A solar cell, a battery module and a photovoltaic system

By incorporating a titanium dioxide ultraviolet absorption layer and a refractive index gradient-varying antireflection layer into solar cells, the problem of photoelectric conversion efficiency degradation caused by ultraviolet light is solved, thereby improving the optical performance and photoelectric conversion efficiency of solar cells and reducing production costs.

CN123124512APending Publication Date: 2026-11-17ZHUHAI FUSHAN AIKO SOLAR ENERGY TECH CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611265491.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The photoelectric conversion efficiency of existing solar cells degrades due to ultraviolet light during long-term outdoor operation, mainly because of poor optical matching between the antireflection layer, the ultraviolet absorption layer, and the encapsulating film of the battery module, which affects the optical performance of the solar cells.

Method used

A passivation layer, an ultraviolet absorption layer, and an antireflection layer are disposed on a silicon substrate of a solar cell. The ultraviolet absorption layer uses titanium oxide, and the antireflection layer is composed of SiNxOy and SiNmOn layers. By controlling the composition ratio and thickness of each layer, a gradual change in refractive index is achieved to match the refractive index of the ultraviolet absorption layer and the encapsulating film, thereby absorbing ultraviolet light and reducing visible light reflection.

Benefits of technology

It effectively blocks ultraviolet rays from entering the battery, reduces the probability of Si-H bond damage, improves the photoelectric conversion efficiency and solar energy utilization of solar cells, and simplifies the production process and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124512A_ABST
    Figure CN123124512A_ABST
Patent Text Reader

Abstract

This invention relates to the field of photovoltaic technology and provides a solar cell, a cell module, and a photovoltaic system. The solar cell includes: a silicon substrate, the silicon substrate including a first surface; a passivation layer disposed on the first surface; an ultraviolet absorbing layer disposed on the passivation layer, the ultraviolet absorbing layer being made of titanium oxide; and an antireflection layer disposed on the ultraviolet absorbing layer, the antireflection layer including stacked SiN... x O y Layers and SiN m O n Layer, SiN x O y Compared to SiN m O n The layer is closer to the ultraviolet absorption layer, SiN x O y The layer satisfies: x / (x+y)>50%; SiN m O n The layer satisfies the following conditions: m / (m+n) < 50%, and the difference between x / (x+y) and m / (m+n) is d, where d ≥ 1%. The solar cell of this invention utilizes an ultraviolet absorption layer to block ultraviolet light, while simultaneously optimizing the design of the antireflection layer, which can improve the optical performance of the solar cell and thus enhance its photoelectric conversion efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photovoltaic technology, and in particular to a solar cell, a battery module, and a photovoltaic system. Background Technology

[0002] During long-term outdoor operation, the battery module is exposed to ultraviolet (UV) light from the sun. The high-energy UV light in the sun can break the Si-H bonds of the solar cell, resulting in a decrease in the photoelectric conversion efficiency of the solar cell.

[0003] In related technologies, in order to reduce the efficiency degradation of solar cells caused by ultraviolet light, an ultraviolet absorption layer is usually set on the surface of the solar cell, and a single-layer anti-reflection layer is set on the ultraviolet absorption layer. Sunlight passes through the encapsulation film of the battery module and enters the solar cell. The solar cell uses the ultraviolet absorption layer to absorb the ultraviolet light in the sunlight. However, it is difficult to achieve good optical matching between the single-layer anti-reflection layer of the solar cell and the ultraviolet absorption layer and the encapsulation film of the battery module, resulting in poor optical performance of the solar cell, thereby affecting the photoelectric conversion efficiency of the solar cell. Summary of the Invention

[0004] This invention provides a solar cell that aims to solve the problem that existing solar cells have poor optical performance due to the difficulty in achieving good optical matching between the antireflection layer and the ultraviolet absorption layer and the encapsulation film of the battery module, which affects the photoelectric conversion efficiency of the solar cell.

[0005] This invention is implemented by providing a solar cell, comprising: A silicon substrate, the silicon substrate including a first surface; A passivation layer is provided on the first surface; An ultraviolet absorption layer is disposed on the passivation layer, wherein the material of the ultraviolet absorption layer includes titanium oxide; and An antireflection layer disposed on the ultraviolet absorption layer, the antireflection layer comprising stacked SiN x O y Layers and SiN m O n Layer, the SiN x O y Compared to the SiN layer m O n The layer is closer to the ultraviolet absorption layer, the SiN x O y The layer satisfies: x / (x+y)>50%; the SiN m O n The layer satisfies: m / (m+n) < 50%, and the difference between x / (x+y) and m / (m+n) is d, where d ≥ 1%.

[0006] Preferably, x / (x+y)≥55%.

[0007] Preferably, x / (x+y)≥60%.

[0008] Preferably, m / (m+n)≤45%.

[0009] Preferably, m / (m+n)≤40%.

[0010] Preferably, d ≥ 5%.

[0011] Preferably, d ≥ 10%.

[0012] Preferably, the general chemical formula of the titanium oxide is TiO2. b The value of b ranges from 1.8 to 2.2.

[0013] Preferably, the SiN m O n The thickness of the layer is greater than that of the SiN x O y The thickness of the layer.

[0014] Preferably, the titanium oxide comprises anatase phase, and the mass fraction of the anatase phase is greater than or equal to 60%.

[0015] Preferably, the titanium oxide comprises anatase phase, and the mass fraction of the anatase phase is greater than or equal to 90%.

[0016] Preferably, the titanium oxide comprises anatase phase, and the mass fraction of the anatase phase is less than or equal to 98%.

[0017] Preferably, the titanium oxide further includes at least one of rutile phase, brookite phase, and amorphous phase.

[0018] Preferably, the sum of the mass fractions of the rutile phase, the brookite phase, and the amorphous phase is 2% to 40%.

[0019] Preferably, the thickness of the passivation layer is 2 to 10 nanometers.

[0020] Preferably, the thickness of the ultraviolet absorption layer is 10~70 nanometers.

[0021] Preferably, the thickness of the antireflective layer is 30~100 nanometers.

[0022] Preferably, the extinction coefficient of the ultraviolet absorption layer for light with a wavelength of 390~780 nm is less than 0.1, and the extinction coefficient of the ultraviolet absorption layer for ultraviolet light with a wavelength of less than or equal to 320 nm is greater than 0.1.

[0023] Preferably, the passivation layer comprises one or at least two of the following: a silicon oxide layer, an aluminum oxide layer, a silicon oxynitride layer, a silicon nitride layer, and a hafnium oxide layer.

[0024] Preferably, the passivation layer includes a first sub-passivation layer and a second sub-passivation layer stacked on the first sub-passivation layer, wherein the second sub-passivation layer is located between the first sub-passivation layer and the ultraviolet absorption layer.

[0025] Preferably, the first sub-passivation layer is a silicon oxide layer, and the second sub-passivation layer is at least one of an aluminum oxide layer, a silicon nitride layer, and a silicon oxynitride layer.

[0026] Preferably, the thickness of the first sub-passivation layer is 0.1~2 nanometers, and the thickness of the second sub-passivation layer is 0.5~8 nanometers.

[0027] The present invention also provides a battery assembly including the solar cell described above.

[0028] The present invention also provides a photovoltaic system including the above-described battery module.

[0029] The present invention provides a solar cell by sequentially depositing a passivation layer, an ultraviolet absorption layer, and an antireflection layer on the first surface of a silicon substrate. In this way, an ultraviolet absorption layer is directly added between the passivation layer and the antireflection layer, and the ultraviolet absorption layer is integrated into the solar cell. As part of the solar cell, the ultraviolet absorption layer absorbs ultraviolet light passing through the front glass and front encapsulant film of the cell module, which can effectively block ultraviolet light from entering the interior of the solar cell, reduce the probability of ultraviolet light damaging Si-H bonds, and thus significantly alleviate the problem of ultraviolet light-induced degradation of solar cells.

[0030] Meanwhile, the ultraviolet absorption layer of the solar cell provided by the present invention includes titanium oxide as its material, and the antireflection layer is configured to include SiN. x O y Layers and SiN m O n This allows the antireflective layer to be composed of at least two silicon oxynitride layers stacked together, while simultaneously controlling the SiN... x O y The layer satisfies: x / (x+y)>50%; SiN m O n The layer satisfies the following conditions: m / (m+n) < 50%, and the difference between x / (x+y) and m / (m+n) is d, where d ≥ 1%. Under these conditions, SiN x O y Layers and SiN m O n The refractive index of SiN is between that of the ultraviolet absorption layer and the encapsulating film. x O yThe refractive index of the layer is greater than that of SiN m O n The refractive index of the layer allows sunlight to pass through the encapsulating film of the battery module sequentially via SiN. m O n Layer, SiN x O y The layer enters the ultraviolet absorption layer, encapsulating film, SiN m O n Layer, SiN x O y The refractive index of the layers decreases sequentially, and the antireflective layer is made of SiN m O n Layer, SiN x O y The refractive index gradient of the layered structure allows for good optical matching between the antireflection layer, the ultraviolet absorption layer, and the encapsulating film of the battery module. This achieves a highly efficient antireflection effect, which can greatly reduce interface reflection in the main visible light band (especially the 600nm~800nm ​​peak response region), thereby improving the optical performance of the solar cell and enhancing its solar energy utilization rate.

[0031] Moreover, SiN m O n In the layer, m / (m+n) < 50%, making SiN m O n The layer is an oxygen-rich layer, and its refractive index is higher than that of SiN. x O y The refractive index of the layer is lower, SiN m O n Layer as SiN x O y The transition layer between the layer and the encapsulating film of the battery module can reduce the reflection of sunlight when it enters the anti-reflection layer from the encapsulating film, thus achieving a better anti-reflection effect; while SiN x O y In the layer, x / (x+y) > 50%, making SiN x O y The layer is a nitrogen-rich layer, made of nitrogen-rich SiN. x O y Compared to SiN m O n The layer has a higher extinction coefficient in the ultraviolet band, utilizing SiN x O y The SiN layer can effectively absorb a portion of ultraviolet light, reducing the penetration of high-energy ultraviolet photons into the battery and thus mitigating performance degradation caused by ultraviolet light. Therefore, SiN... m O n Layer, SiN x O yThe synergy between the SiN layer and the ultraviolet absorption layer allows for excellent optical matching. This not only enhances the antireflective effect of the antireflective layer, improving the solar energy utilization rate of the solar cell, but also reduces the performance degradation caused by ultraviolet light, thereby increasing the photoelectric conversion efficiency of the solar cell. Furthermore, the SiN layer can be individually controlled. x O y Layers and SiN m O n The ratio of N to O in the SiN layer can be used to control the SiN layer. x O y Layers and SiN m O n The refractive index range of the layer means that the antireflective layer does not require the stacking of film layers of different materials, which can greatly simplify the preparation process of the antireflective layer and help reduce production costs. Attached Figure Description

[0032] Figure 1 A cross-sectional schematic diagram of a solar cell provided in an embodiment of the present invention; Figure 2 A cross-sectional schematic diagram of another solar cell provided in an embodiment of the present invention; Figure 3 A cross-sectional schematic diagram of another solar cell provided in an embodiment of the present invention; Figure 4 A cross-sectional schematic diagram of another solar cell provided in an embodiment of the present invention; Figure 5 A cross-sectional schematic diagram of another solar cell provided in an embodiment of the present invention; Figure 6 A graph showing the relationship between the passivation layer thickness and module power loss in a solar cell, provided as an embodiment of the present invention; Figure 7 A graph showing the relationship between the contribution of different wavelengths of sunlight to the UV attenuation and power contribution of the module; Figure 8 This is a graph showing the relationship between the refractive index and extinction coefficient of titanium oxide at different crystal phases corresponding to different wavelengths.

[0033] Explanation of key symbols: Solar cell 100, silicon substrate 1, first surface 11, second surface 12, passivation layer 2, first sub-passivation layer 21, second sub-passivation layer 22, ultraviolet absorption layer 3, antireflection layer 4, SiN x O y Layer 41, SiN m O n Layer 42, first doped layer 5, second doped layer 6, back passivation antireflection layer 7, first metal electrode 81, second metal electrode 82, edge region E, middle region F, first optical coupling layer 91, second optical coupling layer 92. Detailed Implementation

[0034] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. Examples of embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the invention, and should not be construed as limiting the invention. Furthermore, it should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0035] In the description of this invention, it should be understood that the terms "upper", "lower", "back", "front", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this invention.

[0036] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can include direct contact between the first and second features, or contact between the first and second features through another feature between them. Furthermore, "above," "over," and "on top" of the second feature includes the first feature directly above or diagonally above the second feature, or simply indicates that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature includes the first feature directly below or diagonally below the second feature, or simply indicates that the first feature is at a lower horizontal level than the second feature.

[0037] The following disclosure provides numerous different embodiments or examples for implementing various structures of the invention. To simplify the disclosure, specific examples of components and arrangements are described below. These are merely examples and are not intended to limit the invention. Furthermore, reference numerals and / or letters may be repeated in different examples; such repetition is for simplification and clarity and does not in itself indicate a relationship between the various embodiments and / or arrangements discussed. In addition, examples of various specific processes and materials are provided in this invention, but those skilled in the art will recognize the application of other processes and / or the use of other materials.

[0038] In related technologies, early solar cell modules mostly used non-UV-blocking (high-transmittance) EVA encapsulating films, allowing ultraviolet light to penetrate the film and tempered glass to reach the solar cell surface. This is because traditional p-type aluminum back-field cells and early p-type PERC cells had a high surface doping concentration on the front side (p...). +Emitter surface concentration is typically >1×10² 0 cm - ³) and a relatively thick field-effect passivation layer. The passivation quality is not sensitive to UV-induced hydrogen desorption. UV-induced degradation (UVID) was not considered a significant reliability issue in the PERC era, and UV testing was only performed as a routine item in IEC 61215 certification.

[0039] To address the issues of yellowing, acetic acid corrosion of grid lines, and backsheet embrittlement caused by long-term ultraviolet irradiation in early EVA films, the industry once promoted the use of ultraviolet-blocking EVA films (with added organic ultraviolet absorbers and a cutoff wavelength of approximately 380nm), which effectively blocked short-wave ultraviolet rays and alleviated yellowing.

[0040] Subsequently, to improve optical utilization and nominal power, the industry tended to use high-transmittance films (UV transparent EVA or POE), which have a UV transmittance of >85% in the 320~400nm wavelength range. In the PERC module era, because the cells were not sensitive to UV, the loss of UV protection by high-transmittance films did not show significant negative consequences. With the industrialization of N-type tunneling oxide passivated contact (TOPCon) and heterojunction (HJT) solar cells, low surface concentration p-type films were adopted on the front side of the cells. + In doped regions or undoped silicon substrates, field passivation is achieved solely through passivation contact structures, with the passivation effect highly dependent on Si-H chemical passivation. High-permeability films allow ultraviolet B (UVB) light to reach the cell surface directly. The photon energy is sufficient to break Si-H bonds, leading to hydrogen atom desorption, increased interface state density, and decreased minority carrier lifetime. This manifests as a decrease in open-circuit voltage and fill factor—significantly amplifying the UVID phenomenon in N-type high-efficiency cells.

[0041] To address this issue, the mainstream measures currently used in modules include: (1) reusing UV cutoff films but adjusting the cutoff edge from the early 380nm to approximately 340~350nm (UVB cutoff film) to block destructive short-wave UV while retaining some UVA photons; (2) using UV downconversion (light conversion) films to convert harmful UV photons into visible blue light that can be absorbed by the battery, thus providing both protection and efficiency enhancement, but at a relatively high cost. After power / attenuation balance optimization, the nominal power of modules using 350nm cutoff films or light conversion films is usually about 0.5~2W lower than that using high-transparency films.

[0042] Battery-side mitigation measures mainly include: appropriately thickening the front-side ALD AlOx passivation layer (typically from 3~4nm to 5~8nm) to improve hydrogen storage, adjusting AlOx and SiNx deposition parameters to adjust the hydrogen content and bonding configuration of the film, and optimizing high-temperature annealing / hydrogenation annealing processes to improve hydrogen binding energy, but these measures have limited effect on UVID resistance. Simply adjusting the battery-side process involves trade-offs between passivation quality, optical absorption, and process window, and cannot completely offset the effects of high-intensity UVB under high-transmittance films; simply cutting off or downconverting UV at the encapsulation end introduces power loss or increased costs. Therefore, a comprehensive solution that balances UV protection, minimizes power loss, and ensures long-term reliability is still needed.

[0043] Some studies have mentioned using ultraviolet absorption layers such as TiO2 and SnO2 at the battery end to reduce UVID degradation of module products. However, this solution has the following drawbacks: 1) The anti-UV principle is the same as that of the cut-off film, but it increases the cost and complexity of the battery process. In contrast, the cut-off film does not require any process additions or changes, and its cost is the same as that of the high-transparency film; 2) The passivation effect is poor and a mismatch in anti-reflection occurs.

[0044] The following section uses titanium dioxide (TiO2) thin film as an example to introduce the technical problems of using ultraviolet absorption layers in batteries.

[0045] Titanium dioxide (TiO2) thin films, with their ultraviolet absorption edge of approximately 380-410 nm and ability to absorb short-wave ultraviolet light with wavelengths less than 380 nm, were studied as candidate materials for single-layer or double-layer anti-reflection coatings (ARC) in crystalline silicon solar cells during the 1980s and 1990s, with the aim of combining anti-reflection and ultraviolet shielding functions.

[0046] However, TiO2 thin films were ultimately phased out in mainstream photovoltaic cell production lines and failed to gain widespread application. The fundamental reason lies in the inherent performance defects of the TiO2 material itself: (1) Poor film density and insufficient hydrothermal stability: TiO2 films obtained by typical preparation processes such as sol-gel method generally have nanoporous structures, which are very easy to adsorb water vapor in the atmospheric environment, resulting in refractive index drift, film cracking, and the formation of water vapor and corrosive ions (such as Na+). + The penetration channels into the battery surface significantly degrade the passivation effect and the long-term stability of the metal electrodes.

[0047] (2) Photocatalytic activity causes accelerated aging of encapsulation materials: Anatase TiO2 has strong photocatalytic activity. Under ultraviolet light excitation, it will generate highly active free radicals such as hydroxyl radicals and superoxide anion radicals. These active substances will continuously catalyze the decomposition of organic components in adjacent encapsulation materials (such as EVA film), accelerate the yellowing of the film, release of acetic acid and embrittlement of the backsheet, which seriously violates the basic requirement of more than 25 years of weather resistance of battery modules.

[0048] (3) There is an inherent trade-off in optical performance: Although the intrinsic ultraviolet absorption of TiO2 can shield UV-B, this absorption is accompanied by additional parasitic absorption and scattering losses in the visible light region (especially the blue-violet band of 400~450nm). In contrast, single-layer SiN with optimized thickness and refractive index... x It exhibits superior broadband antireflection performance in the 400–1200 nm wavelength range, resulting in a significantly better short-circuit current gain than TiO2 monolayer. In other words, while attempting to block harmful ultraviolet light, TiO2 inevitably sacrifices more valuable visible light energy.

[0049] (4) Lack of effective chemical passivation mechanism: Unlike SiN prepared by plasma-enhanced chemical vapor deposition (PECVD), x Thin films are rich in Si-H and NH bonds, enabling them to serve as efficient hydrogen sources for the diffusion of hydrogen atoms into the silicon bulk for passivation. In contrast, TiO2 films (whether anatase or rutile phase) have extremely low intrinsic hydrogen (H) content and lack good hydrogen diffusion and passivation capabilities. This means that TiO2 can only provide limited field-effect passivation and cannot achieve the same level of passivation as SiN. x This approach reduces the defect state density within the silicon wafer through hydrogen passivation. However, given the extremely high dependence of high-efficiency solar cells (such as TOPCon) on hydrogen passivation, simply introducing a TiO2 layer not only fails to contribute passivation gain but may also obstruct the underlying SiN layer. x The outward diffusion of hydrogen atoms weakens the overall passivation effect.

[0050] Due to the multiple inherent defects at the material level mentioned above—especially photocatalytic risk, poor damp-heat stability, optical parasitic absorption, and passivation failure caused by extremely low intrinsic hydrogen content—TiO2 has never become the mainstream choice for the front-side film system in mass production of crystalline silicon solar cells.

[0051] It is worth noting that although N-type TOPCon / HJT batteries exhibit UV-induced degradation (UVID) sensitivity, there is currently no industrial trend in the industry to actively reintroduce TiO2 films as the front UV absorption layer of the battery. While existing UV cutoff films / phototransfer films are mature, a trade-off between power loss (0.5~2W) remains. Simply adding a TiO2 layer merely to improve cutoff capability would not only inherit the aforementioned fatal flaws but also exacerbate the degradation of battery passivation performance due to the extremely low hydrogen content of TiO2, which is clearly unacceptable. Therefore, a breakthrough technology is urgently needed that can circumvent the inherent defects of TiO2 while unlocking its UV absorption potential and achieving compatibility or even enhancement with existing passivation systems.

[0052] Please refer to Figures 1-2 This invention provides a solar cell 100, comprising: Silicon substrate 1, the silicon substrate 1 includes a first surface 11; Passivation layer 2 is provided on the first surface 11; An ultraviolet absorption layer 3 is disposed on the passivation layer 2, and the material of the ultraviolet absorption layer 3 includes titanium oxide; An antireflection layer 4 is disposed on the ultraviolet absorption layer 3, the antireflection layer 4 comprising stacked SiN x O y Layer 41 and SiN m O n Layer 42, SiN x O y Layer 41 compared to SiN m O n Layer 42 is closer to the ultraviolet absorption layer 3, SiN x O y Layer 41 satisfies: x / (x+y)>50%; SiN m O n Layer 42 satisfies: m / (m+n) < 50%, and the difference between x / (x+y) and m / (m+n) is d, where d ≥ 1%.

[0053] In this embodiment of the invention, the silicon substrate 1 includes a first surface 11 and a second surface 12 disposed opposite to each other along its thickness direction. The first surface 11 is the light-facing surface of the solar cell 100, and the second surface 12 is the back-lighting surface of the solar cell 100. That is, the first surface 11 is the side of the solar cell 100 that mainly receives sunlight when it is working normally, and the second surface 12 can also receive some sunlight when the solar cell 100 is actually working.

[0054] In this embodiment of the invention, the specific cell type of the solar cell 100 is not limited. For example, the solar cell 100 can be a back-contact solar cell or a double-sided contact solar cell.

[0055] like Figure 1 As shown, the solar cell 100 is a back-contact solar cell. In this case, the second surface 12 is alternately provided with a first doped layer 5 and a second doped layer 6. One of the first doped layer 5 and the other of the second doped layer 6 is a P-type doped layer, and the other is an N-type doped layer. A first metal electrode 81 is disposed on the first doped layer 5, and a second metal electrode 82 is disposed on the second doped layer 6. The solar cell 100 may further include a back passivation antireflection layer 7 covering at least the first doped layer 5 and the second doped layer 6. The first metal electrode 81 passes through the back passivation antireflection layer 7 and is electrically connected to the first doped layer 5, and the second metal electrode 82 passes through the back passivation antireflection layer 7 and is electrically connected to the second doped layer 6. The passivation layer 2, the ultraviolet absorption layer 3, and the antireflection layer 4 are sequentially stacked on the first surface 11. The back passivation antireflection layer 7 serves to passivate the second surface 12 and reduce sunlight reflection. The back passivation antireflection layer 7 can be a silicon nitride layer or a silicon oxynitride layer.

[0056] like Figure 2 As shown, the solar cell 100 is a double-sided contact solar cell. A first doped layer 5 is disposed on the first surface 11, and a second doped layer 6 is disposed on the second surface 12. One of the first doped layer 5 and the other of the second doped layer 6 is a P-type doped layer and the other is an N-type doped layer. A first metal electrode 81 is disposed on the first doped layer 5, and a second metal electrode 82 is disposed on the second doped layer 6. A passivation layer 2, an ultraviolet absorption layer 3, and an antireflection layer 4 are sequentially stacked on the first doped layer 5 on the first surface 11. The solar cell 100 may further include a passivation and antireflection layer 7 covering the second doped layer 6. The first metal electrode 81 passes through the antireflection layer 4, the ultraviolet absorption layer 3, and the passivation layer 2, and is electrically connected to the first doped layer 5. The second metal electrode 82 passes through the back passivation and antireflection layer 7 and is electrically connected to the second doped layer 6.

[0057] The present invention provides a solar cell 100 by sequentially depositing a passivation layer 2, an ultraviolet absorption layer 3, and an antireflection layer 4 on the first surface 11 of a silicon substrate 1. Thus, an ultraviolet absorption layer 3 is directly added between the passivation layer 2 and the antireflection layer 4, integrating the ultraviolet absorption layer 3 onto the solar cell 100. As part of the solar cell 100, the ultraviolet absorption layer 3 absorbs ultraviolet light passing through the front glass and front encapsulant film of the battery module. Compared to adding ultraviolet-blocking components to the encapsulant film, the ultraviolet absorption layer 3 of the present invention does not rely on the polymer encapsulant film, and there is no problem of ultraviolet-blocking function degradation caused by encapsulant film degradation. The long-term ultraviolet-blocking effect is more stable, making the solar cell 100 more reliable against long-term ultraviolet light-induced degradation. Furthermore, the ultraviolet absorption layer 3 formed on the first surface 11 of the solar cell 100 effectively blocks ultraviolet light from entering the battery, reducing the probability of defects such as ultraviolet light damaging Si-H bonds, thereby significantly alleviating the problem of ultraviolet light-induced degradation of the solar cell 100. Since the ultraviolet blocking function has been implemented in the solar cell 100, there is no need to specially select an ultraviolet blocking encapsulant film when encapsulating the battery module. This avoids increasing the cost of the encapsulant film and the complexity of the process due to the addition of ultraviolet absorbers, which can reduce the production difficulty and cost of the battery module.

[0058] In this embodiment of the invention, the material of the ultraviolet absorption layer 3 includes titanium oxide, and the antireflection layer 4 is configured to include SiN. x O y Layer 41 and SiN m O n Layer 42, and because the refractive index of silicon oxynitride is less than that of titanium oxide, that is, SiN x O y Layer 41 and SiN m O nThe refractive indices of all layers 42 are lower than those of the ultraviolet absorption layer 3. By superimposing at least two layers of silicon oxynitride with refractive indices between those of the ultraviolet absorption layer 3 and the encapsulating film of the battery module, the refractive index of SiN is controlled. x O y Layer 41 satisfies: x / (x+y)>50%; SiN m O n Layer 42 satisfies: m / (m+n) < 50%, making SiN x The refractive index of Oy layer 41 is greater than that of SiN. m O n The refractive index of layer 42 allows sunlight to pass through the encapsulating film of the battery module sequentially via SiN. m O n Layer 42, SiN x O y Layer 41 enters the ultraviolet absorption layer 3, due to SiN x O y Layer 41 and SiN m O n Layer 42 configuration, encapsulating film, SiN m O n Layer 42, SiN x O y The refractive index of layer 41 and ultraviolet absorption layer 3 increases sequentially, and the refractive index between each layer gradually changes, which can greatly reduce interface reflection in the main visible light band (especially the 600nm~800nm ​​peak response region). The antireflection layer 4 is made of SiN m O n Layer 42, SiN x O y Layer 41 forms a gradually changing refractive index gradient. The antireflection layer 4, the ultraviolet absorption layer 3, and the encapsulating film of the battery module can achieve good optical matching, realizing efficient antireflection of the antireflection layer 4. This can achieve better antireflection effect of the antireflection layer 4, improve the solar energy utilization of the solar cell, and thus improve the photoelectric conversion efficiency of the solar cell.

[0059] Moreover, SiN m O n In layer 42, m / (m+n) < 50%, which means SiN m O n The nitrogen content in layer 42 is less than that in SiN. m O n Oxygen content in layer 42; SiN x O y In layer 41, x / (x+y) > 50%, that is, SiN x O y The nitrogen content in layer 41 is greater than that in SiN. x O yThe oxygen content in layer 41; and the difference between x / (x+y) and m / (m+n) is d, d≥1%, making SiN m O n Layer 42 and SiN x O y The refractive index of layer 41 forms an effective difference, SiN m O n Layer 42 is an oxygen-rich layer, SiN x O y Layer 41 is a nitrogen-rich layer, SiN m O n The refractive index of layer 42 is higher than that of SiN. x O y Layer 41 has a lower refractive index, and SiN m O n The refractive index of layer 42 is higher than that of the encapsulating film, SiN m O n Layer 42 as SiN x O y The transition layer between layer 41 and the encapsulating film of the battery module (the encapsulating film is usually an EVA film with a refractive index of 1.48~1.51) can reduce the reflection of sunlight when it enters the antireflection layer 4 from the encapsulating film, thus achieving a better antireflection effect for the antireflection layer 4; while SiN x O y In layer 41, x / (x+y) > 50%, making SiN x O y Layer 41 is a nitrogen-rich layer, consisting of nitrogen-rich SiN. x O y Layer 41 compared to SiN m O n Layer 42 has a higher extinction coefficient (k value) in the ultraviolet region, SiN x O y Layer 41 can effectively absorb a portion of ultraviolet light, significantly reducing the penetration of high-energy ultraviolet photons into the battery interior and mitigating performance degradation caused by ultraviolet light. Therefore, SiN m O n Layer 42, SiN x O y The combination of layer 41 and ultraviolet absorption layer 3 achieves good optical matching, resulting in better antireflection effect of antireflection layer 4, improving the solar energy utilization rate of the solar cell, and reducing the performance degradation of the cell caused by ultraviolet light, thereby improving the photoelectric conversion efficiency of the solar cell. Furthermore, the SiN layer can be individually controlled. x O y Layer 41 and SiN m O n The ratio of N to O in layer 42 can be used to control the SiN. x Oy Layer 41 and SiN m O n The refractive index range of layer 42 means that the antireflection layer 4 does not require the stacking of film layers of different materials, which can greatly simplify the preparation process of the antireflection layer 4 and help reduce production costs.

[0060] In this embodiment of the invention, SiN x O y When layer 41 satisfies x / (x+y)>50%, specifically, it can be 0.5. <x<1,0<y<0.5。SiN m O n Layer 42 can be 0 if m / (m+n) < 50%. <m<0.5,0.5<n<1。

[0061] As an embodiment of the present invention, x / (x+y)≥55%, which can further increase the SiN content. x O y The difference in nitrogen and oxygen content within the layer is more conducive to increasing the SiN content. x O y Layer 41 and SiN m O n The refractive index difference in layer 42 creates a more effective refractive index gradient and further increases the SiN content. x O y The nitrogen content of layer 41 is more conducive to improving SiN x O y Layer 41 enhances its ultraviolet light absorption performance. Furthermore, x / (x+y) ≥ 60%, further increasing the SiN... x O y The nitrogen content in layer 41 is more conducive to further increasing the SiN content. x O y Layer 41 and SiN m O n The refractive index difference in layer 42 creates a more effective refractive index gradient and is more conducive to improving the performance of SiN. x O y Layer 41 has the ability to absorb ultraviolet light.

[0062] As an embodiment of the present invention, SiN x O y Layer 41 satisfies: x / (x+y)<99%, making SiN x O y Layer 41 can interact with the upper SiN layer m O n Layer 42 provides a good match and also creates a suitable refractive index difference with the underlying ultraviolet absorption layer 3, achieving a better gradient anti-reflection effect; moreover, it can reduce the SiN... x O ytensile stress of layer 41, and improve adhesion and stability.

[0063] As an embodiment of the present invention, m / (m+n) ≤ 45%, which further reduces the nitrogen content of SiN m O n layer 42, increases the oxygen content of SiN m O n layer 42, which is beneficial to ensuring that the refractive indices of SiN x O y layer 41 and SiN m O n layer 42 form a more effective difference, and ensures that the refractive indices of SiN m O n layer 42 and the encapsulant film of the battery assembly form a more effective difference, thereby forming a more effective gradual refractive index gradient, and increasing the oxygen content of SiN m O n layer 42 can reduce the reflection of sunlight by SiN m O n layer 42, so that a better anti-reflection effect of the anti-reflection layer 4 can be achieved.

[0064] Further, m / (m+n) ≤ 40%, which further reduces the nitrogen content of SiN m O n layer 42, increases the oxygen content of SiN m O n layer 42, further increases the refractive index difference between SiN x O y layer 41 and SiN m O n layer 42, forms a more effective gradual refractive index gradient, and further increases the oxygen content of SiN m O n layer 42, further improving the anti-reflection effect of the anti-reflection layer 4.

[0065] As an embodiment of the present invention, SiN m O n layer 42 satisfies: 10% < m / (m+n), which avoids excessively low nitrogen content and excessively high oxygen content of SiN m O n layer 42, so that the refractive indices of SiN m O n layer 42 and the encapsulant film form an effective difference, so as to achieve a better anti-reflection effect of SiN m O n layer 42.

[0066] As an embodiment of the present invention, d≥5%, that is, further increasing the difference between x / (x+y) and m / (m+n), thereby further increasing the SiN m O n Layer 42 and SiN x O y Nitrogen content difference in layer 41 and SiN m O n Layer 42 and SiN x O y The difference in oxygen content in layer 41 is more conducive to the formation of SiN. m O n Layer 42 and SiN x O y Layer 41 provides a more effective refractive index difference, which is beneficial for SiN m O n Layer 42 increases the antireflection effect of antireflection layer 4 and is beneficial to SiN. x O y Layer 41 increases the gain of antireflection layer 4 in terms of ultraviolet absorption. Furthermore, d ≥ 10% further increases the gain of SiN. m O n Layer 42 and SiN x O y Nitrogen content difference in layer 41 and SiN m O n Layer 42 and SiN x O y The difference in oxygen content in layer 41 further benefits SiN m O n Layer 42 increases the antireflection effect of antireflection layer 4 and is beneficial to SiN. x O y Layer 41 increases the gain of antireflection layer 4 in terms of ultraviolet absorption. Furthermore, d ≥ 15% further increases the gain of SiN. m O n Layer 42 and SiN x O y The nitrogen and oxygen content difference in layer 41; furthermore, d≥20%, further increasing SiN m O n Layer 42 and SiN x O y The nitrogen and oxygen content difference in layer 41; furthermore, d≥30%, further increasing SiN m O n Layer 42 and SiN x O y Differences in nitrogen and oxygen content in layer 41.

[0067] As an embodiment of the present invention, the general chemical formula of titanium oxide is TiO2. bThe value of b ranges from 1.8 to 2.2. Here, b can be any TiO₂. b In all cases, b is equal to 2. Alternatively, it could be a partial TiO₂... b In this case, b equals 2, and some TiO2... b In this context, b is not equal to 2, meaning that some TiO2... b b in the equation equals 2, and at the same time, some TiO b The value of b in the range is 1.8~2 and not equal to 2 and / or a portion of TiO. b In this context, b is between 2 and 2.2, and not equal to 2. When a portion of TiO2... b In this case, b equals 2, which makes some TiO2... b As a crystalline state, it possesses sharp band-edge absorption, primarily absorbing high-energy photons in the deep ultraviolet region (wavelength <380nm), while some TiO2... b In this case, b is not equal to 2, which makes some TiO2... b It can capture photons in the near-ultraviolet region and even blue-violet light (wavelength 380~450 nm), which is light that TiO2 cannot utilize. Therefore, different stoichiometric ratios of TiO2 can be used to capture these photons. b Combining TiO₂ with different stoichiometric ratios b It can achieve absorption of ultraviolet light in different wavelengths, thus forming a continuous light absorption coverage in the broadband range from ultraviolet to near-visible light in the ultraviolet absorption layer 3. This greatly increases the absorption of ultraviolet photons in the ultraviolet band of sunlight by the ultraviolet absorption layer 3, further improving the ultraviolet light absorption effect of the ultraviolet absorption layer; and part of the TiO in the ultraviolet absorption layer 3 b b equals 2, making some TiO b The lattice is regular, while TiO2 is present in some regions. b b is not equal to 2, which makes some TiO b Lattice distortion can form lattice mismatch interfaces, which can absorb and dissipate mechanical stress, effectively preventing the propagation of microcracks and thus greatly improving the long-term mechanical stability of solar cells under thermal shock. Therefore, this invention optimizes the TiO₂ content in the ultraviolet absorption layer... b The b-value can balance the good ultraviolet light absorption effect of the ultraviolet absorption layer and the long-term stability of the ultraviolet absorption layer, thereby balancing the photoelectric conversion efficiency and structural stability of the solar cell.

[0068] In this embodiment of the invention, when a portion of TiO b When b is 1.8~2 and not equal to 2, then some TiO2... b In a hypoxic state (b < 2), some TiO2... b Oxygen vacancies will form in the crystal lattice of TiO2, which can broaden the light absorption range. bIntroducing new defect energy levels into the band gap of the ultraviolet absorption layer 3 allows it to absorb lower-energy photons, resulting in overlapping spectral bands across different regions of the layer. This broadens the overall equivalent absorption spectrum of the ultraviolet absorption layer 3, leading to better absorption of ultraviolet light. When some TiO₂... b In this case, b is 2 to 2.2 and not equal to 2 (b > 2), and some TiO2... b In an oxygen-rich state, some TiOb lattices contain excess oxygen atoms or a large number of titanium vacancies. By reducing defects that act as recombination centers, oxygen-rich TiOb... b It can effectively suppress electron recombination inside the battery and improve the long-term stability of solar cells.

[0069] In this embodiment of the invention, the silicon substrate 1 can specifically be an N-type silicon wafer.

[0070] In this embodiment of the invention, the passivation layer 2 can be a single-layer structure or a stacked structure consisting of two or more layers.

[0071] As an embodiment of the present invention, the passivation layer 2 includes a stack of one or at least two of the following: a silicon oxide layer, an aluminum oxide layer, a silicon oxynitride layer, a silicon nitride layer, and a hafnium oxide layer.

[0072] In this embodiment, the passivation layer 2 can be one of silicon oxide layer, aluminum oxide layer, silicon oxynitride layer, silicon nitride layer, and hafnium oxide layer, or it can be a stack of at least two of silicon oxide layer, aluminum oxide layer, silicon oxynitride layer, silicon nitride layer, and hafnium oxide layer.

[0073] In this embodiment, the passivation layer 2 serves as a dual-functional layer for field-effect passivation, hydrogen supply, and hydrogen diffusion regulation. Specifically, the passivation layer 2 can reduce the surface recombination rate at the interface of the silicon substrate 1, compensating for the lack of field passivation in the ultraviolet absorption layer 3 itself, thus providing field-effect passivation. The passivation layer 2 can release hydrogen atoms under annealing or illumination conditions, providing a hydrogen passivation source and hydrogen transport regulation, enabling hydrogen passivation of dangling bonds. Moreover, the passivation layer 2 can smooth the surface of the silicon substrate 1 at the atomic scale, reducing dangling bonds and interface state density. Simultaneously, the passivation layer 2 can also provide stress buffering, buffering the thermal expansion coefficient and lattice mismatch stress between the ultraviolet absorption layer 3 and the silicon substrate 1, suppressing film cracking and interface defect formation.

[0074] As an embodiment of the present invention, the thickness D1 of the passivation layer 2 is 2~10 nanometers.

[0075] In this embodiment, the thickness D1 of the passivation layer 2 is the total thickness of all layers in the passivation layer 2. The thickness of the passivation layer 2 is controlled between 2 and 10 nanometers to avoid poor passivation effect due to an excessively thin passivation layer 2, excessive optical loss due to an excessively thick passivation layer 2, and the potential for bubble formation that could damage the interface passivation structure. Specifically, the thickness D1 of the passivation layer 2 is the average thickness of the passivation layer 2. This can be achieved by selecting 10 points at equal intervals on the passivation layer 2, measuring the thickness of the passivation layer 2 at each of these 10 points, and then calculating the average thickness of the passivation layer 2 at these 10 points as the thickness D1 of the passivation layer 2.

[0076] For example, the thickness D1 of the passivation layer 2 can be any value among 2 nm, 2.5 nm, 3 nm, 3.2 nm, 4 nm, 4.5 nm, 6 nm, 6.6 nm, 7 nm, 7.8 nm, 8 nm, 8.5 nm, 9 nm, 9.2 nm, and 10 nm.

[0077] Please refer to the reference. Figure 3 As an embodiment of the present invention, the passivation layer 2 includes a first sub-passivation layer 21 and a second sub-passivation layer 22 stacked on the first sub-passivation layer 21, wherein the second sub-passivation layer 22 is located between the first sub-passivation layer 21 and the ultraviolet absorption layer 3.

[0078] In this embodiment, the passivation layer 2 is a stacked structure composed of a first sub-passivation layer 21 and a second sub-passivation layer 22. Thus, by using the first sub-passivation layer 21 to contact the silicon substrate 1, the defect density on the surface of the silicon substrate 1 can be reduced. The second sub-passivation layer 22 can provide a hydrogen source and perform field passivation. Therefore, the combination of the first sub-passivation layer 21 and the second sub-passivation layer 22 can better achieve the passivation effect of the passivation layer 2. Preferably, the thickness of the second sub-passivation layer 22 is greater than the thickness of the first sub-passivation layer 21. Using the thinner first sub-passivation layer 21 to contact the silicon substrate 1 can better reduce the defect density on the surface of the silicon substrate 1, while using the thicker second sub-passivation layer 22 can better perform the functions of hydrogen source supply and field passivation. For example, the ratio of the thickness of the second sub-passivation layer 22 to the thickness of the first sub-passivation layer 21 can be 1.2 to 10.

[0079] As an embodiment of the present invention, the first sub-passivation layer 21 is a silicon oxide layer, and the second sub-passivation layer 22 is at least one of an aluminum oxide layer, a silicon nitride layer, and a silicon oxynitride layer.

[0080] In this embodiment, a silicon oxide layer is used as the first sub-passivation layer 21. The contact between the silicon oxide layer and the silicon substrate 1 can reduce the defect density on the surface of the silicon substrate 1. At least one of an aluminum oxide layer, a silicon nitride layer, and a silicon oxynitride layer is used as the second sub-passivation layer 22. The second sub-passivation layer 22 can better play the role of hydrogen source supply and field passivation.

[0081] As an embodiment of the present invention, the thickness of the first sub-passivation layer 21 is 0.1~2 nanometers, and the thickness of the second sub-passivation layer 22 is 0.5~8 nanometers.

[0082] In this embodiment, the thickness of the first sub-passivation layer 21 is controlled to be 0.1~2 nanometers, and the thickness of the second sub-passivation layer 22 is controlled to be 0.5~8 nanometers. This allows for a lower defect density between the first sub-passivation layer 21 and the silicon substrate 1, while ensuring a good hydrogen source supply and field passivation effect for the second sub-passivation layer 22, thus achieving a better passivation effect for the passivation layer 2. For example, the thickness of the first sub-passivation layer 21 can be any value among 0.1 nanometers, 0.3 nanometers, 0.5 nanometers, 0.7 nanometers, 0.8 nanometers, 0.9 nanometers, 1.0 nanometers, 1.1 nanometers, 1.3 nanometers, 1.6 nanometers, 1.8 nanometers, and 2.0 nanometers. The thickness of the second sub-passivation layer 22 is any value among 0.5 nm, 0.6 nm, 0.8 nm, 1 nm, 1.2 nm, 1.5 nm, 1.9 nm, 2 nm, 2.2 nm, 2.5 nm, 2.8 nm, 3 nm, 3.5 nm, 3.8 nm, 4 nm, 4.6 nm, 5 nm, 5.5 nm, 6 nm, 6.3 nm, 7 nm, 7.6 nm, and 8 nm.

[0083] While using UV-absorbing materials such as titanium dioxide to provide dual UV protection (UV cutoff and H-resistance) and reduce reflection loss to increase module power is feasible, it's insufficient for their application in battery cells. Two issues need to be addressed: field passivation and H-passivation on the silicon substrate surface. If the UV-absorbing layer is directly applied between the antireflection layer and the silicon substrate, severe defects such as insufficient field passivation and H-passivation lead to performance failure.

[0084] Therefore, in this embodiment of the invention, a passivation layer 2 needs to be inserted between the silicon substrate 1 and the ultraviolet absorption layer 3 to serve as a dual-functional layer for field-effect passivation and hydrogen supply / hydrogen diffusion regulation. The passivation layer 2 specifically includes the following functions: Providing field-effect passivation: Passivation layer 2 preferably has a high fixed charge density (such as aluminum oxide AlO). x It has a negative fixed charge, and the fixed charge density Qf can reach 10¹²~10¹³cm. - ²) or a dielectric layer with appropriate band shift (such as AlO) x SiO x SiON, SiO x / AlO x Layering, etc., forms band bending at the silicon interface, repelling minority carriers (electrons / holes), reducing the surface recombination rate, and compensating for the lack of field passivation in titanium oxide itself.

[0085] Providing a hydrogen passivation source and regulating hydrogen transport: Passivation layer 2 (especially hydrogen-rich AlO2 prepared by PECVD) x SiN x SiO x Or AlO deposited by ALD x (Followed by hydrogenation annealing) it has a high hydrogen content (1 at%~10 at%), and can release hydrogen atoms under annealing or light irradiation conditions to replenish Si / SiO through interfacial diffusion. x The dangling bonds at the interface are passivated; at the same time, the passivation layer 2 can avoid the "hydrogen blocking effect" caused by the low hydrogen solid solubility and low hydrogen diffusion coefficient of the ultraviolet absorption layer 3, so that hydrogen can escape from the upper anti-reflection layer (such as SiN). x (or diffuse downwards to the surface of silicon substrate 1.)

[0086] Interface state density reduction and chemical passivation: Passivation layer 2 (such as AlO deposited by ALD) x / SiO x Ultrathin tunneling layers can smooth silicon surfaces at the atomic scale, reducing dangling bonds and interface state density (interface state density can be reduced to 10¹). 0 ~10¹¹cm - ²eV - (¹ magnitude), decoupled from the cutoff function of the ultraviolet absorption layer 3, the passivation layer 2 achieves passivation and the ultraviolet absorption layer 3 achieves ultraviolet cutoff in a layered synergistic design.

[0087] Stress buffering: The passivation layer 2 simultaneously buffers the thermal expansion coefficient and lattice mismatch stress between the ultraviolet absorption layer 3 and the silicon substrate 1, suppressing film cracking and interface defect formation.

[0088] Among them, the silicon oxide layer and the silicon substrate 1 can form the lowest defect state, but the field passivation is lacking and the H content is insufficient. The aluminum oxide film layer or the silicon nitride layer has better effects on H content and field passivation. Therefore, the passivation layer 2 is preferably a stacked structure of silicon oxide layer and aluminum oxide film layer or silicon nitride layer. The bottom layer is formed by the silicon oxide layer and the silicon substrate 1 to reduce the defect density, while the top layer covers the aluminum oxide film layer or silicon nitride layer to play the role of H source supply and field passivation.

[0089] Furthermore, since the refractive index of the passivation layer 2 material is much smaller than that of the ultraviolet absorption layer 3, but the passivation layer 2 is inserted between the silicon substrate 1 and the ultraviolet absorption layer 3, it inevitably causes a loss in antireflection. Taking aluminum oxide as an example, the antireflection loss values ​​for passivation layers 2 with different thicknesses are measured as follows: Figure 6 As shown, from Figure 6It can be seen that when the thickness of passivation layer 2 is <4nm, there is no optical impact. When the thickness of passivation layer 2 is <10nm, the optical power loss of the component can be controlled within <1.5W. Considering the balance between passivation effect and optical effect, the thickness of passivation layer 2 should be controlled between 2~10nm. If passivation layer 2 is too thin, the passivation effect will be poor. If passivation layer 2 is too thick, the optical loss will be too large. In addition, if passivation layer 2 is too thick, it will also easily cause bubble problems, which will lead to the destruction of the interface passivation structure.

[0090] Therefore, in a preferred embodiment, the passivation layer 2 includes a first sub-passivation layer 21 and a second sub-passivation layer 22, wherein the first sub-passivation layer 21 may be a silicon oxide layer (SiO2). x The thickness of the first sub-passivation layer 21 is 0.1~2nm, and the first sub-passivation layer 21 serves as a tunneling layer; the second sub-passivation layer 22 can be an aluminum oxide layer (AlO). x The second sub-passivation layer 22 has a thickness of 0.5~8 nm and can serve as a field passivation and hydrogen source layer. Passivation layer 2 can also be made of SiO₂. x SiON, hydrogen-rich SiN x AlO x The single or composite layer consists of one or more of the following, preferably with a hydrogen content of 1 at% to 10 at% and a fixed charge density absolute value ≥ 5 × 10¹¹ cm⁻¹. - ², interfacial state density Dit ≤ 5 × 10¹¹ cm - ²eV - ¹, so that the surface of the silicon substrate 1 can still maintain efficient passivation and long-term UV resistance while ensuring the existence of the ultraviolet absorption layer 3.

[0091] As an embodiment of the present invention, the refractive index of the ultraviolet absorption layer 3 is 2.2~3.4, and the SiN... x O y The refractive index of layer 41 is 1.82~2, SiN m O n The refractive index of layer 42 is 1.55~1.8.

[0092] In this embodiment, SiN m O n Layer 42, SiN x O y The refractive index of layer 41 and ultraviolet absorption layer 3 increases sequentially, allowing incident sunlight to gradually couple into silicon substrate 1 with lower reflection loss, thereby effectively increasing the total amount of photogenerated carriers excited. Preferably, SiN x O y Layer 41 and SiN m O n The difference in refractive index of layer 42 is greater than or equal to 0.1.

[0093] As an embodiment of the present invention, SiN x O y Layer 41 and SiN m O n The difference in refractive index of layer 42 is greater than or equal to 0.2.

[0094] In this embodiment, SiN is further added. x O y Layer 41 and SiN m O n The refractive index difference of layer 42 is more conducive to reducing SiN m O n Layer 42 reflects sunlight and increases SiN content. x O y Layer 41 has the ability to absorb ultraviolet light.

[0095] The refractive indices of various materials used in battery modules and solar cells are shown in Table 1 below. The refractive index values ​​were measured under a light source with a wavelength of 632 nanometers.

[0096] Table 1 As can be seen from Table 1, there is a gap in the range of n=2.1-3.85. The refractive index of the ultraviolet absorption layer 3 can fall in the range of 2.2-3.4. At the same time, the anti-reflection layer 4, which has a refractive index that is more than 0.2 lower than that of the ultraviolet absorption layer 3, can enhance the anti-reflection effect, thereby achieving a technical effect that is superior in power compared to the UV cut-off film and light transfer film at the battery module end.

[0097] As an embodiment of the present invention, the thickness D2 of the ultraviolet absorption layer 3 is 10~70 nanometers.

[0098] In this embodiment, the thickness D2 of the ultraviolet absorption layer 3 is controlled to be 10-70 nanometers. This avoids the ultraviolet absorption layer 3 being too thin, thus achieving effective resistance to ultraviolet light-induced degradation, and also avoids the ultraviolet absorption layer 3 being too thick, which would affect visible light transmission and ensure low battery power loss. Specifically, the thickness D2 of the ultraviolet absorption layer 3 is the average thickness of the ultraviolet absorption layer 3. Specifically, 10 points can be selected at equal intervals on the ultraviolet absorption layer 3, and the thickness of the ultraviolet absorption layer 3 at each of these 10 points can be measured. The average thickness D2 of the ultraviolet absorption layer 3 at these 10 points can then be calculated.

[0099] For example, the thickness D2 of the ultraviolet absorption layer 3 can be any value among 10 nm, 11 nm, 12 nm, 14 nm, 15 nm, 20 nm, 26 nm, 30 nm, 40 nm, 50 nm, 60 nm, and 70 nm.

[0100] Among them, based on the passivation layer 2 having a thickness of 5 nm, and using anatase titanium oxide as the main component of the ultraviolet absorption layer 3, optical matching studies were conducted. The power loss and UV attenuation of the components under ultraviolet absorption layer 3 with different thicknesses are shown in Table 2. Table 2 As can be seen from Table 2, the thickness of the ultraviolet absorption layer 3 needs to be >10nm to achieve an effective anti-UV attenuation effect, while the thickness of the ultraviolet absorption layer 3 needs to be <70nm to keep the power loss less than one level (5W). Therefore, the preferred thickness of the ultraviolet absorption layer 3 is 10~70nm.

[0101] Furthermore, if the ultraviolet absorption layer 3 can achieve a low H content, the effect of H shock can be mitigated. Therefore, the H content of the passivation layer 2 and the antireflection layer 4 is >1E21 / cm. 3 In this case, the H content of the ultraviolet absorption layer 3 is more than 30% lower than that of the passivation layer 2 or the antireflection layer 4, which can play an effective buffering role. Therefore, by selecting a material with lower H solid solubility as the ultraviolet absorption layer 3, a low-H content ultraviolet absorption layer 3 can be formed after sintering and other activation passivation processes.

[0102] Furthermore, due to the low hydrogen content of the ultraviolet absorption layer 3, it is difficult to achieve the ideal H passivation effect through existing chain sintering technology. It requires a longer sintering time and sealing relief, which is due to the lack of chain sintering activation method. Therefore, the preferred sintering method is closed furnace tube sintering, which requires a temperature greater than 650°C and a sintering time greater than 1 min to provide the kinetic process required for H passivation activation. However, the peak temperature needs to be less than 850°C to avoid excessive H leakage, which would deplete the H in the sample and reduce the H passivation effect.

[0103] As an embodiment of the present invention, the extinction coefficient of the ultraviolet absorption layer 3 corresponding to light with a wavelength of 390~780 nm is less than 0.1, and the extinction coefficient of the ultraviolet absorption layer 3 corresponding to ultraviolet light with a wavelength of less than or equal to 320 nm is greater than 0.1.

[0104] In this embodiment, experiments have verified that light with wavelengths greater than 390 nm has almost no impact on battery efficiency degradation, while light with a wavelength of 320 nm has a significant impact on battery efficiency degradation. Therefore, by controlling the extinction coefficient of the ultraviolet absorption layer 3 corresponding to wavelengths of 390-780 nm to be less than 0.1, the absorption rate of the ultraviolet absorption layer 3 corresponding to wavelengths of 390-780 nm is kept low, making it easier for light with wavelengths of 390-780 nm to enter the silicon substrate 1, ensuring good utilization of visible light by the solar cell 100, and improving the battery power generation efficiency. Meanwhile, by controlling the extinction coefficient of the ultraviolet absorption layer 3 for ultraviolet light with wavelengths less than or equal to 320 nm to be greater than 0.1, the ultraviolet absorption layer 3 achieves a high absorption rate for ultraviolet light with wavelengths less than or equal to 320 nm, thus realizing good ultraviolet light absorption performance. Therefore, the ultraviolet absorption layer 3 can achieve good transmittance of visible light with wavelengths of 390~780 nm and good absorption performance of ultraviolet light with wavelengths less than or equal to 320 nm, thereby balancing the utilization of visible light and the cutoff of ultraviolet light by the ultraviolet absorption layer 3.

[0105] In this embodiment, the extinction coefficient of the ultraviolet absorption layer 3 for light with wavelengths of 390-780 nm is further less than 0.05. Furthermore, the extinction coefficient of the ultraviolet absorption layer 3 for light with wavelengths of 390-780 nm is less than 0.01. Furthermore, the extinction coefficient of the ultraviolet absorption layer 3 for light with wavelengths of 390-780 nm is less than 0.005. Furthermore, the extinction coefficient of the ultraviolet absorption layer 3 for light with wavelengths of 390-780 nm is less than 0.001.

[0106] In this embodiment, the ultraviolet absorption layer 3 further exhibits an extinction coefficient greater than 0.15 for ultraviolet light with a wavelength less than or equal to 320 nm. Further, the ultraviolet absorption layer 3 exhibits an extinction coefficient greater than 0.2 for ultraviolet light with a wavelength less than or equal to 320 nm. Further, the ultraviolet absorption layer 3 exhibits an extinction coefficient greater than 0.3 for ultraviolet light with a wavelength less than or equal to 320 nm. Further, the ultraviolet absorption layer 3 exhibits an extinction coefficient greater than 0.5 for ultraviolet light with a wavelength less than or equal to 320 nm.

[0107] Specifically, the contributions of different wavelengths of UV light to the UV attenuation and power of the module are shown in Table 3, and the curves showing the contributions of different wavelengths of UV light to the UV attenuation and power of the module are shown in Figure 3. Figure 7 As shown.

[0108] Table 3 It can be seen that light with a wavelength >390nm has almost no effect on the UV decay of the module, while light with a wavelength of around 350nm reaches the peak of the UV decay of the module. The sensitivity of wavelength to power increases sharply with the increase of wavelength. Photons in the 390~400nm band affect the module power by 3.1W, while light below 320nm has less sensitivity to the module power, but has already had a significant impact on the module decay.

[0109] Therefore, the absorption coefficient (k value) of the ultraviolet absorption layer 3 needs to have certain characteristics: the k value of the material of the ultraviolet absorption layer 3 for light with wavelengths ≥390nm should be small enough, while the k value of the material of the ultraviolet absorption layer 3 for light with wavelengths ≤320nm should be high enough.

[0110] Table 4 shows the k-values, reflection and absorption ratios of the ultraviolet absorption layer 3 under various wavelengths of sunlight. Table 4 It can be seen that a k-value of 0.1 is a crucial point. When the k-value of the ultraviolet absorption layer 3 exceeds 0.1, it will achieve excellent absorption. Therefore, at a wavelength of 320 nm, the k-value of the ultraviolet absorption layer 3 should be >0.1; at a wavelength of 390 nm, the k-value should be <0.1; further, at a wavelength of 390 nm, the k-value should be <0.01; further, at a wavelength of 390 nm, the k-value should be <0.001; further, at a wavelength of 390 nm, the k-value should be <0.0001. In this case, the ultraviolet absorption layer 3 will have better optical performance, allowing visible light to be fully utilized by the silicon substrate 1. Therefore, by controlling the extinction coefficient of the ultraviolet absorption layer 3 for wavelengths of 390~780 nm to be less than 0.1, and the extinction coefficient of the ultraviolet absorption layer 3 for ultraviolet light with wavelengths less than or equal to 320 nm to be greater than 0.1, the solar cell can effectively utilize visible light while effectively blocking ultraviolet light.

[0111] In this embodiment of the invention, the material of the ultraviolet absorption layer 3 may include only titanium oxide, or it may include other metal oxides. For example, the material of the ultraviolet absorption layer 3 may also include one or a combination of at least two of zinc oxide, hafnium oxide, zirconium oxide, yttrium oxide, scandium oxide, magnesium oxide, and tin oxide.

[0112] The bandgap, absorption edge, and refractive index of different metal oxide materials are shown in Table 5 below. The refractive index values ​​were measured under a light source with a wavelength of 632 nanometers.

[0113] Table 5 Therefore, based on a comprehensive evaluation of refractive index, band gap, and extinction coefficient, titanium oxide is the preferred metal oxide.

[0114] As an embodiment of the present invention, the titanium oxide includes anatase phase, and the mass fraction of the anatase phase is greater than or equal to 60%.

[0115] In this embodiment, titanium oxide typically exists in four phases: anatase, rutile, brookite, and amorphous. Under ultraviolet (UV) irradiation, the anatase phase of titanium oxide can more effectively absorb UV light, generate more long-lived photogenerated carriers, and achieve efficient charge separation. Therefore, the mass fraction of the anatase phase in titanium oxide is controlled to be greater than or equal to 60%, meaning the anatase phase in the UV absorption layer 3 accounts for greater than or equal to 60% of the total mass fraction of titanium oxide. This maximizes the proportion of the anatase phase in titanium oxide, which is more conducive to improving the absorption of UV light by titanium oxide, thereby enhancing the UV absorption performance of the UV absorption layer 3. Furthermore, when the UV absorption layer 3 is dominated by anatase-phase titanium oxide, the refractive index of the UV absorption layer 3 is similar to that of SiN... x O y Layer 41 and SiN m O n The refractive index of layer 42 can be smoothly transitioned. The combination of ultraviolet absorption layer 3 and antireflection layer 4 is more conducive to optical coupling into silicon substrate 1. The ultraviolet absorption layer 3 and antireflection layer 4 form a better optical match, which is conducive to improving the solar energy utilization rate of solar cells.

[0116] Among them, the extinction coefficient curves and n-value curves of titanium oxide materials under four different phases—anatase, rutile, brookite, and amorphous—show significant differences, which have a significant impact on UV resistance and optical performance. While the brookite and amorphous phases are unsuitable as the main components of the final UV-absorbing layer due to their poor thermal stability, they can be used as secondary components to regulate the optical properties of the titanium oxide layer. The relationship between the refractive index (n) and extinction coefficient (k) of titanium oxide at corresponding wavelengths for different crystal phases is shown in the figure below. Figure 8 As shown. Compared with rutile, anatase phase exhibits significant absorption of photons that do not trigger UV attenuation in the 390-500nm range, leading to excessive optical loss. Therefore, anatase titanium oxide is preferred as the main component of the UV absorption layer 3.

[0117] As an embodiment of the present invention, the titanium oxide includes anatase phase, and the mass fraction of the anatase phase is greater than or equal to 90%.

[0118] In this embodiment, the mass fraction of the anatase phase in the titanium oxide is further controlled to be greater than or equal to 90%, which further improves the ultraviolet light absorption performance of the titanium oxide, thereby further improving the ultraviolet light absorption performance of the ultraviolet absorption layer 3.

[0119] As an embodiment of the present invention, the titanium oxide includes anatase phase, and the mass fraction of the anatase phase is less than or equal to 98%.

[0120] In this embodiment, the mass fraction of the anatase phase in titanium oxide is controlled to be less than or equal to 98%, so that in addition to the anatase phase, titanium oxide also has other crystalline or amorphous phases. This can form a heterojunction interface. Under ultraviolet light excitation, photogenerated electrons and holes will spatially separate at the heterojunction interface, effectively suppressing the recombination of electron-hole pairs and improving the stability of titanium oxide.

[0121] As an embodiment of the present invention, titanium oxide also includes at least one of rutile phase, brookite phase, and amorphous phase.

[0122] In this embodiment, in addition to the anatase phase, titanium oxide may also include one of the following: rutile phase, brookite phase, and amorphous phase; or two or more of the following: rutile phase, brookite phase, and amorphous phase. The rutile phase, brookite phase, or amorphous phase present in titanium oxide can serve as stress buffer and optical performance adjustment, thereby improving the stability and optical performance of titanium oxide.

[0123] In one embodiment of the present invention, the sum of the mass fractions of rutile phase, brookite phase, and amorphous phase is 2% to 40%. In this embodiment, when titanium oxide includes at least one of rutile phase, brookite phase, and amorphous phase, the sum of the mass fractions of rutile phase, brookite phase, and amorphous phase is controlled to be 2%~40%. Under this ratio, the rutile phase, brookite phase, and amorphous phase can better serve as stress buffers and optical performance regulators, thereby improving the stability and optical performance of titanium oxide and ensuring good ultraviolet light absorption performance of titanium oxide.

[0124] As an embodiment of the present invention, the passivation layer 2 has a thickness of D1, the ultraviolet absorption layer 3 has a thickness of D2, and the ratio of D2 to D1 is greater than or equal to 2.

[0125] In this embodiment, the thickness D2 of the ultraviolet absorption layer 3 is much greater than the thickness D1 of the passivation layer 2, and the ratio of D2 to D1 is greater than or equal to 2. This gives the ultraviolet absorption layer 3 a stronger ability to absorb or reflect high-energy ultraviolet photons, significantly reducing the amount of ultraviolet light reaching the underlying passivation layer 2 and silicon substrate 1, thus improving the resistance of the solar cell 100 to ultraviolet-induced degradation. Furthermore, the thinner passivation layer 2 ensures efficient carrier tunneling and field-effect passivation. Therefore, controlling the ratio of D2 to D1 to be greater than or equal to 2 helps to achieve a balance between the effective blocking of ultraviolet light by the ultraviolet absorption layer 3 and the effective passivation effect of the passivation layer 2. Further, the thickness of the ultraviolet absorption layer 3 is D2, and the ratio of D2 to D1 can be greater than or equal to 3.

[0126] As an embodiment of the present invention, SiN m O n The thickness of layer 42 is greater than that of SiN.x O y The thickness of layer 41.

[0127] In this embodiment, due to SiN x O y For layer 41, x / (x+y) > 50%, SiN m O n The m / (m+n) ratio of layer 42 is less than 50%, which makes SiN m O n The refractive index of layer 42 is higher than that of SiN. x O y Layer 41 has a lower refractive index, requiring a thicker SiN layer. m O n Only layer 42 can achieve an optical retardation effect similar to that of a high-refractive-index inner layer. Furthermore, SiN... x O y Layer 41 is closer to silicon substrate 1, SiN x O y In addition to participating in optical refractive index matching, layer 41 more importantly provides chemical passivation (hydrogen atoms passivate dangling bonds), resulting in a thinner SiN layer. x O y Layer 41 is more conducive to improving its passivation effect. For example, SiN m O n The thickness of layer 42 and SiN x O y The thickness ratio of layer 41 can be 1.1 to 3 times.

[0128] As an embodiment of the present invention, the thickness of the antireflection layer 4 is D3, and the ratio of D3 to D2 is 0.3 to 3.

[0129] In this embodiment, the thickness of the antireflection layer 4 is D3, which is the total thickness of the antireflection layer 4, that is, SiN. x O y Layer 41 and SiN m O nThe sum of the thicknesses of layers 42 is D3. The ratio of the thickness D3 of the antireflection layer 4 to the thickness D2 of the ultraviolet absorption layer 3 is controlled to be between 0.3 and 3. Under the premise of ensuring ultraviolet protection and passivation, a specific thickness matching design is used to minimize the reflection loss of incident light on the battery surface, thereby significantly improving the short-circuit current density and overall photoelectric conversion efficiency of the battery. A ratio of D3 to D2 greater than 0.3 ensures that the antireflection layer 4 is not too thin and loses its optical function. A ratio of D3 to D2 less than 3 avoids the antireflection layer 4 being too thick, which would affect the ultraviolet cutoff function of the underlying ultraviolet absorption layer 3. In this way, the antireflection layer 4 can improve light absorption without weakening the ultraviolet cutoff performance of the ultraviolet absorption layer 3. Specifically, the thickness D3 of the antireflection layer 4 is the average thickness of the antireflection layer 4. Specifically, 10 points can be selected at equal intervals on the antireflection layer 4, and the thickness of the antireflection layer 4 corresponding to the positions of the 10 points can be measured. Then, the average thickness of the antireflection layer 4 corresponding to the positions of the 10 points can be calculated as the thickness D3 of the antireflection layer 4.

[0130] As an embodiment of the present invention, the total thickness of D3 and D2 is less than 150 nanometers.

[0131] In this embodiment, the total thickness of D3 and D2 is controlled to be less than 150 nanometers. While maintaining the good optical performance of the antireflection layer 4 and the ultraviolet absorption layer 3, optical defects caused by excessive total thickness of the antireflection layer 4 and the ultraviolet absorption layer 3 are avoided. This prevents the total thickness from increasing reflectivity and deteriorating the antireflection effect. Moreover, it avoids excessive internal stress caused by excessive film thickness, which could lead to film cracking or peeling, thereby improving the long-term reliability of the film.

[0132] As an embodiment of the present invention, the thickness D3 of the antireflection layer 4 is 30~100 nanometers.

[0133] In this embodiment, the thickness D3 of the antireflection layer 4 is controlled to be 30~100 nanometers to avoid the antireflection layer 4 being too thin, ensuring that the antireflection layer 4 will not be too thin and lose its optical function, and to avoid the antireflection layer 4 being too thick, so as not to affect the ultraviolet cutoff function of the ultraviolet absorption layer 3 below. In this way, the antireflection layer 4 can improve light absorption without weakening the ultraviolet cutoff performance of the ultraviolet absorption layer 3.

[0134] Please refer to Figure 4 As an embodiment of the present invention, a first optical coupling layer 91 is provided between the passivation layer 2 and the ultraviolet absorption layer 3, and the refractive index of the first optical coupling layer 91 is between the refractive index of the passivation layer 2 and the refractive index of the ultraviolet absorption layer 3.

[0135] In this embodiment, a first optical coupling layer 91 is provided between the passivation layer 2 and the ultraviolet absorption layer 3, and the refractive index of the first optical coupling layer 91 is between the refractive index of the passivation layer 2 and the refractive index of the ultraviolet absorption layer 3. This allows sunlight to enter the silicon substrate 1 after passing through the ultraviolet absorption layer 3, the first optical coupling layer 91, and the passivation layer 2, avoiding optical abrupt changes between the passivation layer 2 and the ultraviolet absorption layer 3. This allows sunlight to couple into the silicon substrate 1 with lower loss, thereby effectively increasing the total excitation amount of photogenerated carriers.

[0136] As an embodiment of the present invention, a second optical coupling layer 92 is provided between the ultraviolet absorption layer 3 and the antireflection layer 4, and the refractive index of the second optical coupling layer 92 is between the refractive index of the ultraviolet absorption layer 3 and the refractive index of the antireflection layer 4.

[0137] In this embodiment, a second optical coupling layer 92 is provided between the ultraviolet absorption layer 3 and the antireflection layer 4, and the refractive index of the second optical coupling layer 92 is located between the refractive index of the ultraviolet absorption layer 3 and the refractive index of SiN. x O y Between the refractive indices of layer 41, sunlight passes through SiN m O n Layer 42, SiN x O y After layer 41 and the second optical coupling layer 92, the light enters the ultraviolet absorption layer 3, avoiding optical abrupt changes between the ultraviolet absorption layer 3 and the antireflection layer 4. This allows sunlight to couple into the ultraviolet absorption layer 3 with lower loss, thereby effectively increasing the total amount of photogenerated carriers excited.

[0138] Please refer to Figure 5 As an embodiment of the present invention, the first surface 11 includes an edge region E and an intermediate region F located inside the edge region E, and the thickness D21 of the ultraviolet absorption layer 3 in the edge region E is greater than the thickness D22 of the ultraviolet absorption layer 3 in the intermediate region F.

[0139] In this embodiment of the invention, the edge region E is specifically a region on the first surface 11 whose vertical distance from the edge of the silicon substrate 1 is less than or equal to 2 mm. The edge region E is specifically a ring-shaped region. The middle region F is the region on the first surface 11 excluding the edge region E. Because the edge region E of the silicon substrate 1 of the solar cell 100 has a high defect state density, the edge region E is more prone to photo-induced degradation and accelerated recombination under high-energy ultraviolet light irradiation. Therefore, in this embodiment, by controlling the thickness D21 of the ultraviolet absorption layer 3 in the edge region E to be greater than the thickness D22 of the ultraviolet absorption layer 3 in the middle region F, the ultraviolet absorption performance of the ultraviolet absorption layer 3 in the edge region E is improved. This allows the ultraviolet absorption layer 3 in the edge region E to effectively block and absorb high-energy ultraviolet photons reaching the edge region E, significantly slowing down Si-H bond breaking and hydrogen escape, and reducing ultraviolet-induced degradation in the edge region E. Moreover, the thickened ultraviolet absorption layer 3 enhances the field-effect passivation and chemical passivation effects of the edge region E, effectively suppressing surface recombination caused by high defect state density in the edge region E, thereby significantly improving the battery's ultraviolet resistance and long-term reliability. At the same time, it can reduce the impact of the ultraviolet absorption layer 3 on the light absorption efficiency of the middle region F.

[0140] In this embodiment, the thickness D21 of the ultraviolet absorption layer 3 in the edge region E is the average thickness of the ultraviolet absorption layer 3 in the edge region E. Specifically, 10 points can be taken at equal intervals in the edge region E, and the thickness of the ultraviolet absorption layer 3 at each of the 10 points can be measured. The average thickness of the ultraviolet absorption layer 3 at these 10 points can then be calculated as the thickness D21 of the ultraviolet absorption layer 3 in the edge region E. Similarly, the thickness D22 of the ultraviolet absorption layer 3 in the middle region F is the average thickness of the ultraviolet absorption layer 3 in the middle region F. Specifically, 10 points can be taken at equal intervals in the middle region F, and the thickness of the ultraviolet absorption layer 3 at each of the 10 points can then be measured. The average thickness of the ultraviolet absorption layer 3 at these 10 points can then be calculated as the thickness D22 of the ultraviolet absorption layer 3 in the middle region F.

[0141] In some embodiments, the ratio of the thickness of the ultraviolet absorption layer 3 in the edge region E to the thickness of the ultraviolet absorption layer 3 in the middle region F can be 1.1 to 3. This is beneficial to better improve the ultraviolet absorption performance of the ultraviolet absorption layer 3 in the edge region E, and to better enhance the field effect passivation and chemical passivation effect of the edge region E.

[0142] As an embodiment of the present invention, the ultraviolet absorption layer 3 includes pores.

[0143] In this embodiment, the ultraviolet absorption layer 3 is provided with pores, specifically nanopores. The presence of pores is beneficial to improving the light trapping effect and further enhancing the cutoff effect of the ultraviolet absorption layer 3 on ultraviolet light. The pores in the ultraviolet absorption layer 3 can be cylindrical, conical, spherical, or irregular in shape.

[0144] As an embodiment of the present invention, the first surface 11 includes an edge region E and a middle region F located inside the edge region, and the pore density of the ultraviolet absorption layer 3 in the edge region E is greater than the pore density of the ultraviolet absorption layer 3 in the middle region F.

[0145] In this embodiment, the pore density is specifically the number of pores per unit area. The pore density of the ultraviolet absorption layer 3 in the edge region E is greater than that in the middle region F. That is, for the same area, the number of pores in the ultraviolet absorption layer 3 in the edge region E is greater than the number of pores in the middle region F.

[0146] Because the edge region E of the silicon substrate 1 of the solar cell 100 has a high defect state density, the edge region E is more prone to photo-induced degradation and accelerated recombination under high-energy ultraviolet light irradiation. Therefore, the pore density of the ultraviolet absorption layer 3 in the edge region E is greater than that in the middle region F, which is beneficial to improving the ultraviolet absorption performance of the ultraviolet absorption layer 3 in the edge region E. In some embodiments, the ratio of the pore density of the ultraviolet absorption layer 3 in the edge region E to the pore density in the middle region F can be 1.1 to 3, which is beneficial to further improve the ultraviolet absorption performance of the ultraviolet absorption layer 3 in the edge region E.

[0147] This invention also provides a battery assembly, which includes the solar cell 100 described in the above embodiments. It should be noted that this battery assembly has the same or similar beneficial effects as the solar cell 100 described above, and the related aspects between the two can be referred to each other; to avoid repetition, they will not be repeated here.

[0148] In this embodiment, multiple solar cells 100 in the battery module are connected in series by solder ribbons to form a battery string, thereby realizing the series current collection and output.

[0149] It is understood that in such embodiments, the battery assembly may further include a metal frame, a backsheet, photovoltaic glass, and an encapsulating film. The encapsulating film may be filled between the front and back of the solar cell 100, as well as between the photovoltaic glass and adjacent cells. As a filler, it may be a transparent colloid with good light transmittance and aging resistance. For example, the encapsulating film may be an EVA film or a POE film, and the specific choice can be made according to the actual situation, without limitation.

[0150] Photovoltaic glass can be applied to the encapsulating film on the front side of the solar cell 100. This photovoltaic glass can be ultra-clear glass, possessing high light transmittance, high transparency, and superior physical, mechanical, and optical properties. For example, ultra-clear glass can achieve a light transmittance of over 92%. It can protect the solar cell 100 while minimizing impact on its efficiency. Simultaneously, the encapsulating film bonds the photovoltaic glass and the solar cell 100 together, providing sealing, insulation, and waterproofing / moisture protection for the solar cell 100.

[0151] The backsheet can be attached to the encapsulating film on the back of the solar cell 100. The backsheet provides protection and support for the solar cell 100, offering reliable insulation, water resistance, and aging resistance. Multiple backsheet options are available, typically including tempered glass, acrylic glass, and aluminum alloy TPT composite encapsulating film, etc. The specific choice depends on the specific circumstances and is not limited here. The backsheet, solar cell 100, encapsulating film, and photovoltaic glass can be mounted on a metal frame. The metal frame serves as the main external support structure for the entire battery module, providing stable support and installation. For example, the battery module can be installed at the desired location using the metal frame.

[0152] This invention also provides a photovoltaic system, which includes the battery module described in the above embodiments. It should be noted that this photovoltaic system has the same or similar beneficial effects as the solar cell 100 described above, and the related aspects between the two can be referred to each other; to avoid repetition, they will not be repeated here.

[0153] In this embodiment, the photovoltaic system can be applied in photovoltaic power plants, such as ground-mounted power plants, rooftop power plants, and floating power plants. It can also be applied to equipment or devices that utilize solar energy to generate electricity, such as user solar power supplies, solar streetlights, solar cars, and solar buildings. Of course, it is understood that the application scenarios of the photovoltaic system are not limited to these; that is, the photovoltaic system can be applied in all fields that require solar energy to generate electricity. Taking a photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a combiner box, and an inverter. The photovoltaic array may be an array combination of multiple battery modules; for example, multiple battery modules can form multiple photovoltaic arrays. The photovoltaic array is connected to the combiner box, which can collect the current generated by the photovoltaic array. The collected current flows through the inverter and is converted into AC power required by the mains power grid before being connected to the mains power grid to achieve solar power supply.

[0154] In the description of this specification, references to terms such as "some embodiments," "illustrative embodiments," "examples," "specific examples," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with an embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0155] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A solar cell, characterized in that, include: A silicon substrate, the silicon substrate including a first surface; A passivation layer is provided on the first surface; An ultraviolet absorption layer is disposed on the passivation layer, wherein the material of the ultraviolet absorption layer includes titanium oxide; and An antireflection layer disposed on the ultraviolet absorption layer, the antireflection layer comprising stacked SiN x O y Layers and SiN m O n Layer, the SiN x O y Compared to the SiN layer m O n The layer is closer to the ultraviolet absorption layer, the SiN x O y The layer satisfies: x / (x+y)>50%; the SiN m O n The layer satisfies: m / (m+n) < 50%; the difference between x / (x+y) and m / (m+n) is d, and d ≥ 1%.

2. The solar cell according to claim 1, characterized in that, x / (x+y)≥55%.

3. The solar cell according to claim 1, characterized in that, x / (x+y)≥60%.

4. The solar cell according to claim 1, characterized in that, m / (m+n)≤45%.

5. The solar cell according to claim 1, characterized in that, m / (m+n)≤40%.

6. The solar cell according to claim 1, characterized in that, d≥5%。 7. The solar cell according to claim 1, characterized in that, d≥10%。 8. The solar cell according to claim 1, characterized in that, The general chemical formula of the titanium oxide is TiO. b The value of b ranges from 1.8 to 2.

2.

9. The solar cell according to claim 1, characterized in that, The SiN m O n The thickness of the layer is greater than that of the SiN x O y The thickness of the layer.

10. The solar cell according to claim 1, characterized in that, The titanium oxide comprises anatase phase, and the mass fraction of the anatase phase is greater than or equal to 60%.

11. The solar cell according to claim 1, characterized in that, The titanium oxide comprises anatase phase, and the mass fraction of the anatase phase is greater than or equal to 90%.

12. The solar cell according to claim 10 or 11, characterized in that, The titanium oxide comprises anatase phase, and the mass fraction of the anatase phase is less than or equal to 98%.

13. The solar cell according to claim 10, characterized in that, The titanium oxide also includes at least one of the following: rutile phase, brookite phase, and amorphous phase.

14. The solar cell according to claim 13, characterized in that, The sum of the mass fractions of the rutile phase, the brookite phase, and the amorphous phase is 2% to 40%.

15. The solar cell according to claim 1, characterized in that, The passivation layer has a thickness of 2 to 10 nanometers.

16. The solar cell according to claim 1, characterized in that, The thickness of the ultraviolet absorption layer is 10~70 nanometers.

17. The solar cell according to claim 1, characterized in that, The thickness of the antireflective layer is 30~100 nanometers.

18. The solar cell according to claim 1, characterized in that, The extinction coefficient of the ultraviolet absorption layer for light with wavelengths of 390~780 nm is less than 0.1, and the extinction coefficient of the ultraviolet absorption layer for ultraviolet light with wavelengths less than or equal to 320 nm is greater than 0.

1.

19. The solar cell according to claim 1, characterized in that, The passivation layer comprises one or more of the following: a silicon oxide layer, an aluminum oxide layer, a silicon oxynitride layer, a silicon nitride layer, and a hafnium oxide layer.

20. The solar cell according to claim 1, characterized in that, The passivation layer includes a first sub-passivation layer and a second sub-passivation layer stacked on the first sub-passivation layer, wherein the second sub-passivation layer is located between the first sub-passivation layer and the ultraviolet absorption layer.

21. The solar cell according to claim 20, characterized in that, The first sub-passivation layer is a silicon oxide layer, and the second sub-passivation layer is at least one of an aluminum oxide layer, a silicon nitride layer, and a silicon oxynitride layer.

22. The solar cell according to claim 20, characterized in that, The thickness of the first sub-passivation layer is 0.1~2 nanometers, and the thickness of the second sub-passivation layer is 0.5~8 nanometers.

23. A battery assembly, characterized in that, Includes the solar cell according to any one of claims 1 to 22.

24. A photovoltaic system, characterized in that, Includes the battery assembly as described in claim 23.