Semiconductor substrates and their fabrication methods, solar cells and battery modules, and wafer etching solutions
By forming rounded protrusions and arc-shaped depressions on a semiconductor substrate, the problem of sharp edges in the pyramidal textured structure is solved, thereby improving the uniformity of the film and the photoelectric performance, and enhancing the photoelectric conversion efficiency and stability of the tandem solar cell.
Patent Information
- Application Number
- CN202611400787.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-17
AI Technical Summary
In the prior art, the sharp edges of the pyramidal textured structure lead to uneven thickness of the perovskite layer, which affects the photoelectric conversion efficiency of the tandem solar cell and increases recombination loss and interface defects.
The semiconductor substrate is treated with a circular etching solution to form a circular bump and an arc-shaped depression structure, eliminating sharp edges and ensuring that the film-forming material flows uniformly on the smooth curved surface and arc-shaped depression, thereby improving the film quality.
It improves the uniformity of the film layer, reduces recombination loss, and enhances the photoelectric performance and stability of solar cells.
Smart Images

Figure CN123124500A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of solar cell technology, specifically relating to a semiconductor substrate and its preparation method, solar cells and battery modules, and a circular etching solution. Background Technology
[0002] Currently, the mature process of heterojunction (HJT) solar cells is widely used in industry: anisotropic etching of the silicon wafer surface using an alkaline solution (such as KOH or NaOH) forms a randomly distributed pyramidal textured surface. This pyramidal structure typically has sharp apexes, edges, and corners at the junction of the base and the top.
[0003] However, in actual production, it has been found that the pyramid-shaped textured surface exhibits noticeably sharp edges at the pyramid's apex, edges, and the junctions of adjacent pyramid bases. For tandem solar cells, such as perovskite / crystalline silicon tandem cells, these sharp edges lead to uneven flow and distribution of the perovskite precursor solution during coating or deposition. Specifically, the perovskite material is thinner at the pyramid apex and edges, sometimes even exhibiting leakage points, while the material is thicker at the pyramid's base. This uneven thickness not only affects the crystallinity of the perovskite layer but also increases recombination losses and reduces the photoelectric conversion efficiency of the tandem solar cell. Furthermore, the smooth surface of the pyramids makes it easy for the perovskite material to detach or aggregate before crystallization, forming pinholes or grain boundary defects, further impairing cell performance.
[0004] Therefore, there is an urgent need in the existing technology to eliminate the sharp edges of the pyramid-shaped textured surface and alleviate the problem of uneven thickness of the perovskite layer. Summary of the Invention
[0005] In view of the above problems, this application provides a semiconductor substrate and its preparation method, a solar cell and a battery module to solve the technical problem that the surface functional layer film quality of the existing semiconductor substrate pyramid textured structure is poor due to sharp edges (such as the top, edge and junction).
[0006] In a first aspect, embodiments of this application provide a semiconductor substrate. The semiconductor substrate of this application is used in a solar cell. At least one surface of the semiconductor substrate has a textured structure, and the textured structure includes a plurality of randomly distributed rounded protrusions. Each rounded protrusion has a smooth top surface, and the bottom of adjacent rounded protrusions has an arc-shaped recessed structure.
[0007] In this embodiment, the textured surface of the semiconductor substrate consists of multiple rounded protrusions, each with a smooth top surface and an arc-shaped recess between adjacent protrusions. This structure eliminates the sharp apex, edges, and V-shaped corners at the bottom of traditional pyramid textured surfaces. When a functional layer is formed on its surface (especially through a coating process), the film-forming material can flow and spread uniformly at the smooth surfaces and arc-shaped recesses, effectively reducing the problem of excessively thin film at sharp corners and excessively thick material buildup at the valleys, thereby significantly improving the overall quality of the film.
[0008] Furthermore, in this embodiment, the textured surface of the semiconductor substrate achieves a smooth transition between protrusions through arc-shaped recesses, eliminating sharp edges while retaining a continuous, undulating microstructure and moderate surface roughness. This moderate roughness not only increases nucleation sites but also strengthens the mechanical interlocking and chemical adsorption between the functional layer and the semiconductor silicon substrate, contributing to the formation of a dense, pinhole-free functional layer, thereby improving crystal quality and reducing surface defects.
[0009] Optionally, the ratio of the height of the rounded protrusion to the diameter of the bottom is (0.3 to 1.25):1.
[0010] Optionally, the height of the rounded protrusion is 1.5 μm to 2.5 μm.
[0011] Optionally, the diameter of the bottom of the rounded protrusion is 2 μm to 5 μm.
[0012] Optionally, the depth-to-width ratio of the arc-shaped recessed structure can be (0.15 to 5):1.
[0013] Optionally, the depth of the arc-shaped recessed structure is 0.3 μm to 1.5 μm.
[0014] Optionally, the width of the arc-shaped recessed structure is 0.3 μm to 2 μm.
[0015] Optionally, the rounded protrusion includes at least one of a conical, hill-shaped, or pyramid-like tetrahedron.
[0016] Secondly, embodiments of this application also provide a method for preparing a semiconductor substrate. The method for preparing a semiconductor substrate according to embodiments of this application includes the following steps: At least one surface of a semiconductor substrate is subjected to texturing etching to form a texturing surface with multiple randomly distributed pyramidal structures; The textured surface is etched using a circular etching solution to form circular protrusions in the pyramid structure. Each circular protrusion has a smooth top surface, and the bottom of adjacent circular protrusions has an arc-shaped concave structure.
[0017] The semiconductor substrate fabrication method of this application uses a textured etching process to form a randomly distributed pyramid structure on the surface of the semiconductor substrate as an intermediate template. A circular etching process is then performed on this pyramid structure, utilizing the differential effect of chemical etching on anisotropic morphology to effectively eliminate the sharp apex and edges of the pyramids, as well as the V-shaped valleys between adjacent pyramids. This transforms the pyramid structure into rounded protrusions with smooth top surfaces and arc-shaped depressions between adjacent rounded protrusions. Furthermore, this circular etching process ensures that the textured surface maintains sufficient undulation.
[0018] Optionally, based on 100% of the total mass of the spherical etching solution, the spherical etching solution comprises the following components by mass percentage: Solvent 85%–94%; Alkali compounds 0.05%–4%; Cosolvent 1%–5%; Surfactant 1%–5%; Complexing agent 1%–3%; Corrosion inhibitor 0.5%–4%; pH adjuster 0.1%–3%; Defoamer 0.1%–3%.
[0019] Further, optionally, the cosolvent includes at least one of ethylene glycol, propylene glycol, and glycerin.
[0020] Further optionally, the surfactant includes at least one of a nonionic surfactant and anionic surfactant, wherein the nonionic surfactant includes at least one of fatty alcohol polyoxyethylene ether, polyoxyethylene polyoxypropylene ether, and Tween-80, and the anionic surfactant includes at least one of fatty alcohol ether sodium sulfate and alkyl sulfonate.
[0021] Further optionally, the complexing agent includes at least one of sodium gluconate, sodium citrate, sodium lactate, disodium EDTA, and phytic acid.
[0022] Further optionally, the corrosion inhibitor includes at least one of sodium silicate, chitosan, tannic acid, resveratrol, carboxymethyl cellulose, and polyvinylpyrrolidone.
[0023] Further optionally, the pH adjuster includes at least one of sodium carbonate, sodium bicarbonate, and sodium acetate.
[0024] Further optionally, the defoamer includes at least one of polyether-modified silicone oil and organosilicon emulsion.
[0025] Further optionally, the base includes at least one of the hydroxides NaOH, KOH, and NH4OH.
[0026] Alternatively, the solvent may include water.
[0027] Optionally, the temperature of the circular etching process is 30°C to 80°C; Optionally, the time for the circular etching process is 150 s to 850 s.
[0028] Thirdly, embodiments of this application also provide a solar cell. The solar cell of this application embodiment includes the semiconductor substrate of this application embodiment or the semiconductor substrate prepared by the semiconductor substrate preparation method of this application embodiment.
[0029] The solar cell of this application embodiment includes the semiconductor substrate of the above-described embodiment. Its textured structure consists of multiple rounded protrusions, with an arc-shaped depression at the bottom between adjacent protrusions. The functional film layer formed on one side of the textured surface of this semiconductor substrate can uniformly cover the curved surfaces of the rounded protrusions and the arc-shaped depressions, effectively avoiding the uneven film thickness problem caused by sharp edges in traditional pyramid textured surfaces (i.e., thinner at sharp corners and thicker at valleys). This film uniformity significantly reduces recombination losses and leakage channels caused by coverage defects, thereby improving the photoelectric performance of the solar cell, such as the fill factor and open-circuit voltage. Simultaneously, the rounded protrusions and arc-shaped depressions eliminate microscopic sharp corners, reducing stress concentration and interface defect density at the corners of the functional layer formed on its surface, thereby reducing carrier recombination and improving minority carrier lifetime. Furthermore, compared to traditional pyramid textured surfaces, the textured surface with rounded protrusions and arc-shaped depressions can effectively scatter and trap incident light, improving its omnidirectional reflectivity and increasing the light utilization rate of the photoactive layer.
[0030] Optionally, the solar cell is a tandem solar cell, comprising a crystalline silicon sub-cell and a perovskite sub-cell, wherein the crystalline silicon sub-cell contains the semiconductor substrate, and the perovskite sub-cell is disposed on the surface of the crystalline silicon sub-cell near the semiconductor substrate, on the side having the textured surface structure.
[0031] Fourthly, embodiments of this application also provide a battery module. The battery module of this application includes the solar cell of this application.
[0032] Since the battery module of this application embodiment contains the tandem solar cell of the above application embodiment, the photoelectric conversion efficiency and stability of the battery module of this application embodiment are improved.
[0033] Fifthly, embodiments of this application also provide a circular etching solution. The circular etching solution of this application, based on 100% of its total mass, comprises the following components by mass percentage: Solvent 85%–94%; Alkali compounds 0.05%–4%; Cosolvent 1%–5%; Surfactant 1%–5%; Complexing agent 1%–3%; Corrosion inhibitor 0.5%–4%; pH adjuster 0.1%–3%; Defoamer 0.1%–3%.
[0034] The circular etching solution in this application embodiment can perform circular etching on the pyramid structure in the textured surface of the semiconductor substrate, so that the pyramid structure forms a circular protrusion, and the V-shaped corners at the junction of adjacent pyramid structures are etched to form an arc-shaped concave structure. Attached Figure Description
[0035] To more clearly illustrate the technical solutions in the specific embodiments of this application or the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0036] Figure 1 This is a schematic diagram of the structure of a stacked solar cell according to an embodiment of this application; Figure 2 This is a partial scanning electron microscope (SEM) image of the circularized raised textured surface structure of the semiconductor substrate of the crystalline silicon sub-cell of the tandem solar cell in Embodiment 1 of this application; Figure 3 This is a partial side-view scanning electron microscope (SEM) image of the circularized raised textured surface structure of the crystalline silicon sub-cell semiconductor substrate in Embodiment 1 of this application; Figure 4 This is another partial side-view scanning electron microscope (SEM) image of the circularized raised textured surface structure of the crystalline silicon sub-cell semiconductor substrate in Embodiment 1 of this application; Figure 5 This is a partial side-view scanning electron microscope (SEM) image of the perovskite active layer contained in the perovskite sub-cell of the tandem solar cell in Embodiment 1 of this application; Figure 6 This is a magnified scanning electron microscope (SEM) image of a portion of the perovskite active layer contained in the perovskite sub-cell of the tandem solar cell in Embodiment 1 of this application; Figure 7 This is a top-view scanning electron microscope (SEM) image of the perovskite active layer contained in the perovskite sub-cell of the tandem solar cell in Embodiment 1 of this application; Figure 8This is a partial scanning electron microscope (SEM) image of the pyramidal textured surface structure of the crystalline silicon sub-cell semiconductor substrate in Comparative Example 1. Figure 9 This is a side-view scanning electron microscope (SEM) image of the perovskite active layer contained in the perovskite sub-cell of the tandem solar cell in Comparative Example 1.
[0037] The reference numerals in the detailed embodiments are as follows: 10-Crystal silicon sub-cell, back electrode 11, metal electrode layer 111, transparent electrode layer 112, p-type window layer 12, first passivation layer 13, semiconductor substrate 14, second passivation layer 15, n-type window layer 16; 20-Composite layer; 30-Perovskite sub-cell, hole transport layer 31, self-assembled monolayer 311, transition metal oxide layer 312, perovskite active layer 32, electron transport layer 33, buffer layer 34, transparent conductive layer 35, electrode grid line 36, antireflection layer 37. Detailed Implementation
[0038] To make the technical problems, technical solutions, and beneficial effects of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.
[0039] In this application, the term "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. A and B can be singular or plural. The character " / " generally indicates that the preceding and following related objects have an "or" relationship.
[0040] In this application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.
[0041] It should be understood that in the various embodiments of this application, the order of the above processes does not imply the order of execution. Some or all steps may be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.
[0042] The terminology used in the embodiments of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of this application. The singular forms “a,” “the,” and “the” used in the embodiments of this application and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise.
[0043] The weights of the relevant components mentioned in the embodiments of this application can refer not only to the specific content of each component, but also to the proportional relationship between the weights of the components. Therefore, any scaling up or down of the content of the relevant components according to the embodiments of this application is within the scope disclosed in the embodiments of this application. Specifically, the mass described in the embodiments of this application can be a well-known unit of mass in the chemical industry, such as µg, mg, g, or kg.
[0044] The terms "first" and "second" are used for descriptive purposes only, to distinguish objects, such as substances, from one another, and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. For example, without departing from the scope of the embodiments of this application, "first XX" may also be referred to as "second XX," and similarly, "second XX" may also be referred to as "first XX." Thus, features defined with "first" and "second" may explicitly or implicitly include one or more of that feature.
[0045] With the photovoltaic industry's continuous pursuit of higher photoelectric conversion efficiency, tandem solar cells have become a research hotspot due to their ability to break through the theoretical efficiency limit of single-junction cells. Taking perovskite / crystalline silicon tandem solar cells as an example, they have become a research focus because they can overcome the photoelectric efficiency limit of single-junction cells. Among these, the surface textured structure of the crystalline silicon sub-cells is crucial for light trapping and subsequent thin-film deposition. Currently, the mature process of heterojunction (HJT) cells is widely used in industry: anisotropic etching of the silicon wafer surface using alkaline solutions (such as KOH or NaOH) forms a randomly distributed pyramidal textured surface. This pyramidal structure typically has sharp apexes, edges, and corners at the junction of the base and top. To meet the surface flatness requirements of the amorphous silicon passivation layer in heterojunction cells, the industry further uses a mixed solution of hydrofluoric acid (HF) and ozone (O3) to lightly polish the pyramidal textured surface to remove surface micro-damage and reduce interface state density.
[0046] However, the inventors of this invention have discovered that the above-mentioned HF / O3 polishing treatment has the following technical defects, which particularly limit its application in perovskite / crystalline silicon tandem solar cells: First, the corrosive effect of HF / O3 is limited; it essentially only provides a minor smoothing treatment to the pyramid surface and cannot fundamentally alter the pyramid's geometry. After treatment, the pyramid's apex, edges, and the junctions of adjacent pyramid bases still retain noticeable sharp angles. These angles have a certain impact on the coverage and passivation effect of the amorphous silicon layer, especially for tandem solar cells, such as perovskite / crystalline silicon tandem solar cells. Perovskite sub-cells need to be deposited directly or through an intermediate layer onto the textured surface of a crystalline silicon substrate. Sharp angles can cause uneven flow and distribution of the perovskite precursor solution during coating or deposition. Specifically, the perovskite material is thinner at the apex and edges, even exhibiting leakage points, while the material is thicker at the pyramid's base. This uneven thickness not only affects the crystal quality of the perovskite layer but also increases recombination losses and reduces the photoelectric conversion efficiency of the tandem solar cell.
[0047] Second, HF / O3 polishing can make the pyramid surface too smooth. While a smooth surface is beneficial for the passivation of amorphous silicon, moderate surface roughness is beneficial for the nucleation and crystallization of perovskite materials, as it improves the wettability and adhesion of the perovskite precursor solution, resulting in a more uniform and dense perovskite film. An overly smooth surface makes the perovskite material prone to desorption or aggregation before crystallization, forming pinholes or grain boundary defects, further impairing battery performance.
[0048] To address the aforementioned issues, this application proposes an improved semiconductor substrate as described below. By configuring the textured microstructure of the semiconductor substrate as rounded bumps, the rounded bumps have smooth top curved surfaces, while the bottom between adjacent rounded bumps has an arc-shaped concave structure, thereby effectively improving the quality of the film layer formed on the textured surface of the semiconductor substrate, and thus effectively improving the photoelectric performance of tandem cells, such as perovskite / crystalline silicon tandem cells.
[0049] [Semiconductor substrate] In a first aspect, embodiments of this application provide a semiconductor substrate. The semiconductor substrate of this application is used in a solar cell. At least one surface of the semiconductor substrate has a textured structure, and the textured structure includes a plurality of randomly distributed rounded protrusions. Each rounded protrusion has a smooth top surface, and the bottom between adjacent rounded protrusions has an arc-shaped recessed structure.
[0050] In the semiconductor substrate of this application embodiment, a rounded bump refers to a three-dimensional microstructure protruding outward from the semiconductor substrate. The geometric characteristics of this three-dimensional microstructure are a smooth overall outline, without sharp edges or points, and a curved transition throughout the surface. The top curved surface of the rounded bump refers to the continuously smooth curved surface region of each rounded bump on the side furthest from the substrate body. This region does not have the sharp points or broken lines of existing pyramids, and the radius of curvature is greater than zero at least in one dimension. An arc-shaped depression refers to the inwardly concave arc-shaped structure of the bottom region between two adjacent rounded bumps. This arc-shaped surface smoothly connects the bottoms of the two bumps, forming a smooth arc bottom at its lowest point, without sharp trench bottom corners. At least one surface of the semiconductor substrate has a textured structure, meaning that one surface of the semiconductor substrate has a textured structure; of course, both surfaces can also have a textured structure.
[0051] The textured semiconductor substrate of this application embodiment contains multiple rounded protrusions with smooth top surfaces and arc-shaped depressions at the bottom between adjacent rounded protrusions. This structure completely eliminates the sharp tips, edges, and V-shaped corners at the junction of the pyramids in traditional pyramid textured surfaces. When forming other functional layers on its surface, especially when using coating film deposition, the film-forming material can form a uniform flow and spread on the smooth top surface and arc-shaped depressions, avoiding the phenomenon of thinner thickness at sharp corners and excessively thick material accumulation at the bottom, thereby significantly improving the film quality.
[0052] Meanwhile, in the embodiments of this application, the textured structure of the semiconductor substrate contains rounded protrusions that transition through arc-shaped depressions, resulting in a continuous, undulating microstructure without planarizing the surface. This structure lacks sharp edges while retaining sufficient surface roughness. This moderate roughness provides more nucleation sites, enhancing the mechanical interlocking and chemisorption between the functional layer and the silicon substrate, thereby obtaining a dense, pinhole-free functional layer, improving crystal quality, and reducing surface defects.
[0053] In some embodiments of this application, the rounded bumps contained in the semiconductor substrate have at least one of the following characteristics: In the embodiments, the ratio of the height of the rounded bumps in the semiconductor substrate to the diameter of the bottom is (0.3 to 1.25):1. In exemplary examples, it can be a typical but non-limiting diameter ratio or any range between two ratios, such as 0.30:1, 0.45:1, 0.55:1, 0.60:1, 0.75:1, 0.85:1, 0.95:1, 1.00:1, 1.15:1, 1.25:1.
[0054] In the embodiments, the height of the rounded bumps in the semiconductor substrate is 1.5 μm to 2.5 μm. In the exemplary examples, it can be a typical but non-limiting height such as 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.95 μm, 2.0 μm, 2.1 μm, 2.2 μm, 2.3 μm, 2.4 μm, 2.5 μm, or any range between two height values.
[0055] In the embodiments, the diameter of the bottom of the rounded bump in the semiconductor substrate is 2 μm to 5 μm. In the exemplary examples, typical but non-limiting diameters such as 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, and 5 μm, or any range between two diameter values, are used.
[0056] In some embodiments, the rounded bumps contained in the semiconductor substrate include at least one of cone-shaped, hill-shaped, and pyramid-like tetrahedral shapes.
[0057] In some embodiments, the textured surface structure of the semiconductor substrate has at least one of the following features in the arc-shaped recessed structure at the bottom between adjacent rounded protrusions: In the embodiments, in the textured structure of the semiconductor substrate, the depth-to-width ratio of the arc-shaped recessed structure can be (0.15-5):1, optionally (0.2-0.8):1. In the exemplary examples, typical but non-limiting ratios such as 0.15:1, 0.5:1, 1:1, 2:1, 3:1, 4:1, and 5:1, or any range between two ratios, are also possible.
[0058] In the embodiments, the depth of the arc-shaped recessed structure in the textured surface of the semiconductor substrate is 0.3 μm to 1.5 μm. In the exemplary examples, typical but non-limiting depths such as 0.3 μm, 0.5 μm, 0.8 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, and 1.5 μm, or any range between two depths, are used.
[0059] In the embodiments, the width of the arc-shaped recessed structure in the textured structure of the semiconductor substrate is 0.3 μm to 2 μm. In the exemplary examples, typical but non-limiting widths such as 0.3 μm, 0.5 μm, 0.8 μm, 1.0 μm, 1.3 μm, 1.5 μm, 1.8 μm, and 2.0 μm, or any range between two widths, are used.
[0060] [Methods for fabricating semiconductor substrates] Secondly, embodiments of this application also provide a method for preparing the semiconductor substrate described in the above embodiments. The method for preparing the semiconductor substrate includes the following steps: S10: At least one surface of a semiconductor substrate is subjected to texturing etching to form a texturing surface with multiple randomly distributed pyramidal structures; S20: The textured surface generated in step S10 is subjected to rounding etching with a rounding etching solution to form rounded protrusions in the pyramid structure. Each rounded protrusion has a smooth top surface, and the bottom between adjacent rounded protrusions has an arc-shaped concave structure.
[0061] In the semiconductor substrate fabrication method of this application embodiment, texturing etching refers to a process step of anisotropically etching at least one surface of the semiconductor substrate using a chemical etching solution (commonly an alkaline solution). A pyramid structure refers to a microscopic protrusion, shaped like a square pyramid or approximately a square pyramid, formed on the surface of the semiconductor substrate through the aforementioned texturing etching process. This microscopic protrusion has a sharp top (pyramid tip), multiple edges, and V-shaped grooves (valleys) at the bottom between adjacent pyramids. Texturing refers to a rough surface region of the semiconductor substrate with regular or irregular microscopic undulations obtained after texturing etching. A circular etching solution refers to a chemical solution used to circularize the texturing surface with the pyramid structure. Circular etching refers to a process step of immersing or contacting the semiconductor substrate with the pyramid structure formed by texturing etching into the circular etching solution and performing chemical etching under specific conditions.
[0062] Therefore, the semiconductor substrate fabrication method of this application uses a randomly distributed pyramid structure formed on the surface of the semiconductor substrate through texturing etching as an intermediate template. A circular etching process is then performed on this pyramid structure, utilizing the differential effect of chemical etching on anisotropic morphology to precisely eliminate the sharp apex, edges, and V-shaped valleys between adjacent pyramids. This transforms the pyramid structure into rounded protrusions with smooth top surfaces and arc-shaped depressions between adjacent rounded protrusions. Furthermore, this circular etching process ensures that the overall texturing surface maintains sufficient undulation.
[0063] Step S10: The semiconductor substrate in step S10 can be of the type of semiconductor substrate described in the above application embodiments.
[0064] In some embodiments, the etching solution used in step S10 for textured etching may include a first alkaline compound, a first additive, and a first solvent.
[0065] In the embodiments, the mass content of the first solvent in the etching solution can be 80% to 98%. In the exemplary examples, it can be a typical but non-limiting content such as 80%, 83%, 85%, 88%, 90%, 93%, 93%, 95%, 98%, or a range between any two content values.
[0066] In the embodiments, the first solvent may include, but is not limited to, deionized water.
[0067] In the embodiments, the mass content of the first alkaline compound in the etching solution can be 0.2% to 4%. In exemplary examples, it can be a typical but non-limiting content such as 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, or a range between any two content values.
[0068] In the embodiments, the first alkali compound may include at least one of NaOH, KOH, etc.
[0069] In the embodiments, the first additive includes components such as a first surfactant, a first complexing agent, a first defoamer, a first stabilizer, a first corrosion inhibitor, and inorganic additives.
[0070] In the embodiments, the mass content of the first surfactant contained in the first additive in the etching solution can be 0.1% to 5%. In the exemplary examples, it can be a typical but non-limiting content such as 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or any range between two content values.
[0071] In the embodiments, the first surfactant contained in the first additive may include at least one of nonionic surfactants, anionic surfactants, etc. In an exemplary embodiment, the nonionic surfactant may include at least one of alkylphenol polyoxyethylene ethers, fatty alcohol polyoxyethylene ethers, polyoxyethylene ethers, etc.; in an exemplary embodiment, the anionic surfactant may include at least one of alkyl sulfonates, sodium fatty alcohol ether sulfate (AES), etc.
[0072] In the embodiments, the total mass content of the first complexing agent, the first defoamer, and the first stabilizer contained in the first additive is 0.1% to 10%. In the exemplary examples, it can be a typical but non-limiting content such as 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or any range between two content values.
[0073] In the embodiments, the first complexing agent contained in the first additive may include at least one of glucose, sodium gluconate, sodium citrate, sodium lactate, cyclodextrin, lignin sulfonate, etc.
[0074] In the embodiments, the first defoamer contained in the first additive may include at least one of polyether defoamers, sodium carboxymethyl cellulose (CMC), polyacrylamide (PAM), etc.
[0075] In the embodiments, the first stabilizer contained in the first additive may include at least one of sodium acetate, potassium sorbate, propylene glycol, glycerin, etc.
[0076] In the embodiments, the mass content of the first inorganic auxiliary agent contained in the first additive is 0.01% to 6%. In the exemplary examples, it can be a typical but non-limiting content such as 0.01%, 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, or any range between two content values.
[0077] In the embodiments, the first inorganic additive contained in the first additive may include at least one of sodium silicate (Na2SiO3), sodium carbonate, sodium bicarbonate, sodium phosphate, etc.
[0078] In the embodiments, the mass content of the first corrosion inhibitor contained in the first additive is 0.1% to 3%. In the exemplary examples, it can be a typical but non-limiting content such as 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, or any range between two content values.
[0079] In the embodiments, the first corrosion inhibitor contained in the first additive may include at least one of disodium EDTA, sodium metasilicate, etc.
[0080] The content and types of the above-mentioned components in the etching solution used for textured surface etching can effectively improve the efficiency of textured surface etching, thereby improving the efficiency of textured surface etching and the effect of forming textured surface structure.
[0081] In some embodiments, the temperature of the texturing etching process in step S10 can be 70°C to 90°C. In exemplary cases, it can be a typical but non-limiting temperature such as 70°C, 73°C, 75°C, 78°C, 80°C, 83°C, 85°C, 88°C, or 90°C, or a range between any two content values.
[0082] In some embodiments, when the temperature of the texturing etching process in step S10 is 70°C to 90°C, the time of the texturing etching process can be 150 to 850 s. In the example, it can be a typical but non-limiting range of seconds such as 150 s, 200 s, 300 s, 400 s, 500 s, 600 s, 700 s, 800 s, 850 s, or any two seconds.
[0083] Step S20: In some embodiments, the spherical etching solution comprises the following components by mass percentage, based on 100% of the total mass of the spherical etching solution: Solvent 85%–94%; Alkali compounds 0.05%–4%; Cosolvent 1%–5%; Surfactant 1%–5%; Complexing agent 1%–3%; Corrosion inhibitor 0.5%–4%; Defoamer 0.1%–3%; pH adjuster 0.1%–3%.
[0084] To distinguish the first solvent, first alkali compound, first surfactant, first complexing agent, first defoamer, first stabilizer, and first corrosion inhibitor contained in the etching solution for textured etching in step S10, the solvent, alkali compound, surfactant, complexing agent, and corrosion inhibitor contained in the circular etching solution are respectively named the second solvent, second alkali compound, second surfactant, second complexing agent, and second corrosion inhibitor.
[0085] In the embodiments, based on the fact that the mass content of the second solvent contained in the circular etching solution is 85% to 94%, in the exemplary examples, the mass content of the second solvent can be a typical but non-limiting content such as 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, or any range between two content values.
[0086] In the embodiments, the second solvent contained in the circular etching solution may include water. In the exemplary example, the water may include at least one of deionized water, ultrapure water, etc.
[0087] In the embodiments, the mass content of the second alkaline compound contained in the circular etching solution is 0.05% to 4%, and optionally 0.2% to 4%. In the exemplary examples, the mass content of the first solvent can be a typical but non-limiting content such as 0.05%, 0.1%, 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, or a range between any two content values.
[0088] In the embodiments, the second alkaline compound contained in the circular etching solution includes at least one of sodium hydroxide (NaOH), potassium hydroxide (KOH), and ammonium hydroxide (NH4OH). In the embodiments, based on the fact that the mass content of the co-solvent in the circular etching solution is 1% to 5%, in the exemplary examples, the mass content of the co-solvent can be a typical but non-limiting content such as 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or any range between two content values.
[0089] In the embodiments, the co-solvent contained in the circular etching solution may include at least one of ethylene glycol, propylene glycol, and glycerin.
[0090] In the embodiments, the mass content of the second surfactant contained in the circular etching solution is 1% to 5%. In the exemplary examples, it can be a typical but non-limiting content such as 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or any range between two content values.
[0091] In the embodiments, the second surfactant contained in the circular etching solution may include at least one of a nonionic surfactant and anionic surfactant; wherein, the nonionic surfactant may include at least one of fatty alcohol polyoxyethylene ether, polyoxyethylene polyoxypropylene ether, and Tween-80; in the exemplary example, the anionic surfactant may include at least one of fatty alcohol ether sodium sulfate, alkyl sulfonate, etc.
[0092] In the embodiments, based on the fact that the mass content of the second complexing agent contained in the circular etching solution is 1% to 3%, in the exemplary examples, it can be a typical but non-limiting content such as 1%, 1.2%, 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8%, 3%, or any range between two content values.
[0093] In the embodiments, the second complexing agent contained in the circular etching solution may include at least one of sodium gluconate, sodium citrate, sodium lactate, disodium EDTA, phytic acid, etc.
[0094] In the embodiments, the mass content of the second corrosion inhibitor contained in the circular etching solution is 0.5% to 4%. In the exemplary examples, it can be a typical but non-limiting content such as 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, or any range between two content values.
[0095] In the embodiments, the second etching inhibitor contained in the circular etching solution may include at least one of sodium silicate, chitosan, tannic acid, resveratrol, carboxymethyl cellulose, polyvinylpyrrolidone, etc.
[0096] In the embodiments, the mass content of pH adjuster contained in the circular etching solution is 0.1% to 3%. In the exemplary examples, it can be a typical but non-limiting content such as 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, or any range between two content values.
[0097] In the embodiments, the circular etching solution contains at least one of the pH adjusters sodium carbonate, sodium bicarbonate, and sodium acetate.
[0098] In the embodiments, the mass content of the second defoamer in the circular etching solution is 0.1% to 3%. In the exemplary examples, the mass content of the second defoamer can be a typical but non-limiting content such as 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, or any range between two content values.
[0099] In the embodiments, the second defoamer contained in the circular etching solution may include at least one of polyether modified silicone oil, silicone emulsion, etc.
[0100] In some embodiments, the temperature of the circular etching process in step S20 can be 30°C to 80°C. In an exemplary example, it can be a typical but non-limiting temperature such as 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, or any range between two temperature values.
[0101] In some embodiments, the temperature of the circular etching process in step S20 can be 30°C to 80°C, and the time of the circular etching process can be 150 to 850 s. In the example, it can be a typical but non-limiting range of seconds or any two seconds, such as 150 s, 200 s, 300 s, 400 s, 500 s, 600 s, 700 s, 800 s, 850 s.
[0102] Based on the components contained in the aforementioned spherical etching solution, further controlling the temperature and time of the spherical etching solution within the aforementioned range can optimize the size of the spherical protrusions formed by the spherical etching process. For example, the relevant dimensions of the spherical protrusions formed by the spherical etching process and the arc-shaped recessed structure at the bottom between adjacent spherical protrusions can be controlled within the size range of the spherical protrusions and arc-shaped recessed structures contained in the textured structure of the semiconductor substrate in the embodiments of the above application.
[0103] In some embodiments, after the circular etching process in step S20, subsequent processing steps such as cleaning and drying of the semiconductor substrate after the circular etching process may be included.
[0104] [Circular Etching Solution] Thirdly, embodiments of this application provide a circular etching solution. The circular etching solution of this application embodiment is used on a semiconductor substrate containing circular bumps as described in the above application embodiments and comprises the following components in weight percentage: Solvent 85%–94%; Alkali compounds 0.05%–4%; Cosolvent 1%–5%; Surfactant 1%–5%; Complexing agent 1%–3%; Corrosion inhibitor 0.5%–4%; pH adjuster 0.1%–3%; Defoamer 0.1%–3%.
[0105] The circular etching solution in this application embodiment can perform circular etching on the pyramid structure in the textured surface of the semiconductor substrate, so that the top of the pyramid structure tip is etched to form a circular protrusion, and the circular protrusion has a smooth top surface; at the same time, the V-shaped corners at the junction of adjacent pyramid structures are etched to form an arc-shaped concave structure.
[0106] In the embodiments, the specific compounds that can be selected for each component of the above-mentioned circular etching solution are the same as the specific compounds that can be selected for each component of the circular etching solution in ratio S20 of the semiconductor substrate preparation method described above. To save space, they will not be repeated here.
[0107] [Solar Cell] Fourthly, embodiments of this application provide a solar cell. The solar cell of this application includes a semiconductor substrate, which is either a conductive substrate as described in the above-described application embodiments or a semiconductor substrate prepared by the semiconductor substrate preparation method described in the above-described application embodiments.
[0108] Since the solar cell of this application embodiment contains the semiconductor substrate described in the above application embodiment, the multiple rounded protrusions and the arc-shaped depressions at the bottom between adjacent rounded protrusions in the textured structure of the semiconductor substrate ensure that the functional film layer of the solar cell disposed on one side of the textured surface of the semiconductor substrate has relatively uniform film thickness or crystallinity at the rounded protrusions, adjacent rounded protrusions, and arc-shaped depressions. This effectively overcomes the undesirable phenomenon of thinner thickness at the sharp corners and excessively thick material accumulation at the bottom of the traditional pyramid textured surface. This significantly reduces recombination losses and leakage channels caused by uneven coverage of the functional film layer, improving the photoelectric performance of the solar cell, such as fill factor and open-circuit voltage.
[0109] Furthermore, the rounded protrusions and arc-shaped depressions in the textured semiconductor substrate structure of this application embodiment can eliminate microscopic sharp corners, reducing stress concentration and interface defect density at the corners of the functional layers formed on its surface, thereby reducing carrier recombination and improving minority carrier lifetime. In addition, compared with the traditional pyramidal textured surface, the textured surface with rounded protrusions and arc-shaped depressions can effectively scatter and trap incident light, improve its omnidirectional reflectivity, and increase the light utilization rate of the photoactive layer.
[0110] In some embodiments, the solar cell in this application is a tandem solar cell. Alternatively, it can be a single-junction solar cell, in which case it is a crystalline silicon solar cell.
[0111] In the embodiments, when the solar cell of this application is a tandem solar cell, the structure of the tandem solar cell is as follows: Figure 1As shown, it includes a crystalline silicon sub-cell 10 and a perovskite sub-cell 30. The crystalline silicon sub-cell 10 contains the semiconductor substrate 14, and the perovskite sub-cell 30 is disposed on the textured surface of the crystalline silicon sub-cell 10 near the semiconductor substrate 14. In this way, the thickness or crystallinity of the various functional layers, including the perovskite active layer 32, in the textured surface of the semiconductor substrate 14 is relatively uniform. This effectively overcomes the undesirable phenomenon of thinner thickness at the pyramidal corners and excessively thick material accumulation at the valleys in traditional pyramidal textured surfaces. It can significantly reduce recombination losses and leakage channels caused by uneven functional layer coverage, and improve the photoelectric performance of the solar cell, such as the fill factor and open-circuit voltage. Simultaneously, it can reduce stress concentration and interface defect density of the various functional layers in the perovskite sub-cell 30 at the rounded protrusions and arc-shaped depressions, thereby reducing carrier recombination and improving the photoelectric efficiency of the solar cell.
[0112] Meanwhile, the functional layers contained in the perovskite sub-cell 30 are formed on the textured surface of the semiconductor substrate 14 contained in the crystalline silicon sub-cell 10. Therefore, the functional layers contained in the perovskite sub-cell 30 effectively scatter and trap incident light, reduce its omnidirectional reflectivity, and improve the utilization rate of light by the photoactive layer.
[0113] In the embodiments, in such Figure 1 In the tandem solar cell shown, the crystalline silicon sub-cell 10 includes a back field electrode 11, a p-type window layer 12, a first passivation layer 13, a semiconductor substrate 14, a second passivation layer 15, and an n-type window layer 16, which are stacked sequentially.
[0114] In the embodiments, in such Figure 1 In the tandem solar cell shown, the back field electrode 11 of the crystalline silicon sub-cell 10 may include a metal electrode layer 111. The metal electrode layer 111 efficiently collects holes vented from the p-type window layer 12 and reflects unused long-wavelength photons back into the crystalline silicon sub-cell 10 for secondary absorption.
[0115] Understandably, the metal electrode layer 111 is selected from either a metal gate electrode or a fully covered metal film. The metal gate electrode is arranged in a patterned structure on the back of the crystalline silicon sub-cell 10, suitable for scenarios where light needs to enter from one side of the crystalline silicon sub-cell 10. The fully covered metal film covers the entire back of the crystalline silicon sub-cell 10, suitable for scenarios where light does not need to enter from one side of the crystalline silicon sub-cell 10.
[0116] In the embodiments, in such Figure 1In the illustrated tandem solar cell, the back field electrode 11 of the crystalline silicon sub-cell 10 may further include a transparent electrode layer 112, which is disposed between the p-type window layer 12 and the metal electrode layer 111. The transparent electrode layer 112 reduces the interfacial contact resistance, allowing photogenerated carriers to flow smoothly out, thus uniformly conducting current to the metal electrode layer 111. The metal electrode layer 111 efficiently collects and extracts photogenerated carriers and reflects unused long-wavelength photons back into the crystalline silicon sub-cell 10 for secondary absorption, thereby improving the photoelectric conversion efficiency of the crystalline silicon sub-cell 10.
[0117] In the embodiments, the thickness of the transparent electrode layer 112 is 15 nm to 60 nm. In exemplary embodiments, the thickness of the transparent electrode layer 112 can be a typical but non-limiting thickness of 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, or 60 nm, or a range between any two thickness values.
[0118] In the embodiments, the material of the transparent electrode layer 112 includes at least one of indium tin oxide (ITO), indium zinc oxide (IZO), tungsten-doped indium oxide (IWO), zirconium-doped indium oxide (IZrO), fluorine-doped tin oxide (FTO), aluminum-doped zinc oxide (AZO), antimony-doped tin oxide (ATO), and gallium-doped zinc oxide (GZO).
[0119] In the embodiments, the thickness of the metal electrode layer 111 can be 100 nm to 30 μm, optionally 100 nm to 20 μm, 2 μm to 30 μm. In the exemplary examples, the thickness of the metal electrode layer 111 is a typical but non-limiting thickness such as 100 nm, 500 nm, 1 μm, 2 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, or any range between two thickness values.
[0120] In the embodiments, the material of the metal electrode layer 111 includes at least one of aluminum (Al), copper (Cu), silver (Ag), gold (Au), and silver-plated copper. Aluminum is suitable for the metal electrode layer 111 that covers the entire transparent electrode layer 112, while silver, copper, and silver-plated copper are suitable for the metal electrode layer 111 that patternedly covers the transparent electrode layer 112.
[0121] In a further embodiment, the back electrode 11 further includes an adhesion layer disposed between the metal electrode layer 111 and the transparent electrode layer 112. The adhesion layer serves to adhere the metal electrode layer 111 to the transparent electrode layer 112 and also prevents metal atoms in the metal electrode layer 111 from diffusing into the transparent electrode layer 112 and the p-type window layer 12. The adhesion layer is made of at least one of titanium (Ti), chromium (Cr), nickel (Ni), and cobalt (Co), preferably titanium, chromium, or a composite structure of titanium and chromium. The thickness of the adhesion layer is 5–20 nm.
[0122] In a further embodiment, the back electrode 11 further includes an optical matching layer, which is disposed between the transparent electrode layer 112 and the metal electrode layer 111. Figure 1 (Not shown). The refractive index of the optical matching layer is lower than that of the transparent electrode layer 112. The transparent electrode layer 112, the optical matching layer, and the metal electrode layer 111 constitute an interference-type back reflection structure, which improves back reflection efficiency and light utilization through optical interference effect. In the example, the material of the optical matching layer includes at least one of silicon oxide, aluminum oxide, silicon nitride, sodium fluoride, lithium fluoride, silver fluoride, and calcium fluoride.
[0123] In the embodiments, such as Figure 1 In the tandem solar cell shown, the thickness of the p-type window layer 12 in the crystalline silicon sub-cell 10 can be 5 nm to 30 nm. In an exemplary example, the material of the p-type window layer 22 may include p-type hydrogenated nanocrystalline silicon (p-nc-Si:H) or p-type hydrogenated oxide nanocrystalline silicon (p-nc-SiO). x p-type hydrogenated amorphous silicon (pa-Si:H), p-type silicon carbide nanocrystals (p-nc-SiC:H), p-type amorphous silicon oxide (pa-SiO) x At least one of p-type hydrogenated nanocrystalline silicon (p-nc-Si:H) or p-type hydrogenated oxide nanocrystalline silicon (p-nc-SiO) can be used, optionally p-type hydrogenated nanocrystalline silicon (p-nc-SiO). x :H).
[0124] In the embodiments, such as Figure 1 In the tandem solar cell shown, the semiconductor substrate 14 of the crystalline silicon sub-cell 10 can have a thickness of 80–220 μm. It is primarily used to absorb light and generate charge carriers (holes and electrons). The p-type window layer 12 and the n-type window layer 16 form a PN junction, generating a built-in electric field to separate electrons and holes. The back electrode 11 is used to collect and output the photocurrent, while simultaneously reflecting long-wavelength light not absorbed by the crystalline silicon sub-cell 10 back to the crystalline silicon sub-cell 10 to improve light utilization. In the exemplary example, the semiconductor substrate 14 can be an n-type monocrystalline silicon substrate.
[0125] In the embodiments, in such Figure 1In the cascaded solar cell shown, the first passivation layer 13 and the second passivation layer 15 contained in the crystalline silicon sub-cell 10 may be the same or different, and may be intrinsic hydrogenated amorphous silicon (a-Si:H(i)).
[0126] In the embodiments, in such Figure 1 In the tandem solar cell shown, the thickness of the n-type window layer 16 in the crystalline silicon sub-cell 10 can be 5 nm to 30 nm. In an exemplary example, the material of the n-type window layer 16 may include n-type hydrogenated nanocrystalline silicon (n-nc-Si:H) or n-type hydrogenated oxide nanocrystalline silicon (n-nc-SiO). x n-type hydrogenated amorphous silicon (na-Si:H), n-type amorphous silicon oxide (na-SiO) x At least one of n-type silicon carbide (n-SiC:H(n)) and n-type hydrogenated nanocrystalline silicon (n-nc-Si:H) or n-type hydrogenated oxide nanocrystalline silicon (n-nc-SiO) can be used. x :H).
[0127] In the embodiments, in such Figure 1 In the cascaded solar cell shown, the composite layer 20 is disposed between the crystalline silicon sub-cell 10 and the perovskite sub-cell 30 to achieve electrical series connection and reduce interface charge recombination loss.
[0128] In the embodiments, the material of the composite layer 20 can be a transparent conductive oxide, including but not limited to indium tin oxide (ITO), indium zinc oxide (IZO), tungsten-doped indium oxide (IWO), zirconium-doped indium oxide (IZrO), fluorine-doped tin oxide (FTO), aluminum-doped zinc oxide (AZO), antimony-doped tin oxide (ATO), and gallium-doped zinc oxide (GZO). The transparent conductive oxide can be prepared by methods including but not limited to magnetron sputtering (PVD) and reactive plasma deposition (RPD).
[0129] In the embodiments, when the material of the composite layer 20 is a transparent conductive oxide, the thickness of the composite layer 20 can be 50 to 500 nm. For example, the thickness of the transparent conductive oxide composite layer can be a typical but non-limiting thickness such as 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 120 nm, 140 nm, 150 nm, 200 nm, 220 nm, 250 nm, 270 nm, 300 nm, 320 nm, 350 nm, 370 nm, 400 nm, 420 nm, 450 nm, 470 nm, 500 nm, or any range between two thickness values.
[0130] In the embodiments, the material of the composite layer 20 can also be a tunnel junction, such as a tunnel junction with an n+-Si / p+-Si (microcrystalline / nanocrystalline silicon) structure.
[0131] In the embodiments, when the material of the composite layer 20 is a tunnel junction, the thickness of the composite layer 20 can be 20 to 60 nm. For example, the thickness of the composite layer 20 can be a typical but non-limiting thickness such as 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, or any range between two thickness values.
[0132] In the embodiments, in such Figure 1 In the stacked solar cell shown, along the direction away from the crystalline silicon sub-cell 10, the perovskite sub-cell 30 includes a hole transport layer 31, a perovskite active layer 32, an electron transport layer 33, a buffer layer 34, a transparent conductive layer 35, and an electrode grid line 36 stacked sequentially, and also includes an anti-reflection layer 37, which is disposed on the surface of the transparent conductive layer 35 that is not covered by the electrode grid line 36.
[0133] In the embodiments, in such Figure 1 In the tandem solar cell shown, the hole transport layer 31 contained in the perovskite subcell 30 can have a thickness of 10 nm to 100 nm, and more specifically, 20 nm to 50 nm.
[0134] In the embodiments, in such Figure 1 In the tandem solar cell shown, the hole transport layer 31 of the perovskite sub-cell 30 may include a self-assembled monolayer 311. The self-assembled monolayer 311 can form a dense and uniform monolayer on the surface of the composite layer 20 through self-assembly, thereby effectively adjusting the interfacial electronic structure between the composite layer 20 and the perovskite active layer 32, promoting efficient hole transport, and reducing interfacial nonradiative recombination losses.
[0135] In the embodiments, the thickness of the self-assembled monolayer 311 can be 0.5 nm to 3 nm. In the exemplary examples, it can be a typical but non-limiting thickness such as 0.5 nm, 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, or any range between two thickness values.
[0136] In the embodiments, the self-assembled monolayer (SAM) material of the self-assembled monolayer 311 is generally composed of anchoring groups, alkyl bridges and terminal groups.
[0137] In the embodiments, the anchoring groups of the above-mentioned SAM material contain polar atoms such as oxygen, phosphorus, and sulfur, and exist in the form of active functional groups such as phosphonic acid groups (-PO(OH)2), carboxyl groups (-COOH), hydroxyl groups (-OH), and thiol groups (-SH), which can form covalent bonds, coordination bonds, or hydrogen bonds with the surface of the composite layer 20, thereby achieving firm anchoring; In the embodiments, the terminal groups of the above-mentioned SAM material may include carbazole groups, dibenzocarbazole groups, acridine groups, phenothiazine groups, or phenyl groups. The terminal groups have a conjugated structure, and their π-electron clouds can compensate for the charge of halogen vacancies in the perovskite active layer 32, thereby filling the shallow energy level defects caused by halogen vacancies. Specifically, the nitrogen atoms of nitrogen-containing terminal groups such as carbazole groups, dibenzocarbazole groups, acridine groups, and phenothiazine groups contain lone pairs of electrons, which can interact with uncoordinated divalent cations (e.g., lead ions Pb) on the surface of the perovskite active layer 32. 2+ This forms coordination bonds, thereby precisely passivating deep-level defects caused by uncoordinated divalent cations.
[0138] In the embodiments, substituents may be further introduced onto the terminal groups of the aforementioned SAM material. These substituents can regulate the electron cloud density of the terminal groups, enhancing their coordination strength with uncoordinated divalent cations and improving defect passivation efficiency. Simultaneously, the substituents can form coordination bonds with uncoordinated divalent cations on the surface of the perovskite active layer 32, or occupy halogen vacancies through their own electronegativity and lone pair electrons, achieving charge compensation and space filling at defect sites, thereby effectively suppressing grain boundary defects. Exemplarily, the substituents include at least one of halogen substituents, alkyl groups, alkoxy groups, benzene substituents, and bis(4-methoxyphenyl)amino groups.
[0139] In the embodiments, the alkyl chain bridges of the above-mentioned SAM material are the "backbone" connecting the anchoring group and the terminal group, and are usually composed of saturated carbon chains. The length of the alkyl chain bridges directly determines the spatial distance between the anchoring group and the terminal group, and their chain length and chemical properties further affect the molecular order, conductivity and steric hindrance effect of the self-assembled monolayer material.
[0140] In the embodiments, the above-mentioned SAM material may include [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz, CAS No. 20999-38-6), [2-(3,6-dimethyl-9H-carbazole-9-yl)ethyl]phosphonic acid (Me-2PACz, CAS No. 2996161-30-7), [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz, CAS No. 2377770-18-6), and [2-(3,6-diphenyl-9H-carbazole-9-yl)ethyl]phosphonic acid (Ph-2PACz, CAS No. 3085827-62-6). [2-(3,6-Diiodo-9H-carbazole-9-yl)ethyl]phosphonic acid (I-2PACz, CAS No. 3026275-69-1), [2-(3,6-dibromo-9H-carbazole-9-yl)ethyl]phosphonic acid (Br-2PACz, CAS No. 2762888-11-7), [2-(3,6-dichloro-9H-carbazole-9-yl)ethyl]phosphonic acid (Cl-2PACz, CAS No. 3036926-72-1), [2-(3,6-difluoro-9H-carbazole-9-yl)ethyl]phosphonic acid (F-2PACz, CAS No. 3036926-69-6), [2-(7H-dibenzocarbazole) [2-(9H-9'-phenyl-3,3'-dicarbazole-9-yl)ethyl]phosphoric acid (2PADCB, CAS No. 2882156-61-6), [2-(9H-9'-phenyl-3,3'-dicarbazole-9-yl)ethyl]phosphoric acid (2PABCz), [4-(9H-carbazole-9-yl)butyl]phosphoric acid (4PACz, CAS No. 20999-36-4), [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz, CAS No. 2747959-96-0), [4-(3,6-dimethoxy-9H-carbazole-9-yl)butyl]phosphonic acid (MeO-4PACz, CAS No. 2922526-5) 6-3), [4-(3,6-diphenyl-9H-carbazole-9-yl)butyl]phosphoric acid (Ph-4PACz, CAS No. 2814500-04-2), [4-(3,6-diiodo-9H-carbazole-9-yl)butyl]phosphonic acid (I-4PACz, CAS No. 3026275-67-9), [4-(3,6-dibromo-9H-carbazole-9-yl)butyl]phosphonic acid (Br-4PACz, CAS No. 2996161-28-3), [4-(3,6-dichloro-9H-carbazole-9-yl)butyl]phosphonic acid (Cl-4PACz, CAS No. 3026275-66-8), [4-(3,[6-Difluoro-9H-carbazole-9-yl)butyl]phosphonic acid (F-4PACz, CAS No. 3026275-65-7), [4-[3-bromo-6-(4-methoxyphenyl)-9H-carbazole-9-yl]butyl]phosphonic acid (BrMeOPh-4PACz, CAS No. 3053380-37-0), [4-(3,6-di-tert-butyl-9H-carbazole-9-yl)butyl]phosphonic acid (tBu-4PACz, CAS No. 3023627-39-3), [4-(7H-dibenzo-carbazole-7-yl)butyl]phosphonic acid (4PADCB, CAS No. 2882156-63-8), [4-(9H-9` [Phenylacetic-3,3'-dicarbazole-9-yl)butyl]phosphoric acid (4PABCz), [4-(2,7-dibromo-9,9-dimethylacridin-10(9H)-yl)butyl]phosphonic acid (2Br-4DMAcPA / DMAcPA, CAS No. 2971088-37-4), [2-(3,7-dibromo-10H-phenthiazin-10-yl)ethyl]phosphonic acid (Br-2EPT, CAS No. 2826271-17-2), and [2-(4-(bis(4-methoxyphenyl)amino)phenyl)-1-cyanovinyl]phosphonic acid (MPA-CPA, CAS No. 2212003-31-9)]phosphonic acid.
[0141] In the embodiments, the self-assembled monolayer 311 described above can be prepared according to the following preparation process: First, the self-assembled monolayer material is mixed with a solvent and stirred until completely dissolved to obtain a self-assembled monolayer solution. Then, the self-assembled monolayer solution is coated to obtain a wet film. Finally, it is heated and annealed at a temperature of 80℃~120℃ for 5 min~20 min to form a self-assembled monolayer 311.
[0142] In the embodiments, the concentration of the self-assembled monolayer material in the above-mentioned self-assembled monolayer solution can be from 0.1 mg / mL to 3 mg / mL. In the embodiments, the solvent is selected from at least one of ethanol, isopropanol, and methanol.
[0143] In this embodiment, the coating process of the self-assembled monolayer solution includes spin coating, blade coating, slot coating, and inkjet printing. Exemplarily, the process parameters for inkjet printing can be: nozzle diameter of 10 μm to 50 μm, determining droplet volume of 1 p1 to 100 p1; driving voltage typically of 20 V to 100 V, used to control droplet speed and morphological stability; substrate temperature generally controlled at 40°C to 80°C, used to regulate solvent evaporation rate and crystallization quality; printing resolution of 300 dpi to 1200 dpi, affecting pattern accuracy and film uniformity.
[0144] In the embodiments, in such Figure 1 In the tandem solar cell shown, the hole transport layer 31 of the tantalum sub-cell 30 may further include a transition metal oxide layer 312, which is disposed between the self-assembled monolayer 311 and the composite layer 20. The transition metal oxide layer 312 has excellent stability and high work function, providing good hole transport channels and electron blocking capabilities. The surface of the transition metal oxide layer 312 is rich in hydroxyl groups. The anchoring groups of the self-assembled monolayer material form covalent or coordinate bonds with the metal ions and hydroxyl groups on the surface of the transition metal oxide, promoting the dense and uniform formation of the self-assembled monolayer 311. The terminal groups of the self-assembled monolayer material, on the one hand, compensate for the charge of halogen vacancies in the perovskite active layer 32 through the conjugated π electron cloud, and on the other hand, can form coordinate bonds with uncoordinated divalent cations on the surface of the perovskite active layer 32, achieving dual passivation of interface defects. At the same time, the precise control of the interface energy level arrangement reduces the hole extraction barrier and effectively suppresses non-radiative recombination at the interface.
[0145] In the embodiments, the material of the transition metal oxide layer 312 may include at least one of nickel oxide, copper oxide, cobalt tetroxide, and ferric oxide. The preparation methods of the transition metal oxide layer 312 include solution methods, physical vapor deposition (PVD), atomic layer deposition (ALD), inkjet printing, etc.
[0146] In the embodiments, the thickness of the transition metal oxide layer 312 can be 1 to 20 nm. In the exemplary examples, it can be a typical but non-limiting thickness such as 1 nm, 2 nm, 5 nm, 10 nm, 15 nm, 20 nm, or any range between two thickness values.
[0147] In the embodiments, in such Figure 1 In the tandem solar cell shown, the thickness of the perovskite active layer 32 contained in the perovskite sub-cell 30 can be 100 nm to 1000 nm.
[0148] In the embodiments, the perovskite active layer 32 includes a perovskite structure material with the general formula ABX3; wherein, A is a monovalent cation, including at least one of a monovalent metal cation and a monovalent organic cation, B is a divalent cation, and X is a monovalent anion.
[0149] In the example, A in ABX3 can be a monovalent metal cation, including cesium ions (Cs). + ), rubidium ions (Rb + Lithium ion (Li) + Sodium ions (Na) + ), potassium ions (K) + ) and thallium ions (Tl + At least one of the following, preferably cesium ion (Cs) +).
[0150] In the example, A in ABX3 can be a monovalent organic cation, which includes ammonium ions (NH4+). + ), Methylamine ion (MA)(CH3NH3) + ), ethylammonium ion (CH3CH2NH3) + ), dimethylamine ion ((CH3)2NH2 + ), trimethylammonium ion ((CH3)3NH + ), tetramethylammonium ion ((CH3)4N + ), formamidinium ion (FA)(HC(NH2)2 + ), Methylformamidinium ion (CH3C(NH2)2 + Acetamidinium ion (H3C2(NH2)2) + ), guanidine ion (C(NH2)3) + At least one of the following.
[0151] In the example, the divalent cation represented by B in ABX3 includes lead ions (Pb). 2+ ), tin ions (Sn) 2+ ) and germanium ions (Ge 2+ At least one of the following, preferably lead ion (Pb) 2+ ).
[0152] In the example, the monovalent anion represented by X in ABX3 includes halide anions, and halide anions include bromide ions (Br). - ), iodide ions (I) - ), chloride ions (Cl) - At least one of the following, preferably iodide ions (I) - ).
[0153] In the example, the molecular formulas of the ABX3 perovskite structures are CsPbI3, FAPbI3, MAPbI3, and CsPbI3. 0.3 MA 0.7 Pb(I 0.9 Br 0.1 3. Cs 0.05 FA 0.8 MA 0.15 PbI3, Cs 0.05 FA 0.75 MA 0.2 Pb(I 0.75 Br 0.25 3. Cs 0.05 FA 0.8 MA 0.15 Pb(I) 0.8 Br 0.2 )3 or Cs 0.02FA 0.74 MA 0.24 Pb(Br 0.24 I 0.76 3. This application does not limit the specific composition of perovskite structural materials.
[0154] Monovalent anions also include thiocyanate ions (SCN). - ) and tetrafluoroborate ion (BF4) - At least one of the following, thiocyanate ion (SCN) - ), tetrafluoroborate ion (BF4) - It can partially replace halide anions to reduce carrier recombination, prevent halogen migration, suppress photo-induced phase separation, regulate band gap, and improve crystallization.
[0155] In the embodiments, the perovskite active layer 32 can be prepared using a one-step or two-step preparation process. The one-step preparation process includes a solution-based one-step process and a vapor-phase one-step process. In an exemplary embodiment, the solution-based one-step process for preparing the perovskite active layer 32 includes: coating a perovskite precursor solution to form a perovskite precursor layer, and annealing to obtain the perovskite active layer 32. The vapor-phase one-step process for preparing the perovskite active layer 32 includes: performing multi-source co-evaporation on the perovskite precursor material to form a perovskite precursor layer, and annealing to obtain the perovskite active layer 32. The purpose of annealing is to drive the perovskite precursor material to undergo a chemical reaction and crystallize to form the perovskite active layer 32, while simultaneously removing residual solvent.
[0156] In the embodiments, the annealing temperature for preparing the perovskite active layer 32 using the one-step solution method is 90–150 °C. In the exemplary examples, the annealing temperature for preparing the perovskite active layer 32 using the one-step solution method can be 90 °C, 100 °C, 110 °C, 120 °C, 130 °C, 140 °C, 150 °C, or any range between any two of the aforementioned values. In the embodiments, the annealing time for preparing the perovskite active layer 32 using the one-step solution method is 5 min–30 min. In the exemplary examples, the annealing time for preparing the perovskite active layer 32 using the one-step solution method can be 5 min, 10 min, 15 min, 20 min, 25 min, 30 min, etc., which are typical but non-limiting thicknesses or any range between two thickness values.
[0157] In the embodiments, when the perovskite active layer 32 is prepared by a one-step solution method, the coating can be done by slot coating, blade coating, or spin coating, and this application does not limit the method.
[0158] It is important to note that during the one-step solution preparation of the perovskite active layer 32, an antisolvent can be added dropwise during the coating process, especially in small-area coatings such as spin coating, to precisely control the crystallization process of the perovskite. This ultimately yields a highly dense, low-defect, and high-phase-purity perovskite active layer 32. The antisolvent includes at least one of chlorobenzene, dichlorobenzene, diethyl ether, dichloromethane, chloroform, anisole, toluene, and ethyl acetate. After coating the perovskite precursor solution, a vacuum crystallization drying (VCD) process is performed to obtain the perovskite precursor layer. The vacuum crystallization drying process rapidly and uniformly removes the solvent from the perovskite precursor layer in a precisely controllable vacuum environment. This avoids the problems of contamination, poor uniformity, and difficulty in mass production caused by antisolvent processes, making it suitable for the needs of large-area, industrial-scale perovskite layer preparation.
[0159] In the embodiments, when the perovskite active layer 32 is prepared using a one-step solution method, the molar concentration of the perovskite precursor material in the prepared perovskite precursor solution is 1–2 mol / L during the preparation of the perovskite pre-layer. In exemplary cases, the molar concentrations are 1 mol / L, 1.2 mol / L, 1.5 mol / L, 1.8 mol / L, 2 mol / L, etc. The solvent may include at least one of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), dimethyl sulfoxide (DMSO), 2-methoxyethanol (2-Me), N,N'-dimethylacrylurea (DMPU), 1,3-dimethyl-2-imidazolinone (DMI), N,N-diethylformamide (DEF), and sulfolane. Optionally, the solvent may be a combination of DMF and NMP, a combination of DMF and DMI, or a combination of DMF and DMSO.
[0160] When the solvent is a combination of DMF and NMP, the volume ratio of DMF to NMP is 4:1; When the solvent is a combination of DMF and DMI, the volume ratio of DMF to DMI is 9:1; When the solvent is a combination of DMF and DMSO, the volume ratio of DMF to DMSO is 4:1.
[0161] In the embodiments, the perovskite precursor material used to formulate the perovskite precursor solution may include a first precursor compound and a second precursor compound. The first precursor compound has the chemical formula AX and includes at least one of FAI (formamidine iodide), FABr (formamidine bromide), FACl (formamidine chloride), MAI (methylammonium iodide), MABr (methylammonium bromide), CsI (cesium iodide), CsBr (cesium bromide), and CsCl (cesium chloride). The second precursor compound has the chemical formula BX2 and includes at least one of PbI2 (lead iodide), PbBr2 (lead bromide), SnI2 (stannous iodide), and SnBr2 (stannous bromide).
[0162] Understandably, the molar ratio of the first precursor compound to the second precursor compound is usually 1:1, so as to control the molar ratio of A ions, B ions, and X ions to be 1:1:3. In this way, after annealing, a perovskite structure with the general formula ABX3 can be obtained to form the perovskite active layer 32.
[0163] In the embodiments, the perovskite precursor material used to prepare the perovskite precursor solution can also be classified into organic precursor compounds and inorganic precursor compounds. The organic precursor compounds include at least one of FAI (formamidine iodide), FABr (formamidine bromide), FACl (formamidine chloride), MAI (methylammonium iodide), and MABr (methylammonium bromide). The inorganic precursor compounds include at least one of CsI (cesium iodide), CsBr (cesium bromide), PbI2 (lead iodide), PbBr2 (lead bromide), SnI2 (stannous iodide), and SnBr2 (stannous bromide).
[0164] In this embodiment, when a two-step method is used to prepare the perovskite active layer 32, the process involves separately forming an organic precursor compound and an inorganic precursor compound into films in two steps, followed by annealing and crystallization to obtain the perovskite active layer 32. In this embodiment, the process for forming the film with the organic or inorganic precursor compound includes wet coating or vapor deposition; wherein, wet coating includes spin coating, blade coating, slot coating, spraying, and screen printing. Vapor deposition includes evaporation.
[0165] In the embodiments, when the perovskite active layer 32 is prepared using a two-step method, the organic precursor compound can be coated or vapor-deposited first, followed by the inorganic precursor compound. Alternatively, the inorganic precursor compound can be coated or vapor-deposited first, followed by the organic precursor compound.
[0166] In the embodiment, when the perovskite active layer 32 is prepared by a two-step method, the two-step process includes: coating an inorganic precursor compound solution to obtain an inorganic salt layer, then soaking or coating an organic precursor compound solution to obtain an organic salt layer; and finally annealing to allow the inorganic precursor compound in the inorganic salt layer to react with the organic precursor compound in the organic salt layer to generate the perovskite active layer 32.
[0167] In the exemplary example, the solvent for the inorganic precursor compound solution includes at least one selected from N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), dimethyl sulfoxide (DMSO), 2-methoxyethanol (2-Me), N,N'-dimethylacrylurea (DMPU), 1,3-dimethyl-2-imidazolinone (DMI), N,N-diethylformamide (DEF), sulfolane, and γ-butyrolactone (GBL). The solvent for the organic precursor compound solution includes at least one selected from methanol, ethanol, and isopropanol (IPA). The organic precursor compound solution needs to use a weakly polar, low-boiling-point solvent that is almost insoluble in the inorganic precursor compound, thus avoiding the dissolution of the already formed inorganic salt layer.
[0168] In this embodiment, when the perovskite active layer 32 is prepared using a two-step method, after coating the inorganic precursor compound solution, a drying process is performed to obtain the inorganic salt layer. The drying process helps remove residual solvent. In this embodiment, the drying temperature can be 80–100 °C.
[0169] In the embodiments, when the perovskite active layer 32 is prepared by a two-step method, the two-step preparation process may further include: vapor deposition of inorganic precursor compounds to obtain an inorganic salt layer, followed by vapor deposition of organic precursor compounds, and finally annealing to generate the perovskite active layer 32.
[0170] In this embodiment, when the perovskite active layer 32 is prepared using a two-step method, and the substrate is heated during the above-mentioned evaporation of the organic precursor compound, the organic precursor compound reacts with the inorganic precursor compound in situ after deposition to form perovskite. The final annealing improves the crystallinity of the perovskite, eliminates residual stress, and reduces defects. The temperature conditions for the heat treatment are 90–150 °C.
[0171] In this embodiment, when the perovskite active layer 32 is prepared using a two-step method, the two-step process may further include: vapor deposition of an inorganic precursor compound to obtain an inorganic salt layer, followed by immersion or coating with an organic precursor compound solution to obtain an organic salt layer; and finally annealing to generate the perovskite active layer 32. The purpose of annealing is to drive the perovskite precursor material to undergo a chemical reaction and crystallize to form the perovskite active layer 32, while simultaneously removing residual solvent. In this embodiment, the annealing temperature for the two-step preparation of the perovskite active layer 32 is 90–150 °C. In the exemplary example, the annealing temperature for the two-step preparation of the perovskite active layer 32 can be a typical but non-limiting temperature such as 90 °C, 100 °C, 110 °C, 120 °C, 130 °C, 140 °C, or 150 °C, or a range between any two temperature values.
[0172] In the embodiments, the annealing time for the two-step preparation of the perovskite active layer 32 is 5 to 30 min. In the exemplary examples, the annealing time for the two-step preparation of the perovskite active layer 32 can be 5 min, 10 min, 15 min, 20 min, 25 min, 30 min, or any range between the aforementioned two values.
[0173] In the embodiments, in such Figure 1 In the illustrated tandem solar cell, the electron transport layer 33 of the perovskite sub-cell 30 may include at least one inorganic metal oxide material selected from tin oxide, titanium oxide, and zinc oxide. In the embodiments, the fabrication process of the electron transport layer 33 includes sol-gel method, atomic layer deposition (ALD), chemical vapor deposition (CVD, including plasma-enhanced chemical vapor deposition (PECVD), metal-organic chemical vapor deposition (MOCVD), physical vapor deposition (PVD, including magnetron sputtering, thermal evaporation, pulsed laser deposition (PLD), spray pyrolysis, solution spin coating, electrochemical deposition, and chemical bath deposition, etc.). Atomic layer deposition (ALD) is preferred.
[0174] In this embodiment, when the electron transport layer 33 of the inorganic metal oxide material is prepared using atomic layer deposition (ALD), the process includes: alternately introducing a metal precursor and an oxygen source under a gas pressure of 0.05–1.5 Torr. The flow rate of the metal precursor introduced in each cycle is 10–100 sccm, and the pulse duration of the metal precursor introduction in each cycle is 100–300 ms. The flow rate of the oxygen source introduced in each cycle is 10–100 sccm, and the pulse duration of the oxygen source introduction in each cycle is 100–300 ms.
[0175] In the embodiments, when the electron transport layer 33 of the inorganic metal oxide material is prepared by atomic layer deposition (ALD), the growth rate of the inorganic metal oxide is typically between 0.03 and 0.2 nm / cycle, and the required number of cycles depends on the type of metal precursor, the type of oxygen source, and the process temperature. It should be noted that during the alternating introduction of the metal precursor and oxygen source, the first introduction is of the metal precursor.
[0176] In the embodiments, in such Figure 1 In the illustrated tandem solar cell, the electron transport layer 33 of the perovskite sub-cell 30 may further include organic materials such as C60, fullerene C70, methyl (6,6)-phenyl-C61-butyrate (PCBM), and 4-(1',5'-dihydro-1'-methyl-2'H-(5,6)fullerene-C60-In-(1,9-c)pyrrole-2'-yl)benzylamine chloride (CPMAC). In the embodiments, the electron transport layer 33 is prepared using methods such as vacuum evaporation, spin coating, inkjet printing, blade coating, slot coating, dip coating, spray coating, drop coating, and roll-to-roll printing. When vacuum evaporation is used, the evaporation rate is 0.05–0.1 nm / s.
[0177] In the embodiments, in such Figure 1 In the tandem solar cell shown, the electron transport layer 33 of the perovskite sub-cell 30 may also include one or more inorganic silicon materials such as n-type monocrystalline silicon, n-type polycrystalline silicon, and n-type amorphous silicon. Its fabrication processes mainly include low-pressure chemical vapor deposition (LPCVD), plasma-enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD), magnetron sputtering, thermal diffusion (such as phosphorus diffusion), ion implantation, sol-gel method, and electron beam evaporation.
[0178] In the embodiments, in such Figure 1In the tandem solar cell shown, the electron transport layer 33 of the perovskite sub-cell 30 can also include one or more inorganic salt materials such as barium stannate (BSO), lanthanum-doped barium stannate (LBSO), titanium tin oxide (TiSnOx), and tin zinc oxide (SnZnOx). The preparation processes mainly include sol-gel method, nanoparticle dispersion method, atomic layer deposition (ALD), chemical vapor deposition (CVD, including plasma-enhanced chemical vapor deposition (PECVD), physical vapor deposition (PVD, including magnetron sputtering, pulsed laser deposition (PLD), and electron beam evaporation), spray pyrolysis, solution spin coating, electrochemical deposition, chemical bath deposition, and magnetron sputtering-annealing combined method. It should be noted that among the above processes, only gas-phase, low-temperature, and non-destructive processes such as atomic layer deposition (ALD) and chemical vapor deposition can be applied to prepare the inorganic salt material electron transport layer on the perovskite active layer 32. Other processes, due to the presence of solvent erosion, high-temperature annealing, or high-energy particle bombardment, are relatively suitable for preparing inorganic salt electron transport layers 33 on substrates.
[0179] In the embodiments, in such Figure 1 In the tandem solar cell shown, the electron transport layer 33 contained in the perovskite subcell 30 can be a single material among the above-mentioned inorganic metal oxide materials, organic materials, inorganic silicon materials, and inorganic salt materials, or it can be a combination of multiple materials.
[0180] In the embodiments, in such Figure 1 In the tandem solar cell shown, the thickness of the electron transport layer 33 contained in the perovskite subcell 30 can be 3 to 50 nm.
[0181] Of course, the materials, manufacturing processes, and thicknesses of the electron transport layer 33 mentioned above can also be other materials, processes, and thicknesses.
[0182] In the embodiments, in such Figure 1 In the tandem solar cell shown, the buffer layer 34 contained in the perovskite sub-cell 30 may include at least one of tin oxide, molybdenum oxide, titanium oxide, zinc oxide, zirconium oxide, magnesium oxide, and 2,9-dimethyl-4,7-biphenyl-1,10-o-diazaphenanthroline (also known as bath copper or BCP).
[0183] In this embodiment, the thickness of the buffer layer 34 can be 1 nm to 50 nm. Zirconia, molybdenum oxide, magnesium oxide, or copper hydroxide have relatively weak conductivity, and if the resulting film is too thick, it will reduce electron transport and affect the performance of the perovskite sub-cell. In this case, the thickness of the buffer layer 34 can be relatively thin, such as 1 nm to 10 nm.
[0184] In the embodiments, in such Figure 1In the illustrated tandem solar cell, the transparent conductive layer 35 of the perovskite sub-cell 30 includes, but is not limited to, at least one of indium tin oxide (ITO), indium zinc oxide (IZO), indium tungsten oxide (IWO), fluorine-doped tin oxide (FTO), aluminum-doped zinc oxide (AZO), antimony-doped tin oxide (ATO), and gallium-doped zinc oxide (GZO). In the embodiments, the thickness of the transparent conductive layer 35 can be 10 nm to 100 nm. In the embodiments, the transparent conductive layer 35 is prepared by methods including, but not limited to, magnetron sputtering (PVD) and reactive plasma deposition (RPD). The transparent conductive layer 35 possesses both good conductivity and light transmittance, serving to laterally collect charge carriers and transport them to the electrode grid lines 36. It also reduces the reflection of incident light on the surface of the perovskite sub-cell 30, increasing the absorption of light by the tandem solar cell.
[0185] In such Figure 1 In the illustrated tandem solar cell, the perovskite sub-cell 30 includes an electrode grid line 36 for efficient current collection and extraction of carriers transported by the transparent conductive layer. The electrode grid line 36 and the transparent conductive layer 35 together constitute the high-efficiency current collection and extraction system of the solar cell. In this embodiment, the thickness of the electrode grid line 36 can be from 0.3 μm to 20 μm. In this embodiment, the electrode grid line 36 includes at least one of gold (Au), silver (Ag), aluminum (Al), and copper (Cu); preferably silver, copper, or aluminum.
[0186] In this embodiment, the electrode grid line 36 includes a fine grid and a busbar grid. Multiple fine grids are arranged in parallel on the transparent conductive layer to collect photogenerated electrons exported from the electron transport layer 33. The busbar grid is in contact with the fine grids to collect all the current transmitted through the fine grids and output it outward. The thickness of the fine grid is 5–15 μm, and its width is 20–50 μm. The thickness of the busbar grid is 1.5–2 μm, and its width is 1.2–2 mm.
[0187] In this embodiment, an adhesion layer may also be disposed between the electrode gate line 36 and the transparent conductive layer 35. This adhesion layer binds the electrode gate line 36 to the transparent conductive layer 35, preventing metal atoms in the electrode gate line 36 from extending into the transparent conductive layer 35 and reducing the interfacial contact barrier. The adhesion layer is made of at least one of chromium (Cr), titanium (Ti), nickel (Ni), platinum (Pt), and palladium (Pd). The thickness of the adhesion layer is 5–20 nm.
[0188] In such Figure 1 In the illustrated tandem solar cell, the antireflection layer 37 of the perovskite sub-cell 30 is disposed on the surface of the transparent conductive layer 35 not covered by the electrode grid lines 36. In the embodiment, the antireflection layer 37 may include, but is not limited to, lithium fluoride, or other antireflection materials, and its thickness may be conventional.
[0189] In some embodiments, the tandem solar cells in the above embodiments can be prepared by selecting an appropriate method based on their structure and the types and properties of materials in each layer.
[0190] [Battery Components] Fifthly, embodiments of this application also provide a battery module. The battery module of this application includes the tandem solar cells described in the previous embodiments. Therefore, the photoelectric conversion efficiency and operational stability of the battery module of this application are improved.
[0191] [Example] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0192] Example 1: This embodiment provides a stacked solar cell, the structure of which is as follows: Figure 1 As shown, along the light incident direction, the tandem solar cell includes a crystalline silicon sub-cell 10 as the bottom cell, a composite layer 20, and a perovskite sub-cell 30 as the top cell.
[0193] The crystalline silicon sub-cell 10 includes a 100 μm thick n-type monocrystalline silicon semiconductor substrate 14. Sequentially deposited on the back side (backlight side) of the n-type monocrystalline silicon semiconductor substrate 14 are a 5 nm thick intrinsic hydrogenated amorphous silicon first passivation layer 13, a 10 nm thick p-type hydrogenated nanocrystalline silicon p-type window layer 12, a 20 nm thick indium tin oxide (ITO) transparent electrode layer 112, and a 5 μm thick silver metal electrode layer 111. The transparent electrode layer 112 and the silver metal electrode layer 111 constitute a back field electrode 11. Sequentially deposited on the front side (light-facing side) of the n-type monocrystalline silicon semiconductor substrate 14 are a 5 nm thick intrinsic hydrogenated amorphous silicon second passivation layer 15 and a 10 nm thick n-type hydrogenated nanocrystalline silicon n-type window layer 16. The n-type hydrogenated nanocrystalline silicon n-type window layer 16 is stacked and contacted with the composite layer 20.
[0194] The n-type single-crystal silicon semiconductor substrate 14 has a textured surface on the side closest to the perovskite sub-cell 30. This textured surface includes multiple randomly distributed rounded protrusions, each with a smooth top surface and an arc-shaped recess between adjacent rounded protrusions. The relevant dimensions of the rounded protrusions and the arc-shaped recess are shown in Table 1 below.
[0195] Composite layer 20 is an indium tin oxide (ITO) composite layer with a thickness of 20 nm.
[0196] The perovskite sub-cell 30 includes nickel oxide (NiO) with a thickness of 5 nm stacked sequentially. x Transition metal oxide layer 312, 2 nm thick 4PADCB self-assembled monolayer material self-assembled monolayer 311, 200 nm thick Cs 0.05 FA 0.75 MA 0.2 Pb(I) 0.75 Br 0.25 )3. Perovskite active layer 32, PDAI2 passivation layer with a thickness of 2 nm, C with a thickness of 20 nm 60 Electron transport layer 33, tin oxide (SnO) with a thickness of 10 nm x The composite layer consists of a buffer layer 34, a 100 nm thick indium zinc oxide (IZO) transparent conductive layer 35, a 200 nm thick silver electrode gate line 36, and a 100 nm thick lithium fluoride antireflection layer 37. The transition metal oxide layer 312 is stacked and contacted with the composite layer 20.
[0197] The fabrication method of tandem solar cells includes the following steps: S1. Fabrication of crystalline silicon sub-cell 10: S11. Fabrication of a textured semiconductor substrate 14: An n-type single-crystal silicon wafer was placed in a texturing etching solution and immersed at 80°C for 400 seconds to perform texturing etching, resulting in a pyramid-shaped texturing structure. The peaks of the pyramids in the texturing structure have... Figure 8 The triangular structure shown; wherein the texturing etching solution comprises the following formulation components: Deionized water 87.0%, sodium hydroxide (first alkali compound) 2.0%, fatty alcohol polyoxyethylene ether (surfactant) 2.0%, sodium gluconate (first complexing agent) 2%, polyether defoamer (first defoamer) 1%, sodium acetate (first stabilizer) 2%, sodium carbonate (first inorganic additive) 3.0%, disodium EDTA (first corrosion inhibitor) 1.0%; b. The textured n-type single-crystal silicon wafer is placed in a spherical etching solution and immersed at 50 ℃ for 300 s for spherical etching treatment, so that the peaks of the pyramids in the textured surface structure become like... Figure 1 The conical or hill-shaped morphology shown indicates that one side of the n-type single-crystal silicon semiconductor substrate 14 prepared in this way has... Figure 1 The hill-like morphology shown; wherein, the circular etching solution comprises the following formulation components: Deionized water 87.0%, sodium hydroxide 1.0%, ethylene glycol 1.3%, polyoxyethylene polyoxypropylene ether 2.5%, disodium EDTA 2.5%, carboxymethyl cellulose 2.3%, sodium carbonate 2.0%, polyether-modified silicone oil 1.4%; S12. After cleaning and drying the n-type single-crystal silicon semiconductor substrate 14 prepared in step S11, an intrinsic hydrogenated amorphous silicon first passivation layer 13, a p-type hydrogenated nanocrystalline silicon p-type window layer 12, an indium tin oxide (ITO) transparent electrode layer 112 and a silver metal electrode layer 111 are sequentially deposited on the textured surface of the back side of the semiconductor substrate 14. The transparent electrode layer 112 and the silver metal electrode layer 111 constitute the back field electrode 11. An intrinsic hydrogenated amorphous silicon second passivation layer 15 and an n-type hydrogenated nanocrystalline silicon n-type window layer 16 are sequentially deposited on the textured surface of the front side of the n-type single-crystal silicon semiconductor substrate 14.
[0198] S2. Preparation of composite layer 20: ITO transparent conductive oxide was deposited on the surface of the n-type window layer 16 using physical vapor deposition to form a continuous indium tin oxide (ITO) composite layer 20. S3. Fabrication of the perovskite sub-cell 30: Each layer is fabricated according to the layer structure of the perovskite sub-cell contained in the two-terminal tandem solar cell in Example 1: S31. Fabrication of hole transport layer 31: First, using a spin coater, ethanol is spin-coated at 3000 rpm for 30 seconds on the surface of the composite layer 20 away from the crystalline silicon sub-cell 10. This process is repeated twice. Then, the surface is heat-treated at 200 ℃ for 10 minutes to complete the cleaning. The cleaned crystalline silicon sub-cell 10 is then placed in a sputtered nickel oxide (NiO) layer. x The mask is placed in a magnetron sputtering apparatus and a vacuum of 7 × 10⁻⁶ is drawn. -4 Below Pa, select the radio frequency magnetron sputtering mode, adjust the power to 200 W, set the argon flow rate to 30 sccm, and sputter for 5 min to form nickel oxide (NiO) on the indium tin oxide (ITO) composite layer 20. x ) layer, as transition metal oxide layer 312; Next, the self-assembled monolayer material 4PADCB was mixed with anhydrous ethanol and stirred until completely dissolved to obtain a self-assembled monolayer (SAM) solution with a concentration of 1 mg / mL. The SAM solution was then spin-coated onto the transition metal oxide layer 312 at a spin speed of 3000 rpm for 30 s. The SAM was then heated and annealed on a hot plate at 100°C for 10 min to form a self-assembled monolayer (SAM) as self-assembled monolayer 311. This self-assembled monolayer 311 and the transition metal oxide layer 312 constitute the hole transport layer 31. Preparation of S32. Perovskite active layer 32: The perovskite precursor materials CsI, FABr, MAI, and PbI2 were dissolved in a mixed solvent of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) (volume ratio 4:1), and stirred at room temperature until completely dissolved to obtain a perovskite precursor solution; wherein, the A-site cation Cs + FA + MA + The total molar concentration is 1 mol / L and the atomic ratio of Cs, FA, and MA is 0.05:0.75:0.2, with Pb at the B-site cation. 2+ The molar concentration is 1 mol / L; In a glove box under a nitrogen atmosphere, a perovskite precursor solution was spin-coated onto the hole transport layer 31: first, a wet film was spread by spin-coating at 2500 rpm for 25 s, then the speed was increased to 5500 rpm for 12 s. During the high-speed spin-coating stage, 150 μL of the anti-solvent chlorobenzene was slowly added dropwise. After spin-coating, the film was transferred to a hot stage at 100 °C and heated for annealing for 30 min to form the perovskite active layer 32. S33. Preparation of passivation layer: The passivating material PDAI2 (1,3-diaminopropane dihydroiodate, CAS No.: 120675-53-8) was mixed with isopropanol to obtain a passivation solution. The concentration of PDAI2 in the passivation solution was 1 mg / mL. The passivation solution was coated on the surface of the perovskite active layer 32 and annealed at 65 °C for 5 minutes to obtain the passivation layer. S34. Fabrication of electron transport layer 33: C is deposited on the passivation layer using a vacuum evaporation process. 60 Electron transport layer 33, evaporation rate 0.5 Å / s; S35. Preparation of buffer layer 34: Atomic layer deposition process in C 60 Preparation of tin oxide (SnO) on electron transport layer x ) Buffer layer 34.
[0199] S36. Preparation of transparent conductive layer 35: Using radio frequency magnetron sputtering, an indium zinc oxide (IZO) transparent conductive layer 35 was deposited on a tin oxide buffer layer 34. The sputtering power was controlled at 300 W, the chamber pressure at 0.6 Pa, the argon flow rate at 20 sccm, the 5% argon-oxygen mixed flow rate at 5 sccm, and the sputtering time at 100 s. S37. Fabrication of electrode grid line 36: Silver paste is coated onto the transparent conductive layer 35 of indium zinc oxide (IZO) using a screen printing process to form a patterned silver paste layer, and then annealed to form electrode grid lines 36. S38. Preparation of antireflective layer 37: A lithium fluoride antireflection layer 37 was deposited on the indium zinc oxide (IZO) transparent conductive layer 35, which was not covered by the electrode grid line 36, using a vacuum evaporation process at a deposition rate of 0.1 nm / s.
[0200] Examples 2 to 5: Examples 2 to 5 each provide a tandem solar cell. Compared with the tandem solar cell with two ends in Example 1, the semiconductor substrate 14 textured structure in Examples 2 to 5 contains different dimensions of rounded protrusions and arc-shaped recesses, as shown in Table 1 below. Other aspects are the same as in Example 1.
[0201] In Example 2, the circular etching solution used to prepare the circular textured semiconductor substrate 14 includes the following formulation components: Deionized water 87.0%, sodium hydroxide 1.0%, ethylene glycol 1.3%, polyoxyethylene polyoxypropylene ether 2.5%, disodium EDTA 2.5%, carboxymethyl cellulose 2.3%, sodium carbonate 2.0%, polyether-modified silicone oil 1.4%; The conditions for the circular etching process are: time 300 s, temperature 50 ℃.
[0202] The circular etching solution used in Example 3 to prepare the circular textured semiconductor substrate 14 includes the following formulation components: Deionized water 87.0%, sodium hydroxide 1.0%, ethylene glycol 1.3%, polyoxyethylene polyoxypropylene ether 2.5%, disodium EDTA 2.5%, carboxymethyl cellulose 2.3%, sodium carbonate 2.0%, polyether-modified silicone oil 1.4%; The conditions for the circular etching process are: time 240 s and temperature 50 ℃.
[0203] The circular etching solution used in Example 4 to prepare the circular textured semiconductor substrate 14 includes the following formulation components: Deionized water 87.0%, sodium hydroxide 1.0%, ethylene glycol 1.3%, polyoxyethylene polyoxypropylene ether 1.0%, disodium EDTA 2.5%, carboxymethyl cellulose 3%, sodium carbonate 2.0%, polyether-modified silicone oil 2.2%; The conditions for the circular etching process are: time 240 s and temperature 50 ℃.
[0204] The circular etching solution used in Example 5 to prepare the circular textured semiconductor substrate 14 includes the following formulation components: Deionized water 87.5%, sodium hydroxide 1.0%, ethylene glycol 1.3%, polyoxyethylene polyoxypropylene ether 5%, disodium EDTA 2.0%, carboxymethyl cellulose 0.8%, sodium carbonate 2.0%, polyether-modified silicone oil 0.4%; The conditions for the circular etching process are: time 240 s and temperature 50 ℃.
[0205] Comparative Example 1: This comparative example provides a tandem solar cell, which differs from the tandem solar cell in Example 1 in that the textured structure of the n-type monocrystalline silicon semiconductor substrate 14 contained in the crystalline silicon sub-cell 10 is a traditional pyramid textured structure, while the other structures are the same as in Example 1.
[0206] The method for fabricating a comparative tandem solar cell differs from that in Example 1 in that only the texturing etching process in step S11a is performed to form a pyramid-shaped texturing structure, while the rounding etching process in step S11b is not performed. The other process steps and parameters are the same as in Example 1.
[0207] Electron microscopy analysis: The textured surface structure of the crystalline silicon sub-cell semiconductor substrate and the perovskite active layer of the perovskite sub-cell in Examples 1 to 5 and Comparative Example 1 were analyzed using scanning electron microscopy (SEM). The SEM images of the rounded raised textured surface structure of the crystalline silicon sub-cell semiconductor substrate and the perovskite active layer of the perovskite sub-cell in Example 1, and the pyramidal raised textured surface structure of the crystalline silicon sub-cell semiconductor substrate and the perovskite active layer of the perovskite sub-cell in Comparative Example 1 are attached. Figures 2 to 9 As shown.
[0208] Parameter determination and performance testing of tandem solar cells at both ends: The parameters and performance of the tandem solar cells in Examples 1 to 5 and Comparative Example 1 were measured as shown in Table 1 below. The detection methods for each performance are as follows, and the test results are shown in Table 1 below.
[0209] Photovoltaic efficiency testing method for two-terminal tandem solar cells: IV test method, using FCT650 equipment; Open-circuit voltage test method for two-terminal tandem solar cells: IV test method, using FCT650 equipment; Short-circuit current test method for two-terminal tandem solar cells: IV test method, using FCT650 equipment; The fill factor (FF) test method for tandem solar cells at both ends is the IV test method, and the equipment used is FCT650.
[0210] Table 1
[0211] Combination Figures 2 to 9 As shown in Table 1, comparing Examples 1 to 5, in the semiconductor substrate contained in the crystalline silicon sub-cell of the tandem solar cell, the rounded protrusions and arc-shaped depressions in the textured surface structure have a significant impact on the photoelectric performance of the tandem solar cell. Specifically, as the degree of pyramid rounding increases, the FF of the tandem cell shows an upward trend, the Jsc shows a slight downward trend, and the overall efficiency shows an upward trend.
[0212] The above embodiments merely illustrate several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of this patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.
Claims
1. A semiconductor substrate, characterized in that: For use in solar cells, at least one surface of the semiconductor substrate has a textured structure, and the textured structure includes a plurality of randomly distributed rounded protrusions, each of the rounded protrusions having a smooth top surface, and the bottom of adjacent rounded protrusions having an arc-shaped recessed structure.
2. The semiconductor substrate as described in claim 1, characterized in that: The rounded protrusion satisfies at least one of the following (1) to (3): (1) The ratio of the height of the rounded protrusion to the diameter of the bottom is (0.3~1.25):1; (2) The height of the rounded protrusion is 1.5 μm to 2.5 μm; (3) The diameter of the bottom of the rounded protrusion is 2 μm to 5 μm.
3. The semiconductor substrate as described in claim 1, characterized in that: The arc-shaped concave structure satisfies at least one of the following (1) to (3): (1) The depth to width ratio of the arc-shaped recessed structure can be (0.15~5):1; (2) The depth of the arc-shaped concave structure is 0.3 μm to 1.5 μm; (3) The width of the arc-shaped concave structure is 0.3 μm to 2 μm.
4. The semiconductor substrate according to any one of claims 1 to 3, characterized in that: The rounded protrusion includes at least one of the following: conical, hill-shaped, or pyramid-like tetrahedron.
5. A method for preparing a semiconductor substrate, characterized in that, Includes the following steps: At least one surface of a semiconductor substrate is subjected to texturing etching to form a texturing surface with multiple randomly distributed pyramidal structures; The textured surface is etched using a circular etching solution to form circular protrusions in the pyramid structure. Each circular protrusion has a smooth top surface, and the bottom of adjacent circular protrusions has an arc-shaped concave structure.
6. The preparation method according to claim 5, characterized in that: Based on 100% of the total mass of the spherical etching solution, the spherical etching solution comprises the following components by mass percentage: Solvent 85%–94%; Alkali compounds 0.05%–4%; Cosolvent 1%–5%; Surfactant 1%–5%; Complexing agent 1%–3%; Corrosion inhibitor 0.5%–4%; pH adjuster 0.1%–3%; Defoamer 0.1%–3%.
7. The preparation method according to claim 6, characterized in that: The cosolvent includes at least one of ethylene glycol, propylene glycol, and glycerin; And / or, the surfactant includes at least one of nonionic surfactant and anionic surfactant, wherein the nonionic surfactant includes at least one of fatty alcohol polyoxyethylene ether, polyoxyethylene polyoxypropylene ether, and Tween-80, and the anionic surfactant includes at least one of fatty alcohol ether sodium sulfate and alkyl sulfonate. And / or, the complexing agent includes at least one of sodium gluconate, sodium citrate, sodium lactate, disodium EDTA, and phytic acid; And / or, the corrosion inhibitor includes at least one of sodium silicate, chitosan, tannic acid, resveratrol, carboxymethyl cellulose, and polyvinylpyrrolidone; And / or, the pH adjuster includes at least one of sodium carbonate, sodium bicarbonate, and sodium acetate; And / or, the defoamer includes at least one of polyether-modified silicone oil and organosilicon emulsion; And / or, the alkaline compound includes at least one of the hydroxides NaOH, KOH, and NH4OH; And / or, the solvent includes water.
8. The preparation method according to any one of claims 5 to 7, characterized in that: The temperature for the circular etching process is 30℃~80℃; And / or, the time for the circular etching process is 150 s to 850 s.
9. A solar cell, characterized in that, The semiconductor substrate includes any one of claims 1 to 4 or the semiconductor substrate prepared by any one of claims 5 to 8.
10. The solar cell as claimed in claim 9, characterized in that: The solar cell is a tandem solar cell, comprising a crystalline silicon sub-cell and a perovskite sub-cell. The crystalline silicon sub-cell contains the semiconductor substrate, and the perovskite sub-cell is disposed on the surface of the crystalline silicon sub-cell near the semiconductor substrate, on the side having the textured surface structure.
11. A battery assembly, characterized in that: Including the solar cell as described in any one of claims 9 to 10.
12. A circular etching solution, characterized in that: The components include the following components by mass percentage: Solvent 85%–94%; Alkali compounds 0.05%–4%; Cosolvent 1%–5%; Surfactant 1%–5%; Complexing agent 1%–3%; Corrosion inhibitor 0.5%–4%; pH adjuster 0.1%–3%; Defoamer 0.1%–3%.