Solar cells and their preparation methods, photovoltaic modules
By employing a differentiated textured surface design on the front and back sides of the HTBC battery, combined with the doping type of the passivated contact structure, the problem of the imbalance between optical and electrical performance in the HTBC battery was solved, thereby improving battery efficiency.
Patent Information
- Application Number
- CN202611266549.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
In existing HTBC battery structures, the front and back textured surfaces are the same size, or only the front surface is optimized while the back surface passivation is ignored. This makes it difficult to balance optical and electrical performance, thus affecting battery conversion efficiency.
A differentiated textured surface design is adopted, with a small textured surface structure on the front of the battery to optimize optical performance and a large textured surface structure on the back to improve passivation. By adjusting the size and specific surface area of the textured surface structure and combining it with the doping type of the passivation contact structure, the differentiated configuration of the front and back of the battery can be achieved.
This improved the short-circuit current, fill factor, and series resistance of solar cells, thereby enhancing photoelectric conversion efficiency.
Smart Images

Figure CN123124454A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photovoltaic cell technology, specifically relating to a solar cell and its preparation method, and a photovoltaic module. Background Technology
[0002] With the increasing depletion of fossil fuels, solar energy, as a clean and renewable energy source, has been widely adopted. As research progresses, significant breakthroughs have been made in the conversion efficiency of crystalline silicon solar cells. Cell structures have also evolved from passivated emitter and rear cell (PERC) to heterojunction technology (HJT), tunnel oxide passivated contact (TOPCon), and back contact (BC) cells.
[0003] Solar cell efficiency is primarily limited by both optical and electrical aspects. For heterojunction tunnel oxide back contact (HTBC) cells, the grid-free design on the front eliminates electrode shading losses, and combined with an anti-reflective coating on the light-receiving surface, optical performance can be effectively improved. Simultaneously, optical gains in cell efficiency can also be achieved by designing small-sized textured structures; however, small-sized textured structures are more difficult to passivate, thus affecting the passivation effect on the back side.
[0004] The information disclosed in this background section is intended only to enhance the understanding of the overall background of the invention and should not be construed as an admission or in any way implying that the information constitutes prior art known to those skilled in the art. Summary of the Invention
[0005] The purpose of this invention is to provide a solar cell and its preparation method, as well as a photovoltaic module, which can improve the conversion efficiency and performance of the cell.
[0006] To achieve the above objectives, a specific embodiment of the present invention provides the following technical solution:
[0007] A solar cell, comprising:
[0008] The substrate has a light-receiving surface and a backlighting surface disposed opposite to each other. A first velvet structure is formed on the light-receiving surface, and the backlighting surface includes an alternately distributed first region and a second region. A second velvet structure is formed on the first region, and the average bottom size of the second velvet structure is greater than the average bottom size of the first velvet structure.
[0009] A first passivation contact structure is provided at least in a first region of the backlight surface, and the first passivation contact structure includes a first doped layer;
[0010] A second passivation contact structure is disposed in a second region of the backlight surface. The second passivation contact structure includes a second doped layer, the doping type of which is opposite to that of the first doped layer.
[0011] In one or more embodiments of the present invention, the specific surface area of the backlight surface is greater than the specific surface area of the light-receiving surface.
[0012] In one or more embodiments of the present invention, the ratio of the specific surface area of the backlight surface to the specific surface area of the light-receiving surface is (1.1-2):1.
[0013] In one or more embodiments of the present invention, the first velvet structure and the second velvet structure are both pyramid velvet structures, wherein the average bottom size of the pyramid in the first velvet structure is 0.5μm-3μm, and the average bottom size of the pyramid in the second velvet structure is 2μm-6μm.
[0014] In one or more embodiments of the present invention, the first passivated contact structure further includes an intrinsic layer, wherein the first doped layer is stacked on the surface of the intrinsic layer;
[0015] The second passivated contact structure further includes a tunneling layer, and the second doped layer is stacked on the surface of the tunneling layer.
[0016] In one or more embodiments of the present invention, the solar cell further includes:
[0017] A dielectric layer is disposed on the light-receiving surface of the substrate;
[0018] A conductive layer is disposed on one side of the backlight surface. The conductive layer includes a first conductive portion and a second conductive portion disposed separately. The first conductive portion is in contact with the first doped layer, and the second conductive portion is in contact with the second doped layer.
[0019] The first electrode is in contact with the first conductive part;
[0020] The second electrode is in contact with the second conductive part.
[0021] A method for fabricating a solar cell, comprising:
[0022] A substrate is provided, the substrate having a light-receiving surface and a backlighting surface disposed opposite to each other, the backlighting surface comprising an alternately distributed first region and a second region;
[0023] A second passivated contact structure is prepared on the light-receiving surface and the backlight surface, and a first mask layer is formed thereon. The second passivated contact structure includes a second doped layer.
[0024] Remove the first mask layer from the first region of the backlight surface;
[0025] The substrate is subjected to a first texturing process to remove the second passivation contact structure in the first region of the backlight surface and form an initial texturing structure on the substrate surface in the first region.
[0026] Remove the first mask layer from the light-receiving surface;
[0027] A second texturing process is performed on the substrate to remove the second passivation contact structure of the light-receiving surface and form a first texturing structure on the substrate surface of the light-receiving surface. At the same time, the initial texturing structure on the substrate surface of the first region is etched to form a second texturing structure. The average bottom size of the second texturing structure is greater than the average bottom size of the first texturing structure.
[0028] A first passivated contact structure is prepared in a first region of the backlight surface. The first passivated contact structure includes a first doped layer, the doping type of which is opposite to that of the second doped layer.
[0029] In one or more embodiments of the present invention, a laser process is used to remove the first mask layer of the first region of the backlight surface; and / or,
[0030] The first mask layer of the light-receiving surface is removed by acid etching.
[0031] In one or more embodiments of the present invention, in the first texturing process, the texturing solution is a mixed solution containing an alkaline solution and a texturing additive, the texturing temperature is 65℃-80℃, and the texturing time is 300s-700s.
[0032] In one or more embodiments of the present invention, the alkaline solution comprises a KOH solution or a NaOH solution with a concentration of 3 vol%-10 vol%; and / or,
[0033] The concentration of the fabrication additive is 1 vol%-5 vol.
[0034] In one or more embodiments of the present invention, in the second texturing process, the texturing solution is a mixed solution containing an alkaline solution and texturing additives, the texturing temperature is 65℃-80℃, and the texturing time is 300s-700s.
[0035] In one or more embodiments of the present invention, the alkaline solution comprises a KOH solution or a NaOH solution with a concentration of 1.5 vol%-5 vol%; and / or,
[0036] The concentration of the fabrication additive is 1 vol%-5 vol.
[0037] In one or more embodiments of the present invention, a first passivated contact structure is prepared in a first region of the backlight surface, including:
[0038] A first passivation contact structure is formed on one side of the backlight surface, the first passivation contact structure covering the substrate surface of the first region and the surface of the second passivation contact structure covering the second region;
[0039] A laser process is used to remove part or all of the first passivated contact structure in the second region, exposing the second passivated contact structure.
[0040] In one or more embodiments of the present invention, after the laser process, the method further includes a step of wet processing the exposed surface of the second passivated contact structure:
[0041] The exposed surface of the second passivated contact structure is cleaned with an acidic solution to remove the heat-affected zone and / or molten residue generated by the laser process.
[0042] In one or more embodiments of the present invention, the method for preparing the solar cell further includes:
[0043] A dielectric layer is prepared on the light-receiving surface;
[0044] A conductive layer is formed on one side of the backlight surface and etched to form a first conductive portion that contacts the first doped layer and a second conductive portion that contacts the second doped layer;
[0045] A first electrode is prepared that contacts the first conductive part, and a second electrode is prepared that contacts the second conductive part.
[0046] A photovoltaic module includes the solar cell described above, or includes a solar cell prepared by the method described above for preparing a solar cell.
[0047] Compared with existing technologies, the solar cell and its fabrication method, as well as the photovoltaic module of the present invention, feature a small-sized textured structure on the light-receiving surface combined with a dielectric layer on the light-receiving surface, thereby enhancing the optical performance of the light-receiving surface. The large-sized textured structure on the back surface facilitates the uniform deposition of the first passivation contact structure, resulting in excellent chemical passivation. Through the differentiated design of the textured structure dimensions on the light-receiving and back surfaces, the short-circuit current and fill factor of the solar cell are improved, thereby enhancing the photoelectric conversion efficiency.
[0048] The solar cell and its preparation method, as well as the photovoltaic module of the present invention, feature a large-size textured back surface structure that facilitates more uniform and continuous deposition of the conductive layer, promotes lateral transport of charge carriers, reduces the series resistance Rs of the cell, and improves the photoelectric conversion efficiency of the cell. Attached Figure Description
[0049] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0050] Figure 1 This is a schematic cross-sectional view of the solar cell in this invention;
[0051] Figure 2 This is a process flow diagram of the method for preparing solar cells in this invention;
[0052] Figures 3a to 3k This is a schematic diagram of the process steps for fabricating the solar cell in this application;
[0053] Figure 4 This is a scanning electron microscope image of the textured surface of the light-receiving surface in Example 1;
[0054] Figure 5 This is a histogram (particle size distribution map) of the bottom size distribution of the velvety pyramid structure on the light-receiving surface in Example 1, where the horizontal axis (X-axis) is the size (diameter) of the pyramid bottom, and the vertical axis (Y-axis) is the frequency (the number of pyramids within a certain size range).
[0055] Figure 6 This is a scanning electron microscope image of the textured surface of the backlight in Example 1;
[0056] Figure 7 This is a histogram (particle size distribution diagram) of the bottom size distribution of the velvet structure pyramid on the backlit side in Example 1, where the horizontal axis (X-axis) is the size (diameter) of the pyramid bottom, and the vertical axis (Y-axis) is the frequency (the number of pyramids within a certain size range).
[0057] Figure 8 Scanning electron microscope images of the textured surface of the illuminated and shaded sides in Comparative Example 1;
[0058] Figure 9 The histogram (particle size distribution) shows the size distribution of the base of the velvety pyramid on the light-receiving and back-lit sides in Comparative Example 1. The horizontal axis (X-axis) represents the size (diameter) of the pyramid base, and the vertical axis (Y-axis) represents the frequency (the number of pyramids within a certain size range). Detailed Implementation
[0059] To enable those skilled in the art to better understand the technical solutions in this disclosure, the technical solutions in the embodiments of this disclosure will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this disclosure, and not all embodiments. Based on the embodiments in this disclosure, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this disclosure.
[0060] In this application, unless otherwise expressly specified and limited, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature is in indirect contact with the second feature through an intermediate medium. Furthermore, "above," "on top of," and "over" the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.
[0061] In this application, unless otherwise expressly specified and limited, the disclosed "range" is defined in the form of a lower limit and / or an upper limit. A given range is defined by selecting a lower limit and / or an upper limit, which defines the boundary of the particular range. Ranges defined in this way may include or exclude endpoints and can be combined arbitrarily; that is, any lower limit can be combined with any upper limit to form an unspecified range, and any lower limit can be combined with other lower limits to form an unspecified range. Similarly, any upper limit can be combined with any other upper limit to form an unspecified range. Furthermore, each individually disclosed point or single value can itself serve as a lower limit or upper limit, combined with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.
[0062] In this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.
[0063] In this application, unless otherwise expressly specified and limited, all implementation methods and optional implementation methods, or all technical features and optional technical features, can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of this application.
[0064] With the increasing depletion of fossil fuels, solar energy, as a clean and renewable new energy source, has received extensive attention for its development and utilization. Solar cells, which can directly convert solar energy into electric energy, have become a research hotspot in the new energy field.
[0065] With the continuous deepening of scientific research work, the conversion efficiency of crystalline silicon solar cells has achieved remarkable breakthroughs, and the highest efficiency of crystalline silicon solar cells has currently reached 27.81% (HIBC structure). At the same time, the structure of solar cells has also undergone multiple iterative evolutions from PERC (Passivated Emitter and Rear Contact) cells to HJT (Heterojunction), TOPCon (Tunnel Oxide Passivated Contact), BC (Back Contact) and hybrid BC cells.
[0066] The conversion efficiency of solar cells is mainly restricted by two major aspects: optical loss and electrical loss. For HTBC (Heterojunction Tunnel Oxide Back Contact) cells, in order to increase the number of effective photons entering the interior of the crystalline silicon substrate, no electrodes are arranged on the front side, and all front electrodes are transferred to the back side of the cell to eliminate the shading loss of the front electrodes; at the same time, an anti-reflection film is deposited on the front side of the cell to achieve optical gain. In addition, by designing a small-sized textured structure (such as a pyramid-shaped textured surface) on the front side of the cell, the surface reflectivity can be further reduced, and the light trapping path of light inside the crystalline silicon substrate can be increased, so as to improve the cell efficiency at the optical level.
[0067] However, although the small-sized textured structure is beneficial to optical gain, its surface dangling bond density increases, which significantly increases the difficulty of surface passivation, and further affects electrical performance parameters such as open-circuit voltage and fill factor. In the existing HTBC cell structure, the size of the front and back textured surfaces usually tends to be the same, or only the front textured surface is singly optimized while ignoring the passivation requirement of the back side, making it difficult to balance the front optical performance and the back passivation performance.
[0068] To this end, based on the HTBC cell structure, the present invention proposes a front and back differentiated textured surface design scheme, that is, a small-sized textured structure is adopted on the front side of the cell to optimize the optical performance, and a large-sized textured structure is adopted on the back side of the cell to improve the passivation effect. Through the differentiated configuration of the front and back textured surface sizes, the coordinated improvement of the optical performance and electrical performance of the cell is realized, thereby further improving the overall conversion efficiency of the HTBC cell.
[0069] Reference Figure 1 as shown, the present invention discloses a solar cell, comprising:
[0070] The substrate 10 includes a light-receiving surface S1 (i.e., the front side) and a back surface S2 (i.e., the back side) disposed opposite to each other. A first textured surface structure is formed on the light-receiving surface S1. The back surface S2 includes an alternately distributed first region S21 and a second region S22. A second textured surface structure is formed on the surface of the substrate 10 in the first region S21. The average bottom dimension of the second textured surface structure is greater than the average bottom dimension of the first textured surface structure.
[0071] The first passivation contact structure is provided at least in the first region S21 of the backlight surface S2 of the substrate 10;
[0072] The second passivated contact structure is disposed in the second region S22 of the backlight surface S2 of the substrate 10.
[0073] In this invention, the substrate 10 is a crystalline silicon substrate, which can be a monocrystalline silicon substrate or a polycrystalline silicon substrate. The substrate 10 can be N-type doped or P-type doped, and the thickness of the substrate 10 is 120μm-160μm. For example, the substrate 10 is an N-type polycrystalline silicon substrate with a resistivity of 0.3Ω·cm-7Ω·cm, preferably 0.5Ω·cm-3.5Ω·cm.
[0074] In this invention, the surface of the second region S22 of the backlight surface S2 of the substrate 10 is a polished surface, and the second textured surface structure of the first region S21 is a pyramid textured surface structure. The first textured surface structure of the light-receiving surface S1 of the substrate 10 is a pyramid textured surface structure. The average base size of the pyramid in the first textured surface structure is 0.5μm-3μm, for example, it can be 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, etc., or it can be any range of the above values. The average base size of the pyramid in the second textured surface structure is 2μm-6μm, for example, it can be 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 6μm, etc., or it can be any range of the above values.
[0075] In this invention, the average bottom dimensions of the second textured structure in the first region S21 of the backlight surface S2 and the average bottom dimensions of the first textured structure in the light-receiving surface S1 are respectively adjusted so that the specific surface area of the second textured structure in the first region S21 is greater than that of the first textured structure in the light-receiving surface S1. This results in a lower reflectivity for the light-receiving surface S1, reducing surface recombination and Auger recombination in that region, improving passivation, and reducing current loss. Preferably, the ratio of the specific surface area of the second textured structure in the first region S21 of the backlight surface S2 to the specific surface area of the first textured structure in the light-receiving surface S1 is (1.1-2):1, for example, it can be 1.1:1, 1.5:1, 1.7:1, 2:1, etc., or it can be any range of the above values.
[0076] Specific surface area refers to the ratio of the surface area of the textured surface to the surface area of the original flat surface (such as a polished surface). The textured surface process can increase the specific surface area of the substrate. Different types of textured surfaces have different specific surface areas. Taking a pyramid textured surface as an example, its specific surface area is related to parameters such as the pyramid's dimensions (width, height) and density, while the specific surface area of a polished surface is 1. The pyramid structure in this application can be a tetrahedron, approximately tetrahedron, pentahedron, or approximately pentahedron.
[0077] The specific surface area of the pile structure is controlled by the pile forming process parameters. In the pile forming process, the pile structure is affected by factors such as the mass fraction of the pile forming solution (i.e., the concentration of acid or alkali), the reaction temperature, and the reaction time. Higher mass fractions of the pile forming solution, higher reaction temperatures, and longer reaction times result in larger pile structure sizes and correspondingly larger specific surface areas. By controlling the alkaline pile forming process parameters, the size and density of each pile structure can be controlled, thereby controlling the specific surface area of the pile structure.
[0078] In practical processes, the specific surface area of a velvet surface can be indirectly measured using techniques such as optical measurement or scanning electron microscopy (SEM). For example, the specific surface area can be estimated by measuring the dimensions of the velvet surface (such as the height and base width of a pyramid). The specific measurement methods for specific surface area will not be elaborated here.
[0079] In this invention, the first passivation contact structure includes an intrinsic layer 21 and a first doped layer 22 stacked on the surface of the intrinsic layer 21. The second passivation contact structure includes a tunneling layer 31 and a second doped layer 32 stacked on the surface of the tunneling layer 31. The substrate 10 and the second doped layer 32 have the same doping type, while the first doped layer 22 has the opposite doping type to the substrate 10, thus the doping types of the first doped layer 22 and the second doped layer 32 are opposite. Exemplarily, the substrate 10 and the second doped layer 32 achieve N-type doping by introducing donor impurities such as group VA elements such as phosphorus (P), arsenic (As), or antimony (Sb) into the semiconductor material, and the first doped layer 22 achieves P-type doping by introducing acceptor impurities such as group IIIA elements such as boron (B), aluminum (Al), or gallium (Ga) into the semiconductor material. Exemplarily, N-type doping in this application is illustrated using phosphorus doping (P) as an example, and P-type doping is illustrated using boron (B) doping as an example.
[0080] In this invention, the intrinsic layer 21 is preferably an intrinsic amorphous silicon layer (ia-Si:H) with a thickness of 5nm-10nm, for example, 5nm, 7nm, 9nm, 10nm, or any range of the above values. This intrinsic layer 21 at least covers the surface of the first region S21, serving as a buffer layer between the substrate 10 and the microcrystalline silicon layer. Hydrogen atoms in the intrinsic amorphous silicon layer can effectively saturate the dangling bonds on the crystalline silicon substrate surface, achieving excellent chemical passivation. On the large-size textured structure of the first region S21 (average bottom dimension greater than 2μm and less than or equal to 6μm), the intrinsic amorphous silicon layer can achieve better conformal coverage and thickness uniformity, thereby ensuring consistent passivation effects.
[0081] In this invention, the first doped layer 22 is preferably a doped microcrystalline silicon layer (μc-Si:H(p)) with a thickness of 15nm-30nm, for example, it can be 15nm, 20nm, 25nm, 30nm, etc., or it can be any range of the above values. The doped microcrystalline silicon layer serves as the emitter layer and forms a pn junction with the substrate 10.
[0082] It is understood that in other embodiments of the present invention, the first passivation contact structure may also extend from the first region S21 and be disposed on the surface of the second passivation contact structure in the second region S22.
[0083] In this invention, the thickness of the tunneling layer 31 is 0.5 nm to 2 nm, for example, it can be 0.5 nm, 1 nm, 1.5 nm, 2 nm, etc., or it can be any range of the above values. The tunneling layer 31 is selected from one or more materials selected from silicon oxide, aluminum oxide, titanium oxide, niobium oxide, boron oxide, gallium oxide, tin oxide, hafnium oxide, tantalum oxide, silicon nitride, silicon oxynitride, silicon carbide, lithium fluoride, magnesium fluoride, amorphous silicon, microcrystalline silicon, and nanocrystalline silicon. Preferably, the tunneling layer 31 is a silicon oxide layer.
[0084] In this invention, the doping concentration of the second doped layer 32 is 10. 20 atom / cm 3 -6×10 20 atom / cm 3 For example, it could be 10 20 atom / cm 3 2×10 20 atom / cm 3 3×10 20 atom / cm 3 5×10 20 atom / cm 3 6×10 20 atom / cm 3The thickness of the second doped layer 32 is 100nm-250nm, for example, 100nm, 150nm, 200nm, 250nm, etc., or any of the above values. A thinner second doped layer 32 can reduce parasitic absorption, increase the short-circuit current density of the battery, and significantly improve battery efficiency and bifaciality without affecting the metallization contact performance.
[0085] In this invention, a dielectric layer 41 is provided on the light-receiving surface S1 of the substrate 10. The dielectric layer 41 may include a passivation layer and / or an antireflection layer, which is a stack formed of at least one or more of the following: aluminum oxide layer, silicon oxide layer, gallium oxide layer, silicon nitride layer, aluminum nitride layer, and silicon oxynitride layer. The passivation layer is preferably an aluminum oxide layer with a thickness of 2nm-10nm, for example, 2nm, 4nm, 8nm, 10nm, or any range thereof; the antireflection layer is preferably a silicon nitride / silicon oxynitride stack with a thickness of 50nm-100nm, for example, 50nm, 70nm, 90nm, 100nm, or any range thereof.
[0086] In this invention, a conductive layer 42 is provided on the backlight side S2 of the substrate 10 (see figure). Figure 3j (As shown). The conductive layer 42 includes a first conductive portion 421 and a second conductive portion 422 that are isolated from each other. The first conductive portion 421 is in contact with the first doped layer 22 in the first passivation contact structure, and the second conductive portion 422 is in contact with the second doped layer 32 in the second passivation contact structure.
[0087] The first electrode 61 is in electrical contact with the first conductive part 421, and the second electrode 62 is in electrical contact with the second conductive part 422.
[0088] In this invention, the reference Figure 1 As shown, the backlight surface S2 of the substrate 10 is recessed in the first region S21. In the step of texturing the backlight surface S2 in the first region S21, the second doped layer 32 and the tunneling layer 31 of the first region S21 need to be removed first, and part of the substrate 10 will be etched, so that the substrate 10 in the first region S21 is recessed.
[0089] In other embodiments of the present invention, the first region S21 and the second region S22 may also be arranged flush.
[0090] In the above technical solution, the light-receiving surface adopts a textured structure with a smaller size, which is beneficial to reducing the recombination loss of the light-receiving surface. The small-sized textured structure combined with the light-receiving surface dielectric layer (which functions for passivation and anti-reflection) can achieve excellent optical gain on the light-receiving surface — the small-sized pyramid textured surface can provide a more uniform optical interface, and in cooperation with the passivation and anti-reflection effect of the dielectric layer, it can effectively reduce the reflectivity of the light-receiving surface, increase the short-wavelength response, and thus improve the short-circuit current density of the cell.
[0091] The backlight surface adopts a textured structure with a size larger than that of the textured structure on the light-receiving surface, which has the following technical advantages.
[0092] First, the large-sized textured structure is beneficial to the uniform deposition of the intrinsic amorphous silicon layer, and can obtain an excellent chemical passivation effect. Since the intrinsic amorphous silicon layer needs to achieve conformal coverage on the surface of the substrate, the slope of the large-sized pyramid textured surface is relatively gentle, which is beneficial to the step coverage rate and thickness uniformity of the amorphous silicon thin film, thereby reducing the density of interface defect states and improving the passivation quality.
[0093] Second, the large-sized textured structure facilitates more uniform and continuous deposition of the conductive layer. The conformal deposition quality of the conductive layer on the textured surface directly affects its conductivity and light transmittance. The large-sized textured structure can reduce the thinning at the sharp peaks and pinhole defects of the conductive layer, making the film layer denser and more continuous.
[0094] Third, the uniform and continuous conductive layer facilitates the lateral transport of carriers, which can reduce the series resistance of the cell, thereby improving the fill factor.
[0095] Therefore, through the above design of the differentiated textured structures on the front and back sides, the short-circuit current (Isc), fill factor (pFF) and series resistance (Rs) of the cell are improved, and then the photoelectric conversion efficiency (EFF%) is enhanced.
[0096] Reference Figure 2 as shown, the present invention further discloses a preparation method of a solar cell, which specifically includes the following steps:
[0097] S1: Provide a substrate, the substrate has a light-receiving surface and a backlight surface disposed opposite to each other, and the backlight surface includes a first region and a second region distributed alternately.
[0098] S2: Prepare a second passivation contact structure on the light-receiving surface and the backlight surface, and form a first mask layer. The second passivation contact structure includes a second doped layer.
[0099] S3: Remove the first mask layer in the first region of the backlight surface.
[0100] S4: Perform a first texturing process on the substrate, remove the second passivation contact structure in the first region of the backlight surface, and form an initial textured structure on the surface of the substrate in the first region.
[0101] S5: removing the first mask layer on the light-receiving surface.
[0102] S6: performing a second texturing process on the substrate, removing the second passivation contact structure on the light-receiving surface and forming a first textured structure on the substrate surface of the light-receiving surface, and simultaneously continuing to etch the initial textured structure on the substrate surface of the first region to form a second textured structure, wherein the average bottom dimension of the second textured structure is larger than the average bottom dimension of the first textured structure.
[0103] S7: preparing a first passivation contact structure in the first region of the backlight surface. The first passivation contact structure comprises a first doped layer, and the doping type of the first doped layer is opposite to that of the second doped layer.
[0104] In the present invention, through the strategy of double-sided coating combined with stepwise texturing, the first mask layer is used as a mask to realize independent regulation of the textured structures on the front and back sides of the same substrate. The first texturing: the exposed substrate surface on the backlight surface is used to form a large textured structure, and other regions are protected by the first mask layer from being corroded by the alkaline solution; the second texturing: after removing the first mask layer on the light-receiving surface, a small textured structure is formed on the light-receiving surface, and at the same time, the textured structure on the exposed substrate surface of the backlight surface continues to grow to the target size; the double-sided protection / deprotection steps required by two independent texturing processes are avoided, the process flow is simplified, and the manufacturing cost is reduced.
[0105] The following is combined with Figures 3a-3k and Figure 1 to describe in detail the preparation method of the solar cell of the present invention, so as to facilitate the understanding of the technical solution of the present invention.
[0106] referring Figure 3a as shown, a substrate 10 is provided.
[0107] In the present invention, the substrate 10 includes a light-receiving surface S1 (i.e., the front side) and a backlight surface S2 (i.e., the back side) disposed opposite to each other, and the backlight surface S2 includes a first region S21 and a second region S22 which are alternately and adjacently distributed; that is, one second region S22 is disposed between two adjacent first regions S21, and one first region S21 is disposed between two adjacent second regions S22; there is no interval between the first region S21 and the second region S22.
[0108] In the present invention, the substrate 10 is a crystalline silicon substrate, which may be a monocrystalline silicon substrate or a polycrystalline silicon substrate. The substrate 10 may be N-type doped or P-type doped, and the thickness of the substrate 10 is 120 μm-160 μm. Exemplarily, the substrate 10 is an N-type polycrystalline silicon substrate, with a resistivity of 0.3 Ω·cm-7 Ω·cm, preferably 0.5 Ω·cm-3.5 Ω·cm.
[0109] Exemplarily, the substrate 10 in the present invention is an N-type monocrystalline silicon substrate with a thickness of 120 μm to 160 μm. An alkali polishing process is adopted to remove the damage layer on the surface of the substrate 10, so as to obtain the substrate 10 with a flat surface. The alkali polishing process can remove microcracks and dislocation layers formed on the surface of the substrate 10 during wire cutting or diamond wire cutting, providing a clean and flat substrate surface for subsequent film coating.
[0110] Refe Figure 3b rring to the illustration, a tubular PECVD (Plasma Enhanced Chemical Vapor Deposition) process is adopted to sequentially deposit a tunneling layer 31, a second doped layer 32 and a first mask layer 33 on the light-receiving surface S1 and the backlight surface S2 of the substrate 10.
[0111] The thickness of the tunneling layer 31 is 0.5 nm to 2 nm. As an ultra-thin carrier selective tunneling layer, this ultra-thin tunneling layer 31 allows majority carriers to tunnel through and blocks minority carriers, which is one of the core structures for realizing passivated contact.
[0112] The thickness of the second doped layer 32 is 100 nm to 250 nm. The second doped layer 32 is preferably a phosphorus-doped polysilicon layer, with the doping concentration controlled at 10 20 -6×10 20 atom / cm 3 . The second doped layer 32 and the underlying tunneling layer 31 together form a second passivated contact structure, which provides excellent surface passivation and selective carrier collection.
[0113] The thickness of the first mask layer 33 is 50 nm to 100 nm. The first mask layer 33 is a phosphosilicate glass layer (PSG).
[0114] It should be noted that the purpose of depositing the above stacked structure on the light-receiving surface and the backlight surface at the same time is to use the first mask layer 33 as a protective layer in the subsequent step-by-step texturing process, so as to realize selective texturing and etching.
[0115] Refe Figure 3c rring to the illustration, a laser etching process is adopted to perform window opening on the first mask layer 33 in the first region S21 of the backlight surface S2 of the substrate 10, remove the first mask layer 33 in the first region S21, and form an interdigitated window opening region. The window opening region corresponds to the subsequent first doped layer (emitter region), and the non-window opening region corresponds to the second doped layer 32 (back surface field region).
[0116] Refe Figure 3d rring to the illustration, the substrate 10 after window opening is subjected to a first texturing treatment, so that the second doped layer 32 and the tunneling layer 31 in the window opening region (the first region S21) on the backlight surface are removed, and an initial textured structure is formed on the substrate surface in the window opening region of the backlight surface S2.
[0117] Specifically, the texturing conditions are: alkali concentration of 3vol%-10vol%, temperature of 65°C-80°C, additive concentration of 1vol%-5vol%, and texturing time of 300s-700s. Texturing additives usually contain organic corrosion inhibitors and surfactants, which are used to regulate the growth density and size distribution of pyramids.
[0118] In this step, in the window opening area of the backlight surface, since the first mask layer 33 has been removed, the exposed second doped layer 32 and the tunneling layer 31 are corroded and removed by the alkali solution, and then the alkali solution textures the exposed substrate surface to form the initial textured structure on the backlight surface (pyramids are initially formed). In the non-window opening area of the backlight surface, due to the presence of the first mask layer 33, the alkali solution cannot corrode the covered area.
[0119] Refe Figure 3e as shown, a single-sided HF pickling process is used to remove the first mask layer 33 on the light-receiving surface S1. The HF concentration is 15vol%-25vol%, and the cleaning time is 30s-60s.
[0120] In this step, only the first mask layer on the light-receiving surface is removed, while the first mask layer in the second region of the backlight surface remains. The HF pickling is highly selective to the first mask layer and will not cause significant corrosion to the second doped layer, the tunneling layer or the substrate.
[0121] Refe Figure 3f as shown, the pickled substrate 10 is subjected to a second texturing treatment to remove the second doped layer 32 and the tunneling layer 31 on the light-receiving surface S1 and form a first textured structure on the surface of the substrate 10 on the light-receiving surface S1, and at the same time, continue to etch the initial textured structure on the substrate surface of the first region S21 of the backlight surface S2 to form a second textured structure.
[0122] Specifically, the texturing conditions are: alkali concentration of 1.5vol%-5vol%, temperature of 65°C-80°C, additive concentration of 1vol%-5vol%, and texturing time of 300s-700s.
[0123] In this step, since the first mask layer on the light-receiving surface has been removed, the exposed second doped layer and the tunneling layer are etched away by the alkaline solution, and then the alkaline solution directly acts on the surface of the light-receiving surface substrate to form a first textured structure thereon. The average value of the base size of the pyramids in the first textured structure of the light-receiving surface S1 is mainly distributed in the range of 0.5μm to 3μm. The small-size textured surface is beneficial to reduce the reflectivity, and achieves good optical gain in combination with the anti-reflection effect of the subsequent dielectric layer. The windowed region of the back surface S2 has formed an initial textured structure during the first texturing process, and these initial textured structures further grow in the alkaline solution during the second texturing process to form a second textured structure. The average value of the base size of the pyramids in the second textured structure further increases to more than 2μm and less than or equal to 6μm. Since the non-windowed region of the back surface is still protected by the first mask layer and is not corroded by the alkaline solution, the second textured structure is only formed in the interdigitated windowed region.
[0124] It should be noted that the first mask layer 33 above the second doped layer 32 in the non-windowed region (the second region) of the back surface S2 plays a role of mask protection during both texturing processes. During the first texturing process, the first mask layer on the back surface prevents the non-windowed region from being corroded by the alkaline solution; during the second texturing process, the first mask layer on the back surface still maintains the protective effect in the low-concentration alkaline solution, while allowing the textured surface of the windowed region to continue growing.
[0125] After the texturing is completed, the remaining first mask layer 33 is removed. For example, HF is used to remove the remaining first mask layer 33 on the back surface S2.
[0126] As shown in Figure 3g , an AlO layer is first deposited by an atomic layer deposition (ALD) process X (aluminum oxide) layer, with a thickness of 2nm-10nm. Then, a PECVD process is used to sequentially deposit SiN on the AlO X layer X (silicon nitride) and SiN X O Y (silicon oxynitride) stacked anti-reflection film, with a total thickness of 50nm-100nm.
[0127] The AlO X layer has a high fixed negative charge density, which can provide excellent field effect passivation for the substrate surface, and at the same time, the chemical passivation effect can effectively reduce the interface defect state density.
[0128] The SiN X / SiN X O Y stacked film utilizes the refractive index gradient effect (from high-refractive-index SiN X to low-refractive-index SiN X O Y ), which can achieve low reflectivity in a wide spectral range and further improve the light absorption efficiency.
[0129] AlO X / SiN X / SiN X O Y The SiN in the stacked dielectric layer 41 X and SiN X O Y layers further contain a large amount of hydrogen, which can diffuse to the substrate surface during the subsequent heat treatment process, perform the function of hydrogen passivation, and further improve the surface passivation quality.
[0130] After the deposition of the dielectric layer 41 is completed, a single-side pickling process is adopted to remove the AlO that is deposited around and covers the backlight surface X / SiN X / SiN X O Y stacked dielectric layer 41, while retaining the tunnel layer and the second doped layer on the backlight surface.
[0131] It can be understood that although the above deposition of the dielectric layer 41 is mainly performed on the light-receiving surface, due to gas diffusion in the process chamber and the edge effect of the substrate, a wrap-around deposited layer will inevitably be generated on the backlight surface. This step selectively removes the back-side wrap-around deposited layer through single-side pickling, without damaging the underlying second doped layer and tunnel layer. Y 9>
[0132] As shown in ref Figure 3h , a PECVD process is adopted to sequentially deposit the intrinsic layer 21 and the first doped layer 22 on the backlight surface. The intrinsic layer 21 is preferably an intrinsic amorphous silicon layer, with a thickness of 5 nm to 10 nm. The intrinsic amorphous silicon layer covers the second doped layer 32 on the backlight surface and the laser window region (i.e., the substrate surface of the first region S21). Hydrogen atoms in the intrinsic amorphous silicon layer can effectively saturate dangling bonds on the substrate surface, achieving excellent chemical passivation. On the large-size textured structure of the backlight surface, the intrinsic amorphous silicon layer can obtain better conformal coverage and thickness uniformity, thereby ensuring the consistency of the passivation effect.
[0133] The first doped layer 22 is preferably a P-type doped microcrystalline silicon layer, with a thickness of 15 nm to 30 nm, deposited on the intrinsic layer 21. The P-type doped microcrystalline silicon layer serves as an emitter layer and forms a p-n junction with the n-type substrate. In the interdigitated back contact structure, the region covered by the P-type doped microcrystalline silicon layer corresponds to the p-type doped region (emitter region), and forms an interdigitated alternating arrangement with the subsequently exposed second doped layer (n-type doped region — back surface field region).
[0134] As shown in ref Figure 3i , a green laser etching process is adopted to remove part or all of the intrinsic layer 21 and the first doped layer 22 covered on the surface of the second doped layer 32, so that the second doped layer 32 is exposed.
[0135] In this step, it is necessary to precisely control the energy density and etching depth of the laser, so as to ensure complete removal of the IP layer (intrinsic amorphous silicon layer and P-type doped microcrystalline silicon layer) covering above the second doped layer 32, without damaging the surface and performance of the underlying second doped layer 32, and without damaging the P-type doped microcrystalline silicon layer in the adjacent region.
[0136] After the laser treatment is completed, single-sided acid washing is performed to remove the molten residue and damaged layer generated during the laser etching process, so as to restore the cleanliness of the exposed surface of the second doped layer 32.
[0137] Ref Figure 3j As shown, a physical vapor deposition (PVD) process is adopted to deposit the conductive layer 42 on the surfaces of the first doped layer 22 on the backlight side and the exposed second doped layer 32. The thickness of the conductive layer 42 is about 100 nm. The conductive layer 42 is preferably a TCO thin film. As the conductive layer, the TCO thin film collects carriers transported from the doped regions (the second doped layer and the first doped layer), and laterally transmits the carriers to the metal electrode. On the large-size textured structure on the backlight side, the TCO thin film can achieve more uniform and continuous deposition, reduce thinning and pinhole defects at sharp peaks, thereby improving the lateral transport capability of carriers and reducing the series resistance of the cell.
[0138] Ref Figure 3k As shown, the conductive layer 42 above the second doped layer 32 is partially etched by a screen printing etching paste method to form an isolation trench, so that the conductive layer 42 is divided into a first conductive portion 421 and a second conductive portion 422 that are arranged in isolation. The first conductive portion 421 is arranged in contact with the first doped layer 22, and the second conductive portion 422 is arranged in contact with the second doped layer 32; thereby preventing carriers of two different conductivity types from laterally recombining in the conductive layer to form a leakage channel. The width and depth of the isolation trench need to be precisely controlled, so as not to significantly increase the series resistance while ensuring the electrical isolation effect.
[0139] Ref Figure 1 As shown, a screen printing process is adopted to print the first electrode 61 and the second electrode 62 on the surface of the conductive layer 42. The electrode material is usually selected from silver paste or silver-aluminum paste, which forms a good ohmic contact with the conductive layer 42 after high-temperature sintering, and finally obtains the finished cell product.
[0140] The present invention further provides a photovoltaic module having the above solar cell, comprising: a plurality of the above solar cells connected in series to form a solar cell string; interconnectors electrically connected with the above solar cells to connect the above solar cells into the solar cell string; and an encapsulation layer covering the surfaces of the plurality of solar cells.
[0141] In some embodiments of this application, the interconnecting components can be solder ribbons, metal wires, conductive tapes, etc.; the encapsulation layer can include a backplate, encapsulating film, cover plate, etc., to improve the stability of the solar cell string. The cover plate is located on the front of the solar cell string, and the backplate is located on the back of the solar cell string, both serving a protective function; the adhesive film is the adhesive film between the solar cell string and the cover plate and backplate, serving a bonding and fixing function, and must be made of a transparent material.
[0142] In some examples, the encapsulating film can be an organic encapsulating film such as polyvinyl butyral (PVB) film, ethylene-vinyl acetate copolymer (EVA) film, polyvinyl octene elastomer (POE) film, or polyethylene terephthalate (PET) film. In some examples, the cover or backing plate can be a light-transmitting film layer such as a glass cover or a plastic cover.
[0143] Example 1:
[0144] This embodiment provides a method for preparing an HTBC battery, specifically including the following steps:
[0145] Step 1: Select an n-type crystalline silicon substrate with a thickness of 120μm, and use an alkaline polishing process to remove the damaged layer on the surface of the crystalline silicon substrate to obtain a smooth crystalline silicon substrate.
[0146] Step 2: Using a tubular PECVD process, a tunneling layer (SiO2, 1.2 nm thick), an n-poly layer (180 nm thick), and a PSG layer (80 nm thick) are sequentially deposited on the light-receiving and back-light-receiving surfaces of the crystalline silicon substrate. The doping concentration in the n-poly layer is controlled at 3 × 10⁻⁶. 20 atom / cm 3 .
[0147] Step 3: Using laser etching, windows are created on the PSG layer of the back surface of the crystalline silicon substrate to form interdigitated window regions. The windowed regions correspond to the subsequent p-type doped regions (emitter regions), and the unwindowed regions correspond to the n-type doped regions (back field regions).
[0148] Step 4: Perform the first texturing process on the windowed crystalline silicon substrate. The texturing conditions are: alkali concentration 10 vol%, temperature 80℃, additive concentration 2 vol%, texturing time 600 s.
[0149] Step 5: Remove the PSG layer on the light-receiving surface using single-sided HF acid washing (HF concentration 20 vol%) for 45 seconds. The PSG layer on the back side is retained and continues to serve as a mask to protect the n-poly layer in the back field region.
[0150] Step 6: Perform a second texturing process on the acid-washed crystalline silicon substrate. The texturing conditions are: alkali concentration 3 vol%, temperature 80℃, additive concentration 3 vol%, texturing time 500 s.
[0151] In this step, the alkaline solution texturizes the surface of the crystalline silicon substrate, forming a small textured surface on the light-receiving side. The average size of the pyramid base is approximately 1.5 μm. The textured surface morphology and size distribution are as follows: Figure 4 and Figure 5 As shown; the textured surface structure in the windowed area on the backlit side continues to grow, and the average size of the pyramid base eventually stabilizes at approximately 3 μm. The textured surface morphology and size distribution are shown in the figure. Figure 6 and Figure 7 As shown.
[0152] Step 7: First, deposit AlO using the ALD process. X A layer with a thickness of 5 nm was then deposited using PECVD technology to deposit SiN. X / SiN X O Y The antireflective coating is multilayered with a total thickness of 80nm.
[0153] Step 8: Use a single-sided pickling process to remove the plating.
[0154] Step 9: Using PECVD process, an intrinsic amorphous silicon layer (7nm thick) and a P-type microcrystalline silicon layer (20nm thick) are sequentially deposited on the backlight surface. The intrinsic amorphous silicon layer covers the n-poly layer and the laser windowing area (i.e. the textured substrate surface) of the backlight surface.
[0155] Step 10: Using green laser etching process, remove the intrinsic amorphous silicon layer and P-type microcrystalline silicon layer (IP layer) covering the surface of the n-poly layer to expose the n-poly layer. After laser treatment, acid washing is performed on one side to remove laser damage.
[0156] Step 11: Using physical vapor deposition, deposit a TCO film with a thickness of 100 nm on the surface of the P-type microcrystalline silicon layer on the back side and the exposed n-poly layer.
[0157] Step 12: Using the screen printing etching paste method, locally etch the TCO above the n-poly layer to form isolation trenches, thereby achieving electrical isolation between the n-type doped region and the p-type doped region.
[0158] Step 13: Using screen printing technology, the main grid and sub-grid electrodes are printed on the surface of the TCO thin film, and the finished HTBC battery is obtained after sintering.
[0159] Example 2:
[0160] The difference between this embodiment and Embodiment 1 lies in the different texturing conditions, as detailed below:
[0161] Steps 1-3: Same as in Example 1.
[0162] Step 4: The conditions for flocking are: alkali concentration 5 vol%, temperature 70℃, additive concentration 5 vol%, flocking time 400s.
[0163] Step 5: Same as Example 1.
[0164] Step 6: The conditions for flocking are: alkali concentration 3 vol%, temperature 70℃, additive concentration 5 vol%, flocking time 300s.
[0165] After the above two texturing processes, the light-receiving surface forms a small texturing surface with an average base size of about 1.0 μm, while the back-lit surface forms a large texturing surface with an average base size of about 2.5 μm.
[0166] Steps 7-13: Same as in Example 1.
[0167] Example 3:
[0168] The difference between this embodiment and Embodiment 1 lies in the different texturing conditions, as detailed below:
[0169] Steps 1-3: Same as in Example 1.
[0170] Step 4: The conditions for flocking are: alkali concentration 10 vol%, temperature 80℃, additive concentration 5 vol%, flocking time 700s.
[0171] Step 5: Same as Example 1.
[0172] Step 6: The conditions for flocking are: alkali concentration 5 vol%, temperature 80℃, additive concentration 5 vol%, flocking time 700s.
[0173] After the above two texturing processes, the light-receiving surface forms a small texturing surface with an average base size of about 2.0 μm, while the back-lit surface forms a large texturing surface with an average base size of about 3.5 μm.
[0174] Steps 7-13 are the same as in Example 1.
[0175] Comparative Example 1:
[0176] This comparative example uses a conventional HTBC battery fabrication method, with consistent texturing on both the front and back sides, and does not employ a differentiated texturing process for the front and back sides. The specific differences are:
[0177] Steps 1 to 3: Same as in Example 1.
[0178] Step 4: A one-step flocking process is employed, with the following flocking conditions: alkali concentration 5 vol%, temperature 75℃, additive concentration 3 vol%, flocking time 500 s. A consistent flocked structure is simultaneously formed on both the front and back sides, with an average pyramid base size of approximately 1.6 μm. The flock morphology and size distribution are as follows: Figure 8 and Figure 9 As shown (the front and back velvet surfaces have the same structure).
[0179] Step 5 and subsequent steps are the same as in Example 1.
[0180] The batteries obtained in Examples 1-3 and Comparative Example 1 were subjected to performance tests under the same conditions. Specific performance comparisons are shown in Table 1.
[0181] Table 1: Performance Test Results Statistics for Different Examples
[0182]
[0183] As shown in Table 1, in terms of optical performance, the short-circuit current density Jsc of Examples 1-3 reaches 42.85 mA / mm². 2 -42.87 mA / mm 2 Compared to Comparative Example 1 (42.80 mA / mm) 2 Increased by approximately 0.1 mA / mm 2 This indicates that the small textured surface on the light-receiving side, combined with the anti-reflection effect of the dielectric layer, effectively enhances light absorption. In terms of electrical performance, the series resistance Rs of Examples 1-3 is as low as 0.27 mΩ-0.33 mΩ, and the fill factor FF is as high as 86.45%-86.58%, both significantly better than Comparative Example 1 (Rs=0.35 mΩ, FF=86.41%). The large textured surface on the backlight side is beneficial for uniform TCO film coverage and lateral carrier transport. Regarding passivation, after adjusting the textured surface size, the open-circuit voltage Voc of Examples 1-3 (744.6 mV-744.8 mV) is basically the same as that of Comparative Example 1 (744.5 mV), indicating that the large textured surface on the backlight side does not negatively affect the passivation effect, achieving synergistic optimization of optical and electrical performance. In terms of overall efficiency, the photoelectric conversion efficiency of Examples 1-3 reached 27.56%-27.64%, which is significantly better than the 27.53% of Comparative Example 1, indicating that the differentiated front and back textured surface design of the present invention can effectively improve the overall performance of HTBC batteries.
[0184] Compared with existing technologies, the solar cell and its fabrication method, as well as the photovoltaic module of the present invention, feature a small-sized textured structure on the light-receiving surface combined with a dielectric layer on the light-receiving surface, thereby enhancing the optical performance of the light-receiving surface. The large-sized textured structure on the back surface facilitates the uniform deposition of the first passivation contact structure, resulting in excellent chemical passivation. Through the differentiated design of the textured structure dimensions on the light-receiving and back surfaces, the short-circuit current and fill factor of the solar cell are improved, thereby enhancing the photoelectric conversion efficiency.
[0185] The solar cell and its preparation method, as well as the photovoltaic module of the present invention, feature a large-size textured back surface structure that facilitates more uniform and continuous deposition of the conductive layer, promotes lateral transport of charge carriers, reduces the series resistance Rs of the cell, and improves the photoelectric conversion efficiency of the cell.
[0186] It will be apparent to those skilled in the art that this disclosure is not limited to the details of the exemplary embodiments described above, and that this disclosure can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of this disclosure is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within this disclosure. No reference numerals in the claims should be construed as limiting the scope of the claims.
[0187] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A solar cell, characterized in that, include: The substrate has a light-receiving surface and a backlighting surface disposed opposite to each other. A first velvet structure is formed on the light-receiving surface, and the backlighting surface includes an alternately distributed first region and a second region. A second velvet structure is formed on the first region, and the average bottom size of the second velvet structure is greater than the average bottom size of the first velvet structure. A first passivation contact structure is provided at least in a first region of the backlight surface, and the first passivation contact structure includes a first doped layer; A second passivation contact structure is disposed in a second region of the backlight surface. The second passivation contact structure includes a second doped layer, the doping type of which is opposite to that of the first doped layer.
2. The solar cell according to claim 1, characterized in that, The specific surface area of the second textured structure on the backlit surface is greater than the specific surface area of the first textured structure on the light-receiving surface.
3. The solar cell according to claim 2, characterized in that, The ratio of the specific surface area of the second textured structure on the backlit side to the specific surface area of the first textured structure on the light-receiving side is (1.1-2):
1.
4. The solar cell according to claim 1, characterized in that, Both the first and second velvet structures are pyramid velvet structures. The average bottom size of the pyramid in the first velvet structure is 0.5μm-3μm, and the average bottom size of the pyramid in the second velvet structure is 2μm-6μm.
5. The solar cell according to claim 1, characterized in that, The first passivated contact structure further includes an intrinsic layer, and the first doped layer is stacked on the surface of the intrinsic layer; The second passivated contact structure further includes a tunneling layer, and the second doped layer is stacked on the surface of the tunneling layer.
6. The solar cell according to claim 1, characterized in that, Also includes: A dielectric layer is disposed on the light-receiving surface of the substrate; A conductive layer is disposed on one side of the backlight surface. The conductive layer includes a first conductive portion and a second conductive portion disposed separately. The first conductive portion is in contact with the first doped layer, and the second conductive portion is in contact with the second doped layer. The first electrode is in contact with the first conductive part; The second electrode is in contact with the second conductive part.
7. A method for preparing a solar cell, characterized in that, include: A substrate is provided, the substrate having a light-receiving surface and a backlighting surface disposed opposite to each other, the backlighting surface comprising an alternately distributed first region and a second region; A second passivated contact structure is prepared on the light-receiving surface and the backlight surface, and a first mask layer is formed thereon. The second passivated contact structure includes a second doped layer. Remove the first mask layer from the first region of the backlight surface; The substrate is subjected to a first texturing process to remove the second passivation contact structure in the first region of the backlight surface and form an initial texturing structure on the substrate surface in the first region. Remove the first mask layer from the light-receiving surface; A second texturing process is performed on the substrate to remove the second passivation contact structure of the light-receiving surface and form a first texturing structure on the substrate surface of the light-receiving surface. At the same time, the initial texturing structure on the substrate surface of the first region is etched to form a second texturing structure. The average bottom size of the second texturing structure is greater than the average bottom size of the first texturing structure. A first passivated contact structure is prepared in a first region of the backlight surface. The first passivated contact structure includes a first doped layer, the doping type of which is opposite to that of the second doped layer.
8. The method for preparing a solar cell according to claim 7, characterized in that, The first mask layer of the first region of the backlight surface is removed using a laser process; and / or, The first mask layer of the light-receiving surface is removed by acid etching.
9. The method for preparing a solar cell according to claim 7, characterized in that, In the first texturing process, the texturing solution is a mixed solution containing an alkaline solution and texturing additives, the texturing temperature is 65℃-80℃, and the texturing time is 300s-700s.
10. The method for preparing a solar cell according to claim 9, characterized in that, The alkaline solution includes KOH solution or NaOH solution with a concentration of 3 vol%-10 vol%; and / or, The concentration of the fabrication additive is 1 vol%-5 vol.
11. The method for preparing a solar cell according to claim 7, characterized in that, In the second texturing process, the texturing solution is a mixed solution containing an alkaline solution and texturing additives, the texturing temperature is 65℃-80℃, and the texturing time is 300s-700s.
12. The method for preparing a solar cell according to claim 11, characterized in that, The alkaline solution includes KOH solution or NaOH solution with a concentration of 1.5 vol%-5 vol%; and / or, The concentration of the fabrication additive is 1 vol%-5 vol.
13. The method for preparing a solar cell according to claim 7, characterized in that, A first passivated contact structure is fabricated in a first region of the backlight surface, including: A first passivation contact structure is formed on one side of the backlight surface, the first passivation contact structure covering the substrate surface of the first region and the surface of the second passivation contact structure covering the second region; A laser process is used to remove part or all of the first passivated contact structure in the second region, exposing the second passivated contact structure.
14. The method for preparing a solar cell according to claim 13, characterized in that, Following the laser process, the method further includes a wet treatment step on the exposed surface of the second passivated contact structure: The exposed surface of the second passivated contact structure is cleaned with an acidic solution to remove the heat-affected zone and / or molten residue generated by the laser process.
15. The method for preparing a solar cell according to claim 7, characterized in that, Also includes: A dielectric layer is prepared on the light-receiving surface; A conductive layer is formed on one side of the backlight surface and etched to form a first conductive portion that contacts the first doped layer and a second conductive portion that contacts the second doped layer; A first electrode is prepared that contacts the first conductive part, and a second electrode is prepared that contacts the second conductive part.