Photovoltaic cells and their preparation methods, tandem cells and photovoltaic modules
By forming a passivation layer on the cut cross-section of photovoltaic cells and using laser processing, the problems of poor passivation layer effect and low processing efficiency after cutting are solved, thereby improving the performance of photovoltaic cells and the efficiency of mass production.
Patent Information
- Application Number
- CN202611364028.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-17
AI Technical Summary
After photovoltaic cells are cut, the passivation layer at the cut section has limited effect, and the cutting section processing efficiency is low, which affects the performance of the cells and the efficiency of mass production.
A passivation layer is formed on the cut cross-section of the photovoltaic cell, and the passivation layer is irradiated with a first laser so that the cut cross-sections of multiple cells are stacked in the same direction. The spot of the first laser is used to cover multiple cut cross-sections for batch processing.
This improved the passivation effect of the cut section, reduced carrier recombination, enhanced the photoelectric conversion efficiency of the sectional battery, and increased the efficiency of the cut section processing, thus meeting the mass production requirements of the sectional battery.
Smart Images

Figure CN123124492A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of photovoltaic cells, and particularly to a photovoltaic cell and its preparation method, a tandem cell, and a photovoltaic module. Background Technology
[0002] As fossil fuels are gradually depleted, solar energy is becoming increasingly widely used as a new energy alternative. A solar cell is a device that converts sunlight into electrical energy. Solar cells utilize the photovoltaic principle to generate charge carriers, which are then extracted using electrodes, thus facilitating the efficient use of electrical energy.
[0003] In the manufacturing process of photovoltaic cells, the cells are typically cut into multiple segments. The cutting damage inflicted on these segments leads to a decrease in their performance. Therefore, improving the performance of photovoltaic cells is a pressing issue that needs to be addressed. Summary of the Invention
[0004] This application provides a photovoltaic cell and its preparation method, a tandem cell and a photovoltaic module, which at least helps to solve the problems of limited passivation effect of the cross-section passivation layer on the cut cross-section and low processing efficiency of the cut cross-section of multiple cell segments.
[0005] This application provides a method for fabricating a photovoltaic cell, comprising: obtaining a cell; cutting the cell to divide it into at least two sectional cells, each sectional cell having opposing sectional surfaces and a cut cross-section connecting the sectional surfaces; forming a cross-section passivation layer on the cut cross-section; stacking a plurality of the sectional cells along a first direction such that the cut cross-sections of the plurality of sectional cells face the same direction; the first direction being the thickness direction of the sectional cells; subjecting the cut cross-section to a first laser treatment, irradiating the cross-section passivation layer with a first laser, wherein a first spot of the first laser covers at least a portion of the surface of at least two of the cut cross-sections.
[0006] Optionally, during the first laser processing, the first light spot covers at least a portion of the surface of the plurality of cutting sections, and the first light spot is displaced from one end of the cutting section to the other end along a second direction; the second direction is a direction intersecting the first direction.
[0007] Optionally, the size of the first light spot in the first direction is greater than or equal to the sum of the thicknesses of the two segmented cells, and the size of the first light spot in the first direction is 0.3 mm to 2 mm; and / or, the energy density of the first laser is 0.3 J / cm² to 2 J / cm², and / or, the scanning speed of the first laser is 500 mm / s to 7000 mm / s.
[0008] Optionally, the thickness of the cross-sectional passivation layer is 45 nm to 60 nm.
[0009] Optionally, it may also include: after forming the cross-sectional passivation layer and before stacking the plurality of the segmented cells, performing a second laser treatment, irradiating the segmented surface with a second laser.
[0010] Optionally, the spot size of the second laser is from 10 μm to 500 μm; and / or, the energy density of the second laser is from 1 J / cm² to 30 J / cm².
[0011] Optionally, before forming the passivation layer on the cut section, the cut section is oxidized to form an oxide layer on the cut section.
[0012] This application also provides a photovoltaic cell, which is prepared by the photovoltaic cell preparation method described above. The photovoltaic cell includes: a segmented cell having opposing segmented surfaces and a cut cross section connecting the segmented surfaces; and a cross section passivation layer disposed on the cut cross section.
[0013] This application also provides a stacked solar cell, comprising: a crystalline silicon bottom cell, an intermediate connecting layer, and a perovskite top cell stacked sequentially along a preset direction; wherein the crystalline silicon bottom cell is a photovoltaic cell formed by the photovoltaic cell preparation method described above, or is a photovoltaic cell as described above.
[0014] This application also provides a photovoltaic module, comprising: a battery string, the battery string comprising a plurality of photovoltaic cells formed by the method described above, or a plurality of photovoltaic cells as described above, or a plurality of stacked cells as described above; a solder ribbon, the solder ribbon being electrically connected to at least two of the photovoltaic cells to connect adjacent photovoltaic cells in series; an encapsulation layer for covering the surface of the battery string; and a cover plate for covering the surface of the encapsulation layer away from the battery string.
[0015] The technical solution provided in this application has at least the following advantages: In this application, after the solar cell is cut into wafer cells, a passivation layer is formed on the cut cross-section of the wafer cells, and the passivation layer is irradiated with a first laser. On one hand, the thermal effect generated by the first laser can thermally activate the passivation layer, improving its crystallinity and chemical bonding quality, increasing its fixed charge density, thereby enhancing the passivation effect of the passivation layer on the cut cross-section, reducing carrier recombination at the cut cross-section, and thus improving the photoelectric conversion efficiency of the wafer cells. On the other hand, by stacking multiple wafer cells and ensuring that the cut cross-sections of each wafer cell face the same direction, the cut cross-sections of multiple wafer cells are all within the coverage area of the first laser beam. The first laser beam can cover the cut cross-sections of multiple wafer cells at once, thus simultaneously completing the passivation activation of multiple wafer cell cut cross-sections in a single laser treatment, eliminating the need for processing each wafer individually, improving the processing efficiency of the cut cross-sections, and facilitating the mass production of wafer cells. The two methods work together to improve the passivation effect of the cut cross-sections while also ensuring efficient batch processing. Attached Figure Description
[0016] One or more embodiments are illustrated by way of example with corresponding pictures in the accompanying drawings. These illustrations do not constitute a limitation on the embodiments. Unless otherwise stated, the pictures in the accompanying drawings do not constitute a limitation on scale. In order to more clearly illustrate the technical solutions in the embodiments of this application or in the conventional technology, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0017] Figure 1 A step diagram illustrating a method for preparing a photovoltaic cell according to an embodiment of this application; Figure 2 This is a partial structural diagram of a photovoltaic cell fabrication method provided in an embodiment of this application; Figure 3 This is a schematic diagram of the structure of stacked photovoltaic cells in a method for preparing a photovoltaic cell according to an embodiment of this application. Figure 4 This is a schematic diagram of the process of scanning multiple cut sections with a first light spot in a method for preparing a photovoltaic cell according to an embodiment of this application; Figure 5 This is a schematic diagram of the process of scanning all cut sections with a first spot in a method for preparing a photovoltaic cell according to an embodiment of this application; Figure 6 This is a schematic diagram of a stacked battery structure provided in one embodiment of this application; Figure 7This is a schematic diagram of another structure of a stacked battery provided in an embodiment of this application; Figure 8 This is a partial structural diagram of a cell string in a photovoltaic module provided in an embodiment of this application; Figure 9 This is a partial cross-sectional schematic diagram of a photovoltaic module provided in an embodiment of this application.
[0018] Explanation of reference numerals in the attached figures: 100. Segmented battery; 101. Segmented surface; 102. Cut cross-section; 200. Cross-sectional passivation layer; 310. First light spot; 10. Crystalline silicon bottom cell; 20. Perovskite top cell; 21. First transport layer; 22. Perovskite functional layer; 23. Second transport layer; 24. Transparent conductive layer; 25. Anti-reflective layer; 30. Photovoltaic cell; 31. Encapsulation layer; 32. Cover plate; 33. Solder ribbon. Detailed Implementation
[0019] As the background technology indicates, in the photovoltaic cell slab manufacturing process, the cells are cut to form slab cells. The state of the cut cross-section of the slab cells affects the electrical performance and reliability of both the slab cells and the photovoltaic modules. Although related technologies can form a passivation layer on the cut cross-section, there is still room for improvement in the passivation quality of the cut cross-section, the processing consistency between different slab cells, and the cross-section processing efficiency.
[0020] The root cause of these problems lies in the fact that after the solar cells are cut, damaged areas and interface defects easily form at the cut cross-section, and the cut cross-section and its adjacent areas may become regions where carrier recombination is relatively concentrated. Furthermore, the passivation layer formed on the cut cross-section, in its deposited state, may still require further improvement through subsequent heat treatment in terms of film state, fixed charge density, chemical bonding quality, or interface bonding state. If cross-section processing is performed on each individual solar cell, the heating conditions, processing locations, and processing cycles may differ between different cells, thus affecting the consistency of cross-section processing and batch manufacturing efficiency. Combining the grid electrode processing and the cross-section passivation layer processing within the same processing window may also cause the process conditions of the two types of processing objects to interfere with each other, making it inconvenient to adjust the process parameters of the grid electrode processing and the cross-section passivation layer processing separately.
[0021] Based on this, embodiments of this application provide a method for fabricating photovoltaic cells, slab cells, and photovoltaic modules. The fabrication method involves cutting a solar cell into multiple slab cells and forming a passivation layer on the cut cross-sections. The multiple slab cells are then stacked along their thickness direction, with the cut cross-sections facing the same direction. Subsequently, a first laser is used to irradiate the passivation layer, and the first spot of the first laser covers the multiple cut cross-sections. This allows the first laser to perform batch processing on multiple cut cross-sections, enabling the passivation layers of the multiple slab cells to undergo heat treatment under similar laser processing conditions. This improves the passivation quality of the cut cross-section areas, the processing consistency between different slab cells, and the cross-section processing efficiency.
[0022] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined. Similarly, "multiple sets" refers to two or more sets (including two sets), and "multiple pieces" refers to two or more pieces (including two pieces).
[0023] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0024] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent three cases: A exists, A and B exist simultaneously, and B exists. In addition, the character " / " in this document generally indicates that the related objects before and after it have an "or" relationship.
[0025] In the description of the embodiments of this application, the technical terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential," etc., indicating orientation or positional relationships, are based on the orientation or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the embodiments of this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of this application. For example, if the device or element in the illustration is inverted, then the element described as "below," "under," "below," or "bottom" of other elements or features will be oriented "above" or "top" of said other elements or features. Therefore, the term "below" may cover both above and below orientation depending on the context in which the term is used, which will be obvious to those skilled in the art. Materials may be oriented in other ways (e.g., rotated 90 degrees, inverted, flipped), and the spatial relative descriptive terms used herein may be interpreted accordingly.
[0026] In the description of the embodiments of this application, unless otherwise expressly specified and limited, technical terms such as "installation," "connection," "joining," and "fixing" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. For those skilled in the art, the specific meaning of the above terms in the embodiments of this application can be understood according to the specific circumstances.
[0027] In the description of the embodiments of this application, "electrically connected to one component" means that both components are made of conductive materials, and the two components are in direct contact and connected or indirectly connected via other conductive materials. Therefore, when the photovoltaic module or cell is generating electricity, current flows between the two components. "Electrically contacting one component to another" means that the two components are not only in contact, but also, because both components are made of conductive materials, current flows between the two components when the photovoltaic module or cell is generating electricity.
[0028] In the description of embodiments of this application, the terms "about," "approximately," "roughly," or "about" for a numerical value referring to a specific parameter include the numerical value, and those skilled in the art will understand that the deviation from the numerical value is within the acceptable tolerance of the specific parameter. For example, "about" or "about" for a numerical value may include additional numerical values that are in the range of 90.0% to 110.0% of the numerical value, such as in the range of 95.0% to 105.0%, 97.5% to 102.5%, 99.0% to 101.0%, 99.5% to 100.5%, or 99.9% to 100.1%.
[0029] In the accompanying drawings corresponding to the embodiments of this application, the thickness and / or area of layers, films, panels, regions, etc., are enlarged for better understanding and ease of description. Throughout the specification, the same reference numerals denote the same elements. Furthermore, when describing a component as "generally" formed on another component, it is because, due to manufacturing tolerances or errors, the component is not formed on the entire surface of the other component.
[0030] In the description of embodiments of this application, when a component "includes" another component, other components are not excluded unless otherwise stated, and may be further included. When describing a component (such as a layer, film, region, or substrate) on or on the surface of another component, the component may be "directly" located on the surface of the other component, or there may be an intermediate component between the two components. Conversely, when describing a component on the surface of another component, or a component "directly" on another component, or a component surface on which another component is formed or disposed, it indicates that there is no intermediate component between the two components. For simplicity and clarity, various components may be drawn at any scale. In the drawings, some components may be omitted for simplicity.
[0031] The terminology used in the description of the various embodiments herein is for the purpose of describing particular embodiments only and is not intended to be limiting. As used in the description of the various embodiments and the appended claims, the term "the component" is also intended to include the plural form unless the context clearly indicates otherwise.
[0032] The “components” mentioned above can refer to layers, membranes, regions, parts, plates, or structures, etc.
[0033] The embodiments of this application will now be described in detail with reference to the accompanying drawings. However, those skilled in the art will understand that many technical details have been provided in the embodiments of this application to facilitate a better understanding of the application. However, the technical solutions claimed in this application can be implemented even without these technical details and various variations and modifications based on the following embodiments.
[0034] Figure 1 A step diagram illustrating a method for preparing a photovoltaic cell according to an embodiment of this application; Figure 2 This is a partial structural diagram of a photovoltaic cell fabrication method provided in an embodiment of this application; Figure 3 This is a schematic diagram of the structure of stacked photovoltaic cells in a method for preparing a photovoltaic cell according to an embodiment of this application. Figure 4 This is a schematic diagram of the process of scanning multiple cut sections with a first light spot in a method for preparing a photovoltaic cell according to an embodiment of this application; Figure 5 This is a schematic diagram of the process of scanning all cut sections with a first spot in a method for preparing a photovoltaic cell according to an embodiment of this application.
[0035] refer to Figures 1 to 5 The preparation method of photovoltaic cell 30 includes: Obtain battery cells; The battery cell is cut to divide it into at least two cell segments 100, each cell segment 100 having opposing segmented surfaces 101 and a cut section 102 connecting the segmented surfaces 101. A cross-section passivation layer 200 is formed on the cut section 102; Multiple cell wafers 100 are stacked and arranged along a first direction, such that the cut sections 102 of the multiple cell wafers 100 face the same direction; the first direction is the thickness direction of the cell wafers 100. The cut section 102 is subjected to a first laser treatment, in which the first laser is used to irradiate the section passivation layer 200, and the first laser spot 310 covers at least a portion of the surface of at least two cut sections 102.
[0036] This application involves cutting a battery cell into multiple sub-cells 100 and forming a cross-section passivation layer 200 on the cut cross-section 102. The multiple sub-cells 100 are then stacked along their thickness direction, with the cut cross-sections 102 of the multiple sub-cells 100 facing the same direction. Subsequently, a first laser is used to irradiate the cross-section passivation layer 200, and the first laser spot 310 covers at least a portion of the surface of at least two cut cross-sections 102. This allows the first laser to perform batch processing on multiple cut cross-sections 102, enabling the cross-section passivation layers 200 of the multiple sub-cells 100 to undergo heat treatment under similar laser processing conditions. This improves the passivation quality of the cut cross-section 102 region, the processing consistency between different sub-cells 100, and the cross-section processing efficiency.
[0037] The embodiments of this application will be described in more detail below with reference to the accompanying drawings.
[0038] Reference Figure 1 As shown, Figure 1 This is a step diagram illustrating a method for fabricating a photovoltaic cell according to an embodiment of this application. The method includes: S100, obtain battery cells; S200, the battery cell is cut to divide the battery cell into at least two segmented cells 100, each segmented cell 100 having opposing segmented surfaces 101 and a cut section 102 connecting the segmented surfaces 101. S300, a cross-section passivation layer 200 is formed on the cut cross-section 102; S400, multiple segmented batteries 100 are stacked and arranged along the first direction X, such that the cut sections 102 of the multiple segmented batteries 100 face the same direction; the first direction X is the thickness direction of the segmented battery 100. S500, the cut section 102 is subjected to a first laser treatment, and the first laser is used to irradiate the section passivation layer 200. The first laser spot 310 covers at least a portion of the surface of at least two cut sections 102.
[0039] In step S100, a solar cell is obtained. The solar cell is a whole photovoltaic cell semi-finished product or finished solar cell before cutting. The solar cell is a sheet-like structure with photoelectric conversion function and has two opposing whole surfaces.
[0040] In some embodiments, the solar cell can be one or any combination of BC (Back Contact) cells, TOPCon (Tunnel Oxide Passivated Contact) cells, HIT / HJT (Heterojunction Technology) cells, PERC (Passivated Emitter Rear Cell) cells, thin-film solar cells, and tandem cells. Thin-film solar cells include, but are not limited to, perovskite thin-film solar cells, copper indium selenide (CIGS) thin-film solar cells, gallium arsenide (GaAs) thin-film solar cells, and cadmium sulfide (CdS) thin-film solar cells. Tandem cells include, but are not limited to, perovskite top cells stacked with crystalline silicon cells, perovskite top cells stacked with perovskite top cells, and perovskite top cells stacked with thin-film cells.
[0041] In step S200, the battery cell is cut to divide it into at least two segmented cells 100. Each segmented cell 100 has opposing segmented surfaces 101 and a cutting section 102 connecting the segmented surfaces 101. The segmented cells 100 have intersecting and perpendicular first directions X, second directions Y, and third directions Z. Specifically, the first direction X is the thickness direction of the segmented cell 100, the second direction Y is the length direction of the cutting section 102, and the third direction Z is a direction perpendicular to the plane containing the cutting section 102.
[0042] In some embodiments, the solar cell is cut into at least two, three, four, or more sub-cells 100. The number of sub-cells 100 can be set according to the cell size, module layout, series-parallel connection method, or current matching requirements, and is not specifically limited herein. By dividing the entire solar cell into multiple smaller sub-cells 100, this application can reduce the current density and resistance loss within a single cell, which is beneficial for reducing the power loss of photovoltaic modules assembled from sub-cells 100.
[0043] In some embodiments, the cutting process is performed along a cutting path on the solar cell. The cutting path may be located between opposite edges of the solar cell, or it may extend along the length or width of the solar cell. The cut section 102 formed after the cutting process may expose part of the internal structure of the solar cell and may be accompanied by surface states, microcracks, heat-affected zones, or localized rough areas. Subsequently, a passivation layer 200 is formed on the cut section 102 and a first laser treatment is performed, which enables the establishment of passivation coverage and post-processing of the film layer around the cut section 102 region, thereby giving the edge region formed by the cutting a more stable interface state.
[0044] In some embodiments, the method for cutting the battery cell includes at least one of the following: laser cutting, laser scribing, laser thermal vaporization and melting, and laser-induced scoring separation. Laser cutting uses a laser to directly cut the battery cell along a path. Laser scribing uses a laser to create a score along a path, followed by the application of mechanical force to cause the battery cell to break down along the score. Laser thermal vaporization and melting uses a laser to locally vaporize or melt the material to achieve separation. Laser-induced scoring separation uses a laser to induce scoring to achieve separation. One or more of the above cutting processes can be selected and combined according to different battery structures or production lines, taking into account both cutting efficiency and the flatness of the cut cross-section 102; no specific limitations are made here.
[0045] Reference Figure 2 As shown, in step S300, a cross-section passivation layer 200 is formed on the cut cross-section 102. The cross-section passivation layer 200 is used to passivate defects such as dangling bonds at the cut cross-section 102 to suppress carrier recombination at the cut cross-section 102.
[0046] In some embodiments, the material of the cross-section passivation layer 200 includes at least one of aluminum oxide, silicon oxide, silicon nitride, nickel oxide, zinc oxide, hydrogenated silicon nitride, silicon carbide, amorphous silicon, polycrystalline silicon, and nanocrystalline silicon.
[0047] In some embodiments, the method for forming the cross-sectional passivation layer 200 includes atomic layer deposition.
[0048] In one example, the atomic layer deposition process temperature is 220°C to 280°C, and the process duration can be 1 hour to 3 hours. This process temperature and duration range allows the cross-sectional passivation layer 200 to form a continuous and dense coverage on the cut cross-section 102, while avoiding excessive heat damage to the substrate and the formed gate line contacts caused by excessive temperature.
[0049] In some embodiments, the segmented battery 100 includes a stacked substrate, a doped layer, and a surface passivation layer, wherein the surface of the surface passivation layer is configured as segmented surfaces 101. A cut section 102 is an end face connecting two segmented surfaces 101. A section passivation layer 200 covers the cut section 102 and extends to at least a portion of the segmented surfaces 101 adjacent to the cut section 102. In other words, the section passivation layer 200 extends from the cut section 102 and overlaps with the portion of the surface passivation layer adjacent to the cut section 102, such that the section passivation layer 200 and the surface passivation layer continuously cover each other at the junction of the cut section 102 and the segmented surfaces 101.
[0050] In some embodiments, the extension length of the cross-sectional passivation layer 200 on the segmented surface 101 is 1 mm to 3 mm. Optionally, the extension length of the cross-sectional passivation layer 200 on the segmented surface 101 is 1.5 mm to 2.5 mm. Optionally, the extension length of the cross-sectional passivation layer 200 on the segmented surface 101 can be 1 mm, 1.5 mm, 2 mm, 2.5 mm, or 3 mm. By having the cross-sectional passivation layer 200 and the surface passivation layer overlap and continuously cover at the junction of the cutting cross-section 102 and the segmented surface 101, this application avoids composite leakage points formed due to passivation interruption at the junction, compared to the case where the cross-sectional passivation layer 200 only covers the cutting cross-section 102 and is interrupted at the junction. This makes the overall passivation of the cutting edge more continuous and complete, further improving the passivation effect of the segmented battery 100 edge.
[0051] In some embodiments, the thickness of the cross-section passivation layer 200 is 45 nm to 60 nm. Optionally, the thickness of the cross-section passivation layer 200 is 47 nm to 58 nm. Optionally, the thickness of the cross-section passivation layer 200 can be 45 nm, 50 nm, 55 nm, or 60 nm. This application sets the thickness of the cross-section passivation layer 200 within the above-mentioned range to ensure, on the one hand, that the cross-section passivation layer 200 is sufficient to cover the microscopic defects and rough areas of the cutting cross-section 102; on the other hand, a certain thickness of the cross-section passivation layer 200 makes it difficult for the heat from the first laser to be transferred to the interface near the cutting cross-section 102, thereby preventing the further formation or development of defects in the cutting cross-section 102.
[0052] In some embodiments, after step S200 and before step S300, the method further includes: S210, the cut section 102 is oxidized to form an oxide layer on the cut section 102. The section passivation layer 200 is formed on the side of the oxide layer away from the cut section 102 and is located between the cut section 102 and the section passivation layer 200.
[0053] After cutting, the cut section 102 may contain surface states, microcracks, or locally rough areas. The oxide layer is used to improve the smoothness and interface state density of the cut section 102, providing a good bonding interface for the subsequently formed section passivation layer 200. During the first laser heat treatment process, this interface foundation also helps the section passivation layer 200 maintain a relatively stable bonding state, thereby improving the reliability of the section passivation layer 200 after heat treatment.
[0054] In some embodiments, the oxide layer may be a silicon oxide layer or other oxide layer suitable for being disposed between the cut section 102 and the section passivation layer 200. The specific material may be selected based on the cell substrate material and the section passivation layer 200 material, and is not specifically limited here.
[0055] In some embodiments, the oxidation treatment includes: ultraviolet (UV) oxidation, ozone oxidation, and laser thermal oxidation. The UV oxidation process uses UV light to irradiate the cut section 102 to promote surface oxidation; the ozone oxidation process uses ozone to oxidize the cut section 102; and the laser thermal oxidation process uses the thermal effect of a laser to promote surface oxidation of the cut section 102. These processes can be used individually or in combination depending on the state of the cut section 102 and the production line configuration; no limitation is made here.
[0056] Reference Figure 3 As shown, in step S400, multiple segmented cells 100 are stacked and arranged along the first direction X, so that the cut sections 102 of the multiple segmented cells 100 face the same direction. This direction refers to the direction in which the incident light spot is oriented during the first laser irradiation.
[0057] In some embodiments, multiple cell wafers 100 are stacked sequentially along a first direction X to form a cell stack, such that the cut sections 102 of each cell wafer 100 face the same direction, thereby arranging the cut sections 102 of the multiple cell wafers 100 on the same side perpendicular to the first direction X and making them approximately coplanar. This co-directional arrangement reduces the need to repeatedly switch processing sides around each cell wafer 100 during the subsequent first laser processing and reduces the offset of the light spot landing point caused by the difference in the orientation of the cell wafers 100. The multiple cut sections 102 form a repositionable light-receiving interface on the same processing side, which helps to keep the focal length, incident angle, and scanning path of the laser emitting device within a relatively stable process window, thereby providing a spatial organization basis for subsequent batch heat treatment.
[0058] It should be noted that the cutting sections 102 facing the same direction can be understood as multiple cutting sections 102 being located on the same side of the stacked multi-cell battery 100 and facing the same processing side as a whole. Since the actual cutting sections 102 may have micro-roughness or local morphological differences, the aforementioned "facing the same direction" does not require that the micro-surfaces of each cutting section 102 be strictly coplanar, nor does it exclude manufacturing tolerances, clamping tolerances, or local morphological differences between the multi-cell battery 100. As long as multiple cutting sections 102 can jointly face the processing side of the first laser, allowing the first laser spot 310 to cover multiple cutting sections 102, it can be considered that multiple cutting sections 102 are facing the same direction.
[0059] In some embodiments, multiple segmented batteries 100 can be stacked and positioned using a support platform, clamping structure, limiting structure, or other tooling capable of maintaining the relative positions of the segmented batteries 100. The aforementioned tooling can support the segmented surfaces 101 of the segmented batteries 100 and can also limit their position at the edges of the segmented batteries 100 to reduce the risk of positional displacement of the segmented batteries 100 during the first laser processing.
[0060] In step S500, the cut section 102 is subjected to a first laser treatment, and the first laser is used to irradiate the section passivation layer 200. The first spot 310 of the first laser covers at least a portion of the surface of at least two cut sections 102.
[0061] This application uses a first laser to process the cut section 102. The thermal effect generated by the first laser improves the crystallinity and chemical bonding quality of the passivation layer 200, increases its fixed charge density, and transforms the amorphous or weakly crystalline deposited passivation film into an activated passivation film with better crystallinity and higher fixed charge density. This enhances the passivation effect of the passivation layer 200 on the cut section 102, reduces carrier recombination at the cut section 102, and thus improves the photoelectric conversion efficiency of the segmented cell 100. Furthermore, since multiple segmented cells 100 are stacked along the first direction X and each cut section 102 faces the same direction, the cut sections 102 of multiple segmented cells 100 are all within the coverage area of the first laser spot 310. The first laser spot can cover the cut sections 102 of multiple segmented cells 100 at once, thus simultaneously completing the passivation and activation of the cut sections 102 of multiple segmented cells 100 in a single laser processing, eliminating the need for processing each cell individually. Therefore, while improving the passivation effect of the cutting section 102, the processing efficiency of the cutting section 102 is also improved, which is conducive to meeting the mass production requirements of the segmented battery 100.
[0062] In some embodiments, the first spot 310 of the first laser can cover a portion of the multiple cutting sections 102. In other words, the first spot 310 of the first laser covers the multiple cutting sections 102, and only a portion of the cutting sections 102 covered by the first spot 310 of the first laser is covered by the first spot 310 of the first laser.
[0063] It should be noted that the first laser spot 310 covers multiple cutting sections 102, including both the number of cutting sections 102 spanned by the spot in the first direction X and the coverage area of a single cutting section 102. In terms of quantity, the spot's coverage in the first direction X simultaneously spans two or more cutting sections 102 of the stacked battery cells 100. In terms of coverage area, for each cutting section 102 spanned by the spot, the spot can cover part or all of the surface of that cutting section 102. These two aspects can be set separately. The coverage range of the first laser spot 310 can be set according to the thickness of the battery cell 100, the height of the cutting section 102, the coverage range of the passivation layer 200, the number of stacked battery cells 100, and the area to be processed; this application does not impose any limitations on this.
[0064] In some embodiments, refer to Figure 4 As shown, during the first laser processing, the first laser spot 310 simultaneously covers at least a portion of the surface of multiple cutting sections 102. The first laser spot 310 is displaced from one end of the cutting section 102 to the other along the second direction Y, which intersects with the first direction X. The spot spans multiple cutting sections 102 in the first direction X, and moves from one end of the cutting section 102 to the other in the second direction Y in a scanning manner, so that the multiple cutting sections 102 spanned by the spot are irradiated segment by segment along their length. The first laser can act on the corresponding cross-sectional area of multiple segmented cells 100 at any position on the scanning path, so that the multiple cutting sections 102 simultaneously covered obtain similar heat treatment trajectories along their length, which helps to reduce the passivation unevenness caused by local areas not being covered by the spot.
[0065] In some embodiments, refer to Figure 5 As shown, during the first laser processing, the first laser spot 310 simultaneously covers at least a portion of the surface of all cut sections 102 in the first direction X, and the first laser spot 310 is displaced from one end of the cut section 102 to the other in the second direction Y. This application moves from one end of the cut section 102 to the other in a scanning manner, so that the multiple cut sections 102 spanned by the laser spot are irradiated segment by segment along their length direction. This ensures that multiple cut sections 102 receive light in the same batch, and the first laser can simultaneously act on the corresponding cross-sectional area of multiple segmented cells at any position on the scanning path, so that each segmented cell obtains a similar heat treatment trajectory along the length direction of the cut section, thereby reducing the problem of uneven passivation caused by untreated local areas.
[0066] In some embodiments, the relative displacement of the first laser spot 310 and the stacked multiple segmented cells 100 along the first direction X can be achieved by the stepping movement of the support platform carrying the multiple segmented cells 100 along the first direction X, by the movement of the laser emitting device along the first direction X, or by changing the landing point of the laser spot along the first direction X through a galvanometer system. Optionally, the relative displacement between two adjacent irradiation processes corresponds to the coverage width of the first laser spot 310 in the first direction X, so that the cut sections 102 covered by each irradiation process are sequentially connected along the first direction X. The above methods can be implemented individually or in combination. Other methods that can cause relative displacement between the first laser spot 310 and the multiple segmented cells 100 along the first direction X are also applicable, and this application does not limit them.
[0067] In some embodiments, the coverage areas of the first light spot 310 in the first direction X partially overlap during two adjacent irradiation processes. That is, the cutting section 102 located at the edge of the first light spot 310 during the previous irradiation process is still within the coverage area of the first light spot 310 during the subsequent irradiation process. As a result, there will be no area not covered by the first light spot 310 at the junction of two adjacent sets of cutting sections 102, and the cutting section 102 located at the edge of the first light spot 310 can receive supplementary heat input during the subsequent irradiation process, which helps to reduce the difference in passivation activation between groups caused by the low energy distribution at the edge of the light spot.
[0068] The size of the first light spot 310 in the first direction X is greater than or equal to the sum of the thicknesses of the two segmented cells 100. That is, when the thickness of the segmented cell 100 is 100 μm, the size is not less than 200 μm; when the thickness of the segmented cell 100 is 200 μm, the size is not less than 400 μm. Thus, the first light spot 310 spans at least two cutting sections 102 in the first direction X.
[0069] In some embodiments, the size of the first light spot 310 in the first direction X is 0.3 mm to 2 mm. Optionally, the size of the first light spot 310 in the first direction X is 0.5 mm to 1.5 mm. Optionally, the size of the first light spot 310 in the first direction X can be 0.3 mm, 0.5 mm, 1 mm, 1.5 mm, or 2 mm. When the size is within the above range, the light spot can span the cut sections 102 of multiple stacked slab cells 100 and maintain a relatively controllable energy density, so that the grouped sections obtain similar activation conditions. Wherein, when the light spot size is at the smaller end of the above range, the stacked cut sections 102 can be covered group by group through multiple irradiation processes performed sequentially along the first direction X; when the light spot size is at the larger end of the above range, a single irradiation process can cover a larger number of cut sections 102.
[0070] In some embodiments, the thickness of the segmented battery 100 is 100 μm to 200 μm. Optionally, the thickness of the segmented battery 100 is 130 μm to 180 μm. Optionally, the thickness of the segmented battery 100 can be 100 μm, 130 μm, 150 μm, 180 μm, or 200 μm. The thickness of the segmented battery 100 is the dimension of the segmented battery 100 along the first direction X. When the thickness of the segmented battery 100 is within the above range, the cutting section 102 has a height in the first direction X sufficient to support the section passivation layer 200 and accept laser heat treatment, so that the first spot 310 of the first laser can simultaneously span two or more cutting sections 102 with a limited size in the first direction X.
[0071] In some embodiments, the energy density of the first laser is 0.3 J / cm².2 Up to 2J / cm 2 Optionally, the energy density of the first laser is 0.5 J / cm². 2 Up to 1.8 J / cm 2 Optionally, the energy density of the first laser can be 0.3 J / cm². 2 0.5J / cm 2 0.8J / cm 2 1J / cm 2 1.2J / cm 2 1.5J / cm 2 1.8J / cm 2 or 2J / cm 2 When the energy density is within the above range, the cross-section passivation layer 200 can obtain an activation energy sufficient to promote atomic rearrangement, remove aluminum hydroxyl bonds, eliminate stress, and reduce defect states, while avoiding excessive energy that could damage the film structure of the cross-section passivation layer 200.
[0072] In some embodiments, the power of the first laser is 50W to 300W. Optionally, the power of the first laser is 75W to 250W. Optionally, the power of the first laser can be 50W, 75W, 150W, 250W, or 300W. The power of the first laser determines the amount of heat input to the cross-sectional passivation layer 200 per unit time. Within the above range, the deposited film layer can achieve thermal activation sufficient to improve the bonding state and fixed charge state, while the area adjacent to the cut cross-section 102 is less susceptible to excessive thermal shock.
[0073] In some embodiments, the scanning speed of the first laser is from 500 mm / s to 7000 mm / s. Optionally, the scanning speed of the first laser is from 1000 mm / s to 6000 mm / s. Optionally, the scanning speed of the first laser can be 500 mm / s, 1000 mm / s, 3000 mm / s, 6000 mm / s, or 7000 mm / s. The scanning speed determines the dwell time of the first laser on the unit area of the cross-sectional passivation layer 200. When within the above range, the light spot can form a continuous but not excessively accumulated thermal history as it moves along the cutting section 102, so that the corresponding cross-sectional areas of the multiple segmented cells 100 obtain similar activation levels.
[0074] In some embodiments, after obtaining the battery cell in step S100 and before cutting the battery cell in step S200, the method further includes: Step S110: The battery cell has a relatively complete surface, and a slurry electrode is formed on at least one complete surface; a third laser treatment is performed, in which the complete surface and the slurry electrode are irradiated with a third laser, and a third voltage is applied to the slurry electrode, which is then converted into an electrode.
[0075] In step S110, the third laser treatment can be used to perform laser-assisted sintering of the slurry electrodes on the entire surface of the solar cell. The entire surface of the solar cell and the slurry electrodes thereon are irradiated with a third laser, and a third voltage is applied to the slurry electrodes. The third laser excites charge carriers, and under the influence of the loop current formed by the third voltage, local high temperatures are generated at the metal-semiconductor interface, promoting the formation of a relatively stable ohmic contact between the metal and semiconductor materials, thus transforming the slurry electrodes into electrodes. Therefore, a better electrode contact state can be established before the solar cell is cut, providing an electrical basis for subsequent cutting, cross-section passivation, and slab processing.
[0076] In some embodiments, the energy density of the third laser is from 20 J / cm² to 60 J / cm². Optionally, the energy density of the third laser is from 30 J / cm² to 50 J / cm². Optionally, the energy density of the third laser can be 20 J / cm², 35 J / cm², 50 J / cm², or 60 J / cm². This energy density range corresponds to the interfacial thermal window required for the conversion of the slurry electrode to the electrode; within this window, moderate local rearrangement and interdiffusion can be achieved between the metal particles, the glass phase, and the semiconductor surface, causing the contact interface to transition from a loosely overlapping state to a more stable ohmic contact state.
[0077] In some embodiments, the third voltage is 10V to 30V. Optionally, the third voltage is 15V to 25V. The optional third voltage can be 10V, 15V, 20V, or 30V. When the third voltage is within the above range, it can work in conjunction with the third laser to form an appropriate current path between the grid lines and the solar cell, promoting localized thermal effects at the contact interface, thereby improving the photoelectric conversion efficiency of the photovoltaic cell.
[0078] In some embodiments, the wavelength of the third laser is 532 nm or 1064 nm.
[0079] In some embodiments, the spot size of the third laser is from 80 μm to 500 μm. Optionally, the spot size of the third laser is from 100 μm to 450 μm. Alternatively, the spot size of the third laser can be 80 μm, 150 μm, 300 μm, or 500 μm. When the spot size of the third laser is within the above range, it is beneficial to cover the area adjacent to the slurry electrode or grid line and reduce excessive thermal impact on non-target areas.
[0080] In some embodiments, after forming the cross-section passivation layer 200 on the cut cross-section 102 in step S300 and before stacking the segmented cells 100 in step S400, the method further includes: Step S310: Perform a second laser treatment by irradiating the slice surface 101 and the electrodes with a second laser and applying a second voltage to the electrodes.
[0081] In step S310, the second laser treatment, after cutting and forming the cross-sectional passivation layer 200, involves secondary laser-assisted repair of the electrodes: the second laser irradiates the segmented surface 101 of the segmented cell 100 and the electrodes thereon, and a second voltage is applied to the electrodes. This second laser treatment achieves two effects: the second voltage creates an electric field inside the segmented cell 100, driving glass ions in the electrodes to migrate to the interface; combined with the local thermal effect generated by the second laser, it locally anneals the stress-damaged interface area, repairing microcracks and lattice distortions caused by the thermal process during cutting and forming the cross-sectional passivation layer 200; simultaneously, the thermal effects of the second laser and the second voltage improve the crystallinity and chemical bonding quality of the passivation layer on the segmented surface 101, enhancing the passivation effect of the passivation layer on the cut edges.
[0082] In some embodiments, the energy density of the second laser is from 1 J / cm² to 30 J / cm². Optionally, the energy density of the second laser is from 5 J / cm² to 25 J / cm². Optionally, the energy density of the second laser can be 1 J / cm², 10 J / cm², 20 J / cm², or 30 J / cm². When the energy density of the second laser is within the above range, the second laser can provide sufficient local annealing energy to the contact interface, thereby alleviating contact loosening caused by cutting or deposition thermal processes, while avoiding pushing the formed ohmic contact back into an over-sintering state.
[0083] In some embodiments, the second voltage is 5V to 30V. Optionally, the second voltage is 10V to 25V. Optionally, the second voltage can be 5V, 10V, 20V, or 30V. The second voltage is used to form an auxiliary electric field between the electrode and the segmented cell, so that the heat generated by the second laser is more concentrated on the electrode contact interface. This application sets the second voltage within the above range to avoid insufficient electric field driving due to an excessively low second voltage, resulting in weak carrier injection and current heating effects at local contact points, and limited contact repair depth; on the other hand, it avoids excessively high second voltage, which could lead to excessive concentration of local current at edges or defect areas, causing new electrical damage.
[0084] In some embodiments, the spot size of the second laser is from 10 μm to 500 μm. Optionally, the spot size of the second laser is from 50 μm to 450 μm. Optionally, the spot size of the second laser can be 10 μm, 100 μm, 300 μm, or 500 μm. When the spot size of the second laser is within the above range, the spot can cover the electrode or its adjacent contact area, so that the contact repair is concentrated on the carrier output path.
[0085] In some embodiments, the wavelength of the second laser is 532 nm or 1064 nm. The wavelength of the second laser may be the same as or different from that of the third laser, and no specific limitation is made here.
[0086] In this embodiment, before forming the cross-section passivation layer 200, a third laser is used to laser-assisted sinter the slurry electrode to form an ohmic contact. After cutting and cross-section passivation, a second laser is used to perform secondary contact repair on the electrode. Compared with the case of only performing one sintering without secondary repair, the gate line contact degraded due to the thermal process of cutting and deposition of the cross-section passivation layer 200 is repaired. This improves the cross-section passivation effect while reducing the contact resistance of the gate line electrode, further improving the fill factor and photoelectric conversion efficiency of the sectional cell 100.
[0087] In some embodiments, the energy density of the second laser is less than or equal to the energy density of the third laser. Since the second laser is used for secondary repair of electrodes that have already formed ohmic contacts, its energy density does not exceed that of the third laser used for primary sintering, which can avoid over-processing of the formed ohmic contacts and silicon wafers, resulting in passivation loss or silicon wafer damage.
[0088] In some embodiments, the ratio of the energy density of the third laser to the energy density of the second laser is 1.5 to 60. Optionally, the ratio is 5 to 55. Alternatively, the ratio can be 1.5, 5, 20, or 60. When the ratio is within the above range, the second laser has a sufficient degradation margin relative to the third laser to avoid excessive reprocessing of the formed contact; simultaneously, the degradation margin is not too large, and the second laser retains the ability to repair thermally degraded contacts.
[0089] In some embodiments, the second voltage is less than or equal to the third voltage. This ensures that the second voltage applied during secondary repair does not exceed the third voltage applied during the first sintering, thus preventing damage to the cell 100 from an excessively strong electric field.
[0090] In some embodiments, the ratio between the third voltage and the second voltage is 1 to 6. Optionally, the ratio between the third voltage and the second voltage is 1.5 to 5.5. Optionally, the ratio between the third voltage and the second voltage can be 1, 2, 4, or 6. This ratio range limits the voltage relationship between primary sintering and secondary repair while balancing the contact repair effect and the risk of electrical damage. When the ratio between the third voltage and the second voltage is within the above range, the second voltage can retain sufficient electric field assistance to generate a repairable current-thermal effect at the local contact interface; at the same time, it avoids the second voltage being too high, which would cause current congestion in the edge defect area during the slab formation stage.
[0091] The second laser is used for contact repair of the electrodes, and its target is the grid line area distributed on the segmented surface 101; the first laser is used for thermal activation of the cross-sectional passivation layer 200, and its target is the cut cross-section 102. Since the targets of the two lasers are different in spatial distribution and required thermal action, the spot size and energy density of the second laser and the first laser can be adapted to their respective targets.
[0092] In some embodiments, the spot size of the first laser 310 in the first direction X is larger than the spot size of the second laser. The first laser needs to cross at least two stacked cutting sections 102 in the first direction X, and therefore has a larger size in that direction; the second laser processes the gate line regions distributed on the segmented surface 101, and its spot size is adapted to the gate line width and adjacent contact areas. Thus, the spot sizes of the two lasers are adapted to their respective processing objects, the first laser covers multiple cutting sections 102 in a group, and the second laser focuses the contact repair on the carrier output path.
[0093] In some embodiments, the ratio between the size of the first laser spot 310 in the first direction X and the size of the second laser spot is 2 to 200. Optionally, the ratio between the size of the first laser spot 310 in the first direction X and the size of the second laser spot is 5 to 100. Optionally, this ratio can be 2, 5, 20, 100, or 200. When this ratio is within the above range, the spot of the first laser has sufficient width relative to the spot of the second laser in the first direction X to span the stacked multiple cutting sections 102; at the same time, this width is not too large, so that the energy distribution of the first laser in the first direction X remains relatively uniform, and the energy difference received by the cutting section 102 located at the edge of the spot and the cutting section 102 located in the middle of the spot is small.
[0094] In some embodiments, the energy density of the second laser is greater than that of the first laser. Thus, the second laser, with its higher energy density, provides the heat required for gate contact repair, while the first laser, with its lower energy density, gently thermally activates the passivation film on the cross-section, avoiding excessive energy that could damage the passivation film, thereby matching the energy densities of both lasers to their respective needs.
[0095] In some embodiments, the ratio of the energy density of the second laser to the energy density of the first laser is 1.5 to 100. Optionally, the ratio of the energy density of the second laser to the energy density of the first laser is 5 to 90. Optionally, the ratio of the energy density of the second laser to the energy density of the first laser can be 1.5, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, or 100. This application limits the ratio of the two energy densities to an appropriate range to balance the heat requirements of gate line repair with the gentle processing of cross-section passivation activation.
[0096] In some embodiments, the energy density of the first laser is lower than that of the second laser, so that the thermal activation of the cross-sectional passivation film is carried out at a mild energy level; when the first laser processing is performed in a scanning manner, the energy density of the first laser can be determined by its power, scanning speed and spot size.
[0097] In some embodiments, the second laser processing is performed simultaneously with the first laser processing; or, the second laser processing is performed sequentially with the first laser processing. When the second laser processing is performed simultaneously with the first laser processing, the two sets of laser devices can complete the contact repair of the electrode and the thermal activation of the cross-sectional passivation layer 200 in the same process, shortening the process cycle and improving production efficiency. When the second laser processing is performed sequentially with the first laser processing, the laser parameters for the gate line repair and the cross-sectional activation can be set independently to avoid mutual interference and ensure that both processes are within their respective optimal process windows.
[0098] In some embodiments, after the second laser treatment and / or the first laser treatment, the cell 100 undergoes a stabilization post-treatment. The stabilization post-treatment method includes subjecting the cell 100 to at least one of ultraviolet irradiation, heat treatment, and laser treatment in an inert gas environment. The inert gas includes at least one of nitrogen or argon. This stabilization post-treatment is used to further stabilize the passivation performance of the passivation layer and prevent oxidation and degradation of the passivation layer in subsequent processes. Using an inert gas environment helps avoid oxidation of the passivation layer due to contact with oxygen during the post-treatment process. This application does not limit the specific method of the stabilization post-treatment.
[0099] The process parameters of the third laser treatment, cutting treatment, second laser treatment, and first laser treatment in this application are related, and the parameters of each process can be matched and adjusted accordingly. For example, the flatter and lower the heat-affected zone formed on the cutting section 102 by the cutting treatment, the better the uniformity of the cross-sectional passivation layer 200 subsequently formed on the cutting section 102. The first laser treatment can achieve stable passivation performance of the cross-sectional passivation layer 200 at a lower power or a higher scanning speed. The greater the coating thickness and the denser the film of the cross-sectional passivation layer 200, the greater the power and the lower the scanning speed required for the first laser treatment within a certain range. The power, scanning speed, and second voltage of the second laser treatment can be matched and adjusted according to the processing results of the third laser treatment and the thermal history of the cross-sectional passivation layer 200 deposition process, so that the degree of contact degradation repaired by the second laser treatment is compatible with the degree of damage introduced by the previous process. This allows the laser parameters of the four processes to be set in a correlated manner along the process chain, avoiding deviations in the parameters of a certain process from the actual state of the preceding process. This is beneficial for balancing the stability of contact repair and cross-sectional passivation activation at the overall process chain level.
[0100] The preparation method described above, which includes third laser processing, cutting processing, second laser processing, and first laser processing, firstly uses a third laser to laser-assisted sinter the slurry electrode to form an ohmic contact before forming the cross-sectional passivation layer 200. After cutting and forming the cross-sectional passivation layer 200, the second laser is used to perform secondary contact repair on the electrode, and the first laser is used to independently thermally activate the cross-sectional passivation layer 200. Thus, the gate contact resistance repair, passivation layer thermal annealing, and cross-sectional passivation film activation are achieved simultaneously in the same process chain. At the same time, by using the method of covering multiple cutting sections 102 at one time with the first spot after stacking multiple slab cells 100, the processing is expanded from piece-by-piece to batch processing, which improves the photoelectric conversion efficiency of the slab cells 100 while also taking into account the batch processing efficiency.
[0101] Accordingly, another embodiment of this application also provides a photovoltaic cell. This photovoltaic cell can be prepared using the photovoltaic cell preparation method of any of the above embodiments. For parts that are the same as or corresponding to the foregoing preparation method embodiments, please refer to the corresponding descriptions of the foregoing embodiments, which will not be repeated below.
[0102] Reference Figure 2 As shown, in some embodiments, the photovoltaic cell 30 includes a segmented cell 100 and a cross-sectional passivation layer 200. The segmented cell 100 has opposing segmented surfaces 101 and a cut cross-section 102 connecting the segmented surfaces 101; the cross-sectional passivation layer 200 is disposed on the cut cross-section 102. Since the cross-sectional passivation layer 200 is disposed on the cut cross-section 102, it can passivate dangling bonds, surface states, or other interface defects at the cut cross-section 102; and since the photovoltaic cell 30 can be obtained through the aforementioned batch first laser processing, the film state and interface bonding quality of the cross-sectional passivation layer 200 are improved, thereby helping to reduce carrier recombination at the cut cross-section 102 and improve the photoelectric conversion efficiency and edge reliability of the photovoltaic cell 30.
[0103] In some embodiments, the cross-section passivation layer 200 covers the cut cross-section 102 and extends to at least a portion of the segmented surface 101 adjacent to the cut cross-section 102. This structure enables a continuous passivation coverage at the junction of the cut cross-section 102 and the segmented surface 101, reducing the risk of composite concentration areas forming at the junction due to cutting damage or film interruption.
[0104] In some embodiments, the photovoltaic cell 30 further includes electrodes disposed on the slab surface 101. The electrodes can be formed by a third laser process, or they can be repaired by a second laser process after the formation of the cross-section passivation layer 200. By having the electrodes and the cross-section passivation layer 200 processed within corresponding process windows, both electrode contact reliability and passivation quality of the cut cross-section 102 can be achieved.
[0105] Accordingly, one embodiment of this application also provides a tandem solar cell, which uses the photovoltaic cell provided in any of the above embodiments, or the photovoltaic cell formed by the preparation method of the photovoltaic cell provided in any of the above embodiments, as the crystalline silicon base cell. For parts that are the same as or corresponding to the foregoing embodiments, please refer to the corresponding descriptions of the foregoing embodiments; detailed descriptions will not be repeated below.
[0106] Reference Figure 6 As shown, Figure 6 This is a schematic diagram of the structure of a stacked battery provided in an embodiment of this application. The stacked battery includes a crystalline silicon bottom cell 10 and a perovskite top cell 20. The crystalline silicon bottom cell 10 is the photovoltaic cell 30 in any of the foregoing embodiments, or the crystalline silicon bottom cell 10 is a photovoltaic cell prepared by the preparation method of the photovoltaic cell in any of the foregoing embodiments. The perovskite top cell 20 is located on one side of the crystalline silicon bottom cell 10.
[0107] Reference Figure 7 As shown, Figure 7 This is another schematic diagram of the structure of the stacked solar cell provided in an embodiment of this application. In some embodiments, the perovskite top solar cell 20 may include: a first transport layer 21, a perovskite functional layer 22, a second transport layer 23, a transparent conductive layer 24, and an anti-reflection layer 25 stacked together. The first transport layer 21 is directly opposite the crystalline silicon bottom solar cell 10.
[0108] In some examples, the first transport layer 21 can be one of an electron transport layer and a hole transport layer, and the second transport layer 23 can be the other of an electron transport layer and a hole transport layer.
[0109] In some embodiments, the bandgap width of the perovskite top cell 20 is greater than that of the crystalline silicon bottom cell 10. Therefore, stacking the perovskite top cell 20 on top of the crystalline silicon bottom cell 10 can give the stacked cell a wider spectral response range, further improving the utilization rate of sunlight and the efficiency of the cell.
[0110] In some embodiments, the tandem solar cell may further include an intermediate connecting layer (not shown) for electrically connecting the crystalline silicon bottom cell 10 and the perovskite top cell 20.
[0111] In some embodiments, the intermediate connection layer is generally a tunnel junction or a very thin metal or transparent electrode composite layer. Optionally, the intermediate connection layer can be a transparent conductive oxide, which has good optoelectronic properties, high photon transmittance and high conductivity, thereby enabling the perovskite top cell 20 and the crystalline silicon bottom cell 10 to maintain good ohmic contact.
[0112] In some embodiments, the tandem solar cells can be configured as a 2T (two-terminal series / two-terminal stacked) structure or a 4T (four-terminal series / four-terminal stacked) structure. The tandem solar cells can also be configured as a 3T (three-terminal series / three-terminal stacked) structure. The three-terminal stacked structure is mainly used in tandem solar cells manufactured by combining photovoltaic cell 30 with perovskite top cell 20, which produces three electrodes. In the four-terminal stacked solar cell, the two sub-cells are manufactured independently, and they are only optically connected; their circuits are independent. It can be understood that the perovskite top cell 20 and the crystalline silicon bottom cell 10 are merely physically stacked, and in reality, they each output independently. Therefore, the four-terminal stacked solar cell will have two positive electrodes and two negative electrodes.
[0113] Accordingly, in another aspect, this application also provides a photovoltaic module, which includes the photovoltaic cell described in any of the above embodiments, the photovoltaic cell prepared by the preparation method of the photovoltaic cell in any of the embodiments, or the tandem cell described in the above embodiments. It should be noted that the parts that are the same as or corresponding to the foregoing embodiments can be referred to the corresponding descriptions of the foregoing embodiments, and will not be repeated below.
[0114] Figure 8 This is a partial structural diagram of a cell string in a photovoltaic module provided in an embodiment of this application. Figure 9 This is a partial cross-sectional schematic diagram of a photovoltaic module provided in an embodiment of this application.
[0115] Reference Figure 8 and Figure 9 As shown, the photovoltaic module includes: a cell string, which is formed by connecting multiple photovoltaic cells 30 as described above, or by connecting photovoltaic cells prepared by the method of preparing photovoltaic cells according to any of the above embodiments, or by connecting multiple stacked cells as described in the above embodiments. The photovoltaic module also includes an encapsulation layer 31 and a cover plate 32; the encapsulation layer 31 is used to cover the surface of the cell string; the cover plate 32 is used to cover the surface of the encapsulation layer 31 facing away from the cell string.
[0116] In some embodiments, photovoltaic cells 30 can be electrically connected in the form of whole cells or segmented cells to form multiple cell strings, and the multiple cell strings are electrically connected in series and / or parallel. A segmented solar cell refers to a cell formed by cutting a complete whole cell. Segmented cells can be two-segmented cells, three-segmented cells, or four-segmented cells, etc.
[0117] Multiple photovoltaic cells 30 can be electrically connected through solder strips 33.
[0118] In some embodiments, the encapsulation layer 31 includes a first encapsulation sublayer and a second encapsulation sublayer. The first encapsulation sublayer covers one of the front and back sides of the photovoltaic cell 30, and the second encapsulation sublayer covers the other of the front and back sides of the photovoltaic cell 30. Specifically, at least one of the first and second encapsulation sublayers can be an organic encapsulation layer 31 such as polyvinyl butyral (PVB) film, ethylene-vinyl acetate copolymer (EVA) film, polyvinyl octene coelastomer (POE) film, or polyethylene terephthalate (PET) film. Alternatively, at least one of the first and second encapsulation sublayers can also be an EP film, EPE film, or PEP film. Among them, EP film refers to a co-extruded film composed of stacked EVA film and POE film; EPE film refers to a co-extruded film formed by sequentially stacking EVA film, POE film, and EVA film; and PEP film refers to a co-extruded film formed by stacking POE film, EVA film, and POE film. Co-extruded films can be prepared by sequentially extruding one or more raw materials onto another pre-made film during the film processing, or by bonding different types of pre-made films together.
[0119] In some cases, the first encapsulation sublayer and the second encapsulation sublayer still have a boundary line before lamination. After lamination, the photovoltaic module will no longer have the concept of the first encapsulation sublayer and the second encapsulation sublayer. That is, the first encapsulation sublayer and the second encapsulation sublayer have formed an integral encapsulation layer 31.
[0120] In some embodiments, the cover plate 32 can be a glass cover plate 32, a plastic cover plate 32, or other cover plate 32 with light-transmitting function. Specifically, the surface of the cover plate 32 facing the encapsulation layer 31 can be an uneven surface or a textured surface containing multiple raised structures, thereby increasing the utilization rate of incident light. The cover plate 32 may include a first cover plate and a second cover plate, the first cover plate being opposite to the first encapsulation sublayer, and the second cover plate being opposite to the second encapsulation sublayer.
[0121] Those skilled in the art will understand that the above embodiments are specific implementations of this application, and in practical applications, various changes in form and detail can be made without departing from the spirit and scope of this application. Any person skilled in the art can make various alterations and modifications without departing from the spirit and scope of this application; therefore, the scope of protection of this application should be determined by the scope defined in the claims.
Claims
1. A method for preparing a photovoltaic cell, characterized in that, include: Obtain battery cells; The battery cell is cut into at least two battery segments, each battery segment having opposing segments and a cut section connecting the segments. A cross-section passivation layer is formed at the cut cross-section; Multiple cell wafers are stacked and arranged along a first direction, such that the cut sections of the multiple cell wafers face the same direction; the first direction is the thickness direction of the cell wafers. The cut cross-section is subjected to a first laser treatment, in which the first laser irradiates the passivation layer of the cross-section, and the first spot of the first laser covers at least a portion of the surface of at least two of the cut cross-sections.
2. The method for preparing a photovoltaic cell according to claim 1, characterized in that, During the first laser processing, the first light spot covers at least a portion of the surface of the plurality of cut sections, and the first light spot is displaced from one end of the cut section to the other end along a second direction; the second direction is a direction that intersects with the first direction.
3. The method for preparing a photovoltaic cell according to claim 1, characterized in that, The size of the first light spot in the first direction is greater than or equal to the sum of the thicknesses of the two segmented cells, and the size of the first light spot in the first direction is 0.3 mm to 2 mm; And / or, the energy density of the first laser is 0.3 J / cm². 2 Up to 2J / cm 2 ; And / or, the scanning speed of the first laser is from 500 mm / s to 7000 mm / s.
4. The method for preparing a photovoltaic cell according to claim 1, characterized in that, The thickness of the cross-sectional passivation layer is 45 nm to 60 nm.
5. The method for preparing a photovoltaic cell according to any one of claims 1 to 4, characterized in that, Also includes: After the cross-sectional passivation layer is formed and before the plurality of the segmented cells are stacked, a second laser treatment is performed, in which the segmented surface is irradiated with a second laser.
6. The method for preparing a photovoltaic cell according to claim 5, characterized in that, The spot size of the second laser is 10 μm to 500 μm; And / or, the energy density of the second laser is from 1 J / cm² to 30 J / cm².
7. The method for preparing a photovoltaic cell according to claim 1, characterized in that, Before the step of forming the passivation layer on the cut section, the cut section is oxidized to form an oxide layer on the cut section.
8. A photovoltaic cell, characterized in that, The photovoltaic cell is prepared by the method of any one of claims 1 to 7, wherein the photovoltaic cell comprises: The cell is a segmented battery having opposing segmented surfaces and a cut section connecting the segmented surfaces. A cross-section passivation layer is disposed on the cut cross-section.
9. A stacked battery, characterized in that, include: A crystalline silicon bottom cell, wherein the crystalline silicon bottom cell is a photovoltaic cell prepared by the photovoltaic cell preparation method according to any one of claims 1 to 7, or the crystalline silicon bottom cell is the photovoltaic cell according to claim 8; a perovskite top cell, wherein the perovskite top cell is located on one side of the crystalline silicon bottom cell.
10. A photovoltaic module, characterized in that, include: A battery string, comprising: a plurality of photovoltaic cells formed by the method of preparing photovoltaic cells as described in any one of claims 1 to 7; or a plurality of photovoltaic cells as described in claim 8; or a plurality of stacked cells as described in claim 9. A solder strip, which is electrically connected to at least two of the photovoltaic cells to connect adjacent photovoltaic cells in series; Encapsulation layer, the encapsulation layer being used to cover the surface of the battery string; A cover plate for covering the surface of the encapsulation layer away from the battery string.