A BIPV Color High-Efficiency CdTe Photovoltaic Module and Its Preparation Method
By constructing a synergistic structure of a spectrally selective color filter composite layer, a gradient refractive index anti-reflection and light-harvesting coupling layer, and a high-efficiency CdTe thin-film battery cell, the contradiction between aesthetics and power generation performance of BIPV modules is resolved, realizing a high-efficiency and stable color photovoltaic module that meets the dual requirements of architectural aesthetics and power generation performance.
Patent Information
- Application Number
- CN202611424778.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing BIPV modules struggle to balance architectural aesthetics and power generation performance. Colored modules suffer from high photon loss, low efficiency, insufficient optical path optimization, and poor performance stability, failing to meet the demands for high efficiency, light transmission, and customized colors.
By employing a layered structure of a spectrally selective color filter composite layer, a gradient refractive index antireflection and light-harvesting coupling layer, and a high-efficiency CdTe thin-film battery cell, combined with photonic crystal structures and gallium-doped zinc oxide transparent conductive films, synergistic optimization of spectral management and light harvesting is achieved.
It achieves a wide range of visible light transmittance adjustment from 30% to 60%, multiple color options, stable photoelectric conversion efficiency of ≥15.2%, color retention rate of ≥95% after aging, and efficiency decay of ≤3.5%, meeting the long-term service life requirements of building materials.
Smart Images

Figure CN123124456A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of building-integrated photovoltaics (BIPV) technology, and in particular to a color high-efficiency CdTe photovoltaic module based on spectrally selective transmission and microstructure coupling, and its preparation method. Background Technology
[0002] With the rapid development of the green building industry, building-integrated photovoltaics (BIPV) has become a core technology for combining building energy conservation and power generation. CdTe thin-film solar cells, due to their advantages such as good low-light response, low temperature coefficient, low energy consumption in fabrication, and no risk of microcracks, have significant application potential in the BIPV field. However, existing BIPV modules still face the core dilemma of balancing architectural aesthetics and power generation performance, and related technologies have obvious limitations, specifically: 1. The quantitative contradiction between aesthetics and function: In pursuit of high efficiency, traditional CdTe photovoltaic modules are all dark black with visible light transmittance ≤10%, which cannot meet the aesthetic requirements of modern buildings for transmittance of more than 30% and customized color schemes; while existing colored BIPV modules use colored glaze screen printing or colored film composite technology to achieve color and light transmission, resulting in photon loss of ≥40% in the sensitive wavelength band of 500-800nm CdTe cells, and photoelectric conversion efficiency is generally ≤10%, with mass production efficiency even as low as 6-8%.
[0003] 2. Lack of spectral management capability: Existing colored photovoltaic modules do not perform precise management of the solar spectrum by wavelength. Traditional color layers non-selectively absorb light across the entire spectrum, which not only causes effective photon loss but also leads to a temperature rise of ≥8℃ in the module due to photon thermalization, further reducing efficiency by ≥5%. Moreover, without a targeted spectral reflection / scattering structure, the light energy utilization rate is only about 45%.
[0004] 3. Insufficient optical path optimization design: Traditional BIPV modules mostly use single-layer / multi-layer dielectric antireflective films, which can only achieve a reflectivity of ≤5% under vertical incident light. Under wide-angle incident light of 0-60°, the reflectivity increases sharply to 15-20%, which cannot adapt to the multi-angle and non-direct lighting conditions of building facades; and there is no dedicated light-capturing structure, so the power generation gain is ≤5% under weak light, making it difficult to improve the actual power generation revenue.
[0005] 4. Poor performance stability: The color structure of existing colored BIPV modules is prone to photolysis and migration. After 1000h of UV aging, the color difference ΔE is ≥5.0 and the color retention rate is ≤70%. Moreover, the efficiency decreases by ≥10% after damp heat aging (85℃ / 85%RH, 1000h), which cannot meet the 25-year service life requirement of building materials.
[0006] Current mainstream technologies focus only on improving transparency through antireflective layers, without achieving color customization. Some technologies employ through-body coloring with metal oxide doping during the melting stage, but this still doesn't solve the problem of spectral loss. The market lacks a systematic technical solution that can simultaneously achieve high efficiency (≥15%), high transmittance (30%-60%), color customization, and high stability. There is an urgent need to develop entirely new BIPV module structures and fabrication processes. Summary of the Invention
[0007] The purpose of this invention is to provide a BIPV color high-efficiency CdTe photovoltaic module and its preparation method, so as to solve the problems existing in the prior art.
[0008] To achieve the above objectives, the present invention provides a BIPV color high-efficiency CdTe photovoltaic module, comprising an outer protective glass, a spectrally selective color filter composite layer, a gradient refractive index antireflection and light-harvesting coupling layer, a high-efficiency CdTe thin-film battery cell, and an inner encapsulation glass, all stacked together; the spectrally selective color filter composite layer comprises a matrix layer and a photonic crystal structure layer; the high-efficiency CdTe thin-film battery cell comprises a front electrode, a window layer, an absorption layer, a back contact layer, and a back electrode, stacked sequentially.
[0009] Preferably, the matrix layer is an optical-grade polymer matrix with inorganic-organic hybrid nanochromophores dispersed inside; the photonic crystal structure layer is a periodic anatase titanium dioxide nanopillar array.
[0010] Preferably, the gradient refractive index antireflection and light-trapping coupling layer is a nanoporous film with a continuously varying refractive index along the thickness direction; the nanopores of the nanoporous film can produce a diffuse scattering effect on incident light.
[0011] Preferably, the front electrode is a gallium-doped zinc oxide transparent conductive film; the window layer is a cadmium sulfide layer; the absorption layer is a magnesium-doped cadmium telluride layer; and the back contact layer is a zinc telluride:copper / molybdenum oxide composite structure.
[0012] Preferably, the inorganic-organic hybrid nanochromophore comprises mesoporous silica nanoparticles and organic dye molecules anchored to the mesoporous silica nanoparticles via covalent bonds.
[0013] Preferably, the periodic nanopillar array is made of anatase titanium dioxide or silicon nitride.
[0014] Preferably, an interlayer film is provided between the outer protective glass and the inner encapsulation glass.
[0015] Preferably, the outer protective glass is ultra-clear float glass.
[0016] This invention also provides a method for preparing a BIPV color high-efficiency CdTe photovoltaic module, comprising the following steps: Fabrication of photonic crystal templates: Photonic crystal templates are fabricated on the outer protective glass using nanoimprint technology; Preparation of a spectrally selective color filter composite layer: A polymer precursor solution containing inorganic-organic hybrid nanochromophores is applied to the photonic crystal template, and after curing, a spectrally selective color filter composite layer is formed. Preparation of gradient refractive index antireflection and light-trapping coupling layer: A silica precursor film is deposited on the spectrally selective color filter composite layer, and after etching, a nanoporous silica layer is formed, namely the gradient refractive index antireflection and light-trapping coupling layer. Fabrication of high-efficiency CdTe thin-film battery cells: a front electrode, a window layer, a magnesium-doped cadmium telluride absorption layer, a back contact layer, and a back electrode are sequentially fabricated on the gradient refractive index antireflection and light-harvesting coupling layer, and the magnesium-doped cadmium telluride absorption layer is subjected to activation annealing treatment. Encapsulation: The outer protective glass and the inner encapsulation glass are laminated and encapsulated using an intermediate film.
[0017] Preferably, the magnesium doping concentration in the magnesium-doped cadmium telluride absorber layer is from 0.6 at% to 1.0 at%.
[0018] Compared with the prior art, the present invention has the following advantages and technical effects: The present invention provides a color-coated high-efficiency CdTe photovoltaic module and its fabrication method. By constructing a synergistic optical-electrical structure of "spectrally selective color filter composite layer - gradient refractive index anti-reflection and light-harvesting coupling layer - high-efficiency CdTe thin-film battery unit", it effectively solves the core contradiction between architectural aesthetics and power generation performance in existing BIPV modules. The module of the present invention can achieve a wide range of visible light transmittance adjustment of 30%-60%, and can be customized with multiple color systems such as red, blue, gray, and green. The average photoelectric conversion efficiency in mass production is stable at ≥15.2%, and the laboratory efficiency reaches 17.6%. After 2000h of ultraviolet aging and 1000h of damp heat aging, the color retention rate is ≥95%, and the efficiency decay is ≤3.5%, which is superior to traditional color BIPV modules. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention.
[0020] Figure 1 This is a schematic diagram of the cross-sectional structure of the BIPV color high-efficiency CdTe photovoltaic module of the present invention.
[0021] In the figure: 1. Outer protective glass; 2. Spectral selective color filter composite layer; 21. Matrix layer; 22. Photonic crystal structure layer; 3. Gradient refractive index antireflection and light-trapping coupling layer; 4. High-efficiency CdTe thin-film battery cell; 41. Front electrode; 42. Window layer; 43. Absorption layer; 44. Back contact layer; 45. Back electrode; 5. Intermediate film; 6. Inner encapsulation glass. Detailed Implementation
[0022] It should be noted that, unless otherwise specified, the embodiments and features described in this invention can be combined with each other. The described embodiments are merely some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art without inventive effort are within the scope of protection of this invention. The invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0023] like Figure 1 As shown, the present invention provides a BIPV color high-efficiency CdTe photovoltaic module, comprising an outer protective glass 1, a spectrally selective color filter composite layer 2, a gradient refractive index antireflection and light-harvesting coupling layer 3, a high-efficiency CdTe thin-film battery cell 4, and an inner encapsulation glass 6 stacked together; the spectrally selective color filter composite layer 2 includes a matrix layer 21 and a photonic crystal structure layer 22; the high-efficiency CdTe thin-film battery cell 4 includes a front electrode 41, a window layer 42, an absorption layer 43, a back contact layer 44, and a back electrode 45 stacked sequentially.
[0024] By stacking an outer protective glass 1, a spectrally selective color filter composite layer 2, a gradient refractive index antireflection and light-trapping coupling layer 3, a high-efficiency CdTe thin-film battery unit 4, and an inner encapsulation glass 6, a synergistic optical-electrical structure of "spectrally selective color filter composite layer - gradient refractive index antireflection and light-trapping coupling layer - high-efficiency CdTe thin-film battery unit" can be constructed. This effectively solves the core contradiction between architectural aesthetics and power generation performance of existing BIPV modules, achieving 30%-60% transmittance adjustment and multi-color customization, while ensuring high photoelectric conversion efficiency of the module.
[0025] Further optimization of the scheme: the matrix layer 21 is an optical-grade polymer matrix with inorganic-organic hybrid nanochromophores dispersed inside; the photonic crystal structure layer 22 is a periodic anatase titanium dioxide nanopillar array. The photonic crystal structure layer 22 has a reflection / scattering effect on the non-sensitive wavelength light of the high-efficiency CdTe thin film battery unit 4, and a transmission effect on the sensitive wavelength light.
[0026] Architectural-grade color customization is achieved through the dispersed inorganic-organic hybrid nanochromophores within the matrix layer 21. Combined with the periodic anatase titanium dioxide nanopillar array in the photonic crystal structure layer 22, precise band-specific management of the solar spectrum is achieved, resulting in high light reflection / scattering efficiency in insensitive bands and high light transmission efficiency in sensitive bands. This significantly reduces photon thermal loss, fundamentally ensuring the photon utilization efficiency of the battery. Furthermore, the periodic anatase titanium dioxide nanopillar array can act as a buffer layer, improving the band alignment at the CdTe interface of the nanopillars and more effectively reducing interfacial recombination.
[0027] Further optimization of the scheme: the gradient refractive index antireflection and light-trapping coupling layer 3 is a nanoporous film with a continuously varying refractive index along the thickness direction; the nanopores of the nanoporous film can produce a diffuse scattering effect on incident light.
[0028] By using a gradient refractive index antireflection and a continuously varying refractive index design for the light-trapping coupling layer 3, high antireflection efficiency can be achieved over an ultra-wide wavelength and wide angle, solving the problem of poor angle adaptability of traditional antireflection films. The diffuse scattering effect of its nanoporous structure significantly increases the effective optical path of light within the absorption layer, resulting in significant power generation gain under weak light conditions, perfectly adapting to the complex lighting environment of BIPV.
[0029] Further optimization of the scheme: the gradient refractive index antireflection and light-harvesting coupling layer 3 is a nanoporous SiO2 thin film, which adopts an integrated design of "continuously gradient refractive index + nanoporous light harvesting" to solve the problems of poor wide-angle adaptability and low low light utilization efficiency of traditional antireflection films. By controlling the porosity (55% on the surface to 15% on the bottom) using a sol-gel method combined with a template agent, a linear and continuous gradient of the refractive index from 1.50 (matching glass) to 2.40 (matching CdTe battery front-end materials) was achieved (linearity R). 2 =0.992); According to ellipsometer testing, the average antireflection efficiency in the 400-1100nm solar spectrum band reaches 98.5%, and the reflectivity under wide incident light angles of 0-60° is ≤2.3%, which is far superior to the 60° incident reflectivity of traditional multilayer antireflection films (18%).
[0030] Its nanopores (8 nm in diameter, with a uniformity variation coefficient of 7%) produce a diffuse scattering effect on incident light. Optical path simulation tests show that this increases the effective optical path length within the CdTe absorption layer to 2.8 times the original optical path length; at 200 W / m 2 Under low light conditions, the module's power generation gain reaches 20%, and the actual power generation revenue is increased by more than 18% under complex lighting conditions on building facades.
[0031] Further optimization of the design: front electrode 41 is a gallium-doped zinc oxide transparent conductive film; window layer 42 is a cadmium sulfide layer; absorption layer 43 is a magnesium-doped cadmium telluride layer; back contact layer 44 is a zinc telluride:copper / molybdenum oxide composite structure.
[0032] The front electrode 41 uses a gallium-doped zinc oxide transparent conductive film, which has high transmittance and low sheet resistance in the 400-800nm wavelength range, superior to traditional ITO electrodes. The absorption layer 43 uses a magnesium-doped cadmium telluride layer, which can optimize the band gap width, passivate grain boundary defects, and promote grain growth, thus significantly improving carrier lifetime and battery efficiency. The back contact layer 44 uses a zinc telluride:copper / molybdenum oxide composite structure, which can achieve low contact resistance and improve the fill factor.
[0033] Further optimization of the design resulted in the front electrode 41 employing a gallium-doped zinc oxide (GZO) transparent conductive film with a thickness of 200 nm. Testing showed a transmittance of 92.5% in the 400-800 nm wavelength range, a sheet resistance of 12 Ω / □, and a carrier migration of 220 cm⁻¹. 2 / (V·s), which is superior to the transmittance (89%) and sheet resistance (18Ω / □) of traditional ITO electrodes.
[0034] Window layer 42 uses the CdS window layer.
[0035] The absorber layer 43 is a 0.8 at% Mg-doped CdTe layer with a thickness of 3.0-4.0 μm. After deposition using the CSS process, it was activated and annealed for 20 min at 390℃, a CdCl2 partial pressure of 8 Pa, and an O2 volume fraction of 2%. XRD analysis showed that the diffraction peak intensity of absorber layer 43 was 3500 a.u., and the grain size was 650 nm, representing a 117% improvement over the grain size of the pure CdTe absorber layer (300 nm). TRPL analysis showed a carrier lifetime of 220 ns and a defect density of 4.5 × 10⁻⁶. 10 cm -3 The carrier lifetime (80 ns) is increased by 175% compared to that of a pure CdTe absorber layer.
[0036] The back contact layer 44 adopts a ZnTe:Cu (3at%Cu, 80-150nm) / MoOx (32at%O, 20-50nm) composite structure.
[0037] The back electrode 45 is made of Ag metal.
[0038] Further optimization of the scheme involves inorganic-organic hybrid nanochromophores comprising mesoporous silica nanoparticles and organic dye molecules covalently anchored to the mesoporous silica nanoparticles.
[0039] The design of organic dye molecules being covalently anchored to mesoporous silica nanoparticles can give chromophores excellent color fastness. After long-term UV aging, the color difference is small and the color retention rate is high, which is far superior to traditional physically doped dyes and meets the requirements for long service life of building materials.
[0040] Further optimization of the scheme: the matrix layer 21 is made of fluorinated polyimide / modified acrylic resin optical grade polymer (transmittance ≥92%, glass transition temperature ≥200℃), with inorganic-organic hybrid nanochromophores uniformly dispersed inside; these chromophores are covalently anchored by organic dye molecules (azo / anthraquinone / phthalocyanine) to mesoporous SiO2 nanoparticles (pore size 10-20nm, specific surface area 350m²). 2 The dye loading is 6wt%; tested according to national standard GB / T1865-2009, the color fastness reaches level 7-8, and after aging under 340nm ultraviolet light for 2000h, the color difference ΔE=1.0, and the color retention rate is 96.5%, which is far better than the ΔE=5.8 and color retention rate of 68% of traditional physically doped dyes; by changing the type of dye, four mainstream architectural colors, namely red, blue, gray and green, can be achieved, with CIE color coordinates of: red (0.62,0.35), blue (0.15,0.08), gray (0.33,0.33), and green (0.25,0.60), respectively, and the color uniformity deviation is ≤2.5%.
[0041] Further optimization of the scheme involves using anatase titanium dioxide or silicon nitride as the material for the periodic nanopillar array.
[0042] By using periodic nanopillar arrays made of anatase titanium dioxide or silicon nitride, a photonic crystal structure with high reflection / scattering efficiency for light in the non-sensitive bands of CdTe cells and high transmission efficiency for light in the sensitive bands can be formed, thus achieving precise band-specific management of the solar spectrum.
[0043] Further optimization of the scheme resulted in a photonic crystal structure layer 22 consisting of a periodic anatase TiO2 nanopillar array (100 nm in diameter, 250 nm in height, and 250 nm in period), fabricated on the matrix layer near the battery side. Measurements using a UV-Vis-NIR spectrophotometer showed that this layer achieved a light reflection / scattering efficiency of 88% in the non-sensitive wavelength range (300-450 nm / 800-1100 nm) of the CdTe battery, and a transmission efficiency of 92% in the sensitive wavelength range (500-800 nm). Compared to traditional dyed layers, the photon thermal loss was reduced by 72% (65%) to only 18%, fundamentally ensuring the photon utilization efficiency of the battery.
[0044] To further optimize the design, an intermediate film 5 is provided between the outer protective glass 1 and the inner encapsulation glass 6.
[0045] By setting an intermediate film 5 between the outer protective glass 1 and the inner encapsulation glass 6, reliable encapsulation of the component can be achieved, with high interlayer peel strength, meeting the long-term reliability requirements of building BIPV components.
[0046] Further optimization of the design resulted in interlayer 5 being an SGP ionomer interlayer (0.76 mm thick). After lamination (140℃, 0.9 MPa, 25 min), the interlayer peel strength reached 85 N / cm, far exceeding the national standard requirement of 50 N / cm. The insulation resistance of the encapsulated module was ≥1×10⁻⁶. 12 Ω, impact resistance ≥3.0J, meeting the long-term reliability requirements of building BIPV components.
[0047] The design was further optimized, with the outer protective glass 1 being ultra-clear float glass.
[0048] The outer protective glass 1 is made of ultra-clear float glass, which has high transmission efficiency in the 400-1100nm solar spectrum band. After tempering, it has high impact resistance and bending strength, meeting the mechanical performance requirements of building curtain walls.
[0049] Further optimization of the scheme: the outer protective glass 1 is made of sodium-calcium ultra-white float glass with a thickness of 3.2-4.0mm and a transmission efficiency of ≥91% in the 400-1100nm solar spectrum band. After tempering, the impact strength is ≥2.5J and the bending strength is ≥90MPa, which meets the mechanical performance requirements of building curtain walls.
[0050] This invention also provides a method for fabricating a BIPV color high-efficiency CdTe photovoltaic module, comprising the following steps: Preparing a photonic crystal template: a photonic crystal template is prepared on an outer protective glass layer using nanoimprinting technology; Preparing a spectrally selective color filter composite layer 2: a polymer precursor solution containing inorganic-organic hybrid nanochromophores is applied to the photonic crystal template, and after curing, a spectrally selective color filter composite layer 2 is formed; Preparing a gradient refractive index antireflection and light-harvesting coupling layer 3: on the spectrally selective color filter composite layer 2... A silica precursor film is deposited on the substrate, and after etching, a nanoporous silica layer is formed, namely the gradient refractive index antireflection and light-trapping coupling layer 3. A high-efficiency CdTe thin-film battery cell 4 is prepared: a front electrode 41, a window layer 42, a magnesium-doped cadmium telluride absorption layer 43, a back contact layer 44, and a back electrode 45 are sequentially prepared on the gradient refractive index antireflection and light-trapping coupling layer 3, and the magnesium-doped cadmium telluride absorption layer 43 is activated and annealed. Encapsulation: the outer protective glass 1 and the inner encapsulation glass 6 are laminated and encapsulated through an intermediate film 5.
[0051] Using the above preparation method, BIPV color high-efficiency CdTe photovoltaic modules with spectrally selective transmission and microstructure coupling can be prepared. The layers work together to achieve a dual breakthrough in aesthetics and efficiency.
[0052] Further optimization of the scheme, the specific steps for preparing the photonic crystal template are as follows: After the outer protective glass 1 is subjected to gradient cleaning (acetone → anhydrous ethanol → deionized water and ultrasonication), a TiO2 nanopillar array template is prepared by nanoimprinting technology. The imprinting accuracy is ±4nm, the template surface roughness Ra=0.6nm, and the period deviation of the nanopillar array is ≤±2nm. The nanoimprinting temperature is usually 80-160℃, depending on the type of imprinting adhesive; the imprinting pressure is usually 10-50bar; the UV curing time / thermal curing time depends on the type of imprinting adhesive; the demolding method is hot demolding or cold demolding; the TiO2 deposition method is such as atomic layer deposition (ALD), magnetron sputtering, or sol-gel method; the TiO2 deposition temperature affects the crystallinity and phase purity. The photonic crystal structure layer 22 is a periodic anatase TiO2 nanopillar array (100 nm in diameter, 250 nm in height, and 250 nm in period), fabricated on the matrix layer 21 near the battery side. After gradient cleaning (acetone → anhydrous ethanol → deionized water, ultrasonication) of the outer protective glass 1, a TiO2 nanopillar array template was prepared using nanoimprinting technology, with an imprinting accuracy of ±4 nm, a template surface roughness (Ra) of 0.6 nm, and a nanopillar array period deviation ≤ ±2 nm. A fluorinated polyimide precursor solution containing 6 wt% inorganic-organic hybrid nanochromophores was spin-coated onto the template at 3500 r / min, pre-cured at 130 °C for 2.5 h, and then cured at 190 °C for 1.5 h; the resulting composite layer has a thickness of 50 μm and a thickness uniformity deviation of ±1.8%, forming a spectrally selective color filter composite layer.
[0053] Tested by a UV-Vis-NIR spectrophotometer: light reflection / scattering efficiency in the non-sensitive band (300-450nm / 800-1100nm) is 88%, and transmission efficiency in the sensitive band (500-800nm) is 92%, with photon thermal loss.
[0054] Further optimization of the scheme, the specific steps for preparing the spectrally selective color filter composite layer 2 are as follows: A fluorinated polyimide precursor solution containing 6wt% inorganic-organic hybrid nanochromophores is spin-coated onto a template at a speed of 3500 r / min, pre-cured at 130℃ for 2.5 h, and then cured at 190℃ for 1.5 h; the resulting composite layer has a thickness of 50 μm and a thickness uniformity deviation of ±1.8%. After testing, its transmission efficiency in the 500-800 nm wavelength band is 92%.
[0055] Further optimization of the scheme, the specific steps for preparing the gradient refractive index antireflection and light-trapping coupling layer 3 are as follows: A SiO2 precursor film is deposited on the filter layer using PECVD, combined with controllable etching using a polyethylene glycol template agent to prepare a nanoporous SiO2 layer. The CVD deposition rate is 0.8 nm / s, and the etching rate is 0.15 nm / s. The final layer thickness is 100 nm, and the linearity of the refractive index gradient R... 2=0.992, average antireflection efficiency of 98.5% in the 400-1100nm range.
[0056] By using a sol-gel method combined with a template agent to control the porosity (55% on the surface layer → 15% on the bottom layer), a linear and continuous gradient of the refractive index from 1.50 (matching glass) to 2.40 (matching CdTe battery front-end material) was achieved (linearity R² = 0.992). Ellipsometry tests showed that the average antireflection efficiency reached 98.5% in the 400-1100nm solar spectrum band, and the reflectivity under wide incident light angles of 0-60° was ≤2.3%, which is far superior to the 60° incident reflectivity of traditional multilayer antireflection films (18%).
[0057] Further optimization of the scheme, the specific steps for preparing the high-efficiency CdTe thin film battery unit 4 are as follows: sputtering a GZO layer on the substrate glass, and then sequentially depositing a 60-100nm CdS window layer and a 3.2-4.0μm 0.8at%Mg-doped CdTe absorber layer using the CSS process; The table below shows a comparison of the lattice constant, band gap width, carrier lifetime, and corresponding cell efficiency of the absorber layer under different Mg doping concentrations (e.g., 0.2at%, 0.4at%, 0.6at%, 0.8at%, 1.0at%). Lattice constant variation: As the Mg doping concentration increases, the lattice constant gradually decreases from 6.481 Å for pure CdTe to 6.422 Å for 1.0 at% doping. This is due to the Mg doping concentration. 2+ The ionic radius (0.72 Å) is smaller than that of Cd. 2+ The ionic radius is 0.97 Å, and Mg substitution for Cd leads to lattice shrinkage. At 0.8 at%, the lattice constant is 6.435 Å, indicating moderate lattice shrinkage, which improves lattice matching (reduces lattice mismatch with the CdS window layer) without introducing excessive lattice distortion.
[0058] Bandgap width variation: Mg doping gradually increases the CdTe bandgap from 1.50 eV (pure CdTe) to 1.63 eV (1.0 at%). At 0.8 at%, the bandgap is 1.60 eV, which is near the upper limit of the optimal bandgap window (1.5–1.65 eV) for CdTe solar cells. This is beneficial for maintaining a high open-circuit voltage without significantly sacrificing the short-circuit current density.
[0059] Carrier lifetime variation: Carrier lifetime initially increases and then decreases with increasing Mg doping concentration. It reaches a peak of 220 ns at 0.8 at%, a 175% improvement over pure CdTe (80 ns). This is due to appropriate Mg doping. 1. Passivation of grain boundary defects: Mg forms Mg-O bonds at grain boundaries, effectively reducing the density of non-radiative recombination centers (defect density is only 4.5 × 10⁻⁶). 10 cm -3 ); 2. Promotes grain growth: XRD shows that the crystal plane diffraction peak intensity reaches 3500 a.u. and the grain size is 650 nm, which is 117% higher than that of pure CdTe (300 nm), and reduces grain boundary recombination; 3. However, when the doping exceeds 0.8at% (e.g., 1.0at%), the excess Mg induces lattice mismatch stress and impurity phase precipitation, and the carrier lifetime actually drops back to 185ns.
[0060] Corresponding battery efficiency: Battery efficiency exhibits a parabolic trend of "first increasing and then decreasing" with Mg doping concentration. It reaches a peak of 18.2% at 0.8 at%, which is 34.8% higher than that of pure CdTe (13.5%).
[0061] The 1.60 eV bandgap is highly matched to the 500-800 nm CdTe sensitive band, with a photonic thermal loss of only 18% (compared to about 30% for conventional CdTe); the carrier lifetime of 220 ns is combined with a ZnTe:Cu / MoOx composite back contact layer of 0.25 Ω·cm. 2 Low contact resistance increases the fill factor to 79.5%; 200W / m 2 The module's power generation gain reaches 20% under low light conditions.
[0062] Considering four key indicators—lattice constant, band gap, carrier lifetime, and cell efficiency—a Mg doping concentration of 0.8 at% is the optimal choice for this invention. At this concentration: the lattice constant is moderate (6.435 Å), with minimal lattice mismatch with the CdS window layer; the band gap is 1.60 eV, within the optimal spectral absorption window. It has the longest carrier lifetime (220 ns) and the lowest defect density (4.5 × 10⁻⁶). 10 cm -3 The battery has the highest efficiency (18.2%), balancing open-circuit voltage and short-circuit current density.
[0063] If the doping concentration is below 0.8at%, the grain refinement and defect passivation effects are insufficient; if it is above 0.8at%, the band gap is too wide, resulting in long-wavelength photon loss, and lattice distortion and impurity phase precipitation reduce carrier lifetime, with overall performance inferior to 0.8at.
[0064] The effect of Mg doping on the long-term stability of the absorber layer exhibits a pattern of initial improvement followed by degradation. 0.8 at% is the optimal doping concentration, and its stability advantages are reflected in three aspects: Structural stability: maximized grain size (650 nm), reduced grain boundary density to 46% of pure CdTe, and reduced water and oxygen intrusion channels; Chemical stability: high bond energy of Mg-O bonds enhances the lattice's resistance to degradation, and the in-situ generated MgO passivation layer effectively inhibits oxidation and Cu diffusion; Optical stability: ultra-low defect density (4.5 × 10⁻⁶). 10 cm -3 It suppresses the formation of photo-induced metastable defects, with only 2.5% photo-induced decay after 2000 hours.
[0065] The 0.8 at% Mg doping concentration not only achieves the highest initial efficiency (18.2%), but also endows the absorber layer with optimal long-term stability, enabling the BIPV module of this invention to have a reliable foundation to meet the 25-year service life of building materials.
[0066] Subsequently, it was activated and annealed for 20 min in an atmosphere of 390℃, CdCl2 partial pressure 8 Pa, and O2 volume fraction 2%; according to PL testing, the defect density of the absorber layer was 4.5 × 10⁻⁶. 10 cm -3 Then, a ZnTe:Cu / MoOx composite back contact layer and an Ag electrode were prepared by magnetron sputtering.
[0067] Further optimization of the scheme, the specific encapsulation steps are as follows: the outer protective glass 1, the spectrally selective color filter composite layer 2, the gradient refractive index antireflection and light-trapping coupling layer 3, the high-efficiency CdTe thin film battery unit 4, and the inner encapsulation glass 6 are aligned and stacked, and placed in a laminator. The SGP interlayer film is used for lamination at 140℃ and 0.9MPa for 25 minutes. After cooling, edge processing and junction box installation are performed to obtain the finished component.
[0068] Further optimization of the scheme resulted in a magnesium doping concentration of 0.6 at% to 1.0 at% in the magnesium-doped cadmium telluride absorber layer 43.
[0069] By controlling the magnesium doping concentration in the magnesium-doped cadmium telluride absorber layer 43 between 0.6 at% and 1.0 at%, the lattice constant, band gap width, and carrier lifetime of the absorber layer can be optimized. 0.8 at% is the optimal doping concentration, resulting in the largest grain size, lowest defect density, longest carrier lifetime, and highest cell efficiency. If the doping concentration is below 0.6 at%, the grain refinement and defect passivation effects are insufficient; if it is above 1.0 at%, the excessively wide band gap leads to long-wavelength photon loss, and lattice distortion and impurity phase precipitation reduce carrier lifetime.
[0070] This invention provides a BIPV (Building Integrated Photovoltaic) color high-efficiency CdTe photovoltaic module and its fabrication method. From the spectral inlet filter composite layer and the interface light coupling anti-reflection trapping layer to the magnesium-doped CdTe absorption layer and composite back contact layer in the cell core, the entire chain is optimized, resulting in a long carrier lifetime and high fill factor for the CdTe cell. Simultaneously, the covalent bond anchoring design of inorganic-organic hybrid nanochromophores ensures high color retention after UV aging and low efficiency degradation after damp heat aging, meeting the 25-year service life requirement for building materials. This invention constructs a complete technical solution from nanochromophore materials, photonic crystal microstructures, gradient refractive index optical path design to high-efficiency CdTe cells and double-glass system encapsulation, providing a more effective approach for exploring high-end color BIPV modules.
[0071] Example 1: BIPVCdTe photovoltaic module with 40% red light transmittance Glass preparation: Sodium-calcium ultra-clear float glass was selected as the outer protective glass 1, with a thickness of 3.2mm and a transmission efficiency of 93% in the 400-1100nm solar spectrum band. After tempering, it has an impact strength of 3.0J and a bending strength of 110MPa, which meets the mechanical performance requirements of BIPV modules.
[0072] Preparation of red spectrally selective color filter composite layer 2: Inorganic-organic hybrid nano-chromophores were prepared using azo red dyes, with a chromophore loading of 6wt%; Photonic crystal structure layer 22 was constructed using titanium dioxide nanopillars with a diameter of 100nm, a height of 250nm, and a period of 250nm; The visible light transmittance of the component was tested to be 40%, with CIE chromaticity coordinates of (0.62, 0.35) and a color uniformity deviation of 2.2%.
[0073] Preparation of gradient refractive index antireflection and light-trapping coupling layer 3: The thickness of the nanoporous silica layer is 100 nm, the refractive index is 1.50→2.40, and the average antireflection efficiency is 98.5% from 400 to 1100 nm.
[0074] Fabrication of a high-efficiency CdTe thin-film battery cell 4: A gallium-doped zinc oxide front electrode 41 with a thickness of 200 nm was prepared by magnetron sputtering; a cadmium sulfide window layer 42 with a thickness of 80 nm was prepared by near-space sublimation; a 0.8 at% magnesium-doped cadmium telluride absorber layer 43 with a thickness of 3.5 μm was prepared by near-space sublimation; then, activation and annealing were carried out for 20 min at 390 °C, a CdCl2 partial pressure of 8 Pa, and an O2 volume fraction of 2%; a zinc telluride:copper / molybdenum oxide composite back contact layer 44 was prepared by magnetron sputtering. The specific preparation process was as follows: sputtering of a ZnTe:Cu buffer layer under an Ar atmosphere (target: ZnTe:Cu (Cu doping concentration 2-5 at%); working pressure: 0.5-1.0 Pa; power density: 2.5 W / cm³). 2(Film thickness: 100-200 nm); annealed at 200 °C for 30 minutes to promote Cu diffusion and ohmic contact formation. Then, MoO was sputtered in an Ar+O2 mixed gas atmosphere. x Hole transport layer (target: MoO3 ceramic target (purity 99.99%), working pressure: 0.5-2.0 Pa; substrate temperature: room temperature; film thickness: 10-50 nm), the zinc telluride: copper / molybdenum oxide composite back contact layer is now complete; silver back electrode is prepared by magnetron sputtering.
[0075] Double glass encapsulation: SGP interlayer film 5 is used, and it is laminated at 140℃ and 0.9MPa for 25 minutes.
[0076] Product performance: Module photoelectric conversion efficiency 16.8% (laboratory) / 15.5% (mass production); after 2000h of 340nm UV aging, color difference ΔE=0.9, color retention rate 97%; after 1000h of 85℃ / 85%RH damp heat aging, efficiency decay 3.0%.
[0077] Example 2: BIPVCdTe photovoltaic module with 50% blue light transmittance Preparation of blue spectrally selective color filter composite layer 2: Inorganic-organic hybrid nanochromophores were prepared using phthalocyanine blue dyes with a chromophore loading of 5wt%; Photonic crystal structure layer 22 uses silicon nitride nanopillars with a diameter of 90nm, a height of 220nm, and a period of 220nm; The visible light transmittance of the component is 50%, the CIE chromaticity coordinates are (0.15, 0.08), and the color uniformity deviation is 2.0%.
[0078] The remaining process parameters are the same as in Example 1.
[0079] Finished product performance: Module photoelectric conversion efficiency 17.6% (laboratory) / 15.8% (mass production); color difference ΔE=1.1 after 2000h UV aging, color retention rate 96%; efficiency decay of 3.2% after 1000h damp heat aging.
[0080] Example 3: BIPVCdTe photovoltaic module with 60% gray light transmittance Preparation of gray spectrally selective color filter composite layer 2: Inorganic-organic hybrid nanochromophores were prepared by using compound dyes, with a chromophore loading of 8wt%; Photonic crystal structure layer 22 is made of titanium dioxide nanopillars with a diameter of 120nm, a height of 300nm, and a period of 300nm; The visible light transmittance of the component is 60%, the CIE chromaticity coordinates are (0.33, 0.33), and the color uniformity deviation is 2.5%.
[0081] The remaining process parameters are the same as in Example 1.
[0082] Finished product performance: Module photoelectric conversion efficiency 16.2% (laboratory) / 15.2% (mass production); color difference ΔE=1.2 after 2000h UV aging, color retention rate 95%; efficiency decay of 3.5% after 1000h damp heat aging.
[0083] Comparative Example: Colored BIPVCdTe Components Prepared by Traditional Dyeing Method Blue coloring is achieved using a polyimide layer with traditionally physically doped anthraquinone dyes, with a light transmittance of 50%. No photonic crystal layer or gradient anti-reflection trapping layer is set. The CdTe cell has a pure CdTe absorption layer and a CuTe back contact. Test performance: the module photoelectric conversion efficiency is 9.8%; after 2000h of UV aging, the color difference ΔE=6.2, and the color retention rate is 65%; after 1000h of damp heat aging, the efficiency decreases by 12.5%.
[0084] Comparison of the embodiments and comparative examples: The photoelectric conversion efficiency of the component of the present invention is improved by more than 55%, the color retention rate is improved by more than 30%, and the efficiency decay is reduced by more than 74%, which fully verifies the advanced nature and superiority of the technical solution of the present invention.
[0085] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A BIPV color high-efficiency CdTe photovoltaic module, characterized in that, It includes an outer protective glass (1), a spectrally selective color filter composite layer (2), a gradient refractive index anti-reflection and light-harvesting coupling layer (3), a high-efficiency CdTe thin-film battery cell (4), and an inner encapsulation glass (6). The spectrally selective color filter composite layer (2) includes a matrix layer (21) and a photonic crystal structure layer (22). The high-efficiency CdTe thin-film battery cell (4) includes a front electrode (41), a window layer (42), an absorption layer (43), a back contact layer (44), and a back electrode (45) stacked in sequence.
2. The BIPV color high-efficiency CdTe photovoltaic module according to claim 1, characterized in that, The matrix layer (21) is an optical-grade polymer matrix with inorganic-organic hybrid nanochromophores dispersed inside; the photonic crystal structure layer (22) is a periodic anatase titanium dioxide nanopillar array.
3. The BIPV color high-efficiency CdTe photovoltaic module according to claim 1, characterized in that, The gradient refractive index anti-reflection and light-trapping coupling layer (3) is a nanoporous film with a continuously varying refractive index along the thickness direction; the nanopores of the nanoporous film can produce a diffuse scattering effect on incident light.
4. The BIPV color high-efficiency CdTe photovoltaic module according to claim 1, characterized in that, The front electrode (41) is a gallium-doped zinc oxide transparent conductive film; the window layer (42) is a cadmium sulfide layer; the absorption layer (43) is a magnesium-doped cadmium telluride layer; and the back contact layer (44) is a zinc telluride:copper / molybdenum oxide composite structure.
5. The BIPV color high-efficiency CdTe photovoltaic module according to claim 2, characterized in that, The inorganic-organic hybrid nanochromophores include mesoporous silica nanoparticles and organic dye molecules anchored to the mesoporous silica nanoparticles via covalent bonds.
6. The BIPV color high-efficiency CdTe photovoltaic module according to claim 2, characterized in that, The periodic nanopillar array is made of anatase titanium dioxide or silicon nitride.
7. The BIPV color high-efficiency CdTe photovoltaic module according to claim 1, characterized in that, An interlayer film (5) is provided between the outer protective glass (1) and the inner encapsulation glass (6).
8. The BIPV color high-efficiency CdTe photovoltaic module according to claim 1, characterized in that, The outer protective glass (1) is ultra-white float glass.
9. A method for preparing a BIPV color high-efficiency CdTe photovoltaic module, characterized in that, Includes the following steps: Preparation of photonic crystal templates: A photonic crystal template was prepared on the outer protective glass (1) using nanoimprint technology; Preparation of spectrally selective color filter composite layer (2): A polymer precursor solution containing inorganic-organic hybrid nanochromophores is applied to the photonic crystal template and cured to form a spectrally selective color filter composite layer (2). Fabrication of gradient refractive index antireflection and light-trapping coupling layer (3): A silica precursor film is deposited on the spectrally selective color filter composite layer (2), and after etching, a nanoporous silica layer is formed, namely the gradient refractive index anti-reflection and light-trapping coupling layer (3). Preparation of high-efficiency CdTe thin-film battery cells (4): A front electrode (41), a window layer (42), a magnesium-doped cadmium telluride absorption layer (43), a back contact layer (44), and a back electrode (45) are sequentially prepared on the gradient refractive index antireflection and light-trapping coupling layer (3), and the magnesium-doped cadmium telluride absorption layer (43) is subjected to activation annealing treatment. Packaging: The outer protective glass (1) and the inner encapsulation glass (6) are laminated and encapsulated through an intermediate film (5).
10. The method for preparing a BIPV color high-efficiency CdTe photovoltaic module according to claim 9, characterized in that, The magnesium doping concentration in the magnesium-doped cadmium telluride absorber layer (43) is 0.6 at% to 1.0 at%.