A back-contact solar cell and its fabrication method
By using doped amorphous silicon as a conductive layer precursor in back-contact solar cells, combined with laser selective film cutting and annealing processes, the problems of precise formation and damage of doped regions during laser grooving were solved, thereby improving the photoelectric conversion efficiency and electrical performance of the cells.
Patent Information
- Application Number
- CN202611324892.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
In existing back-contact solar cells, it is difficult to accurately form alternating P-type and N-type doped regions and achieve reliable electrical isolation during the laser grooving process. Furthermore, laser damage leads to an increase in carrier recombination centers, affecting cell performance.
Doped amorphous silicon is used as the precursor for the conductive layer. By selectively opening the film with laser and combining it with an annealing process, the film material is precisely removed and laser damage is repaired, thus avoiding redistribution of doping concentration.
Higher quality doped polycrystalline silicon was achieved, improving carrier passivation and contact performance, and enhancing the photoelectric conversion efficiency and electrical performance of back-contact solar cells.
Smart Images

Figure CN123124499A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solar cell technology, specifically to a back-contact solar cell and its fabrication method. Background Technology
[0002] Back-contact solar cells place both the positive and negative electrodes on the back of the cell, completely eliminating light loss due to shading by the grid lines on the front electrode, and have become the mainstream technology for high-efficiency crystalline silicon solar cells. However, the back-mounted electrode design also brings new manufacturing challenges—how to accurately form alternating P-type and N-type doped regions on the back and achieve reliable electrical isolation between them has become a core process node that determines cell performance and yield.
[0003] Laser grooving technology, with its advantages of high precision, non-contact operation, and flexible patterns, has been deeply embedded in many key processes of back-contact solar cells. When the laser interacts with the polycrystalline silicon of the cell, the temperature of the heat-affected zone (HAZ) can instantly reach above the melting point of silicon. This thermal process triggers the redistribution of dopants and inevitably leaves lattice distortions, dislocations, and even microcracks at the groove edges and bottom surface. These defect states introduce deep energy levels into the bandgap, becoming effective recombination centers for charge carriers, directly resulting in a decrease in minority carrier lifetime and open-circuit voltage. How to achieve precise material removal while minimizing damage to functional films such as polycrystalline silicon is currently a key focus and challenge in the development of back-contact solar cell processes.
[0004] For example, CN120224828A discloses a low-laser-damage laser grooving method for back-contact solar cells. This method utilizes an additional intrinsic polycrystalline silicon layer and a second mask layer, combined with laser delamination technology and RCA cleaning, to replace the original passivation contact structure of the tunneling oxide layer and heavily doped polycrystalline silicon layer to complete the laser grooving task. During laser action, the additional intrinsic polycrystalline silicon layer and the second mask layer stack absorb all the laser radiation and laser damage, acting as an outer protective layer and preventing high-energy laser damage to the inner tunneling oxide layer and the passivation contact structure of the heavily doped polycrystalline silicon layer. While this method can reduce laser damage to the underlying film layer to some extent, it requires additional film layer and wet cleaning processes, making the process cumbersome, and the lattice damage caused by the laser to the underlying film layer still exists. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a back-contact solar cell and its preparation method.
[0006] Based on this, the present invention discloses a method for fabricating a back-contact solar cell, comprising the following fabrication steps: S1. A silicon wafer is provided; the back side of the silicon wafer includes alternating first and second regions, and an isolation region is provided between adjacent first and second regions; S2. First doped amorphous silicon and first mask layer are sequentially prepared on the back side of silicon wafer; S3. Laser selectively open the first mask layer of the second region and the isolation region, and then remove the first mask layer and the first doped amorphous silicon of the second region and the isolation region by wet cleaning, while retaining the first doped amorphous silicon and the first mask layer of the first region. S4. Annealing transforms the first-doped amorphous silicon into the first-doped polycrystalline silicon and activates its doping source to repair laser damage. S5. A second doped amorphous silicon and a second mask layer are sequentially prepared on the back side of the silicon wafer after the process in step S4. S6. Perform laser selective film opening on the second mask layer of the first region and the isolation region. After removing the second mask layer and the second doped amorphous silicon of the first region and the isolation region by wet cleaning, remove the first mask layer of the first region and the second mask layer of the second region, while retaining the second doped amorphous silicon of the second region. S7. Annealing transforms the second-doped amorphous silicon into the second-doped polycrystalline silicon and activates its doping source to repair laser damage. The first-doped polycrystalline silicon and the second-doped polycrystalline silicon have opposite conductivity types (correspondingly, the first-doped amorphous silicon and the second-doped amorphous silicon also have opposite conductivity types). S8. The back contact solar cell is obtained by passivation and metallization treatment.
[0007] The back-contact solar cell fabrication method of the present invention uses doped amorphous silicon as a precursor for the first and second doped conductive layers (i.e., the first and second doped polycrystalline silicon). A laser is applied to a mask layer above the doped amorphous silicon, which enables precise removal of the film material in the first, second, and isolation regions, and reduces laser damage to the underlying film layers (such as silicon wafers, doped polycrystalline silicon, etc.) during the laser patterning process. Furthermore, the subsequent annealing process repairs the lattice damage to the doped polycrystalline silicon, and the annealing after laser patterning activates the dopant source, avoiding the redistribution of dopant concentration caused by the laser process. Therefore, this fabrication method yields higher quality doped polycrystalline silicon, effectively avoids carrier recombination, and improves the passivation and contact performance of the doped polycrystalline silicon, thereby effectively improving the photoelectric conversion efficiency and other electrical properties of the back-contact solar cell.
[0008] Preferably, in step S1, the silicon wafer is an N-type silicon wafer or a P-type silicon wafer, and the back side of the silicon wafer is a polished surface; the first region is a P-region or an N-region, the second region is an N-region or a P-region, and the first region and the second region are functional regions with opposite conductivity types.
[0009] More preferably, step S2 further includes: preparing a first tunneling oxide layer between the back side of the silicon wafer and the first doped amorphous silicon; the thickness of the first tunneling oxide layer is 0.5~2nm, and its material is one or more of silicon oxide, titanium oxide, and aluminum oxide; The first doped amorphous silicon is a p-type doped amorphous silicon with a thickness of 200~400nm, and its doping source is one or more of B, Ga, and Al; The thickness of the first mask layer is 50~100nm, and its material is one or more of silicon oxide, silicon nitride, and silicon oxynitride.
[0010] More preferably, in step S3, the laser is a green-skinned laser or a purple-skinned laser. When a green-skinned laser is used, the laser energy density is 0.2~0.8 J / cm². 2 ; More preferably, in step S3, the first mask layer, the first doped amorphous silicon and the first tunneling oxide layer of the second region and the isolation region are removed by alkaline washing, while the first tunneling oxide layer, the first doped amorphous silicon and the first mask layer of the first region are retained, and the thickness of the first mask layer retained in the first region is greater than or equal to 30 nm (e.g., 30~50 nm).
[0011] Preferably, in step S4, the annealing temperature is 900~1000℃, the time is 10~40min, and the annealing is carried out under inert gas protection.
[0012] More preferably, before preparing the second doped amorphous silicon, step S5 further includes: preparing a second tunneling oxide layer on the back side of the silicon wafer after the treatment in step S4; the thickness of the second tunneling oxide layer is 0.5~2nm, and its material is one or more of silicon oxide, titanium oxide, and aluminum oxide; The second doped amorphous silicon is N-type doped amorphous silicon with a thickness of 100~300nm, and its doping source is one or more of P, As, and Sb; The thickness of the second mask layer is 50~100nm, and its material is one or more of silicon oxide, silicon nitride, and silicon oxynitride.
[0013] More preferably, in step S6, the laser is a green-skinned laser or a purple-skinned laser. When a green-skinned laser is used, the laser energy density is 0.1~0.6 J / cm². 2 ; More preferably, in step S6, the second mask layer, the second doped amorphous silicon, and the second tunneling oxide layer of the first region and the isolation region are first removed by alkaline washing, then alkaline washing is used to texturize the silicon wafer to form a pyramid textured surface on the back isolation region and the front side, and then acid washing is used to remove the first mask layer of the first region and the second mask layer of the second region, while retaining the second tunneling oxide layer and the second doped amorphous silicon of the second region.
[0014] Preferably, in step S7, the annealing temperature is 800~900℃, the time is 20~50min, and the annealing is carried out under inert gas protection.
[0015] Preferably, after step S7, the thickness difference of the back surface of the isolation region, the first region, and the second region does not exceed ±50nm.
[0016] Preferably, in step S8, passivation layers are first prepared on the front and back sides of the silicon wafer after the processing in step S7, and then the first and second regions on the back side are metallized to obtain the back electrode.
[0017] The present invention also discloses a back-contact solar cell, which is prepared by the back-contact solar cell preparation method described above in the present invention.
[0018] Compared with the prior art, the present invention has at least the following beneficial effects: The method for fabricating a back-contact solar cell of the present invention uses doped amorphous silicon instead of the existing doped polycrystalline silicon, and superimposes a commonly used mask layer as the laser processing film layer. Because doped amorphous silicon has a stronger ability to absorb laser energy than doped polycrystalline silicon, on the one hand, laser selective ablation can be achieved with a lower laser energy density, resulting in a larger processing window; on the other hand, more laser energy can be concentrated on the doped amorphous silicon, reducing laser damage to the film layer below the doped amorphous silicon (for example, reducing damage to the silicon wafer during the first laser selective ablation, and reducing damage to the first doped polycrystalline silicon during the second laser selective ablation). After laser selective ablation, the mask layer and doped amorphous silicon in the laser area are removed by wet process, and then annealing is performed to crystallize the retained doped amorphous silicon. After the laser patterning process, annealing is performed to activate and distribute the doped atoms, avoiding the redistribution of doping concentration in the doped polycrystalline silicon caused by high laser energy. High-temperature annealing can also be used to repair surface damage and lattice damage of crystalline silicon.
[0019] Therefore, this preparation method can not only achieve precise removal of film materials in the first region, second region, and isolation region, but also effectively reduce laser damage to silicon wafers and doped polycrystalline silicon, repair lattice damage caused by doped polycrystalline silicon during laser film opening, and effectively solve the problem of redistribution of doped atoms in doped polycrystalline silicon. It can provide higher quality doped polycrystalline silicon films, while improving the passivation and contact performance of doped polycrystalline silicon, thereby effectively improving the electrical performance of back contact solar cells, such as open circuit voltage, fill factor, and photoelectric conversion efficiency.
[0020] Moreover, compared with existing technologies such as CN120224828A, the preparation method of the present invention does not require the addition of intrinsic polycrystalline silicon and mask layer on the film layer that needs to be protected. The preparation method of the present invention directly utilizes the high absorption capacity of doped amorphous silicon for laser energy to reduce laser damage to the underlying film layer. Its process steps are simpler and the process processing window is larger, which is conducive to industrial promotion and application. Attached Figure Description
[0021] Figure 1 This is a schematic diagram of the cross-sectional structure after step 2 of the preparation method of a back-contact solar cell according to the present invention.
[0022] Figure 2 This is a schematic diagram of the cross-sectional structure of a back-contact solar cell after step 3 of the preparation method of the present invention.
[0023] Figure 3 This is a schematic diagram of the cross-sectional structure of a back-contact solar cell after step 4 of the preparation method of the present invention.
[0024] Figure 4 This is a schematic diagram of the cross-sectional structure after step 5 of the preparation method of a back-contact solar cell according to the present invention.
[0025] Figure 5 This is a schematic diagram of the cross-sectional structure of a back-contact solar cell after step 6 in the preparation method of the present invention.
[0026] Figure 6 This is a schematic diagram of the cross-sectional structure of a back-contact solar cell after step 7 of the preparation method of the present invention.
[0027] Reference numerals: Pyramid textured surface 01; Silicon wafer 11; First tunneling oxide layer 12; P-type doped amorphous silicon 13; P-type doped polycrystalline silicon 131; First mask layer 14; Remaining first mask layer 15; First patterning region T1; Isolation region 22; Second tunneling oxide layer 32; N-type doped amorphous silicon 33; N-type doped polycrystalline silicon 331; Second mask layer 34; Second patterning region T2. Detailed Implementation
[0028] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0029] The present invention discloses a method for fabricating a back-contact solar cell, comprising the following fabrication steps: Step 1, Polishing and Cleaning: The original silicon wafer 11 is placed in a tank cleaning machine for polishing and cleaning. This removes mechanical damage to the silicon wafer 11 while cleaning it, and forms a smooth polished surface on both the front and back sides of the silicon wafer 11. The back side of the silicon wafer 11 includes alternating P-type and N-type functional areas, and there is an isolation area 22 between adjacent P-type and N-type functional areas.
[0030] In step 1, silicon wafer 11 is an N-type silicon wafer or a P-type silicon wafer.
[0031] Step 2: Sequentially fabricate a first tunneling oxide layer 12, a P-type doped amorphous silicon 13, and a first mask layer 14 on the back side of silicon wafer 11 (e.g., ...). Figure 1 (As shown).
[0032] In step 2, the material of the first tunneling oxide layer 12 can be one or more of silicon oxide, titanium oxide, and aluminum oxide, and its preparation method can be chemical oxidation, plasma oxidation, or chemical vapor deposition (preferably chemical vapor deposition). Taking PECVD (plasma-enhanced chemical vapor deposition) as an example, the thickness and density of the first tunneling oxide layer 12 are mainly optimized by changing the deposition time and deposition temperature. The deposition temperature is 300~500℃, the deposition time is 50~150s, and the thickness of the first tunneling oxide layer 12 is 0.5~2 nm.
[0033] In step 2, the doping element of P-type doped amorphous silicon 13 is one or more of B (boron), Ga (gallium), and Al (aluminum). The preparation method can be LPCVD (low-pressure chemical vapor deposition), PECVD, APCVD (atmospheric pressure chemical vapor deposition), or PVD (physical vapor deposition). Taking PECVD as an example, the doping amount, film thickness, and crystallinity of P-type doped amorphous silicon 13 are mainly optimized by adjusting the gas ratio, deposition time, and deposition temperature. The deposition temperature is 300~600℃, the deposition time is 30~80min, the doping ratio of B2H6 (diborane) to SiH4 (silane) is 0.2~2%, the gas flow ratio of H2 (hydrogen) to SiH4 (silane) is 10~40:1, and the thickness of P-type doped amorphous silicon 13 is 200~400 nm.
[0034] In step 2, the material of the first mask layer 14 includes, but is not limited to, one or more of SiO2 (silicon oxide), SiNx (silicon nitride), and SiON (silicon oxynitride). SiO2 and SiNx are traditional mask materials, and their fabrication and wet cleaning processes are simpler and more mature. The fabrication method of the first mask layer 14 can be LPCVD, PECVD, or APCVD. Taking PECVD as an example, the uniformity and thickness of the mask are mainly optimized by controlling the pressure, pulse width ratio, and deposition time. The furnace tube pressure is 80~200Pa, the ratio of the effective pulse width to the ineffective pulse width of the RF power supply is 1:40~70, the deposition time is 500~1000s, and the thickness of the first mask layer 14 is 50~100nm.
[0035] It is worth noting that the first tunneling oxide layer 12, the P-type doped amorphous silicon 13 and the first mask layer 14 can be prepared sequentially using different equipment, or they can be prepared sequentially in the same equipment.
[0036] Step 3: Perform the first graphicization process (e.g.) Figure 2 As shown): A high-energy-density laser beam is used to selectively ablate the first mask layer 14 of the N-type functional region and isolation region 22 on the back side (the N-type functional region and isolation region 22 are the first patterning region T1, also known as the first laser ablation region), so as to basically remove the first mask layer 14 of the first patterning region T1. Then, the remaining first mask layer 14, P-type doped amorphous silicon 13 and the first tunneling oxide layer 12 of the first patterning region T1 are removed by wet cleaning (such as alkaline polishing cleaning with alkaline etching solution). The non-first laser ablation region (i.e., the P-type functional region) retains the complete first tunneling oxide layer 12, P-type doped amorphous silicon 13 and a remaining first mask layer 15 of a certain thickness. The thickness of the remaining first mask layer 15 retained in the P-type functional region is not less than 30 nm, such as 30~50 nm.
[0037] In step 3, the high-energy-density laser beam can be a UV (ultraviolet) laser or a green laser, with a pulse width ranging from femtosecond to nanosecond. A green picosecond laser beam (referred to as a green picosecond laser) or an ultraviolet picosecond laser is preferred; a green picosecond laser is more preferred, with a laser energy density of 0.2~0.8 J / cm². 2 .
[0038] Step 4: Perform a first thermal annealing process on the silicon wafer after the first patterning process to crystallize the P-type doped amorphous silicon 13 in the P-type functional region into P-type doped polycrystalline silicon 131 (e.g., Figure 3 As shown in the figure, the P-type doped atoms are activated and laser damage is repaired. The annealing temperature is 900~1000℃ and the annealing time is 10~40min. The annealing process is carried out under the protection of an inert gas (such as N2).
[0039] Step 5: On the back side of the silicon wafer processed in Step 4, a second tunneling oxide layer 32, an N-type doped amorphous silicon layer 33, and a second mask layer 34 are deposited sequentially. Figure 4 (As shown).
[0040] In step 5, the material of the second tunneling oxide layer 32 can be one or more of silicon oxide, titanium oxide, and aluminum oxide, and its preparation method can be chemical oxidation, plasma oxidation, or chemical vapor deposition. Taking plasma oxidation as an example, the thickness and density of the second tunneling oxide layer 32 are mainly optimized by changing the oxygen flow rate, radio frequency power, and oxidation temperature. The oxygen flow rate is 400~800 sccm, the radio frequency power is 70~150W, the oxidation temperature is 200~400℃, and the thickness of the second tunneling oxide layer 32 is 0.5~2 nm.
[0041] In step 5, the doping element of N-type doped amorphous silicon 33 is one or more of P (phosphorus), As (arsenic), and Sb (antimony), and its preparation method can be LPCVD, PECVD, APCVD, or PVD. Taking PVD as an example, the doping amount and thickness of N-type doped amorphous silicon 33 are mainly optimized by changing the gas flow rate, power supply power, and carrier speed. The gas flow rate ratio of PH3 (phosphine) to Ar (argon) is 0.1~0.5%, the power supply power is 22~33kW, the carrier speed of the silicon wafer is 50~200cm / min, and the thickness of N-type doped amorphous silicon 33 is 100~300 nm.
[0042] In step 5, the material of the second mask layer 34 includes, but is not limited to, one or more of SiO2, SiNx, and SiON. The preparation method of the second mask layer 34 can be LPCVD, PECVD, or APCVD. The thickness of the second mask layer 34 is 50~100nm.
[0043] It is worth noting that the second tunneling oxide layer 32, the N-type doped amorphous silicon 33, and the second mask layer 34 can be prepared sequentially using different equipment, or they can be prepared sequentially in the same equipment.
[0044] Step 6: Perform a second patterning process (e.g.) Figure 5As shown): A high-energy-density laser beam is used to selectively ablate the second mask layer 34 of the P-type functional region and isolation region 22 on the back side (the P-type functional region and isolation region 22 are the second patterning region T2, also known as the second laser ablation region), so as to basically remove the second mask layer 34 of the second patterning region T2. Then, the remaining second mask layer 34, N-type doped amorphous silicon 33 and second tunneling oxide layer 32 of the second patterning region T2 are removed by wet cleaning (such as alkaline polishing cleaning with alkaline etching solution). A pyramid textured surface 01 is formed on the back isolation region 22 and the entire front side of the silicon wafer 11 by alkaline texturing. Then, the remaining first mask layer 15 of the P-type functional region and the second mask layer 34 of the non-second laser ablation region (i.e., N-type functional region) are removed by acid washing (using acidic etching solution). The N-type functional region retains the complete second tunneling oxide layer 32 and N-type doped amorphous silicon 33.
[0045] In step 6, the high-energy-density laser beam can be a UV (ultraviolet) laser or a green laser, with a laser pulse width ranging from femtosecond to nanosecond, preferably a green picosecond laser beam; more preferably a green picosecond laser, with a laser energy density of 0.1~0.6 J / cm². 2 .
[0046] The wet cleaning processes in steps 3 and 6 (such as alkaline polishing, alkaline texturing, and acid washing) refer to the existing back-contact solar cell fabrication processes, so they will not be described in detail here.
[0047] Step 7: Perform a second thermal annealing process on the silicon wafer after the second patterning process to crystallize the N-type doped amorphous silicon 33 in the N-type functional region into N-type doped polycrystalline silicon 331 (e.g., Figure 6 As shown in the figure, the N-type doped atoms are activated and laser damage is repaired. The annealing temperature is 800~900℃ and the annealing time is 20~50min. The annealing process is carried out under the protection of an inert gas (such as N2).
[0048] Thus, after step 7, the P-type functional region on the back side of silicon wafer 11 is sequentially formed with a first tunneling oxide layer 12 and P-type doped polysilicon 131, while the N-type functional region on the back side is sequentially formed with a second tunneling oxide layer 32 and N-type doped polysilicon 331. Furthermore, an isolation region 22 (e.g., the pyramidal textured surface 01 on the back side of silicon wafer 11) is formed between the P-type and N-type functional regions on the back side of silicon wafer 11. Figure 6 (As shown).
[0049] Step 8: Deposit passivation layers on the front and back sides of silicon wafer 11. The passivation layers can be SiO2 (silicon oxide), Al2O3 (aluminum oxide), or SiN. x One or more combinations of silicon nitride. The fabrication process of the passivation layer is based on the existing fabrication process of back-contact solar cells, and therefore will not be described in detail here.
[0050] Step 9: Screen-print metal paste onto the P-type and N-type functional regions on the back side of silicon wafer 11 and perform sintering to obtain interdigitated back electrodes (the P-type back electrode contacts the P-type doped polycrystalline silicon 131 of the P-type functional region, while the N-type back electrode contacts the N-type doped polycrystalline silicon 331 of the N-type functional region). The specific fabrication process of the back electrodes refers to the existing metallization process of back contact solar cells, and therefore will not be elaborated here.
[0051] After step 9, a back-contact solar cell of the present invention is obtained, see [link to relevant documentation]. Figure 6 The device includes: a silicon wafer 11, the back side of which includes alternating P-type and N-type functional regions, and an isolation region 22 is formed between adjacent P-type and N-type functional regions (the isolation region 22 on the back side of the silicon wafer 11 does not have a tunneling oxide layer and doped polysilicon, so as to isolate the P-type doped polysilicon 131 and the N-type doped polysilicon 331); the P-type functional regions on the back side of the silicon wafer 11 are sequentially formed with a first tunneling oxide layer 12 and P-type doped polysilicon 131, while the N-type functional regions on the back side are sequentially formed with a second tunneling oxide layer 32 and N-type doped polysilicon 331, and the thickness difference between the back surfaces of the isolation region 22, the P-type functional regions, and the N-type functional regions does not exceed ±50 nm; a pyramid textured surface 01 is formed on the front side of the silicon wafer 11 and the back surface of the isolation region 22 of the silicon wafer 11. Passivation layers are formed on the back sides of the P-type doped polysilicon 131, the N-type doped polysilicon 331, and the isolation region 22, and a passivation layer is also formed on the front side of the silicon wafer 11. The passivation layers include an aluminum oxide passivation layer and a silicon nitride anti-reflection passivation layer formed sequentially. The P-type doped polysilicon 131 is in contact with the P-type back electrode, while the N-type doped polysilicon 331 is in contact with the N-type back electrode.
[0052] The following is a specific embodiment of a method for fabricating a back-contact solar cell according to the present invention: Example 1 This embodiment describes a method for fabricating a back-contact solar cell, see [link to relevant documentation]. Figures 1-6 The preparation steps 1-7 are the same as those in the specific embodiment described above for the preparation method of a back contact solar cell. The difference in this embodiment is as follows: In step 1 of this embodiment, silicon wafer 11 is an N-type silicon wafer.
[0053] In step 2 of this embodiment, the first tunneling oxide layer 12 is made of silicon oxide and is prepared by PECVD at a deposition temperature of 400°C for 80 seconds, with a thickness of 1.5 nm. The p-type doped amorphous silicon 13 is doped with boron (B) and is prepared by PECVD at a deposition temperature of 450°C for 40 minutes. The doping ratio of B₂H₆ to SiH₄ is 1%, the gas flow rate ratio of H₂ to SiH₄ is 30:1, and the thickness of the p-type doped amorphous silicon 13 is 250 nm. The first mask layer 14 is made of SiO₂ and is prepared by PECVD at a furnace pressure of 120 Pa. The ratio of the effective pulse width to the ineffective pulse width of the RF power supply is 1:55, the deposition time is 800 seconds, and the thickness of the first mask layer 14 is 60 nm.
[0054] In step 3 of this embodiment, the laser beam used in the first patterning process is a green-skinned laser with a laser energy density of 0.3 J / cm². 2 .
[0055] In step 4 of this embodiment, the annealing temperature is 960℃ and the annealing time is 20min.
[0056] In step 5 of this embodiment, the second tunneling oxide layer 32 is made of silicon oxide and is prepared by plasma oxidation. The oxygen flow rate is 600 sccm, the RF power is 120 W, the oxidation temperature is 250 °C, and the thickness of the second tunneling oxide layer 32 is 0.8 nm. The N-type doped amorphous silicon 33 is doped with P and is prepared by PVD. The gas flow rate ratio of PH3 to Ar is 0.2%, the power supply is 29 kW, the carrier speed is 120 cm / min, and the thickness of the N-type doped amorphous silicon 33 is 220 nm. The second mask layer 34 is made of SiO2 and is prepared by PECVD. The thickness of the second mask layer 34 is 60 nm.
[0057] In step 6 of this embodiment, the laser beam used in the second patterning process is a green-skinned laser with a laser energy density of 0.25 J / cm². 2 .
[0058] In step 7 of this embodiment, the annealing temperature of the second thermal annealing process is 850°C, and the annealing time is 35 minutes. After processing in step 9, the back-contact solar cell of this embodiment is obtained.
[0059] Comparative Example 1 The comparative example describes a method for fabricating a back-contact solar cell, which includes the following fabrication steps: Step 1, Polishing and Cleaning: Refer to Step 1 of Example 1.
[0060] Step 2: Deposit a first tunneling silicon oxide layer (made of silicon oxide) with a thickness of 1.5 nm and a first intrinsic polycrystalline silicon layer with a thickness of 250 nm on the back side of the silicon wafer using the LPCVD method.
[0061] Step 3: P-type doped polysilicon is formed by thermal diffusion of P-type doped atoms (B) into the first intrinsic polysilicon layer, and a borosilicate glass layer (BSG) with a thickness of 80 nm is formed on the back surface of the P-type doped polysilicon by post-oxidation process as the first mask layer.
[0062] Step 4: Perform the first patterning process: Selectively open the first mask layer of the N-type functional region and isolation region on the back side using a high-energy-density laser beam to essentially remove the first mask layer of the first patterned region. Then, remove the remaining first mask layer, P-type doped polysilicon, and first tunneling oxide layer of the first patterned region by alkaline polishing. The non-first laser-opened region (i.e., the P-type functional region) retains the complete first tunneling oxide layer, P-type doped polysilicon, and a certain thickness of the remaining first mask layer; the thickness of the first mask layer retained in the P-type functional region is not less than 30 nm. The specific process conditions for step 4 of this comparative example are the same as those for step 3 of Example 1.
[0063] Step 5: Using LPCVD, a 1 nm thick second tunneling oxide layer (made of silicon oxide) and a 250 nm thick second intrinsic polycrystalline silicon layer are sequentially deposited on the back side of the silicon wafer.
[0064] Step 6: N-type doped polysilicon is formed by thermal diffusion of N-type doped atoms (P) into the second intrinsic polysilicon, and a phosphosilicate glass (PSG) layer with a thickness of 60 nm is formed on the back surface of the N-type doped polysilicon as a second mask layer by post-oxidation process.
[0065] Step 7: Perform the second patterning process: Selectively open the second mask layer of the P-type functional region and isolation region on the back side using a high-energy-density laser beam to essentially remove the second mask layer of the second patterning region T2. Then, remove the remaining second mask layer, N-type doped polysilicon, and second tunneling oxide layer of the second patterning region T2 by alkaline polishing. Form a pyramid textured surface on the back isolation region and the entire front side of the silicon wafer by alkaline texturing. Then, remove the remaining first mask layer of the P-type functional region and the second mask layer of the second laser-opened region (i.e., the N-type functional region) by acid washing. The N-type functional region retains the complete second tunneling oxide layer and N-type doped polysilicon.
[0066] Step 8: Deposit passivation layers on the front and back sides of the silicon wafer (refer to step 8 of Example 1 for details).
[0067] Step 9: Fabricate interdigitated back electrodes on the P-type and N-type functional regions on the back of the silicon wafer (refer to step 9 of Example 1 for details). After step 9, the back-contact solar cell of this comparative example is obtained.
[0068] Performance testing 1. The sheet resistance (SRT) values of the P-type functional region (P-region) and N-type functional region (N-region) of the silicon wafer samples of Example 1 and Comparative Example 1 (the silicon wafer samples are silicon wafers before the deposition of the passivation layer) were tested, and the test results are shown in Table 1 below.
[0069] Table 1
[0070] In Table 1, the P-region is the P-type functional region and the N-region is the N-type functional region. Five points are tested on each back-contact solar cell. These five points are the upper left corner, upper right corner, middle area, lower left corner, and lower right corner of the cell. The numbers of these five points are 1, 2, 3, 4, and 5 in Table 1.
[0071] Referring to Table 1, it can be seen that compared with Comparative Example 1, Embodiment 1 of the present invention can obtain P-region doped polysilicon and N-region doped polysilicon with more uniform distribution of doped atoms.
[0072] 2. The electrical performance of the back-contact solar cells of Example 1 and Comparative Example 1 was tested, and the test results are shown in Table 2 below.
[0073] Table 2
[0074] In Table 2, Uoc is the open-circuit voltage, Isc is the short-circuit current, FF is the fill factor, Eta is the photoelectric conversion efficiency, Rs is the series resistance, and Rshunt is the parallel resistance.
[0075] Referring to the test data in Table 2, it can be seen that during the laser patterning process, replacing the existing doped polycrystalline silicon layer with doped amorphous silicon and superimposing a mask layer as the laser processing film reduces the laser damage caused by high-energy lasers to the silicon wafer and the tunneling oxide layer and passivation contact structure formed by the doped polycrystalline silicon. This effectively improves the open-circuit voltage and fill factor of the back-contact solar cell, thereby improving the cell conversion efficiency of the back-contact solar cell. Furthermore, the thermal annealing process after the patterning process not only transforms the doped amorphous silicon into doped polycrystalline silicon, but also activates and distributes the doped atoms after the laser patterning process. This effectively avoids the redistribution problem of doped atoms in the doped polycrystalline silicon caused by high-energy lasers, and can use high-temperature annealing to repair surface damage and lattice damage of crystalline silicon, providing a higher quality doped polycrystalline silicon film layer and improving the passivation and contact performance of the doped polycrystalline silicon. Therefore, compared with the existing doped polycrystalline silicon + laser patterning film-making process in Comparative Example 1, the back contact solar cell prepared in Example 1 of this invention has effectively improved electrical properties such as open circuit voltage, short circuit current, fill factor, series resistance, and parallel resistance, thereby further improving the photoelectric conversion efficiency of the back contact solar cell.
[0076] Although preferred embodiments of the present invention have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of the embodiments of the present invention.
[0077] The technical solution provided by the present invention has been described in detail above. Specific examples have been used to illustrate the principle and implementation of the present invention. The description of the above embodiments is only for the purpose of helping to understand the method and core idea of the present invention. At the same time, for those skilled in the art, there will be changes in the specific implementation and application scope based on the idea of the present invention. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A method for fabricating a back-contact solar cell, characterized in that, The preparation steps include the following: S1. A silicon wafer is provided; the back side of the silicon wafer includes alternating first and second regions, and an isolation region is provided between adjacent first and second regions; S2. First doped amorphous silicon and first mask layer are sequentially prepared on the back side of silicon wafer; S3. Laser selectively open the first mask layer of the second region and the isolation region, and then remove the first mask layer and the first doped amorphous silicon of the second region and the isolation region by wet cleaning, while retaining the first doped amorphous silicon and the first mask layer of the first region. S4. Annealing transforms the first-doped amorphous silicon into the first-doped polycrystalline silicon and activates its doping source to repair laser damage. S5. A second doped amorphous silicon and a second mask layer are sequentially prepared on the back side of the silicon wafer after the process in step S4. S6. Perform laser selective film opening on the second mask layer of the first region and the isolation region. After removing the second mask layer and the second doped amorphous silicon of the first region and the isolation region by wet cleaning, remove the first mask layer of the first region and the second mask layer of the second region, while retaining the second doped amorphous silicon of the second region. S7. Annealing transforms the second-doped amorphous silicon into the second-doped polycrystalline silicon and activates its doping source to repair laser damage; the first-doped polycrystalline silicon and the second-doped polycrystalline silicon have opposite conductivity types. S8. The back contact solar cell is obtained by passivation and metallization treatment.
2. The method for fabricating a back-contact solar cell according to claim 1, characterized in that, In step S1, the silicon wafer is an N-type silicon wafer or a P-type silicon wafer, and the back side of the silicon wafer is a polished surface; the first region is a P-region or an N-region, the second region is an N-region or a P-region, and the first region and the second region are functional regions with opposite conductivity types.
3. A method for fabricating a back-contact solar cell according to claim 1 or 2, characterized in that, Step S2 further includes: preparing a first tunneling oxide layer between the back side of the silicon wafer and the first doped amorphous silicon; the thickness of the first tunneling oxide layer is 0.5~2nm, and its material is one or more of silicon oxide, titanium oxide, and aluminum oxide; The first doped amorphous silicon is a p-type doped amorphous silicon with a thickness of 200~400nm, and its doping source is one or more of B, Ga, and Al; The thickness of the first mask layer is 50~100nm, and its material is one or more of silicon oxide, silicon nitride, and silicon oxynitride.
4. A method for fabricating a back-contact solar cell according to claim 3, characterized in that, In step S3, the laser is a green-skinned laser or a purple-skinned laser; when a green-skinned laser is used, the laser energy density is 0.2~0.8 J / cm². 2 ; The first mask layer, the first doped amorphous silicon, and the first tunneling oxide layer of the second region and the isolation region are removed by alkaline washing, while the first tunneling oxide layer, the first doped amorphous silicon, and the first mask layer of the first region are retained, and the thickness of the first mask layer retained in the first region is greater than or equal to 30 nm.
5. The method for fabricating a back-contact solar cell according to claim 1, characterized in that, In step S4, the annealing temperature is 900~1000℃, the time is 10~40min, and the annealing is carried out under inert gas protection.
6. A method for fabricating a back-contact solar cell according to claim 1 or 2, characterized in that, Step S5, before preparing the second doped amorphous silicon, further includes: preparing a second tunneling oxide layer on the back side of the silicon wafer after the treatment in step S4; the thickness of the second tunneling oxide layer is 0.5~2nm, and its material is one or more of silicon oxide, titanium oxide, and aluminum oxide; The second doped amorphous silicon is N-type doped amorphous silicon with a thickness of 100~300nm, and its doping source is one or more of P, As, and Sb; The thickness of the second mask layer is 50~100nm, and its material is one or more of silicon oxide, silicon nitride, and silicon oxynitride.
7. A method for fabricating a back-contact solar cell according to claim 6, characterized in that, In step S6, the laser is a green-skinned laser or a purple-skinned laser; when a green-skinned laser is used, the laser energy density is 0.1~0.6 J / cm². 2 ; First, alkaline washing removes the second mask layer, second doped amorphous silicon, and second tunneling oxide layer of the first region and the isolation region. Then, alkaline washing is used to texturize the silicon wafer to form a pyramid textured surface on the back isolation region and the front side. Next, acid washing removes the first mask layer of the first region and the second mask layer of the second region, while retaining the second tunneling oxide layer and the second doped amorphous silicon of the second region.
8. The method for fabricating a back-contact solar cell according to claim 1, characterized in that, In step S7, the annealing temperature is 800~900℃, the time is 20~50min, and the annealing is carried out under inert gas protection. After step S7, the thickness difference of the back surface of the isolation region, the first region, and the second region does not exceed ±50nm.
9. The method for fabricating a back-contact solar cell according to claim 1, characterized in that, In step S8, passivation layers are first prepared on the front and back sides of the silicon wafer after the processing in step S7, and then the first and second regions on the back side are metallized to obtain the back electrode.
10. A back-contact solar cell, characterized in that, The back-contact solar cell is prepared by the method for preparing a back-contact solar cell according to any one of claims 1-9.
Citation Information
Patent Citations
Back contact battery laser grooving method and device with low laser damage
CN120224828A