Solar cells and photovoltaic modules
By employing a stacked first and second sub-body structure in the solar cell, adjusting the phosphorus content, and using metal particles, the problem of weak bonding force of base metal electrodes was solved, improving current collection efficiency and battery reliability, and achieving a technology that is easy to mass-produce.
Patent Information
- Application Number
- CN202611141126.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-29
- Publication Date
- 2026-11-17
AI Technical Summary
Base metal current collectors have relatively weak bonding with semiconductor substrates and doped layers, making them prone to detachment from the battery surface, which affects current collection efficiency and reduces battery reliability and lifespan.
The structure employs a first sub-body and a second sub-body layered configuration. The first sub-body has a higher phosphorus content than the second sub-body. Stress is adjusted by regulating the phosphorus content to enhance bonding strength. Metal particles are used as components of the seed part to improve contact performance.
It improves the bonding force between the electrode and the doped layer, reduces the risk of electrode detachment, enhances current collection efficiency and battery reliability and lifespan, while also reducing process difficulty and facilitating mass production.
Smart Images

Figure CN123124502A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of photovoltaic technology, specifically relating to a solar cell and a photovoltaic module. Background Technology
[0002] Solar cells are components that convert light energy into electrical energy. Because they use clean energy, they have broad application prospects. The current collector electrodes in a solar cell are mainly used to collect charge carriers or current in the cell and drain the current.
[0003] Currently, base metals are typically used in the current collector electrodes of solar cells to reduce the cost of solar cells.
[0004] However, the bonding force between the current collector electrode containing base metal and the semiconductor substrate and doped layer is relatively weak, making it easy to detach from the battery surface, which reduces the reliability and lifespan of the battery and also affects the current collection effect. Summary of the Invention
[0005] This application aims to provide a solar cell and a photovoltaic module that at least solves the problem of relatively weak bonding between the base metal current collector electrode and the semiconductor substrate and doped layer.
[0006] In a first aspect, embodiments of this application provide a solar cell, comprising: Semiconductor substrate; A doped layer and a passivation layer are sequentially disposed on the semiconductor substrate, and the passivation layer has a window. An electrode structure is located on the side of the passivation layer opposite to the semiconductor substrate. The electrode structure includes a seed portion and a base metal portion, with at least a portion of the seed portion located within the window. The seed portion contacts the doped layer through the window, and the base metal portion covers at least a portion of the seed portion. The seed portion includes a body portion. In the thickness direction of the solar cell, the main body includes at least a first sub-main body and a second sub-main body stacked together, wherein the first sub-main body is further away from the semiconductor substrate than the second sub-main body; and the phosphorus content of the first sub-main body is greater than the phosphorus content of the second sub-main body.
[0007] In this application, the second sub-body with a lower phosphorus content is closer to the silicon substrate, and thus closer to the doped layer. It has a lower contact resistance with the doped layer, which can improve the current collection effect. Moreover, the second sub-body with a lower phosphorus content grows faster and is easier to form on the doped layer, with lower process difficulty and easier mass production. However, the second sub-body with a lower phosphorus content is prone to tensile stress, especially when the second sub-body and the doped layer are of different material types (one is a metal layer and the other is a semiconductor layer). The internal shrinkage deformation of the body caused by tensile stress is more obvious between dissimilar material layers, resulting in poor bonding between the body and the doped layer, and it is easy to fall off from the surface of the doped layer. In this application, a first sub-body with a higher phosphorus content is provided on a second sub-body with a lower phosphorus content. As the phosphorus content in the body increases, its internal stress will also change. The tensile stress weakens and gradually transitions to compressive stress, which can offset the tensile stress of the second sub-body with a lower phosphorus content, weaken the overall stress of the body, reduce the overall deformation of the body, and ultimately reduce the shrinkage deformation between the body and the doped layer, thus preventing the body or electrode structure from falling off the surface of the doped layer. Meanwhile, the growth rate of the first sub-body with a high phosphorus content is low, and its formation speed on the doped layer is slow. Therefore, there is an urgent need for a conductive underlayer, which can significantly improve the plating activity of the first sub-body, making it easier to form the first sub-body with a high phosphorus content, reducing the process difficulty, and making it easier to achieve mass production.
[0008] In summary, the reduced stress and internal deformation of the main body of this application improve its adhesion to the surface of the doped layer, reduce the risk of electrode detachment, and enhance reliability and lifespan; at the same time, the process is simple and easy to mass-produce.
[0009] In some embodiments, the first sub-body portion and the second sub-body portion are distributed adjacent to each other in the thickness direction of the solar cell.
[0010] In some embodiments, in the thickness direction of the solar cell: The thickness H1 of the first sub-body portion is greater than the thickness H2 of the second sub-body portion; and / or, The thickness H1 of the first sub-body portion is 100 nm to 500 nm; and / or, The thickness H2 of the second sub-body portion is greater than or equal to 100 nm; and / or, The thickness H3 of the main body is 200 nm to 900 nm; and / or, The main body has a portion that extends beyond the passivation layer, and the thickness H4 of the extended portion is 150 nm to 800 nm.
[0011] In some embodiments, the seed portion further includes metal particles, and the body portion encloses at least a portion of the metal particles; the body element of the metal particles is different from the body element of the body portion and the body element of the base metal portion; In the main body, at least the second sub-main body contains a void, and at least some of the metal particles are located in the void.
[0012] In a second aspect, a semiconductor substrate; a doped layer and a passivation layer are sequentially disposed on the semiconductor substrate, the passivation layer having a window; an electrode structure is located on the side of the passivation layer away from the semiconductor substrate, the electrode structure comprising: a seed portion and a base metal portion, at least a portion of the seed portion being located within the window; the seed portion contacting the doped layer through the window, the base metal portion covering at least a portion of the seed portion; the seed portion comprising: a main body portion; wherein, in the thickness direction of the solar cell, the main body portion comprises at least a first sub-main body portion and a second sub-main body portion stacked together, the first sub-main body portion being further away from the semiconductor substrate than the second sub-main body portion, and in some embodiments, the first sub-main body portion being more dense than the second sub-main body portion.
[0013] It should be noted that, based on the aforementioned improvement in the contact bonding effect between the main body and the metal particles or doped layer, or the semiconductor substrate through the stacking of at least the first and second sub-main bodies, in this application, the first sub-main body 15 is more dense than the second sub-main body 16, further forming more nested fixation closer to the semiconductor substrate to enhance the contact bonding effect between the main body and the metal particles or doped layer, or the semiconductor substrate. In this application, the fact that the first sub-main body 15 is more dense than the second sub-main body 16 can be combined with other content or implemented separately, all of which are within the scope of protection of this application. In this application, all content related to gaps is related to the aforementioned greater density of the first sub-main body 15 compared to the second sub-main body 16.
[0014] In some embodiments, both the first sub-body portion and the second sub-body portion contain gaps; The number of voids per unit area in the second sub-body is greater than the number of voids per unit area in the first sub-body; and / or, The volume ratio of the void per unit volume in the second sub-body is greater than the volume ratio of the void per unit volume in the first sub-body.
[0015] The following features satisfy both the first and second aspects. In some embodiments, the height difference between the main body and the surface of the semiconductor substrate is 30 nm to 200 nm.
[0016] In some embodiments, the seed portion further includes metal particles, and the body portion encloses at least a portion of the metal particles; the window includes an edge region and a central region located inside the edge region; the body portion includes a first surface remote from the semiconductor substrate; for the same window: For the same window: the degree of unevenness in the edge region of the first surface is greater than the degree of unevenness in the middle region of the first surface; and / or, The size of at least a portion of the agglomerates of the metal particles in the edge region is larger than the size of the agglomerates of the metal particles in the middle region.
[0017] In some embodiments, in the thickness direction of the solar cell: for the same window: the height difference of the edge regions in the first surface is H5, and the height difference of the middle regions in the first surface is H6; 1 < H5 / H6 ≤ 8; and / or, H6 ≤ 50 nm; and / or, 30 nm ≤ H5 ≤ 150 nm.
[0018] In some embodiments, the doped layer includes a P-type doped layer and an N-type doped layer, the window includes an edge region and a middle region located inside the edge region; the body portion includes a first surface remote from the semiconductor substrate; In the first surface corresponding to the P-type doped layer, the height difference between the middle region and the edge region is greater than the height difference between the edge region and the middle region in the first surface corresponding to the N-type doped layer.
[0019] In some embodiments, the doped layer includes a P-type doped layer and an N-type doped layer, the window includes an edge region and a middle region located inside the edge region; the body portion includes a first surface remote from the semiconductor substrate; In the first surface corresponding to the N-type doped layer, the degree of unevenness H6 in the middle region is greater than that in the first surface corresponding to the P-type doped layer.
[0020] In some embodiments, the variance of the size of the cellular particles per unit area in the second sub-body portion is greater than the variance of the size of the cellular particles per unit area in the first sub-body portion; and / or, The average size of the cellular particles per unit area in the first sub-body portion is greater than the average size of the cellular particles per unit area in the second sub-body portion; and / or, The number of cellular particles per unit area in the second sub-body portion is greater than the number of cellular particles per unit area in the first sub-body portion.
[0021] In some embodiments, the main elements of each sub-main body in the main body are the same.
[0022] In some embodiments, the undulation of the surface of the second sub-body portion away from the semiconductor substrate is greater than the undulation of the surface of the second sub-body portion away from the semiconductor substrate; and / or, The surface roughness of the second sub-body portion away from the semiconductor substrate is greater than the surface roughness of the first sub-body portion away from the semiconductor substrate.
[0023] In some embodiments, the main body includes an amorphous portion located in the main body away from the semiconductor substrate; the thickness of the amorphous portion is 1 nm to 150 nm.
[0024] In some embodiments, the doped layer includes a P-type doped layer and an N-type doped layer; The thickness of the main body portion corresponding to the N-type doped layer position is greater than the thickness of the main body portion corresponding to the P-type doped layer position.
[0025] In some embodiments, the seed portion further includes metal particles, and the body portion encloses at least a portion of the metal particles; the body element of the metal particles is different from the body element of the body portion and the body element of the base metal portion; The main body includes a first surface remote from the semiconductor substrate; the doped layer has a second surface remote from the semiconductor substrate, the first surface has protrusions and depressions, and in the seed portion, the projection of at least one agglomerate of the metal particles onto the semiconductor substrate at least partially overlaps with the projection of at least one protrusion onto the semiconductor substrate.
[0026] In some embodiments, the mass percentage of phosphorus in the first sub-body portion is 5% to 10%, and the mass percentage of phosphorus in the second sub-body portion is greater than or equal to 1% and less than 5%.
[0027] In some embodiments, the doped layer is divided into a first doped layer and a second doped layer with different polarities, the passivation layer is divided into a first passivation layer and a second passivation layer; the electrode structure is divided into a first electrode structure and a second electrode structure; the first doped layer has the same doping type as the semiconductor substrate, and the second doped layer has a different doping type than the semiconductor substrate. The first doped layer, the first passivation layer, and the first electrode structure are located on different sides of the semiconductor substrate, respectively, as are the second doped layer, the second passivation layer, and the second electrode structure; or, The first doped layer, the first passivation layer, and the first electrode structure are all located on the same side of the semiconductor substrate as the second doped layer, the second passivation layer, and the second electrode structure.
[0028] In some embodiments, along a first direction X, the backlight surface of the semiconductor substrate includes a first region and a second region sequentially distributed; a first doped layer is disposed in the first region of the backlight surface, and a second doped layer is disposed in the second region of the backlight surface; the main body extends along a second direction, and the first direction X intersects with the second direction. The solar cell further includes: a front passivation layer located on the light-facing surface of the semiconductor substrate; A back passivation layer is located on the side of the first doped layer and the second doped layer away from the semiconductor substrate. The back passivation layer includes a portion of the passivation layer that is deposited around the edge region of the front passivation layer away from the semiconductor substrate.
[0029] In some embodiments, the surface of the doped layer away from the semiconductor substrate is a second surface, and the metal particles include: a first metal particle and a second metal particle, wherein the projections of the first metal particle and the second metal particle on the second surface at least partially overlap or are located close to each other; and / or, The first metal particles are distributed on the second surface in the form of scattered points and / or aggregates, and / or the second metal particles are distributed on the second surface in the form of scattered points and / or aggregates.
[0030] In some embodiments, the first metal particle and the second metal particle are made of different materials; The material of the first metal particle is selected from at least one of platinum, gold, silver, cobalt, and indium; and / or, The material of the second metal particle is selected from at least one of zinc, platinum, gold, silver, chromium, rhodium, indium, palladium, and tin; and / or, The material of the main body is selected from at least one of the following: titanium, tungsten, chromium, nickel, cobalt, molybdenum, tin, lead, palladium, niobium, ruthenium, indium, zinc, titanium boride, tantalum nitride, tungsten nitride, titanium tungsten alloy, titanium silicon compound, titanium silicon nitride, tantalum silicon nitride compound, nickel vanadium, and hexagonal boron nitride; and / or, The base metal part is made of at least one of the following: copper, chromium, lead, aluminum, and silver-plated copper.
[0031] Thirdly, embodiments of this application propose a photovoltaic module, comprising: Multiple battery strings connected in series and / or in parallel, the battery strings comprising: electrical connectors and any of the aforementioned solar cells, the electrical connectors being electrically connected to the electrode structures of at least two of the solar cells; An encapsulation layer is used to cover the surface of the battery string; A cover plate is used to cover the surface of the encapsulation layer away from the battery string.
[0032] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description
[0033] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figures 1 to 2 These are schematic diagrams of two types of solar cells according to embodiments of this application; Figures 3 to 4 These are enlarged schematic diagrams of several partial cross-sections of a solar cell according to embodiments of this application; Figures 5 to 6 This is a partially enlarged schematic diagram of different sub-body portions of a solar cell according to an embodiment of this application; Figures 7 to 8 This is a schematic diagram showing the relative positional relationship between two types of first metal particles and second metal particles according to embodiments of this application; Figure 9 This is an enlarged schematic diagram of the window corresponding to the P-type doped layer at the edge of the solar cell according to an embodiment of this application.
[0034] Figure label: 1-Semiconductor substrate, 2-First doped layer, 3-Second doped layer, 4-First passivation layer, 5-Second passivation layer, 6-First seed portion, 7-First base metal portion, 8-Second seed portion, 9-Second base metal portion, 10-Tunneling oxide layer, 11-Front passivation layer, 12-Window, 13-First metal particle, 14-Second metal particle, 15-First sub-body portion, 16-Second sub-body portion, 17-Void, 18-Metal particle, 19-Amorphous portion. Detailed Implementation
[0035] The embodiments of this application will now be described in detail. Examples of these embodiments are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.
[0036] The inventors of this application discovered that the main reason for the relatively weak adhesion between current collector electrodes containing base metals and the semiconductor substrate and doped layer is that phosphorus in current collector electrodes containing base metals is a product obtained by the reduction of the reducing agent during the formation of the seed part in the redox reaction. The formation of the seed part through redox reaction can reduce battery costs; therefore, the main body of the seed part usually contains phosphorus. Furthermore, a main body with a lower phosphorus content is easier to form on the doped layer. However, the tensile stress of the main body with a lower phosphorus content is greater, which easily leads to poor surface adhesion between the main body and the doped layer and semiconductor substrate. This not only makes the electrode structure prone to detaching from the surface of the doped layer but also affects the current collection effect.
[0037] Furthermore, the inventors of this application have discovered that: In a body portion with excessive phosphorus content, the compressive stress also increases, which can easily lead to poor adhesion between the body portion and the aforementioned doped layer surface. This not only causes the electrode structure to easily detach from the doped layer surface but also affects the current collection effect. Additionally, a body portion with a high phosphorus content is difficult to form directly on the doped layer.
[0038] To address the aforementioned technical issues, in this application, the second sub-body with a lower phosphorus content is closer to the silicon substrate, and thus closer to the doped layer. It has a lower contact resistance with the doped layer, which can improve the current collection effect. Furthermore, the second sub-body with a lower phosphorus content is easier to form on the doped layer, with lower process difficulty, and is easier to achieve mass production. However, the second sub-body with a lower phosphorus content is prone to tensile stress, resulting in poor adhesion to the doped layer and easy detachment from the surface of the doped layer. In this application, a first sub-body with a higher phosphorus content is provided on a second sub-body with a lower phosphorus content. The first sub-body with a higher phosphorus content is prone to compressive stress, which can offset the tensile stress of the second sub-body with a lower phosphorus content. Alternatively, the first sub-body with a higher phosphorus content has almost no stress, ensuring the adhesion between the body and the doped layer, preventing the body or electrode structure from detaching from the doped layer surface, and improving reliability and lifespan. At the same time, the first sub-body with a higher phosphorus content is difficult to form on the doped layer. The second sub-body with a lower phosphorus content can significantly improve the plating activity of the first sub-body, making the first sub-body with a higher phosphorus content easier to form, reducing the process difficulty, and facilitating mass production. The following description, in conjunction with the accompanying drawings, further explains this application.
[0039] This application provides a solar cell, with reference to... Figures 1 to 4 The solar cell may include: a semiconductor substrate 1, a doped layer, a passivation layer, and a current collector electrode. The semiconductor substrate may be a silicon substrate, for example, the semiconductor substrate 1 may be N-type monocrystalline silicon or P-type monocrystalline silicon, which can provide long-lived charge carriers. For ease of description, the following embodiments will first be described using N-type monocrystalline silicon as an example of semiconductor substrate 1.
[0040] The doped layer can be either a P-type or N-type doped layer. A P-type doped layer can contain one or more elements from Group IIIA (e.g., boron). An N-type doped layer can contain one or more elements from Group VA (e.g., phosphorus). The materials for both N-type and P-type doped layers can include any semiconductor material such as silicon, germanium-silicon, germanium, or gallium arsenide. In terms of the arrangement of matter, the crystal phase of the doped layer can contain microcrystalline silicon, polycrystalline silicon, amorphous silicon, etc. The materials for both N-type and P-type doped layers can include at least one of doped polycrystalline silicon, doped microcrystalline silicon, or doped amorphous silicon. Both P-type and N-type doped layers can be obtained by in-situ doping on the surface of a semiconductor substrate or by deposition on the surface of a semiconductor substrate.
[0041] The passivation layer refers to the surface passivation layer. The material of the passivation layer can be selected from alumina, silicon nitride, etc., and the specific material is not limited. The passivation layer is located on the side of the doped layer away from the semiconductor substrate. A window is formed in the passivation layer to expose the doped layer portion beneath it. The size of the window can be at the micrometer level, and laser windowing can be used, with no limitation on the specific laser parameters. For example, a picosecond laser can be selected. For example, Gaussian beams and laser-shaped beams can be used to create the window. Gaussian beams have poor energy distribution uniformity, resulting in different roughness or undulations in different areas within the formed window. Laser-shaped beams have a more uniform energy distribution, and the portion of the doped layer surface facing away from the semiconductor substrate located within the window is relatively smooth. A collector electrode, located on the side of the passivation layer facing away from the semiconductor substrate, is used to collect charge carriers or current from the doped layer and conduct the current.
[0042] The solar cells mentioned in this application can be any type of solar cell that requires current collector electrodes. Both back-contact cells with all current collector electrodes located on the same side of the cell and bifacial cells with current collector electrodes located on different sides of the cell are within the scope of protection of this application.
[0043] Reference Figures 1 to 2 The doped layer is divided into a first doped layer 2 and a second doped layer 3 with different polarities. One of them is an N-type doped layer and the other is a P-type doped layer. In this application, the first doped layer 2 can be described as an N-type doped layer and the second doped layer 3 is a P-type doped layer. However, in this application, the first doped layer is a P-type doped layer and the second doped layer is an N-type doped layer, which is also within the scope of protection of this application.
[0044] In some embodiments, the first doped layer and the semiconductor substrate have the same doping type, while the second doped layer has a different polarity or doping type than the semiconductor substrate. For example, both the first doped layer and the semiconductor substrate are N-type doped, and the second doped layer is P-type doped.
[0045] The electrode structure described in this application can refer to an electrode structure including a current collector electrode. The passivation layer is divided into a first passivation layer 4 and a second passivation layer 5; the current collector electrode is divided into a first current collector electrode and a second current collector electrode. Along the thickness direction Z of the semiconductor substrate 1, the semiconductor substrate 1 includes a first side and a second side, one of which is the light-facing side and the other is the second side. In this application, the first side is described as the backlight side. The case where the first side is the light-facing side is also within the scope of protection of this application. During the normal operation of the solar cell, the side of the semiconductor substrate that mainly receives light is its light-facing side, and the backlight side is opposite to the light-facing side. For example, Figure 1 In the semiconductor substrate, the lower side is its backlight side, and the upper side is its light-facing side.
[0046] Reference Figure 1 A first doped layer 2 and a first passivation layer 4 are sequentially disposed on the first side of a semiconductor substrate 1, with the first doped layer 2 closer to the semiconductor substrate 1. A first current collector electrode is located on the side of the first passivation layer 4 away from the semiconductor substrate 1, used to collect and conduct current or charge carriers within the first doped layer. A second doped layer 3 and a second passivation layer 5 are sequentially disposed on the second side of the semiconductor substrate 1, with the second doped layer 3 closer to the semiconductor substrate 1. A second current collector electrode is located on the side of the second passivation layer 5 away from the semiconductor substrate 1, used to collect and conduct current or charge carriers within the second doped layer. This solar cell is a bifacial solar cell. For example, this bifacial solar cell can be a TOPcon (tunneling oxide passivated contact) cell, etc. This application does not limit the specific type of bifacial solar cell.
[0047] Reference Figure 2 A first doped layer 2 and a first passivation layer 4 are sequentially disposed in a first region on a first side of a semiconductor substrate 1, with the first doped layer 2 closer to the semiconductor substrate 1. A first current collector electrode is located on the side of the first passivation layer 4 away from the semiconductor substrate 1, used to collect and conduct current or charge carriers within the first doped layer. A second doped layer 3 and a second passivation layer 5 are sequentially disposed in a second region on the first side of the semiconductor substrate 1, with the second doped layer 3 closer to the semiconductor substrate 1. A second current collector electrode is located on the side of the second passivation layer 5 away from the semiconductor substrate 1, used to collect and conduct current or charge carriers within the second doped layer. This solar cell is a back-contact solar cell with the current collector electrode located on the back-light side of the semiconductor substrate. For example, this back-contact solar cell can be a TBC cell (a cell combining tunneling oxide passivation contact and interdigitated back contact), a back-contact hybrid cell, etc. This application does not limit the specific cell type. In a back-contact solar cell, the light-facing side of the semiconductor substrate 1 is not blocked by electrodes, resulting in better performance and potentially a more aesthetically pleasing appearance. The relative sizes of the first and second regions are not limited here. Figure 2The dashed lines L1 and L2 in the diagram are only for distinguishing different areas. In actual solar cells, there is no such clear boundary between different areas.
[0048] It should be noted that, Figure 1 and Figure 2 In addition, a tunneling oxide layer 10 is provided between the doped layer and the semiconductor substrate to improve the interface passivation contact and further enhance battery performance.
[0049] The materials of the aforementioned first passivation layer and second passivation layer can be the same or different. In a back-contact solar cell, the first and second passivation layers can be an integral structure, or they can be formed in different processes, both of which are within the scope of protection of this application. The back-contact solar cell may also include a front passivation layer 11 disposed on the light-facing side of the semiconductor substrate 1 to passivate and protect the light-facing side of the semiconductor substrate 1. When the doped layer is a doped polycrystalline silicon layer, the thickness of the doped layer can be 50 to 250 nm, etc. When the passivation layer includes an aluminum oxide layer, the thickness of the aluminum oxide layer can be 4 to 10 nm, etc. When the passivation layer includes a silicon nitride layer, the thickness of the silicon nitride layer can be 50 to 150 nm, etc.
[0050] It should be noted that, unless otherwise specified, the content described in this application applies to at least one of the following four types of cells: the first collector electrode in a bifacial solar cell, the second collector electrode in a bifacial solar cell, the first collector electrode in a back-contact solar cell, and the second collector electrode in a back-contact solar cell.
[0051] Reference Figures 1 to 3 The current collector electrode of this application includes a seed portion and a base metal portion. At least a portion of the seed portion and at least a portion of the base metal portion are located within a window of the passivation layer. The seed portion is electrically contacted with the doped layer through this window. In the same current collector electrode, the base metal portion covers at least a portion of the seed portion. The seed portion can act as a barrier to the base metal, thereby preventing the diffusion of base metal elements in the base metal portion into the doped layer and the semiconductor substrate, reducing the recombination probability. The current collector electrode extends along a second direction Y and is spaced apart along a first direction X. The overall orientation of the current collector electrode or the main body is the second direction Y, but bending in other directions is allowed locally. Extensions mentioned in other locations in this application are similar and will not be described again. Here, the second direction Y and the first direction X intersect, and the included angle between them is not limited. For example, it can be close to 90°, such as 80° to 100°.
[0052] Reference Figures 3 to 4The seed portion includes a main body portion. In some embodiments, the seed portion further includes metal particles, and the main body portion encapsulates at least a portion of the metal particles. The metal particles can serve as arrangement sites for subsequent formation of the main body portion, reducing the plating difficulty of the main body portion and improving its uniformity. The surface of the doped layer away from the semiconductor substrate is the second surface. The metal particles are distributed on the second surface of the doped layer away from the semiconductor substrate in the form of scattered dots and / or agglomerates. The scattered dot distribution allows the metal particles to be more uniformly and dispersed on the second surface, thereby enabling the main body portion to be formed uniformly on the second surface as well. Ultimately, this results in a more uniform size of the main body portion of the seed portion at various locations. In addition, the metal particles contain noble metals, and this scattered distribution in the window also reduces costs. At the same time, agglomerates are beneficial for improving local contact effects. Therefore, the morphology of the metal particles in this application balances the dimensional uniformity of the main body portion of the seed portion at various locations, cost, and improved local contact effects.
[0053] It should be noted that the scattered distribution of metal particles mentioned in this application means that within the window, at least some of the metal particles are discontinuously distributed, and at least some of the metal particles have gaps between them.
[0054] In this application, the main element of the metal particles (including both the first metal particle and the second metal particle) differs from the main element of the seed portion and the main element of the base metal portion. The main element of the seed portion refers to an element comprising 50% or more by weight or mass. The main element of the base metal portion refers to an element comprising 50% or more by weight or mass. The main element of the metal particles refers to an element comprising 50% or more by weight or mass. Because the main element of the metal particles differs from the main element of the seed portion and the main element of the base metal portion, and therefore possesses different characteristics, it can fulfill the desired function of the metal particles.
[0055] Figure 3 This is a partially enlarged schematic diagram of the cross-section of the second doped layer 3 (corresponding to P-type) at the corresponding position in the solar cell of this application. Figure 4 This is a partially enlarged schematic diagram of the cross-section of the first doped layer 2 (corresponding to N-type) at the corresponding position in the solar cell of this application. Figure 3 and Figure 4 The diagram of some metal particles on the surface of the doped layer in the window is omitted. Figure 3 and Figure 4 The main purpose is to characterize the internal features of the first sub-body and the second sub-body, as well as the relevant features of the first doped layer and the second doped layer. Figure 3 and Figure 4They correspond to the same magnification factor.
[0056] Reference Figures 3 to 6 In the thickness direction Z of the solar cell, the main body of the seed section includes at least a first sub-main body 15 and a second sub-main body 16 stacked together. The first sub-main body 15 is farther away from the semiconductor substrate than the second sub-main body 16. The phosphorus content of the first sub-main body 15 is greater than that of the second sub-main body 16. The second sub-main body with a lower phosphorus content is easier to form on the doped layer and metal particles, and can reduce the formation difficulty of the second sub-main body with a higher phosphorus content. The first sub-main body with a higher phosphorus content can offset the tensile stress of the second sub-main body with a lower phosphorus content, which can improve the contact bonding effect between the main body and the metal particles, doped layer, and semiconductor substrate. This not only improves the current collection effect, but also reduces the risk of electrode detachment, thereby improving reliability and lifespan.
[0057] It should be noted that the phosphorus content here can refer to at least one of the following: mass percentage, weight percentage, atomic percentage, and volume percentage of phosphorus in the corresponding sub-subbody. It should also be noted that in some examples, the boundary between the first and second sub-subbody in the seed section can be distinguished according to the different mass percentages of phosphorus. For example, the mass percentage of phosphorus can be determined by methods such as EDS (energy dispersive spectroscopy). In other examples, the portion of the seed section extending more than 200 nm beyond the passivation layer surface on the side furthest from the semiconductor substrate can be considered the first sub-subbody.
[0058] In some embodiments, the phosphorus content of the first sub-body portion is 5% to 10% by mass, and the phosphorus content of the second sub-body portion is greater than or equal to 1% and less than 5% by mass. Directly plating a body portion or first sub-body portion with a phosphorus content of 5% to 10% by mass onto metal particles or a doped layer results in poor plating activity, demanding process conditions, and difficulty in plating, leading to low production efficiency and hindering mass production. Therefore, in this application, a second sub-body portion with a phosphorus content of greater than or equal to 1% and less than 5% by mass is first plated onto the doped layer or metal particles. For example, an alkaline reaction solution is used for plating. In an alkaline reaction solution, the second sub-body portion 16 with this phosphorus content is easily plated, and the plating speed is fast and readily available. Meanwhile, the plating activity of the second sub-body portion 16, with a phosphorus content of 1% to 5% by mass, is generally higher than that of metal particles. In this application, the second sub-body portion 16 with a slightly lower phosphorus content is plated first, and then the first sub-body portion 15 with a slightly higher phosphorus content is plated on top of the second sub-body portion 16. This second sub-body portion 16 significantly improves the plating activity of the first sub-body portion 15 with a slightly higher phosphorus content, reduces plating difficulty, increases plating speed, improves production efficiency, and facilitates mass production. The first sub-body portion of the seed portion, with a phosphorus content of 5% to 10% by mass, has almost no stress and good surface adhesion to metal particles or doped layers or semiconductor substrates. This improves the contact bonding effect between the body portion and the metal particles or doped layers or semiconductor substrates, not only improving the current collection effect but also reducing the risk of electrode detachment, thus improving reliability and lifespan. For example, the phosphorus content in the first sub-body portion can be 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, or 10%.
[0059] An acidic reaction solution can be used to plate and form a phosphorus-containing first sub-body portion 15, at least on the second sub-body portion. The acid pickling reaction solution here facilitates the plating formation of the first sub-body portion 15, which has a slightly higher phosphorus content. The acid pickling reaction solution can be one of: lactic acid-malic acid, lactic acid-propionic acid, or lactic acid-citric acid. The alkaline reaction solution used in this application can be one of: ammonia-ammonium chloride, sodium citrate, sodium gluconate, or triethanolamine.
[0060] In the plating step of the second sub-body 16, the pH value of the alkaline reaction solution is between 7.5 and 11. If the pH is too low, the plating is slow; if the pH is too high, the plating is too fast, resulting in poor quality of the second sub-body 16 and poor adhesion to metal particles or doped layers. Furthermore, an excessively high pH may also adversely affect other structures in the battery. Therefore, in this application, by controlling the pH of the alkaline reaction solution within the above-mentioned range, production efficiency is improved, the quality of the second sub-body 16 is guaranteed, and other structures in the battery are not affected. For example, the pH of the alkaline reaction solution can be 7.5, 7.8, 8, 8.3, 8.5, 9, 9.5, 10, 10.5, or 11.
[0061] In some embodiments, along the thickness direction Z of the solar cell, a second sub-body portion with a lower phosphorus content is distributed adjacent to a first sub-body portion with a higher phosphorus content. As mentioned earlier, the second sub-body portion with a lower phosphorus content is easier to form on the doped layer and metal particles, and can reduce the formation difficulty of the first sub-body portion with a higher phosphorus content. Therefore, their adjacent distribution directly promotes the formation process of the first sub-body portion with a higher phosphorus content, further reducing the process difficulty of the first sub-body portion with a higher phosphorus content. In this application, "adjacent distribution" means that the two parts can be in contact with each other, or that there are no other film layers blocking them.
[0062] In some embodiments, if the main elements of each sub-main body in the main body are the same, then the various sub-main bodies in the main body can share the main elements, and the relevant process parameters can also be compatible, which can improve production efficiency. The main element of a sub-main body refers to the element in the sub-main body that accounts for more than or equal to 50% of the mass.
[0063] In some embodiments, refer to Figure 3 and Figure 4 The main body includes a second sub-main body 16 and a first sub-main body 15 stacked sequentially along the thickness direction Z of the semiconductor substrate. The first sub-main body 15 is farther away from the semiconductor substrate 1 than the second sub-main body 16, and the first sub-main body 15 is denser than the second sub-main body 16. Specifically, the second sub-main body closer to the semiconductor substrate in the main body is more sparse, with more voids 17 per unit area. Metal particles 18 may fill the voids 17, or adjacent sub-main bodies may also be partially located in the voids, thus forming nested fixation. More nested fixation is formed closer to the semiconductor substrate, further improving the bonding force between the main body or current collector and the doped layer and semiconductor substrate, and reducing the risk of the current collector detaching from the battery. In addition, the first sub-main body closer to the base metal is denser, with tighter grain bonding and better electrical contact, strengthening the longitudinal transport of charge carriers and allowing charge carriers to be conducted more smoothly from the main body to the base metal.
[0064] It should be noted that, as mentioned earlier, the boundary between the first and second sub-sub-body portions in the seed section can be distinguished by their different degrees of density. By forming more nested fixation in the second sub-body portion closer to the semiconductor substrate, the adhesion between the current collector electrode and the doped layer and the semiconductor substrate can be significantly improved. The degree of density here can be characterized by the volume ratio of voids and the number of voids per unit area. A larger volume ratio of voids indicates a more porous sub-body portion. A larger number of voids per unit area indicates a more porous sub-body portion.
[0065] In some embodiments, refer to Figure 3 and Figure 4 In the main body portion, at least the second sub-main body portion closest to the semiconductor substrate contains a void 17. At least a portion of the metal particles 18 may fill this void, and at least a portion of the void 17 may also be filled with adjacent portions of the sub-main body portion. The metal particles filling the void, and the adjacent portions of the sub-main body portion filling the void 17, form a nested fixation between the metal particles 18, the portions of the adjacent sub-main body portion filling the void 17, and the sub-main body portion containing the void, thus improving their bonding strength. Simultaneously, since the sub-main body portion containing the void is closer to the semiconductor substrate, it also improves the bonding strength between the main body portion or current collector electrode and the doped layer and semiconductor substrate, reducing the risk of the current collector electrode detaching from the battery.
[0066] In some embodiments, refer to Figure 3 and Figure 4 The main body includes a second sub-main body 16 and a first sub-main body 15 stacked sequentially along the thickness direction Z of the semiconductor substrate. The first sub-main body 15 is farther away from the semiconductor substrate 1 than the second sub-main body 16. The number of voids 17 per unit area in the second sub-main body is greater than the number of voids 17 per unit area in the first sub-main body. That is, along the direction away from the semiconductor substrate (i.e., closer to the outside of the battery): in the same main body, the number of voids 17 per unit area in each sub-main body tends to decrease. Consequently, the sub-main body closer to the semiconductor substrate has more voids 17 per unit area, forming more nesting and fixing at positions closer to the semiconductor substrate. This further improves the bonding force between the main body or current collector and the doped layer and semiconductor substrate, reducing the risk of the current collector detaching from the battery. In addition, the first sub-main body with fewer voids per unit area is closer to the base metal portion, making the first sub-main body more dense and providing better electrical contact performance.
[0067] The unit area here can be 10nm×10nm, 5nm×10nm, 9nm×10nm, 8nm×10nm, etc. Alternatively, the number of voids in the sub-body within a unit area can be calculated by cropping the same area from the SEM or TEM images and counting the number of voids within that area. The above are merely examples of methods for counting the number of voids, and this application is not limited to the methods described above. In this application, SEM images refer to scanning electron microscope images, and TEM images refer to transmission electron microscope images.
[0068] Figure 5 and Figure 6 These are schematic diagrams showing the surface topography of two sub-main bodies within the same main body, facing away from the semiconductor substrate. Figure 5 and Figure 6 They all correspond to the same magnification factor. Figure 5 This is a partially enlarged schematic diagram of the cellular particles on the surface of the second sub-body portion of the main body portion, away from the semiconductor substrate. Figure 6 This is a partially enlarged schematic diagram of the cellular particles on the surface of the first sub-subbody in the main body that are far from the semiconductor substrate.
[0069] For example, Figure 3 and Figure 4 In the second sub-body portion, which is closer to the semiconductor substrate, the seed portion shown has a void 17 per unit area, while Figure 3 and Figure 4 The seed portion shown is located further away from the semiconductor substrate, and there are almost no gaps in the first subbody portion. Figure 6 In the middle layer, cellular particles are densely packed, providing a larger contact area with the upper slurry, and their surfaces are smooth. Cellular particles refer to the cell-like microstructures in the main body of the slurry.
[0070] In some embodiments, refer to Figure 3 and Figure 4The main body includes a second sub-main body 16 and a first sub-main body 15 stacked sequentially along the thickness direction Z of the semiconductor substrate. The first sub-main body 15 is farther from the semiconductor substrate 1 than the second sub-main body 16. The volume ratio of voids 17 per unit volume in the second sub-main body is greater than that in the first sub-main body. That is, along the direction farther from the semiconductor substrate (i.e., closer to the outside of the battery): within the same main body, the volume ratio of voids 17 per unit volume in each sub-main body tends to decrease. Consequently, the sub-main body closer to the semiconductor substrate has a larger volume ratio of voids 17 per unit volume, forming more nested fixation closer to the semiconductor substrate. This further enhances the bonding force between the main body or current collector and the doped layer and semiconductor substrate, reducing the risk of the current collector detaching from the battery. In addition, the first sub-main body with a smaller volume ratio of voids per unit area is closer to the base metal portion, making the first sub-main body more dense and providing better electrical contact performance.
[0071] The unit volume here can be 10nm×10nm×10nm, 5nm×10nm×10nm, 9nm×10nm×10nm, 8nm×10nm×10nm, etc. Alternatively, the volume percentage of voids in the sub-body within a unit volume can be determined by cropping the same area from the SEM or TEM images and calculating the area percentage of voids within that area. The above are merely examples of methods for determining the volume percentage of voids, and this application is not limited to the methods described above.
[0072] In some embodiments, refer to Figure 3 and Figure 4 In the first sub-body portion, which is closer to the surface of the main body portion and farther from the semiconductor substrate, the number of voids per unit area is less, and / or the volume ratio of voids per unit volume is smaller. That is, the first sub-body portion, which has a smaller volume ratio of voids per unit area and a smaller number of voids per unit area, is closer to the base metal portion. On the one hand, the first sub-body portion is more compact and has better electrical contact performance. On the other hand, the second sub-body portion, which is closer to the semiconductor substrate in the main body portion, has a larger volume ratio and more voids 17 per unit volume, forming more nested fixation at a position closer to the semiconductor substrate. This further enhances the bonding force between the main body portion or current collector electrode and the doped layer and semiconductor substrate, and reduces the risk of the current collector electrode detaching from the battery.
[0073] In some embodiments, each sub-body portion of the main body contains a microcrystalline portion, and the main body portion of the microcrystalline portion has good contact performance and good conductivity, which can improve the current collection effect.
[0074] In some embodiments, within the same main body portion, the number of grain boundaries in the second sub-main body portion is greater than the number of grain boundaries in the first sub-main body portion. Along the thickness direction Z of the solar cell, the second sub-main body portion with a larger number of grain boundaries is closer to the semiconductor substrate than the first sub-main body portion with a smaller number of grain boundaries. That is, along the direction away from the semiconductor substrate (i.e., closer to the outer edge of the cell), the number of grain boundaries in each sub-main body portion tends to decrease per unit area. Specifically, grain boundaries easily become crack propagation paths, and excessive grain boundaries can lead to tensile stress and delamination. In this application, along the direction away from the semiconductor substrate, the number of grain boundaries in the sub-main body portion tends to decrease; that is, the further away from the semiconductor substrate, the fewer grain boundaries the sub-main body portion has, and the less prone it is to delamination. This improves the contact bonding effect between the main body portion and the doped layer and semiconductor substrate, not only improving current collection efficiency but also reducing the risk of electrode detachment, thus improving reliability and lifespan. The statistical method for the number of grain boundaries per unit area here can be similar to the aforementioned method for counting the number of voids; to avoid repetition, it will not be elaborated here. In this application, the grain boundary in the subbody can refer to the grain boundary of microcrystals in the fingerprint-like lattice of the subbody as observed by TEM (transmission electron microscopy).
[0075] In some embodiments, the proportion of the microcrystalline portion in at least the first sub-body portion is greater than the proportion of the microcrystalline portion in the second sub-body portion. In the thickness direction Z of the solar cell, the second sub-body portion with a larger proportion of the microcrystalline portion is closer to the semiconductor substrate than the first sub-body portion with a smaller proportion of the microcrystalline portion. That is, along the direction away from the semiconductor substrate (i.e., closer to the outer edge of the cell): within the same body portion, the proportion of the microcrystalline portion in each sub-body portion tends to decrease, while the proportion of the amorphous portion increases. This proportion can be a volume percentage, etc. Along the direction away from the semiconductor substrate (i.e., closer to the outer edge of the cell): within the same body portion, each sub-body portion tends to transition from microcrystalline to amorphous, increasing the proportion of amorphous phase, reducing grain boundaries and defects, and rapidly decreasing tensile stress. This improves the contact bonding effect between the body portion and the doped layer and semiconductor substrate, not only improving current collection efficiency but also reducing the risk of electrode detachment, thus improving reliability and lifespan. Furthermore, the microcrystalline portion of the body portion has good contact performance and good conductivity, which can further improve current collection efficiency. Therefore, the main body of this application has both high contact performance and good current conductivity, as well as good adhesion to the doped layer and semiconductor substrate.
[0076] In some embodiments, the proportion of amorphous portion in the first sub-body portion is greater than the proportion of amorphous portion in the second sub-body portion. In the thickness direction of the solar cell, the sub-body portion with a larger proportion of amorphous portion is farther away from the semiconductor substrate than the sub-body portion with a smaller proportion of amorphous portion. Similarly, along the direction away from the semiconductor substrate (that is, closer to the outside of the cell), the proportion of amorphous portion in each sub-body portion of the same body portion tends to increase. This also improves the contact bonding effect between the body portion and the doped layer and semiconductor substrate, which not only improves the current collection effect but also reduces the risk of electrode detachment, thereby improving reliability and lifespan.
[0077] In some embodiments, the main body includes a second sub-main body 16 and a first sub-main body 15 stacked sequentially along the thickness direction Z of the semiconductor substrate. The first sub-main body 15 is farther away from the semiconductor substrate 1 than the second sub-main body 16. The surface undulation of the second sub-main body away from the semiconductor substrate is greater than that of the first sub-main body away from the semiconductor substrate. That is, along the direction away from the semiconductor substrate (i.e., closer to the outside of the battery), the surface undulation of each sub-main body away from the semiconductor substrate tends to decrease in the same main body. Consequently, the sub-main body closer to the semiconductor substrate in the main body has a greater surface undulation away from the semiconductor substrate, resulting in a larger contact area with the semiconductor substrate or doped layer, and better surface adhesion with the doped layer and semiconductor substrate. This improves the contact bonding effect between the main body and the doped layer and semiconductor substrate, not only improving the current collection effect but also reducing the risk of electrode detachment, thus improving reliability and lifespan. Furthermore, the more distant the sub-body portion from the semiconductor substrate is from the main body, the smaller and smoother the surface undulations are from the semiconductor substrate. Thus, the surface of the sub-body portion adjacent to the base metal portion in the main body is even smoother from the semiconductor substrate. Therefore, the formation conditions of the base metal portion at various positions on it are roughly the same, resulting in a more uniform base metal portion at various positions and better conductivity.
[0078] The undulation of the surface of the subbody that is far from the semiconductor substrate can be measured by the height difference between the highest and lowest points of the surface. More specifically, the undulation mainly refers to the degree of undulation caused by the relatively large high and low structure of the surface. In the same main body, in one case, the number of protrusions and / or depressions on the surface of the second sub-main body near the semiconductor substrate away from the semiconductor substrate is greater than the number of protrusions and / or depressions on the surface of the first sub-main body away from the semiconductor substrate away from the semiconductor substrate; in another case, the degree of protrusions and / or depressions on the surface of the second sub-main body near the semiconductor substrate away from the semiconductor substrate may be greater than the degree of protrusions and / or depressions on the surface of the first sub-main body away from the semiconductor substrate away from the semiconductor substrate; in yet another case, the arrangement of protrusions and / or depressions on the surface of the second sub-main body near the semiconductor substrate away from the semiconductor substrate may be more disordered than the arrangement of protrusions and / or depressions on the surface of the first sub-main body away from the semiconductor substrate away from the semiconductor substrate; in yet another case, the height of the protrusions and / or the depth of the depressions on the surface of the second sub-main body near the semiconductor substrate away from the semiconductor substrate may be greater than the height of the protrusions and / or the depth of the depressions on the surface of the first sub-main body away from the semiconductor substrate away from the semiconductor substrate.
[0079] By controlling the process parameters for forming each sub-subbody in the same main body, the process parameters for forming the first metal particle, and the process parameters for forming the second metal particle, it is possible to reduce the surface undulation of each sub-subbody in the same main body away from the semiconductor substrate along the direction away from the semiconductor substrate.
[0080] In some embodiments, the main body includes a second sub-main body 16 and a first sub-main body 15 stacked sequentially along the thickness direction Z of the semiconductor substrate. The first sub-main body 15 is farther from the semiconductor substrate 1 than the second sub-main body 16. The surface roughness of the second sub-main body away from the semiconductor substrate is greater than that of the first sub-main body away from the semiconductor substrate. That is, along the direction away from the semiconductor substrate (i.e., closer to the outside of the battery), the surface roughness of each sub-main body away from the semiconductor substrate tends to decrease in the same main body. Consequently, the surface roughness of the sub-main body closer to the semiconductor substrate in the main body is greater, resulting in a larger contact area with the semiconductor substrate or doped layer, and better surface adhesion with the doped layer and semiconductor substrate. This improves the contact bonding effect between the main body and the doped layer and semiconductor substrate, not only improving the current collection effect but also reducing the risk of electrode detachment, thus improving reliability and lifespan. Furthermore, the surface roughness and flatness of the sub-subbody portion further away from the semiconductor substrate in the main body portion are smaller. Therefore, the surface of the sub-subbody portion adjacent to the base metal portion in the main body portion is flatter. Thus, the formation conditions of the base metal portion are roughly the same at each position, and the formed base metal portion is more uniform at each position, resulting in better conductivity.
[0081] The method for measuring and implementing the roughness of the surface of the subbody that is far from the semiconductor substrate can be similar to the method for measuring and implementing the undulation of the surface of the subbody that is far from the semiconductor substrate, and will not be repeated here to avoid repetition.
[0082] Figure 5 and Figure 6 They all correspond to the same main body, and Figure 5 and Figure 6 They all correspond to the same magnification factor. Figure 5 This corresponds to the surface of the second sub-body portion in the main body that is away from the semiconductor substrate. Figure 6 The first sub-subbody in the main body corresponds to the surface away from the semiconductor substrate.
[0083] In some embodiments, refer to Figure 5 and Figure 6Within the same main body, the variance of the size of the cellular particles per unit area in the second sub-main body is greater than that in the first sub-main body. Along the thickness direction Z of the solar cell, the second sub-main body with a larger variance in the size of the cellular particles per unit area is closer to the semiconductor substrate than the first sub-main body with a smaller variance. In other words, the variance of the size of the cellular particles per unit area reflects the uniformity of the particle size. Within the main body, the further away from the semiconductor substrate, the more uniform the size of the cellular particles in the sub-main body. This results in a more uniform surface of the first sub-main body adjacent to the base metal portion, leading to roughly the same formation conditions for the base metal portion at various locations, resulting in a more uniform base metal portion and better conductivity.
[0084] Reference Figure 5 and Figure 6 The size of the cellular particles in the sub-body portion mainly refers to the particle diameter, etc. The variance of the size of the cellular particles in the sub-body portion can be calculated by taking the same area from the SEM or TEM images of the sub-body portion and then calculating the variance of the size of the cellular particles within that area. This is only an example and is not intended to limit this application. The number of cellular particles per unit area is not limited here. For example, one way to determine the unit area here is: for two sub-body portions with different average cellular particle sizes in the same body portion, the area of the sub-body portion with the larger average cellular particle size containing more than or equal to 5 cellular particles can be used as the unit area here. The selection of the unit area includes, but is not limited to, the example above. Subsequent determinations of the unit area of cellular particles are similar or the same, and will not be repeated here to avoid repetition.
[0085] In some embodiments, refer to Figure 5 and Figure 6 The average size of the cellular particles per unit area in the first sub-subbody is greater than that in the second sub-subbody. Along the thickness direction Z of the solar cell, the first sub-subbody with a larger average size of cellular particles per unit area is farther from the semiconductor substrate than the second sub-subbody with a smaller average size. The average size of the cellular particles per unit area reflects the size of the particles within that area. In the main body, the farther away from the semiconductor substrate, the larger the size of the cellular particles in each sub-subbody. This results in a larger sub-surface area for each cellular particle and a larger contact area between the cellular particles and the base metal portion. This increases the contact area between the main body and the base metal portion at a more microscopic level, leading to stronger adhesion and better conductivity.
[0086] In some embodiments, refer to Figure 5 and Figure 6The number of cellular particles per unit area in the second sub-body portion is greater than that in the first sub-body portion. In the thickness direction of the solar cell, the second sub-body portion with a larger number of cellular particles per unit area is closer to the semiconductor substrate than the first sub-body portion with a smaller number of cellular particles per unit area. The number of cellular particles per unit area reflects their size. A second sub-body portion with a larger number of cellular particles per unit area has smaller cellular particles, and a first sub-body portion with a smaller number of cellular particles per unit area has larger cellular particles. Therefore, the first sub-body portion with larger cellular particles per unit area is farther from the semiconductor substrate than the second sub-body portion with smaller cellular particles per unit area. Within the main body, the farther away from the semiconductor substrate, the larger the size of the cellular particles in each sub-body portion. This results in a larger sub-surface area for each cellular particle and a larger contact area between the cellular particles and the base metal portion. This increases the contact area between the main body and the base metal portion at a more microscopic level, leading to stronger adhesion and better conductivity.
[0087] In some embodiments, refer to Figure 3 and Figure 4 The main body contains 19 amorphous portions. Specifically, when the mass percentage of phosphorus is less than 5%, the phosphorus content in the sub-main body or the main body is low, exhibiting a microcrystalline structure with smaller crystal grains and more grain boundaries, which easily become crack propagation paths. This often manifests as tensile stress leading to delamination, affecting the contact and bonding between the main body or sub-main body and the metal particles or doped layers. When the mass percentage of phosphorus is greater than 5%, the main body or the first sub-main body typically has uniform cellular particles (larger crystal grains) and a moderate level of internal stress, improving the contact and adhesion with the metal particles or doped layers. With good strength, when the phosphorus content is in the range of 5% to 6%, the main body or the first sub-main body transforms from a microcrystalline state to an amorphous state (called the "critical phosphorus content"). The microcrystalline structure begins to disintegrate, the proportion of amorphous phase increases, grain boundaries and defects decrease, and tensile stress decreases rapidly. It can be considered that the amorphous part 19 is the part with very low stress. Therefore, the first sub-main body or main body with a phosphorus mass ratio of 5% to 10% has both high contact performance and good current conductivity, as well as good adhesion to metal particles or doped layers and semiconductor substrates, thus avoiding electrode structure detachment.
[0088] In some embodiments, the reference Figure 3 and Figure 4The amorphous portion 19 is located in the main body away from the semiconductor substrate. The amorphous portion 19 is further outward. On the one hand, the amorphous portion is more dense and has a better barrier effect against moisture, which can fully protect the internal doped layer and semiconductor substrate. On the other hand, the main body contains metal, and the amorphous portion is a metal amorphous layer, which is more dense and can also improve conductivity, thereby improving the contact bonding effect between the main body and the base metal. In addition, the amorphous portion is further outward, or rather, the more dense portion is further outward, which also has a better barrier effect against metal elements in the base metal portion, further reducing recombination and improving battery performance.
[0089] In some embodiments, refer to Figure 3 and Figure 4 In the main body, the thickness H7 of the amorphous portion 19 is 10 nm to 150 nm, and more specifically, 40 nm to 80 nm. If the thickness of the amorphous portion is too large, and the thickness of the microcrystalline portion in the main body is too small, it will have a certain impact on conductivity. If the thickness of the amorphous portion is too small, its effect on improving adhesion is poor. Therefore, in this application, the thickness of the amorphous portion is within the above-mentioned range, which not only provides good conductivity but also better adhesion to metal particles or doped layers and semiconductor substrates, preventing electrode structure detachment. For example, the thickness H7 of the amorphous portion 19 in the main body can be 10 nm, 30 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 100 nm, 140 nm, or 150 nm.
[0090] In some embodiments, refer to Figure 3 and Figure 4 The thickness H1 of the first sub-body portion 15 is greater than the thickness H2 of the second sub-body portion 16. Specifically, the main function of the second sub-body portion 16 is to enhance the plating activity of the first sub-body portion 15. Its thickness is sufficient to meet the requirements for enhancing the plating activity of the first sub-body portion 15. The main function of the first sub-body portion 15 is to reduce stress, hence its larger thickness further enhances the surface adhesion between the body portion and the metal particles or doped layer, further improving the contact bonding effect. This not only improves the current collection effect but also reduces the risk of electrode detachment, thereby improving reliability and lifespan. The thicknesses of both the first sub-body portion 15 and the second sub-body portion 16 are parallel to the thickness direction Z of the semiconductor substrate.
[0091] In some embodiments, refer to Figure 3 and Figure 4The thickness H2 of the second sub-body portion 16 is greater than or equal to 100 nm. If the thickness of the second sub-body portion 16 is too small, the improvement on the plating activity of the first sub-body portion 15 will be poor. Therefore, the thickness of the second sub-body portion 16 within the above-mentioned range significantly improves the plating activity of the first sub-body portion 15. For example, the thickness of the second sub-body portion 16 can be 100 nm, 200 nm, 300 nm, or 400 nm.
[0092] In the deposition step of the first sub-body portion 15, the pH value of the acidic reaction solution is between 4 and 6. If the pH is too low, the deposition of the first sub-body portion 15 is too rapid, affecting the quality of the first sub-body portion 15 and potentially impacting the performance of other structures in the solar cell. If the pH is too high, deposition is difficult, resulting in low production efficiency. In this application, by controlling the pH of the acidic reaction solution within the aforementioned range, production efficiency is improved while ensuring the quality of the first sub-body portion 15, without affecting the performance of other structures in the solar cell. For example, the pH value of the acidic reaction solution can be 4, 4.2, 4.5, 4.8, 5, 5.3, 5.5, 5.9, or 6.
[0093] In some embodiments, refer to Figure 3 and Figure 4 In the thickness direction Z of the solar cell: the main body has a portion extending beyond the passivation layer, and the thickness H4 of this extended portion is 150 nm to 800 nm. Too much of this extended portion is wasteful, while too little affects the resistivity of the main body and the current collection effect. Therefore, the thickness of the extended portion is within the above range, resulting in good contact between the main body and the doped layer and the base metal main body, good improvement of the plating activity of the first sub-main body, and without waste. For example, the thickness of this extended portion can be 150 nm, 180 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm, 750 nm, or 800 nm.
[0094] The thickness of the excess portion is the thickness at any location within the excess portion, or the maximum thickness, minimum thickness, or average of the thicknesses at multiple locations within the excess portion.
[0095] In some embodiments, refer to Figure 3 and Figure 4In the thickness direction Z of the solar cell: the thickness of the first sub-body portion H1 is between 100 nm and 500 nm. If this thickness is too small, it will affect the contact effect between the first sub-body portion and the base metal portion; if the thickness is too large, it will lead to waste. Therefore, the thickness of the first sub-body portion is within the above range, which ensures good contact between the first sub-body portion and the base metal portion without waste. For example, the thickness of the first sub-body portion can be 100 nm, 120 nm, 150 nm, 190 nm, 200 nm, 230 nm, 250 nm, 280 nm, 300 nm, 350 nm, 400 nm, 450 nm, or 500 nm.
[0096] The thickness of the first sub-body portion is calculated from the surface of the second sub-body portion away from the semiconductor substrate. The thickness of the first sub-body portion is the thickness at any position in the first sub-body portion, or the maximum thickness, minimum thickness, or the average of the thicknesses at multiple positions.
[0097] In some embodiments, refer to Figure 3 and Figure 4 The main body includes a first surface away from the semiconductor substrate. This first surface has protrusions and depressions, with the protrusions further away from the semiconductor substrate and the depressions closer to it. This first surface away from the semiconductor substrate is the surface where the main body and the base metal portion contact. The presence of protrusions and depressions on this surface results in a larger surface area, leading to a larger contact area with the base metal portion. This improves the bonding and contact effect between the main body and the base metal portion, enhancing the adhesion between them and making it difficult for the base metal portion or current collector electrode to detach from the battery surface, thus improving battery reliability and lifespan, and also enhancing current collection efficiency.
[0098] In some embodiments, refer to Figure 3 and Figure 4 The doped layer has a second surface away from the semiconductor substrate. In the seed portion, the projection of at least one metal particle agglomerate on the second surface at least partially overlaps with the projection of at least one protrusion on the first surface of the main body onto the second surface of the doped layer. Specifically, the metal agglomerates are beneficial for improving local contact effects. In this application, the projection of at least one metal particle agglomerate on the second surface at least partially overlaps with the projection of at least one protrusion on the second surface of the main body. That is, the position of at least one metal particle agglomerate corresponds to the position of the protrusion on the first surface of the main body. By controlling the distribution position and density of the metal particle agglomerates, more metal particle agglomerates can be placed in locations with poor contact bonding, thereby specifically improving the contact effect at specific locations while also considering battery costs.
[0099] It should be noted that if at least one agglomerate of metal particles in at least one seed portion of a solar cell at least partially overlaps with the projection of a protrusion on the first surface of the main body portion on the second surface, it falls within the protection scope of this application.
[0100] In some embodiments, the one-dimensional size of the metal particle agglomerates is between 10 nm and 200 nm. If the one-dimensional size of the metal particle agglomerates is too small, the improvement effect on contact and bonding strength at local locations is poor. If the maximum one-dimensional size of the metal particle agglomerates is too large, the metal particles, especially the agglomerates, are difficult to process, the process window is small, and the amount of metal particles used is not excessive, thus balancing cost. Therefore, the maximum one-dimensional size of the metal particle agglomerates is within the above range, balancing the improvement effect on contact and bonding strength at local locations with process difficulty and cost. Further, the one-dimensional size of the metal particle agglomerates can be between 50 nm and 150 nm. For example, the maximum one-dimensional size of the metal particle agglomerates can be 10 nm, 30 nm, 50 nm, 80 nm, 90 nm, 100 nm, 120 nm, 150 nm, 180 nm, or 200 nm. Here, the one-dimensional size of the metal particle agglomerates can refer to its maximum one-dimensional size, or the average of the one-dimensional sizes in several directions.
[0101] Specifically, the agglomeration of the first metal particles easily attracts the deposition of the second metal particles, forming agglomerations of the second metal particles. The agglomerations of the second metal particles, in turn, attract the body to deposit more quickly, forming a thicker layer and thus creating a protrusion.
[0102] In some embodiments, refer to Figure 3 and Figure 4 Aggregates of metal particles whose projections at least partially overlap with the projections of at least one protrusion on the first surface of the main body onto the semiconductor substrate or the second surface. Figure 3 , Figure 4 The metal particles (18) within the voids are located from the second surface of the doped layer to half the thickness of the seed portion. Specifically, the metal particles are the arrangement sites of the main body on the second surface of the doped layer. Therefore, the distribution position of the metal particle agglomerates is not too far away from the second surface of the doped layer, or in other words, the distribution position of the metal particle agglomerates is relatively close to the second surface of the doped layer. This means that the thickness of the metal particle agglomerates is not too large, which can reduce the amount of metal particles used and reduce costs. At the same time, it also improves the contact and bonding force at local locations.
[0103] For example, agglomerates of metal particles are located on the second surface, or from the second surface to 1 / 8, 1 / 7, 1 / 6, 1 / 5, 1 / 4, 1 / 3, or 1 / 2 of the thickness of the seed portion.
[0104] In some embodiments, the seed portion further includes metal particles, and the body portion encapsulates at least a portion of the metal particles; the body portion includes a first surface remote from the semiconductor substrate. The window includes an edge region and a middle region located inside the edge region. The edge region is closer to the remaining silicon nitride layer. For the same window, in the edge region of the body portion, the base metal portion is blocked by the remaining silicon nitride layer, resulting in poor contact between it and the body portion. The base metal portion is at risk of being pulled off in the window edge region. Therefore, in this application, by controlling the fabrication process, the degree of unevenness in the edge region of the first surface of the body portion remote from the semiconductor substrate is increased, thereby increasing the surface junction between the base metal portion and the body portion and improving the adhesion between them. The degree of unevenness can be measured by the height difference between the highest and lowest points at corresponding locations. For example, the difference between the highest and lowest points in the edge region of the first surface of the body portion remote from the semiconductor substrate is larger, while the difference between the highest and lowest points in the middle region of the first surface of the body portion remote from the semiconductor substrate is smaller. For example, the doped layer includes a P-type doped layer (which can be...). Figure 3 In the second doped layer 3), for the window located at the P-type doped layer position, the degree of unevenness H5 of the edge region of the first surface of the main body away from the semiconductor substrate is greater than that of the middle region of the first surface of the main body away from the semiconductor substrate, and the degree of unevenness H6 of the middle region of the first surface of the main body away from the semiconductor substrate. This is due to the different thermal responses of P-type and N-type doped layers to the instantaneous heat of the laser. Because the middle region of the P-type layer receives more laser heat, it is easier to thermally melt and form a flatter surface, which is detrimental to the adhesion of the P-type doped layer to the main body. In order to compensate for this thermal effect disadvantage, this application makes the edge region of the P-type doped layer more uneven, improves the overall bonding force of the region, and the electrical contact area between the P-type and the main body, thereby compensating for the difference caused by the doping concentration of the N-type and P-type doped layers and improving the performance of the battery.
[0105] More specifically, the unevenness mainly refers to the degree of undulation caused by the relatively large height difference structure of the first surface: the degree of unevenness in the edge region of the first surface of the main body is greater than that in the middle region of the first surface. In one case, the number of protrusions and / or depressions in the edge region of the first surface may be greater than the number of protrusions and / or depressions in the middle region of the first surface; in another case, the degree of protrusions and / or depressions in the edge region of the first surface may be greater than that in the middle region of the first surface; in yet another case, the arrangement of protrusions and / or depressions in the edge region of the first surface may be greater than that in the middle region of the first surface. The arrangement of protrusions and / or recesses is more disordered; in another case, the height of the protrusions and / or the depth of the recesses (quantitatively speaking, the longitudinal distance between the depression and the adjacent protrusion) in the edge region of the first surface may be greater than the height of the protrusions and / or the depth of the recesses in the middle region of the first surface; furthermore, the edge region of the first surface of the main body away from the semiconductor substrate has a greater degree of unevenness and the plating activity in the edge region is higher. Therefore, at various positions in the edge region of the first surface of the main body away from the semiconductor substrate, the thickness of the main body is relatively high, thereby compensating for the differences in the electrode structure at different positions caused by the shielding of the remaining passivation layer, improving the performance of the electrode structure, and improving the performance of the battery.
[0106] By controlling the process parameters for window formation, the formation of the first metal particle, and the formation of the second metal particle, a greater degree of unevenness can be achieved in the edge region of the first surface of the main body away from the semiconductor substrate. For example, if the laser energy is set at the edge of the laser opening, and a high-refractive-index film of silicon nitride remains at the bottom of the passivation layer during window opening, the silicon content at this location is high and the activity is strong, making it easy for the first metal particles to accumulate and form agglomerates of the first metal particles. This attracts the deposition of the second metal particles, forming agglomerates of the second metal particles, which in turn attracts faster deposition of the main body, thereby achieving a greater degree of unevenness in the edge region of the first surface of the main body away from the semiconductor substrate.
[0107] In some embodiments, for the same window: the size of at least some agglomerates of metal particles in the edge region is larger than the size of agglomerates of metal particles in the middle region. Similarly, at various locations in the edge region of the first surface of the main body away from the semiconductor substrate, the thickness of the main body is relatively high. This compensates for the differences in electrode structure at different locations caused by the obstruction of the remaining passivation layer, thereby improving the performance of the electrode structure and the battery performance. For example, for the same window located at the P-type doped layer location: the size of at least some agglomerates of metal particles in the edge region is larger than the size of agglomerates of metal particles in the middle region. This also compensates for the differences in electrode structure at different locations caused by the obstruction of the remaining passivation layer, improving the performance of the P-type electrode structure. This also compensates for the differences in doping concentration between the N-type and P-type doped layers, thereby improving the battery performance.
[0108] In some embodiments, refer to Figure 3 and Figure 4 The doped layers include P-type doped layers (corresponding to...) Figure 3 The second doped layer 3) and the N-type doped layer (corresponding to Figure 4 The first doped layer 2), the window includes an edge region and a middle region located inside the edge region; the main body includes a first surface away from the semiconductor substrate; in the first surface corresponding to the position of the P-type doped layer, the height difference between the middle region and the edge region (can be...) Figure 3 The difference between H5 and H6 is greater than the height difference between the edge and middle regions of the first surface corresponding to the N-type doped layer (which could be...). Figure 4 The degree of unevenness in the middle edge region, and Figure 4 (The difference between H6 in the middle) means that the height difference between the middle region and the edge region is large in the first surface corresponding to the P-type doped layer. This is because the thermal effects of the P-region and the N-region are different. This setting can compensate for the bonding force and electrical contact area of the P-region and balance the performance difference between the P-region doped layer and the N-region doped layer. The specific reasons are as described above.
[0109] Similarly, by controlling the process conditions for forming the window at the position corresponding to the N-type doped layer and the window at the position corresponding to the P-type doped layer, it can be achieved that the height difference between the middle region and the edge region in the first surface corresponding to the N-type doped layer position is small, while the height difference between the middle region and the edge region in the first surface corresponding to the P-type doped layer position is large.
[0110] In some embodiments, refer to Figure 3In the thickness direction Z of the solar cell, for the same window, the aforementioned H5 / H6 ratio is greater than 1 and less than or equal to 8. If the ratio is too large, the initial surface of the base metal portion on the main body becomes too undulating, making it difficult to form the base metal portion and resulting in poor uniformity. Therefore, a ratio within the aforementioned range not only compensates for the differences in electrode structure caused by the remaining passivation layer but also balances the process window and film quality of the base metal portion, further improving cell performance. For example, for the same window, the H5 / H6 ratio can be 1.1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, or 8.
[0111] Here, H5 can refer to the height difference between the highest and lowest points within at least a portion of the edge region of the main body portion away from the semiconductor substrate, per unit area or per unit length, within the same window. H6 is similar. The unit area here can be referred to in other relevant descriptions in this application. The unit length can be 0.5 nm, 0.1 nm, 1 nm, etc.
[0112] In some embodiments, refer to Figure 3 For the same window, the unevenness of the middle region of the first surface of the main body away from the semiconductor substrate is relatively gentle, and the height difference, or the difference between the high and low points, H6 in the middle region of the first surface is 0 to 50 nm. However, the unevenness of the edge region of the first surface of the main body away from the semiconductor substrate is relatively severe, and the difference between the high and low points, H5, in the edge region of the first surface of the main body away from the semiconductor substrate is 50 nm to 150 nm, with H5 significantly greater than H6. Similarly, at various positions in the edge region of the first surface of the main body away from the semiconductor substrate, the thickness of the main body is relatively high, thereby compensating for the differences in the electrode structure caused by the remaining passivation layer, improving the performance of the electrode structure, and thus improving the performance of the battery. For example, H6 can be 0, 1 nm, 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, or 50 nm. For example, H5 can be 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, or 150nm.
[0113] In some embodiments, refer to Figure 3 and Figure 4 The height difference between the surface of the main body and the surface away from the silicon substrate is 30nm to 200nm (e.g., it could be...). Figure 3 H5 in Figure 6The height difference between the main body and the surface of the silicon substrate (H6 in the original text) is not too large, making the formation of the film layer on it easier. Furthermore, this height difference can enhance the interlocking or nesting effect between the main body and the structures thereon, further improving contact and adhesion. Similarly, the height difference between the highest and lowest points can be determined at least a portion of the surface of the main body away from the silicon substrate, within a unit area or unit length. The unit area here can be referred to in other relevant descriptions in this application. The unit length can be 0.5 nm, 0.1 nm, 1 nm, etc. For example, the height difference between the main body and the surface of the silicon substrate can be 30 nm, 50 nm, 80 nm, 100 nm, 130 nm, 150 nm, 180 nm, 190 nm, or 200 nm.
[0114] In some embodiments, the doped layer includes a P-type doped layer (the second doped layer 3 in the figures) and an N-type doped layer (the first doped layer 2 in the figures), the window includes an edge region and a middle region located inside the edge region; the main body includes a first surface remote from the semiconductor substrate; Reference Figure 3 and Figure 4 In the first surface corresponding to the N-type doped layer, the degree of unevenness H6 in the middle region is greater than that in the first surface corresponding to the P-type doped layer. That is to say... Figure 4 In the first surface corresponding to the N-type doped layer, the degree of unevenness H6 in the middle region is greater than... Figure 3 In the first surface corresponding to the P-type doped layer, the degree of unevenness in the middle region is H6. If the degree of unevenness in the middle region of the first surface corresponding to the P-type doped layer is slightly smaller, then the degree of unevenness in the middle region of the first surface corresponding to the P-type doped layer is relatively small. Specifically, compared to the N-type doped layer, the P-type doped layer is usually difficult to obtain a high doping concentration. Moreover, the middle region is the main region in this electrode structure. The middle region of the first surface corresponding to the P-type doped layer is relatively flat, and the growth conditions of the base metal part on it are relatively uniform, which can make up for the difference caused by the doping concentration of the N-type doped layer and the P-type doped layer.
[0115] Similarly, by controlling the process conditions for forming the window at the position corresponding to the N-type doped layer and the process conditions for forming the window at the position corresponding to the P-type doped layer, it can be achieved that the degree of unevenness H6 in the middle region of the first surface corresponding to the N-type doped layer position is larger, and the degree of unevenness H6 in the middle region of the first surface corresponding to the P-type doped layer position is smaller.
[0116] In some embodiments, refer to Figure 3 and Figure 4 The thickness H3 of the main body corresponding to the N-type doped layer (first doped layer 2) is greater than the thickness H3 of the main body corresponding to the P-type doped layer (second doped layer 3), which can improve the current collection efficiency.
[0117] In some embodiments, the window includes an edge region and a middle region located inside the edge region. Specifically, due to the presence of the remaining passivation layer, the contact area or contact reliability between the doped layer and the current collector electrode in the edge region of the window is relatively weak. In this application, the agglomerates of the first metal particles and the agglomerates of the second metal particles in the edge region of the window are larger, thereby enhancing the electrical connection between the doped layer and the electrode structure in the edge region of the window, further improving the current collection and conduction effect of the solar cell, and improving the performance of the cell.
[0118] In this application, the size of the agglomerate can refer to at least one of the following: the length, width, and height of the agglomerate; the area of the agglomerate's orthographic projection onto the first surface; or the volume of the agglomerate. For example, in the embodiment using a Gaussian laser spot for windowing, the energy is higher in the center of the Gaussian spot, resulting in higher heating and more severe melting in the center of the doped layer. This leads to a decrease in the surface roughness of the doped layer at the center of the window due to melting and collapse. Conversely, the surface roughness of the doped layer near the edge of the window is greater. Since greater roughness usually indicates higher activity, it is easier to attract metal particles to deposit there. Therefore, the size of at least some agglomerates of the first metal particles in the edge region of the same window is greater than the size of agglomerates of the first metal particles in the center region. In other words, agglomerates of the first metal particles are more likely to accumulate in the edge region of the window.
[0119] It should be noted that, for the same window, the relative sizes of the central and edge regions are not limited. When comparing the sizes of aggregates in the central and edge regions, the comparison can be limited to the same area or volume.
[0120] For the same window, the difference between the size of a single aggregate in the edge region and the size of a single aggregate in the middle region is not limited. It should be noted that, in this application, when the sizes of aggregates at different locations in the edge region of the same window differ, the size of the aggregates in the edge region of the same window can be the minimum size, the maximum size, or the arithmetic mean of two or more aggregates in the edge region of the same window. The method for determining the size of aggregates in the middle region of the same window is the same as the method for determining the size of aggregates in the edge region of the same window, and will not be repeated to avoid repetition.
[0121] Specifically, by controlling the process parameters for forming the window, the size of the agglomerates of the first metal particles in the edge region of the aforementioned window can be increased. For example, when using laser opening, the laser energy is lower at the edge of the laser opening, and the high-refractive-index film of the residual silicon nitride at the bottom of the passivation layer remains when the window is opened. This location has a high silicon content and strong activity, making it easy for the first metal particles to accumulate, and thus more likely to attract the deposition of the second metal particles.
[0122] In some embodiments, in a back-contact solar cell, reference Figure 2 Along the first direction X, the backlight surface of the semiconductor substrate includes a first region and a second region distributed sequentially; a first doped layer is disposed in the first region of the backlight surface of the semiconductor substrate, and a second doped layer is disposed in the second region of the backlight surface of the semiconductor substrate. A back passivation layer is located on the side of the first and second doped layers away from the semiconductor substrate, and the back passivation layer includes a portion that is deposited around the edge region of the front passivation layer away from the semiconductor substrate. Specifically, for a back-contact solar cell, the front passivation layer 11 is made first, followed by the passivation layer on the backlight side of the semiconductor substrate 1, and the backlight-side passivation layer will wrap around the edge region of the front passivation layer 11. Specifically, in a back-contact solar cell, when the backlight-side back passivation layer is made first, and then the front passivation layer 11 is made, the front passivation layer 11 typically contains a passivation layer such as a silicon nitride layer, and the front passivation layer is deposited around the backlight side. When making the front passivation layer, it is usually located in the isolation region between the first and second regions. Figure 2In the semiconductor substrate 1, the region between the dashed lines L1 and L2 on the backlight side already exists. Due to the numerous corners or complex shapes of the isolation region, during the formation of the front passivation layer such as the silicon nitride layer, at least a portion of the isolation region on the backlight side of the semiconductor substrate may have gaps with the coating boat. This can easily lead to gas not contacting at least a portion of the isolation region at the backlight side edge of the semiconductor substrate according to the preset ratio. Therefore, active silicon may exist at at least a portion of the isolation region at the backlight side edge of the semiconductor substrate. During the metal particle deposition step, at least a portion of the isolation region at the backlight side edge of the semiconductor substrate may be affected. Metal particles are also formed in at least some locations. However, there is usually a height difference between the isolation region and the first and second regions. During the cleaning step, due to the height difference, the cleaning liquid may not be able to fully contact the isolation region, resulting in metal particles remaining in at least some isolation regions at the back-side edge of the semiconductor substrate. These metal particles will attract and form the main body in the subsequent main body formation step. Both the main body and the residual metal particles have good conductivity, causing the main body and the residual metal particles in at least some isolation regions at the back-side edge of the semiconductor substrate to conduct electricity to the adjacent first and second doped layers, resulting in severe leakage. Therefore, in this application, by first preparing the front passivation layer 11 and then preparing the back passivation layer such as a silicon nitride layer on the back side, the structure of the back side is simple when preparing the front passivation layer. Using existing processes, the portion of the front silicon nitride layer that can be deposited around the back side can be completely or substantially cleaned, avoiding the aforementioned leakage problem and improving the performance of the back contact solar cell.
[0123] In some embodiments, refer to Figure 7 and Figure 8 The metal particles include: a first metal particle 13 and a second metal particle 14. The main body encapsulates at least a portion of the first metal particle and / or at least a portion of the second metal particle. The first and second metal particles serve as arrangement sites for subsequent plating to form the main body, which can reduce the plating difficulty of the main body and improve the uniformity of the main body. The surface of the doped layer away from the semiconductor substrate is the second surface, and the projections of the first metal particle 13 and the second metal particle 14 on the second surface at least partially overlap or are located close to each other. For example, Figure 7 In this process, the second metal particle 14 is attached to the first metal particle 13, and the second metal particle 14 encapsulates at least a portion of the first metal particle 13. For example, Figure 8 In this configuration, the second metal particle 14 is positioned approximately the same as the first metal particle 13, and the second metal particle 14 is interspersed and fills the gaps between adjacent first metal particles 13. It should be noted that the relative positions of the first metal particle 13 and the second metal particle 14 include, but are not limited to, those described above. Figure 7 and Figure 8Example method.
[0124] It should be noted that one reason for including the first metal particles in this application is that the second metal particles serve as catalytic sites for the main body of the seed section. However, research has shown that the reduction activity of the second metal particles from ionic to metal particle state on the surface of the doped layer is weak. This makes it difficult to form a sufficient number of catalytic sites on the first surface of the doped layer for the subsequent reduction of the main body of the seed section. Ultimately, this not only leads to a longer reaction time and reduced battery production efficiency, but also results in fewer and unevenly distributed second metal particles on the first surface, leading to weaker adhesion with the doped layer and poor contact performance. Therefore, in this application, by first including cheaper and more reactive first metal particles, better-dispersed metal particle dots or aggregates are formed on the second surface of the doped layer. This encourages the second metal particles to preferentially reduce and deposit at the locations of the first metal particles, allowing the subsequently formed second metal particles to be more widely and evenly distributed on the first surface of the doped layer within the window. This improves the adhesion between the first metal particles, the main body of the seed section, the base metal section, and the doped layer, thereby enhancing contact performance and reaction speed.
[0125] In this application, the advantage of setting a second metal particle is that it is usually difficult to form the main body of the seed part on the first metal particle by means of redox reaction, which affects the quality of the main body of the seed part and results in low production efficiency; in this application, by setting a second metal particle as a catalyst for the main body, the difficulty of forming the seed part by means of redox reaction is reduced, and the production efficiency is high.
[0126] In summary, in this application, the first metal particle and the second metal particle work together to make the first metal particle and the second metal particle widely and uniformly distributed on the doped layer within the window, which improves the contact performance between the metal particle and the main body of the seed part, increases the specific surface area of the catalytic site, and accelerates the formation rate of the main body of the seed part; at the same time, using the cheaper first metal particle can reduce the amount of second metal particle (catalyst) used, further reducing production costs.
[0127] In some embodiments, the main elements of the first metal particle and the second metal particle are different, and the characteristics of the first metal particle and the second metal particle are different, which facilitates the first metal particle and the second metal particle to achieve the aforementioned corresponding functions. The main element of the first metal particle refers to the element with a mass percentage greater than or equal to 50% in the first metal particle.
[0128] In some embodiments, the material of the first metal particle is selected from at least one of platinum, gold, silver, cobalt, and indium. On the one hand, the doped layer usually contains silicon, and the above materials can be quickly reduced by the silicon-containing doped layer, which can not only reduce the damage to the doped layer and the semiconductor substrate, but also reduce the reaction cost and further reduce the battery cost. On the other hand, the first metal particle of the above materials can play a greater activating role for the second particle.
[0129] In some embodiments, the material of the second metal particle is selected from at least one of zinc, platinum, gold, silver, chromium, rhodium, indium, palladium and tin. The second metal particles of the above materials are more likely to be attracted by the first metal particle to nucleate and grow in its vicinity, so that the first metal particle and the second metal particle can be more uniformly and dispersedly distributed on the second surface of the doped layer away from the semiconductor substrate.
[0130] In some embodiments, the Fermi level of the first metal particle can be higher than that of the doped layer. This facilitates the simple and rapid formation of the aforementioned first metal particle using redox reactions or other methods with the doped layer. This not only reduces damage to the doped layer and the semiconductor substrate but also lowers reaction costs, further reducing battery costs. The Fermi level of the doped layer mentioned in this application refers to the core parameter describing the electron filling state in the doped layer; it refers to the energy level position where electrons occupy a 50% probability under thermal equilibrium conditions. The doping type and concentration of the doped layer all affect its Fermi level. The Fermi level of the first metal particle is the highest energy level occupied by electrons at absolute zero, and this position directly reflects the conductivity of the first metal particle. Specifically, generally, the higher the Fermi level of the first metal particle, the better its conductivity. The size and material of the first metal particle also affect its Fermi level. If the Fermi level of the first metal particle is higher than that of the doped layer, the cations of the first metal particle are more easily reduced to the first metal particle by the doped layer.
[0131] It should be noted that there is no limitation on whether the second metal particles will also directly adhere to the doped layer within the window. For example, a small number of second metal particles may directly adhere to the doped layer within the window, while most of the second metal particles may directly adhere to the first metal particles.
[0132] In some embodiments, the first metal particles are distributed in the form of scattered dots and / or agglomerates on the second surface of the doped layer away from the semiconductor substrate. The scattered dot distribution allows the first metal particles to be more uniformly and dispersed on the second surface, thereby enabling the second metal particles to also be uniformly and dispersedly distributed on the second surface. Ultimately, the first and second metal particles can be uniformly and dispersedly distributed on the second surface of the doped layer away from the semiconductor substrate, thereby improving the dimensional uniformity of the main body of the seed portion at various locations. On the other hand, the first metal particles here contain noble metals, and the scattered distribution in this window also reduces costs. At the same time, agglomerates are beneficial for improving local contact effects. Therefore, the morphology of the first metal particles in this application takes into account the dimensional uniformity of the main body of the seed portion at various locations, cost, and local improvement of contact effects. The second metal particles are also distributed in the form of scattered dots and / or agglomerates on the second surface of the doped layer away from the semiconductor substrate, with beneficial effects similar to the distribution of the first metal particles, and will not be described again to avoid repetition.
[0133] It should be noted that the first metal particles mentioned in this application being distributed in a scattered manner means that within the window, at least some of the first metal particles are discontinuously distributed, and at least some of the first metal particles have gaps between them.
[0134] In some embodiments, the material of the main body of the seed section (the main body of the first seed section of the first electrode structure, the main body of the second seed section of the first electrode structure) is selected from: titanium (Ti), tungsten (W), chromium (Cr), nickel (Ni), cobalt (Co), molybdenum (Mo), tin (Sn), lead (Pb), palladium (Pd), niobium (Nb), ruthenium (Ru), indium (In), zinc (Zn), titanium boride (TiB). x ), Tantalum nitride (TaN) x ), Tungsten nitride (WN) x Titanium nitride (TiN) x Titanium-tungsten alloy (TiW) x ), titanium silicon compounds (TiSi) x Titanium silicon nitride (TiSiN), tantalum silicon nitride (TaSiN) x At least one of nickel vanadium (NiV) and hexagonal boron nitride. Specifically, the resistivity and barrier properties of the above materials are suitable for the main body of the seed section. In particular, choosing nickel and / or zinc and / or titanium as the material for the main body of the seed section has the following advantages: firstly, it has good contact performance; secondly, it does not penetrate into the semiconductor substrate, resulting in less recombination; and thirdly, it has a good barrier effect on the metals in the base metal section, which can prevent the metals in the base metal section from penetrating into the semiconductor substrate, thus reducing recombination.
[0135] It should be noted that there is no specific limitation on whether the main elements of the first seed section and the second seed section are the same; they can be the same or different. It should also be noted that x in the above chemical formula is a number greater than 0. The main elements of the first seed section and the second seed section can be the same or different; there is no specific limitation on this. In particular, if the main elements of the first seed section and the second seed section are the same, their main materials are compatible, which can improve production efficiency. The main element of the first seed section refers to the element whose mass percentage in the main body of the first seed section is greater than or equal to 50%. The main element of the second seed section is similar, and will not be repeated here to avoid repetition.
[0136] In some embodiments, refer to Figure 3 and Figure 4 The thickness H3 of the seed portion or the main body of the seed portion can be 200-900 nm. If this thickness is too large, it may be wasteful; if it is too small, the barrier effect against alkali metals is poor. Therefore, a thickness within the above range not only provides good barrier effect against alkali metals but also avoids waste. For example, the thickness H3 of the seed portion or the main body of the seed portion can be 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, or 900 nm.
[0137] In some embodiments, the base metal portion is made of at least one of copper, chromium, lead, aluminum (Al), and silver-clad copper. Firstly, the above-mentioned materials have good electrical conductivity. Secondly, except for silver, the above-mentioned materials have low cost, which can reduce the cost of the electrode. Thirdly, the seed portion has a good barrier effect on the above-mentioned materials, preventing their penetration into the semiconductor substrate and reducing recombination. Fourthly, the above-mentioned materials are suitable for forming the base metal portion using low-temperature processes, avoiding the introduction of more thermal effects into the solar cell.
[0138] It should be noted that there is no specific limitation on whether the materials of the first base metal part and the second base metal part are the same; they can be the same or different. For example, copper or silver-plated copper can be used to form the base metal part using a low-temperature process. The materials of the first base metal part and the second base metal part can be the same or different; there is no specific limitation on this.
[0139] In some embodiments, refer to Figure 9For at least some windows corresponding to the P-type doped layer located at the edge region of the solar cell, the central area of these windows may be discontinuous, resulting in exposed passivation layer (second passivation layer 5). For example, in the windows corresponding to the P-type current collectors of at least five P-type doped layers at the edge of the solar cell, the central area may be discontinuous. Specifically, due to the presence of wrap-around plating, the passivation layer at the edge of the solar cell may be thicker. During the window formation process, the passivation layer at the edge of the solar cell may not be completely removed. Because the N-type doped layer has a higher doping concentration and may have higher plating activity, the central area of the window corresponding to the N-type doped layer is generally continuous, and there is no mixing of passivation layer and central area. Because the doping concentration of the P-type doped layer is relatively low, and as mentioned above, the edge of the window may have greater roughness, the plating activity is higher. Therefore, the central area of the window corresponding to the P-type doped layer is usually also continuous, thus compensating for the contact differences at different locations of the P-type doped layer.
[0140] This application also provides a photovoltaic module comprising multiple series-connected and / or parallel-connected cell strings, each cell string including: an electrical connector and any of the aforementioned solar cells. The electrical connector electrically connects at least two of the aforementioned solar cells. The electrical connector mentioned in this application may be a solder ribbon, a conductive electrical connector, etc. The photovoltaic module may further include: an encapsulation layer covering the surface of the cell strings, the encapsulation layer may include an encapsulating film, etc., and a cover plate covering the surface of the encapsulation layer away from the cell strings. The electrical connector here may refer to a solder ribbon, a conductive backplate, etc., without specific limitation. The cover plate may be glass, etc., without limitation on the specific material.
[0141] For example, in a battery string, an electrical connector electrically connects the first current collector electrode of one of two adjacent solar cells to the second current collector electrode of the other solar cell.
[0142] It should be noted that the solar cells and photovoltaic modules provided in this application are related to each other, and to avoid duplication, the relevant parts will not be repeated.
[0143] It should be noted that the various embodiments provided in this application may exist independently or in combination without contradiction, and all are within the protection scope of this application.
[0144] The following specific examples further illustrate the implementation of the first layer independently. The example uses a back-contact solar cell; bifacial solar cells are similar and will not be discussed further.
[0145] Example First step, refer to Figure 2The battery body includes a semiconductor substrate 1. Along the thickness direction Z of the solar cell, the semiconductor substrate 1 includes a light-facing surface and a back-light-facing surface opposite to each other. Along a first direction X, the back-light-facing surface includes a first region and a second region sequentially distributed. A first doped layer 2 is disposed in the first region of the back-light-facing surface of the semiconductor substrate, and a second doped layer 3 is disposed in the second region of the back-light-facing surface. A passivation layer is disposed on the side of the first doped layer 2 and the second doped layer 3 away from the semiconductor substrate 1. The passivation layer has a window, which exposes part of the first doped layer and the second doped layer. Specifically, the front passivation layer 11 is formed first, and then the passivation layer on the back-light-facing side of the semiconductor substrate 1 is formed. The window can be formed by means of a laser, which can remove laser byproducts and oxides within the window. The first doped layer is an N-type doped layer, and the second doped layer is a P-type doped layer.
[0146] The second step involves depositing a first metal particle on the exposed doped layer within the window. The first metal particle is cobalt.
[0147] The third step involves depositing a second metal particle on the first metal particle exposed in the window and its vicinity. The second metal particle is tin.
[0148] The fourth step involves depositing a substrate onto at least the exposed metal particles of the doped layer in the window to form the main body. This can be achieved using methods such as electroless plating to form a second sub-sub ...
[0149] The difference in phosphorus content between the first sub-body portion 15 and the second sub-body portion 16 is shown in the elemental distribution map of the cross-section of the body portions by TEM testing. In the first sub-body portion 15, the phosphorus content is relatively dense, while in the second sub-body portion 16, the phosphorus content is relatively sparse. The first sub-body portion 15 has a 50-70 nm amorphous portion on its surface layer away from the semiconductor substrate. (Refer to...) Figure 3 and Figure 4 As shown.
[0150] The second sub-body 16 uses an alkaline (ammonium) system as the reaction solution, with a process temperature of 45-60℃ and a pH range of 7.5-11. It has a fast plating initiation time and is easy to deposit on metal particles. The first sub-body 15 uses an acidic system as the reaction solution, with a process temperature of 75-85℃ and a pH range of 4-6. It has a slow plating initiation time on metal particles and is difficult to deposit autonomously. However, it can deposit normally in the second sub-body 16.
[0151] The fifth step involves printing the base metal portion onto at least the main body. Simultaneously, the battery's main grid pattern is added to the printing screen, and a low-temperature base metal paste is printed to form the battery. The main element of the base metal portion can be copper.
[0152] Performance tests were conducted on 1000 solar cells formed in the example, and the average value was calculated. The average contact resistance of the N-type current collector electrode was ≤0.1 mΩ × cm. 2 The average contact resistance of the P-type collector electrode is ≤0.8 mΩ×cm. 2 Both exhibited low contact resistance, indicating that the current collector electrode in this example achieved good contact with the doped layer and semiconductor substrate. This not only improves the current collection effect but also enhances the bonding force between the main body and the base metal part, making it difficult for the base metal part or the current collector electrode to detach from the battery surface, thereby improving the reliability and lifespan of the battery.
[0153] The terms "first" and "second" in the specification and claims of this application may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise stated, "multiple" means two or more. Furthermore, "and / or" in the specification and claims indicates at least one of the connected objects, and the character " / " generally indicates that the preceding and following objects are in an "or" relationship.
[0154] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.
[0155] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection between two components. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.
[0156] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0157] Although embodiments of this application have been shown and described, those skilled in the art will understand that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of this application, the scope of which is defined by the claims and their equivalents.
Claims
1. A solar cell, characterized in that, include: Semiconductor substrate; A doped layer and a passivation layer are sequentially disposed on the semiconductor substrate, and the passivation layer has a window. An electrode structure is located on the side of the passivation layer opposite to the semiconductor substrate. The electrode structure includes a seed portion and a base metal portion, with at least a portion of the seed portion located within the window. The seed portion contacts the doped layer through the window, and the base metal portion covers at least a portion of the seed portion. The seed portion includes a body portion. In the thickness direction of the solar cell, the main body includes at least a first sub-main body and a second sub-main body stacked together, wherein the first sub-main body is further away from the semiconductor substrate than the second sub-main body; and the phosphorus content of the first sub-main body is greater than the phosphorus content of the second sub-main body.
2. The solar cell according to claim 1, characterized in that, In the thickness direction of the solar cell, the first sub-body portion and the second sub-body portion are distributed adjacent to each other.
3. The solar cell according to claim 2, characterized in that, In the thickness direction of the solar cell: The thickness H1 of the first sub-body portion is greater than the thickness H2 of the second sub-body portion; and / or, The thickness H1 of the first sub-body portion is 100 nm to 500 nm; and / or, The thickness H2 of the second sub-body portion is greater than or equal to 100 nm; and / or, The thickness H3 of the main body is 200 nm to 900 nm; and / or, The main body has a portion that extends beyond the passivation layer, and the thickness H4 of the extended portion is 150 nm to 800 nm.
4. The solar cell according to claim 1, characterized in that, The seed portion further includes metal particles, and the main body portion encloses at least a portion of the metal particles; the main element of the metal particles is different from the main element of the main body portion and the main element of the base metal portion; In the main body, at least the second sub-main body contains a void, and at least some of the metal particles are located in the void.
5. The solar cell according to claim 1, characterized in that, The first sub-body portion is denser than the second sub-body portion.
6. The solar cell according to claim 1, characterized in that, Both the first sub-body portion and the second sub-body portion contain gaps; The number of voids per unit area in the second sub-body is greater than the number of voids per unit area in the first sub-body; and / or, The volume ratio of the void per unit volume in the second sub-body is greater than the volume ratio of the void per unit volume in the first sub-body.
7. The solar cell according to claim 1, characterized in that, The height difference between the main body and the surface of the semiconductor substrate is 30nm to 200nm.
8. The solar cell according to claim 1, characterized in that, The seed portion further includes metal particles, and the body portion encloses at least a portion of the metal particles; the window includes an edge region and a central region located inside the edge region; the body portion includes a first surface remote from the semiconductor substrate; for the same window: The degree of unevenness H5 in the edge region of the first surface is greater than the degree of unevenness H6 in the middle region of the first surface; and / or, The size of at least a portion of the agglomerates of the metal particles in the edge region is larger than the size of the agglomerates of the metal particles in the middle region.
9. The solar cell according to claim 8, characterized in that, 1 < H5 / H6 ≤ 8; and / or, H6 ≤ 50 nm; and / or, 30 nm ≤ H5 ≤ 150 nm.
10. The solar cell according to claim 1, characterized in that, The doped layer includes a P-type doped layer and an N-type doped layer; the window includes an edge region and a middle region located inside the edge region; the main body includes a first surface remote from the semiconductor substrate. In the first surface corresponding to the P-type doped layer, the height difference between the middle region and the edge region is greater than the height difference between the edge region and the middle region in the first surface corresponding to the N-type doped layer.
11. The solar cell according to claim 1, characterized in that, The doped layer includes a P-type doped layer and an N-type doped layer; the window includes an edge region and a middle region located inside the edge region; the main body includes a first surface remote from the semiconductor substrate. In the first surface corresponding to the N-type doped layer, the degree of unevenness H6 in the middle region is greater than that in the first surface corresponding to the P-type doped layer.
12. The solar cell according to claim 1, characterized in that, The variance of the size of the cellular particles per unit area in the second sub-body portion is greater than the variance of the size of the cellular particles per unit area in the first sub-body portion; and / or, The average size of the cellular particles per unit area in the first sub-body portion is greater than the average size of the cellular particles per unit area in the second sub-body portion; and / or, The number of cellular particles per unit area in the second sub-body portion is greater than the number of cellular particles per unit area in the first sub-body portion.
13. The solar cell according to claim 1, characterized in that, The main elements of each sub-main body in the main body are the same.
14. The solar cell according to claim 1, characterized in that, The surface roughness of the second sub-body portion away from the semiconductor substrate is greater than the surface roughness of the first sub-body portion away from the semiconductor substrate; and / or, The surface roughness of the second sub-body portion away from the semiconductor substrate is greater than the surface roughness of the first sub-body portion away from the semiconductor substrate.
15. The solar cell according to claim 1, characterized in that, The main body includes an amorphous portion located in the main body away from the semiconductor substrate; the thickness of the amorphous portion is 1 nm to 150 nm.
16. The solar cell according to claim 1, characterized in that, The doped layer includes a P-type doped layer and an N-type doped layer; The thickness of the main body portion corresponding to the N-type doped layer position is greater than the thickness of the main body portion corresponding to the P-type doped layer position.
17. The solar cell according to claim 1, characterized in that, The seed portion further includes metal particles, and the main body portion encloses at least a portion of the metal particles; the main element of the metal particles is different from the main element of the main body portion and the main element of the base metal portion; The main body includes a first surface that is away from the semiconductor substrate; The first surface has protrusions and depressions, and in the seed portion, the projection of at least one agglomerate of the metal particles onto the semiconductor substrate at least partially overlaps with the projection of at least one protrusion onto the semiconductor substrate.
18. The solar cell according to any one of claims 1 to 17, characterized in that, The phosphorus content of the first sub-body is 5% to 10% by mass, and the phosphorus content of the second sub-body is greater than or equal to 1% and less than 5% by mass.
19. The solar cell according to any one of claims 1 to 17, characterized in that, The doped layer is divided into a first doped layer and a second doped layer with different polarities; the passivation layer is divided into a first passivation layer and a second passivation layer; the electrode structure is divided into a first electrode structure and a second electrode structure. The first doped layer has the same doping type as the semiconductor substrate, and the second doped layer has a different doping type than the semiconductor substrate; The first doped layer, the first passivation layer, and the first electrode structure are located on different sides of the semiconductor substrate, respectively, as are the second doped layer, the second passivation layer, and the second electrode structure; or, The first doped layer, the first passivation layer, and the first electrode structure are all located on the same side of the semiconductor substrate as the second doped layer, the second passivation layer, and the second electrode structure.
20. The solar cell according to any one of claims 1 to 17, wherein the solar cell is characterized in that, The surface of the doped layer away from the semiconductor substrate is a second surface. The metal particles include: a first metal particle and a second metal particle. The projections of the first metal particle and the second metal particle on the second surface at least partially overlap or are close to each other. The first metal particle and the second metal particle are made of different materials; The material of the first metal particle is selected from at least one of platinum, gold, silver, cobalt, and indium; and / or, The material of the second metal particle is selected from at least one of zinc, platinum, gold, silver, chromium, rhodium, indium, palladium, and tin; and / or, The material of the main body is selected from at least one of the following: titanium, tungsten, chromium, nickel, cobalt, molybdenum, tin, lead, palladium, niobium, ruthenium, indium, zinc, titanium boride, tantalum nitride, tungsten nitride, titanium tungsten alloy, titanium silicon compound, titanium silicon nitride, tantalum silicon nitride compound, nickel vanadium, and hexagonal boron nitride; and / or, The base metal part is made of at least one of the following: copper, chromium, lead, aluminum, and silver-plated copper.
21. A photovoltaic module, characterized in that, include: Multiple battery strings connected in series and / or in parallel, the battery strings comprising: electrical connectors and solar cells according to any one of claims 1 to 20, the electrical connectors electrically connecting at least two electrode structures of the solar cells; An encapsulation layer is used to cover the surface of the battery string; A cover plate is used to cover the surface of the encapsulation layer away from the battery string.