Solar cells and their preparation methods, photovoltaic modules

By employing a regionally distributed tunneling oxide layer and multiple passivation layers in the solar cell, and adapting to the Polyfinger patterned structure, the problem of the tunneling oxide layer's inability to adapt is solved, achieving a balance between high efficiency and high PID resistance stability.

CN123124451APending Publication Date: 2026-11-17SHANDONG RONMA SOLAR CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611378707.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-17

Smart Images

  • Figure CN123124451A_ABST
    Figure CN123124451A_ABST
Patent Text Reader

Abstract

This application provides a solar cell, its fabrication method, and a photovoltaic module. The solar cell comprises a substrate, a tunneling oxide layer, a phosphorus-doped polycrystalline silicon layer, and a passivation layer stacked sequentially. The substrate has conductive contact areas corresponding to electrodes and non-contact passivation areas that avoid the electrodes. The tunneling oxide layer includes a first oxide sublayer located in the conductive contact area and a second oxide sublayer located in the non-contact passivation area. The oxygen-to-silicon ratio of the first oxide sublayer is (1.85~1.92):1, and the oxygen-to-silicon ratio of the second oxide sublayer is (1.98~2.02):1. This application adapts the tunneling oxide layer to the Polyfinger patterned structure by setting first and second oxide sublayers with different functions to match the conductive contact area and the non-contact passivation area, thus achieving both high efficiency and high PID resistance stability of the solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of solar cell technology, specifically relating to solar cells and their preparation methods, and photovoltaic modules. Background Technology

[0002] The current fabrication process for TOPCon cells with a Polyfinger structure on the back side is as follows: after cleaning and texturing the silicon wafer, an ultra-thin SiO2 tunneling oxide layer of equal thickness is prepared over the entire back side, and then a polycrystalline silicon thin film is formed. The Polyfinger pattern is formed by photolithography and dry etching, and then a single-layer passivation film is formed. Finally, the cell is fabricated by conventional high-temperature overall annealing and screen printing of electrodes.

[0003] However, current TOPCon battery fabrication processes cannot adapt the tunneling oxide layer to the characteristics of the Polyfinger patterned structure. Patterning etching generates numerous edge defects and interface porosity, disrupting the continuity of the passivation layer. Under high temperature, high humidity, and high voltage bias conditions, sodium ions in the encapsulation glass readily migrate and accumulate along defect channels to the back of the battery, inducing interface charge polarization and significantly increasing the carrier recombination rate. Traditional Polyfinger batteries typically experience efficiency degradation of 5% to 8% after PID testing, exhibiting extremely poor long-term outdoor power generation stability and failing to balance high battery efficiency with high PID resistance. Summary of the Invention

[0004] In view of this, the first aspect of this application provides a solar cell, the solar cell comprising a substrate, a tunneling oxide layer, a phosphorus-doped polycrystalline silicon layer, and a passivation layer stacked sequentially; The substrate has a conductive contact area corresponding to the electrode and a non-contact passivation area that avoids the electrode. The tunneling oxide layer includes a first oxide sub-layer located in the conductive contact area and a second oxide sub-layer located in the non-contact passivation area. The oxygen-silicon ratio of the first oxide sub-layer is (1.85~1.92):1, and the oxygen-silicon ratio of the second oxide sub-layer is (1.98~2.02):1.

[0005] Wherein, the thickness of the first oxide sublayer is less than the thickness of the second oxide sublayer; And / or, the density of the first oxide sublayer is less than the density of the second oxide sublayer; And / or, the porosity of the first oxide sublayer is greater than the porosity of the second oxide sublayer; And / or, the interfacial dangling bond density of the first oxide sublayer is greater than that of the second oxide sublayer; And / or, the contact resistance of the first oxide sublayer is less than the contact resistance of the second oxide sublayer.

[0006] The thickness of the first oxide sublayer is 1.2 nm to 1.5 nm, and the thickness of the second oxide sublayer is 1.8 nm to 2.2 nm. And / or, the density of the first oxide sublayer is 2.05 g / cm³. 3 ~2.12g / cm 3 The density of the second oxide sublayer is 2.18 g / cm³. 3 ~2.22g / cm 3 ; And / or, the porosity of the first oxide sublayer is 2.8%~3.8%, and the porosity of the second oxide sublayer is 0.6%~1.2%; And / or, the interfacial dangling bond density of the first oxide sublayer is 3.2 × 10⁻⁶. 11 cm -2 ~4.5×10 11 cm -2 The interfacial dangling bond density of the second oxide sublayer is ≤1.2×10⁻⁶. 11 cm -2 ; And / or, the contact resistance of the first oxide sublayer is 0.25Ω. cm 2 ~0.45Ω cm 2 The contact resistance of the second oxide sublayer is ≥1×10 9 Ω cm 2 .

[0007] The phosphorus-doped polycrystalline silicon layer is located in the conductive contact region and is disposed away from the non-contact passivation region. The phosphorus-doped polycrystalline silicon layer forms a conductive structure, which includes multiple conductive parts arranged in an array. The width of the conductive parts is 40μm to 80μm, the spacing between the conductive parts is 0.8mm to 1.2mm, and the sheet resistance of the phosphorus-doped polycrystalline silicon layer is 80Ω / sq to 100Ω / sq. The phosphorus doping concentration of the conductive structure is 1×10⁻⁶. 20 cm -3 ~5×10 20 cm -3 .

[0008] The passivation layer includes: A transition sublayer is disposed on the phosphorus-doped polycrystalline silicon layer, wherein the transition sublayer is a SiOxNy layer; A barrier sublayer is disposed on the side of the transition sublayer away from the phosphorus-doped polycrystalline silicon layer, and the barrier sublayer is a SiNx layer.

[0009] The total thickness of the passivation layer is 70nm~90nm; And / or, the thickness of the transition sublayer is 20nm~30nm; And / or, the thickness of the barrier sublayer is 50nm~60nm; And / or, the refractive index of the barrier sublayer is 2.05~2.15.

[0010] A second aspect of this application provides a method for preparing a solar cell, the method comprising: A substrate is provided, the substrate having a conductive contact area corresponding to an electrode and a non-contact passivation area that avoids the electrode; A tunneling oxide layer is formed on the substrate, the tunneling oxide layer comprising a first oxide sublayer located in the conductive contact region and a second oxide sublayer located in the non-contact passivation region, the oxygen-silicon ratio of the first oxide sublayer being (1.85~1.92):1, and the oxygen-silicon ratio of the second oxide sublayer being (1.98~2.02):1; A phosphorus-doped polycrystalline silicon layer is formed on the side of the tunneling oxide layer opposite to the substrate; A passivation layer is formed on the side of the phosphorus-doped polysilicon layer opposite to the substrate.

[0011] The preparation method includes: A substrate is provided, the substrate having a conductive contact area corresponding to an electrode and a non-contact passivation area that avoids the electrode; A tunneling oxide layer is formed on the substrate, the tunneling oxide layer comprising a first oxide sublayer located in the conductive contact region and a second oxide sublayer located in the non-contact passivation region, the oxygen-silicon ratio of the first oxide sublayer being (1.85~1.92):1, and the oxygen-silicon ratio of the second oxide sublayer being (1.98~2.02):1; A phosphorus-doped polycrystalline silicon layer is formed on the side of the tunneling oxide layer opposite to the substrate; A passivation layer is formed on the side of the phosphorus-doped polysilicon layer opposite to the substrate.

[0012] During the formation of the tunnel oxide layer, the process pressure is 750 mbar to 850 mbar, the process temperature is 850°C to 900°C, and the nitrogen flow rate is 6000 sccm to 8000 sccm. The step of forming the first oxide sublayer includes: The initial oxygen flow rate of the dry oxygen was controlled at 1200 sccm to 1800 sccm, and the initial oxidation time was 8 min to 12 min. The step of forming the second oxide sublayer includes: The second oxygen flow rate of the dry oxygen is controlled at 3500 sccm~5000 sccm, and the second oxidation time is 18 min~28 min.

[0013] A third aspect of this application provides a photovoltaic module, which includes a solar cell as provided in the first aspect of this application.

[0014] The solar cell and its fabrication method, as well as the photovoltaic module provided in this application, divide the tunneling oxide layer into regions by combining conductive contact areas and non-contact passivation areas. The first oxide sublayer has a relatively high silicon content and is an oxygen-deficient sub-oxide structure, which reduces the carrier tunneling barrier, decreases the contact resistance, and improves the tunneling conductivity, thereby improving the fill factor and conversion efficiency of the solar cell. Furthermore, the oxygen-silicon ratio of the second oxide sublayer is close to the standard silica stoichiometry, with a dense structure, excellent chemical stability, and low interfacial dangling bond density, which effectively blocks the migration of sodium ions along defect channels, suppresses interfacial charge polarization, forms a dense physical ion barrier, and improves the anti-PID performance of the solar cell.

[0015] Therefore, this application adapts the tunneling oxide layer to the Polyfinger patterned structure by setting a first oxide sublayer and a second oxide sublayer with different functions to the conductive contact area and the non-contact passivation area, thus balancing the high efficiency and high PID resistance stability of the solar cell. Attached Figure Description

[0016] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the embodiments of this application will be described below.

[0017] Figure 1 This is a schematic diagram of the structure of a solar cell provided in one embodiment of this application.

[0018] Figure 2 A schematic diagram of the structure of a solar cell provided for another embodiment of this application.

[0019] Figure 3 This is a schematic flowchart illustrating a method for fabricating a solar cell according to an embodiment of this application.

[0020] Labeling: Solar cell 1, substrate 10, conductive contact area 11, non-contact passivation area 12, tunneling oxide layer 20, first oxide sublayer 21, second oxide sublayer 22, phosphorus-doped polycrystalline silicon layer 30, passivation layer 40, transition sublayer 41, barrier sublayer 42. Detailed Implementation

[0021] The following are preferred embodiments of this application. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principles of this application, and these improvements and modifications are also considered to be within the scope of protection of this application.

[0022] In view of this, to solve the above problems, please refer to Figure 1 This embodiment provides a solar cell 1, which includes a substrate 10, a tunneling oxide layer 20, a phosphorus-doped polycrystalline silicon layer 30, and a passivation layer 40 stacked sequentially.

[0023] The substrate 10 has a conductive contact area 11 corresponding to the electrode and a non-contact passivation area 12 that avoids the electrode. The tunneling oxide layer 20 includes a first oxide sub-layer 21 located in the conductive contact area 11 and a second oxide sub-layer 22 located in the non-contact passivation area 12. The oxygen-silicon ratio of the first oxide sub-layer 21 is (1.85~1.92):1, and the oxygen-silicon ratio of the second oxide sub-layer 22 is (1.98~2.02):1.

[0024] Optionally, the solar cell 1 is a TOPCon cell.

[0025] The substrate 10 serves multiple functions, including light absorption, carrier generation, carrier transport, and mechanical support, supporting the entire thin film layer and electrodes of the solar cell 1. Optionally, the substrate 10 is a silicon wafer. More preferably, the substrate 10 is an n-type silicon wafer.

[0026] The substrate 10 has a conductive contact area 11 corresponding to the electrode and a non-contact passivation area 12 that avoids the electrode. The conductive contact area 11 is the vertical projection area of ​​the metal electrode of the subsequent solar cell 1 onto the substrate 10. The non-contact passivation area 12 is the area that is not covered by any subsequent metal electrode.

[0027] The tunneling oxide layer 20 is used to achieve selective carrier tunneling. Optionally, the tunneling oxide layer 20 may be a silicon dioxide layer.

[0028] The phosphorus-doped polycrystalline silicon layer 30 is used to achieve field passivation and electron collection.

[0029] The passivation layer 40 serves as a physicochemical barrier, isolating the internal structure of the solar cell 1 from the external environment.

[0030] The first oxide sublayer 21 and the second oxide sublayer 22 are disposed in the same layer, located between the substrate 10 and the phosphorus-doped polysilicon layer 30.

[0031] The oxygen-silicon ratio of the first oxide sublayer 21 refers to the ratio of the number of oxygen atoms to the number of silicon atoms in the first oxide sublayer 21.

[0032] The oxygen-silicon ratio of the first oxide sublayer 21 can be exemplified as 1.85:1, 1.86:1, 1.87:1, 1.88:1, 1.89:1, 1.9:1, 1.91:1, or 1.92:1, etc.

[0033] If the oxygen-silicon ratio of the first oxide sublayer 21 is less than 1.85:1, the silicon content of the first oxide sublayer 21 is too high. The oxide layer tends to be a non-stoichiometric silicon-rich silicon oxide or even a silicon nanocrystal embedded structure. The insulation properties of the tunnel oxide layer 20 are destroyed, leakage current channels are formed, the parallel resistance of the cell drops sharply, the open circuit voltage and fill factor deteriorate significantly, and the yield of the solar cell 1 decreases.

[0034] If the oxygen-silicon ratio of the first oxide sublayer 21 is greater than 1.92:1, then the oxygen content of the first oxide sublayer 21 is too high, the tunneling barrier thickness and height increase synchronously, the carrier tunneling probability decreases exponentially, the contact resistance increases, the series resistance of the cell increases, the fill factor of the solar cell 1 decreases, and the conversion efficiency decreases.

[0035] The oxygen-silicon ratio of the second oxide sublayer 22 refers to the ratio of the number of oxygen atoms to the number of silicon atoms in the second oxide sublayer 22.

[0036] The oxygen-silicon ratio of the second oxide sublayer 22 can be exemplified by 1.98:1, 1.99:1, 2:1, 2.01:1, or 2.02:1, etc.

[0037] If the oxygen-silicon ratio of the second oxide sublayer 22 is less than 1.98:1, the SiO2 network structure in the second oxide sublayer 22 is incomplete, the density of dangling bonds at the interface increases, the interface recombination rate accelerates, and the open-circuit voltage decreases. At the same time, the number of defect channels in the second oxide sublayer 22 increases, the sodium ion diffusion coefficient increases, and the anti-PID performance of the solar cell 1 decreases.

[0038] If the oxygen-silicon ratio of the second oxide sublayer 22 is greater than 2.02:1, then the oxygen in the second oxide sublayer 22 is severely excessive, a large number of peroxy bonds and non-bridged oxygen structures are generated in the second oxide sublayer 22, the internal stress increases significantly, the interface is prone to microcracks and peeling, the long-term thermal cycling reliability decreases, and excessive oxidation may actually increase the interface state density, thus reducing the passivation effect.

[0039] In summary, the solar cell 1 provided in this embodiment divides the tunneling oxide layer 20 into regions by coordinating the conductive contact region 11 and the non-contact passivation region 12. The first oxide sublayer 21 has a relatively high silicon content and is an oxygen-deficient sub-oxide structure, which reduces the carrier tunneling barrier, decreases the contact resistance, and improves the tunneling conductivity, thereby improving the fill factor and conversion efficiency of the solar cell 1. Furthermore, the oxygen-silicon ratio of the second oxide sublayer 22 is close to the standard silica stoichiometry, with a dense structure, excellent chemical stability, and low interfacial dangling bond density, which effectively blocks the migration of sodium ions along defect channels, suppresses interfacial charge polarization, and forms a dense physical ion barrier, thereby improving the anti-PID performance of the solar cell 1.

[0040] Therefore, this embodiment provides a first oxide sublayer 21 and a second oxide sublayer 22 with different functions to adapt to the conductive contact region 11 and the non-contact passivation region 12, so that the tunneling oxide layer 20 adapts to the Polyfinger patterned structure, taking into account both the high efficiency and high anti-PID stability of the solar cell 1.

[0041] In one embodiment, the thickness of the first oxide sublayer 21 is less than the thickness of the second oxide sublayer 22.

[0042] Furthermore, the thickness of the first oxide sublayer 21 is 1.2 nm to 1.5 nm, and the thickness of the second oxide sublayer 22 is 1.8 nm to 2.2 nm.

[0043] The thickness of the first oxide sublayer 21 can be specifically exemplified as 1.2nm, 1.25nm, 1.3nm, 1.35nm, 1.4nm, 1.45nm, or 1.5nm, etc.

[0044] If the thickness of the first oxide sublayer 21 is less than 1.2 nm, the first oxide sublayer 21 will be too thin, the probability of pinhole defects will increase significantly, ohmic leakage channels will be easily generated, the parallel resistance will decrease, and the yield of solar cell 1 will be reduced.

[0045] If the thickness of the first oxide sublayer 21 is greater than 1.5 nm, it will lead to an increase in tunneling resistance, an increase in contact resistance, an increase in series resistance, a decrease in fill factor, and a reduction in the efficiency of solar cell 1.

[0046] The thickness of the second oxide sublayer 22 can be specifically exemplified as 1.8nm, 1.85nm, 1.9nm, 1.95nm, 2nm, 2.05nm, 2.1nm, 2.15nm, or 2.2nm, etc.

[0047] If the thickness of the second oxide sublayer 22 is less than 1.8 nm, the sodium ion diffusion path length will be insufficient, the blocking ability will decrease, and the anti-PID performance of the solar cell 1 will be reduced.

[0048] If the thickness of the second oxide sublayer 22 is greater than 2.2 nm, the internal stress of the second oxide sublayer 22 will exceed the critical value, the density of microcracks at the interface will increase, the step coverage will be poor during subsequent polysilicon layer deposition, the film layer at the edge will be discontinuous, and the reliability will decrease.

[0049] Furthermore, the thickness difference between the first oxide sublayer 21 and the second oxide sublayer 22 is limited to 0.6~0.7nm, the step height is moderate, the subsequent phosphorus-doped polycrystalline silicon layer 30 and passivation layer 40 have good step coverage, and the film continuity is maintained.

[0050] And / or, the density of the first oxide sublayer 21 is less than the density of the second oxide sublayer 22.

[0051] Furthermore, the density of the first oxide sublayer 21 is 2.05 g / cm³. 3 ~2.12g / cm 3 The density of the second oxide sublayer 22 is 2.18 g / cm³. 3 ~2.22g / cm 3 .

[0052] For example, the density of the first oxide sublayer 21 can be 2.05 g / cm³. 3 or 2.06 g / cm 3 or 2.07 g / cm 3 or 2.08 g / cm 3 or 2.09 g / cm 3 or 2.1g / cm 3 or 2.11 g / cm 3 or 2.12 g / cm 3 wait.

[0053] If the density of the first oxide sublayer 21 is less than 2.05 g / cm³ 3 This results in the first oxide layer 21 having an overly porous structure, insufficient mechanical strength, and is easily damaged during subsequent processing. It also reduces insulation and increases the risk of leakage current.

[0054] If the density of the first oxide sublayer 21 is greater than 2.12 g / cm³ 3 This leads to a decrease in the tunneling channel density of the first oxide sublayer 21, an increase in contact resistance, and a greater difference in thermal expansion coefficient between it and the silicon substrate 10, making it prone to interface peeling.

[0055] For example, the density of the second oxide sublayer 22 can be 2.18 g / cm³. 3 or 2.19 g / cm 3 or 2.2g / cm 3 or 2.21 g / cm 3or 2.22g / cm 3 wait.

[0056] If the density of the second oxide sublayer 22 is less than 2.18 g / cm³ 3 This results in insufficient compactness of the second oxide sublayer 22, with a high porosity, allowing sodium ions to migrate along the pores and increasing PID attenuation.

[0057] If the density of the second oxide sublayer 22 is greater than 2.22 g / cm³ 3 This results in an excessively high density of the second oxide sublayer 22, leading to extremely high internal stress and making the interface prone to peeling and microcracks.

[0058] And / or, the porosity of the first oxide sublayer 21 is greater than the porosity of the second oxide sublayer 22.

[0059] Furthermore, the porosity of the first oxide sublayer 21 is 2.8%~3.8%, and the porosity of the second oxide sublayer 22 is 0.6%~1.2%.

[0060] The porosity of the first oxide sublayer 21 can be specifically exemplified as 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, or 3.8%, etc.

[0061] If the porosity of the first oxide sublayer 21 is less than 2.8%, the tunneling path density of the first oxide sublayer 21 will be insufficient, the contact resistance will increase, the stress release channels will decrease, and the interface crack density will increase.

[0062] If the porosity of the first oxide sublayer 21 is greater than 3.8%, it will result in too many interconnected pores in the first oxide sublayer 21, which will reduce the mechanical strength of the first oxide sublayer 21 and may form through holes in local areas, increasing the risk of leakage.

[0063] The porosity of the second oxide sublayer 22 can be specifically exemplified as 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, or 1.2%, etc.

[0064] If the porosity of the second oxide sublayer 22 is less than 0.6%, the second oxide sublayer 22 will be too dense, resulting in increased internal stress, decreased interfacial adhesion, and reduced reliability.

[0065] If the porosity of the second oxide sublayer 22 is greater than 1.2%, the pores in the second oxide sublayer 22 will be too large, and the pores can form sodium ion migration channels, which will increase the PID attenuation and reduce the anti-PID performance of solar cell 1.

[0066] And / or, the interfacial dangling bond density of the first oxide sublayer 21 is greater than the interfacial dangling bond density of the second oxide sublayer 22.

[0067] Furthermore, the interfacial dangling bond density of the first oxide sublayer 21 is 3.2 × 10⁻⁶. 11 cm -2 ~4.5×10 11 cm -2 The interfacial dangling bond density of the second oxide sublayer 22 is ≤1.2×10⁻⁶. 11 cm -2 .

[0068] For example, the interfacial dangling bond density of the first oxide sublayer 21 can be 3.2 × 10⁻⁶. 11 cm -2 or 3.3×10 11 cm -2 or 3.4×10 11 cm -2 or 3.5×10 11 cm -2 or 3.6×10 11 cm -2 or 3.7×10 11 cm -2 or 3.8×10 11 cm -2 or 3.9×10 11 cm -2 or 4×10 11 cm -2 or 4.1×10 11 cm -2 or 4.2×10 11 cm -2 or 4.3×10 11 cm -2 or 4.4×10 11 cm -2 or 4.5×10 11 cm -2 wait.

[0069] If the dangling bond density of the first oxide sublayer 21 is greater than 3.2 × 10 11 cm -2 This leads to instability in the tunneling barrier height of the first oxide sublayer 21, a decrease in tunneling efficiency, large fluctuations in contact resistance, and poor consistency in the electrical performance of solar cell 1.

[0070] If the dangling bond density of the first oxide sublayer 21 is less than 4.5 × 10 11 cm -2 This leads to an excessively high interfacial recombination rate in the first oxide sublayer 21, resulting in a large recombination of charge carriers, a decrease in short-circuit current, and a decrease in open-circuit voltage.

[0071] For example, the interfacial dangling bond density of the second oxide sublayer 22 can be 1.2 × 10⁻⁶. 11 cm -2 or 1.1×10 11 cm -2 or 1×10 11 cm -2 or 0.9×10 11 cm -2 or 0.8×10 11 cm -2 or 0.7×10 11 cm -2 or 0.6×10 11 cm -2 or 0.5×10 11 cm -2 wait.

[0072] If the dangling bond density of the second oxide sublayer 22 is greater than 1.2 × 10 11 cm -2 This leads to severe recombination at the interface of the second oxide sublayer 22, a decrease in open-circuit voltage, and defect states becoming sodium ion trapping centers. Under bias, these defect states form fixed charges, exacerbating the PID effect and causing battery efficiency degradation.

[0073] And / or, the contact resistance of the first oxide sublayer 21 is less than the contact resistance of the second oxide sublayer 22.

[0074] Furthermore, the contact resistance of the first oxide sublayer 21 is 0.25Ω. cm 2 ~0.45Ω cm 2 The contact resistance of the second oxide sublayer 22 is ≥1×10⁻⁶. 9 Ω cm 2 .

[0075] For example, the contact resistance of the first oxide sublayer 21 can be 0.25Ω. cm 2 or 0.275Ω cm 2 or 0.3Ω cm 2 or 0.325Ω cm 2 or 0.35Ω cm 2 or 0.375Ω cm 2 or 0.4Ω cm 2 or 0.425Ω cm 2 or 0.45Ω cm 2 wait.

[0076] If the contact resistance of the first oxide layer 21 is less than 0.25Ω cm 2 This results in the first oxide sublayer 21 being too thin, making it prone to leakage, and the parallel resistance decreases.

[0077] If the contact resistance of the first oxide layer 21 is greater than 0.45Ω cm 2 This leads to a decrease in the fill factor and a reduction in the efficiency of solar cell 1.

[0078] For example, the contact resistance of the second oxide sublayer 22 can be 1×10⁻⁶. 9 Ω cm 2 or 1.2×10 9 Ω cm 2 or 1.4 × 10 9 Ω cm 2 or 1.6×10 9 Ω cm 2 or 1.8×10 9 Ω cm 2 or 2×10 9 Ω cm 2 or 2.2×10 9 Ω cm 2 or 2.4×10 9 Ω cm 2 or 2.6×10 9 Ω cm 2 or 2.8×10 9 Ω cm 2 or 3×10 9 Ω cm 2 wait.

[0079] If the contact resistance of the second oxide layer 22 is less than 1×10 9 Ω cm 2 This results in insufficient isolation effect of the second oxide sublayer 22, intensified sodium ion migration, and decreased anti-PID performance of solar cell 1.

[0080] In summary, this embodiment further limits the thickness, density, porosity, interfacial dangling bond density, and contact resistance of the first oxide sublayer 21 and the second oxide sublayer 22 to obtain a thin, sparse, porous first oxide sublayer 21 with high dangling bond density and low resistance. This results in a short carrier tunneling path, high tunneling probability, low contact resistance, and high current collection efficiency in the first oxide sublayer 21, thereby improving the fill factor of the solar cell 1. Furthermore, it obtains a thick, dense, less porous second oxide sublayer 22 with low dangling bond density and high resistance. This allows the second oxide sublayer 22 to form a dense physical barrier and a chemically stable interface, resulting in a tortuous sodium ion penetration path, low diffusion coefficient, and effective suppression of interfacial charge polarization, thus improving the anti-PID performance of the solar cell 1.

[0081] Please refer to Figure 1 In another embodiment, the phosphorus-doped polycrystalline silicon layer 30 is located in the conductive contact region 11 and is disposed away from the non-contact passivation region 12.

[0082] The phosphorus-doped polycrystalline silicon layer 30 forms a conductive structure, which includes multiple conductive parts arranged in an array. The width of the conductive parts is 40μm to 80μm, the spacing between the conductive parts is 0.8mm to 1.2mm, and the sheet resistance of the phosphorus-doped polycrystalline silicon layer 30 is 80Ω / sq to 100Ω / sq.

[0083] The phosphorus doping concentration of the conductive structure is 1×10⁻⁶. 20 cm -3 ~5×10 20 cm -3 .

[0084] Optionally, the thickness of the phosphorus-doped polycrystalline silicon layer 30 is 80 nm to 120 nm.

[0085] For example, using LPCVD (low-pressure chemical vapor deposition) technology, an intrinsic polycrystalline silicon layer is deposited on the tunnel oxide layer 20; then, the intrinsic polycrystalline silicon layer is phosphorus-doped to form a phosphorus-doped polycrystalline silicon layer 30. Furthermore, in the LPCVD process, the deposition temperature is 600℃~640℃, and the chamber pressure is 160Pa~200Pa.

[0086] The phosphorus-doped polysilicon layer 30 is only disposed in the conductive contact region 11, and there is no phosphorus-doped polysilicon layer 30 in the non-contact passivation region 12. For example, the phosphorus-doped polysilicon layer 30 located in the non-contact passivation region 12 can be removed by photolithography alignment and dry etching processes.

[0087] Conductive structures can also be understood as Polyfinger patterned structures. For example, conductive structures are formed through photolithography alignment and dry etching processes.

[0088] The width of the conductive part can be specifically exemplified as 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, 75μm, or 80μm, etc.

[0089] Specific examples of the spacing between conductive parts include 0.8mm, 0.9mm, 1mm, 1.1mm, or 1.2mm.

[0090] The sheet resistance of the phosphorus-doped polycrystalline silicon layer 30 can be specifically exemplified as 80Ω / sq, or 82Ω / sq, or 84Ω / sq, or 86Ω / sq, or 88Ω / sq, or 90Ω / sq, or 92Ω / sq, or 94Ω / sq, or 96Ω / sq, or 98Ω / sq, or 100Ω / sq, etc.

[0091] For example, the phosphorus doping concentration of the conductive structure can be 1×10⁻⁶. 20 cm -3 or 1.5×10 20 cm -3 or 2×10 20 cm -3 or 2.5×10 20 cm -3 or 3×10 20 cm -3 or 3.5×10 20 cm -3 or 4×10 20 cm -3 or 4.5×10 20 cm -3 or 5×10 20 cm -3 wait.

[0092] Therefore, this embodiment removes the phosphorus-doped polysilicon layer 30 in the non-contact passivation region 12 and selectively performs high-concentration plasma doping only on the conductive structure to precisely construct an interface negative electric field shielding layer. Through the field effect, it actively repels cation migration and counteracts high-voltage polarization charge, thereby suppressing PID decay from the electric field dimension without damaging the passivation performance.

[0093] Please refer to Figure 2 In another embodiment, the passivation layer 40 includes a transition sub-layer 41 and a barrier sub-layer 42. The transition sub-layer 41 is disposed on the phosphorus-doped polysilicon layer 30 and is a SiOxNy layer. The barrier sub-layer 42 is disposed on the side of the transition sub-layer 41 away from the phosphorus-doped polysilicon layer 30 and is a SiNx layer.

[0094] The transition sublayer 41 is in direct contact with the phosphorus-doped polycrystalline silicon layer 30. The interface stress of the transition sublayer 41 is small and the adhesion is strong. Moreover, the transition sublayer 41 is a SiOxNy layer, which contains oxygen elements that can further chemically passivate silicon dangling bonds and reduce the interface state density.

[0095] The barrier layer 42 is a SiNx layer, which has excellent chemical stability and sodium ion blocking ability, good density, and effectively blocks the permeation of ions and water vapor.

[0096] Therefore, this embodiment solves the problems of numerous defects and weak barrier ability of traditional single-layer passivation layer 40 by setting a passivation layer 40 composed of a transition sublayer 41 and a barrier sublayer 42. The transition sublayer 41 buffers the stress of the patterned structure and seals micro-defects, while the barrier sublayer 42 blocks the penetration of ions and water vapor.

[0097] Furthermore, the total thickness of the passivation layer 40 is 70nm~90nm.

[0098] The total thickness of the passivation layer 40 can be exemplified by 70nm, 75nm, 80nm, 85nm, or 90nm, etc.

[0099] And / or, the thickness of the transition sublayer 41 is 20nm~30nm.

[0100] The thickness of the transition sublayer 41 can be specifically exemplified as 20nm, 22nm, 24nm, 26nm, 28nm, or 30nm, etc.

[0101] And / or, the thickness of the barrier sublayer 42 is 50nm~60nm.

[0102] The thickness of the barrier sublayer 42 can be specifically exemplified as 50nm, 52nm, 54nm, 56nm, 58nm, or 60nm, etc.

[0103] And / or, the refractive index of the barrier sublayer 42 is 2.05~2.15.

[0104] The refractive index of the barrier sublayer 42 can be specifically exemplified as 2.05, 2.07, 2.09, 2.11, 2.13, or 2.15, etc.

[0105] The refractive index of the barrier sublayer 42 is 2.05~2.15, which can form a good refractive index gradient between air and silicon, reduce light reflectivity, and enable the barrier sublayer 42 to have both optical anti-reflection and electrical isolation functions.

[0106] Please refer to Figures 1-3 This application also provides a method for preparing a solar cell 1, the method comprising: S100, a substrate 10 is provided, the substrate 10 having a conductive contact area 11 corresponding to the electrode and a non-contact passivation area 12 avoiding the electrode.

[0107] For example, a 130μm thick n-type monocrystalline silicon wafer is selected and subjected to alkaline texturing, alternating acid and alkali cleaning, pure water ultra-clean rinsing, and hot air drying processes to thoroughly remove oil stains, metal impurities, and cutting damage layers from the silicon wafer surface, obtaining a clean back substrate with a surface flatness of ≤0.5μm, thus eliminating the potential for composite defects caused by substrate impurities.

[0108] S200, a tunneling oxide layer 20 is formed on the substrate 10. The tunneling oxide layer 20 includes a first oxide sublayer 21 located in the conductive contact region 11 and a second oxide sublayer 22 located in the non-contact passivation region 12. The oxygen-silicon ratio of the first oxide sublayer 21 is (1.85~1.92):1, and the oxygen-silicon ratio of the second oxide sublayer 22 is (1.98~2.02):1.

[0109] For example, by using a segmented heating thermal oxidation process, the oxygen flux and the zoned heat preservation time are precisely controlled to form a differentiated first oxide sublayer 21 and second oxide sublayer 22 on the back of the battery.

[0110] Furthermore, the heating rate is 2℃ / min~3℃ / min, and 6000sccm~8000sccm of nitrogen is introduced into the furnace tube throughout the process as a protective base gas, and the pressure inside the furnace is stabilized at 750mbar~850mbar; the temperature is raised to 850℃~900℃ for isothermal oxidation.

[0111] S300, a phosphorus-doped polysilicon layer 30 is formed on the side of the tunneling oxide layer 20 opposite to the substrate 10.

[0112] For example, an 80nm~120nm phosphorus-doped polysilicon layer 30 is deposited on the surface of the tunneling oxide layer 20 using LPCVD technology at a deposition temperature of 600℃~640℃ and a chamber pressure of 160Pa~200Pa. The phosphorus-doped polysilicon layer 30 located in the non-contact passivation region 12 is removed by photolithography alignment and dry etching processes to prepare an array-type conductive structure.

[0113] Phosphine plasma doping technology was used to locally dope the conductive structure, with a doping power of 150W~200W and a doping time of 30s~60s, thereby increasing the phosphorus doping concentration of the conductive structure to 1×10⁻⁶. 20 cm -3 ~5×10 20 cm -3 .

[0114] S400, a passivation layer 40 is formed on the side of the phosphorus-doped polysilicon layer 30 opposite to the substrate 10.

[0115] For example, a SiOxNy transition sublayer 41 is deposited over the entire back of the battery using PECVD process, followed by the deposition of a SiNx barrier sublayer 42 to achieve dual barrier against water vapor and metal ions.

[0116] Please refer to the above description of the substrate 10, tunneling oxide layer 20, phosphorus-doped polysilicon layer 30, and passivation layer 40 in this application, and will not be repeated here.

[0117] In another embodiment, during the formation of the tunnel oxide layer 20, the process pressure is 750 mbar to 850 mbar, the process temperature is 850°C to 900°C, and the nitrogen flow rate is 6000 sccm to 8000 sccm.

[0118] Specifically, during the formation of the tunnel oxide layer 20, the process pressure can be exemplified as 750 mbar, 760 mbar, 770 mbar, 780 mbar, 790 mbar, 800 mbar, 810 mbar, 820 mbar, 830 mbar, 840 mbar, or 850 mbar, etc.

[0119] Specific examples of process temperatures include 850℃, 860℃, 870℃, 880℃, 890℃, and 900℃.

[0120] Specific examples of nitrogen flow rates include 6000 sccm, 6500 sccm, 7000 sccm, 7500 sccm, or 8000 sccm.

[0121] By limiting the process pressure, process temperature, and nitrogen flow rate during the formation of the tunnel oxide layer 20, a stable low-pressure chemical vapor deposition environment is formed, the oxidation rate is controllable, the film thickness uniformity is small, and the consistency between the cells and between cells of the solar cell 1 is high.

[0122] In step S200, which forms the first oxide sublayer 21, the following is included: The initial oxygen flow rate of the dry oxygen was controlled at 1200 sccm to 1800 sccm, and the initial oxidation time was 8 min to 12 min.

[0123] The first oxygen flow rate for dry oxygen can be exemplified by 1200 sccm, 1300 sccm, 1400 sccm, 1500 sccm, 1600 sccm, 1700 sccm, or 1800 sccm, etc.

[0124] The specific first oxidation time can be 8 min, 9 min, 10 min, 11 min, or 12 min, etc.

[0125] In step S200 of forming the second oxide sublayer 22, the following are included: The second oxygen flow rate of the dry oxygen is controlled at 3500 sccm~5000 sccm, and the second oxidation time is 18 min~28 min.

[0126] Specific examples of the second oxygen flow rate for dry oxygen include 3500 sccm, 3600 sccm, 3700 sccm, 3800 sccm, 3900 sccm, 4000 sccm, 4100 sccm, 4200 sccm, 4300 sccm, 4400 sccm, 4500 sccm, 4600 sccm, 4700 sccm, 4800 sccm, 4900 sccm, or 5000 sccm, etc.

[0127] The second oxidation time can be exemplified by 18 min, 19 min, 20 min, 21 min, 22 min, 23 min, 24 min, 25 min, 26 min, 27 min, or 28 min, etc.

[0128] This embodiment uses staged control of oxygen flow rate and oxidation time of dry oxygen to obtain a first oxide sublayer 21 and a second oxide sublayer 22 with different functions to adapt to the conductive contact region 11 and the non-contact passivation region 12, so that the tunneling oxide layer 20 can be adapted to the Polyfinger patterned structure, taking into account the high efficiency and high anti-PID stability of the solar cell 1.

[0129] Optionally, after oxidation is complete, oxygen is cut off, nitrogen flow rate is increased to 10000 sccm, purging for 6 minutes, and then the temperature is reduced to 600℃ at 3℃ / min before being removed from the furnace, thereby controlling the overall thickness of the first oxide sublayer 21 and the second oxide sublayer 22 to within ±0.1nm.

[0130] In another embodiment, after the passivation layer 40 is formed, an annealing process is performed in a protective atmosphere, the annealing process comprising: The first annealing stage is carried out, wherein the first annealing temperature is 400℃~450℃ and the first annealing time is 50s~70s; The second annealing stage is carried out, wherein the second annealing temperature is 600℃~650℃ and the second annealing time is 30s~50s; The third annealing stage is carried out, with the third annealing temperature being 750℃~800℃ and the third annealing time being 10s~30s.

[0131] Optionally, the protective atmosphere is selected from at least one of nitrogen and inert gases.

[0132] Specifically, the first annealing temperature can be exemplified by 400℃, 410℃, 420℃, 430℃, 440℃, or 450℃, etc.

[0133] Specific examples of the first annealing time include 50s, 52s, 54s, 56s, 58s, 60s, 62s, 64s, 66s, 68s, or 70s.

[0134] The second annealing temperature can be exemplified by 600℃, 610℃, 620℃, 630℃, 640℃, or 650℃.

[0135] The specific examples of the second annealing time are 30s, 32s, 34s, 36s, 38s, 40s, 42s, 44s, 46s, 48s, or 50s, etc.

[0136] The third annealing temperature can be exemplified by 750℃, 760℃, 770℃, 780℃, 790℃, or 800℃, etc.

[0137] The specific annealing time can be 10s, 12s, 14s, 16s, 18s, 20s, 22s, 24s, 26s, 28s, or 30s, etc.

[0138] Therefore, this embodiment employs a three-stage annealing process. In the first annealing stage, residual moisture and organic impurities at the interface are removed, and interface stress is released. In the second annealing stage, doped ions are fully activated, and the doping distribution at the interface is homogenized. In the third annealing stage, the passivation layer 40 and the polycrystalline silicon structure are solidified, and edge defects generated by the patterning process are repaired. This balances the high efficiency and high PID resistance of the solar cell 1, and a TOPCon cell with a Polyfinger structure and low PID degradation is prepared.

[0139] This application also provides a photovoltaic module, which includes the solar cell provided above in this application.

[0140] The photovoltaic module provided in this application adopts the solar cell provided in this application. The solar cell divides the tunneling oxide layer into regions by combining the conductive contact area and the non-contact passivation area. The first oxide sublayer has a relatively high silicon content and is an oxygen-deficient sub-oxide structure, which reduces the carrier tunneling barrier, reduces the contact resistance, and improves the tunneling conductivity, thereby improving the fill factor and conversion efficiency of the solar cell. Furthermore, the oxygen-silicon ratio of the second oxide sublayer is close to the standard silica stoichiometry, with a dense structure, excellent chemical stability, and low interfacial dangling bond density, which effectively blocks the migration of sodium ions along the defect channel, suppresses interfacial charge polarization, forms a dense physical ion barrier, and improves the anti-PID performance of the solar cell.

[0141] Therefore, this application adapts the tunneling oxide layer to the Polyfinger patterned structure by setting a first oxide sublayer and a second oxide sublayer with different functions to the conductive contact area and the non-contact passivation area, thus balancing the high efficiency and high PID resistance stability of the solar cell.

[0142] To make the objectives and advantages of this application clearer, the effects of the solar cell preparation method of this application will be further explained in detail below with reference to specific embodiments 1-2 and comparative example 1.

[0143] Example 1: Step 1, silicon wafer substrate pretreatment: Select a 130μm thick n-type monocrystalline silicon wafer, and perform alkaline texturing, acid-alkali alternating cleaning, pure water ultra-clean rinsing, and 120℃ hot air drying for 20 minutes to remove surface oil, metal impurities, and cut the damaged layer to obtain a clean and flat back substrate.

[0144] Step 2, Preparation of the tunneling oxide layer: Segmented heating thermal oxidation was used, with a heating rate of 2.5℃ / min and an oxidation temperature of 880℃; the substrate nitrogen gas concentration was 6500 sccm. Preparation of the first oxide sublayer: The first oxygen flow rate of dry oxygen was 1500 sccm, and the temperature was maintained for 10 min. The film thickness was 1.3 nm, and the O:Si ratio was approximately 1.88:1. Preparation of the second oxide sublayer: The oxygen flow rate of the dry oxygen was 4200 sccm, the temperature was maintained for 22 min, the film thickness was 2.0 nm, and the O:Si ratio was approximately 1.99:1. Subsequent nitrogen purging and cooling before unloading ensured thickness control accuracy of ±0.1nm.

[0145] Step 3, fabrication of conductive structure: A 100nm phosphorus-doped polysilicon layer was deposited using LPCVD process at a deposition temperature of 620℃ and a chamber pressure of 180Pa; an array conductive structure was fabricated by photolithography alignment and dry etching, with a conductive part width of 60μm, a conductive part spacing of 1.0mm, and a sheet resistance of 90Ω / sq for the phosphorus-doped polysilicon layer.

[0146] Step 4, selective plasma doping modification of the conductive structure: localized doping with phosphine plasma was performed at a power of 180 W for 45 s; the phosphorus doping concentration of the conductive structure reached 3 × 10⁻⁶. 20 cm -3 This forms a stable interface negative electric field shielding layer.

[0147] Step 5, preparation of passivation layer: A composite passivation layer is deposited using PECVD process. The thickness of the transition sublayer is 25 nm, the thickness of the barrier sublayer is 55 nm, and the total thickness of the passivation layer is 80 nm. The refractive index of the barrier sublayer is 2.10.

[0148] Step 6, Annealing: Nitrogen inert protection throughout the process, three-stage annealing process: 420℃ low temperature holding for 60s, 630℃ medium temperature holding for 40s, 780℃ high temperature holding for 20s, to complete impurity removal, doping activation, structural curing and defect repair.

[0149] Example 2: Step one is the same as step one in Example 1.

[0150] Step 2, Preparation of tunneling oxide layer: Segmented heating thermal oxidation is adopted, with a heating rate of 2℃ / min and an oxidation temperature of 860℃; the substrate nitrogen gas is 6300 sccm; Preparation of the first oxide sublayer: The first oxygen flow rate of dry oxygen was 1300 sccm, and the temperature was maintained for 9 min. The film thickness was 1.2 nm, and the O:Si ratio was approximately 1.86:1. Preparation of the second oxide sublayer: The oxygen flow rate of the dry oxygen was 3800 sccm, the temperature was maintained for 20 min, the film thickness was 1.9 nm, and the O:Si ratio was approximately 1.98:1; Subsequent nitrogen purging and cooling before unloading ensured thickness control accuracy of ±0.1nm.

[0151] Step 3, fabrication of conductive structure: A 90nm phosphorus-doped polysilicon layer was deposited using LPCVD process at a deposition temperature of 610℃ and a chamber pressure of 170Pa; an array conductive structure was fabricated by photolithography alignment and dry etching, with a conductive part width of 50μm, a conductive part spacing of 0.9mm, and a sheet resistance of 85Ω / sq for the phosphorus-doped polysilicon layer.

[0152] Step 4, selective plasma doping modification of the conductive structure: localized doping with phosphine plasma was performed at a power of 160 W for 35 s; the phosphorus doping concentration of the conductive structure reached 2 × 10⁻⁶. 20 cm -3 This forms a uniform negative electric field shielding layer.

[0153] Step 5, preparation of passivation layer: A composite passivation layer is deposited using PECVD process. The thickness of the transition sublayer is 20 nm, the thickness of the barrier sublayer is 50 nm, and the total thickness of the passivation layer is 70 nm. The refractive index of the barrier sublayer is 2.08.

[0154] Step 6, Annealing: Nitrogen inert protection throughout the process, three-stage annealing process: 410℃ low temperature holding for 60s, 620℃ medium temperature holding for 40s, 760℃ high temperature holding for 20s.

[0155] Comparative Example 1: Step one is the same as step one in Example 1.

[0156] Step 2, Tunneling oxide layer preparation: Using the traditional global uniform thickness thermal oxidation process, a uniform 1.5nm SiO2 tunneling oxide layer is prepared on the back side, with no partitioned differential structure.

[0157] The uniform dry oxygen flow rate is 2200 sccm, and the temperature is kept constant at 870℃ for 15 minutes at one time. A uniform 1.5nm thick SiO2 tunneling oxide layer is generated on the entire silicon wafer. The overall O:Si ≈ 1.90:1 and porosity ≈ 2.6%. Without the segmented oxidation and time- and zoned oxidation steps, it is impossible to take into account both tunneling conductivity and ion barrier performance.

[0158] Step 3, Preparation of conductive structure: Deposit a 100nm global phosphorus-doped polycrystalline silicon layer to prepare a conductive structure consistent with that in Example 1. The sheet resistance of the phosphorus-doped polycrystalline silicon layer is 90Ω / sq.

[0159] Step four: Non-localized selective plasma doping process, using thin film native uniform doping, without interface electric field enhancement structure.

[0160] Step 5, preparation of the passivation layer: only a single 80nm SiNx monolayer passivation film is deposited, without the SiOxNy transition sublayer.

[0161] Step 6, Annealing: Using the traditional single high-temperature annealing process, the temperature is kept constant at 780℃ for 20 seconds, without segmented gradient impurity removal, activation, or curing processes.

[0162] The electrical performance data of the solar cells in Examples 1-2 and Comparative Example 1 are shown in Table 1: Table 1: Electrical performance data of solar cells in Examples 1-2 and Comparative Example 1

[0163] In summary, by adopting the solar cell fabrication method provided in this application, the tunneling oxide layer is adapted to the Polyfinger patterned structure, achieving both high efficiency and high PID resistance stability of the solar cell. The specific beneficial effects are as follows: First, the anti-PID performance is greatly improved: compared with the traditional battery in Comparative Example 1, the PID decay rate of Examples 1-2 is reduced by more than 75%, completely solving the problem of severe PID decay in the Polyfinger structure.

[0164] Second, photoelectric performance is improved without loss and with a slight increase: traditional anti-PID process will cause the cell efficiency to decrease by 0.3%-0.6%; however, the initial conversion efficiency of the solar cells in Examples 1-2 is 0.3%~0.4% higher than that of Comparative Example 1, and the fill factor is not decayed, thus achieving a two-way improvement in anti-PID performance and power generation efficiency.

[0165] Third, the interface stability is significantly enhanced: after testing, the battery interface defect density is reduced by more than 40% compared with the traditional process, and there are no failure problems such as passivation layer peeling, ion penetration, and interface polarization. It can be adapted to harsh working conditions such as coastal areas, high temperature and humidity, and high voltage power stations.

[0166] Fourth, it has excellent economic efficiency in mass production: This application requires no new equipment or complex process modifications, and the cost of single-cell preparation does not increase significantly. It is compatible with existing TOPCon mass production lines.

[0167] Unless otherwise stated or in case of conflict, the terms or phrases used in this application shall have the following meanings: In this application, terms such as "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined with "first" or "second" may explicitly or implicitly include at least one of that feature.

[0168] In this application, "one or more" refers to any one, any two, or any two or more of the listed items. "Several" refers to any two or more.

[0169] In this application, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," and "counterclockwise," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.

[0170] In this application, unless otherwise expressly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part. They can refer to a mechanical connection or an electrical connection. They can refer to a direct connection or an indirect connection through an intermediate medium, or the internal communication of two components or the interaction between two components. For those skilled in the art, the specific meaning of the above terms in this application can be understood according to the specific circumstances.

[0171] In this application, the terms "embodiment" and "implementation" mean that a specific feature, structure, or characteristic described in connection with an embodiment can be included in at least one embodiment of this application. The appearance of these phrases in various locations throughout the specification does not necessarily refer to the same embodiment, nor are they independent or alternative embodiments mutually exclusive with other embodiments. Those skilled in the art will understand, explicitly and implicitly, that the embodiments described in this application can be combined with other embodiments. Furthermore, it should be understood that the features, structures, or characteristics described in the various embodiments of this application can be arbitrarily combined to form yet another embodiment that does not depart from the spirit and scope of the technical solution of this application, provided there is no contradiction between them.

[0172] The above description represents some embodiments of this application. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of this application, and these improvements and modifications are also considered to be within the scope of protection of this application.

Claims

1. A solar cell, characterized in that, The solar cell comprises a substrate, a tunneling oxide layer, a phosphorus-doped polycrystalline silicon layer, and a passivation layer stacked sequentially. The substrate has a conductive contact area corresponding to the electrode and a non-contact passivation area that avoids the electrode. The tunneling oxide layer includes a first oxide sub-layer located in the conductive contact area and a second oxide sub-layer located in the non-contact passivation area. The oxygen-silicon ratio of the first oxide sub-layer is (1.85~1.92):1, and the oxygen-silicon ratio of the second oxide sub-layer is (1.98~2.02):

1.

2. The solar cell as described in claim 1, characterized in that, The thickness of the first oxide sublayer is less than the thickness of the second oxide sublayer; And / or, the density of the first oxide sublayer is less than the density of the second oxide sublayer; And / or, the porosity of the first oxide sublayer is greater than the porosity of the second oxide sublayer; And / or, the interfacial dangling bond density of the first oxide sublayer is greater than that of the second oxide sublayer; And / or, the contact resistance of the first oxide sublayer is less than the contact resistance of the second oxide sublayer.

3. The solar cell as described in claim 1, characterized in that, The thickness of the first oxide sublayer is 1.2 nm to 1.5 nm, and the thickness of the second oxide sublayer is 1.8 nm to 2.2 nm. And / or, the density of the first oxide sublayer is 2.05 g / cm³. 3 ~2.12g / cm 3 The density of the second oxide sublayer is 2.18 g / cm³. 3 ~2.22g / cm 3 ; And / or, the porosity of the first oxide sublayer is 2.8%~3.8%, and the porosity of the second oxide sublayer is 0.6%~1.2%; And / or, the interfacial dangling bond density of the first oxide sublayer is 3.2 × 10⁻⁶. 11 cm -2 ~4.5×10 11 cm -2 The interfacial dangling bond density of the second oxide sublayer is ≤1.2×10⁻⁶. 11 cm -2 ; And / or, the contact resistance of the first oxide sublayer is 0.25Ω. cm 2 ~0.45Ω cm 2 The contact resistance of the second oxide sublayer is ≥1×10 9 Ω cm 2 .

4. The solar cell as described in claim 1, characterized in that, The phosphorus-doped polycrystalline silicon layer is located in the conductive contact region and is disposed away from the non-contact passivation region; The phosphorus-doped polycrystalline silicon layer forms a conductive structure, which includes multiple conductive parts arranged in an array. The width of the conductive parts is 40μm to 80μm, the spacing between the conductive parts is 0.8mm to 1.2mm, and the sheet resistance of the phosphorus-doped polycrystalline silicon layer is 80Ω / sq to 100Ω / sq. The phosphorus doping concentration of the conductive structure is 1×10⁻⁶. 20 cm -3 ~5×10 20 cm -3 .

5. The solar cell as described in claim 1, characterized in that, The passivation layer includes: A transition sublayer is disposed on the phosphorus-doped polycrystalline silicon layer, wherein the transition sublayer is a SiOxNy layer; A barrier sublayer is disposed on the side of the transition sublayer away from the phosphorus-doped polycrystalline silicon layer, and the barrier sublayer is a SiNx layer.

6. The solar cell as described in claim 5, characterized in that, The total thickness of the passivation layer is 70nm~90nm; And / or, the thickness of the transition sublayer is 20nm~30nm; And / or, the thickness of the barrier sublayer is 50nm~60nm; And / or, the refractive index of the barrier sublayer is 2.05~2.

15.

7. A method for preparing a solar cell, characterized in that, The preparation method includes: A substrate is provided, the substrate having a conductive contact area corresponding to an electrode and a non-contact passivation area that avoids the electrode; A tunneling oxide layer is formed on the substrate, the tunneling oxide layer comprising a first oxide sublayer located in the conductive contact region and a second oxide sublayer located in the non-contact passivation region, the oxygen-silicon ratio of the first oxide sublayer being (1.85~1.92):1, and the oxygen-silicon ratio of the second oxide sublayer being (1.98~2.02):1; A phosphorus-doped polycrystalline silicon layer is formed on the side of the tunneling oxide layer opposite to the substrate; A passivation layer is formed on the side of the phosphorus-doped polysilicon layer opposite to the substrate.

8. The method for preparing a solar cell as described in claim 7, characterized in that, During the formation of the tunnel oxide layer, the process pressure is 750 mbar to 850 mbar, the process temperature is 850°C to 900°C, and the nitrogen flow rate is 6000 sccm to 8000 sccm. The step of forming the first oxide sublayer includes: The initial oxygen flow rate of the dry oxygen was controlled at 1200 sccm to 1800 sccm, and the initial oxidation time was 8 min to 12 min. The step of forming the second oxide sublayer includes: The second oxygen flow rate of the dry oxygen is controlled at 3500 sccm~5000 sccm, and the second oxidation time is 18 min~28 min.

9. The method for preparing a solar cell as described in claim 7, characterized in that, After the passivation layer is formed, an annealing process is performed in a protective atmosphere. The annealing process includes the following steps: The first annealing stage is carried out, wherein the first annealing temperature is 400℃~450℃ and the first annealing time is 50s~70s; The second annealing stage is carried out, wherein the second annealing temperature is 600℃~650℃ and the second annealing time is 30s~50s; The third annealing stage is carried out, with the third annealing temperature being 750℃~800℃ and the third annealing time being 10s~30s.