A method for laser-synchronized aluminum-doped edge field passivation of solar cells
By simultaneously supplying an aluminum-containing precursor during laser cutting, the aluminum diffuses into the cutting edge using the laser thermal field, forming an aluminum-doped region. This solves the problem of damage to the cutting edge during the slab preparation of crystalline silicon solar cells, improves cell performance, and simplifies the process.
Patent Information
- Application Number
- CN202611310915.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-17
AI Technical Summary
In the laser slicing process of crystalline silicon solar cells, existing technologies suffer from lattice damage, dangling bonds, and microcracks at the cutting edges, leading to carrier recombination and leakage. Furthermore, existing passivation methods involve high equipment investment, high energy consumption, and uneven or incomplete passivation film coverage.
A pulsed laser is used to synchronously supply aluminum-containing precursors. The instantaneous thermal field generated by laser cutting causes the aluminum precursors to decompose and diffuse into the cutting edge, forming an aluminum doped region along the cutting edge. This constructs a stable and continuous edge-doped structure and reduces the carrier recombination rate.
It reduces the recombination speed at the cutting edge, improves the open-circuit voltage, fill factor, and photoelectric conversion efficiency of solar cells, simplifies the process, and reduces equipment and energy costs.
Smart Images

Figure CN123124489A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solar cell technology, and in particular to a method for laser-synchronized aluminum-doped edge field passivation of solar cells. Background Technology
[0002] As photovoltaic modules develop towards higher power, lower loss, and higher reliability, crystalline silicon solar cells are typically processed into half-cells or multiple slabs using laser slicing to reduce current transmission losses and module series resistance. However, the instantaneous high temperature, thermal stress, and material ablation generated by laser cutting can create lattice damage, dangling bonds, microcracks, and local defect states at the cutting edges. This makes the cutting edges a high-risk area for carrier recombination and leakage, thus affecting the open-circuit voltage, fill factor, and photoelectric conversion efficiency of the solar cell. Existing technologies typically deposit alumina, silicon oxide, or silicon nitride passivation films at the cutting edges using methods such as ALD or PECVD after laser cutting, followed by annealing to improve the passivation effect. However, these methods require additional processes such as post-cutting transfer, thin film deposition, and annealing, resulting in high equipment investment and energy consumption. They may also lead to problems such as passivation film wrapping around the electrode or junction isolation area, uneven film thickness, and incomplete edge coverage.
[0003] To simplify the edge passivation process, existing technologies propose first forming a pre-cut groove using a laser, then depositing aluminum-containing coating powder into the groove, and finally using a second laser to melt the aluminum-containing coating powder, forming an aluminum-containing edge coating on the groove wall surface to achieve edge coverage and a certain degree of field passivation. However, this method still requires sequential steps such as pre-cutting, aluminum-containing material deposition, secondary laser melting, and physical separation. The external coating formed after the aluminum-containing powder melts may still have uneven thickness, porosity, cracks, or residual contamination, and multiple laser treatments can easily expand the heat-affected zone of the cut edge. Therefore, how to reduce independent thin film deposition and repeated laser treatments, introduce doping elements in a timely manner during the formation of the cut edge, and construct a stable and continuous edge doping structure within the silicon material has become a technical problem that needs to be solved in the tiling and edge passivation process of crystalline silicon solar cells. Summary of the Invention
[0004] This application provides a method for laser-synchronized aluminum-doped edge field passivation of solar cells, including the following steps:
[0005] S1. Provide a complete crystalline silicon solar cell wafer, and define a laser-cut area on the complete crystalline silicon solar cell wafer;
[0006] S2. Aluminum-containing precursor is supplied directionally to the laser cutting area so that the aluminum-containing precursor covers the laser cutting area;
[0007] S3. Under the condition of continuous supply of the aluminum-containing precursor, the entire crystalline silicon solar cell is sliced along the laser cutting area using a pulsed laser, so that the area of action of the pulsed laser at least partially overlaps with the area covered by the aluminum-containing precursor; the instantaneous thermal field generated by the laser cutting is used to decompose the aluminum-containing precursor, and the aluminum atoms released by the aluminum-containing precursor diffuse into the cutting edge formed by the laser cutting, forming an aluminum doped region extending along the cutting edge inside the silicon material at the cutting edge;
[0008] S4. Stop supplying the aluminum-containing precursor and cool the laser-cut and aluminum-doped sectional cells to obtain a sectional solar cell with an aluminum-doped edge field passivation structure.
[0009] It should be noted that the aluminum-containing precursor is directionally and continuously supplied to the laser cutting area, covering the corresponding cutting position before the pulsed laser arrives. During the pulsed laser's action, a localized high-temperature and transient molten layer forms in the cutting area within a very short time. The aluminum-containing precursor decomposes thermally, releasing aluminum-containing active species. Aluminum, under the combined influence of the concentration gradient, molten silicon mass transfer, and the diffusion channels of cutting defects, enters the newly formed cutting edge. Because the diffusion rate of aluminum in silicon is significantly increased in the molten state, subsequent rapid cooling and solidification cause some aluminum to remain in the silicon lattice in a substitutional form, forming an aluminum-doped region extending along the cutting edge. Aluminum, acting as an acceptor impurity in silicon, causes the cutting edge to form a localized p-type or p-type... + The laser creates a morphological region and induces band bending and space charge regions between it and the adjacent silicon material, thereby forming an edge-built-in electric field. This reduces the minority carrier concentration near the high-defect cut surface and inhibits the migration of carriers to recombination centers such as dangling bonds, lattice distortions, and microcracks, thus reducing the recombination rate at the cut edge. At the same time, the pulsed laser has a short thermal action time and a concentrated action range, which can reduce thermal damage to the main junction region of the battery and the original passivation structure while completing the slab cutting and aluminum doping. This achieves field-effect passivation without the need for independent diffusion annealing and edge passivation film deposition.
[0010] Preferably, the aluminum precursor in the aluminum-containing precursor is selected from at least one of trimethylaluminum, aluminum chloride, aluminum nitrate and aluminum isopropoxide.
[0011] It should be noted that trimethylaluminum, aluminum chloride, aluminum nitrate, and aluminum isopropoxide are all used as precursors to provide aluminum to the laser-cut area, but this does not mean that they retain their original chemical form at the final cut edge. Among them, trimethylaluminum has high volatility and is suitable for supplying it in the form of precursor vapor carried by a carrier gas in a closed inert atmosphere; aluminum chloride can be supplied using precursor vapor or aerosol formed by solution atomization; aluminum nitrate and aluminum isopropoxide are suitable for supplying them in the form of aerosol or micro-spray after being prepared into precursor solutions. During pulsed laser treatment, the above precursors undergo volatilization, thermal decomposition, and interfacial reactions at instantaneous high temperature to form aluminum-containing active species. At least some of the aluminum enters the transient molten silicon layer formed by laser treatment and remains inside the silicon material at the cut edge during rapid cooling; the aluminum that does not enter the silicon material may exist on the cut surface in the form of aluminum oxide, chloride, or other decomposition residues, which can be removed after cooling. Therefore, the main function of the aluminum-containing precursor described in this application is to provide the aluminum source required for laser doping, and the purpose is not to deposit a continuous aluminum oxide passivation film on the cutting edge; different aluminum precursors can be used individually or in combination according to volatility, decomposition temperature and aluminum supply rate.
[0012] Preferably, the aluminum-containing precursor is supplied to the laser-cutting area in the form of aerosol, micro-spray, or precursor vapor.
[0013] It should be noted that the supply method of the aluminum-containing precursor can be selected based on the volatility, solubility, and thermal decomposition characteristics of the precursor. For volatile trimethylaluminum or aluminum chloride, an inert carrier gas can be used to carry the precursor vapor and deliver it through a directional nozzle; for aluminum chloride, aluminum nitrate, or aluminum isopropoxide dissolved in solvents such as alcohols, aerosols or micro-droplets can be formed through ultrasonic atomization, pneumatic atomization, or micro-spraying. All of the above supply methods allow the aluminum source to be locally concentrated in the laser-cut area, avoiding the need for aluminum-containing material coating on the entire battery surface, and ensuring that the aluminum-containing precursor can promptly contact the newly formed cut surface during laser operation.
[0014] Preferably, the aluminum-containing precursor is supplied in the form of an aerosol, wherein the concentration of the aluminum precursor in the aerosol is 0.1–1 mol / L, the particle size of the aerosol droplets is 50–200 nm, the supply flow rate is 5–20 L / min, and the angle between the aerosol spraying direction and the laser cutting line is 30°–60°.
[0015] It should be noted that the concentration of aluminum precursor in the aerosol refers to the molar concentration of aluminum precursor in the aluminum-containing precursor solution used for atomization. When the concentration is below 0.1 mol / L, the aluminum source delivered to the laser cutting area per unit time may be insufficient, making it difficult to form a continuous and uniform aluminum-doped region. When the concentration is above 1 mol / L, problems such as difficulty in atomization, droplet coalescence, nozzle crystallization blockage, and increased residue on the cutting surface are likely to occur. A droplet size of 50–200 nm is beneficial for the stable delivery of droplets with the carrier gas and their uniform spread in the laser action area. A supply flow rate of 5–20 L / min can balance the precursor supply and the stability of the laser optical path. An angle of 30°–60° between the jet direction and the laser cutting line allows the aerosol to enter the cutting position before the laser arrives, while reducing the interference of the jet gas flow on the discharge of molten material and the propagation of the laser beam. The angle can be determined according to the angle between the projection direction of the nozzle central axis on the battery surface and the extension direction of the laser cutting line.
[0016] Preferably, in step S2, the supply of the aluminum-containing precursor begins before the pulsed laser reaches the corresponding laser cutting position and continues during the process of the pulsed laser acting on the corresponding laser cutting position, and the supply path of the aluminum-containing precursor moves synchronously with the scanning path of the pulsed laser.
[0017] It should be noted that the aluminum-containing precursor is supplied before the pulsed laser reaches the corresponding cutting position to ensure that the position has sufficient aluminum source coverage before the laser action. Continuous supply during the pulsed laser action replenishes the precursor consumed by volatilization, decomposition, splashing, or removal by the carrier gas, ensuring that the newly formed cut sidewall remains in contact with the aluminum-containing active species. The supply path moves synchronously with the laser scanning path, which can be achieved by fixing the nozzle and laser head to the same motion mechanism, or by separately controlling the movement of the nozzle, laser head, and support platform, as long as they maintain a predetermined relative position and speed during the cutting process. This dynamic synchronous supply, unlike pre-coating and drying to form a solid aluminum-containing layer, improves the uniformity of aluminum supply and doping distribution along the cutting edge.
[0018] Preferably, the pulsed laser is an infrared nanosecond laser or an infrared picosecond laser, and the pulse width of the pulsed laser is 10 ps to 100 ns, with a power density of 1 × 10⁻⁶. 6 ~5×10 6 W / cm 2 .
[0019] It should be noted that both infrared nanosecond lasers and infrared picosecond lasers can be absorbed by crystalline silicon materials, forming a highly concentrated transient thermal field in the cutting area. Picosecond lasers have a shorter pulse duration and a smaller thermal diffusion range, which helps reduce the heat-affected zone and microcracks at the cutting edge; nanosecond lasers have a higher single-pulse heat input, which is beneficial for forming a transient molten layer sufficient to promote precursor decomposition and aluminum diffusion. The power density refers to the effective power density of the laser on the battery surface or in the focal area; below 1×10⁻⁶. 6 W / cm 2 At times, it may not be possible to simultaneously meet the energy requirements for slicing, precursor decomposition, and aluminum diffusion, exceeding 5 × 10⁻⁶. 6 W / cm 2 If this is not done properly, it can easily cause excessive ablation of the cutting edge, molten spatter, edge chipping, and thermal damage to the adjacent passivation layer or electrode structure. Therefore, the pulse width and power density should be adjusted in conjunction with the laser wavelength, spot size, scanning speed, and battery thickness.
[0020] Preferably, the focal point of the pulsed laser is located on the surface of the entire crystalline silicon solar cell, or 5 to 20 μm below the surface of the entire crystalline silicon solar cell.
[0021] It should be noted that focusing the pulsed laser on the entire surface of the crystalline silicon solar cell allows the laser energy to be directly concentrated on the predetermined cutting area, suitable for initial surface cutting and slicing of thinner cells. Focusing the laser at a depth of 5–20 μm below the cell surface allows for higher energy density applied to the shallow interior of the silicon material, which is beneficial for forming a stable local thermal field and transient melting zone, and reduces sputtering and edge chipping caused by excessive surface energy concentration. When the focal depth is less than 5 μm, the effect is similar to surface focusing; when the focal depth is greater than 20 μm, it may reduce the energy coupling efficiency between the laser and the aluminum-containing precursor on the cutting surface, hindering the complete decomposition of the precursor and the diffusion of aluminum to the newly cut sidewalls. The actual focal position can be adjusted according to the cell thickness, laser pulse width, and cutting method.
[0022] Preferably, the aluminum-doped region is distributed in a continuous strip, continuous arc, or segmented continuous shape along the cutting edge formed by laser cutting; in step S4, the laser-cut and aluminum-doped slab cells are cooled in an inert atmosphere or an air atmosphere, and after cooling, the cutting edge is no longer subjected to passivation film deposition or independent thermal annealing treatment.
[0023] It should be noted that the distribution pattern of the aluminum-doped regions corresponds to the laser scanning trajectory and the edge structure of the battery: when the laser cuts along a straight line, the aluminum-doped regions can be distributed in a continuous strip shape; when the laser cuts along a curved or irregular path, they can be distributed in a continuous arc shape; when it is necessary to avoid electrodes, busbar areas, or local functional structures, they can be distributed in a segmented continuous shape. After cutting, the aluminum-doped regions can be cooled in an inert atmosphere such as nitrogen or argon to reduce oxidation of the high-temperature cutting edges and aluminum-containing species. They can also be cooled in air to simplify the process, but air cooling may form a natural oxide layer or a small amount of aluminum-containing oxide on the cutting surface. The statement that no passivation film deposition or independent thermal annealing is performed after cooling means that no subsequent deposition steps are set for the purpose of forming edge alumina films, silicon oxide films, or other passivation films, nor are annealing steps specifically used for aluminum diffusion or passivation activation. The oxide layer naturally formed on the cutting surface or the small amount of aluminum-containing oxide generated by the decomposition of precursors are not considered as additional passivation film deposition processes.
[0024] This application utilizes a pulsed laser slicing process to continuously and directionally supply an aluminum-containing precursor to the laser-cutting area. The instantaneous thermal field generated by the laser simultaneously completes precursor decomposition, aluminum atom diffusion, and edge modification, allowing aluminum to penetrate the newly formed silicon material at the slicing edge and form an aluminum-doped region extending along the edge. This generates local bandgap bending and a built-in electric field, reducing carrier concentration near high-defect slicing surfaces and suppressing carrier migration to recombination centers such as dangling bonds, lattice distortions, and microcracks. This reduces the recombination rate at the slicing edge, minimizing losses in open-circuit voltage, fill factor, and conversion efficiency caused by slicing. Simultaneously, the aluminum-containing precursor supply path moves synchronously with the laser scanning path, improving the continuity and uniformity of aluminum supply and doping distribution along the slicing edge. Furthermore, local melting and rapid resolidification can improve the edge morphology. This method eliminates the need for pre-depositing a solid aluminum layer and post-cutting passivation film deposition or independent thermal annealing, shortening the process flow, reducing equipment and energy costs, and is applicable to various types of crystalline silicon solar cells, including TOPCon, PERC, HJT, and back-contact types. Attached Figure Description
[0025] Figure 1 The image shows a cross-sectional scanning electron microscope image and elemental distribution map of the cut edge of the TOPCon half-cell solar cell prepared in Example 1.
[0026] Figure 2 The image shows a scanning electron microscope image of the laser-cut edge of the TOPCon half-cell solar cell obtained in Comparative Example 1 without aluminum doping and passivation.
[0027] Figure 3 The image shows a scanning electron microscope (SEM) image of the cut edge of the TOPCon half-cell solar cell obtained in Example 1 after laser-synchronized aluminum doping field passivation. Detailed Implementation
[0028] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the examples in the specification.
[0029] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0030] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.
[0031] Example 1
[0032] This embodiment provides a laser-synchronized aluminum-doped edge field passivation method for n-type TOPCon solar cells, including the following steps:
[0033] S1. A complete n-type TOPCon crystalline silicon solar cell wafer with a size of 210 mm and a thickness of 150 μm is provided, wherein the crystalline silicon solar cell wafer has undergone junction fabrication, surface passivation, and electrode fabrication. A straight laser-cut area is defined in the middle of the crystalline silicon solar cell wafer to divide the crystalline silicon solar cell wafer into two halves.
[0034] S2. Dissolve aluminum chloride in anhydrous ethanol to prepare an aluminum precursor solution with a concentration of 0.5 mol / L. Use an ultrasonic atomization device to prepare an aerosol with an average droplet size of 100 nm from the aluminum precursor solution. Use nitrogen as the carrier gas and directionally supply the aerosol to the laser cutting area at a flow rate of 10 L / min. The angle between the aerosol spray direction and the laser cutting line is 45°.
[0035] The aerosol nozzle is positioned in front of the laser scanning direction. The aerosol nozzle moves synchronously with the laser head, so that the aluminum-containing precursor covers the cutting position before the pulsed laser reaches the corresponding cutting position, and is continuously supplied during the process of the pulsed laser acting on the cutting position.
[0036] S3. The infrared picosecond laser is used to perform segmented cutting along the laser cutting area. The infrared picosecond laser has a wavelength of 1064 nm, a pulse width of 50 ps, and a power density of 2 × 10⁻⁶. 6 W / cm 2The laser focus is located 10 μm below the surface of the entire crystalline silicon solar cell.
[0037] When a pulsed laser acts on the laser-cut area, the instantaneous thermal field generated by the laser cutting causes aluminum chloride to decompose. The released aluminum atoms diffuse into the newly formed cutting edge, forming a strip-shaped aluminum doped region that extends continuously along the cutting edge inside the silicon material of the cutting edge.
[0038] S4. After laser cutting, the supply of aluminum-containing precursor is stopped, and nitrogen gas is continuously introduced to cool the resulting half-cell to room temperature. Anhydrous ethanol is used to remove unreacted precursor residues from the cutting edges. No passivation film deposition or independent thermal annealing treatment is performed on the cutting edges to obtain a TOPCon half-cell solar cell with an aluminum-doped edge field passivation structure.
[0039] Example 2
[0040] This embodiment provides a laser-synchronized aluminum-doped edge field passivation method for p-type PERC solar cells, including the following steps:
[0041] S1. Provide a p-type PERC crystalline silicon solar cell with a size of 182 mm and a thickness of 160 μm, and determine a straight laser-cut area in the middle of the crystalline silicon solar cell.
[0042] S2. Prepare an aluminum precursor solution with a concentration of 0.1 mol / L using aluminum nitrate, and load it into a micro-spray device. Orient the nozzle of the micro-spray device towards the laser cutting area, with the spray direction at a 30° angle to the laser cutting line. Activate the micro-spray device before the pulsed laser reaches the corresponding cutting position, and move the nozzle synchronously with the laser head to form a continuous aluminum precursor coverage band in the laser cutting area.
[0043] S3. A 1064nm infrared nanosecond laser is used to perform slicing along the laser cutting area. The laser pulse width is 100ns and the power density is 1×10⁻⁶. 6 W / cm 2 The laser focus is located on the entire surface of the crystalline silicon solar cell.
[0044] During laser cutting, aluminum nitrate decomposes under the instantaneous thermal field of the laser, and the released aluminum atoms diffuse into the silicon material at the cutting edge, forming an aluminum-doped region that extends continuously along the cutting edge.
[0045] S4. After laser cutting is completed, stop supplying aluminum-containing precursors, allow the resulting PERC half-cell solar cells to cool to room temperature in air, and remove precursor residues from the cut edges without performing passivation film deposition or independent thermal annealing.
[0046] Example 3
[0047] This embodiment provides a laser-synchronized aluminum-doped edge field passivation method for n-type HJT solar cells, including the following steps:
[0048] S1. Provide an n-type HJT crystalline silicon solar cell with a size of 210mm and a thickness of 130μm, and define two parallel laser cutting areas on the crystalline silicon solar cell to divide the crystalline silicon solar cell into three segments.
[0049] S2. Add aluminum isopropoxide to anhydrous isopropanol to prepare an aluminum precursor solution with a concentration of 1 mol / L. Atomize the aluminum precursor solution into an aerosol with an average droplet size of 200 nm, using nitrogen as the carrier gas, and supply it to the laser cutting area at a flow rate of 20 L / min. The angle between the aerosol spray direction and the laser cutting line is 60°.
[0050] The aerosol nozzle is positioned on the laser head and moves synchronously with the laser head, ensuring that the aerosol supply path coincides with the pulsed laser scanning path.
[0051] S3. Using a 1064nm infrared picosecond laser, the laser is sequentially cut along two laser cutting regions, with a laser pulse width of 10ps and a power density of 5×10⁻⁶. 6 W / cm 2 The laser focus is located 20 μm below the entire surface of the crystalline silicon solar cell.
[0052] During laser cutting, aluminum isopropoxide decomposes under the action of a transient thermal field, and the released aluminum atoms diffuse into the silicon material of the two cutting edges, forming continuous strip-shaped aluminum doped regions at each cutting edge.
[0053] S4. After laser cutting is completed, the supply of aerosol is stopped, and the resulting HJT slab solar cells are cooled to room temperature in a nitrogen atmosphere. The residue on the cutting edge is removed, and no subsequent passivation film deposition or independent thermal annealing is performed.
[0054] Example 4
[0055] This embodiment provides a laser-synchronized aluminum-doped edge field passivation method for n-type back-contact solar cells, including the following steps:
[0056] S1. Provide an n-type TBC back-contact solar cell with a size of 230 mm and a thickness of 150 μm, wherein the back side of the solar cell has alternately arranged P-type regions, N-type regions, and corresponding electrodes. A laser-cut area is determined at a position avoiding the main electrode busbar area on the back side.
[0057] S2. The entire crystalline silicon solar cell is placed in an inert atmosphere processing chamber with a localized extraction structure, and nitrogen gas is introduced into the processing chamber. The nitrogen gas carries the trimethylaluminum precursor vapor and is delivered to the laser cutting area through a directional nozzle.
[0058] The directional nozzle for the precursor vapor is positioned in front of the laser scanning direction and moves synchronously with the laser head, so that the trimethylaluminum precursor vapor covers the cutting position before the laser reaches the corresponding cutting position and is continuously supplied during the laser cutting process.
[0059] S3. A 1064nm infrared picosecond laser is used to perform slicing along the laser cutting area. The laser pulse width is 20ps and the power density is 3×10⁻⁶. 6 W / cm 2 The laser focus is located 5μm below the entire surface of the crystalline silicon solar cell.
[0060] Trimethylaluminum decomposes under the instantaneous thermal field of a laser, and the released aluminum atoms diffuse into the silicon material at the cutting edge, forming a segmented continuous aluminum-doped region at the cutting edge that avoids the contact position with the back electrode.
[0061] S4. After laser cutting is completed, the supply of trimethylaluminum precursor vapor is stopped, and nitrogen is continued to be introduced to purge the residual trimethylaluminum precursor vapor in the processing chamber and collect the exhaust gas, so that the obtained sectional solar cells are cooled to room temperature without subsequent passivation film deposition and independent thermal annealing.
[0062] Comparison Example 1: No aluminum-containing precursors supplied
[0063] Compared with Example 1, the difference is that step S2 is omitted, and no aluminum-containing precursor is supplied to the laser cutting area during the laser cutting process; only a pulse width of 50 ps and a power density of 2 × 10⁻⁶ are used. 6 W / cm 2 The infrared picosecond laser completes the slicing.
[0064] Comparative Example 2: Laser cutting performed after pre-depositing an alumina film.
[0065] Compared to Example 1, the difference lies in that: instead of dynamically supplying aluminum chloride aerosol during laser cutting, an aluminum oxide film with a thickness of 20 nm is pre-deposited on the entire surface of the crystalline silicon solar cell using atomic layer deposition, with the aluminum oxide film serving as the aluminum source; subsequently, a pulse width of 50 ps and a power density of 2 × 10⁻⁶ are used. 6 W / cm 2 The infrared picosecond laser is used to cut the aluminum oxide film in sections along the predetermined cutting area, causing the aluminum oxide film to be ablated under the action of the laser; after the cutting is completed, the remaining aluminum oxide film is removed with dilute hydrochloric acid.
[0066] Performance testing methods
[0067] 1. Cutting edge composite speed
[0068] The recombination of charge carriers near the cutting edge was tested using calibrated photoluminescence imaging. PL images were acquired under the same excitation light intensity and temperature. The PL intensity decay curve was extracted along the direction perpendicular to the cutting edge, and the recombination velocity at the cutting edge was obtained by fitting a carrier diffusion-recombination model. A lower edge recombination velocity and a narrower low-emission region at the edge indicate a better edge passivation effect generated by the aluminum-doped region.
[0069] 2. Photovoltaic conversion performance of solar cells
[0070] At 25℃, AM1.5G spectrum and 1000W / m 2 The current-voltage curves of the segmented cells were tested under irradiation intensity, and the photoelectric conversion efficiency, open-circuit voltage, short-circuit current and fill factor were recorded. The results were compared with those of the unpassivated sample after cutting, the step-by-step laser-doped sample and the aluminum-coated passivated sample.
[0071] Table 1. Edge recombination characteristics and photoelectric conversion performance of the sliced solar cells in Examples 1 to 4 and Comparative Examples 1 to 2
[0072] Group Cutting edge composite speed (cm / s) Conversion efficiency (%) Open circuit voltage (mV) <![CDATA[Short-circuit current density (mA / cm 2 )]]> Fill factor (%) Example 1 85±5 26.16±0.04 737.0±0.8 42.20±0.08 84.10±0.12 Example 2 108±7 24.31±0.05 699.0±1.0 41.70±0.09 83.40±0.15 Example 3 78±5 26.54±0.04 747.0±0.7 42.30±0.07 84.00±0.11 Example 4 82±6 27.02±0.04 751.0±0.8 42.10±0.08 85.50±0.12 Compare with Example 1 245±14 25.75±0.06 729.0±1.2 42.10±0.10 83.90±0.18 Compare with Example 2 135±9 25.96±0.05 733.0±1.0 42.15±0.09 84.00±0.15
[0073] Combining Example 1 and Figure 1 It can be seen that the cutting edge remains continuously connected to the silicon substrate, with a complete overall outline and no obvious large-area chipping, through cracks, or severe peeling, indicating that the thermal impact of the picosecond laser is mainly concentrated in the cutting area. Elemental distribution results show that Si is continuously distributed in the substrate, while Al is significantly enriched in the cutting surface and adjacent silicon material, and is continuously distributed along the cutting edge, rather than being merely isolated particles attached to the surface. This indicates that the aluminum chloride precursor decomposes under the instantaneous thermal field of the laser, and the released aluminum atoms enter the newly cut edge through the rapid diffusion channels formed by local high temperature, melting, and cutting defects. During rapid cooling, they remain inside the silicon material, thus forming an aluminum-doped region extending along the cutting edge. The O element signal in the figure may originate from natural oxidation of the cutting edge or a small amount of oxygen residue, and cannot be used to conclude that a continuous aluminum oxide film has been formed. Therefore, Example 1 can continuously introduce Al into the silicon material at the cutting edge while completing laser slicing, providing a microscopic morphology and elemental distribution basis for the formation of an aluminum-doped edge field passivation structure.
[0074] In conjunction with Example 1 and Comparative Example 1, Figure 2 as well as Figure 3 It can be seen that, Figure 2The comparative example 1 shown uses only pulsed laser for slicing without supplying aluminum-containing precursor. Its cutting edge surface is relatively rough, with large irregular protrusions, molten agglomerates, pits and pores. This indicates that laser ablation and non-uniform resolidification of molten material have formed many structural defects at the cutting edge, which are prone to generating carrier recombination centers such as dangling bonds, lattice distortion and microcracks. Figure 3 In Example 1, aluminum chloride aerosol was simultaneously supplied under the same laser conditions. The resulting large-sized protrusions, agglomerated regions, and obvious pores at the cutting edge were significantly reduced, and the surface transformed into a more uniform and dense morphology composed of fine particles. This indicates that the aluminum-containing precursor participated in the instantaneous melting and rapid resolidification process in the laser-affected region, which is beneficial for improving the migration and filling of molten material and reducing local defects and morphological inhomogeneity at the cutting edge. Simultaneously, the aluminum released from the precursor decomposition entered the newly formed silicon material at the cutting edge and formed an aluminum-doped region, generating a built-in electric field that inhibits the migration of minority carriers to the cutting damage area. Correspondingly, the recombination velocity at the cutting edge in Example 1 decreased from 245 cm / s in Control Example 1 to 85 cm / s, the conversion efficiency increased from 25.75% to 26.16%, and the open-circuit voltage increased from 729 mV to 737 mV. This demonstrates that laser-synchronized aluminum doping not only improves the surface morphology of the cutting edge but also effectively reduces edge carrier recombination, minimizing photoelectric performance losses caused by laser slicing.
[0075] As can be seen from Examples 1 to 4 and Comparative Examples 1 to 2, after processing with the method of this application, the recombination velocity at the cutting edge of different types of sectional solar cells is 78–108 cm / s, the conversion efficiency is 24.31%–27.02%, the open-circuit voltage is 699–751 mV, and the short-circuit current density is 41.70–42.30 mA / cm². 2 The fill factor was 83.40%–85.50%, indicating that the method is applicable to TOPCon, PERC, HJT, and back-contact solar cells. Compared to Control Example 1, Example 1, based on the same TOPCon cell, showed a reduction in the edge recombination velocity from 245 cm / s to 85 cm / s (a decrease of approximately 65.3%), an increase in conversion efficiency from 25.75% to 26.16%, an increase in open-circuit voltage from 729 mV to 737 mV, and an increase in short-circuit current density from 42.10 mA / cm². 2 Increased to 42.20 mA / cm 2 The fill factor increased from 83.90% to 84.10%, indicating that without an aluminum-containing precursor, dangling bonds and lattice defects generated during laser cutting would form severe edge recombination centers. Compared to Control Example 2, Example 1 showed a further reduction in the cutting edge recombination velocity from 135 cm / s to 85 cm / s, a decrease of approximately 37.0%, an increase in conversion efficiency of 0.20 percentage points, an increase in open-circuit voltage of 4 mV, and an increase in short-circuit current density of 0.05 mA / cm².2 The fill factor increased by 0.10 percentage points, indicating that although the pre-deposited alumina film can produce a certain passivation effect, it is difficult to make the aluminum source act continuously and uniformly on the newly formed sidewalls during the laser cutting process. However, this application uses the same instantaneous thermal field of the laser to synchronously complete the cutting, precursor decomposition and aluminum diffusion into the silicon material at the cutting edge by moving the aluminum-containing precursor supply path and the laser scanning path. This can form a more continuous aluminum doped region, thereby more effectively suppressing edge carrier recombination and reducing the photoelectric performance loss caused by slicing.
[0076] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for aluminum-doped edge field passivation of solar cells in conjunction with laser synchronization, characterized in that, Includes the following steps: S1. Provide a complete crystalline silicon solar cell wafer, and define a laser-cut area on the complete crystalline silicon solar cell wafer; S2. Aluminum-containing precursor is supplied directionally to the laser cutting area so that the aluminum-containing precursor covers the laser cutting area; S3. Under the condition of continuous supply of the aluminum-containing precursor, the entire crystalline silicon solar cell is sliced along the laser cutting area using a pulsed laser, so that the area of action of the pulsed laser at least partially overlaps with the area covered by the aluminum-containing precursor. The instantaneous thermal field generated by laser cutting decomposes the aluminum-containing precursor and allows the aluminum atoms released by the aluminum-containing precursor to diffuse into the cutting edge formed by laser cutting, forming an aluminum-doped region extending along the cutting edge inside the silicon material at the cutting edge. S4. Stop supplying the aluminum-containing precursor and cool the laser-cut and aluminum-doped sectional cells to obtain a sectional solar cell with an aluminum-doped edge field passivation structure.
2. The method for aluminum-doped edge field passivation of solar cells in laser synchronization according to claim 1, characterized in that, The aluminum precursor in the aluminum-containing precursor is selected from at least one of trimethylaluminum, aluminum chloride, aluminum nitrate, and aluminum isopropoxide.
3. The method for aluminum-doped edge field passivation of solar cells in laser synchronization according to claim 1, characterized in that, The aluminum-containing precursor is supplied to the laser-cutting area in the form of aerosol, micro-spray, or precursor vapor.
4. The method for laser-synchronized aluminum-doped edge field passivation of solar cells according to claim 3, characterized in that, The aluminum-containing precursor is supplied in the form of an aerosol, wherein the concentration of the aluminum precursor in the aerosol is 0.1–1 mol / L, the particle size of the aerosol droplets is 50–200 nm, the supply flow rate is 5–20 L / min, and the angle between the aerosol spray direction and the laser cutting line is 30°–60°.
5. The method for aluminum-doped edge field passivation of solar cells in laser synchronization according to claim 1, characterized in that, In step S2, the supply of the aluminum-containing precursor begins before the pulsed laser reaches the corresponding laser cutting position and continues during the process of the pulsed laser acting on the corresponding laser cutting position. The supply path of the aluminum-containing precursor moves synchronously with the scanning path of the pulsed laser.
6. The method for aluminum-doped edge field passivation of solar cells in laser synchronization according to claim 1, characterized in that, The pulsed laser is an infrared nanosecond laser or an infrared picosecond laser, with a pulse width of 10 ps to 100 ns and a power density of 1 × 10⁻⁶. 6 ~5×10 6 W / cm 2 .
7. The method for laser-synchronized aluminum-doped edge field passivation of solar cells according to claim 6, characterized in that, The focal point of the pulsed laser is located on the surface of the entire crystalline silicon solar cell, or 5 to 20 μm below the surface of the entire crystalline silicon solar cell.
8. The method for aluminum-doped edge field passivation of solar cells in laser synchronization according to claim 1, characterized in that, The aluminum-doped region is distributed in a continuous strip, continuous arc, or segmented continuous shape along the cutting edge formed by laser cutting; in step S4, the laser-cut and aluminum-doped slab cells are cooled in an inert atmosphere or an air atmosphere, and after cooling, the cutting edge is no longer subjected to passivation film deposition or independent thermal annealing treatment.