A solar cell and its preparation method
By matching the absorption band of the barrier layer with the laser wavelength during solar cell fabrication, and using green or purple lasers to remove unwanted areas, the thermal damage to the silicon substrate caused by laser film opening is solved, thus improving the fabrication quality and electrical performance of the cells.
Patent Information
- Application Number
- CN202611264395.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
In the current back-contact cell fabrication process, when laser film is opened, the laser energy can easily pass through the BSG barrier layer and cause thermal damage to the silicon substrate, affecting patterning processing and solar cell performance.
By matching the absorption band of the first blocking layer with the wavelength of the first laser, the absorption efficiency of the blocking layer to the laser is improved, thermal damage is reduced, and green or purple lasers are used to remove unwanted areas.
This improved the fabrication quality and electrical performance of solar cells, and reduced the thermal damage caused by laser-induced film opening and the thermal impact on non-film-opened areas.
Smart Images

Figure CN123124486A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solar energy technology, and more particularly to a solar cell and its preparation method. Background Technology
[0002] A back contact (BC) cell includes P-regions and N-regions formed on the back side of a silicon substrate, and electrodes electrically connected to the P-regions and N-regions, respectively.
[0003] In existing back-contact solar cell fabrication processes, a tunneling oxide layer, a boron-doped polycrystalline silicon layer, and a borosilicate glass (BSG) barrier layer can be formed on the back side of a silicon substrate. Subsequently, a laser can be used to remove the BSG barrier layer in a predetermined area, and the remaining BSG barrier layer can be used as a mask to remove the boron-doped polycrystalline silicon layer and tunneling oxide layer in the exposed area, thus forming a patterned region for subsequent fabrication of passivation contact structures with different doping types. However, during the laser-induced masking process, some laser energy can easily penetrate the BSG barrier layer and be transferred to the underlying doped polycrystalline silicon layer, tunneling oxide layer, and silicon substrate, potentially causing thermal damage to the silicon substrate and thermally affecting adjacent non-patterned areas, thereby impacting subsequent patterning processing and the performance of the solar cell. Summary of the Invention
[0004] This invention provides a solar cell and a method for its fabrication. By matching the absorption band of the first barrier layer with the wavelength of the first laser, the absorption efficiency of the first barrier layer for the first laser is improved, thereby enhancing the electrical performance of the solar cell.
[0005] The first aspect of this invention provides a method for preparing a solar cell, the method comprising: A silicon substrate is provided; the silicon substrate includes a front side and a back side opposite to each other, the back side including a first region and a second region arranged at intervals, and an isolation region between the first region and the second region; A first dielectric layer and a first doped layer are sequentially formed on the back side of the silicon substrate, and a first barrier layer is also provided on the first doped layer; A first laser is used to remove the first blocking layer, the first doped layer, and the first dielectric layer outside the first region; wherein the wavelength of the first laser is located within the absorption band of the first blocking layer.
[0006] Optionally, the first laser may be a green-skinned laser or a purple-skinned laser; The first blocking layer has a first absorption band corresponding to the wavelength of the green laser, or the first blocking layer has a second absorption band corresponding to the wavelength of the purple laser.
[0007] Optionally, the first blocking layer has a first refractive index corresponding to the first absorption band, or the first blocking layer has a second refractive index corresponding to the second absorption band.
[0008] Optionally, the refractive index of the first barrier layer is in the range of 1.51-1.6.
[0009] Optionally, the first doped layer and the first barrier layer have doping elements of a first conductivity type; The first barrier layer is formed on the back side of the silicon substrate, comprising: The absorption band of the first barrier layer can be adjusted by controlling the concentration of doping elements of the first conductivity type in the first barrier layer.
[0010] Optionally, the silicon substrate has a doping element of a second conductivity type; The second conductivity type dopant has the opposite conductivity type to the first conductivity type dopant.
[0011] Optionally, the first conductivity type doping element is a group IIIA element, and the second conductivity type doping element is a group VA element.
[0012] Optionally, the concentration range of the first conductivity type dopant element in the first barrier layer satisfies 1×10⁻⁶. 20 atoms / cm 3 -5×10 20 atoms / cm 3 So that the first barrier layer has the first absorption band, or, the concentration range of the first conductivity type dopant element in the first barrier layer satisfies 1×10 21 atoms / cm 3 -1×10 22 atoms / cm 3 This is to give the first blocking layer the second absorption band.
[0013] Optionally, the concentration range of the first conductivity type dopant element in the first doped layer satisfies 6 × 10⁻⁶. 18 atoms / cm 3 -6×10 20 atoms / cm 3 .
[0014] Optionally, the thickness of the first dielectric layer is in the range of 1nm-2nm.
[0015] Optionally, the thickness of the first doped layer is in the range of 50nm-500nm.
[0016] Optionally, the thickness of the first barrier layer is in the range of 30nm-80nm.
[0017] Optionally, the method for fabricating solar cells also includes: A second dielectric layer and a second doped layer are sequentially formed on the back side of the silicon substrate, and a second barrier layer is further provided on the second doped layer; wherein the first doped layer and the second doped layer are insulated from each other, and the first barrier layer and the second barrier layer are insulated from each other. Remove the second barrier layer, the second doped layer, and the second dielectric layer from the regions outside the second region.
[0018] Optionally, the method for fabricating solar cells also includes: A passivation layer and an anti-reflection layer are formed covering the first area, the second area, the isolation area, and the front side; A first electrode is formed that contacts the first doped layer, and a second electrode is formed that contacts the second doped layer.
[0019] A second aspect of the present invention provides a solar cell, which is prepared by the solar cell preparation method described above.
[0020] The technical solution of this invention involves sequentially forming a first dielectric layer and a first doped layer on the back side of a silicon substrate. The first doped layer also has a first barrier layer. A first laser is used to remove the first barrier layer, the first doped layer, and the first dielectric layer from areas outside the first region, thereby forming a first region retaining the first dielectric layer, the first doped layer, and the first barrier layer. By matching the absorption band of the first barrier layer with the wavelength of the first laser, the absorption efficiency of the first barrier layer to the first laser is improved, and the thermal damage caused by laser-induced film opening and the thermal impact on non-opened areas are reduced, thereby improving the fabrication quality and electrical performance of the solar cell.
[0021] It should be understood that the description in this section is not intended to identify key or essential features of the embodiments of the present invention, nor is it intended to limit the scope of the invention. Other features of the invention will become readily apparent from the following description. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1 This is a flowchart of a method for preparing a solar cell according to an embodiment of the present invention; Figure 2 This is a process flow diagram of a solar cell fabrication method provided in an embodiment of the present invention; Figure 3 This is a flowchart of a method for preparing the second region in a solar cell according to an embodiment of the present invention; Figure 4 This is a process flow diagram of the fabrication process of the second region in a solar cell provided by an embodiment of the present invention; Figure 5 This is a schematic diagram of the structure of a solar cell provided in an embodiment of the present invention. Detailed Implementation
[0024] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.
[0025] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of the invention described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.
[0026] Figure 1 This is a flowchart of a method for preparing a solar cell according to an embodiment of the present invention. Figure 2 This is a process flow diagram of a solar cell fabrication method provided in an embodiment of the present invention, in conjunction with reference to [reference needed]. Figure 1 and Figure 2 As shown, the method for fabricating this solar cell includes: S101 provides a silicon-based substrate.
[0027] The silicon substrate 00 includes a front side 01 and a back side 02, the back side 02 includes a first region 1 and a second region 2 arranged at intervals, and an isolation region 3 is provided between the first region 1 and the second region 2.
[0028] Specifically, the silicon substrate 00 can be an N-type single-crystal silicon substrate. The front side 01 is used to receive incident light and generate photogenerated carriers. The back side 02 includes a first region 1 and a second region 2 arranged at intervals. There is an isolation region 3 between the first region 1 and the second region 2, so that the back side 02 can form passivated contact regions of different conductivity types that are spaced apart from each other to form the back functional structure of the back contact solar cell.
[0029] In some embodiments, the silicon substrate 00 can be double-sided polished before forming the back film layer. For example, a mixed solution of KOH and H₂O₂ can be used to remove cutting damage layers, contaminants, and surface defects from the surface of the silicon substrate 00, followed by alkaline polishing with NaOH or KOH solution to improve the smoothness and cleanliness of the silicon substrate 00 surface. After double-sided polishing, a relatively smooth base structure can be formed on the surface of the silicon substrate 00, facilitating uniform deposition of subsequent film layers and improving the bonding stability between the film layer and the silicon substrate 00. For example, the reflectivity of the silicon substrate 00 surface after alkaline polishing can be greater than 40%, and the base size can be 10 μm-50 μm.
[0030] S102. A first dielectric layer and a first doped layer are sequentially formed on the back side of a silicon substrate, and a first barrier layer is also formed on the first doped layer.
[0031] Specifically, a first dielectric layer 11 can be formed on the back surface 02 of the silicon substrate 00, and a first amorphous silicon layer 12 can be formed on the side of the first dielectric layer 11 away from the silicon substrate 00. The first dielectric layer 11 may include a silicon oxide layer, and the first dielectric layer 11 can be formed by thermal oxidation, wet oxidation, ozone oxidation, or chemical vapor deposition. The first dielectric layer 11 is used to passivate the back surface 02 of the silicon substrate 00, reduce interfacial recombination between the silicon substrate 00 and the subsequently formed doped polycrystalline silicon layer, and allow target carriers to be transported by tunneling. In some embodiments, the thickness of the first tunneling oxide layer 11 can be 1 nm-2 nm. The first amorphous silicon layer 12 can be deposited using a low-pressure chemical vapor deposition (LPCVD) process or a plasma-enhanced chemical vapor deposition (PECVD) process. The first amorphous silicon layer 12 is used to receive dopant atoms of a first conductivity type during subsequent atomic diffusion and is transformed into a first doped layer 13 under high temperature. In some embodiments, the thickness of the first amorphous silicon layer 12 can be 50nm-500nm, and the deposition temperature can be 500℃-650℃.
[0032] Optionally, the first doped layer 13 and the first barrier layer 14 have doped elements of a first conductivity type; forming the first barrier layer 14 on the back side 02 of the silicon substrate 00 includes: adjusting the absorption band of the first barrier layer 14 by controlling the concentration of the first conductivity type doped element in the first barrier layer 14.
[0033] Specifically, after forming the first amorphous silicon layer 12, the silicon substrate 00 can be placed in a diffusion device, and the first amorphous silicon layer 12 can be subjected to atomic diffusion of a first conductivity type according to the first preset process parameters. Doping atoms of the first conductivity type enter the first amorphous silicon layer 12, and the first amorphous silicon layer 12 crystallizes under high temperature, thereby transforming into the first doped layer 13. During the atomic diffusion process of the first conductivity type, a first barrier layer 14 can also be formed on the side of the first doped layer 13 away from the silicon substrate 00.
[0034] Optionally, the silicon substrate 00 has a second conductivity type dopant element; the second conductivity type dopant element has the opposite conductivity type to the first conductivity type dopant element.
[0035] It is understood that by making the second conductivity type dopant in the silicon substrate 00 have the opposite conductivity type to the first conductivity type dopant in the first doped layer 13, a carrier selective transport structure can be formed between the silicon substrate 00 and the first doped layer 13 to promote the collection of target carriers and suppress the transport of non-target carriers. Optionally, the silicon substrate 00 can be an N-type silicon substrate doped with group VA elements, the first doped layer 13 can be a P-type doped polycrystalline silicon layer doped with group IIIA elements, and the first barrier layer 14 can be a borosilicate glass (BSG) layer. For example, BCl3 or BBr3 can be used as a boron diffusion source to diffuse boron atoms into the first amorphous silicon layer 12. At the same time, the boron diffusion source, oxygen, and silicon material react to form a boron-containing first barrier layer 14 on the surface of the first doped layer 13.
[0036] It is also understood that a first preset process parameter can be used to control the concentration of the first conductivity type dopant element in the first barrier layer 14, thereby adjusting the absorption band of the first barrier layer 14. The first preset process parameter may include at least one of boron diffusion temperature, boron diffusion source flow rate, oxygen flow rate, and boron diffusion duration. By adjusting the boron diffusion source flow rate, the number of boron atoms supplied to the first amorphous silicon layer 12 and its surface during diffusion can be adjusted; by adjusting the oxygen flow rate, the formation rate of the first barrier layer 14, the film thickness, and the ratio of boron to silicon-oxygen components in the first barrier layer 14 can be adjusted; by adjusting the boron diffusion temperature and the boron diffusion duration, the degree of boron atom diffusion and the formation state of the first barrier layer 14 can be adjusted. Thus, the boron doping concentration in the first barrier layer 14 can reach the first preset doping concentration.
[0037] It should be noted that the first barrier layer 14 with different boron doping concentrations exhibits different absorption characteristics for different wavelengths of light. Therefore, a first preset doping concentration can be predetermined based on the wavelength of the first laser used in subsequent laser film opening, and further, a first preset process parameter corresponding to the first preset doping concentration can be determined. By performing boron diffusion according to the first preset process parameter, the absorption band of the formed first barrier layer 14 can be matched with the wavelength of the subsequent first laser.
[0038] Optionally, the first laser is a green laser or a purple laser; the first blocking layer has a first absorption band corresponding to the wavelength of the green laser, or the first blocking layer has a second absorption band corresponding to the wavelength of the purple laser.
[0039] For example, when using a 355nm purple laser for subsequent film opening, the boron doping concentration of the first barrier layer 14 can be adjusted to the range corresponding to the 355nm purple laser by controlling the boron diffusion source flow rate, oxygen flow rate, boron diffusion temperature, and boron diffusion duration. Similarly, when using a 532nm green laser for subsequent film opening, the boron diffusion source flow rate, oxygen flow rate, and / or boron diffusion duration can be increased accordingly to achieve the same concentration range as the 532nm green laser. By specifically adjusting the process parameters during boron diffusion according to the preset laser wavelength, the optical absorption characteristics of the first barrier layer 14 are adapted to the wavelength of the first laser, providing a basis for the subsequent selective removal of the first barrier layer 14 by the first laser.
[0040] In an exemplary embodiment, when the wavelength of the first laser is a 355nm violet laser, the boron diffusion temperature can be controlled at 800℃-900℃, for example, 850℃; the flow rate of the boron diffusion source in the boron diffusion cavity can be controlled at 80sccm-100sccm, for example, 90sccm; the flow rate of oxygen in the boron diffusion cavity can be controlled at 250sccm-350sccm, for example, 300sccm; and the boron diffusion duration can be controlled at 10min-20min, for example, 15min. Through the above boron diffusion process, the boron doping concentration of the first barrier layer 14 can be 1×10⁻⁶. 20 atoms / cm 3 -5×10 20 atoms / cm 3 For example, 2×10 20 atoms / cm 3 Within this boron doping concentration range, the first barrier layer 14 exhibits strong absorption at a wavelength of 355 nm, with an absorption coefficient of 1 × 10⁻⁶. 5 cm -1 -1×10 6 cm -1 This allows for more complete absorption of the energy from the 355nm purple laser, thereby improving the opening efficiency of the first blocking layer 14.
[0041] In another exemplary embodiment, when the wavelength of the first laser is a 532nm green laser, the boron diffusion temperature can be controlled at 800℃-900℃, for example, 850℃; the flow rate of the boron diffusion source in the boron diffusion cavity can be controlled at 110sccm-130sccm, for example, 120sccm; the flow rate of oxygen in the boron diffusion cavity can be controlled at 310sccm-410sccm, for example, 360sccm; and the boron diffusion duration can be controlled at 16min-26min, for example, 21min. By increasing the boron diffusion source flow rate, oxygen flow rate, and boron diffusion duration, the boron doping concentration of the first barrier layer 14 can be maintained at 1×10⁻⁶. 21 atoms / cm 3 -1×10 22 atoms / cm 3 Within this boron doping concentration range, the absorption coefficient of the first barrier layer 14 at a wavelength of 532 nm can be 1 × 10⁻⁶. 3 cm -1 -1×10 4 cm -1 This enhances the absorption of the 532nm green laser by the first blocking layer 14.
[0042] Furthermore, it should be noted that the absorption coefficient of the first barrier layer 14 at different wavelengths can be determined by transmission spectroscopy. For example, multiple sets of BSG test samples with various boron doping concentrations can be prepared, each set having the same boron doping concentration and different film thicknesses. For instance, for each boron doping concentration, BSG test samples with thicknesses of 50 nm, 100 nm, 200 nm, and 500 nm can be prepared, and the transmittance of each test sample at different wavelengths can be measured using a spectrophotometer. For the same boron doping concentration and the same wavelength, the transmittance of light after passing through the BSG decreases with increasing BSG thickness. The transmittance T, BSG thickness d, and absorption coefficient α can satisfy the following relationship: T = T0 × e -αd Taking the natural logarithm of the above relationship, we obtain: lnT = lnT0 - αd. Here, T0 represents the initial transmission coefficient, which is related to factors such as interface reflection and substrate transmission of the test sample. Therefore, we can perform a linear fit on the measurement results of multiple test samples with different thicknesses at the same boron doping concentration, using the BSG thickness d as the abscissa and the natural logarithm of the transmittance lnT as the ordinate. The absolute value of the slope of the fitted line is the absorption coefficient of the BSG at the corresponding wavelength for that boron doping concentration.
[0043] Furthermore, a spectrophotometer can be used to measure the reflectance of each BSG test sample at different wavelengths. Specifically, an integrating sphere attachment can be used to collect the reflected light from the BSG test sample to obtain the total reflectance at the corresponding wavelength, or the absolute specular reflectance of the BSG test sample can be measured. Since the incident light is divided into reflected light, transmitted light, and absorbed light after passing through the BSG test sample, the absorptivity of the BSG test sample at the corresponding wavelength can be determined by combining the reflectance and transmittance, and the absorption coefficient can be determined by combining the measurement results of multiple BSG test samples with different thicknesses. This reduces the influence of sample surface reflection on the absorption coefficient calculation results and improves the detection accuracy of the absorption coefficient corresponding to different boron doping concentrations.
[0044] By performing the above measurements on BSG test samples with various boron doping concentrations, the absorption coefficient spectra of the absorption coefficient as a function of wavelength under different boron doping concentrations can be obtained. Furthermore, the absorption coefficients of BSG with different boron doping concentrations at wavelengths of 355 nm and 532 nm can be compared. Therefore, the boron doping concentration with the larger absorption coefficient at 355 nm or 532 nm can be determined and designated as the first preset doping concentration. Subsequently, based on the correspondence between the first preset doping concentration and boron diffusion process parameters, the corresponding boron diffusion source flow rate, oxygen flow rate, boron diffusion temperature, and boron diffusion duration can be selected as the first preset process parameters.
[0045] S103, The first laser is used to remove the first blocking layer, the first doped layer and the first dielectric layer in the area outside the first region.
[0046] The wavelength of the first laser is located within the absorption band of the first blocking layer 14.
[0047] Specifically, the local opening region of the first barrier layer 14 can be determined based on the preset patterns of the first region 1, the second region 2, and the isolation region 3 on the back surface 02. When the first doped layer 13 is a P-type doped polysilicon layer, the local opening region may include the region subsequently used to form an N-type passivation contact structure and the region used to form the isolation region 3, while the region retaining the first barrier layer 14 is used to form the first region 1. For example, the first laser can sequentially pass through a beam expander, a reflector, a galvanometer, and a shaping mirror before irradiating the surface of the first barrier layer 14. The beam expander is used to adjust the diameter and divergence angle of the first laser, the reflector is used to guide the laser beam path, the galvanometer is used to control the laser spot to move according to the preset opening pattern, and the shaping mirror is used to focus and shape the laser spot. The size of the laser spot formed on the surface of the first barrier layer 14 can be, for example, 190 μm × 190 μm, and the galvanometer can control the spot to continuously scan along a predetermined path to form the desired opening pattern. The power of a purple laser with a wavelength of 355nm can be 60W, and the power of a green laser with a wavelength of 532nm can be 100W.
[0048] Understandably, since the wavelength of the first laser is within the absorption band of the first barrier layer 14, the first barrier layer 14 can absorb the energy of the first laser relatively fully and convert the absorbed laser energy into heat energy, causing the local area of the first barrier layer 14 to heat up rapidly. This allows the first barrier layer 14 to be removed from the surface of the first doped layer 13 through vaporization, ablation, and / or stripping. Compared to the case where the first barrier layer 14 does not absorb the first laser sufficiently, by matching the wavelength of the first laser to the absorption band of the first barrier layer 14, the absorption efficiency of the first barrier layer 14 is improved. This allows more laser energy to be concentrated on the first barrier layer 14, thus enabling the film opening to be completed with relatively low laser input energy or fewer scans. This improves the integrity of the removal of the first barrier layer 14 in the local area of the back surface 02 and reduces barrier layer residue in the opened area.
[0049] It is also understandable that the first barrier layer 14 can effectively absorb the first laser, thereby reducing the laser energy transmitted through the first barrier layer 14 to the first doped layer 13, the first dielectric layer 11, and the silicon substrate 00. This reduces the thermal damage caused by the first laser to the film layer below the first barrier layer 14 and the silicon substrate 00. Furthermore, while meeting the requirements for opening the film, the energy of the first laser can be appropriately reduced or the laser action time shortened. This reduces the lateral diffusion of heat to adjacent non-opened areas and shrinks the heat-affected zone, preventing cracks, warping, or localized peeling of the first barrier layer 14 remaining in the first region 1. This improves the integrity of the back-side patterned structure and the fabrication quality of the solar cell.
[0050] After removing the first barrier layer 14 in a localized area of the back surface 02, the first doped layer 13 in that localized area is exposed, while the first barrier layer 14 that was not removed by the first laser can continue to cover and protect the film structure in the first region 1. Then, using the remaining first barrier layer 14 as a mask, an alkaline etching solution can be used to remove the exposed first doped layer 13 in the localized area. The first dielectric layer 11 can provide some barrier and protection to the silicon substrate 00 during the alkaline etching process. After the first doped layer 13 in the localized area is removed, an acidic solution can be used to remove the exposed first dielectric layer 11. In some embodiments, the first barrier layer 14, the first doped layer 13, and the first dielectric layer 11 formed on the front surface 01 and / or the side surface of the silicon substrate 00 can also be removed simultaneously to remove the swirling plating structure generated during boron diffusion and film deposition. For example, a single-sided chain device can be used to remove the first barrier layer 14 on the front surface 01 and / or the side surface using hydrofluoric acid, and an alkaline etching solution and an acidic solution can be used to remove the swirling plating of the first doped layer 13 and the first dielectric layer 11 on the front surface 01 and / or the side surface. After the above local patterning process, a first region 1 can be formed on the back side 02 of the silicon substrate 00, which retains the first dielectric layer 11, the first doped layer 13 and the first barrier layer 14.
[0051] Optional, continue to refer to Figure 2 The method for fabricating a solar cell further includes: sequentially forming a second dielectric layer 21 and a second doped layer 22 on the back side 02 of a silicon substrate 00, wherein the second doped layer 22 also has a second barrier layer 23; wherein the first doped layer 13 and the second doped layer 22 are insulated from each other, and the first barrier layer 14 and the second barrier layer 23 are insulated from each other; and removing the second barrier layer 23, the second doped layer 22 and the second dielectric layer 21 from the area outside the second region 2.
[0052] Specifically, after forming the first region 1, a second dielectric layer 21 can be formed on the back surface 02 of the silicon substrate 00, and then a second amorphous silicon layer can be formed on the side of the second dielectric layer 21 away from the silicon substrate 00. Due to the deposition process, the second dielectric layer 21 and the second amorphous silicon layer can simultaneously cover the first region 1 and other regions in the back surface 02 besides the first region 1.
[0053] Subsequently, atomic diffusion of a second conductivity type can be performed on the second amorphous silicon layer to transform it into a second doped layer 22, and a second barrier layer 23 can be formed on the surface of the second doped layer 22. The atoms of the second conductivity type have different conductivity types than those of the first conductivity type. For example, if the first conductivity type atom is boron, the second conductivity type atom can be phosphorus, the second doped layer 22 can be an N-type doped polycrystalline silicon layer, and the second barrier layer 23 can be a phosphosilicate glass (PSG) layer. After the atomic diffusion of the second conductivity type is completed, the second barrier layer 23, the second doped layer 22, and the second dielectric layer 21 in the first region 1 and the isolation region 3 can be removed accordingly, leaving only the second dielectric layer 21, the second doped layer 22, and the second barrier layer 23 in the preset positions of the second region 2. This removal process can be completed by a combination of laser film opening, wet etching, and acid washing, and can simultaneously remove the second barrier layer 23, the second doped layer 22, and the second dielectric layer 21 formed on the front side 01 and / or the side side of the silicon substrate 00.
[0054] Thus, the first dielectric layer 11 and the first doped layer 13 are retained in the first region 1, and the second dielectric layer 21 and the second doped layer 22 are retained in the second region 2. The first region 1 and the second region 2 are separated by an isolation region 3, so that the first doped layer 13 and the second doped layer 22 of different conductivity types are insulated from each other, avoiding short circuits or leakage between passivation contact areas of different conductivity types. This allows for the formation of alternating passivation contact structures of different conductivity types on the back side 02 of the silicon substrate 00.
[0055] In this embodiment, a first dielectric layer 11 and a first doped layer 13 are sequentially formed on the back surface 02 of a silicon substrate 00. The first doped layer 13 also has a first barrier layer 14. A first laser is used to remove the first barrier layer 14, the first doped layer 13, and the first dielectric layer 11 from the area outside the first region 1, thereby forming a first region 1 that retains the first dielectric layer 11, the first doped layer 13, and the first barrier layer 14. By matching the absorption band of the first barrier layer 14 with the wavelength of the first laser, the absorption efficiency of the first barrier layer 14 to the first laser is improved, and the thermal damage caused by laser-induced film opening and the thermal impact on non-opened areas are reduced, thereby improving the fabrication quality and electrical performance of the solar cell.
[0056] Optionally, after removing the first barrier layer 14 in a localized area of the back surface 02 using a first laser, the method further includes: performing a first push-junction treatment on the first doped layer 13 in an oxygen-free atmosphere; and performing a second push-junction treatment on the first doped layer 13 after the first push-junction treatment in an oxygen-containing atmosphere, so that the concentration range of the first conductivity type dopant element in the first doped layer 13 meets 6 × 10⁻⁶. 18 atoms / cm 3 -6×10 20 atoms / cm 3 .
[0057] Understandably, to match the absorption band of the first barrier layer 14 with different wavelengths of the first laser, different boron diffusion source flow rates, oxygen flow rates, boron diffusion temperatures, and boron diffusion durations can be used to give the first barrier layer 14 a corresponding boron doping concentration. Since both the first barrier layer 14 and the first doped layer 13 are formed during the boron diffusion process, different boron diffusion process parameters may also cause differences in the boron doping concentration and boron atom distribution in the first doped layer 13. Therefore, after removing the first barrier layer 14 in a local area of the back surface O2 using the first laser, the first doped layer 13 can be subjected to a first push-junction process and a second push-junction process in sequence to adjust the boron doping concentration and boron atom distribution in the first doped layer 13.
[0058] During the first bonding process, the first doped layer 13 can be subjected to high-temperature treatment in an oxygen-free atmosphere to further diffuse and redistribute boron atoms already present in the first doped layer 13, thereby reducing the concentration gradient of boron atoms along the thickness direction of the first doped layer 13. After completing the first bonding process, a second bonding process can be performed in an oxygen-containing atmosphere to further diffuse and activate boron atoms. By controlling the temperature, duration, and oxygen flow rate of the second bonding process, the boron doping concentration in the first doped layer 13 can be further adjusted. Thus, by adjusting the first preset doping concentration of the first blocking layer 14 according to the wavelength of the first laser, and by correspondingly adjusting the process conditions of the first and second bonding processes, it can be ensured that the boron doping concentration of the first doped layer 13 subsequently retained in the first region 1 reaches the preset doping concentration, thereby achieving both the laser-induced film opening effect and the consistency of the electrical properties of the first doped layer 13.
[0059] Understandably, since the 355nm purple laser and the 532nm green laser correspond to different boron doping concentrations in the first barrier layer 14, the boron diffusion source flux, oxygen flux, and boron diffusion duration used in forming the first barrier layer 14 will also differ. Correspondingly, different boron diffusion processes may also result in differences in the number of boron atoms entering the first doped layer 13, their activation level, and concentration distribution. To ensure that the concentration of the first conductivity type dopant element in the first doped layer 13 formed using different first preset process parameters reaches the preset doping concentration, different bonding conditions can be set for different wavelengths of the first laser.
[0060] For example, when the first laser is a purple laser, the boron diffusion source flux and oxygen flux used to form the first barrier layer 14 are relatively small, the boron diffusion duration is relatively short, and the initial diffusion and activation degree of boron atoms in the first doped layer 13 may also be relatively low. Therefore, the push-junction temperature of the first push-junction treatment can be controlled at 900℃-1000℃, for example, 950℃; the duration of the first push-junction treatment can be controlled at 5min-7min, for example, 6min, so that boron atoms can further diffuse into the interior of the first doped layer 13 and redistribute; then, a second push-junction treatment is performed in an oxygen-containing atmosphere for a duration of 20min-30min, for example, 25min, and the oxygen flux is controlled at 6500sccm-7000sccm, for example, 6000sccm, to further promote the diffusion and activation of boron atoms and adjust the boron doping concentration and its distribution state in the first doped layer 13. When the wavelength of the first laser is a green laser, in order to achieve a high boron doping concentration in the first barrier layer 14, the boron diffusion source flux and oxygen flux used in the boron diffusion process are relatively large, and the boron diffusion duration is relatively long. Therefore, the initial diffusion degree and doping degree of boron atoms in the first doped layer 13 are also relatively high. To avoid excessive diffusion of boron atoms due to excessively long subsequent push-junction time, the push-junction temperature of the first push-junction treatment can be controlled at 900℃-1000℃, for example, 950℃; the duration of the first push-junction treatment can be controlled at 3min-6min, for example, 4min; then, the duration of the second push-junction treatment can be controlled at 13min-23min, for example, 18min; and the oxygen flux can be controlled at 6500sccm-7000sccm, for example, 6000sccm, thereby completing the further diffusion, activation, and concentration distribution adjustment of boron atoms within a shorter push-junction time.
[0061] By setting corresponding push-junction processing conditions according to different first preset process parameters, it can be ensured that the final boron doping concentration of the first doped layer 13 remains within the preset doping concentration range. This balances the laser-opening effect of the first barrier layer 14 with the conductivity, passivation contact performance, and process consistency of the first doped layer 13. It can also be understood that when the boron doping concentration of the first doped layer 13 is below 6 × 10⁻⁶... 18 atoms / cm 3 When the boron doping concentration of the first doped layer 13 is higher than 6 × 10⁻⁶, the conductivity of the first doped layer 13 decreases and its lateral conductivity is insufficient, resulting in an increase in series resistance. 20 atoms / cm 3 In such cases, excessive defects or enhanced interfacial recombination may be introduced, which is detrimental to the quality of interfacial passivation. For example, the boron doping concentration C2 of the first doped layer 13 can be 6 × 10⁻⁶. 19 atoms / cm 3 .
[0062] Optionally, the first blocking layer 14 has a first refractive index corresponding to the first absorption band, or the first blocking layer 14 has a second refractive index corresponding to the second absorption band.
[0063] It is understandable that the boron doping concentration of the first barrier layer 14 affects its material composition and optical properties, causing the refractive index of the first barrier layer 14 at a corresponding wavelength to change with the boron doping concentration. Therefore, the correspondence between the boron doping concentration of the first barrier layer 14 and its refractive index at the wavelength of the first laser can be established experimentally in advance, and the first refractive index of the first barrier layer 14 corresponding to the first absorption band or the second refractive index of the first barrier layer 14 corresponding to the second absorption band can be obtained. Specifically, after the first barrier layer 14 is formed, a spectroscopic ellipsometer, a reflectance spectrometer, or other optical detection equipment can be used to obtain the refractive index of the first barrier layer 14 at the wavelength of the first laser. When the first refractive index meets the first refractive index corresponding to the first absorption band or the second refractive index corresponding to the second absorption band, it indicates that the boron doping concentration and optical properties of the first barrier layer 14 meet the requirements of the subsequent first laser film opening, and the first laser can continue to remove the first barrier layer 14 in the local area of the back surface 02; when the first refractive index does not meet the first refractive index corresponding to the first absorption band or the second refractive index corresponding to the second absorption band, the laser film opening can be paused, and the first preset process parameters can be adjusted.
[0064] Optionally, the refractive index of the first barrier layer is in the range of 1.51-1.6.
[0065] Specifically, when the first laser is a violet laser with a wavelength of 355 nm and the refractive index of the first blocking layer is in the range of 1.51-1.55, it indicates that the boron doping concentration of the first blocking layer 14 is within a preset range that matches the wavelength of the violet laser. When the first laser is a green laser with a wavelength of 532 nm and the refractive index of the first blocking layer is in the range of 1.56-1.60, it indicates that the boron doping concentration of the first blocking layer 14 is within a preset range that matches the wavelength of the green laser.
[0066] By detecting the refractive index of the first barrier layer 14 before laser delamination, a non-contact, non-destructive method is used to quickly determine whether the boron doping concentration and optical properties of the first barrier layer 14 meet preset requirements. By performing laser delamination only when the refractive index of the first barrier layer 14 meets the preset refractive index range, problems such as incomplete delamination, barrier layer residue, or excessive laser energy transfer to lower layers caused by deviations in the boron doping concentration of the first barrier layer 14 can be reduced, thereby further improving the consistency and stability of laser delamination.
[0067] Optional, continue to refer to Figure 2 The thickness of the first dielectric layer 11 is in the range of 1 nm to 2 nm. The thickness of the first doped layer 13 is in the range of 50 nm to 500 nm. The thickness of the first barrier layer 14 is in the range of 30 nm to 80 nm.
[0068] Specifically, the thickness of the first dielectric layer 11 is between 1 nm and 2 nm. This thickness range ensures, on the one hand, the selective permeability of the first dielectric layer 11 to charge carriers, thereby improving the open-circuit voltage and short-circuit current of the solar cell and thus enhancing its photoelectric conversion efficiency; on the other hand, it ensures that the first dielectric layer 11 has sufficient thickness to guarantee its continuity and density, thereby effectively reducing the interface defect density between the silicon substrate 00 and the first doped layer 13, and improving the performance and stability of the solar cell. For example, the thickness of the first dielectric layer 11 can be 1.5 nm.
[0069] The thickness of the first doped layer 13 is between 50 nm and 500 nm. This thickness range ensures that the first doped layer 13 has good lateral conductivity and carrier transport capability. If the thickness of the first doped layer 13 is too thin, its continuity and conductivity may be insufficient, which can easily lead to increased lateral transport resistance of carriers in the back contact region, thereby affecting the fill factor and conversion efficiency of the solar cell. If the thickness of the first doped layer 13 is too thick, it will increase the difficulty of subsequent local removal, patterning etching, and formation of the isolation region 3, affecting the structural accuracy of the first region 1 and the second region 2 of the back surface 02. For example, the thickness of the first doped layer 13 can be 300 nm.
[0070] The thickness of the first barrier layer 14 is between 30 nm and 80 nm. This thickness range ensures that the first barrier layer 14 has good continuity and mask protection capabilities, and can fully absorb the first laser of the corresponding wavelength. If the thickness of the first barrier layer 14 is too thin, it may have local discontinuities or insufficient blocking ability, and its absorption of the first laser is small, making it easy for some laser energy to pass through the first barrier layer 14 and act on the underlying first doped layer 13, first dielectric layer 11, and silicon substrate 00, thereby increasing the risk of laser thermal damage. If the thickness of the first barrier layer 14 is too thick, the energy or number of scans required for laser film opening may increase, which will reduce the film opening efficiency, expand the heat-affected zone, and increase the difficulty of subsequent removal of the first barrier layer 14. For example, the thickness of the first barrier layer 14 can be 60 nm.
[0071] In another alternative embodiment, Figure 3 This is a flowchart illustrating a method for preparing the second region in a solar cell according to an embodiment of the present invention. Figure 4 This is a process flow diagram of the fabrication process of the second region in a solar cell provided by an embodiment of the present invention, in conjunction with reference to [reference needed]. Figure 3 and Figure 4 As shown, the method for fabricating the second region in this solar cell includes: S201. A second dielectric layer and a second doped layer are sequentially formed on the back side of a silicon substrate, and a second barrier layer is also formed on the second doped layer.
[0072] The first doped layer 13 and the second doped layer 22 are insulated from each other, and the first barrier layer 14 and the second barrier layer 23 are insulated from each other.
[0073] Specifically, after forming the first region 1, a second dielectric layer 21 can be formed on the back surface 02 of the silicon substrate 00, and a second amorphous silicon layer 24 can be formed on the side of the second dielectric layer 21 away from the silicon substrate 00. The second dielectric layer 21 and the second amorphous silicon layer 24 can cover the first region 1 and other regions in the back surface 02 besides the first region 1.
[0074] The second dielectric layer 21 can be formed by thermal oxidation, chemical oxidation, or chemical vapor deposition, and may include a silicon oxide layer. The second dielectric layer 21 is used to passivate the interface of the silicon substrate 00 on which the second region 2 is subsequently formed, and allows corresponding types of charge carriers to tunnel through. The second amorphous silicon layer 24 can be formed using LPCVD or PECVD processes. The second amorphous silicon layer 24 is used to receive subsequently diffused atoms of the second conductivity type, and is transformed into a second doped layer 22 during atomic diffusion and high-temperature processing.
[0075] Subsequently, the second amorphous silicon layer 24 can undergo atomic diffusion treatment of a second conductivity type, allowing dopant atoms of the second conductivity type to enter the second amorphous silicon layer 24, and causing the second amorphous silicon layer 24 to crystallize under high temperature, thereby forming the second doped layer 22. At the same time, during the atomic diffusion process of the second conductivity type, a second barrier layer 23 can be formed on the side of the second doped layer 22 away from the silicon substrate 00.
[0076] The second type of conductive atom can be phosphorus atom. For example, phosphine, phosphorus oxychloride, or other phosphorus-containing diffusion sources can be used to perform phosphorus diffusion treatment on the second amorphous silicon layer 24, allowing phosphorus atoms to diffuse into the second amorphous silicon layer 24, thereby forming an N-type second doped layer 22. Simultaneously, the phosphorus-containing material reacts with components such as silicon oxide to form a PSG layer on the surface of the second doped layer 22. The PSG layer can serve as a second barrier layer 23. The second barrier layer 23 is used to protect the second doped layer 22 and the second dielectric layer 21 in the second region 2 during subsequent local etching processes.
[0077] It should be noted that the second amorphous silicon layer 24 can be subjected to atomic diffusion of a second conductivity type using second preset process parameters, so that the second barrier layer 23 reaches a corresponding preset doping concentration, and the wavelength of the second laser used to remove the second barrier layer 23 is located within the absorption band of the second barrier layer 23. The second preset process parameters may include at least one of the diffusion source flux of the second conductivity type atoms, oxygen flux, diffusion temperature, and diffusion duration. By matching the doping concentration of the second barrier layer 23 with the wavelength of the second laser, the absorption efficiency of the second barrier layer 23 for the second laser can be improved, allowing the laser energy to be more concentrated on the second barrier layer 23, improving the local opening effect of the second barrier layer 23, and reducing the energy transferred by the second laser to the second doped layer 22, the second dielectric layer 21, and the silicon substrate 00 below the second barrier layer 23, thereby reducing the thermal damage caused by laser opening. The second preset process parameters, the preset doping concentration of the second barrier layer 23, and the wavelength of the second laser can be set according to actual process needs, and the present invention does not impose specific limitations on them.
[0078] S202, Remove the second barrier layer, the second doped layer, and the second dielectric layer from the regions outside the second region.
[0079] Specifically, after the formation of the second doped layer 22 and the second barrier layer 23 is completed, since the second barrier layer 23, the second doped layer 22 and the second dielectric layer 21 simultaneously cover the first region 1 and other regions in the back surface 02 except for the first region 1, it is necessary to remove the second barrier layer 23, the second doped layer 22 and the second dielectric layer 21 in the regions other than the second region 2 to expose the original first barrier layer 14 in the first region 1, and retain the second barrier layer 23, the second doped layer 22 and the second dielectric layer 21 in a preset region of the back surface 02, thereby forming the second region 2.
[0080] For example, a second laser can be used to remove the second barrier layer 23 in a localized area of the back side 02. The second laser can scan according to a preset pattern of the first region 1 and the isolation region 3 to remove the second barrier layer 23 covering the preset area of the first region 1 and the isolation region 3, exposing the second doped layer 22 in the corresponding area. Afterwards, a single-sided wet etching method can be used to remove the second barrier layer 23 of the front side 01. For example, a single-sided chain device can be used to apply an etching solution containing hydrofluoric acid to the front side 01 of the silicon substrate 00 to remove the PSG layer formed on the front side 01 during atomic diffusion.
[0081] After removing the second barrier layer 23 in the first region 1 and the second barrier layer 23 on the front side 01, an alkaline polishing tank can be used to remove the second doped layer 22 in the preset areas of the first region 1 and the isolation region 3 using sodium hydroxide solution or potassium hydroxide solution, and to remove the second doped layer 22 deposited around the front side 01 and the side. At this time, the second barrier layer 23 on the surface of the second region 2 acts as an etching mask, which can prevent the alkaline solution from contacting the second doped layer 22 in the second region 2, thereby protecting the film structure of the second region 2. After removing the second doped layer 22 in the corresponding areas, the exposed second dielectric layer 21 can be removed by acid washing or acid etching process. For example, an acidic solution containing hydrofluoric acid can be used to remove the second dielectric layer 21 in the preset areas of the first region 1 and the isolation region 3. Since the original first barrier layer 14 in the first region 1 is located below the second dielectric layer 21, after removing the second dielectric layer 21 covering the first region 1, the first barrier layer 14 in the first region 1 can be exposed, while the first doped layer 13 and the first dielectric layer 11 below the first barrier layer 14 are retained.
[0082] After the aforementioned laser film opening, wet etching, alkaline polishing, and acid washing processes, the second dielectric layer 21, the second doped layer 22, and the second barrier layer 23, which are sequentially stacked, can be retained in the second region 2, forming an isolation region 3 between the first region 1 and the second region 2. The isolation region 3 is used to isolate the first doped layer 13 and the second doped layer 22 from each other, preventing direct contact between doped polysilicon layers of different conductivity types, which could cause short circuits or leakage.
[0083] It is also understandable that after removing the second dielectric layer 21, the second doped layer 22, and the second barrier layer 23 from the surface of the silicon substrate 00 (excluding the second region 2), the isolation region 3 and the front side 01 of the silicon substrate 00 can be exposed. By further polishing the silicon substrate 00 with an alkaline solution, the isolation region 3 and the front side 01 of the silicon substrate 00 can be etched, thereby forming a tower base again in the isolation region 3 and the front side 01 of the silicon substrate 00, ensuring that the surface of the silicon substrate 00 has a large light-receiving area. At the same time, polishing the surface of the silicon substrate 00 can remove impurities from the surface of the silicon substrate 00, thereby ensuring the cleanliness of the surface of the silicon substrate 00 and improving the yield of the film layer formed in subsequent processes.
[0084] Furthermore, before completing the solar cell fabrication process, it is necessary to remove the second barrier layer 14 of the first region 1 and the second barrier layer 23 of the second region 2 to prevent the presence of the BSG and PSG layers from affecting the conversion efficiency of the solar cell, while providing a good foundation for subsequent processes. The methods for removing the BSG and PSG layers can include, but are not limited to, laser removal or wet removal. For example, hydrofluoric acid etching can be used to remove the BSG layer of the first region 1 and the PSG layer of the second region 2.
[0085] Optionally, the method for fabricating a solar cell further includes: forming a passivation layer and an antireflection layer covering the first region 1, the second region 2, the isolation region 3 and the front side 01; forming a first electrode in contact with the first doped layer 13 and a second electrode in contact with the second doped layer 22.
[0086] For example, aluminum oxide can be deposited on the surface of the first region 1, the second region 2, the isolation region 3 and the front surface 01 by atomic layer deposition (ALD) to form a passivation layer, and an anti-reflection layer can be formed on the side of the passivation layer away from the silicon substrate 00 by PECVD. The anti-reflection layer may include one or more stacked structures of silicon nitride, silicon oxynitride and silicon oxide.
[0087] Specifically, the first electrode and the second electrode may include silver electrodes, etc. Silver paste can be printed onto the side surface of the first doped layer 13 and the second doped layer 22 away from the silicon substrate 00 by screen printing. Then, the silver paste in the first region 1 and the second region 2 is sintered by laser sintering technology to form the first electrode in contact with the first doped layer 13 and the second electrode in contact with the second doped layer 22, respectively, thereby forming a passivated contact structure.
[0088] Optionally, a main grid electrode on the back side O2 may be formed simultaneously with the formation of the first and second electrodes. The first and second electrodes can be electrically connected to external devices or other solar cells via the main grid electrode. The formation method of the main grid electrode can be similar to that of the formation method of the first and second electrodes, that is, the main grid electrode, the first electrode, and the second electrode can be fabricated under the same process. The specific implementation method can be designed according to actual needs, and the embodiments of the present invention do not specifically limit this.
[0089] In addition, after the solar cells are fabricated, their electrical performance needs to be tested, such as their open-circuit voltage, maximum output power, and conversion efficiency, in order to sort and store them.
[0090] Based on the same inventive concept, this invention also provides a solar cell, which is prepared by the solar cell preparation method of this invention. Figure 5 This is a schematic diagram of the structure of a solar cell provided in an embodiment of the present invention, as shown below. Figure 5 As shown, the solar cell includes a silicon substrate 00, which includes a front side 01 and a back side 02. The back side 02 includes a first region 1, a second region 2, and an isolation region 3 located between the first region 1 and the second region 2. The first region 1 includes a first dielectric layer 11 and a second doped layer 13. The second region 2 includes a second dielectric layer 21 and a second doped layer 22. There is also a passivation layer 4, an antireflection layer 5, a first electrode 6, and a second electrode 7.
[0091] The aforementioned solar cells can be prepared by the solar cell preparation method provided in any embodiment of the present invention, and possess the corresponding functions and beneficial effects of the solar cell preparation method. Technical details not described in detail in this embodiment can be found in the solar cell preparation method provided in any embodiment of the present invention.
[0092] Since the solar cells described above can be prepared by the solar cell preparation methods provided in any embodiment of the present invention, those skilled in the art can understand the specific implementation methods and various variations of the solar cells in this embodiment based on the solar cell preparation methods described in the embodiments of the present invention. Therefore, how the solar cell preparation methods in the embodiments of the present invention are implemented to prepare the solar cells will not be described in detail here. Any solar cells prepared by those skilled in the art using the solar cell preparation methods in the embodiments of the present invention fall within the scope of protection of this application.
[0093] It should be understood that the various forms of processes shown above can be used to reorder, add, or delete steps. For example, the steps described in this invention can be executed in parallel, sequentially, or in different orders, as long as the desired result of the technical solution disclosed in this invention can be achieved, and this is not limited herein.
[0094] The specific embodiments described above do not constitute a limitation on the scope of protection of this invention. Those skilled in the art should understand that various modifications, combinations, sub-combinations, and substitutions can be made according to design requirements and other factors. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this invention should be included within the scope of protection of this invention.
Claims
1. A method for preparing a solar cell, characterized in that, include: A silicon substrate is provided; the silicon substrate includes a front side and a back side opposite to each other, the back side including a first region and a second region arranged at intervals, and an isolation region between the first region and the second region; A first dielectric layer and a first doped layer are sequentially formed on the back side of the silicon substrate, and a first barrier layer is also provided on the first doped layer; A first laser is used to remove the first blocking layer, the first doped layer, and the first dielectric layer outside the first region; wherein the wavelength of the first laser is located within the absorption band of the first blocking layer.
2. The method for preparing a solar cell according to claim 1, characterized in that, The first laser is either a green-skinned laser or a purple-skinned laser; The first blocking layer has a first absorption band corresponding to the wavelength of the green laser, or the first blocking layer has a second absorption band corresponding to the wavelength of the purple laser.
3. The method for preparing a solar cell according to claim 2, characterized in that, The first blocking layer has a first refractive index corresponding to the first absorption band, or the first blocking layer has a second refractive index corresponding to the second absorption band.
4. The method for preparing a solar cell according to claim 1, characterized in that, The refractive index of the first barrier layer is in the range of 1.51-1.
6.
5. The method for preparing a solar cell according to claim 2, characterized in that, The first doped layer and the first barrier layer have doping elements of a first conductivity type; The first barrier layer is formed on the back side of the silicon substrate, comprising: The absorption band of the first barrier layer can be adjusted by controlling the concentration of doping elements of the first conductivity type in the first barrier layer.
6. The method for preparing a solar cell according to claim 5, characterized in that, The silicon substrate contains doping elements of a second conductivity type; The second conductivity type dopant has the opposite conductivity type to the first conductivity type dopant.
7. The method for preparing a solar cell according to claim 6, characterized in that, The first conductivity type doping element is a group IIIA element, and the second conductivity type doping element is a group VA element.
8. The method for preparing a solar cell according to claim 7, characterized in that, The concentration range of the first conductivity type dopant element in the first barrier layer satisfies 1×10 20 atoms / cm 3 -5×10 20 atoms / cm 3 So that the first barrier layer has the first absorption band, or, the concentration range of the first conductivity type dopant element in the first barrier layer satisfies 1×10 21 atoms / cm 3 -1×10 22 atoms / cm 3 This is to give the first blocking layer the second absorption band.
9. The method for preparing a solar cell according to claim 5, characterized in that, The concentration range of the first conductivity type dopant element in the first doped layer satisfies 6 × 10⁻⁶. 18 atoms / cm 3 -6×10 20 atoms / cm 3 .
10. The method for preparing a solar cell according to claim 1, characterized in that, The thickness of the first dielectric layer is in the range of 1nm-2nm.
11. The method for preparing a solar cell according to claim 1, characterized in that, The thickness of the first doped layer is in the range of 50nm-500nm.
12. The method for preparing a solar cell according to claim 1, characterized in that, The thickness of the first barrier layer is in the range of 30nm-80nm.
13. The method for preparing a solar cell according to claim 1, characterized in that, Also includes: A second dielectric layer and a second doped layer are sequentially formed on the back side of the silicon substrate, and a second barrier layer is further provided on the second doped layer; wherein the first doped layer and the second doped layer are insulated from each other, and the first barrier layer and the second barrier layer are insulated from each other. Remove the second barrier layer, the second doped layer, and the second dielectric layer from the regions outside the second region.
14. The method for preparing a solar cell according to claim 13, characterized in that, Also includes: A passivation layer and an anti-reflection layer are formed covering the first area, the second area, the isolation area, and the front side; A first electrode is formed that contacts the first doped layer, and a second electrode is formed that contacts the second doped layer.
15. A solar cell, characterized in that, The solar cell is prepared by the method for preparing a solar cell as described in any one of claims 1-14.