Photovoltaic modules, their manufacturing methods and manufacturing equipment

By setting an intermediate layer between the solder ribbon and the encapsulant film, and utilizing the chemical bonds and intermolecular forces of the active layer and the interface modification layer, the problem of insufficient adhesion of the encapsulant film in photovoltaic modules is solved, thereby improving the reliability and stability of the modules.

CN123124462APending Publication Date: 2026-11-17JINKO SOLAR CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611316684.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing photovoltaic modules, the interfacial adhesion between the encapsulant film and the cells and solder ribbons is insufficient in the low-temperature stringing process, leading to delamination after cooling and affecting the long-term reliability of the modules.

Method used

An intermediate layer is provided between the solder ribbon and the adhesive film. The intermediate layer includes an active layer and/or an interface modification layer. The surface energy of the active layer is greater than that of the adhesive film. It is bonded to the solder ribbon through chemical bonds and/or intermolecular forces to form a stable composite connection.

Benefits of technology

It significantly improves the wettability and physical adhesion between the adhesive film and the solder ribbon, prevents delamination, enhances the reliability and interface stability of the components, and avoids delamination caused by insufficient adhesion during cooling and delamination after high-temperature baking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124462A_ABST
    Figure CN123124462A_ABST
Patent Text Reader

Abstract

This application relates to the photovoltaic field, providing a photovoltaic module, its preparation method, and its preparation equipment. The photovoltaic module includes: a solar cell; a solder ribbon located on one side of the solar cell; an intermediate layer located on the side of the solder ribbon opposite to the solar cell; and an encapsulant film located on the side of the intermediate layer opposite to the solar cell. The intermediate layer includes an active layer and / or an interface modification layer. The surface energy of the active layer is greater than the surface energy of the encapsulant film. The interface modification layer is used to bond with the solder ribbon through chemical bonds and / or intermolecular forces. When the intermediate layer includes both an active layer and an interface modification layer, the active layer is located on the side of the interface modification layer opposite to the solar cell. The photovoltaic module provided by this application can at least improve the problems of low coating tensile strength and easy delamination of the coating after cooling of the cell string, leading to subsequent reliability failures, in existing photovoltaic modules.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the photovoltaic field, and in particular to a photovoltaic module, a method for preparing a photovoltaic module, and equipment for preparing a photovoltaic module. Background Technology

[0002] In existing low-temperature stringing processes, a film coating method is typically used instead of traditional welding to better secure the solder ribbons and cells during low-temperature lamination. However, the film is prone to wrinkling and delamination after cooling. Specifically, the interfacial adhesion between the film and the cells and solder ribbons is low. During the cooling process of the cell string, the thermal expansion and contraction stress of the film itself, combined with insufficient interfacial adhesion, leads to delamination or blistering between the film and the cells. Furthermore, this insufficient adhesion can cause the film to delaminate again during subsequent module lamination and high-temperature baking, severely impacting the long-term reliability of photovoltaic modules. Summary of the Invention

[0003] This application provides a photovoltaic module, a method for preparing a photovoltaic module, and a device for preparing a photovoltaic module, which at least helps to improve the problems in the prior art where the coating tensile strength of photovoltaic modules is low and the skin film is prone to delamination after the battery string cools down, leading to subsequent reliability failures.

[0004] According to some embodiments of this application, one aspect of this application provides a photovoltaic module, including: a solar cell; a solder ribbon located on one side of the solar cell; an intermediate layer located on the side of the solder ribbon opposite to the solar cell; and an encapsulant film located on the side of the intermediate layer opposite to the solar cell; wherein the intermediate layer includes an active layer and / or an interface modification layer, the surface energy of the active layer is greater than the surface energy of the encapsulant film, and the interface modification layer is used to bond with the solder ribbon through chemical bonds and / or intermolecular forces; when the intermediate layer includes the active layer and the interface modification layer, the active layer is located on the side of the interface modification layer opposite to the solar cell.

[0005] In some embodiments, the active layer is made of the same material as the adhesive film.

[0006] In some embodiments, the material of the film comprises an uncrosslinked thermoplastic polyolefin.

[0007] In some embodiments, the material of the interface modification layer includes a silane coupling agent.

[0008] In some embodiments, there are multiple solar cells, intermediate layers, and adhesive films, with each adhesive film corresponding to a solar cell and each intermediate layer corresponding to an adhesive film.

[0009] In some embodiments, the thickness of the intermediate layer is less than the thickness of the adhesive film.

[0010] In some embodiments, the surface energy of the active layer ranges from 38 mN / m to 60 mN / m.

[0011] According to some embodiments of this application, another aspect of this application provides a method for preparing a photovoltaic module. The method is used to prepare any of the photovoltaic modules described above. The method includes: providing a solar cell; placing a solder ribbon on one side of the solar cell; forming an encapsulant film and forming an intermediate layer on one side of the encapsulant film; covering the side of the solder ribbon opposite to the solar cell with the encapsulant film forming the intermediate layer, and the intermediate layer being located on the side of the encapsulant film close to the solder ribbon.

[0012] In some embodiments, the intermediate layer includes an active layer forming an adhesive film, and the intermediate layer is formed on one side of the adhesive film, including: providing a pre-adhesive film, and, during the traction of the pre-adhesive film, subjecting one side surface of the pre-adhesive film to corona treatment or plasma treatment, such that the treated area of ​​the pre-adhesive film forms the active layer, and the untreated area of ​​the pre-adhesive film forms the adhesive film.

[0013] In some embodiments, the intermediate layer includes an interface modification layer, which is formed on one side of the adhesive film and includes at least one of the following: spraying a silane coupling agent onto one side of the adhesive film to form the interface modification layer; or spraying a silane coupling agent onto one side of the solder ribbon and the solar cell to form the interface modification layer.

[0014] In some embodiments, during the traction process of the pre-coated film, corona treatment or plasma treatment is performed on one side surface of the pre-coated film, including: controlling the pre-coated film to pass through the discharge area of ​​the corona treatment mechanism at a traction speed of 400 m / min-450 m / min, so as to use the corona treatment mechanism to perform corona treatment on the surface of the pre-coated film, wherein the voltage of the corona treatment mechanism is 20KV-30KV, the discharge frequency of the corona treatment mechanism is 20KHz-30KHz, and the corona treatment mechanism is disposed on the traction path of the pre-coated film; or, controlling the pre-coated film to pass through the processing nozzle of the plasma treatment mechanism at a uniform traction speed, so as to use the plasma treatment mechanism to perform plasma treatment on the surface of the pre-coated film, wherein the processing nozzle of the plasma treatment mechanism maintains a distance of 10mm-15mm from the surface of the film, and the plasma treatment mechanism is disposed on the traction path of the pre-coated film.

[0015] According to some embodiments of this application, another aspect of this application provides a photovoltaic module fabrication apparatus. The fabrication apparatus is used to fabricate any of the photovoltaic modules described above. The fabrication apparatus includes: a providing module for providing solar cells; a placing module for placing solder ribbons on one side of the solar cells; a forming module for forming an encapsulant film and forming an intermediate layer on one side of the encapsulant film; and an assembly module for covering the side of the solder ribbon opposite to the solar cells with the encapsulant film forming the intermediate layer, wherein the intermediate layer is located on the side of the encapsulant film closer to the solder ribbon.

[0016] The technical solution provided in this application has at least the following advantages:

[0017] A photovoltaic module includes solar cells, solder ribbons, an interlayer, and an encapsulant film stacked sequentially. The interlayer includes an active layer and / or an interface modification layer. The surface energy of the active layer is greater than that of the encapsulant film. The interface modification layer is used to bond with the solder ribbon through chemical bonds and / or intermolecular forces. When the interlayer includes an active layer and an interface modification layer, the active layer is located on the side of the interface modification layer away from the solar cells. To address the issues of low coating tensile strength and easy delamination of the coating film after cooling of the cell string in existing photovoltaic modules, leading to subsequent reliability failures, this application proposes an intermediate layer located between the solder ribbon and the encapsulant film. This intermediate layer comprises an active layer and / or an interface modification layer. The active layer, due to its higher surface energy than the encapsulant film, significantly improves the wettability and physical adhesion between the non-polar or low surface energy encapsulant film and the solder ribbon, preventing delamination. The interface modification layer binds to the solder ribbon through chemical bonds and / or intermolecular forces, forming a stable composite connection at the interface. This effectively solves the cooling delamination problem caused by the low adhesion of the encapsulant film (such as TPO (Thermoplastic Polyolefin)) during low-temperature stringing processes, and maintains interface stability after high-temperature lamination. Ultimately, this achieves the technical effect of suppressing delamination of the encapsulant film after cooling due to insufficient adhesion and delamination of the finished module after lamination, thereby improving the reliability of the module. Attached Figure Description

[0018] One or more embodiments are illustrated by way of example with reference to the accompanying drawings. These illustrations do not constitute a limitation on the embodiments. Unless otherwise stated, the drawings in the accompanying drawings do not constitute a limitation on scale. In order to more clearly illustrate the technical solutions in the embodiments of this application or in the conventional art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1This is a schematic cross-sectional view of a photovoltaic module according to an embodiment of this application;

[0020] Figure 2 This is a cross-sectional structural diagram of another photovoltaic module provided according to an embodiment of this application;

[0021] Figure 3 This is a schematic cross-sectional view of a photovoltaic module after the solder ribbon is placed in a method for manufacturing a photovoltaic module according to an embodiment of this application.

[0022] Figure 4 This is a schematic cross-sectional view of a photovoltaic module in which an active layer is formed during the fabrication method of a photovoltaic module according to an embodiment of this application.

[0023] Figure 5 This is a schematic cross-sectional view of a photovoltaic module in which an interface modification layer is formed during the preparation method of a photovoltaic module according to an embodiment of this application.

[0024] Figure 6 This is a cross-sectional structural diagram of a photovoltaic module in which the cell film is coated according to a method for manufacturing a photovoltaic module provided in this application.

[0025] The above figures include the following reference numerals:

[0026] 10. Solar cell; 11. Solder ribbon; 12. Intermediate layer; 13. Encapsulant film; 14. Active layer; 15. Interface modification layer; 16. Preparatory encapsulant film; 17. Traction mechanism; 18. Corona discharge mechanism; 181. High voltage electrode; 182. Grounding metal cylinder. Detailed Implementation

[0027] As is known from the background art, the existing photovoltaic modules have low coating tensile strength, and the coating is prone to delamination after the battery string cools down, leading to subsequent reliability failures. In order to solve the above problems, this application provides a photovoltaic module, a method for preparing a photovoltaic module, and a device for preparing a photovoltaic module.

[0028] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.

[0029] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0030] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent three cases: A exists, A and B exist simultaneously, and B exists. In addition, the character " / " in this document generally indicates that the related objects before and after it have an "or" relationship.

[0031] In the description of the embodiments of this application, the term "multiple" refers to two or more (including two), similarly, "multiple sets" refers to two or more (including two sets), and "multiple pieces" refers to two or more (including two pieces).

[0032] In the description of the embodiments of this application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the embodiments of this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of this application.

[0033] In the description of the embodiments of this application, unless otherwise expressly specified and limited, the technical terms such as "installation," "connection," "joining," and "fixing" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. For those skilled in the art, the specific meaning of the above terms in the embodiments of this application can be understood according to the specific circumstances.

[0034] In the accompanying drawings corresponding to the embodiments of this application, the thickness and area of ​​the layers are enlarged for better understanding and ease of description. When describing a component (such as a layer, film, region, or substrate) on or on the surface of another component, the component may be "directly" located on the surface of the other component, or there may be a third component between the two components. Conversely, when describing a component on the surface of another component, or when another component is formed or disposed on the surface of a component, it indicates that there is no third component between the two components. Furthermore, when describing a component as being "generally" formed on another component, it means that the component is not formed on the entire surface (or front surface) of the other component, nor is it formed on a portion of the edge of the entire surface.

[0035] In the description of the embodiments of this application, when a component "includes" another component, other components are not excluded unless otherwise stated, and other components may be further included. Furthermore, when a component such as a layer, film, region, or plate is referred to as being "on / located" on another component, it can be "directly on" the other component (i.e., located on the surface of the other component with no other components between them), or another component may be present therein. Moreover, when a component such as a layer, film, region, or plate is "directly located" on another component, or when a component such as a layer, film, region, or plate is located on the surface of another component, it indicates that no other components are located therein.

[0036] The terminology used in the description of the various embodiments described herein is for the purpose of describing particular embodiments only and is not intended to be limiting. As used in the description of the various embodiments and the appended claims, the term "foreword" is also intended to include the plural form unless the context clearly indicates otherwise. Components include layers, films, regions, or plates, etc.

[0037] The embodiments of this application will now be described in detail with reference to the accompanying drawings. However, those skilled in the art will understand that many technical details have been provided in the embodiments of this application to facilitate a better understanding of the application. However, the technical solutions claimed in this application can be implemented even without these technical details and various variations and modifications based on the following embodiments.

[0038] This application provides a photovoltaic module, such as... Figure 1 and Figure 2 As shown, it includes:

[0039] 10 solar cells;

[0040] The solder strip 11 is located on one side of the aforementioned solar cell 10;

[0041] Intermediate layer 12 is located on the side of the solder strip 11 that is opposite to the solar cell 10;

[0042] In one embodiment, the solder strip is located on one side surface of the solar cell, and the intermediate layer covers the solder strip and the solar cell.

[0043] The adhesive film 13 is located on the side of the intermediate layer 12 that is opposite to the solar cell 10.

[0044] In practical applications, those skilled in the art can flexibly select appropriate materials for the above-mentioned adhesive film according to actual needs, and this application does not impose specific restrictions in this regard.

[0045] In one embodiment, the material of the adhesive film includes TPO.

[0046] The intermediate layer 12 includes an active layer 14 and / or an interface modification layer 15. The surface energy of the active layer 14 is greater than the surface energy of the adhesive film 13. The interface modification layer 15 is used to bond with the solder ribbon 11 through chemical bonds and / or intermolecular forces. When the intermediate layer 12 includes the active layer 14 and the interface modification layer 15, the active layer 14 is located on the side of the interface modification layer 15 that is away from the solar cell 10.

[0047] According to the above embodiments, the photovoltaic module includes solar cells, solder ribbons, an intermediate layer and an encapsulant film stacked sequentially. The intermediate layer includes an active layer and / or an interface modification layer. The surface energy of the active layer is greater than that of the encapsulant film. The interface modification layer is used to bond with the solder ribbon through chemical bonds and / or intermolecular forces. When the intermediate layer includes an active layer and an interface modification layer, the active layer is located on the side of the interface modification layer away from the solar cell. To address the issues of low coating tensile strength and easy delamination of the coating film after cooling of the cell string in existing photovoltaic modules, leading to subsequent reliability failures, this application proposes an intermediate layer located between the solder ribbon and the encapsulant film. This intermediate layer comprises an active layer and / or an interface modification layer. The active layer, due to its higher surface energy than the encapsulant film, significantly improves the wettability and physical adhesion between the non-polar or low surface energy encapsulant film and the solder ribbon, preventing delamination. The interface modification layer binds to the solder ribbon through chemical bonds and / or intermolecular forces, forming a stable composite connection at the interface. This effectively solves the cooling delamination problem caused by the low adhesion of the encapsulant film (such as TPO) in low-temperature stringing processes and maintains interface stability after high-temperature lamination. Ultimately, this achieves the technical effect of suppressing delamination of the encapsulant film after cooling due to insufficient adhesion and delamination of the finished module after lamination, thereby improving the reliability of the module.

[0048] It should be noted that in existing low-temperature stringing processes, pre-crosslinked EVA (Ethylene-Vinyl Acetate) is commonly used to cover the cell strings during the lamination process. Although the EL (Electroluminescence) test results are normal after low-temperature lamination, the string EL test images show blackening, with the blackened area accounting for 20-30%. This severe blackening area affects the judgment of defects such as scratches and broken cells during the defect screening of the module strings, resulting in the inability to screen defects in the laminated modules in advance. To address this, we have tried changing the type of encapsulant film during stringing. Currently, there is an amorphous TPO encapsulant film, which shows good EL test results after low-temperature stringing. However, this encapsulant film is prone to wrinkling and delamination after cooling, and it also delaminates after high-temperature baking after lamination, leading to subsequent reliability failures. This application improves the adhesion between the encapsulant film and the solder ribbon and cell by adding an intermediate layer between the solder ribbon and the encapsulant film.

[0049] In one alternative embodiment, the active layer is made of the same material as the adhesive film. In this embodiment, the consistency of the material between the active layer and the adhesive film ensures high compatibility at the interface, eliminating potential interface defects or micro-voids caused by differences in molecular chain structure between different material systems (such as mismatch in polarity, crystallinity, or coefficient of thermal expansion). By utilizing the natural affinity between molecules of the same material, the active layer and the adhesive film can form a more uniform and dense molecular-level bond during lamination or curing. This effectively compensates for the potential bonding force fluctuations when relying solely on surface energy differences to establish energy level differences, significantly enhancing the interfacial bonding stability between the active layer and the adhesive film, and preventing delamination due to insufficient interfacial adhesion under low-temperature stringing cooling or high-temperature baking conditions.

[0050] In another alternative, the material of the aforementioned film includes uncrosslinked thermoplastic polyolefin. In this embodiment, the material of the film includes uncrosslinked thermoplastic polyolefin, which means that the film maintains a linear molecular structure rather than a network crosslinked structure before lamination. This material has good flowability and thermoplasticity, but its adhesion is relatively weak at room temperature. Therefore, it needs to work together with the intermediate layer located below it. The interface modification layer of the intermediate layer is tightly bonded to the solder ribbon through chemical bonds or intermolecular forces, which solves the problem of poor adhesion between the thermoplastic polyolefin and the metal solder ribbon caused by its non-polarity. Its active layer, because its surface energy is higher than that of the film, can form an effective physical or chemical bond with the film, making up for the defect of insufficient interfacial adhesion of the film itself. At the same time, since uncrosslinked thermoplastic polyolefin is used instead of precrosslinked EVA film, the blackening phenomenon of the cell string EL caused by uneven stress release or by-products of side reactions in the film during low-temperature stringing and subsequent high-temperature baking is avoided. Thus, while ensuring the reliability of the module interface bonding, the appearance consistency and long-term operational reliability of the photovoltaic module are significantly improved.

[0051] It should be noted that this application uses an amorphous, non-pre-crosslinked TPO film instead of a conventional pre-crosslinked EVA film, which improves the blackening problem in the serial EL detection image and thus improves the module yield.

[0052] According to some exemplary embodiments of this application, the material of the interface modification layer includes a silane coupling agent. In this embodiment, the silane coupling agent is a bifunctional molecule containing two different reactive groups. One end of its molecular structure contains an alkoxy group that is easily hydrolyzed, and the other end contains an organic functional group that can react with organic polymer materials. The silane coupling agent can improve the interfacial bonding strength between the adhesive film and the battery cell through molecular bridging. The alkoxy group at one end can undergo hydrolysis-condensation reaction with the silanol groups and metal oxides on the surface of the battery cell to form covalent bonds. The organic functional group at the other end interacts with the non-polar adhesive film through entanglement and compatibility, forming a stable covalent bond and intermolecular force composite interface layer at the interface between the adhesive film and the adherend. This significantly improves the interfacial adhesion and high-temperature stability, thereby inhibiting delamination of the adhesive film after cooling due to insufficient adhesion and delamination and EL blackening after high-temperature baking of the finished module after lamination.

[0053] According to some other exemplary embodiments of this application, there are multiple solar cells, intermediate layers, and encapsulant films, with each encapsulant film corresponding to a solar cell and each intermediate layer corresponding to an encapsulant film. In this embodiment, the photovoltaic module is composed of multiple independent cell units connected in series or parallel, and each cell unit is independently configured with its own intermediate layer and encapsulant film, forming an independent corresponding hierarchical structure of cell-intermediate layer-encapsulant film. This ensures that the interfacial adhesion between each cell and its encapsulant film is effectively guaranteed during low-temperature stringing and subsequent high-temperature baking, avoiding stress concentration or uneven peeling caused by large-area shared film layers, and further improving the overall reliability of the module.

[0054] According to some exemplary embodiments of this application, the thickness of the intermediate layer is less than the thickness of the adhesive film. In this embodiment, the thickness of the intermediate layer is less than the thickness of the adhesive film. Through this specific thickness ratio, the intermediate layer can accurately perform its function as an active layer or interface modification layer without significantly increasing the overall lamination thickness or rigidity burden of the component. This ensures that the intermediate layer can fully wet the solder ribbon surface to form strong chemical bonds or intermolecular forces, while avoiding the problem of additional interlayer stress or uneven heat transfer during the lamination process caused by an excessively thick intermediate layer. Thus, while maintaining good mechanical strength of the component, the bonding quality of the interlayer interface is optimized, achieving the technical effect of balancing interface adhesion performance and lamination process stability within a limited space.

[0055] In other embodiments, the surface energy of the active layer ranges from 38 mN / m to 60 mN / m. In this embodiment, by limiting the surface energy of the active layer to the range of 38 mN / m to 60 mN / m, it is ensured that it has sufficient polarity to significantly improve the wettability between the low surface energy adhesive film and the solder ribbon or battery cell, thereby further enhancing the physical adhesion of the interface and further preventing cooling delamination due to insufficient adhesion.

[0056] This application also provides a method for preparing a photovoltaic module. The method is used to prepare any of the aforementioned photovoltaic modules. The method includes:

[0057] Step S101, as follows Figure 3 As shown, a solar cell 10 is provided;

[0058] Step S102, as follows Figure 3 As shown, a solder strip 11 is placed on one side of the aforementioned solar cell 10;

[0059] Step S103, as follows Figure 4 and Figure 5 As shown, an adhesive film 13 is formed, and an intermediate layer 12 is formed on one side of the adhesive film 13;

[0060] Step S104, as follows Figure 1 , Figure 2 and Figure 6 As shown, the adhesive film 13 forming the intermediate layer 12 covers the side of the solder ribbon 11 away from the solar cell 10, and the intermediate layer 12 is located on the side of the adhesive film 13 close to the solder ribbon 11.

[0061] In the above embodiments, a solder ribbon is first placed on one side of the solar cell, then an adhesive film is formed, and an intermediate layer is formed on one side of the adhesive film. Finally, the adhesive film forming the intermediate layer is covered on the side of the solder ribbon away from the solar cell, wherein the intermediate layer is located on the side of the adhesive film close to the solder ribbon. To address the issues of low coating tensile strength and easy delamination of the coating film after cooling of the cell string in existing photovoltaic modules, leading to subsequent reliability failures, this application proposes an intermediate layer located between the solder ribbon and the encapsulant film. This intermediate layer comprises an active layer and / or an interface modification layer. The active layer, due to its higher surface energy than the encapsulant film, significantly improves the wettability and physical adhesion between the non-polar or low surface energy encapsulant film and the solder ribbon, preventing delamination. The interface modification layer binds to the solder ribbon through chemical bonds and / or intermolecular forces, forming a stable composite connection at the interface. This effectively solves the cooling delamination problem caused by the low adhesion of the encapsulant film (such as TPO) in low-temperature stringing processes and maintains interface stability after high-temperature lamination. Ultimately, this achieves the technical effect of suppressing delamination of the encapsulant film after cooling due to insufficient adhesion and delamination of the finished module after lamination, thereby improving the reliability of the module.

[0062] In one alternative, such as Figure 4 As shown, the intermediate layer 12 includes an active layer 14, forms an adhesive film 13, and the intermediate layer 12 is formed on one side of the adhesive film 13. The intermediate layer 12 includes: providing a pre-adhesive film 16, and, during the traction of the pre-adhesive film 16, performing corona treatment or plasma treatment on one side surface of the pre-adhesive film 16, so that the treated area of ​​the pre-adhesive film 16 forms the active layer 14, and the untreated area of ​​the pre-adhesive film 16 forms the adhesive film 13. In this embodiment, by performing corona or plasma treatment on one side of the pre-coated film during the traction process, high-energy particles or free radicals are used to etch and graft the polymer chains on the surface of the pre-coated film, forming an active layer rich in polar groups in the treated area. During actual assembly, this active layer faces the solder ribbon, and its high surface energy characteristics can significantly enhance the wettability and chemical bonding ability between the film and the metal solder ribbon. Compared with untreated ordinary film, this structure effectively improves the adhesion strength between the film and the cell / solder ribbon interface under low-temperature stringing and high-temperature baking conditions, avoiding delamination due to insufficient interfacial bonding or delamination after high-temperature baking, and ensuring the long-term stability and reliability of the internal structure of the photovoltaic module.

[0063] In one embodiment, such as Figure 4As shown, the preparative adhesive film 16 is pulled by the traction mechanism 17, and the active layer 14 is formed by the corona treatment mechanism 18 / plasma treatment mechanism (not shown in the figure). Then the adhesive film 13 is cut. The corona treatment mechanism 18 includes a high voltage electrode 181 and a grounded metal cylinder 182.

[0064] In another alternative embodiment, the intermediate layer includes an interface modification layer, formed on one side of the adhesive film, comprising at least one of the following: spraying a silane coupling agent onto one side of the adhesive film to form the interface modification layer; or spraying a silane coupling agent onto one side of the solder ribbon and the solar cell to form the interface modification layer. In this embodiment, by spraying a silane coupling agent onto the adhesive film and / or the solder ribbon and the cell surface to form an interface modification layer, the bifunctional characteristics of the silane coupling agent are utilized to construct molecular bridges between the inorganic metal / silicon surface and the organic adhesive film, enhancing the chemical bonding and physical adsorption force at the interface. This effectively improves the adhesion strength between the adhesive film and the solder ribbon / cell interface, resulting in a more stable interface bond during the cooling process after low-temperature stringing and subsequent high-temperature baking processes. This avoids delamination problems caused by insufficient interface adhesion during cooling and delamination after high-temperature baking, thereby improving the structural reliability and long-term service stability of the photovoltaic module.

[0065] In one embodiment, such as Figure 5 As shown, the intermediate layer 12 includes an interface modification layer 15. The adhesive film 13 is pulled by the traction mechanism 17, then the adhesive film 13 is cut, and finally a silane coupling agent is sprayed on one side of the cut adhesive film 13 to form the interface modification layer 15.

[0066] In one embodiment, the intermediate layer includes the active layer and the interface modification layer. Forming the intermediate layer on one side of the adhesive film includes: spraying a silane coupling agent onto one side of the adhesive film to form the interface modification layer. That is, when the intermediate layer includes an active layer and an interface modification layer, it is only necessary to spray the silane coupling agent onto one side of the adhesive film; it is not necessary to spray the silane coupling agent onto the solder ribbon surface and the cell surface.

[0067] According to some exemplary embodiments of this application, during the traction process of the aforementioned pre-coated film, corona treatment or plasma treatment is performed on one side surface of the aforementioned pre-coated film, including: controlling the aforementioned pre-coated film to pass through the discharge area of ​​the corona treatment mechanism at a traction speed of 400 m / min to 450 m / min, so as to use the aforementioned corona treatment mechanism to perform the corona treatment on the surface of the aforementioned pre-coated film, wherein the voltage of the aforementioned corona treatment mechanism is 20KV to 30KV, the discharge frequency of the aforementioned corona treatment mechanism is 20KHz to 30KHz, and the aforementioned corona treatment mechanism is disposed on the traction path of the aforementioned pre-coated film; or, controlling the aforementioned pre-coated film to pass through the processing nozzle of the plasma treatment mechanism at a uniform traction speed, so as to use the aforementioned plasma treatment mechanism to perform the plasma treatment on the surface of the aforementioned pre-coated film, wherein the processing nozzle of the aforementioned plasma treatment mechanism maintains a distance of 10mm to 15mm from the surface of the film, and the aforementioned plasma treatment mechanism is disposed on the traction path of the aforementioned pre-coated film. In this embodiment, the pre-coated film is controlled to pass through the discharge area of ​​the corona treatment mechanism at a traction speed of 400 m / min-450 m / min, coupled with a voltage of 20KV-30KV and a discharge frequency of 20KHz-30KHz. This aims to ensure a stable and uniform surface energy increase on the surface of the pre-coated film within the treatment area by precisely matching the film's travel speed with the corona energy input density, avoiding insufficient treatment due to excessive speed or localized overheating damage due to excessively slow speed. Alternatively, the pre-coated film is controlled to pass through the plasma treatment mechanism at a uniform traction speed, maintaining a specific distance of 10mm-15mm between the treatment nozzle and the film surface. This utilizes the uniform coverage characteristics of the plasma jet to activate and modify the surface of the pre-coated film within an optimal working distance, preventing uneven treatment intensity caused by spacing fluctuations. By limiting these specific process parameters, a highly active intermediate layer can be consistently formed in the treatment area of ​​the pre-coated film, thereby significantly improving the bonding quality between the intermediate layer and the film substrate, and thus improving the lamination reliability of photovoltaic modules under low-temperature stringing and high-temperature baking environments.

[0068] It should be noted that the process of low-temperature coating of battery strings is generally as follows: film traction → film cutting → film adsorption → battery cell coating.

[0069] In one embodiment, to prevent the TPO film from delaminating and blistering during cooling after stringing due to low adhesion between the film and the solar cells and its own thermal expansion and contraction stress, a corona treatment mechanism / plasma treatment mechanism is added at the position after the film roll is pulled by the stringing machine. This mechanism forms an active layer before the film is cut. The corona treatment mechanism includes a high-voltage electrode and a grounded metal cylinder. A discharge region is formed between the high-voltage electrode and the grounded metal cylinder, with a spacing of 0.8mm-1.5mm. The high-voltage electrode is configured to generate corona discharge at a voltage of 20-30KV and a frequency of 20-30KHz, so that a uniform active layer (with a thickness ranging from 20nm to 300nm) is formed on the surface of the pre-applied film traveling through the discharge region at a speed of 400-450m / min. This results in a dyne value of 42-46 on the surface of the treated pre-applied film, and the module is encapsulated within 48 hours to avoid surface energy degradation. The plasma treatment unit can be a small jet-type atmospheric low-temperature plasma treatment unit, using oxygen or nitrogen as the working gas. The treatment nozzle of the plasma treatment unit is kept stationary at a distance of 10-15 mm from the surface of the pre-coated film, and the pre-coated film is moved uniformly to form a polar oxide layer (i.e., the above-mentioned active layer) with a thickness of 80nm-180nm on the surface of the pre-coated film. The dyne value of the surface of the pre-coated film after treatment reaches 52-60.

[0070] In one embodiment, to prevent the TPO film from delaminating and blistering during cooling due to low adhesion between the film and the solar cell and its own thermal expansion and contraction stress after stringing, a silane coupling agent can be sprayed onto the bottom of the film. To prevent premature volatilization of the silane coupling agent, this process is placed between film cutting and film adsorption. The silane coupling agent is directly sprayed onto the bottom of the film using a spraying device located at the bottom of the film. The silane coupling agent can enhance the interfacial bonding strength through molecular bridging. The alkoxy group at one end can undergo hydrolysis-condensation reaction with the silanol groups and metal oxides on the surface of the solar cell to form covalent bonds. The organic functional group at the other end entangles and is compatible with the non-polar film, forming a stable covalent bond + intermolecular force composite interface layer (i.e., the above-mentioned interface modification layer) at the interface between the film and the adherend. This significantly improves the interfacial adhesion and high-temperature stability, thereby suppressing delamination of the film after stringing and cooling due to insufficient adhesion, as well as delamination and EL blackening after high-temperature baking of the finished module lamination.

[0071] This application embodiment also provides a photovoltaic module fabrication apparatus, which is used to fabricate any of the above-mentioned photovoltaic modules. The fabrication apparatus includes:

[0072] Provide modules for supplying solar cells;

[0073] A placement module for placing solder strips on one side of the aforementioned solar cell;

[0074] A forming module is used to form an adhesive film and to form an intermediate layer on one side of the adhesive film;

[0075] An assembly module is used to cover the adhesive film forming the intermediate layer on the side of the solder ribbon opposite to the solar cell, and the intermediate layer is located on the side of the adhesive film close to the solder ribbon.

[0076] Through the above embodiments, the photovoltaic module fabrication equipment is used to fabricate the photovoltaic module described above. The fabrication equipment includes a providing module, a placement module, a forming module, and an assembly module. The providing module is used to provide solar cells, the placement module is used to place solder ribbons on one side of the solar cells, the forming module is used to form an encapsulant film and form an intermediate layer on one side of the encapsulant film, and the assembly module is used to cover the side of the solder ribbons away from the solar cells with the encapsulant film forming the intermediate layer, and the intermediate layer is located on the side of the encapsulant film close to the solder ribbons. To address the issues of low coating tensile strength and easy delamination of the coating film after cooling of the cell string in existing photovoltaic modules, leading to subsequent reliability failures, this application proposes an intermediate layer located between the solder ribbon and the encapsulant film. This intermediate layer comprises an active layer and / or an interface modification layer. The active layer, due to its higher surface energy than the encapsulant film, significantly improves the wettability and physical adhesion between the non-polar or low surface energy encapsulant film and the solder ribbon, preventing delamination. The interface modification layer binds to the solder ribbon through chemical bonds and / or intermolecular forces, forming a stable composite connection at the interface. This effectively solves the cooling delamination problem caused by the low adhesion of the encapsulant film (such as TPO) in low-temperature stringing processes and maintains interface stability after high-temperature lamination. Ultimately, this achieves the technical effect of suppressing delamination of the encapsulant film after cooling due to insufficient adhesion and delamination of the finished module after lamination, thereby improving the reliability of the module.

[0077] Those skilled in the art will understand that the above embodiments are specific examples of implementing this application, and in practical applications, various changes in form and detail can be made without departing from the spirit and scope of this application. Any person skilled in the art can make various alterations and modifications without departing from the spirit and scope of this application; therefore, the scope of protection of this application should be determined by the scope defined in the claims.

Claims

1. A photovoltaic module, characterized by, include: Solar cells; The solder strip is located on one side of the solar cell. The intermediate layer is located on the side of the solder strip opposite to the solar cell. The adhesive film is located on the side of the intermediate layer opposite to the solar cell. The intermediate layer includes an active layer and / or an interface-modified layer. The surface energy of the active layer is greater than that of the adhesive film. The interface-modified layer is used to bond with the solder ribbon through chemical bonds and / or intermolecular forces. When the intermediate layer includes the active layer and the interface-modified layer, the active layer is located on the side of the interface-modified layer opposite to the solar cell.

2. The photovoltaic module of claim 1, wherein, The active layer is made of the same material as the adhesive film.

3. The photovoltaic module of claim 1, wherein, The film is made of thermoplastic polyolefins that have not undergone cross-linking.

4. The photovoltaic module of claim 1, wherein, The material of the interface modification layer includes a silane coupling agent.

5. The photovoltaic module of claim 1, wherein, There are multiple solar cells, intermediate layers, and adhesive films. Each adhesive film corresponds to a solar cell, and each intermediate layer corresponds to an adhesive film.

6. The photovoltaic module of claim 1, wherein, The thickness of the intermediate layer is less than the thickness of the adhesive film.

7. The photovoltaic module of claim 1, wherein, The surface energy of the active layer ranges from 38mN / m to 60mN / m.

8. A method of making a photovoltaic module, characterized by, The preparation method is used to prepare the photovoltaic module according to any one of claims 1-7, and the preparation method includes: Provide solar cells; A solder strip is placed on one side of the solar cell; A film is formed, and an intermediate layer is formed on one side of the film; The adhesive film forming the intermediate layer is applied to the side of the solder ribbon facing away from the solar cell, and the intermediate layer is located on the side of the adhesive film closer to the solder ribbon.

9. The method of claim 8, wherein the method further comprises, The intermediate layer includes an active layer forming an adhesive film, and an intermediate layer is formed on one side of the adhesive film, comprising: A pre-coated film is provided, and during the traction process of the pre-coated film, one side surface of the pre-coated film is subjected to corona treatment or plasma treatment, so that the treated area of ​​the pre-coated film forms the active layer, and the untreated area of ​​the pre-coated film forms the adhesive film.

10. The method of claim 8, wherein the method further comprises, The intermediate layer includes an interface modification layer, which is formed on one side of the adhesive film and includes at least one of the following: A silane coupling agent is sprayed onto one side of the adhesive film to form the interface modification layer; A silane coupling agent is sprayed onto one side of the solder strip and the solar cell to form the interface modification layer.

11. The method of claim 9, wherein the method further comprises: During the traction process of the prepared adhesive film, one side surface of the prepared adhesive film is subjected to corona treatment or plasma treatment, including: The prepared adhesive film is controlled to pass through the discharge area of ​​the corona mechanism at a traction speed of 400 m / min-450 m / min, so as to perform corona treatment on the surface of the prepared adhesive film using the corona mechanism. The voltage of the corona mechanism is 20KV-30KV, the discharge frequency of the corona mechanism is 20KHz-30KHz, and the corona mechanism is set on the traction path of the prepared adhesive film. or, The prepared adhesive film is controlled to pass through the processing nozzle of the plasma processing mechanism at a uniform traction speed, so as to perform plasma processing on the surface of the prepared adhesive film using the plasma processing mechanism. The processing nozzle of the plasma processing mechanism maintains a distance of 10mm-15mm from the surface of the adhesive film, and the plasma processing mechanism is arranged on the traction path of the prepared adhesive film.

12. An apparatus for the production of a photovoltaic module, characterized in that The fabrication equipment is used to fabricate the photovoltaic module according to any one of claims 1-7, and the fabrication equipment comprises: Provide modules for supplying solar cells; A placement module for placing solder strips on one side of the solar cell; A forming module for forming an adhesive film and forming an intermediate layer on one side of the adhesive film; An assembly module is used to cover the adhesive film forming the intermediate layer onto the side of the solder ribbon opposite to the solar cell, wherein the intermediate layer is located on the side of the adhesive film closer to the solder ribbon.