A solar cell, a battery module and a photovoltaic system

By setting a passivation layer, an ultraviolet absorption layer, and an antireflection layer on the surface of the silicon substrate of the solar cell, the problem of efficiency degradation caused by ultraviolet light is solved, and effective cutoff of ultraviolet light and good utilization of visible light are achieved, thereby improving the photogenerated carrier excitation and power output of the battery module.

CN123124510APending Publication Date: 2026-11-17ZHUHAI FUSHAN AIKO SOLAR ENERGY TECH CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611265404.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The problem of efficiency degradation of existing solar cells under ultraviolet light irradiation is mainly due to the lack of good optical matching between the ultraviolet absorption layer and the antireflection layer, making it difficult to simultaneously achieve good cutoff of ultraviolet light and good utilization of visible light.

Method used

A passivation layer, an ultraviolet absorption layer, and an antireflection layer are disposed on the surface of a silicon substrate in a solar cell. The refractive index of the ultraviolet absorption layer is 2.2~3.4, and the refractive index of the antireflection layer is 1.5~2.2. By adding an ultraviolet absorption layer between the passivation layer and the antireflection layer, a low-medium-high refractive index gradient transition is formed, which achieves effective cutoff of ultraviolet light and good utilization of visible light.

Benefits of technology

It improves the UV cutoff effect of solar cells, reduces the probability of UV damage to Si-H bonds, stabilizes the UV cutoff function, avoids increased film cost and process complexity, increases the total excitation of photogenerated carriers, and enhances the power output of the battery module.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124510A_ABST
    Figure CN123124510A_ABST
Patent Text Reader

Abstract

This invention relates to the field of photovoltaic technology and provides a solar cell, a battery module, and a photovoltaic system. The solar cell includes: a silicon substrate, the silicon substrate including a first surface; a passivation layer disposed on the first surface; an ultraviolet (UV) absorption layer disposed on the passivation layer, the UV absorption layer having a refractive index of 2.2 to 3.4; and an antireflection layer disposed on the UV absorption layer, the antireflection layer having a refractive index of 1.5 to 2.2, and the difference between the refractive index of the UV absorption layer and the refractive index of the antireflection layer being greater than or equal to 0.2. The solar cell of this invention utilizes the UV absorption layer to block UV light, while simultaneously optimizing the refractive indices of the UV absorption layer and the antireflection layer, achieving good utilization of visible light and good UV light blocking in the solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photovoltaic technology, and in particular to a solar cell, a battery module, and a photovoltaic system. Background Technology

[0002] During long-term outdoor operation, battery modules are exposed to ultraviolet (UV) light from sunlight. The wavelength of UV light is 280nm~400nm. High-energy UV light in sunlight can break the Si-H bonds of solar cells, resulting in a decrease in the photoelectric conversion efficiency of solar cells (referred to as UV-induced degradation).

[0003] In related technologies, in order to reduce the efficiency degradation of solar cells caused by ultraviolet light, an ultraviolet absorption layer is set on the surface of the solar cell. However, the refractive index of the ultraviolet absorption layer of the solar cell is not well optically matched with the antireflection layer of the solar cell, making it difficult for the solar cell to simultaneously achieve good ultraviolet light cutoff and good visible light utilization. Summary of the Invention

[0004] This invention provides a solar cell that aims to solve the problem that existing solar cells have poor optical matching between the ultraviolet absorption layer and the antireflection layer, making it difficult to simultaneously achieve good ultraviolet light cutoff and good visible light utilization.

[0005] This invention is implemented by providing a solar cell, comprising: A silicon substrate, the silicon substrate including a first surface; A passivation layer is provided on the first surface; An ultraviolet absorbing layer is disposed on the passivation layer, the refractive index of the ultraviolet absorbing layer being 2.2~3.4; and An antireflection layer is disposed on the ultraviolet absorption layer, the refractive index of the antireflection layer is 1.5~2.2, and the difference between the refractive index of the ultraviolet absorption layer and the refractive index of the antireflection layer is greater than or equal to 0.2.

[0006] Preferably, the passivation layer has a thickness of D1, the ultraviolet absorption layer has a thickness of D2, and the ratio of D2 to D1 is greater than or equal to 2.

[0007] Preferably, the thickness of the antireflective layer is D3, and the ratio of D3 to D2 is 0.3 to 3.

[0008] Preferably, the total thickness of D3 and D2 is less than 150 nanometers.

[0009] Preferably, the thickness of the passivation layer is 2 to 10 nanometers.

[0010] Preferably, the thickness of the ultraviolet absorption layer is 10~70 nanometers.

[0011] Preferably, the extinction coefficient of the ultraviolet absorption layer for light with a wavelength of 390~780 nm is less than 0.1, and the extinction coefficient of the ultraviolet absorption layer for ultraviolet light with a wavelength of less than or equal to 320 nm is greater than 0.1.

[0012] Preferably, the difference between the refractive index of the ultraviolet absorption layer and the refractive index of the antireflection layer is greater than or equal to 0.5.

[0013] Preferably, the first surface includes an edge region and a middle region located inside the edge region, and the thickness of the ultraviolet absorption layer in the edge region is greater than the thickness of the ultraviolet absorption layer in the middle region.

[0014] Preferably, the ultraviolet absorption layer includes pores.

[0015] Preferably, the first surface includes an edge region and a middle region located inside the edge region, and the pore density of the ultraviolet absorption layer in the edge region is greater than the pore density of the ultraviolet absorption layer in the middle region.

[0016] Preferably, the ultraviolet absorption layer comprises a metal oxide, wherein the band gap of the metal oxide is 2.8~4.0 eV.

[0017] Preferably, the metal oxide includes one or a combination of at least two of titanium oxide, zinc oxide, hafnium oxide, zirconium oxide, yttrium oxide, scandium oxide, magnesium oxide, and tin oxide.

[0018] Preferably, the metal oxide includes titanium oxide.

[0019] Preferably, the titanium oxide comprises anatase phase.

[0020] Preferably, the metal oxide includes titanium oxide, which comprises anatase phase, rutile phase, and brookite phase, and the proportion of the anatase phase is greater than the proportion of the rutile phase or the brookite phase.

[0021] Preferably, the ratio of oxygen content to metal content in the ultraviolet absorption layer is greater than 2.

[0022] Preferably, the passivation layer comprises one or at least two of the following: a silicon oxide layer, an aluminum oxide layer, a silicon oxynitride layer, a silicon nitride layer, and a hafnium oxide layer.

[0023] Preferably, the passivation layer includes a first sub-passivation layer and a second sub-passivation layer stacked on the first sub-passivation layer, the second sub-passivation layer being located between the first sub-passivation layer and the ultraviolet absorption layer, and the thickness of the second sub-passivation layer being greater than the thickness of the first sub-passivation layer.

[0024] Preferably, the first sub-passivation layer is a silicon oxide layer, and the second sub-passivation layer is at least one of an aluminum oxide layer, a silicon nitride layer, and a silicon oxynitride layer.

[0025] Preferably, the thickness of the first sub-passivation layer is 0.1~2 nanometers, and the thickness of the second sub-passivation layer is 0.5~8 nanometers.

[0026] Preferably, a first optical coupling layer is provided between the passivation layer and the ultraviolet absorption layer, and the refractive index of the first optical coupling layer is between the refractive index of the passivation layer and the refractive index of the ultraviolet absorption layer.

[0027] Preferably, a second optical coupling layer is provided between the ultraviolet absorption layer and the antireflection layer, and the refractive index of the second optical coupling layer is between the refractive index of the ultraviolet absorption layer and the refractive index of the antireflection layer.

[0028] The present invention also provides a battery assembly including the solar cell described above.

[0029] The present invention also provides a photovoltaic system including the above-described battery module.

[0030] This invention provides a solar cell by sequentially depositing a passivation layer, an ultraviolet (UV) absorption layer, and an antireflection layer on the first surface of a silicon substrate. This allows for the direct addition of a UV absorption layer between the passivation layer and the antireflection layer, integrating the UV absorption layer onto the solar cell. As part of the solar cell, the UV absorption layer absorbs UV light passing through the front glass and the front encapsulant film of the cell module. Compared to adding UV-blocking components to the encapsulant film, the UV absorption layer in this application does not rely on the polymer encapsulant film, eliminating the problem of UV-blocking function degradation caused by encapsulant film degradation. This results in a more stable long-term UV-blocking effect, enhancing the long-term reliability of the solar cell against UV-induced degradation. Furthermore, forming a UV absorption layer on the first surface of the solar cell effectively blocks UV light from entering the silicon substrate, reducing the probability of defects such as UV damage to Si-H bonds, thereby significantly mitigating the UV-induced degradation problem of the solar cell. Since the ultraviolet (UV) cutoff function has already been implemented in solar cells, there is no need to specially select UV-cutting encapsulant films when encapsulating battery modules. This avoids increasing the cost of encapsulant films and the complexity of the process due to the addition of UV absorbers, thereby reducing the difficulty and cost of battery module production.

[0031] Meanwhile, this invention controls the refractive index of the ultraviolet absorption layer to be 2.2~3.4 and the refractive index of the antireflection layer to be 1.5~2.2, while the refractive index of a typical silicon substrate is 3.85~3.90. Furthermore, the difference between the refractive index of the ultraviolet absorption layer and the refractive index of the antireflection layer is controlled to be greater than or equal to 0.2, resulting in a low-to-medium-to-high gradient transition in the refractive indices of the antireflection layer, the ultraviolet absorption layer, and the silicon substrate. This allows incident sunlight to gradually couple into the silicon substrate with lower reflection loss, thereby effectively increasing the total number of photogenerated carriers excited. Moreover, the difference between the refractive index of the ultraviolet absorption layer and the refractive index of the antireflection layer is greater than or equal to 0.2, ensuring a smooth transition between low-to-medium-to-high refractive indices of the ultraviolet absorption layer and the antireflection layer. Maintaining an effective refractive index difference between the layers prevents the difference between the refractive index of the ultraviolet absorption layer and the antireflection layer from being too small. This ensures that the antireflection layer has a sufficiently high refractive index to perform broadband antireflection function, while ensuring that the ultraviolet absorption layer has a sufficiently high refractive index to construct a gradient refractive index gradient and ultraviolet interface interference effect. This achieves a significant reduction in the reflectivity of the solar cell in the visible light band and a significant improvement in the cutoff efficiency in the ultraviolet band. It also enables the solar cell to achieve good utilization of visible light and good cutoff of ultraviolet light. Furthermore, through the optical refractive index matching design of the two layers, it also compensates for the current loss caused by the ultraviolet absorption layer blocking ultraviolet light, ensuring good power of the battery module. Attached Figure Description

[0032] Figure 1 A cross-sectional schematic diagram of a solar cell provided in an embodiment of the present invention; Figure 2 A cross-sectional schematic diagram of another solar cell provided in an embodiment of the present invention; Figure 3 A cross-sectional schematic diagram of another solar cell provided in an embodiment of the present invention; Figure 4 A cross-sectional schematic diagram of another solar cell provided in an embodiment of the present invention; Figure 5 A cross-sectional schematic diagram of another solar cell provided in an embodiment of the present invention; Figure 6 A graph showing the relationship between the passivation layer thickness and module power loss in a solar cell, provided as an embodiment of the present invention; Figure 7 A graph showing the relationship between the contribution of different wavelengths of sunlight to the UV attenuation and power contribution of the module; Figure 8 This is a graph showing the relationship between the refractive index and extinction coefficient of titanium oxide at different crystal phases corresponding to different wavelengths.

[0033] Explanation of key symbols: Solar cell 100, silicon substrate 1, first surface 11, second surface 12, passivation layer 2, first sub-passivation layer 21, second sub-passivation layer 22, ultraviolet absorption layer 3, antireflection layer 4, first doped layer 5, second doped layer 6, back passivation and antireflection layer 7, first metal electrode 81, second metal electrode 82, edge region E, middle region F, first optical coupling layer 91, second optical coupling layer 92. Detailed Implementation

[0034] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. Examples of embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the invention, and should not be construed as limiting the invention. Furthermore, it should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0035] In the description of this invention, it should be understood that the terms "upper", "lower", "back", "front", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this invention.

[0036] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of the second feature includes the first feature directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature includes the first feature directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.

[0037] The following disclosure provides numerous different embodiments or examples for implementing various structures of the invention. To simplify the disclosure, specific examples of components and arrangements are described below. These are merely examples and are not intended to limit the invention. Furthermore, reference numerals and / or letters may be repeated in different examples; such repetition is for simplification and clarity and does not in itself indicate a relationship between the various embodiments and / or arrangements discussed. In addition, examples of various specific processes and materials are provided in this invention, but those skilled in the art will recognize the application of other processes and / or the use of other materials.

[0038] In related technologies, early solar cell modules mostly used non-UV-blocking (high-transmittance) EVA encapsulating films, allowing ultraviolet light to penetrate the film and tempered glass to reach the solar cell surface. This is because traditional p-type aluminum back-field cells and early p-type PERC cells had a high surface doping concentration on the front side (p...). + Emitter surface concentration is typically >1×10² 0 cm - ³) and a relatively thick field-effect passivation layer. The passivation quality is not sensitive to UV-induced hydrogen desorption. UV-induced degradation (UVID) was not considered a significant reliability issue in the PERC era, and UV testing was only performed as a routine item in IEC 61215 certification.

[0039] To address the issues of yellowing, acetic acid corrosion of grid lines, and backsheet embrittlement caused by long-term ultraviolet irradiation in early EVA films, the industry once promoted the use of ultraviolet-blocking EVA films (with added organic ultraviolet absorbers and a cutoff wavelength of approximately 380nm), which effectively blocked short-wave ultraviolet rays and alleviated yellowing.

[0040] Subsequently, to improve optical utilization and nominal power, the industry tended to use high-transmittance films (UV transparent EVA or POE), which have a UV transmittance of >85% in the 320~400nm wavelength range. In the PERC module era, because the cells were not sensitive to UV, the loss of UV protection by high-transmittance films did not show significant negative consequences. With the industrialization of N-type tunneling oxide passivated contact (TOPCon) and heterojunction (HJT) solar cells, low surface concentration p-type films were adopted on the front side of the cells. + In doped regions or undoped silicon substrates, field passivation is achieved solely through passivation contact structures, with the passivation effect highly dependent on Si-H chemical passivation. High-permeability films allow ultraviolet B (UVB) light to reach the cell surface directly. The photon energy is sufficient to break Si-H bonds, leading to hydrogen atom desorption, increased interface state density, and decreased minority carrier lifetime. This manifests as a decrease in open-circuit voltage and fill factor—significantly amplifying the UVID phenomenon in N-type high-efficiency cells.

[0041] To address this issue, the mainstream measures currently used in modules include: (1) reusing UV cutoff films but adjusting the cutoff edge from the early 380nm to approximately 340-350nm (UVB cutoff film) to block destructive short-wave UV while retaining some UVA photons; (2) using UV downconversion (light conversion) films to convert harmful UV photons into visible blue light that can be absorbed by the battery, thus providing both protection and efficiency enhancement, but at a relatively high cost. After power / attenuation balance optimization, the nominal power of modules using 350nm cutoff films or light conversion films is usually about 0.5~2W lower than that using high-transparency films.

[0042] Battery-side mitigation measures mainly include: appropriately thickening the front-side ALD AlOx passivation layer (typically from 3~4nm to 5~8nm) to improve hydrogen storage, adjusting AlOx and SiNx deposition parameters to adjust the hydrogen content and bonding configuration of the film, and optimizing high-temperature annealing / hydrogenation annealing processes to improve hydrogen binding energy, but these measures have limited effect on UVID resistance. Simply adjusting the battery-side process involves trade-offs between passivation quality, optical absorption, and process window, and cannot completely offset the effects of high-intensity UVB under high-transmittance films; simply cutting off or downconverting UV at the encapsulation end introduces power loss or increased costs. Therefore, a comprehensive solution that balances UV protection, minimizes power loss, and ensures long-term reliability is still needed.

[0043] Some studies have mentioned using ultraviolet absorption layers such as TiO2 and SnO2 at the battery end to reduce UVID degradation of module products. However, this solution has the following drawbacks: 1) The anti-UV principle is the same as that of the cut-off film, but it increases the cost and complexity of the battery process. In contrast, the cut-off film does not require any process additions or changes, and its cost is the same as that of the high-transparency film; 2) The passivation effect is poor and a mismatch in anti-reflection occurs.

[0044] The following section uses titanium dioxide (TiO2) thin film as an example to introduce the technical problems of using ultraviolet absorption layers in batteries.

[0045] Titanium dioxide (TiO2) thin films, with their ultraviolet absorption edge of approximately 380–410 nm and ability to absorb short-wave ultraviolet light with wavelengths < 380 nm, were used as single-layer or double-layer antireflective coatings for crystalline silicon solar cells in the 1980s and 1990s. We are studying candidate materials for Reflection Coating (ARC) with the aim of combining anti-reflection and ultraviolet shielding functions.

[0046] However, TiO2 thin films were ultimately phased out in mainstream photovoltaic cell production lines and failed to gain widespread application. The fundamental reason lies in the inherent performance defects of the TiO2 material itself: (1) Poor film density and insufficient hydrothermal stability: sol TiO2 films obtained by typical preparation processes such as the gelation method generally possess a nanoporous structure, which readily adsorbs water vapor in the atmospheric environment, leading to refractive index shift, film cracking, and the release of water vapor and corrosive ions (such as Na+). + The penetration channels into the battery surface significantly degrade the passivation effect and the long-term stability of the metal electrodes.

[0047] (2) Photocatalytic activity accelerates the aging of encapsulation materials: Anatase TiO2 has strong photocatalytic activity and generates hydroxyl radicals (·OH) and superoxide anion radicals (·O2) under ultraviolet light excitation. - Highly reactive free radicals such as EVA film can continuously catalyze the decomposition of organic components in adjacent encapsulation materials, accelerating film yellowing, acetic acid release, and backsheet embrittlement, which seriously violates the basic requirement of 25 years or more of weather resistance for battery modules.

[0048] (3) There is an essential trade-off in optical performance: Although the intrinsic ultraviolet absorption of TiO2 can shield UV, B, but this absorption is accompanied by additional parasitic absorption and scattering losses in the visible light region (especially the blue-violet band 400~450nm). In contrast, monolayer SiN with optimized thickness and refractive index... x It exhibits superior broadband antireflection performance in the 400–1200 nm wavelength range, resulting in a significantly better short-circuit current gain than TiO2 monolayer. In other words, while attempting to block harmful ultraviolet light, TiO2 inevitably sacrifices more valuable visible light energy.

[0049] (4) Lack of effective chemical passivation mechanism: Unlike SiN prepared by plasma-enhanced chemical vapor deposition (PECVD), x Thin films are rich in Si-H and NH bonds, enabling them to serve as efficient hydrogen sources for the diffusion of hydrogen atoms into the silicon bulk for passivation. In contrast, TiO2 films (whether anatase or rutile phase) have extremely low intrinsic hydrogen (H) content and lack good hydrogen diffusion and passivation capabilities. This means that TiO2 can only provide limited field-effect passivation and cannot achieve the same level of passivation as SiN. x This approach reduces the defect state density within the silicon wafer through hydrogen passivation. However, given the extremely high dependence of high-efficiency solar cells (such as TOPCon) on hydrogen passivation, simply introducing a TiO2 layer not only fails to contribute passivation gain but may also obstruct the underlying SiN layer. x The outward diffusion of hydrogen atoms weakens the overall passivation effect.

[0050] Due to the multiple inherent defects at the material level mentioned above—especially photocatalytic risk, poor damp-heat stability, optical parasitic absorption, and passivation failure caused by extremely low intrinsic hydrogen content—TiO2 has never become the mainstream choice for the front-side film system in mass production of crystalline silicon solar cells.

[0051] It is worth noting that although N-type TOPCon / HJT batteries exhibit UV-induced degradation (UVID) sensitivity, there is currently no industrial trend in the industry to actively reintroduce TiO2 films as the front UV absorption layer of the battery. While existing UV cutoff films / phototransfer films are mature, a trade-off between power loss (0.5~2W) remains. Simply adding a TiO2 layer merely to improve cutoff capability would not only inherit the aforementioned fatal flaws but also exacerbate the degradation of battery passivation performance due to the extremely low hydrogen content of TiO2, which is clearly unacceptable. Therefore, a breakthrough technology is urgently needed that can circumvent the inherent defects of TiO2 while unlocking its UV absorption potential and achieving compatibility or even enhancement with existing passivation systems.

[0052] Please refer to Figures 1-2 This invention provides a solar cell 100, comprising: Silicon substrate 1, the silicon substrate 1 includes a first surface 11; Passivation layer 2 is provided on the first surface 11; An ultraviolet absorption layer 3 is disposed on the passivation layer 2, and the refractive index of the ultraviolet absorption layer 3 is 2.2~3.4; and An antireflection layer 4 is disposed on the ultraviolet absorption layer 3. The refractive index of the antireflection layer 4 is 1.5~2.2, and the difference between the refractive index of the ultraviolet absorption layer 3 and the refractive index of the antireflection layer 4 is greater than or equal to 0.2.

[0053] In this embodiment of the invention, the silicon substrate 1 includes a first surface 11 and a second surface 12 disposed opposite to each other along its thickness direction. The first surface 11 is the light-facing surface of the solar cell 100, and the second surface 12 is the back-lighting surface of the solar cell 100. That is, the first surface 11 is the side of the solar cell 100 that mainly receives sunlight when it is working normally, and the second surface 12 can also receive some sunlight when the solar cell 100 is actually working.

[0054] In this embodiment of the invention, the specific cell type of the solar cell 100 is not limited. For example, the solar cell 100 can be a back-contact solar cell or a double-sided contact solar cell.

[0055] like Figure 1As shown, when the solar cell 100 is a back-contact solar cell, the second surface 12 is alternately provided with a first doped layer 5 and a second doped layer 6. One of the first doped layer 5 and the other of the second doped layer 6 is a P-type doped layer, and the other is an N-type doped layer. A first metal electrode 81 is disposed on the first doped layer 5, and a second metal electrode 82 is disposed on the second doped layer 6. The solar cell 100 may further include a back passivation antireflection layer 7 covering at least the first doped layer 5 and the second doped layer 6. The first metal electrode 81 passes through the back passivation antireflection layer 7 and is electrically connected to the first doped layer 5, and the second metal electrode 82 passes through the back passivation antireflection layer 7 and is electrically connected to the second doped layer 6. The passivation layer 2, the ultraviolet absorption layer 3, and the antireflection layer 4 are sequentially stacked on the first surface 11. The back passivation antireflection layer 7 serves to passivate the second surface 12 and reduce sunlight reflection. The back passivation antireflection layer 7 can be a silicon nitride layer or a silicon oxynitride layer.

[0056] like Figure 2 As shown, when the solar cell 100 is a double-sided contact solar cell, a first doped layer 5 is disposed on the first surface 11, and a second doped layer 6 is disposed on the second surface 12. One of the first doped layer 5 and the second doped layer 6 is a P-type doped layer, and the other is an N-type doped layer. A first metal electrode 81 is disposed on the first doped layer 5, and a second metal electrode 82 is disposed on the second doped layer 6. A passivation layer 2, an ultraviolet absorption layer 3, and an antireflection layer 4 are sequentially stacked on the first doped layer 5 on the first surface 11. The solar cell 100 may further include a passivation and antireflection layer 7 covering the second doped layer 6. The first metal electrode 81 passes through the antireflection layer 4, the ultraviolet absorption layer 3, and the passivation layer 2 and is electrically connected to the first doped layer 5. The second metal electrode 82 passes through the back passivation and antireflection layer 7 and is electrically connected to the second doped layer 6.

[0057] The present invention provides a solar cell 100 by sequentially depositing a passivation layer 2, an ultraviolet absorption layer 3, and an antireflection layer 4 on the first surface 11 of a silicon substrate 1. Thus, an ultraviolet absorption layer 3 is directly added between the passivation layer 2 and the antireflection layer 4, integrating the ultraviolet absorption layer 3 onto the solar cell 100. As part of the solar cell 100, the ultraviolet absorption layer 3 absorbs ultraviolet light passing through the front glass and front encapsulant film of the cell module. Compared to adding ultraviolet-blocking components to the encapsulant film, the ultraviolet absorption layer 3 of this application does not rely on the polymer encapsulant film, and there is no problem of ultraviolet-blocking function degradation caused by encapsulant film degradation. The long-term ultraviolet-blocking effect is more stable, making the solar cell 100 more reliable against long-term ultraviolet light-induced degradation. Furthermore, the ultraviolet absorption layer 3 formed on the first surface 11 of the solar cell 100 effectively blocks ultraviolet light from entering the cell, reducing the probability of defects such as ultraviolet light damaging Si-H bonds, thereby significantly alleviating the problem of ultraviolet light-induced degradation of the solar cell 100. Since the ultraviolet blocking function has been implemented in the solar cell 100, there is no need to specially select an ultraviolet blocking encapsulant film when encapsulating the battery module. This avoids increasing the cost of the encapsulant film and the complexity of the process due to the addition of ultraviolet absorbers, which can reduce the production difficulty and cost of the battery module.

[0058] Meanwhile, this invention controls the refractive index of the ultraviolet absorption layer 3 to be 2.2~3.4, and the refractive index of the antireflection layer 4 to be 1.5~2.2, while the refractive index of the silicon substrate 1 is typically 3.85~3.90. Furthermore, the difference between the refractive index of the ultraviolet absorption layer 3 and the refractive index of the antireflection layer 4 is controlled to be greater than or equal to 0.2, resulting in a low-to-medium-to-high gradient transition in the refractive indices of the antireflection layer 4, the ultraviolet absorption layer 3, and the silicon substrate 1. This allows incident sunlight to gradually couple into the silicon substrate 1 with lower reflection loss, thereby effectively increasing the total number of photogenerated carriers excited. The difference between the refractive index of the ultraviolet absorption layer 3 and the refractive index of the antireflection layer 4 is greater than or equal to 0.2, ensuring a low-to-medium-to-high gradient transition in the refractive indices of the ultraviolet absorption layer 3 and the antireflection layer 4. Maintaining an effective refractive index difference between layers 4 avoids the refractive index difference between the ultraviolet absorption layer 3 and the antireflection layer 4 being too small. This ensures that the antireflection layer 4 has a sufficiently high refractive index to perform broadband antireflection function, and that the ultraviolet absorption layer 3 has a sufficiently high refractive index to construct a gradient refractive index gradient and ultraviolet interface interference effect. At the same time, this achieves a significant reduction in the reflectivity of the solar cell 100 in the visible light band and a significant improvement in the cutoff efficiency in the ultraviolet band. This results in good utilization of visible light and good cutoff of ultraviolet light for the solar cell 100. Furthermore, through the optical refractive index matching design of the two layers, it also compensates for the current loss caused by the ultraviolet absorption layer 3 blocking ultraviolet light, ensuring good power of the battery module.

[0059] Currently, the refractive indices of various materials used in battery modules and solar cells are shown in Table 1 below. The "refractive index" value referred to in this invention was measured under a light source with a wavelength of 632 nanometers.

[0060] Table 1 As can be seen from Table 1, there is a gap in the range of n=2.1-3.85. The refractive index of the ultraviolet absorption layer can fall in the range of 2.2-3.4. At the same time, matching the antireflection layer 4, whose refractive index is more than 0.2 lower than that of the ultraviolet absorption layer 3, can enhance the antireflection effect, thereby achieving a technical effect with advantages in power compared to the UV cut-off film and light transfer film at the battery module end.

[0061] In this embodiment of the invention, the silicon substrate 1 can specifically be an N-type silicon wafer.

[0062] In this embodiment of the invention, the passivation layer 2 can be a single-layer structure or a stacked structure consisting of two or more layers.

[0063] As an embodiment of the present invention, the passivation layer 2 includes a stack of one or at least two of the following: a silicon oxide layer, an aluminum oxide layer, a silicon oxynitride layer, a silicon nitride layer, and a hafnium oxide layer.

[0064] In this embodiment, the passivation layer 2 can be one of silicon oxide layer, aluminum oxide layer, silicon oxynitride layer, silicon nitride layer, and hafnium oxide layer, or it can be a stack of at least two of silicon oxide layer, aluminum oxide layer, silicon oxynitride layer, silicon nitride layer, and hafnium oxide layer.

[0065] While using UV-absorbing materials such as TiO2 to provide dual UV protection (UV cutoff and H-resistance) and reduce reflection loss to improve module power is feasible, it's insufficient for their application in battery cells. Two issues need to be addressed: field passivation and H-passivation on the silicon substrate surface. If the UV-absorbing layer is directly applied between SiNx and the silicon substrate, severe defects such as insufficient field passivation and H-passivation lead to performance failure.

[0066] Therefore, in this embodiment of the invention, a passivation layer 2 needs to be inserted between the silicon substrate 1 and the ultraviolet absorption layer 3 to serve as a dual-functional layer for field-effect passivation and hydrogen supply / hydrogen diffusion regulation. The passivation layer 2 specifically includes the following functions: Providing field-effect passivation: Passivation layer 2 preferably has a high fixed charge density (such as aluminum oxide AlO). x It has a negative fixed charge, and the fixed charge density Qf can reach 10¹²~10¹³cm. - ²) or a dielectric layer with appropriate band shift (such as AlO) x SiO x SiON, SiOx / AlO x Layering, etc., forms band bending at the silicon interface, repelling minority carriers (electrons / holes), reducing the surface recombination rate, and compensating for the lack of field passivation in titanium oxide itself.

[0067] Providing a hydrogen passivation source and regulating hydrogen transport: Passivation layer 2 (especially hydrogen-rich AlO2 prepared by PECVD) x SiN x SiO x Or AlO deposited by ALD x (Followed by hydrogenation annealing) it has a high hydrogen content (1~10 at%), and can release hydrogen atoms under annealing or light irradiation conditions to replenish Si / SiO through interfacial diffusion. x The dangling bonds at the interface are passivated; at the same time, the passivation layer 2 can avoid the "hydrogen blocking effect" caused by the low hydrogen solid solubility and low hydrogen diffusion coefficient of the ultraviolet absorption layer 3, so that hydrogen can escape from the upper anti-reflection layer (such as SiN). x (or diffuse downwards to the surface of silicon substrate 1.)

[0068] Interface state density reduction and chemical passivation: Passivation layer 2 (such as AlO deposited by ALD) x / SiO x Ultrathin tunneling layers can smooth silicon surfaces at the atomic scale, reducing dangling bonds and interface state density (interface state density can be reduced to 10¹). 0 ~10¹¹cm - ²eV - (¹ magnitude), decoupled from the cutoff function of the ultraviolet absorption layer 3, the passivation layer 2 achieves passivation and the ultraviolet absorption layer 3 achieves ultraviolet cutoff in a layered synergistic design.

[0069] Stress buffering: The passivation layer 2 simultaneously buffers the thermal expansion coefficient and lattice mismatch stress between the ultraviolet absorption layer 3 and the silicon substrate 1, suppressing film cracking and interface defect formation.

[0070] Among them, the silicon oxide layer and the silicon substrate 1 can form the lowest defect state, but the field passivation is lacking and the H content is insufficient. The aluminum oxide film layer or the silicon nitride layer has better effects on H content and field passivation. Therefore, the passivation layer 2 is preferably a stacked structure of silicon oxide layer and aluminum oxide film layer or silicon nitride layer. The bottom layer is formed by the silicon oxide layer and the silicon substrate 1 to reduce the defect density, while the top layer covers the aluminum oxide film layer or silicon nitride layer to play the role of H source supply and field passivation.

[0071] Furthermore, since the refractive index of the passivation layer 2 material is much smaller than that of the ultraviolet absorption layer 3, but the passivation layer 2 is inserted between the silicon substrate 1 and the ultraviolet absorption layer 3, it inevitably causes a loss in antireflection. Taking aluminum oxide as an example, the antireflection loss values ​​for passivation layers 2 with different thicknesses are measured as follows: Figure 6 As shown, from Figure 6 It can be seen that when the thickness of passivation layer 2 is <4nm, there is no optical impact. When the thickness of passivation layer 2 is <10nm, the optical power loss of the component can be controlled within <1.5W. Considering the balance between passivation effect and optical effect, the thickness of passivation layer 2 should be controlled between 2~10nm. If passivation layer 2 is too thin, the passivation effect will be poor. If passivation layer 2 is too thick, the optical loss will be too large. In addition, if passivation layer 2 is too thick, it will also easily cause bubble problems, which will lead to the destruction of the interface passivation structure.

[0072] Please refer to the reference. Figure 3 In a preferred embodiment of the present invention, the passivation layer 2 includes a first sub-passivation layer 21 and a second sub-passivation layer 22 stacked on the first sub-passivation layer 21, wherein the second sub-passivation layer 22 is located between the first sub-passivation layer 21 and the ultraviolet absorption layer 3.

[0073] In this embodiment, the passivation layer 2 is a stacked structure composed of a first sub-passivation layer 21 and a second sub-passivation layer 22. Thus, by using the first sub-passivation layer 21 to contact the silicon substrate 1, the defect density on the surface of the silicon substrate 1 can be reduced. The second sub-passivation layer 22 can provide a hydrogen source and perform field passivation. Therefore, the combination of the first sub-passivation layer 21 and the second sub-passivation layer 22 can better achieve the passivation effect of the passivation layer 2. Preferably, the thickness of the second sub-passivation layer 22 is greater than the thickness of the first sub-passivation layer 21. Using the thinner first sub-passivation layer 21 to contact the silicon substrate 1 can better reduce the defect density on the surface of the silicon substrate 1, while using the thicker second sub-passivation layer 22 can better perform the functions of hydrogen source supply and field passivation. For example, the ratio of the thickness of the second sub-passivation layer 22 to the thickness of the first sub-passivation layer 21 can be 1.2 to 10.

[0074] In one embodiment of the present invention, the first sub-passivation layer 21 is a silicon oxide layer, and the second sub-passivation layer 22 is at least one of an aluminum oxide layer, a silicon nitride layer, and a silicon oxynitride layer. Thus, using a silicon oxide layer as the first sub-passivation layer 21 allows for better contact between the silicon oxide layer and the silicon substrate 1, thereby reducing the defect density on the surface of the silicon substrate 1. Using at least one of an aluminum oxide layer, a silicon nitride layer, and a silicon oxynitride layer as the second sub-passivation layer 22 better facilitates hydrogen source supply and field passivation, achieving a better passivation effect for the passivation layer 2.

[0075] As an embodiment of the present invention, the thickness of the first sub-passivation layer 21 is 0.1~2 nanometers, and the thickness of the second sub-passivation layer 22 is 0.5~8 nanometers.

[0076] In this embodiment, the thickness of the first sub-passivation layer 21 is controlled to be 0.1~2 nanometers, and the thickness of the second sub-passivation layer 22 is controlled to be 0.5~8 nanometers. This allows for a lower defect density between the first sub-passivation layer 21 and the silicon substrate 1, while ensuring a good hydrogen source supply and field passivation effect for the second sub-passivation layer 22, thus achieving a better passivation effect for the passivation layer 2. For example, the thickness of the first sub-passivation layer 21 can be any value among 0.1 nanometers, 0.3 nanometers, 0.5 nanometers, 0.7 nanometers, 0.8 nanometers, 0.9 nanometers, 1.0 nanometers, 1.1 nanometers, 1.3 nanometers, 1.6 nanometers, 1.8 nanometers, and 2.0 nanometers. The thickness of the second sub-passivation layer 22 can be any value among 0.5 nm, 0.6 nm, 0.8 nm, 1 nm, 1.2 nm, 1.5 nm, 1.9 nm, 2 nm, 2.2 nm, 2.5 nm, 2.8 nm, 3 nm, 3.5 nm, 3.8 nm, 4 nm, 4.6 nm, 5 nm, 5.5 nm, 6 nm, 6.3 nm, 7 nm, 7.6 nm, and 8 nm.

[0077] In a preferred embodiment, the passivation layer 2 includes a first sub-passivation layer 21 and a second sub-passivation layer 22, wherein the first sub-passivation layer 21 may be a silicon oxide layer (SiO2). x The first sub-passivation layer 21 has a thickness of 0.1~2 nanometers and serves as a tunneling layer; the second sub-passivation layer 22 can be an aluminum oxide layer (AlO). x The second sub-passivation layer 22 has a thickness of 0.5~8 nanometers and can serve as a field passivation and hydrogen source layer. Passivation layer 2 can also be made of SiO2. x SiON, hydrogen-rich SiN x AlO x The single-layer or composite layer consists of one or more of the following, preferably with a hydrogen content of 1 at% to 10 at% and a fixed charge density absolute value ≥ 5 × 10¹¹ cm⁻¹. - ², interfacial state density Dit ≤ 5 × 10¹¹ cm⁻¹ - ²eV - ¹, so that the surface of the silicon substrate 1 can still maintain efficient passivation and long-term UV resistance while ensuring the existence of the ultraviolet absorption layer 3.

[0078] As an embodiment of the present invention, the thickness D1 of the passivation layer 2 is 2~10 nanometers.

[0079] In this embodiment, the thickness D1 of the passivation layer 2 is the total thickness of all layers in the passivation layer 2. The thickness of the passivation layer 2 is controlled within 2-10 nanometers to avoid poor passivation effect due to an excessively thin passivation layer 2, and to avoid excessive optical loss due to an excessively thick passivation layer 2. Furthermore, an excessively thick passivation layer 2 is prone to bubble problems that could damage the interface passivation structure. Specifically, the thickness D1 of the passivation layer 2 is the average thickness of the passivation layer 2. Specifically, 10 points can be selected at equal intervals on the passivation layer 2, and the thickness of the passivation layer 2 at each of these 10 points can be measured. The average thickness of the passivation layer 2 at these 10 points can then be calculated as the average thickness D1 of the passivation layer 2.

[0080] For example, the thickness D1 of the passivation layer 2 can be any value among 2 nm, 2.5 nm, 3 nm, 3.2 nm, 4 nm, 4.5 nm, 6 nm, 6.6 nm, 7 nm, 7.8 nm, 8 nm, 8.5 nm, 9 nm, 9.2 nm, and 10 nm.

[0081] Among them, based on the passivation layer 2 having a thickness of 5 nm, and using anatase titanium oxide as the main component of the ultraviolet absorption layer 3, optical matching studies were conducted. The power loss and UV attenuation of the components under ultraviolet absorption layer 3 with different thicknesses are shown in Table 2. Table 2 As can be seen from Table 2, the thickness of the ultraviolet absorption layer 3 needs to be >10nm to achieve an effective anti-UV attenuation effect, while the thickness of the ultraviolet absorption layer 3 needs to be <70nm to keep the power loss less than one level (5W). Therefore, the preferred thickness of the ultraviolet absorption layer 3 is 10~70nm.

[0082] Furthermore, if the ultraviolet absorption layer 3 can achieve a low H content, the effect of H shock can be mitigated. Therefore, the H content of the passivation layer 2 and the antireflection layer 4 is >1E21 / cm. 3 In this case, the H content of the ultraviolet absorption layer 3 is more than 30% lower than that of the passivation layer 2 or the antireflection layer 4, which can play an effective buffering role. Therefore, by selecting a material with lower H solid solubility as the ultraviolet absorption layer 3, a low-H content ultraviolet absorption layer 3 can be formed after sintering and other activation passivation processes.

[0083] Furthermore, due to the low hydrogen content of the ultraviolet absorption layer 3, it is difficult to achieve the ideal H passivation effect through existing chain sintering technology. It requires a longer sintering time and sealing relief, which is due to the lack of chain sintering activation method. Therefore, the preferred sintering method is closed furnace tube sintering, which requires a temperature greater than 700°C and a sintering time greater than 3 minutes to provide the kinetic process required for H passivation activation. However, the peak temperature needs to be less than 850°C to avoid excessive H leakage, which would make the sample H-poor and reduce the H passivation effect.

[0084] In this embodiment of the invention, the refractive index of the ultraviolet absorption layer 3 can be any value from 2.2 to 3.4, and the refractive index of the antireflection layer 4 can be any value from 1.5 to 2.2, as long as the difference between the refractive index of the ultraviolet absorption layer 3 and the refractive index of the antireflection layer 4 is greater than or equal to 0.2. For example, the refractive index of the ultraviolet absorption layer 3 can be 2.2, and the refractive index of the antireflection layer 4 can be 1.5; for example, the refractive index of the ultraviolet absorption layer 3 can be 3.4, and the refractive index of the antireflection layer 4 can be 2.2; for another example, the refractive index of the ultraviolet absorption layer 3 can be 3.2, and the refractive index of the antireflection layer 4 can be 2.5; for yet another example, the refractive index of the ultraviolet absorption layer 3 can be 2.8, and the refractive index of the antireflection layer 4 can be 2.0; for yet another example, the refractive index of the ultraviolet absorption layer 3 can be 2.3, and the refractive index of the antireflection layer 4 can be 2.1.

[0085] Both the ultraviolet absorption layer 3 and the antireflection layer 4 can be single-layer structures or stacked structures of two or more layers. When the ultraviolet absorption layer 3 is a single-layer structure, its refractive index is 2.2~3.4. When the ultraviolet absorption layer 3 is a stacked structure composed of two or more layers, the refractive index of each layer of the ultraviolet absorption layer 3 is 2.2~3.4. Similarly, when the antireflection layer 4 is a single-layer structure, its refractive index is 1.5~2.2. When the antireflection layer 4 is a stacked structure composed of two or more layers, the refractive index of each layer of the antireflection layer 4 is 1.5~2.2.

[0086] As an embodiment of the present invention, the difference between the refractive index of the ultraviolet absorption layer 3 and the refractive index of the antireflection layer 4 is greater than or equal to 0.5.

[0087] In this embodiment, the difference between the refractive index of the ultraviolet absorption layer 3 and the refractive index of the antireflection layer 4 is greater than or equal to 0.5. Further increasing this difference facilitates a significant reduction in the reflectivity of the ultraviolet absorption layer 3 in the visible light band and a significant improvement in its cutoff efficiency in the ultraviolet band. Further, the difference between the refractive index of the ultraviolet absorption layer 3 and the refractive index of the antireflection layer 4 is greater than or equal to 0.6. Further, the difference between the refractive index of the ultraviolet absorption layer 3 and the refractive index of the antireflection layer 4 is greater than or equal to 0.8. Further, the difference between the refractive index of the ultraviolet absorption layer 3 and the refractive index of the antireflection layer 4 is greater than or equal to 1.

[0088] As an embodiment of the present invention, the thickness D2 of the ultraviolet absorption layer 3 is 10~70 nanometers.

[0089] In this embodiment, the thickness D2 of the ultraviolet absorption layer 3 is controlled to be 10-70 nanometers. This avoids the ultraviolet absorption layer 3 being too thin, thus achieving effective resistance to ultraviolet light-induced degradation, and also avoids the ultraviolet absorption layer 3 being too thick, which would affect visible light transmission and ensure low battery power loss. Specifically, the thickness D2 of the ultraviolet absorption layer 3 is the average thickness of the ultraviolet absorption layer 3. Specifically, 10 points can be selected at equal intervals on the ultraviolet absorption layer 3, and the thickness of the ultraviolet absorption layer 3 at each of these 10 points can be measured. The average thickness D2 of the ultraviolet absorption layer 3 at these 10 points can then be calculated.

[0090] For example, the thickness D2 of the ultraviolet absorption layer 3 can be any value among 10 nm, 11 nm, 12 nm, 14 nm, 15 nm, 20 nm, 26 nm, 30 nm, 40 nm, 50 nm, 60 nm, and 70 nm.

[0091] As an embodiment of the present invention, the extinction coefficient of the ultraviolet absorption layer 3 corresponding to light with a wavelength of 390~780 nm is less than 0.1, and the extinction coefficient of the ultraviolet absorption layer 3 corresponding to ultraviolet light with a wavelength of less than or equal to 320 nm is greater than 0.1.

[0092] Experiments have verified that light with wavelengths greater than 390 nm has almost no impact on battery efficiency degradation, while light with a wavelength of 320 nm has a significant effect on battery efficiency degradation. Therefore, by controlling the extinction coefficient of the ultraviolet absorption layer 3 for light with wavelengths of 390-780 nm to be less than 0.1, the absorption rate of the ultraviolet absorption layer 3 for light with wavelengths of 390-780 nm is kept low, making it easier for light with wavelengths of 390-780 nm to enter the silicon substrate 1, ensuring good utilization of visible light by the solar cell 100, and improving the battery power generation efficiency. Simultaneously, by controlling the extinction coefficient of ultraviolet light with wavelengths less than or equal to 320 nm corresponding to the ultraviolet absorption layer 3 to be greater than 0.1, the absorption rate of ultraviolet light with wavelengths less than or equal to 320 nm corresponding to the ultraviolet absorption layer 3 is made high, thus achieving good ultraviolet light absorption performance of the ultraviolet absorption layer 3. Therefore, the ultraviolet absorption layer 3 can achieve good transmittance of visible light with wavelengths of 390~780 nm and good absorption performance of ultraviolet light with wavelengths less than or equal to 320 nm, thereby balancing the utilization of visible light and the cutoff of ultraviolet light by the ultraviolet absorption layer 3.

[0093] Specifically, the contributions of different wavelengths of UV light to the UV attenuation and power of the module are shown in Table 3, and the curves showing the contributions of different wavelengths of UV light to the UV attenuation and power of the module are shown in Figure 3. Figure 7 As shown.

[0094] Table 3 It can be seen that light with a wavelength >390nm has almost no effect on the UV decay of the module, while light with a wavelength of around 350nm reaches the peak of the UV decay of the module. The sensitivity of wavelength to power increases sharply with the increase of wavelength. Photons in the 390~400nm band affect the module power by 3.1W, while light below 320nm has less sensitivity to the module power, but has already had a significant impact on the module decay.

[0095] Therefore, the absorption coefficient (k value) of the ultraviolet absorption layer 3 needs to exhibit certain characteristics: the k value of the material of the ultraviolet absorption layer 3 for light with wavelengths ≥390nm should be sufficiently small, while the k value of the material of the ultraviolet absorption layer 3 for light with wavelengths ≤320nm should be sufficiently high.

[0096] Table 4 shows the k-values, reflection and absorption ratios of the ultraviolet absorption layer 3 under various wavelengths of sunlight. Table 4 It can be seen that a k-value of 0.1 is a crucial point. When the k-value of the ultraviolet absorption layer 3 exceeds 0.1, it will achieve excellent absorption. Therefore, at a wavelength of 320 nm, the k-value of the ultraviolet absorption layer 3 should be >0.1; at a wavelength of 390 nm, the k-value should be <0.1; further, at a wavelength of 390 nm, the k-value should be <0.01; further, at a wavelength of 390 nm, the k-value should be <0.001; further, at a wavelength of 390 nm, the k-value should be <0.0001. In this case, the ultraviolet absorption layer 3 will have better optical performance, allowing visible light to be fully utilized by the silicon substrate 1. Therefore, by controlling the extinction coefficient of the ultraviolet absorption layer 3 for wavelengths of 390~780 nm to be less than 0.1, and the extinction coefficient of the ultraviolet absorption layer 3 for ultraviolet light with wavelengths less than or equal to 320 nm to be greater than 0.1, the solar cell 100 can effectively utilize visible light while effectively blocking ultraviolet light.

[0097] In this embodiment, the extinction coefficient of the ultraviolet absorption layer 3 for light with wavelengths of 390-780 nm is further less than 0.05. Furthermore, the extinction coefficient of the ultraviolet absorption layer 3 for light with wavelengths of 390-780 nm is less than 0.01. Furthermore, the extinction coefficient of the ultraviolet absorption layer 3 for light with wavelengths of 390-780 nm is less than 0.005. Furthermore, the extinction coefficient of the ultraviolet absorption layer 3 for light with wavelengths of 390-780 nm is less than 0.001.

[0098] In this embodiment, further, the extinction coefficient of the ultraviolet absorption layer 3 for ultraviolet light with a wavelength less than or equal to 320 nm is greater than 0.15. Further, the extinction coefficient of the ultraviolet absorption layer 3 for ultraviolet light with a wavelength less than or equal to 320 nm is greater than 0.2. Further, the extinction coefficient of the ultraviolet absorption layer 3 for ultraviolet light with a wavelength less than or equal to 320 nm is greater than 0.3. Further, the extinction coefficient of the ultraviolet absorption layer 3 for ultraviolet light with a wavelength less than or equal to 320 nm is greater than 0.5.

[0099] As an embodiment of the present invention, the ultraviolet absorption layer 3 comprises a metal oxide with a band gap of 2.8 to 4.0 eV.

[0100] In this embodiment, the ultraviolet absorption layer 3 is made of metal oxide. The band gap of the metal oxide in the ultraviolet absorption layer 3 is 2.8~4.0 eV to control the absorption edge of the material. Too low a band gap will lead to excessive absorption of non-UV harmful photons, causing unnecessary power loss. Too high a band gap will result in the failure to absorb important UV harmful photons, failing to achieve the ideal UV protection effect. Thus, the metal oxide has good absorption performance for ultraviolet light, enabling the ultraviolet absorption layer 3 to achieve good resistance to ultraviolet light-induced degradation of the solar cell 100. In this embodiment, due to the presence of the metal oxide in the ultraviolet absorption layer 3, for double-sided contact solar cells, the first metal electrode 81 simultaneously passes through the antireflection layer 4, the ultraviolet absorption layer 3, the passivation layer 2, and is electrically connected to the first doped layer 5. The contact between the metal oxide and the first metal electrode 81 is beneficial to increase the bonding force of the first metal electrode 81.

[0101] The band gap of the metal oxide is determined by the specific material. For example, when the metal oxide is titanium oxide, the band gap is 3.02~3.31; when the metal oxide is zinc oxide, the band gap is 3.30~3.37; and when the metal oxide is tin oxide, the band gap is 3.6~4.0.

[0102] As an embodiment of the present invention, the metal oxide includes one or a combination of at least two of titanium oxide, zinc oxide, hafnium oxide, zirconium oxide, yttrium oxide, scandium oxide, magnesium oxide, and tin oxide.

[0103] In this embodiment, the metal oxide can be one of titanium oxide, zinc oxide, hafnium oxide, zirconium oxide, yttrium oxide, scandium oxide, magnesium oxide, and tin oxide, or a combination of at least two of titanium oxide, zinc oxide, hafnium oxide, zirconium oxide, yttrium oxide, scandium oxide, magnesium oxide, and tin oxide. Preferably, the metal oxide includes titanium oxide, because titanium oxide has good ultraviolet light absorption properties and is easy to process and prepare the ultraviolet absorption layer 3.

[0104] The bandgap, absorption edge, and refractive index of different metal oxide materials are shown in Table 5 below. The refractive index values ​​were measured under a light source with a wavelength of 632 nanometers.

[0105] Table 5 Therefore, based on a comprehensive evaluation of refractive index, band gap, and extinction coefficient, the preferred metal oxides include one or at least two combinations of titanium oxide, zinc oxide, hafnium oxide, zirconium oxide, yttrium oxide, scandium oxide, magnesium oxide, and tin oxide.

[0106] As an embodiment of the present invention, the metal oxide includes titanium oxide, which comprises anatase phase.

[0107] In this embodiment, titanium oxide typically exists in four phases: anatase, rutile, brookite, and amorphous. Due to their poor thermal stability, brookite and amorphous phases are unsuitable as the main components of the final ultraviolet (UV) absorption layer, but can be used as secondary components to modulate the optical properties of titanium oxide. Compared to rutile, anatase exhibits significant absorption even for photons at wavelengths of 390-500 nm that do not trigger UV attenuation, leading to excessive optical loss. Therefore, anatase-phase titanium oxide is preferred as the composition of the UV absorption layer 3, as it is more conducive to improving the UV absorption performance of the UV absorption layer 3. Additionally, cerium or strontium can be doped into the UV absorption layer 3 to adjust its irradiation effect.

[0108] As an embodiment of the present invention, the metal oxide includes titanium oxide, which comprises anatase phase, rutile phase, and brookite phase, and the proportion of anatase phase is greater than the proportion of rutile phase or brookite phase.

[0109] In this embodiment, when the ultraviolet absorption layer 3 includes titanium oxide, and the titanium oxide contains anatase phase, rutile phase, and brookite phase, the mass proportion of the anatase phase in the titanium oxide is greater than the mass proportion of the rutile phase or brookite phase in the titanium oxide. By controlling the proportion of the anatase phase in the titanium oxide to be greater than the proportion of the rutile phase or brookite phase in the titanium oxide, the proportion of the anatase phase in the titanium oxide is maximized, which is more conducive to improving the ultraviolet light absorption performance of the ultraviolet absorption layer 3.

[0110] Among them, the extinction coefficient curves and n-value curves of titanium oxide materials under four different phases—anatase, rutile, brookite, and amorphous—show significant differences, which have a significant impact on UV resistance and optical performance. While the brookite and amorphous phases are unsuitable as the main components of the final UV-absorbing layer due to their poor thermal stability, they can be used as secondary components to regulate the optical properties of the titanium oxide layer. The relationship between the refractive index (n) and extinction coefficient (k) of titanium oxide at corresponding wavelengths for different crystal phases is shown in the figure below. Figure 8 As shown, compared to rutile, the rutile phase exhibits significant absorption of photons that do not trigger UV attenuation in the 390-500 nm range, leading to excessive optical loss. Therefore, anatase titanium oxide is preferred as the main light-absorbing layer. Furthermore, the irradiation effect of adjusting the optical performance of the UV absorption layer 3 can be achieved by adding porous structures, cerium doping, strontium doping, etc.

[0111] As an embodiment of the present invention, the ratio of oxygen content to metal content in the ultraviolet absorption layer 3 is greater than 2.

[0112] In this embodiment, the ratio of oxygen content to metal content in the ultraviolet absorption layer 3 can be understood as follows: if the ultraviolet absorption layer 3 is a single type of metal oxide, then the ratio of oxygen content to metal content in that metal oxide; if the ultraviolet absorption layer 3 is composed of multiple metal oxides, then the ratio of oxygen content to total metal content in all metal oxides. For example, if the metal oxide in the ultraviolet absorption layer 3 is titanium oxide, then the ratio of oxygen content to metal content is the ratio of oxygen content to titanium content. As another example, if the metal oxide in the ultraviolet absorption layer 3 is titanium oxide and zinc oxide, then the ratio of oxygen content to metal content is the ratio of oxygen content to the total content of titanium and zinc. Yet another example, if the metal oxide in the ultraviolet absorption layer 3 is titanium oxide, zinc oxide, and tin oxide, then the ratio of oxygen content to metal content is the ratio of oxygen content to the total content of titanium, zinc, and tin.

[0113] In this embodiment, the ratio of oxygen content to metal content in the metal oxide in the ultraviolet absorption layer 3 is controlled to be greater than 2, so that oxygen vacancies in the crystal lattice are filled in large quantities, and metal vacancies or interstitial oxygen become the dominant defects. This can better suppress the drift of the cutoff wavelength towards the long wavelength direction, and is more conducive to improving the ultraviolet absorption effect of the ultraviolet absorption layer 3 on ultraviolet light.

[0114] As an embodiment of the present invention, the passivation layer 2 has a thickness of D1, the ultraviolet absorption layer 3 has a thickness of D2, and the ratio of D2 to D1 is greater than or equal to 2.

[0115] In this embodiment, the ratio of D2 to D1 is greater than or equal to 2, making the thickness D2 of the ultraviolet absorption layer 3 much larger than the thickness D1 of the passivation layer 2. This gives the ultraviolet absorption layer 3 a stronger ability to absorb or reflect high-energy ultraviolet photons, significantly reducing the amount of ultraviolet light reaching the underlying passivation layer 2 and silicon substrate 1, thus improving the UV-induced degradation resistance of the solar cell 100. Furthermore, the thinner passivation layer 2 ensures efficient carrier tunneling and field-effect passivation. Therefore, controlling the ratio of D2 to D1 to be greater than or equal to 2 helps to balance the effective UV blocking effect of the ultraviolet absorption layer 3 with the effective passivation effect of the passivation layer 2, ensuring that the thickness of the ultraviolet absorption layer is sufficient to achieve effective cutoff while reducing the optical impact of the passivation layer 2. Furthermore, the thickness of the ultraviolet absorption layer 3 is D2, and the ratio of D2 to D1 can be greater than or equal to 3.

[0116] As an embodiment of the present invention, the thickness of the antireflection layer 4 is D3, and the ratio of D3 to D2 is 0.3 to 3.

[0117] In this embodiment, the ratio of the thickness D3 of the antireflection layer 4 to the thickness D2 of the ultraviolet absorption layer 3 is controlled to be 0.3~3. While ensuring ultraviolet protection and passivation, a specific thickness matching design maximizes the reduction of incident light reflection loss on the battery surface, thereby significantly improving the battery's short-circuit current density and overall photoelectric conversion efficiency. A ratio of D3 to D2 greater than 0.3 ensures that the antireflection layer 4 is not too thin and loses its optical function. A ratio of D3 to D2 less than 3 avoids the antireflection layer 4 being too thick, thus avoiding affecting the ultraviolet cutoff function of the underlying ultraviolet absorption layer 3. This ensures that the antireflection layer 4 improves light absorption without weakening the ultraviolet cutoff performance of the ultraviolet absorption layer 3. Specifically, the thickness D3 of the antireflection layer 4 is the average thickness of the antireflection layer 4. Specifically, 10 points can be selected at equal intervals on the antireflection layer 4, and the thickness of the antireflection layer 4 at each of these 10 points can be measured. The average thickness of the antireflection layer 4 at these 10 points can then be calculated as the thickness D3 of the antireflection layer 4.

[0118] As an embodiment of the present invention, the total thickness of D3 and D2 is less than 150 nanometers.

[0119] In this embodiment, the total thickness of D3 and D2 is controlled to be less than 150 nanometers. This maintains the good optical performance of the antireflective layer 4 and the ultraviolet absorption layer 3 while avoiding optical defects caused by excessive thickness of the two layers. It also prevents increased reflectivity due to excessive thickness, which would degrade the antireflective effect. Furthermore, it avoids excessive internal stress leading to cracking or peeling of the film due to excessive thickness, thereby improving the long-term reliability of the film. Additionally, keeping the total thickness of the antireflective layer 4 and the ultraviolet absorption layer 3 within a reasonable range avoids increased costs and decreased process capability caused by surface stress due to excessive thickness.

[0120] As an embodiment of the present invention, the antireflection layer 4 is at least one of silicon nitride layer and silicon oxynitride layer.

[0121] As an embodiment of the present invention, the thickness D3 of the antireflection layer 4 is 30~100 nanometers.

[0122] In this embodiment, the thickness D3 of the antireflection layer 4 is controlled to be 30~100 nanometers to avoid the antireflection layer 4 being too thin, ensuring that the antireflection layer 4 will not be too thin and lose its optical function, and to avoid the antireflection layer 4 being too thick, so as not to affect the ultraviolet cutoff function of the ultraviolet absorption layer 3 below. In this way, the antireflection layer 4 can improve light absorption without weakening the ultraviolet cutoff performance of the ultraviolet absorption layer 3.

[0123] Please refer to Figure 4As an embodiment of the present invention, a first optical coupling layer 91 is provided between the passivation layer 2 and the ultraviolet absorption layer 3, and the refractive index of the first optical coupling layer 91 is between the refractive index of the passivation layer 2 and the refractive index of the ultraviolet absorption layer 3.

[0124] In this embodiment, a first optical coupling layer 91 is provided between the passivation layer 2 and the ultraviolet absorption layer 3, and the refractive index of the first optical coupling layer 91 is between the refractive index of the passivation layer 2 and the refractive index of the ultraviolet absorption layer 3. After passing through the ultraviolet absorption layer 3, the first optical coupling layer 91, and the passivation layer 2, sunlight enters the silicon substrate 1, avoiding optical abrupt changes between the passivation layer 2 and the ultraviolet absorption layer 3, so that sunlight can be gradually coupled into the silicon substrate 1 with lower loss, thereby effectively increasing the total amount of photogenerated carriers excited.

[0125] As an embodiment of the present invention, a second optical coupling layer 92 is provided between the ultraviolet absorption layer 3 and the antireflection layer 4, and the refractive index of the second optical coupling layer 92 is between the refractive index of the ultraviolet absorption layer 3 and the refractive index of the antireflection layer 4.

[0126] In this embodiment, the ultraviolet absorption layer 3 and the antireflection layer 4 have a second optical coupling layer 92, and the refractive index of the second optical coupling layer 92 is located between the refractive index of the ultraviolet absorption layer 3 and the refractive index of the antireflection layer 4. After passing through the antireflection layer 4 and the second optical coupling layer 92, sunlight enters the ultraviolet absorption layer 3, avoiding optical abrupt changes between the ultraviolet absorption layer 3 and the antireflection layer 4, so that sunlight can gradually couple into the ultraviolet absorption layer 3 with low loss, thereby effectively increasing the total amount of photogenerated carriers excited.

[0127] Please refer to Figure 5 As an embodiment of the present invention, the first surface 11 includes an edge region E and an intermediate region F located inside the edge region E, and the thickness D21 of the ultraviolet absorption layer 3 in the edge region E is greater than the thickness D22 of the ultraviolet absorption layer 3 in the intermediate region F.

[0128] In this embodiment of the invention, the edge region E is specifically a region on the first surface 11 whose vertical distance from the edge of the silicon substrate 1 is less than or equal to 2 mm. The edge region E is specifically a ring-shaped region. The middle region F is the region on the first surface 11 excluding the edge region E. Because the edge region E of the silicon substrate 1 of the solar cell 100 has a high defect state density, the edge region E is more prone to photo-induced degradation and accelerated recombination under high-energy ultraviolet light irradiation. Therefore, in this embodiment, by controlling the thickness D21 of the ultraviolet absorption layer 3 in the edge region E to be greater than the thickness D22 of the ultraviolet absorption layer 3 in the middle region F, the ultraviolet absorption performance of the ultraviolet absorption layer 3 in the edge region E is improved. This allows the ultraviolet absorption layer 3 in the edge region E to effectively block and absorb high-energy ultraviolet photons reaching the edge region E, significantly slowing down Si-H bond breaking and hydrogen escape, and reducing ultraviolet-induced degradation in the edge region E. Moreover, the thickened ultraviolet absorption layer 3 enhances the field-effect passivation and chemical passivation effects of the edge region E, effectively suppressing surface recombination caused by high defect state density in the edge region E, thereby significantly improving the battery's ultraviolet resistance and long-term reliability. At the same time, it can reduce the impact of the ultraviolet absorption layer 3 on the light absorption efficiency of the middle region F.

[0129] In this embodiment, the thickness D21 of the ultraviolet absorption layer 3 in the edge region E is the average thickness of the ultraviolet absorption layer 3 in the edge region E. Specifically, 10 points can be taken at equal intervals in the edge region E, and the thickness of the ultraviolet absorption layer 3 at each of the 10 points can be measured. The average thickness of the ultraviolet absorption layer 3 at these 10 points can then be calculated as the thickness D21 of the ultraviolet absorption layer 3 in the edge region E. Similarly, the thickness D22 of the ultraviolet absorption layer 3 in the middle region F is the average thickness of the ultraviolet absorption layer 3 in the middle region F. Specifically, 10 points can be taken at equal intervals in the middle region F, and the thickness of the ultraviolet absorption layer 3 at each of the 10 points can then be measured. The average thickness of the ultraviolet absorption layer 3 at these 10 points can then be calculated as the thickness D22 of the ultraviolet absorption layer 3 in the middle region F.

[0130] In some embodiments, the ratio of the thickness of the ultraviolet absorption layer 3 in the edge region E to the thickness of the ultraviolet absorption layer 3 in the middle region F can be 1.1 to 3. This is beneficial to better improve the ultraviolet absorption performance of the ultraviolet absorption layer 3 in the edge region E, and to better enhance the field effect passivation and chemical passivation effect of the edge region E.

[0131] As an embodiment of the present invention, the ultraviolet absorption layer 3 includes pores.

[0132] In this embodiment, the ultraviolet absorption layer 3 is provided with a porous structure, which is beneficial to improving the light trapping effect and further enhancing the cutoff effect of the ultraviolet absorption layer 3 on ultraviolet light. The pores in the ultraviolet absorption layer 3 can be cylindrical, conical, spherical, or irregular in shape.

[0133] As an embodiment of the present invention, the first surface 11 includes an edge region E and a middle region F located inside the edge region, and the pore density of the ultraviolet absorption layer 3 in the edge region E is greater than the pore density of the ultraviolet absorption layer 3 in the middle region F.

[0134] In this embodiment, the pore density is specifically the number of pores per unit area. The pore density of the ultraviolet absorption layer 3 in the edge region E is greater than that in the middle region F. That is, for the same area, the number of pores in the ultraviolet absorption layer 3 in the edge region E is greater than the number of pores in the middle region F.

[0135] Because the edge region E of the silicon substrate 1 of the solar cell 100 has a high defect state density, the edge region E is more prone to photo-induced degradation and accelerated recombination under high-energy ultraviolet light irradiation. Therefore, the pore density of the ultraviolet absorption layer 3 in the edge region E is greater than that in the middle region F, which is beneficial to improving the ultraviolet absorption performance of the ultraviolet absorption layer 3 in the edge region E. In some embodiments, the ratio of the pore density of the ultraviolet absorption layer 3 in the edge region E to the pore density in the middle region F can be 1.1 to 3, which is beneficial to further improve the ultraviolet absorption performance of the ultraviolet absorption layer 3 in the edge region E.

[0136] This invention also provides a battery assembly, which includes the solar cell 100 described in the above embodiments. It should be noted that this battery assembly has the same or similar beneficial effects as the solar cell 100 described above, and the related aspects between the two can be referred to each other; to avoid repetition, they will not be repeated here.

[0137] In this embodiment, multiple solar cells 100 in the battery module are connected in series by solder ribbons to form a battery string, thereby realizing the series current collection and output.

[0138] It is understood that in such embodiments, the battery assembly may further include a metal frame, a backsheet, photovoltaic glass, and an encapsulating film. The encapsulating film may be filled between the front and back of the solar cell 100, as well as between the photovoltaic glass and adjacent cells. As a filler, it may be a transparent colloid with good light transmittance and aging resistance. For example, the encapsulating film may be an EVA film or a POE film, and the specific choice can be made according to the actual situation, without limitation.

[0139] Photovoltaic glass can be applied to the encapsulating film on the front side of the solar cell 100. This photovoltaic glass can be ultra-clear glass, possessing high light transmittance, high transparency, and superior physical, mechanical, and optical properties. For example, ultra-clear glass can achieve a light transmittance of over 92%. It can protect the solar cell 100 while minimizing impact on its efficiency. Simultaneously, the encapsulating film bonds the photovoltaic glass and the solar cell 100 together, providing sealing, insulation, and waterproofing / moisture protection for the solar cell 100.

[0140] The backsheet can be attached to the encapsulating film on the back of the solar cell 100. The backsheet provides protection and support for the solar cell 100, offering reliable insulation, water resistance, and aging resistance. Multiple backsheet options are available, typically including tempered glass, acrylic glass, and aluminum alloy TPT composite encapsulating film, etc. The specific choice depends on the specific circumstances and is not limited here. The backsheet, solar cell 100, encapsulating film, and photovoltaic glass can be mounted on a metal frame. The metal frame serves as the main external support structure for the entire battery module, providing stable support and installation. For example, the battery module can be installed at the desired location using the metal frame.

[0141] This invention also provides a photovoltaic system, which includes the battery module described in the above embodiments. It should be noted that this photovoltaic system has the same or similar beneficial effects as the solar cell 100 described above, and the related aspects between the two can be referred to each other; to avoid repetition, they will not be repeated here.

[0142] In this embodiment, the photovoltaic system can be applied in photovoltaic power plants, such as ground-mounted power plants, rooftop power plants, and floating power plants. It can also be applied to equipment or devices that utilize solar energy to generate electricity, such as user solar power supplies, solar streetlights, solar cars, and solar buildings. Of course, it is understood that the application scenarios of the photovoltaic system are not limited to these; that is, the photovoltaic system can be applied in all fields that require solar energy to generate electricity. Taking a photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a combiner box, and an inverter. The photovoltaic array may be an array combination of multiple battery modules; for example, multiple battery modules can form multiple photovoltaic arrays. The photovoltaic array is connected to the combiner box, which can collect the current generated by the photovoltaic array. The collected current flows through the inverter and is converted into AC power required by the mains power grid before being connected to the mains power grid to achieve solar power supply.

[0143] In the description of this specification, references to terms such as "some embodiments," "illustrative embodiments," "examples," "specific examples," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with an embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0144] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A solar cell, characterized in that, include: A silicon substrate, the silicon substrate including a first surface; A passivation layer is provided on the first surface; An ultraviolet absorption layer is disposed on the passivation layer, wherein the refractive index of the ultraviolet absorption layer is 2.2~3.4; and An antireflection layer is disposed on the ultraviolet absorption layer, the refractive index of the antireflection layer is 1.5~2.2, and the difference between the refractive index of the ultraviolet absorption layer and the refractive index of the antireflection layer is greater than or equal to 0.

2.

2. The solar cell according to claim 1, characterized in that, The passivation layer has a thickness of D1, the ultraviolet absorption layer has a thickness of D2, and the ratio of D2 to D1 is greater than or equal to 2.

3. The solar cell according to claim 2, characterized in that, The thickness of the antireflective layer is D3, and the ratio of D3 to D2 is 0.3 to 3.

4. The solar cell according to claim 3, characterized in that, The total thickness of D3 and D2 is less than 150 nanometers.

5. The solar cell according to claim 1, characterized in that, The passivation layer has a thickness of 2 to 10 nanometers.

6. The solar cell according to claim 1, characterized in that, The thickness of the ultraviolet absorption layer is 10~70 nanometers.

7. The solar cell according to claim 1, characterized in that, The thickness of the antireflective layer is 30~100 nanometers.

8. The solar cell according to claim 1, characterized in that, The extinction coefficient of the ultraviolet absorption layer for light with wavelengths of 390~780 nm is less than 0.1, and the extinction coefficient of the ultraviolet absorption layer for ultraviolet light with wavelengths less than or equal to 320 nm is greater than 0.

1.

9. The solar cell according to claim 1, characterized in that, The difference between the refractive index of the ultraviolet absorption layer and the refractive index of the antireflection layer is greater than or equal to 0.

5.

10. The solar cell according to claim 1, characterized in that, The first surface includes an edge region and a middle region located inside the edge region, wherein the thickness of the ultraviolet absorption layer in the edge region is greater than the thickness of the ultraviolet absorption layer in the middle region.

11. The solar cell according to claim 1, characterized in that, The ultraviolet absorption layer includes pores.

12. The solar cell according to claim 11, characterized in that, The first surface includes an edge region and a middle region located inside the edge region, wherein the pore density of the ultraviolet absorption layer in the edge region is greater than the pore density of the ultraviolet absorption layer in the middle region.

13. The solar cell according to claim 1, characterized in that, The ultraviolet absorption layer comprises a metal oxide with a band gap of 2.8 to 4.0 eV.

14. The solar cell according to claim 13, characterized in that, The metal oxide includes one or a combination of at least two of the following: titanium oxide, zinc oxide, hafnium oxide, zirconium oxide, yttrium oxide, scandium oxide, magnesium oxide, and tin oxide.

15. The solar cell according to claim 13 or 14, characterized in that, The metal oxide includes titanium oxide, which comprises anatase phase.

16. The solar cell according to claim 13 or 14, characterized in that, The metal oxide includes titanium oxide, which comprises anatase phase, rutile phase, and brookite phase, and the proportion of the anatase phase is greater than the proportion of the rutile phase or the brookite phase.

17. The solar cell according to claim 13, characterized in that, The ratio of oxygen content to metal content in the ultraviolet absorption layer is greater than 2.

18. The solar cell according to claim 1, characterized in that, The passivation layer comprises one or more of the following: a silicon oxide layer, an aluminum oxide layer, a silicon oxynitride layer, a silicon nitride layer, and a hafnium oxide layer.

19. The solar cell according to claim 1, characterized in that, The passivation layer includes a first sub-passivation layer and a second sub-passivation layer stacked on the first sub-passivation layer, wherein the second sub-passivation layer is located between the first sub-passivation layer and the ultraviolet absorption layer.

20. The solar cell according to claim 19, characterized in that, The first sub-passivation layer is a silicon oxide layer, and the second sub-passivation layer is at least one of an aluminum oxide layer, a silicon nitride layer, and a silicon oxynitride layer.

21. The solar cell according to claim 19, characterized in that, The thickness of the first sub-passivation layer is 0.1~2 nanometers, and the thickness of the second sub-passivation layer is 0.5~8 nanometers.

22. The solar cell according to claim 1, characterized in that, A first optical coupling layer is provided between the passivation layer and the ultraviolet absorption layer, and the refractive index of the first optical coupling layer is between the refractive index of the passivation layer and the refractive index of the ultraviolet absorption layer.

23. The solar cell according to claim 1, characterized in that, A second optical coupling layer is provided between the ultraviolet absorption layer and the antireflection layer, and the refractive index of the second optical coupling layer is between the refractive index of the ultraviolet absorption layer and the refractive index of the antireflection layer.

24. A battery assembly, characterized in that, Includes the solar cell described in any one of claims 1 to 23.

25. A photovoltaic system, characterized in that, Includes the battery assembly as described in claim 24.