Solar cells and their fabrication methods, photovoltaic modules
By introducing a silver source and a reducing sintering aid of organic carboxylic acids/alkyl thiols into the low-temperature silver paste, the problems of high grid resistivity and microcracks in traditional low-temperature silver pastes were solved, achieving efficient interfacial fusion between silver particles at low temperatures and improving the electrical and mechanical properties of solar cells.
Patent Information
- Application Number
- CN202611390272.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional low-temperature silver paste has a high grid line volume resistivity, which cannot reach the level of high-temperature sintered silver paste. Furthermore, microcracks and insufficient welding tensile strength are prone to occur during the low-temperature sintering process.
By using a combination of silver source and reducing sintering aids of organic carboxylic acids/alkyl thiols, highly active nano-silver particles are generated through in-situ decomposition at low temperatures. Organic carboxylic acids and alkyl thiols are used to reduce the oxide layer on the surface of silver powder, exposing a fresh active metal surface. A protective film is formed to prevent secondary oxidation. Organic carboxylic acids and alkyl thiols with a specific number of carbon atoms leave trace atoms at the grain boundaries to release thermal stress and promote interfacial fusion between silver particles.
The volume resistivity of the grid line is significantly reduced to near the high-temperature sintering level under low temperature conditions of 150℃~250℃, avoiding microcracks and insufficient welding tensile strength, and improving the mechanical and electrical reliability of the electrode.
Smart Images

Figure CN123124493A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of batteries, and in particular to solar cells and their preparation methods, and photovoltaic modules. Background Technology
[0002] Traditional low-temperature silver pastes generally use resin-curing formulations, which consist of a matrix resin binder phase, a conductive functional phase, organic solvents, and other additives. Summary of the Invention
[0003] This application provides a solar cell and its preparation method, as well as a photovoltaic module, which at least helps to improve the volume resistivity of the grid lines.
[0004] The first aspect of this application provides a method for preparing a solar cell, the method comprising: coating a conductive material containing an additive onto at least one surface of a solar cell body, and curing it to form grid lines to obtain a solar cell; The auxiliary agent includes a silver source and a reducing agent, wherein the reducing agent includes organic carboxylic acids and / or alkyl thiols; the organic carboxylic acids include organic carboxylic acids with a carbon number of C2 to C20, and the alkyl thiols include alkyl thiols with a carbon number of C8 to C18.
[0005] Optionally, the organic carboxylic acid includes organic carboxylic acids with C8 to C18 carbon atoms, and the alkyl thiol includes alkyl thiols with C12 to C18 carbon atoms.
[0006] Further optionally, the organic carboxylic acid is selected from at least one of phthalic acid, octanoic acid and oleic acid, and the alkyl thiol is selected from at least one of dodecyl thiol, hexadecyl thiol and octadecyl thiol.
[0007] Optionally, the silver source includes an organosilver compound, the decomposition temperature of which is 120°C to 250°C, and the organosilver compound includes silver carboxylate and / or silver complexes.
[0008] Further optionally, the silver carboxylate includes silver oxalate, and the silver complex includes silver citrate complex and / or silver-amine complex.
[0009] Optionally, the conductive material further includes a conductive phase, which comprises a first spherical powder, a second spherical powder, and a flake-shaped powder, wherein the D50 particle size of the first spherical powder is smaller than the D50 particle size of the second spherical powder.
[0010] Further optionally, when the conductive phase comprises a silver-copper alloy and / or a silver-nickel alloy, the reducing agent comprises an organic carboxylic acid and an alkyl thiol, and the mass ratio of the organic carboxylic acid to the alkyl thiol is (0.5~5):1.
[0011] Optionally, before curing to form grid lines, the conductive material coated on the surface of the solar cell body is dried three times in sequence. The temperature of the first drying is lower than that of the second drying, and the temperature of the second drying is lower than that of the third drying. The second drying is carried out in an inert atmosphere, and the third drying is carried out in a vacuum environment.
[0012] A second aspect of this application provides a solar cell obtained according to the preparation method described above, the solar cell comprising: a solar cell body and grid lines located on at least one side surface of the solar cell body.
[0013] A third aspect of this application provides a photovoltaic module, including a battery string, the battery string including a plurality of solar cells as described above arranged along a first direction, and the plurality of battery strings also arranged along a second direction; A solder strip extending along a first direction and arranged along a second direction, the solder strip being used to connect two adjacent solar cells or two stacked cells along the first direction; A backplate, located on the side of the solder strip away from the back of the battery string.
[0014] The technical solution provided in this application has at least the following advantages: This invention introduces a reducing sintering aid combination of "silver source + organic carboxylic acid and / or alkyl thiol" into the additive system of conductive materials. During sintering, the silver source decomposes in situ to generate highly active nano-silver particles that fill the gaps between silver powder particles as additional nucleation sites. Meanwhile, the organic carboxylic acid and / or alkyl thiol with a specific number of carbon atoms reduce the oxide layer on the surface of the silver powder under heating conditions, exposing a fresh active metal surface. At the same time, it utilizes its "film protection" to prevent secondary oxidation and its unique function of "controlled decomposition" to leave trace atoms at the grain boundaries to release thermal stress. This achieves a significant reduction in sintering activation energy and promotes interfacial fusion between silver particles at low temperatures of 150℃~250℃, reducing the volume resistivity of the gate line to near the level of high-temperature sintering. Attached Figure Description
[0015] One or more embodiments are illustrated by way of example with reference to the accompanying drawings. These illustrations do not constitute a limitation on the embodiments. Unless otherwise stated, the drawings in the accompanying drawings do not constitute a limitation on scale. In order to more clearly illustrate the technical solutions in the embodiments of this application or in the conventional art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0016] Figure 1This is a flowchart of the method for preparing a solar cell according to an embodiment of this application; Figure 2 This is a schematic diagram of the structure of the photovoltaic module in the embodiments of this application.
[0017] Figure Labels 100. Battery string; 101. Solar cell; 120. Backsheet; 4. Solder strip. Detailed Implementation
[0018] In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly specified.
[0019] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0020] The embodiments of this application will now be described in detail with reference to the accompanying drawings. However, those skilled in the art will understand that many technical details have been provided in the embodiments of this application to facilitate a better understanding of the application. However, the technical solutions claimed in this application can be implemented even without these technical details and various variations and modifications based on the following embodiments.
[0021] As can be seen from the background technology, the volume resistivity of electrodes prepared by traditional low-temperature curing silver paste is 2 to 3 times higher than that of high-temperature sintered silver paste.
[0022] Firstly, this application provides a method for preparing a solar cell, such as... Figure 1 As shown, the preparation method includes the following steps: S1. A solar cell body and a conductive material containing additives are provided, wherein the additives include a silver source and a reducing agent, the reducing agent includes an organic carboxylic acid and / or an alkyl thiol; the organic carboxylic acid includes organic carboxylic acids with a carbon number of C2 to C20, and the alkyl thiol includes alkyl thiols with a carbon number of C8 to C18.
[0023] S2. The conductive material containing the additive is coated on at least one side surface of the solar cell body and cured to form grid lines to obtain a solar cell.
[0024] During the sintering process, the silver source decomposes in situ to generate highly active nano-silver particles that fill the gaps between silver powder particles as additional nucleation sites. Meanwhile, organic carboxylic acids and / or alkyl thiols reduce the oxide layer on the surface of the silver powder and expose fresh active metal surfaces under heating conditions. At the same time, they utilize their "film protection" to prevent secondary oxidation and their unique function of "controlled decomposition" to leave trace atoms at the grain boundaries to release thermal stress. This achieves a significant reduction in sintering activation energy and promotes interfacial fusion between silver particles at low temperatures of 150℃~250℃, reducing the volume resistivity of the gate line to near the level of high-temperature sintering.
[0025] The organic carboxylic acid can have C2~C7, C8~C18, C19~C20 carbon atoms, for example, C2, C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18, C19 or C20; the alkyl thiol can have C8~C11, C12~C18 carbon atoms, for example, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17 or C18. Choosing C2-C20 organic carboxylic acids and C8-C18 alkyl thiols represents the optimal balance among several interdependent factors: 1. Providing sufficient steric hindrance to prevent silver powder agglomeration and ensure paste stability; 2. Complete decomposition or desorption within the low-temperature sintering window to achieve "zero residue," a necessary condition for obtaining a pure silver-silver interface; 3. Decomposition products (such as sulfur atoms) can play a beneficial "grain boundary lubrication" role, improving the mechanical and electrical reliability of the electrodes. It is this synergistic effect achieved through precise molecular design that allows the final grid line volume resistivity to be as low as that of high-temperature sintered silver paste, while avoiding damage to the solar cell caused by high-temperature processes.
[0026] In some embodiments, the solar cell body can be a heterojunction solar cell, a perovskite / silicon tandem solar cell, or a tunnel oxide passivated contact (TOPCon) solar cell.
[0027] In some embodiments, the reducing agent includes alkyl thiols.
[0028] In traditional understanding, during the sintering and cooling process of double-layer printing (seed layer + copper paste), the mismatch in the coefficients of thermal expansion (CTE) between silver and the underlying silicon substrate easily leads to microcracks at the root of the gate lines, resulting in insufficient solder pull strength. However, the trace sulfur (S) atoms left at the silver grain boundaries after the decomposition of alkyl thiols (such as dodecyl thiols) act as a "grain boundary lubricant," absorbing some of the thermal stress during cooling. This results in higher density and enhanced flexibility of the sintered seed layer gate lines, effectively eliminating microcracks.
[0029] In some embodiments, the organic carboxylic acid includes organic carboxylic acids having a carbon number of C8 to C18, and the alkyl thiol includes alkyl thiols having a carbon number of C12 to C18.
[0030] In some embodiments, the organic carboxylic acid is selected from at least one of phthalic acid, octanoic acid, and oleic acid, and the alkyl thiol is selected from at least one of dodecyl thiol, hexadecyl thiol, and octadecyl thiol.
[0031] In some embodiments, the silver source comprises an organosilver compound, the decomposition temperature of which is 120°C to 250°C. The decomposition temperature can be 120°C to 140°C, 140°C to 160°C, or 160°C to 250°C, for example, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, or 250°C. The organosilver compound comprises silver carboxylate and / or silver complexes.
[0032] In some embodiments, the silver carboxylate comprises silver oxalate, and the silver complex comprises silver citrate complex and / or silver-amine complex.
[0033] In some embodiments, based on the total mass of the conductive material as 100%, the content of the silver source is 0.05% to 0.8%, and the content of the reducing agent is 0.05% to 0.7%.
[0034] In some embodiments, the conductive material further includes a conductive phase comprising a first spherical powder, a second spherical powder, and a flake-like powder, wherein the D50 particle size of the first spherical powder is smaller than the D50 particle size of the second spherical powder.
[0035] In some embodiments, the content of the conductive phase is 75% to 88% based on the total mass of the conductive material being 100%.
[0036] In some embodiments, based on the total mass of the conductive phase as 100%, the content of the first spherical powder is 10% to 25%, the content of the second spherical powder is 50% to 70%, and the content of the flake powder is 5% to 25%.
[0037] Adding too much of the first spherical powder will lead to an abnormally high viscosity of the slurry and a decrease in printability, while adding too little will prevent the effective construction of low-temperature conductive pathways. Adding too much of the second spherical powder will result in an excessively high solid content in the slurry, leading to poor ink penetration and difficulty in controlling fine grid linewidth, while adding too little will result in an incomplete three-dimensional conductive framework, an increased percolation threshold, and increased resistivity. Adding too much of the flake powder will result in excessive cohesion in the slurry, leading to decreased ink permeability and easy screen clogging, while adding too little will result in insufficient surface contact conductive pathways and limited reduction in contact resistance.
[0038] In some embodiments, the first spherical powder is nano-spherical silver powder, and the second spherical powder is submicron spherical silver powder.
[0039] Nano-spherical silver powder can rapidly form conductive pathways below 200℃ due to its high specific surface area. Submicron silver powder acts as a skeleton filler to reduce porosity, while flake silver powder effectively reduces contact resistance through surface contact mechanism. The synergistic effect of the three makes the conductive network denser and significantly reduces resistivity.
[0040] In some embodiments, when the conductive phase comprises a silver-copper alloy and / or a silver-nickel alloy, the reducing agent comprises an organic carboxylic acid and an alkyl thiol, and the mass ratio of the organic carboxylic acid to the alkyl thiol is (0.5~5):1. This mass ratio can be (0.5~1):1, (1~2):1, or (2~5):1, for example, 0.5:1, 1:1, 2:1, 3:1, 4:1, or 5:1. The silver content in the silver-copper alloy or silver-nickel alloy is 15wt%~50wt%.
[0041] Traditionally, incorporating nickel or copper powder into low-silver-content formulations typically leads to a sharp increase in volume resistivity because these base metals are highly susceptible to oxidation, forming an insulating layer. However, organic carboxylic acids and alkyl thiols preferentially "protect" and reduce the nickel / copper oxide layer on the base metal powder surface during heating, exposing a fresh metal interface. This means that silver-copper alloys and / or silver-nickel alloys are no longer merely "inert cores" encased in silver, but truly participate in the eutectic bonding of the sintering neck, ultimately effectively reducing the volume resistivity of the gate lines.
[0042] In some embodiments, the first spherical powder has a D50 particle size of 50nm~200nm and a specific surface area of 5m². 2 / g~15m 2 / g of silver powder; the second spherical powder has a D50 particle size of 0.5μm~2μm and a specific surface area of 1m². 2 / g~2.5m 2 / g of silver powder; the flaky powder has a D50 particle size of 0.5μm~3μm, an aspect ratio ≥10, and a specific surface area of 0.5m². 2 / g~2m 2 / g of silver powder.
[0043] Nano-spherical silver powder with specific D50 particle size and specific surface area is used. Its high surface activity and low sintering activation energy allow for rapid particle interconnection via surface diffusion at temperatures below 200℃, forming a dense conductive network. Submicron-sized spherical silver powder with specific D50 particle size and specific surface area is also incorporated. This serves as the main conductive filler, constructing a three-dimensional conductive framework and reducing the percolation threshold. Combined with the nano-silver powder, it creates a graded filling effect of varying particle sizes, significantly reducing porosity after sintering and increasing the density of the conductive network. Finally, flake-shaped silver powder with specific D50 particle size and specific surface area is added. During sintering, it conducts electricity through surface contact rather than traditional point contact, significantly reducing contact resistance. The flake morphology also facilitates a higher aspect ratio for fine grids during printing, supporting narrow linewidth printing. The synergistic effect of these three components results in a denser conductive network and a significant reduction in resistivity.
[0044] In some embodiments, the conductive material further includes resin, organic solvent and additives, wherein the resin content is 8% to 18% based on the total mass of the conductive material (100%), the organic solvent content is 3% to 8%, and the additive content is 0.5% to 2.5%.
[0045] In some embodiments, the resin comprises a thermosetting epoxy resin and a thermoplastic polyester resin in a mass ratio of (0.5~1.2):1, wherein the epoxy equivalent of the thermosetting epoxy resin is 180 g / eq~500 g / eq, and the number average molecular weight of the thermoplastic polyester resin is 5000~20000. The thermosetting epoxy resin undergoes a cross-linking and curing reaction under heating conditions to form a three-dimensional network structure, providing a strong bond and fixation for the silver powder particles; the thermoplastic polyester resin softens and flows during solvent evaporation and heating, wetting the surface of the silver powder particles, and then solidifies upon cooling to form a flexible skeleton, compensating for the insufficient flexibility of the epoxy resin. The purpose of controlling the epoxy equivalent of the thermosetting epoxy resin within the range of 180 g / eq to 500 g / eq is primarily to ensure that the resin has a suitable crosslinking density. Too low an epoxy equivalent results in excessive crosslinking and high brittleness after curing; too high an epoxy equivalent results in insufficient crosslinking and inadequate bond strength. Controlling the number-average molecular weight of the thermoplastic polyester resin within the range of 5000 to 20000 ensures good solubility and suitable melt flowability in solvents. Too low a molecular weight results in poor film-forming properties and insufficient flexibility; too high a molecular weight leads to difficulty in dissolving and excessive slurry viscosity. The mass ratio of the two resins is controlled within the range of (0.5 to 1.2):1. At this ratio, the epoxy resin provides sufficient bond strength and heat resistance, while the polyester resin imparts good printability and flexibility to the slurry, preventing brittleness after fine grid curing.
[0046] In some embodiments, the thermosetting epoxy resin can be a conventional thermosetting epoxy resin in the art, as long as it satisfies the functions described above. For example, the thermosetting epoxy resin is selected from bisphenol A type epoxy resin and / or bisphenol F type epoxy resin.
[0047] In some embodiments, the thermoplastic polyester resin can be a conventional thermoplastic polyester resin in the art, as long as it satisfies the functions described above. For example, the thermoplastic polyester resin is selected from saturated polyester resin or polyurethane-modified polyester resin.
[0048] In some embodiments, the organic solvent includes diethylene glycol butyl ether acetate, terpineol, and dimethyl adipate, wherein the mass ratio of diethylene glycol butyl ether acetate, terpineol, and dimethyl adipate is (4~6):(2~4):(1~2).
[0049] In some embodiments, the additive includes a thixotropic agent, a dispersant, and a coupling agent. The mass ratio of the thixotropic agent, dispersant, and coupling agent is (0.5~2):(0.1~1):1.
[0050] In some embodiments, the thixotropic agent is selected from at least one of polyamide wax, hydrogenated castor oil derivatives, and fumed silica. The thixotropic agent imparts shear-thinning properties to the paste, giving it good flowability during screen printing and allowing it to quickly regain its high viscosity after printing to maintain fine grid lines.
[0051] In some embodiments, the dispersant is selected from polymeric dispersants with anchoring groups, such as BYK-111, BYK-112, or the Solsperse 30000 series. The dispersant prevents silver powder particle agglomeration by forming a steric hindrance layer on the silver powder surface, thereby improving the storage stability of the paste and the uniformity of printing.
[0052] In some embodiments, the coupling agent is selected from silane coupling agents (such as KH-550, KH-560) to improve the interfacial compatibility between silver powder and organic resin and increase the bonding strength.
[0053] In some embodiments, the preparation process of the conductive material containing the additives includes the following steps: (1) Weigh the conductive phase (first spherical powder, second spherical powder and flake powder) according to the ratio, and dry it in a vacuum drying oven at 80℃~120℃ for 2h~4h to remove the surface adsorbed moisture and volatile impurities. The dried conductive phase is then passed through a 200-mesh sieve for later use. (2) Preparation of organic carrier: The resin, organic solvent and dispersant and coupling agent in the additive are added to the reaction vessel according to the ratio, and stirred and dissolved at 60℃~90℃ for 1h~2h until the resin is completely dissolved to form a transparent and uniform organic carrier solution; then, after cooling to room temperature, the thixotropic agent is added, and dispersed in a high-speed disperser at 1000rpm~2000rpm for 15min~30min to fully activate the thixotropic agent to form a thixotropic structure and obtain the organic carrier; (3) Initial mixing of slurry: The conductive phase is added to the organic carrier in batches. After each batch is added, the mixture is stirred at a low speed of 500 rpm to 800 rpm for 5 min to 10 min to fully wet the silver powder with the organic carrier and obtain the initial mixed slurry. (4) Three-roll milling and dispersion: The initially mixed slurry is transferred to a three-roll mill for grinding and dispersion. The grinding gap is gradually adjusted from the initial 50μm to 20μm and 10μm. The slurry is ground 3 to 5 times until the fineness of the slurry is ≤8μm. (5) Addition and mixing of sintering aids: Add the silver source and reducing agent (organic carboxylic acid and / or alkyl thiol) to the slurry after grinding in batches, and stir at a low speed of 300 rpm to 500 rpm for 15 min to 30 min to ensure that the sintering aids are evenly distributed in the slurry; (6) Vacuum degassing: Place the uniformly mixed slurry in a vacuum degassing machine and degas for 15 min to 30 min under vacuum degree ≤ -0.09MPa and temperature 25℃~35℃ to remove entrained air bubbles in the slurry; (7) Filtration and packaging: The deaerated slurry is filtered through a 200-400 mesh stainless steel filter screen to remove impurities or large agglomerates that may be introduced during the grinding process. After packaging, the finished low-temperature sintering fine grid slurry is obtained.
[0054] In some embodiments, before curing to form grid lines, the conductive material coated on the surface of the solar cell body is dried three times in sequence. The temperature of the first drying is lower than that of the second drying, the temperature of the second drying is lower than that of the third drying, the second drying is carried out in an inert atmosphere, and the third drying is carried out in a vacuum environment.
[0055] The solvent in the slurry evaporates at a higher rate at the edges than in the center, triggering capillary flow that carries silver particles to the edges of the grid lines. This results in a U-shaped grid line cross-section after drying (thicker at the edges and thinner in the middle), which not only reduces the grid line aspect ratio but also causes microcracks due to stress concentration at the edges. If the heating rate is too fast, the high-boiling-point solvent inside the slurry vaporizes and expands instantaneously, breaking through the uncured surface resin and forming pinholes, bubbles, or causing grid line breakage. The three-stage microenvironment gradient drying method of this invention is not a simple segmented heating process, but rather a precise intervention in the solvent evaporation rate and resin gelation process through three-dimensional coupling control of the "temperature field-atmosphere field-pressure field," thereby eliminating the above-mentioned defects at their source.
[0056] In some embodiments, the first drying is carried out in air, and the conditions for the first drying include: a temperature of 50°C to 80°C, a relative humidity of 40% to 60%, and a time of 2 to 5 minutes.
[0057] Anti-coffee ring mechanism: This stage employs a low-temperature, high-humidity microenvironment. The relative humidity (RH) is maintained at 40%–60%, significantly reducing the vapor pressure difference between the solvent on the slurry surface and the environment, resulting in extremely slow evaporation of the low-boiling-point solvent on the surface. This "slow evaporation" strategy suppresses the evaporation rate gradient between the grid edge and the central region, weakening Marangoni flow at its source and preventing excessive silver powder particles from being carried to the edges. Anti-boiling mechanism: Low temperature conditions ensure uniform internal temperature of the slurry, preventing the internal solvent from vaporizing due to local overheating, thus laying a safe foundation for subsequent heating.
[0058] In some embodiments, the second drying is carried out under a nitrogen atmosphere, and the conditions for the second drying include: a temperature of 100°C to 130°C, a relative humidity of 30% to 50%, and a time of 3 to 8 minutes.
[0059] Anti-coffee ring mechanism: As the temperature rises to medium, the thermosetting epoxy resin begins to undergo a partial pre-crosslinking reaction (B-stage), and the overall viscosity of the slurry increases significantly, gradually "freezing" the thixotropic structure. Since the slurry has lost its fluidity at this point, even with a slight temperature difference, the silver powder particles are anchored in their current position and cannot migrate, thus completely terminating the formation process of the "coffee ring".
[0060] Anti-boiling mechanism: Nitrogen gas is introduced as a protective atmosphere during this stage, and the relative humidity is controlled at 30%~50% to ensure that the solvent (mainly medium-boiling solvents such as diethylene glycol butyl ether acetate) diffuses from the interior to the surface and escapes at a relatively stable rate, rather than boiling violently. At the same time, the nitrogen atmosphere effectively prevents the polyester resin from oxidizing and yellowing at high temperatures.
[0061] In some embodiments, the third drying is carried out under vacuum / reduced pressure conditions, including a temperature of 140°C to 160°C, a vacuum degree of ≤-0.09MPa, and a time of 2 min to 5 min.
[0062] Anti-boiling mechanism: This stage is the most critical innovation of this process. A vacuum or reduced-pressure environment (vacuum degree ≤ -0.09MPa) is used, effectively lowering the boiling point of residual high-boiling-point solvents (such as terpineol, with a normal-pressure boiling point of approximately 220℃). By applying negative pressure at 140℃~160℃, the residual solvent can achieve a smooth "cold boiling" escape without increasing the temperature. Because this process is under negative pressure and the temperature is already stable, the solvent escape process is extremely gentle and uniform, completely avoiding the damage to the grid morphology caused by the instantaneous "boiling" of the solvent at normal-pressure high temperatures.
[0063] Densification effect: The complete removal of solvent eliminates the pore defects inside the electrode after curing. At the same time, the thermoplastic polyester resin melts and flows completely at this temperature, filling the gaps between the silver powder and making the grid line cross-section more dense and flat.
[0064] Secondly, this application provides a solar cell obtained according to the preparation method described above, the solar cell comprising: a solar cell body and grid lines located on at least one side surface of the solar cell body.
[0065] This application also provides a stacked battery, comprising: A crystalline silicon bottom cell, wherein the crystalline silicon bottom cell is the solar cell described above; A perovskite solar cell, wherein the perovskite solar cell is located on one side of the crystalline silicon substrate solar cell.
[0066] Thirdly, this application provides a photovoltaic module, such as Figure 2 As shown, it includes a battery string 100, which includes a plurality of solar cells 101 as described above arranged along a first direction X, and the plurality of battery strings 100 are also arranged along a second direction Y. Solder strip 4, which extends along the first direction X and is arranged along the second direction Y, is used to connect two adjacent solar cells 101 or two stacked cells along the first direction X. Back plate 120, the back plate 120 is located on the side of the solder strip 4 away from the back of the battery string 100.
[0067] In some embodiments, the backsheet is made of polyvinyl fluoride composite film or thermoplastic elastomer, which further isolates water vapor and oxygen, provides good electrical insulation, and provides weather resistance and corrosion resistance, enabling it to withstand harsh environments and long-term exposure to ultraviolet radiation.
[0068] In some embodiments, the backplate is made of glass, which has stronger weather resistance, a longer service life (up to 30 years or more) and better anti-PID performance.
[0069] In some implementations, the solar cells in the cell string can be either monocrystalline silicon cells (high efficiency, deep black color, typically single-cell or half-cell) or polycrystalline silicon cells (slightly lower efficiency, bright blue color, with ice-flower-like patterns), such as half-cell monocrystalline PERC cells. Multiple solar cells are connected in series via solder ribbons (tinned copper ribbons) to achieve the desired voltage.
[0070] In some implementations, photovoltaic modules also include external auxiliary structures such as frames and junction boxes. These external auxiliary structures ensure the safety and lifespan of the module during installation and use. The frame, often made of anodized aluminum alloy, protects the edges of the laminated cover and backsheet, preventing damage during installation and transportation, and providing additional mechanical strength to the entire photovoltaic module. The junction box, typically installed on the back of the backsheet, is the "power outlet" of the photovoltaic module, containing conductive electrodes to collect the direct current generated by the cell strings. In some embodiments, the junction box also contains bypass diodes. When some cell strings are shaded, these cells become power-consuming units (resistors), generating hot spots. The bypass diodes guide current around the shaded cell strings, protecting them from burnout and reducing system power generation losses.
[0071] The present application will now be described in detail through specific embodiments.
[0072] Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods in the art. Unless otherwise specified, the experimental materials used in the following embodiments are commercially available.
[0073] Preparation Example 1 This preparation example provides a method for preparing a conductive material, including the following steps: (1) 25wt% of the first spherical powder (D50 particle size of 50nm, specific surface area of 5m²) 2 / g spherical silver powder), 50wt% second spherical powder (D50 particle size of 0.5μm, specific surface area of 1m²). 2 / g spherical silver powder) and 25wt% flake powder (D50 particle size 0.5μm, aspect ratio 10, specific surface area 0.5m²) 2 Weigh the flake silver powder (g / g) according to the formula, dry it in a vacuum drying oven at 80℃ for 4 hours, and then pass the dried conductive phase (first spherical powder, second spherical powder and flake powder) through a 200-mesh sieve for later use. (2) Add the resin (the mass ratio of bisphenol A epoxy resin to saturated polyester resin is 1:1), organic solvent (the mass ratio of diethylene glycol butyl ether acetate, terpineol and dimethyl adipate is 4:2:1), and the additives BYK-111 (dispersant) and KH-550 (coupling agent) to the reactor. Stir and dissolve at 60°C for 2 hours until the resin is completely dissolved to form a transparent and uniform organic carrier solution. Then, cool to room temperature (25°C) and add polyamide wax (thixotropic agent). The mass ratio of polyamide wax, BYK-111 and KH-550 is 0.8:0.4:1. Disperse in a high-speed disperser at 1000 rpm for 30 minutes to fully activate the thixotropic agent and form a thixotropic structure to obtain the organic carrier. (3) The conductive phase is added to the organic carrier in batches. After each batch is added, the mixture is stirred at a low speed of 500 rpm for 10 min to fully wet the silver powder with the organic carrier and obtain the initial mixed slurry. (4) The initially mixed slurry is transferred to a three-roll mill for grinding and dispersion. The grinding gap is gradually adjusted from the initial 50 μm to 20 μm and 10 μm. The slurry is ground 3 times until the fineness of the slurry is 8 μm. (5) Add silver source (silver citrate complex, decomposition temperature is 200℃) and reducing agent (phthalic acid) to the ground slurry in batches, and stir at low speed of 300 rpm for 30 min to obtain a uniformly mixed slurry; Of which, based on the total mass of conductive materials as 100%, the content of conductive phase is 75%, the content of resin is 15%, the content of organic solvent is 8%, the content of additive is 1.9%, the content of silver source is 0.05%, and the content of reducing agent is 0.05%; (6) Place the well-mixed slurry in a vacuum degassing machine and degas for 30 minutes under a vacuum of -0.09 MPa and a temperature of 25°C; (7) The degassed slurry is filtered through a 200-mesh stainless steel filter screen and then packaged to obtain conductive material.
[0074] Preparation Example 2 The preparation method was carried out as in Example 1, except that the reducing agent (phthalic acid) was replaced with a reducing agent (dodecyl mercaptan).
[0075] Preparation Example 3 The preparation method was carried out as in Example 1, except that the elemental silver in both the spherical and flake silver powders in the conductive phase was replaced with a silver-copper alloy (silver content was 30 wt%), and the reducing agent (phthalic acid) was replaced with (a mixture of phthalic acid and dodecyl mercaptan, with a mass ratio of phthalic acid to dodecyl mercaptan of 2:1).
[0076] Preparation Example 4 The preparation method was carried out as in Example 1, except that the elemental silver in both the spherical and flake silver powders in the conductive phase was replaced with a silver-nickel alloy (silver content was 30 wt%), and the reducing agent (phthalic acid) was replaced with (a mixture of oleic acid and octadecyl mercaptan, with a mass ratio of oleic acid to octadecyl mercaptan of 2:1).
[0077] Preparation Example 5 The preparation was carried out in the same manner as in Example 1, except that the elemental silver in both the spherical and flake silver powders in the conductive phase was replaced with a silver-nickel alloy (silver content of 30 wt%), but phthalic acid was still used as the reducing agent.
[0078] Preparation Example 6 The preparation method was carried out as in Example 1, except that the silver source (silver citrate complex, decomposition temperature 200°C) was replaced with (silver oxalate, decomposition temperature 180°C).
[0079] Preparation Example 7 The preparation was carried out in the same manner as in Example 1, except that the silver source (silver citrate complex, decomposition temperature 200°C) was replaced with (silver-amine complex, decomposition temperature 160°C).
[0080] Preparation Example 8 The preparation method was carried out as in Example 1, except that the reducing agent (phthalic acid) was completely replaced with ascorbic acid.
[0081] Preparation Example 9 The preparation was carried out in the same manner as in Example 1, except that 25 wt% flake powder (D50 particle size 0.5 μm, aspect ratio 10, specific surface area 0.5 m²) was used. 2 All flake silver powder (g) was replaced with 25wt% of second spherical powder (D50 particle size 0.5μm, specific surface area 1m²). 2 / g spherical silver powder), finally, the conductive phase includes: 25wt% first spherical powder (D50 particle size of 50nm, specific surface area of 5m²), 2 / g spherical silver powder) and 75wt% second spherical powder (D50 particle size of 0.5μm, specific surface area of 1m²) 2 / g of spherical silver powder).
[0082] Preparation Example 10 The preparation was carried out in accordance with the method of Preparation Example 1, except that 25 wt% of the first spherical powder (D50 particle size of 50 nm and specific surface area of 5 m²) was used. 2 All of the / g spherical silver powder was replaced with 25wt% of the second spherical powder (D50 particle size of 0.5μm, specific surface area of 1m²). 2 / g spherical silver powder), finally, the conductive phase includes: 50wt% second spherical powder (D50 particle size of 0.5μm, specific surface area of 1m²), 2 / g spherical silver powder) and 25wt% flake powder (D50 particle size 0.5μm, aspect ratio 10, specific surface area 0.5m²) 2 / g of flake silver powder).
[0083] Preparation of Comparative Example 1 The preparation method was carried out as in Example 1, except that the reducing agent (phthalic acid) was completely replaced with glucose.
[0084] Preparation of Comparative Example 2 The preparation was carried out in the same manner as in Example 2, except that the reducing agent (dodecyl mercaptan) was completely replaced with hydrazine hydrate.
[0085] Preparation of Comparative Example 3 The preparation method was carried out as in Example 1, except that the reducing agent (phthalic acid) was completely replaced with erucic acid.
[0086] Preparation of Comparative Example 4 The preparation method was carried out in accordance with Example 2, except that the reducing agent (dodecyl mercaptan) was completely replaced with heptane mercaptan.
[0087] Preparation of Comparative Example 5 The preparation method was carried out in accordance with Preparation Example 2, except that the reducing agent (dodecyl mercaptan) was completely replaced with eicosyl mercaptan.
[0088] Example 1 This embodiment provides a method for preparing a solar cell, including the following steps: S1. Provide a solar cell body and the conductive material prepared in Example 1; S2. The conductive material is coated onto at least one side surface of the solar cell body, and the conductive material coated on the surface of the solar cell body is dried three times in sequence. The first drying is carried out in air, and the conditions for the first drying are: temperature of 60°C, relative humidity of 50%, and time of 3 minutes. The second drying is carried out in a nitrogen atmosphere, and the conditions for the second drying are: temperature of 120°C, relative humidity of 40%, and time of 5 minutes. The third drying is carried out under vacuum conditions, and the conditions for the third drying are: temperature of 150°C, vacuum degree of -0.09MPa, and time of 3 minutes. Then, it is cured at 200°C for 15 minutes to form grid lines, thereby obtaining the solar cell.
[0089] Example 2 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Example 1 was replaced with the conductive material prepared in Example 2.
[0090] Example 3 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Example 1 was replaced with the conductive material prepared in Example 3.
[0091] Example 4 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Example 1 was replaced with the conductive material prepared in Example 4.
[0092] Example 5 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Preparation Example 1 was replaced with the conductive material prepared in Preparation Example 5.
[0093] Example 6 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Example 1 was replaced with the conductive material prepared in Example 6.
[0094] Example 7 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Preparation Example 1 was replaced with the conductive material prepared in Preparation Example 7.
[0095] Example 8 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Preparation Example 1 was replaced with the conductive material prepared in Preparation Example 8.
[0096] Example 9 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Preparation Example 1 was replaced with the conductive material prepared in Preparation Example 9.
[0097] Example 10 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Preparation Example 1 was replaced with the conductive material prepared in Preparation Example 10.
[0098] Example 11 The procedure was carried out in accordance with Example 1, except that the conductive material coated on the surface of the solar cell body was dried once, and the drying conditions included a temperature of 150°C and a time of 13 minutes.
[0099] Comparative Example 1 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Example 1 was replaced with the conductive material prepared in Comparative Example 1.
[0100] Comparative Example 2 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Example 1 was replaced with the conductive material prepared in Comparative Example 2.
[0101] Comparative Example 3 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Example 1 was replaced with the conductive material prepared in Comparative Example 3.
[0102] Comparative Example 4 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Example 1 was replaced with the conductive material prepared in Comparative Example 4.
[0103] Comparative Example 5 The procedure was carried out in accordance with Example 1, except that the conductive material prepared in Example 1 was replaced with the conductive material prepared in Comparative Example 5.
[0104] Test case Bulk resistivity: The bulk resistivity of the gate electrode was tested using the four-probe method, and the test standard was in accordance with GB / T 1551-2021 "Method for Determination of Resistivity of Single Crystal Silicon". Broken grid rate: The number of broken grid lines per unit length (100mm) is counted under a microscope. Broken grid rate (‰) = number of broken grid lines / total number of grid lines × 1000‰; Weld strip peel strength: The peel strength between the weld strip and the grid electrode was tested using a universal tensile testing machine at a peel angle of 180° and a tensile speed of 50 mm / min. The test standard refers to IEC 61215. Cell conversion efficiency: A solar cell IV characteristic testing system was used, under standard test conditions (AM1.5, 1000W / m²). 2 Tested at 25℃.
[0105] The solar cells prepared in Examples 1-11 and Comparative Examples 1-5 were tested for bulk resistivity, grid breakage rate, solder strip peel strength, and cell conversion efficiency, respectively. The test results are shown in Table 1.
[0106] According to the results in Table 1, the bulk resistivity of the solar cells prepared in Examples 1-7 of this application can be as low as 3.2 × 10⁻⁶. -6 Ω·cm ~4.1×10 -6The battery exhibits excellent performance, with a grid breakage rate ≤0.7‰, a solder strip peel strength ≥1.9 N / mm, and a battery conversion efficiency ≥24.7%, significantly outperforming comparative examples 1-5. Examples 1 (using pure silver powder + phthalic acid reducing agent) and 2 (using pure silver powder + dodecyl mercaptan reducing agent) demonstrate the best performance. Examples 3-4 show that when the conductive phase is a silver-copper alloy or a silver-nickel alloy, the combined use of organic carboxylic acids and alkyl mercaptans (Examples 3 and 4) further reduces bulk resistivity and improves grid breakage rate and peel strength compared to using organic carboxylic acids alone (Example 5), verifying the technical effect of "combining carboxylic acids and mercaptans in the alloy system" in claim 7.
[0107] Example 8 shows that after replacing the reducing agent in this application with ascorbic acid, the volume resistivity increased sharply to 6.8 × 10⁻⁶. -6 The Ω·cm value was reduced, and the breakage rate and peel strength also deteriorated, demonstrating that organic carboxylic acids and / or alkyl thiols have irreplaceable technical advantages as reducing agents.
[0108] Comparative Examples 3-5 show that when the carbon chain length of the reducing agent exceeds the limits defined in this application—that is, when erucic acid with 22 carbon atoms is used (Comparative Example 3), heptanethiol with 7 carbon atoms is used (Comparative Example 4), or eicosylthiol with 20 carbon atoms is used (Comparative Example 5)—the bulk resistivity of the gate line increases to 6.3, 5.9, and 6.6 × 10⁻⁶, respectively. -6 The increase in Ω·cm and the decrease in breakage rate and strip peel strength indicate that the number of carbon atoms in organic carboxylic acids should be limited to C2~C20 and the number of carbon atoms in alkyl thiols should be limited to C8~C18 in order to balance steric stability, zero residue in the low-temperature sintering window and grain boundary lubrication of decomposition products (such as sulfur atoms).
[0109] Examples 9 and 10 show that the absence of flake-shaped or nano-spherical silver powder in the ternary composite leads to increased resistivity and stencil breakage rate, verifying the necessity of synergistic composite of the three morphologies of silver powder. Example 11 shows that after replacing the three-stage microenvironment gradient drying with a single drying process, the stencil breakage rate increased sharply to 2.5‰, demonstrating the key role of the three-stage drying process in eliminating the coffee ring effect and solvent boiling defects.
[0110] Those skilled in the art will understand that the above embodiments are specific examples of implementing this application, and in practical applications, various changes in form and detail can be made without departing from the spirit and scope of this application. Any person skilled in the art can make various alterations and modifications without departing from the spirit and scope of this application; therefore, the scope of protection of this application should be determined by the scope defined in the claims.
Claims
1. A method for preparing a solar cell, characterized in that, The preparation method includes: coating a conductive material containing additives onto at least one side surface of the solar cell body, and curing it to form grid lines to obtain a solar cell; The auxiliary agent includes a silver source and a reducing agent, wherein the reducing agent includes organic carboxylic acids and / or alkyl thiols; the organic carboxylic acids include organic carboxylic acids with a carbon number of C2 to C20, and the alkyl thiols include alkyl thiols with a carbon number of C8 to C18.
2. The preparation method according to claim 1, characterized in that, The organic carboxylic acids include organic carboxylic acids with C8 to C18 carbon atoms, and the alkyl thiols include alkyl thiols with C12 to C18 carbon atoms.
3. The preparation method according to claim 2, characterized in that, The organic carboxylic acid is selected from at least one of phthalic acid, octanoic acid and oleic acid, and the alkyl thiol is selected from at least one of dodecyl thiol, hexadecyl thiol and octadecyl thiol.
4. The preparation method according to claim 1, characterized in that, The silver source includes an organosilver compound, the decomposition temperature of which is 120°C to 250°C, and the organosilver compound includes silver carboxylate and / or silver complexes.
5. The preparation method according to claim 4, characterized in that, The silver carboxylic acid includes silver oxalate, and the silver complex includes silver citrate complex and / or silver-amine complex.
6. The preparation method according to claim 1, characterized in that, The conductive material further includes a conductive phase, which comprises a first spherical powder, a second spherical powder, and a flake-shaped powder, wherein the D50 particle size of the first spherical powder is smaller than the D50 particle size of the second spherical powder.
7. The preparation method according to claim 6, characterized in that, When the conductive phase comprises a silver-copper alloy and / or a silver-nickel alloy, the reducing agent comprises an organic carboxylic acid and an alkyl thiol, and the mass ratio of the organic carboxylic acid to the alkyl thiol is (0.5~5):
1.
8. The preparation method according to claim 1, characterized in that, Before curing to form grid lines, the conductive material coated on the surface of the solar cell body is dried three times in sequence. The temperature of the first drying is lower than that of the second drying, and the temperature of the second drying is lower than that of the third drying. The second drying is carried out in an inert atmosphere, and the third drying is carried out in a vacuum environment.
9. A solar cell obtained according to the preparation method of any one of claims 1 to 8, characterized in that, The solar cell includes: a solar cell body and grid lines located on at least one side surface of the solar cell body.
10. A photovoltaic module, characterized in that, The battery string includes a plurality of solar cells prepared according to any one of claims 1 to 8 or the solar cell of claim 9, arranged along a first direction, and the plurality of battery strings are further arranged along a second direction; A solder strip extending along a first direction and arranged along a second direction, the solder strip being used to connect two adjacent solar cells or two stacked cells along the first direction; A backplate, located on the side of the solder strip away from the back of the battery string.