between the source electrode 13 and the drain electrode 14. S13. A gate electrode 15 is fabricated at the groove of the gate electrode 15, such that the gate electrode 15 is located at the first n + Material layer 9 and the second n + The material layers 10 are arranged between the gate electrode 15 and above the arrayed nanochannel 111 structure and the high thermal conductivity material layer 12.
[0038] The high-power device fabrication method provided in this application involves forming a double-channel heterojunction structure by sequentially stacking a second channel layer 4, a second barrier layer 5, a first channel layer 6, and a first barrier layer 7. High-concentration two-dimensional electron gases are formed at the interfaces of the two heterojunction layers through polarization effects, significantly increasing the total carrier density of the device and thus achieving a higher current density to meet high-power output requirements. Since the increase in current density inevitably leads to a sharp increase in heat near the channel, especially below the gate electrode 15, to address the more severe heat accumulation problem caused by high power density, the method first forms n in the source electrode 13 region and the drain electrode 14 region. +A material layer is then etched between the source electrode 13 and the drain electrode 14 to form an arrayed nanochannel 111 structure composed of a double-layer channel structure. A high thermal conductivity material layer 12 is filled in the channel grooves 112 between the nanochannels 111, allowing the high thermal conductivity material layer 12 to directly contact the peak hotspot region of the conductive channel. The heat generated in the channel can be rapidly transferred laterally through the high thermal conductivity material layer 12 and diffused to other areas, significantly shortening the heat transfer path, rapidly reducing the peak temperature inside the device, achieving instantaneous heat dissipation, and improving the output power, efficiency, and operational reliability of high-power devices. At the same time, the high thermal conductivity material layer 12 is selectively grown only in the channel grooves 112, without affecting the material and thickness selection of the passivation layer 11, greatly preserving the freedom of the passivation process. This is beneficial for supporting the device to achieve excellent current collapse characteristics, enabling the device to maintain high performance without degradation for a long time under continuous high-power operation. The device combines instantaneous heat dissipation and steady-state heat dissipation functions, solving the thermal management problems brought about by high power density. The bilayer nanochannel 111 structure is fabricated through a single epitaxial growth process, which is simple, compatible with existing semiconductor manufacturing processes, and suitable for mass production.
[0039] In one feasible implementation, when etching the second channel layer 4, the etching extends through the interface between the second barrier layer 5 and the second channel layer 4, and below the depth where the channel of the second channel layer 4 is located, so as to expose the channel of the second channel layer 4 on the sidewall of the channel groove 112.
[0040] In this technical solution, by controlling the etching depth to penetrate the interface between the second barrier layer 5 and the second channel layer 4 but below the depth of the channel in the second channel layer 4, the sidewall of the channel groove 112 is exposed to expose the conductive channel. This allows the high thermal conductivity material layer 12 subsequently filled in the channel groove 112 to be adjacent to the exposed conductive channel, ensuring that the heat transfer path directly acts on the channel hot spot area where the heat is most concentrated, effectively shortening the distance of heat conduction outward and achieving instantaneous heat dissipation. At the same time, the high thermal conductivity material layer 12 is in direct contact with the peak hot spot area of the conductive channel, significantly improving the heat conduction efficiency between the peak hot spot and other areas. The heat in the channel heat accumulation area at the root of the gate electrode 15 is quickly transferred out and diffused to other areas through the high thermal conductivity material, which is beneficial for rapid heat equalization inside the high-power device, reducing the impact of thermal stress caused by the internal temperature difference of the high-power device, and improving the operational reliability of the high-power device.
[0041] It should be noted that if the etching depth only reaches the interface and does not go below the channel of the second channel layer 4, the bottom surface of the channel groove 112 is located above the depth of the two-dimensional electron gas, and the sidewall cannot fully expose the conductive channel area. The contact area between the high thermal conductivity material and the channel hot spot is insufficient, which affects the heat dissipation effect. If the etching depth is too deep or even penetrates the second channel layer 4, it will damage the device structure and increase the risk of leakage.
[0042] In one feasible implementation, a high thermal conductivity material layer 12 is filled in the channel groove 112, the high thermal conductivity material layer 12 is in direct contact with the sidewall of the arrayed nanochannel 111 structure, and the high thermal conductivity material layer 12 is adjacent to the channel of the second channel layer 4.
[0043] In this technical solution, the high thermal conductivity material layer 12 fills the channel groove 112 and directly contacts the sidewall of the arrayed nanochannel 111 structure, thus being adjacent to the conductive channel. Since the conductive channel (two-dimensional electron gas at the heterojunction interface) is located at the interface between the barrier layer and the channel layer, i.e., at the sidewall of the arrayed nanochannel 111 structure, the high thermal conductivity material layer 12 directly contacts the sidewall of the nanochannel 111 within the channel groove 112, making it almost impossible to separate the high thermal conductivity material layer 12 from the heat source. The heat transfer path is greatly shortened, and heat can be conducted from the channel hot spot to the high thermal conductivity material layer 12 in the shortest distance, and then rapidly diffuse to the entire high thermal conductivity material layer 12 and be transferred to the outside of the device, achieving instantaneous heat dissipation.
[0044] It should be noted that, compared to placing high thermal conductivity materials at the bottom of the device or covering the surface of the device, this application shortens the heat transfer distance from the source, significantly reduces the thermal resistance, and can effectively suppress the sharp rise in the peak temperature inside the device under narrow pulse operating mode, thereby improving the operating reliability of high power devices.
[0045] In one feasible implementation, the high thermal conductivity material layer 12 and the passivation layer 11 within the channel groove 112 do not overlap in the vertical direction.
[0046] In this technical solution, the high thermal conductivity material layer 12 and the passivation layer 11 within the channel groove 112 do not overlap in the vertical direction. That is, the high thermal conductivity material layer 12 does not cover the area where the passivation layer 11 is located, and the passivation layer 11 does not cover the area where the high thermal conductivity material layer 12 is located, thus spatially separating the high thermal conductivity material layer 12 and the passivation layer 11. The selection of the material and thickness of the passivation layer 11 is no longer constrained by the thermal conductivity performance of the high thermal conductivity material layer 12. Optimal passivation material and thickness can be used to suppress current collapse and optimize the device surface states without having to consider thermal conductivity. This allows the passivation layer 11 to be independently optimized to suppress current collapse, enabling the device to maintain high performance without degradation for extended periods under continuous high-power operation, ensuring reliable steady-state heat dissipation performance. Furthermore, the filling height and position of the high thermal conductivity material layer 12 only need to consider the contact efficiency with channel hotspots and are not limited by the passivation process. The functions of the high thermal conductivity material layer 12 and the passivation layer 11 are completely decoupled in space and optimized independently, so that the device can simultaneously obtain excellent heat dissipation performance and excellent current collapse suppression characteristics, thus solving the technical contradiction that the high thermal conductivity passivation layer 11 and the passivation effect cannot be achieved at the same time.
[0047] In one feasible implementation, a high thermal conductivity material layer 12 is deposited in the trench 112 and above the second mask layer 101. By removing the second mask layer 101, the high thermal conductivity material layer 12 above the second mask layer 101 is simultaneously peeled off, so as to retain the high thermal conductivity material layer 12 filling the trench 112.
[0048] In this technical solution, a high thermal conductivity material layer 12 is simultaneously deposited into the trench 112 and covers the second mask layer 101. Then, by removing the second mask layer 101, the high thermal conductivity material layer 12 covering it is simultaneously peeled off, leaving only the high thermal conductivity material layer 12 within the trench 112. Through a single deposition and peel-off process, selective filling of the high thermal conductivity material within the trench 112 is achieved, eliminating the need for additional chemical mechanical polishing or etch-back processes. The process is simple, highly compatible with existing semiconductor manufacturing processes, and suitable for mass production. Furthermore, the high thermal conductivity material layer 12 remaining in the trench 112 after peeling does not cover the passivation layer 11 region above the barrier layer. This allows the selection of the material and thickness of the passivation layer 11 to be independent of thermal conductivity constraints, facilitating independent optimization of the passivation process to suppress current collapse and improve the overall performance and reliability of the device.
[0049] The method for fabricating high-power devices provided in this application is used to fabricate high-power devices as described in any of the above technical solutions, and therefore the method for fabricating high-power devices possesses all the beneficial effects of the high-power devices described in the above technical solutions.
[0050] Example 1: This embodiment provides a method for fabricating a high-power device, see [link to documentation]. Figures 6a to 6n-3 The following explanation uses a high-power gallium nitride (GaN)-based high electron mobility transistor as an example. This device is fabricated on a silicon carbide (SiC) substrate. Specifically, the fabrication method of the high-power device includes the following steps: S1': Provides a double-channel heterojunction material substrate, and grows a first mask layer on the cap layer of the double-channel heterojunction material substrate, see [link to documentation]. Figures 6a-6b The specific steps include: a. A silicon carbide substrate is provided, and a core layer, a buffer layer, a second channel layer, a second barrier layer, a first channel layer, a first barrier layer, and a cap layer are sequentially deposited on the silicon carbide substrate to form a double-channel heterojunction material substrate. See [link to documentation]. Figure 6a .
[0051] b. Using plasma-enhanced chemistry vapor deposition, silicon dioxide (SiO2) is deposited on the cap layer to grow the first mask layer.
[0052] Specifically, silane (SiH4) and nitrous oxide (N2O) are used as precursors during deposition. Silica is deposited at a furnace temperature of 300℃ as the first mask layer for regrowth, and the thickness of the first mask layer reaches 40nm~400nm.
[0053] S2': Define the ohmic regrowth region pattern on the first mask layer, and etch the cap layer, first barrier layer, first channel layer, second barrier layer, and part of the second channel layer of the ohmic regrowth region pattern to form a first groove located in the source electrode region and a second groove located in the drain electrode region. See [link to documentation]. Figure 6c The specific steps include: a. Spin-coat photoresist onto the first mask layer and expose and develop it to lithographically create the ohmic regrowth region, thus exposing the first mask layer.
[0054] Specifically, photoresist is applied to the first mask layer to a thickness of about 1 μm and pre-baked for 1 min; then the ohmic regrowth area is exposed; after exposure, it is post-baked for 1 min; after post-baking, the sample temperature is allowed to drop to room temperature before development is performed to remove the photoresist in the patterned area. The photolithography is then completed, forming the ohmic regrowth area pattern and exposing the first mask layer in that area.
[0055] b. The first mask layer exposed after photolithography is removed using a fluorine-based (F-based) dry etching process, and then the cap layer, first barrier layer, first channel layer, second barrier layer and part of the second channel layer of the ohmic regrowth region are removed using a chlorine-based (Cl-based) dry etching process to form the first groove and the second groove.
[0056] Specifically, before etching, the sample is baked at 100°C for 1 minute using a hot plate to enhance the etching resistance of the photoresist. Then, fluorine-based dry etching is performed using inductively coupled plasma etching (ICP-C1) to remove the first mask layer exposed after photolithography. Next, inductively coupled plasma chloride-based etching (ICP-C1) is used to remove the cap layer, first barrier layer, first channel layer, second barrier layer, and part of the second channel layer under the first mask layer, etching to the channel that passes through the top of the second channel layer, with an etching depth of 65 nm, to form the first and second grooves.
[0057] c. Remove the photoresist after etching.
[0058] Specifically, the sample is placed in acetone and isopropanol in sequence for ultrasonic cleaning to remove the surface photoresist, and then rinsed with ultrapure water and dried.
[0059] S3': n grows in the first and second grooves + Material layer, see Figure 6d .
[0060] Specifically, highly doped n-type atoms are grown using organometallic chemical vapor deposition (HCVD) or molecular beam epitaxy (MBE). + Type II gallium nitride (n) + -GaN) layer, doped with silicon (Si), with a silicon doping concentration of not less than 1×10⁻⁶. 19 cm -3 , so that n + The material layer has a growth thickness of 80 nm.
[0061] S4': Remove the first mask layer, remove n outside the first groove and the second groove. + Material layer, retaining the source electrode region and the drain electrode region n + Material layer, forming the first n + Material layer and second n + Material layer, see Figure 6e .
[0062] Specifically, the sample is immersed in hydrofluoric acid solution (hydrofluoric acid:water = 2:3) for 15 minutes to completely etch the first mask layer on the device surface. After rinsing with ultrapure water for 2 minutes, it is dried with nitrogen. Then, the sample is placed in acetone, stripping solution, acetone and isopropanol in sequence for ultrasonic cleaning, rinsed with ultrapure water and dried.
[0063] S5': Deposited passivation layer, see [link] Figure 6f .
[0064] Specifically, a silicon nitride (SiN) passivation layer is deposited on the cap layer using a low-pressure chemical vapor deposition process.
[0065] Specifically, silane and ammonia (NH3) are used as precursors, and silicon nitride is deposited at a furnace temperature of 700℃ as a passivation layer, so that the thickness of the passivation layer reaches 20nm~200nm.
[0066] S6': Remove the first n + Material layer and second n + The passivation layer covering the material layer, see [link / reference]. Figure 6g .
[0067] Specifically, an anti-etching photoresist with a thickness of approximately 0.6 μm is applied to the passivation layer; then the ohmic regrowth area is exposed; after exposure, it is post-baked for 1 minute; after post-baking, once the sample temperature has cooled to room temperature, development is performed to remove the photoresist in the patterned area, exposing the passivation layer of the ohmic regrowth area; then, dry etching is performed using inductively coupled plasma (ICP) technology to remove the exposed passivation layer; finally, the etched photoresist is removed.
[0068] S7': Deposition of the second mask layer, see [link to documentation] Figure 6h .
[0069] Specifically, silicon dioxide is deposited on the passivation layer as a second mask layer using plasma-enhanced chemical vapor deposition.
[0070] Specifically, silane and nitrous oxide are used as precursors, and silicon dioxide is deposited at a furnace temperature of 300°C to serve as a mask for highly thermally conductive selective growth, resulting in a second mask layer thickness of 80nm~2000nm.
[0071] S8': Define nanochannel patterns on the second mask layer, and use dry etching to remove the second mask layer, passivation layer, cap layer, first barrier layer, first channel layer, second barrier layer, and part of the second channel layer in the region between the arrayed nanochannel patterns, forming a nanochannel pattern located in the first n... + Material layer and second n + Arrayed nanochannel structures between material layers, see Figures 6i-1 to 6i-3 The specific steps include: a. Photoresist is coated onto the second mask layer and exposed and developed to photolithographically create a nanochannel pattern, thus exposing the second mask layer. See [link to documentation]. Figure 6i-1 .
[0072] Specifically, photoresist with a thickness of about 1.2 μm is coated on the second mask layer; then the nanochannel pattern area is exposed; after the post-baking is completed and the sample temperature drops to room temperature, development is performed to remove the photoresist in the nanochannel pattern area. The photolithography is completed, forming the nanochannel pattern and exposing the second mask layer of the nanochannel pattern area.
[0073] b. The second mask layer and passivation layer exposed after photolithography are removed using a fluorine-based dry etching process. Then, the cap layer, first barrier layer, first channel layer, second barrier layer, and part of the second channel layer in the region between the arrayed nanochannel patterns are removed using a chlorine-based dry etching process, forming an arrayed nanochannel structure composed of a double-layer channel structure. See [link to relevant documentation]. Figures 6i-2 to 6i-3 .
[0074] Specifically, before etching, the sample is baked at 100°C for 1 minute using a hot plate to enhance the etching resistance of the photoresist. Then, fluorine-based dry etching is performed using inductively coupled plasma etching (ICP-C1) to remove the second mask layer and passivation layer exposed after photolithography. Then, the cap layer, first barrier layer, first channel layer, second barrier layer, and part of the second channel layer under the second mask layer are removed by inductively coupled plasma chlorine-based etching (ICP-C1 etching), etching to the channel through the second channel layer, with an etching depth of 80 nm, forming an arrayed nanochannel structure.
[0075] c. Remove the photoresist after etching.
[0076] Specifically, the sample is placed in acetone and isopropanol in sequence for ultrasonic cleaning to remove the surface photoresist, and then rinsed with ultrapure water and dried.
[0077] S9': Deposit of a high thermal conductivity material layer, see [link / reference] Figures 6j-1 to 6j-3 .
[0078] Specifically, plasma is used to treat the sample surface, and a layer of high thermal conductivity material is deposited using microwave plasma chemical vapor deposition.
[0079] Specifically, methane (CH4) and hydrogen (H2) are used as reaction sources, and diamond is deposited at a furnace temperature of 700℃ as a high thermal conductivity material layer, so that the thickness of the high thermal conductivity material layer reaches 80nm~800nm.
[0080] S10': Remove the second mask layer, remove the high thermal conductivity material layer covering the second mask layer, and retain the high thermal conductivity material layer in the trench. See below. Figures 6k-1 to 6k-3 .
[0081] Specifically, the sample is immersed in hydrofluoric acid solution (hydrofluoric acid:water = 2:3) for 30 minutes to completely etch the second mask layer on the device surface. After rinsing with ultrapure water for 2 minutes, it is dried with nitrogen. Blue film is used to remove any adhering particles that are not completely removed from the surface. Then, the sample is placed in acetone, stripping solution, acetone and isopropanol in sequence for ultrasonic cleaning, and then rinsed with ultrapure water and dried.
[0082] S11': In the first n + The source electrode is fabricated on the material layer, and in the second n + Drain electrode fabricated on material layer, see [link to documentation]. Figures 6l-1 to 6l-2 The specific steps include: a. In the first n + Photolithographically patterned source electrode pattern on material layer, in the second n + Photolithographically patterned drain electrode pattern on the material layer.
[0083] Specifically, a double layer of photoresist is applied to the sample, with the bottom layer of stripper approximately 0.35 μm thick and the top layer of photoresist approximately 0.56 μm thick. Then, the metal electrode pattern area is exposed. After exposure, it is post-baked for 1 minute. After the post-baking is completed and the sample temperature drops to room temperature, development is performed to remove the photoresist in the pattern area. The photolithography is then complete, forming the source electrode pattern and the drain electrode pattern.
[0084] b. Evaporate titanium / gold (Ti / Au) metal electrodes using an electron beam evaporation apparatus.
[0085] Specifically, a plasma stripper is first used to remove the residual photoresist in the exposed area, and then an electron beam evaporator is used to sequentially evaporate 20 nm thick titanium (Ti) and 200 nm thick gold (Au).
[0086] c. Strip the metal from the unexposed areas to form the source and drain electrodes.
[0087] Specifically, the sample after metal evaporation is immersed in acetone for more than 3 hours, and then ultrasonically cleaned until the metal in the unexposed area is completely removed; then the sample is placed in a 60°C stripping solution and heated in a water bath for 15 minutes; the sample is then placed in acetone and isopropanol in sequence, ultrasonically cleaned for 3 minutes, rinsed with ultrapure water for 2 minutes, and then dried with nitrogen to form the source electrode and drain electrode.
[0088] S12': Defines the gate electrode channel groove pattern and etches the passivation layer to form the gate electrode groove located between the source and drain electrodes. See [link to documentation]. Figures 6m-1 to 6m-3 The specific steps include: a. Coat the sample surface with photoresist and expose and develop it to photolithographically create the gate electrode channel groove area.
[0089] Specifically, photoresist is coated onto the sample surface to a thickness of approximately 0.5 μm; then, the gate electrode channel recess area is exposed; the photoresist in the patterned area is removed by development, completing the photolithography and forming the gate electrode recess pattern. See [link to documentation]. Figure 6m-1 .
[0090] b. Use a dry etching process to remove the passivation layer exposed after photolithography to form a gate electrode groove.
[0091] Specifically, fluorine-based dry etching is performed using inductively coupled plasma (ICP) technology to remove the silicon nitride (SiN) passivation layer exposed after photolithography, forming a gate electrode groove.
[0092] c. Remove the photoresist after etching.
[0093] Specifically, the sample is placed in acetone and isopropanol in sequence for ultrasonic cleaning to remove the surface photoresist, and then rinsed with ultrapure water and dried.
[0094] S13': Fabricate a gate electrode on the gate electrode groove, such that the gate electrode is located in the first n + Material layer and second n + Between material layers, see Figures 6n-1 to 6n-3 The specific steps include: a. Photolithographically pattern the gate electrode onto the sample.
[0095] Specifically, a double layer of photoresist is applied to the sample, with the bottom layer having a stripping thickness of approximately 0.35 μm and the top layer approximately 0.56 μm. Then, the gate electrode pattern area is exposed using a photolithography machine through a mask. The photoresist in the gate electrode pattern area is removed by development, and the photolithography is completed, forming the gate electrode pattern.
[0096] b. Evaporate the nickel / gold (Ni / Au) metal electrode using an electron beam evaporation device.
[0097] Specifically, a plasma stripper is first used to remove the residual photoresist in the exposed area, and then an electron beam evaporator is used to sequentially evaporate 45nm thick nickel (Ni) and 200nm thick gold (Au).
[0098] c. Strip the metal from the unexposed areas to form the gate electrode.
[0099] Specifically, the sample after metal evaporation is immersed in acetone for more than 3 hours, and then ultrasonically cleaned until the metal in the unexposed areas is completely removed; the sample is placed in a stripping solution at 60°C and heated in a water bath for 15 minutes; the sample is then ultrasonically cleaned in acetone and isopropanol for 3 minutes, rinsed with ultrapure water for 2 minutes, and dried with nitrogen to form a gate electrode, wherein the gate electrode is located above the arrayed nanochannel structure and the high thermal conductivity material layer.
[0100] It will be readily understood by those skilled in the art that the above embodiments can be freely combined and superimposed without conflict.
[0101] The above are merely preferred embodiments of this application and are not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application. The above are merely preferred embodiments of this application. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of this application, and these improvements and modifications should also be considered within the protection scope of this application.
Claims
1. A high-power device, characterized in that, The high-power device includes: The substrate layer, nucleation layer, buffer layer, second channel layer, second barrier layer, first channel layer, first barrier layer, cap layer and passivation layer are stacked in sequence. First n + Material layer, the first n + The material layer penetrates the cap layer, the first barrier layer, the first channel layer, and the second barrier layer, the first n + The bottom of the material layer extends below the channel of the second channel layer; Source electrode, the source electrode being located at the first n + Above the material layer; Second n + Material layer, the second n + The material layer penetrates the cap layer, the first barrier layer, the first channel layer, and the second barrier layer, and the second n + The bottom of the material layer extends below the channel of the second channel layer; Drain electrode, the drain electrode being located at the second n + Above the material layer; Arrayed nanochannel structure, wherein the arrayed nanochannel structure is composed of the first n + Material layer and the second n + The material layers consist of a second channel layer, a second barrier layer, a first channel layer, a first barrier layer, and a cap layer. A high thermal conductivity material layer, wherein the high thermal conductivity material layer fills the channel grooves of the arrayed nanochannel structure; Gate electrode, the gate electrode being located at the first n + Material layer and the second n + Between the material layers, and the gate electrode is located above the arrayed nanochannel structure and the high thermal conductivity material layer.
2. The high-power device according to claim 1, characterized in that: The material of the first barrier layer includes at least one of aluminum nitride (AlN), indium aluminum nitride (InAlN), scandium aluminum nitride (ScAlN), aluminum gallium nitride (AlGaN), and indium aluminum gallium nitride (InAlGaN); The material of the second barrier layer includes at least one of aluminum nitride (AlN), indium aluminum nitride (InAlN), scandium aluminum nitride (ScAlN), aluminum gallium nitride (AlGaN), and indium aluminum gallium nitride (InAlGaN).
3. A high-power device according to claim 1, characterized in that: The arrayed nanochannel structure includes nanochannels that are uniformly distributed along the gate width direction of the gate electrode, and a channel groove is formed between two adjacent nanochannels.
4. A high-power device according to claim 3, characterized in that: The width of the nanochannel is 20nm~20000nm; the spacing between two adjacent nanochannels is 20nm~2000nm.
5. A high-power device according to claim 1, characterized in that: The thickness of the first channel layer is 10nm~60nm; the thickness of the second channel layer is 50nm~500nm.
6. A method for fabricating a high-power device, characterized in that, A method for fabricating a high-power device as described in any one of claims 1 to 5, wherein the fabrication method of the high-power device comprises: S1. A double-channel heterojunction material substrate is provided, the double-channel heterojunction material substrate comprising a substrate layer, a nucleation layer, a buffer layer, a second channel layer, a second barrier layer, a first channel layer, a first barrier layer and a cap layer stacked sequentially; a first mask layer is grown on the cap layer; S2. Define an ohmic regrowth region pattern on the first mask layer, and etch the cap layer, the first barrier layer, the first channel layer, the second barrier layer and part of the second channel layer to form a first groove located in the source electrode region and a second groove located in the drain electrode region. S3. Growing n in the first groove and the second groove. + Material layer; S4. Remove the first mask layer to remove the n outside the first groove and the second groove. + Material layer, retaining the n in the first groove and the second groove + Material layer, forming the first n + Material layer and the second n + Material layer; S5, Deposited passivation layer; S6, Remove the first n + Material layer and the second n + The passivation layer covering the material layer; S7, Deposit the second mask layer; S8. Define a nanochannel pattern on the second mask layer, and etch the second mask layer, the passivation layer, the cap layer, the first barrier layer, the first channel layer, the second barrier layer, and a portion of the second channel layer to form a nanochannel pattern located on the first n + Material layer and the second n + Arrayed nanochannel structures between material layers; S9. Deposit a high thermal conductivity material layer, so that the high thermal conductivity material layer fills the channel groove of the arrayed nanochannel structure and covers the second mask layer; S10. Remove the second mask layer and the high thermal conductivity material layer covering the second mask layer, while retaining the high thermal conductivity material layer within the channel groove; S11, in the first n + The source electrode is fabricated on the material layer, in the second n + Drain electrodes are fabricated on the material layer; S12. Define the gate electrode groove region pattern, etch the passivation layer, and form a gate electrode groove located between the source electrode and the drain electrode; S13. A gate electrode is fabricated at the gate electrode groove, such that the gate electrode is located at the first n + Material layer and the second n + Between the material layers, and with the gate electrode positioned above the arrayed nanochannel structure and the high thermal conductivity material layer.
7. The method for fabricating a high-power device according to claim 6, characterized in that: When etching the second channel layer, the etching extends through the interface between the second barrier layer and the second channel layer, and below the depth where the channel of the second channel layer is located, so as to expose the channel of the second channel layer on the sidewall of the channel recess.
8. The method for fabricating a high-power device according to claim 7, characterized in that: The high thermal conductivity material layer fills the channel groove, the high thermal conductivity material layer is in direct contact with the sidewall of the arrayed nanochannel structure, and the high thermal conductivity material layer is adjacent to the channel of the second channel layer.
9. The method for fabricating a high-power device according to claim 6, characterized in that: The high thermal conductivity material layer and the passivation layer within the groove do not overlap in the vertical direction.
10. The method for fabricating a high-power device according to claim 6, characterized in that: The high thermal conductivity material layer is deposited in the trench and above the second mask layer. By removing the second mask layer, the high thermal conductivity material layer above the second mask layer is simultaneously peeled off, so as to retain the high thermal conductivity material layer filling the trench.