Photovoltaic cells, their preparation methods and photovoltaic modules

By optimizing the thickness of the intrinsic layer and doped layer on the side of the heterojunction cell, a passivation structure with optimized thickness is formed, which solves the problem of recombination at the side edge of the cell and improves the cell efficiency and reliability.

CN123124514APending Publication Date: 2026-11-17嘉兴阿特斯阳光能源科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611477800.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The recombination problem at the side edge of existing heterojunction solar cells limits the improvement of cell efficiency. Too thin an intrinsic layer has a weak passivation effect, while too thick a doped layer increases edge leakage.

Method used

The thickness of the intrinsic layer and doped layer on the side of the battery is optimized to form a thicker intrinsic stack and a thinner doped stack. The film thickness is controlled by PECVD process to ensure that an optimized passivation structure is formed on the side of the substrate.

Benefits of technology

It improves the passivation effect on the battery side, reduces edge leakage, and enhances the battery's photoelectric conversion efficiency and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124514A_ABST
    Figure CN123124514A_ABST
Patent Text Reader

Abstract

This application discloses a photovoltaic cell, its fabrication method, and a photovoltaic module. The photovoltaic cell includes: a substrate, the substrate including a substrate surface and a plurality of substrate side surfaces, the substrate surface including a first surface and a second surface disposed opposite to each other; a first intrinsic layer and a second intrinsic layer, the first intrinsic layer and the second intrinsic layer overlapping at least one substrate side surface to form an intrinsic stack; a first doped layer and a second doped layer, the first doped layer and the second doped layer overlapping at least one substrate side surface to form a doped stack; a first electrode and a second electrode; wherein, in at least a portion of the overlapping region on the substrate side surface, the thickness of the intrinsic stack is greater than the thickness of the doped stack, so as to improve the side passivation effect and reduce edge leakage current. This application improves the side passivation effect and reduces edge leakage current by optimizing the substrate side surface film layer, forming a thicker intrinsic layer and a thinner doped layer on the substrate side surface, thereby improving the cell efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of photovoltaic cell technology, specifically relating to a photovoltaic cell, its preparation method, and a photovoltaic module. Background Technology

[0002] Heterojunction (HJT) solar cells are a hybrid type of solar cell made using crystalline silicon wafers and amorphous silicon layers. By passivating the surface of the amorphous silicon layer, its open-circuit voltage is significantly higher than that of conventional crystalline silicon solar cells, resulting in superior performance. It has many advantages such as simple fabrication process, low processing temperature, high open-circuit voltage, high photoelectric conversion efficiency, and low temperature coefficient, and is one of the most widely used high-efficiency crystalline silicon solar cell technologies.

[0003] As battery efficiency continues to improve, it has reached a bottleneck, leading to increased concern about edge recombination. To further enhance battery efficiency, passivation of the silicon wafer sides is crucial. When intrinsic and doped layers are used for passivation, a thin intrinsic layer provides weak passivation, while an excessively thick doped layer exacerbates edge leakage.

[0004] Therefore, it is necessary to provide a photovoltaic cell, its preparation method, and a photovoltaic module. Summary of the Invention

[0005] The purpose of this application is to provide a photovoltaic cell, its preparation method and photovoltaic module, which improves the side passivation effect and reduces edge leakage by optimizing the intrinsic layer and doped layer on the side of the cell.

[0006] The above-mentioned objective of this application is achieved through the following technical solution:

[0007] In a first aspect, this application provides a photovoltaic cell, the photovoltaic cell comprising:

[0008] A substrate, the substrate including a substrate surface and a plurality of substrate side surfaces, the substrate surface including a first surface and a second surface disposed opposite to each other;

[0009] A first intrinsic layer and a second intrinsic layer, wherein the first intrinsic layer is located on a first surface or a second surface of the substrate, the second intrinsic layer is located on a first surface or a second surface of the substrate, and the first intrinsic layer and the second intrinsic layer overlap at least one side of the substrate to form an intrinsic stack.

[0010] A first doped layer and a second doped layer, wherein the first doped layer is located on the first intrinsic layer, the second doped layer is located on the second intrinsic layer, and the first doped layer and the second doped layer overlap at least one side of a substrate to form a doped stack, wherein the first doped layer has the same doping type as the substrate, and the second doped layer has the opposite doping type to the substrate;

[0011] The first electrode and the second electrode are in electrical contact, the first electrode is in electrical contact with the first doped layer, and the second electrode is in electrical contact with the second doped layer;

[0012] In at least a portion of the overlapping region on the side of the substrate, the thickness of the intrinsic stack is greater than the thickness of the doped stack.

[0013] In one or more embodiments of this application, the thickness of the intrinsic stack is 3 nm to 6 nm in at least a portion of the overlapping region on the side surface of the substrate; and / or,

[0014] In at least a portion of the overlapping region on the side of the substrate, the thickness of the doped stack is 1 nm to 2.5 nm.

[0015] In one or more embodiments of this application, the total thickness of the first intrinsic layer and the second intrinsic layer along the substrate thickness direction is less than the total thickness of the first doped layer and the second doped layer along the substrate thickness direction.

[0016] In one or more embodiments of this application, the total thickness of the first intrinsic layer and the second intrinsic layer along the substrate thickness direction is 9 nm to 13.5 nm; and / or,

[0017] The total thickness of the first doped layer and the second doped layer along the thickness direction of the substrate is 45 nm to 65 nm.

[0018] In one or more embodiments of this application, the first intrinsic layer on the substrate surface and the substrate side surface is prepared by a one-step deposition process, the thickness of the first intrinsic layer on the substrate surface along the substrate thickness direction is 4 nm to 6.5 nm, and the thickness of the first intrinsic layer in the intrinsic stack is 0.5 nm to 3 nm; and / or,

[0019] The second intrinsic layer on the substrate surface and the substrate side surface is prepared by a one-step deposition process. The thickness of the second intrinsic layer on the substrate surface is 5nm~7nm, and the thickness of the second intrinsic layer in the intrinsic stack is 0.5nm~3nm.

[0020] In one or more embodiments of this application, the first doped layer on the substrate surface and the substrate side surface is prepared by a one-step deposition process, wherein the thickness of the first doped layer on the substrate surface is 20 nm to 30 nm, and the thickness of the first doped layer on the substrate side surface is 0.5 nm to 1.5 nm; and / or,

[0021] The second doped layer on the substrate surface and the substrate side surface is prepared by a one-step deposition process. The thickness of the second doped layer on the substrate surface is 25nm~35nm, and the thickness of the second doped layer on the substrate side surface is 0.5nm~1nm.

[0022] In one or more embodiments of this application, the second intrinsic layer, the first intrinsic layer, the first doped layer, and the second doped layer are sequentially stacked along a direction away from the side surface of the substrate; or,

[0023] The first intrinsic layer, the second intrinsic layer, the first doped layer, and the second doped layer are stacked sequentially in a direction away from the side surface of the substrate.

[0024] In one or more embodiments of this application, the first intrinsic layer and the second intrinsic layer are located on the first surface and the second surface of the substrate, respectively; or,

[0025] Both the first intrinsic layer and the second intrinsic layer are located on the first surface or the second surface of the substrate.

[0026] In one or more embodiments of this application, the first intrinsic layer is an intrinsic amorphous silicon layer; and / or,

[0027] The second intrinsic layer is an intrinsic amorphous silicon layer; and / or,

[0028] The first doped layer is any one of amorphous silicon, microcrystalline silicon, or nanocrystalline silicon; and / or,

[0029] The second doped layer is any one of amorphous silicon doped layer, microcrystalline silicon doped layer, or nanocrystalline silicon doped layer; and / or,

[0030] The substrate is an N-type crystalline silicon substrate, the first doped layer is an N-type doped layer, and the second doped layer is a P-type doped layer; and / or,

[0031] The surface of the substrate has a light-trapping velvet structure.

[0032] In one or more embodiments of this application, the photovoltaic cell further includes:

[0033] A first transparent conductive layer and a second transparent conductive layer, wherein the first transparent conductive layer is at least partially located on the first doped layer, and the second transparent conductive layer is at least partially located on the second doped layer.

[0034] In one or more embodiments of this application, the first transparent conductive layer or the second transparent conductive layer covers the doped stack on the sidewall of the substrate.

[0035] In one or more embodiments of this application, the thickness of the first transparent conductive layer on the substrate surface is 60 nm to 120 nm; and / or,

[0036] The thickness of the second transparent conductive layer on the substrate surface is 60nm~120nm; and / or,

[0037] The thickness of the first or second transparent conductive layer on the side of the substrate is 3nm to 6nm.

[0038] In one or more embodiments of this application, the first transparent conductive layer and the second transparent conductive layer are transparent conductive oxide layers, and the oxygen concentration of each film layer on the side of the substrate gradually increases in the direction away from the side of the substrate.

[0039] A second aspect of this application provides a method for preparing a photovoltaic cell, the method comprising the following steps:

[0040] A substrate is provided, the substrate including a substrate surface and a substrate side surface, the substrate surface including a first surface and a second surface disposed opposite to each other;

[0041] A first intrinsic layer is deposited on the substrate surface and the substrate sidewalls, and a second intrinsic layer is deposited on the substrate surface and the substrate sidewalls. The first and second intrinsic layers are deposited using a PECVD process with a power density of 100 W / m². 2 ~600W / m 2 The first intrinsic layer and the second intrinsic layer overlap at at least one side of the substrate to form an intrinsic stack;

[0042] A first doped layer is deposited on the first intrinsic layer on the substrate surface and the substrate side surface, and a second doped layer is deposited on the second intrinsic layer on the substrate surface and the substrate side surface. The first doped layer and the second doped layer overlap at at least one substrate side surface to form a doped stack. The first doped layer and the second doped layer are deposited using a PECVD process with a power density of 1500 W / m². 2 ~5000W / m 2 ;

[0043] A first electrode that is in electrical contact with the first doped layer is prepared on the first doped layer, and a second electrode that is in electrical contact with the second doped layer is prepared on the second doped layer.

[0044] In at least a portion of the overlapping region on the side of the substrate, the thickness of the intrinsic stack is greater than the thickness of the doped stack.

[0045] In one or more embodiments of this application, in the PECVD process for depositing the first intrinsic layer, an RF power source is used to excite the plasma at a power density of 100 W / m². 2 ~600W / m 2 The introduced gas is silane and hydrogen, with a silane to hydrogen flow rate ratio of 1:(1~5), a chamber pressure of 0.4 Torr~0.7 Torr, a first intrinsic layer thickness of 4 nm~6.5 nm on the substrate surface, and a first intrinsic layer thickness of 0.5 nm~3 nm on the substrate side surface; and / or,

[0046] In the PECVD process for depositing the second intrinsic layer, an RF power source was used to excite the plasma at a power density of 100 W / m². 2 ~500W / m 2 The introduced gas is silane and hydrogen, with a silane to hydrogen flow rate ratio of 1:(1~20), a chamber pressure of 0.4 Torr~0.7 Torr, a second intrinsic layer thickness of 5 nm~7 nm on the substrate surface, and a second intrinsic layer thickness of 0.5 nm~3 nm on the substrate side surface; and / or,

[0047] In the PECVD process for depositing the first doped layer, a VHF power supply was used to excite the plasma, with a power density of 1500 W / m². 2 ~5000W / m 2 The introduced gas is silane, hydrogen, and a first dopant gas. The flow rate ratio of silane to hydrogen is 1:(150~300), and the flow rate ratio of the first dopant gas to silane is 1:(2~4). The chamber pressure is 3 Torr~6 Torr. The thickness of the first doped layer on the substrate surface is 20nm~30nm, and the thickness of the first doped layer on the side surface of the substrate is 0.5nm~1.5nm; and / or,

[0048] In the PECVD process for depositing the second doped layer, a VHF power supply was used to excite the plasma at a power density of 3000 W / m. 2 ~5000W / m 2 The introduced gas is silane, hydrogen, and a second doped gas. The flow rate ratio of silane to hydrogen is 1:(150~350), and the flow rate ratio of the second doped gas to silane is 1:(0.5~5). The chamber pressure is 3 Torr~5 Torr. The thickness of the second doped layer on the substrate surface is 25nm~35nm, and the thickness of the second doped layer on the side surface of the substrate is 0.5nm~1nm.

[0049] In one or more embodiments of this application, during the PECVD process for depositing the first intrinsic layer and / or the second intrinsic layer, the substrate sidewalls are exposed to increase the thickness of the first intrinsic layer and / or the second intrinsic layer on the substrate sidewalls.

[0050] In one or more embodiments of this application, a first intrinsic layer is deposited on a first surface and a side surface of the substrate, and a second intrinsic layer is deposited on a second surface and a side surface of the substrate;

[0051] A first doped layer is deposited on the first intrinsic layer on the first surface and side surface of the substrate, and a second doped layer is deposited on the second intrinsic layer on the second surface and side surface of the substrate.

[0052] In one or more embodiments of this application, the first doped layer is deposited prior to the second doped layer; and / or,

[0053] The second intrinsic layer is deposited before the first intrinsic layer.

[0054] In one or more embodiments of this application, the preparation method further includes:

[0055] A first transparent conductive layer is deposited on the first doped layer on the substrate surface and the substrate side surface, wherein the thickness of the first transparent conductive layer on the substrate surface is 60 nm to 120 nm, and the thickness of the first transparent conductive layer on the substrate side surface is 3 nm to 6 nm; and / or,

[0056] A second transparent conductive layer is deposited on the second doped layer on the surface of the substrate, and the thickness of the second transparent conductive layer on the surface of the substrate is 60 nm to 120 nm.

[0057] In a third aspect, this application provides a photovoltaic module comprising a plurality of battery strings, wherein the battery strings include the aforementioned photovoltaic cells.

[0058] Compared with the prior art, this application improves the passivation effect of the side surface and reduces edge leakage by optimizing the film layer on the side surface of the substrate, thereby improving the battery efficiency. Attached Figure Description

[0059] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0060] Figure 1 This is a schematic diagram of the structure of a photovoltaic cell in the prior art;

[0061] Figure 2 This is a schematic diagram of the structure of a photovoltaic cell in one embodiment of this application;

[0062] Figure 3 for Figure 2 A magnified view of a section at point A in the middle;

[0063] Figure 4 for Figure 2 A magnified view of a section at point B in the middle;

[0064] Figure 5 for Figure 2 A magnified view of a section at point C;

[0065] Figure 6 This is a top view of the first carrier plate in one embodiment of this application;

[0066] Figure 7 This is a side view of the first carrier plate in one embodiment of this application;

[0067] Figure 8 This is a top view of the second carrier plate in one embodiment of this application;

[0068] Figure 9 This is a side view of the third carrier plate in one embodiment of this application;

[0069] Figure 10 This is a topographic view of the side surface of the substrate in one embodiment of this application.

[0070] Explanation of key figure labels:

[0071] 10', 10 - substrate; 21', 21, 211, 212 - first intrinsic layer; 22', 22, 221, 222 - second intrinsic layer; 31', 31, 311, 312 - first doped layer; 32', 32, 321, 322 - second doped layer; 41', 41, 411, 412 - first transparent conductive layer; 42', 42 - second transparent conductive layer; 51', 51 - first electrode; 52', 52 - second electrode.

[0072] 60-First carrier plate, 61-First frame, 62-First support member, 63-Limiting member, 70-Second carrier plate, 71-Second frame, 711-Receiving part, 72-Second support member. Detailed Implementation

[0073] To enable those skilled in the art to better understand the technical solutions in the present disclosure, the following will clearly and completely describe the technical solutions in the embodiments of the present disclosure in conjunction with the accompanying drawings in the embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all of them. Based on the embodiments of the present disclosure, all other embodiments obtained by a person of ordinary skill in the art without creative work shall fall within the protection scope of the present disclosure.

[0074] In the present application, unless otherwise explicitly specified and defined, a first feature being "on" or "under" a second feature may mean that the first and second features are in direct contact, or that the first and second features are in indirect contact via an intermediate medium. Moreover, the first feature being "above", "over" and "on" the second feature may mean that the first feature is directly or obliquely above the second feature, or merely indicates that the horizontal height of the first feature is higher than that of the second feature. The first feature being "below", "beneath" and "under" the second feature may mean that the first feature is directly or obliquely below the second feature, or merely indicates that the horizontal height of the first feature is lower than that of the second feature.

[0075] In the present application, unless otherwise explicitly specified and defined, the disclosed "range" is defined in the form of lower and / or upper limits, a given range is defined by selecting one lower limit and / or one upper limit, and the selected lower limit and / or upper limit defines the boundaries of the specific range. A range defined in this manner may be inclusive or exclusive of endpoints, and may be arbitrarily combined, that is, any lower limit may be combined with any upper limit to form a range not explicitly stated, any lower limit may be combined with other lower limits to form a range not explicitly stated, and similarly any upper limit may be combined with any other upper limit to form a range not explicitly stated. In addition, each individually disclosed point or single value may itself serve as a lower or upper limit to combine with any other point or single value, or combine with other lower or upper limits to form a range not explicitly stated.

[0076] In the present application, the term "and / or" is merely an association relationship describing associated objects, indicating that three relationships may exist. For example, A and / or B may represent: the presence of A alone, the co-presence of A and B, and the presence of B alone. In addition, the character " / " in this text generally indicates that the associated objects before and after are in an "or" relationship.

[0077] In the present application, unless otherwise explicitly specified and defined, all embodiments and optional embodiments, or all technical features and optional technical features may be combined with each other to form new technical solutions, and such technical solutions shall be deemed to be included in the disclosure content of the present application.

[0078] Reference Figure 1 as shown, the photovoltaic cell in the prior art comprises:

[0079] The substrate 10' includes a substrate surface and a plurality of substrate side surfaces (or side surfaces), the substrate surface including a first surface and a second surface disposed opposite to each other;

[0080] The first intrinsic layer 21' and the second intrinsic layer 22' are located on the first surface and the second surface of the substrate 10', respectively, and the first intrinsic layer and the second intrinsic layer overlap on at least one side of the substrate to form an intrinsic stack.

[0081] The first doped layer 31' and the second doped layer 32' are located on the first intrinsic layer 21' and the second doped layer 32' is located on the second intrinsic layer 22'. The first doped layer 31' has the same doping type as the substrate 10' and the second doped layer 32' has the opposite doping type to the substrate 10'.

[0082] A first transparent conductive layer 41' and a second transparent conductive layer 42', wherein the first transparent conductive layer 41' is located on the first doped layer 31' and the second transparent conductive layer 42' is located on the second doped layer 32';

[0083] The first electrode 51' and the second electrode 52' are located on the first transparent conductive layer 41' and are in electrical contact with the first doped layer 31'. The second electrode 52' is located on the second transparent conductive layer 42' and is in electrical contact with the second doped layer 32'.

[0084] For example, the substrate 10' is an N-type silicon substrate; the first intrinsic layer 21' and the second intrinsic layer 22' are both intrinsic amorphous silicon layers; the first doped layer 31' is an N-type doped amorphous silicon layer or a microcrystalline silicon layer; the second doped layer 32' is a P-type doped amorphous silicon layer or a microcrystalline silicon layer; the first transparent conductive layer 41' and the second transparent conductive layer 42' are both TCO (Transparent Conductive Oxides) layers; the first electrode 51' and the second electrode 52' are both gate electrodes.

[0085] In existing photovoltaic cells, the sides are not passivated, which leads to edge recombination on the sides of the cell, thus affecting further improvement of cell efficiency.

[0086] Based on existing photovoltaic cells, a passivation stack consisting of an intrinsic layer and a doped layer can be further formed on the side of the substrate 10' to passivate the side of the cell and improve cell efficiency. The side intrinsic layer can be formed simultaneously during the deposition of the first intrinsic layer 21' and the second intrinsic layer 22', and the side doped layer can be formed simultaneously during the deposition of the first doped layer 31' and the second doped layer 32'.

[0087] However, the thickness of the intrinsic layer on the surface of the photovoltaic cell is much smaller than the thickness of the doped layer. For example, the thickness of the first intrinsic layer 21' is 4 nm to 6.5 nm, the thickness of the second intrinsic layer 22' is 5 nm to 7 nm, the thickness of the first doped layer 31' is 20 nm to 30 nm, and the thickness of the second doped layer 32' is 25 nm to 35 nm. In the passivation film layer formed by synchronous deposition on the side surface, the thickness of the side intrinsic layer will be much smaller than the thickness of the doped layer. An excessively thin intrinsic layer has a weak passivation effect on the side surface, and an excessively thick doped layer will aggravate edge leakage current.

[0088] In view of the above problems, the applicant optimizes the structure and preparation method of the side passivation stack to form a relatively thick intrinsic layer and a relatively thin doped layer on the side surface of the substrate, so as to improve the passivation effect on the side surface and reduce edge leakage current.

[0089] Taking the heterojunction cell as an example, the present application can overcome the inherent defect of "thin intrinsic layer and thick doped layer" on the side surface caused by the deposition of the front and back film layers of the heterojunction cell. By optimizing the structural thickness of the side film layers, the side passivation effect and the suppression of edge leakage current can be both achieved, and the photoelectric conversion efficiency and reliability of the cell are improved.

[0090] Reference Figure 2 in conjunction with Figures 3 to 5 shown in the drawings, the present application provides a photovoltaic cell, which comprises:

[0091] a substrate 10, wherein the substrate 10 comprises a substrate surface and a plurality of substrate side surfaces (also referred to as side surfaces), and the substrate surface comprises a first surface (i.e., front surface or light-receiving surface) and a second surface (i.e., back surface or backlight surface) arranged opposite to each other;

[0092] a first intrinsic layer 21 and a second intrinsic layer 22, wherein the first intrinsic layer 21 and the second intrinsic layer 22 are respectively located on the first surface and the second surface of the substrate, and the first intrinsic layer 21 and the second intrinsic layer 22 overlap on at least one side surface of the substrate to form an intrinsic stack;

[0093] a first doped layer 31 and a second doped layer 32, wherein the first doped layer 31 is located on the first intrinsic layer 21, the second doped layer 32 is located on the second intrinsic layer 22, the first doped layer 31 and the second doped layer 32 overlap on at least one side surface of the substrate 10 to form a doped stack, the doping type of the first doped layer 31 is the same as that of the substrate 10, and the doping type of the second doped layer 32 is opposite to that of the substrate 10;

[0094] a first electrode 51 and a second electrode 52, wherein the first electrode 51 is in electrical contact with the first doped layer 31, and the second electrode 52 is in electrical contact with the second doped layer 32.

[0095] In some embodiments of the present application, the photovoltaic cell further includes: a first transparent conductive layer 41 and a second transparent conductive layer 42. The first transparent conductive layer 41 is at least partially located on the first doped layer 31 on the first surface of the substrate 10, and the second transparent conductive layer 42 is at least partially located on the second doped layer 32 on the second surface of the substrate 10.

[0096] In some embodiments of the present application, the material of the substrate 10 may be at least one of monocrystalline silicon, polycrystalline silicon, amorphous silicon, or microcrystalline silicon. Taking an N-type substrate as an example, the substrate 10 is doped with an N-type doping element. The N-type doping element may be at least one of Group V elements such as phosphorus (P), bismuth (Bi), antimony (Sb), or arsenic (As). Preferably, the substrate 10 is a monocrystalline silicon substrate doped with phosphorus element.

[0097] In other embodiments of the present application, the substrate 10 may also be a P-type substrate. In this case, the substrate 10 is doped with a P-type doping element, and the P-type doping element may be at least one of Group III elements such as boron (B), indium (In), or gallium (Ga).

[0098] In the present application, the first surface, the second surface and the side surface of the substrate 10 may be polished surfaces, or may be light-trapping textured structures. For example, an alkali texturing process may be used to form a pyramid textured structure on the first surface, the second surface and the side surface of the substrate 10.

[0099] In some embodiments of the present application, the first intrinsic layer 21 and the second intrinsic layer 22 may be intrinsic amorphous silicon layers or intrinsic hydrogenated amorphous silicon layers, and may also be intrinsic microcrystalline silicon layers or intrinsic hydrogenated microcrystalline silicon layers. The intrinsic layers mainly function for surface passivation.

[0100] Reference Figure 2 in conjunction with Figures 3 to 5 as shown, the first intrinsic layer 21 includes a first intrinsic layer 211 located on the first surface of the substrate 10 and a first intrinsic layer 212 located on the side surface of the substrate 10. The second intrinsic layer 22 includes a second intrinsic layer 221 located on the second surface of the substrate 10 and a second intrinsic layer 222 located on the side surface of the substrate 10. The first intrinsic layer 212 on the side surface of the substrate 10 and the second intrinsic layer 222 on the side surface of the substrate 10 are stacked to form an intrinsic stack. The thicknesses of the first intrinsic layer 211 and the second intrinsic layer 221 refer to the thicknesses along the thickness direction of the substrate 10. The thicknesses of the first intrinsic layer 212, the second intrinsic layer 222 and the intrinsic stack refer to the thicknesses in at least a partial overlapping region on the side surface of the substrate 10.

[0101] It is worth noting that when the first surface or the second surface of the substrate 10 is a polished surface, the thickness direction is the direction perpendicular to the first surface or the second surface; when the first surface or the second surface of the substrate 10 is a light-trapping textured surface, the thickness direction is the direction perpendicular to the textured surface. Similarly, when the side surface of the substrate 10 is a polished surface, the thickness direction is the direction perpendicular to the side surface; when the side surface of the substrate 10 is a light-trapping textured surface, the thickness direction is the direction perpendicular to the textured surface.

[0102] In some embodiments, the first intrinsic layer 212 is stacked on the second intrinsic layer 222 in a direction away from the side surface of the substrate 10, and the second intrinsic layer 222 is directly stacked on the side surface of the substrate 10. In other embodiments, the positions of the first intrinsic layer 212 and the second intrinsic layer 222 on the side surface of the substrate 10 may be reversed, that is, the second intrinsic layer 222 is stacked on the first intrinsic layer 212 in a direction away from the side surface of the substrate 10, and the first intrinsic layer 212 is directly stacked on the side surface of the substrate 10.

[0103] Ref Figure 3 erence Figure 4 as shown, in the present application, the thickness of the first intrinsic layer 211 located on the first surface of the substrate 10 is H11, the thickness of the first intrinsic layer 212 located on the side surface of the substrate 10 is H12, the thickness of the second intrinsic layer 221 located on the second surface of the substrate 10 is H21, and the thickness of the second intrinsic layer 222 located on the side surface of the substrate 10 is H22.

[0104] Wherein, the total thickness H11+H21 of the first intrinsic layer 211 and the second intrinsic layer 221 along the thickness direction of the substrate 10 is 9 nm to 13.5 nm, for example, may be 9 nm, 9.5 nm, 10 nm, 10.5 nm, 11 nm, 11.5 nm, 12 nm, 12.5 nm, 13 nm or 13.5 nm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable. The thickness H12+H22 of the intrinsic stack on the side surface of the substrate 10 is 3 nm to 6 nm, for example, may be 3 nm, 3.5 nm, 4 nm, 4.5 nm, 5 nm, 5.5 nm or 6 nm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.

[0105] In some preferred embodiments, the first intrinsic layer 211 on the first surface of the substrate 10 and the first intrinsic layer 212 on the side surface are prepared by a one-step deposition process, for example, a PECVD (Plasma Enhanced Chemical Vapor Deposition) process. The thickness H11 of the first intrinsic layer 211 on the first surface of the substrate 10 is 4 nm to 6.5 nm, which may be, for example, 4 nm, 4.5 nm, 5 nm, 5.5 nm, 6 nm or 6.5 nm, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable; the thickness H12 of the first intrinsic layer 212 on the side surface of the substrate 10 is 0.5 nm to 3 nm, which may be, for example, 0.5 nm, 1 nm, 1.5 nm, 2 nm, 2.5 nm or 3 nm, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.

[0106] In some preferred embodiments, the second intrinsic layer 221 on the second surface of the substrate 10 and the second intrinsic layer 222 on the side surface are prepared by a one-step deposition process, for example, a PECVD (Plasma Enhanced Chemical Vapor Deposition) process. The thickness H21 of the second intrinsic layer 221 on the second surface of the substrate 10 is 5 nm to 7 nm, which may be, for example, 5 nm, 5.5 nm, 6 nm, 6.5 nm or 7 nm, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable; the thickness H22 of the second intrinsic layer 222 on the side surface of the substrate 10 is 0.5 nm to 3 nm, which may be, for example, 0.5 nm, 1 nm, 1.5 nm, 2 nm, 2.5 nm or 3 nm, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.

[0107] In the present application, the thickness of the intrinsic stack on the side surface of the substrate 10 is controlled to be in the range of 3 nm to 6 nm, so that the intrinsic stack can provide a sufficient amount of hydrogen element, which can passivate the silicon dangling bonds on the side surface of the substrate, thereby improving the side surface passivation effect.

[0108] In some embodiments of the present application, the first doped layer 31 may be an N-type doped amorphous silicon layer, an N-type doped microcrystalline silicon layer, or an N-type doped nanocrystalline silicon layer, and the N-type doping element may be at least one of Group V elements such as phosphorus (P), bismuth (Bi), antimony (Sb) or arsenic (As). The second doped layer 32 may be a P-type doped amorphous silicon layer, a P-type doped microcrystalline silicon layer, or a P-type doped nanocrystalline silicon layer, and the P-type doping element may be at least one of Group III elements such as boron (B), indium (In) or gallium (Ga).

[0109] Reference Figure 2 in conjunction with Figures 3 to 5As shown, the first doped layer 31 includes a first doped sub-layer 311 located on the first surface of the substrate 10 and a first doped sub-layer 312 located on the side surface of the substrate 10, the second doped layer 32 includes a second doped sub-layer 321 located on the second surface of the substrate 10 and a second doped sub-layer 322 located on the side surface of the substrate 10, and the first doped sub-layer 312 on the side surface of the substrate 10 and the second doped sub-layer 322 on the side surface of the substrate 10 are stacked to form a doped stack. The thicknesses of the first doped sub-layer 311 and the second doped sub-layer 321 refer to the thicknesses along the thickness direction of the substrate 10, and the thicknesses of the first doped sub-layer 312, the second doped sub-layer 322 and the doped stack refer to the thicknesses in at least a partial overlapping region on the side surface of the substrate 10.

[0110] In some embodiments, the second doped sub-layer 322 is stacked on the first doped sub-layer 312 in a direction away from the side surface of the substrate 10, and the first doped sub-layer 312 is stacked on the intrinsic stack.

[0111] Reference Figure 3 and Figure 4 as shown, in the present application, the thickness of the first doped sub-layer 311 located on the first surface of the substrate 10 is H31, the thickness of the first doped sub-layer 312 located on the side surface of the substrate 10 is H32, the thickness of the second doped sub-layer 321 located on the second surface of the substrate 10 is H41, and the thickness of the second doped sub-layer 322 located on the side surface of the substrate 10 is H42.

[0112] Wherein, the total thickness H31+H41 of the first doped sub-layer 311 and the second doped sub-layer 321 along the thickness direction of the substrate 10 is 45 nm to 65 nm, for example, may be 45 nm, 50 nm, 55 nm, 60 nm or 65 nm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable. The thickness H32+H42 of the doped stack on the side surface of the substrate 10 is 1 nm to 2.5 nm, for example, may be 1 nm, 1.5 nm, 2 nm or 2.5 nm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.

[0113] In some preferred embodiments, the first doped layer 311 on the first surface of the substrate 10 and the first doped layer 312 on the side surface are prepared by a one-step deposition process, for example, a PECVD (Plasma Enhanced Chemical Vapor Deposition) process. The thickness H31 of the first doped layer 311 on the first surface of the substrate 10 is 20 nm to 30 nm, which may be, for example, 20 nm, 22 nm, 24 nm, 26 nm, 28 nm or 30 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable; the thickness H32 of the first doped layer 312 on the side surface of the substrate 10 is 0.5 nm to 1.5 nm, which may be, for example, 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, 1 nm or 1.5 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.

[0114] In some preferred embodiments, the second doped layer 321 on the second surface of the substrate 10 and the second doped layer 322 on the side surface are prepared by a one-step deposition process, for example, a PECVD (Plasma Enhanced Chemical Vapor Deposition) process. The thickness H41 of the second doped layer 321 on the second surface of the substrate 10 is 25 nm to 35 nm, which may be, for example, 25 nm, 27 nm, 29 nm, 30 nm, 31 nm, 33 nm or 35 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable; the thickness H42 of the second doped layer 322 on the side surface of the substrate 10 is 0.5 nm to 1 nm, which may be, for example, 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm or 1 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.

[0115] Since the doped layer has a high doping concentration, the P-type doped layer and the N-type doped layer have better conductivity than the intrinsic layer, and edge leakage is likely to occur when they overlap on the side surfaces. In the present application, the thickness of the doped stack on the side surface of the substrate 10 is controlled within the range of 1 nm to 2.5 nm. The relatively thin first doped layer 312 and second doped layer 322 on the side surface of the substrate 10 can greatly reduce the conductivity of the doped layers, thereby reducing edge leakage caused by the overlap of the two doped layers.

[0116] In some embodiments of the present application, the first transparent conductive layer 41 and the second transparent conductive layer 42 may be transparent conductive oxide layers. The transparent conductive oxide layer may be an In-containing oxide conductive layer or an In-free oxide conductive layer, and the In-containing oxide conductive layer may be any one or a combination of at least two of ITO, VTTO, HITO or IWO.

[0117] Reference Figure 2 in conjunction with Figures 3 to 5As shown, the first transparent conductive layer 41 includes a first transparent conductive layer 411 located on the first surface of the substrate 10 and a first transparent conductive layer 412 located on the side surface of the substrate 10, the first transparent conductive layer 412 on the side surface of the substrate 10 is stacked on the doped stack on the side surface of the substrate 10, the second transparent conductive layer 42 is only located on the second surface of the substrate 10, and the second transparent conductive layer 42 is electrically isolated from the first transparent conductive layer 412 located on the side surface of the substrate 10.

[0118] Reference Figure 3 and Figure 4 As shown, in the present application, the thickness of the first transparent conductive layer 411 located on the first surface of the substrate 10 is H51, the thickness of the first transparent conductive layer 412 located on the side surface of the substrate 10 is H52, and the thickness of the second transparent conductive layer 42 located on the second surface of the substrate 10 is H61.

[0119] In some preferred embodiments, the first transparent conductive layer 411 on the first surface of the substrate 10 and the first transparent conductive layer 412 on the side surface are prepared by a one-step deposition process, for example, a PVD (Physical Vapor Deposition) process. The thickness H51 of the first transparent conductive layer 411 on the first surface of the substrate 10 is 60 nm to 120 nm, which may be, for example, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm or 120 nm, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable; the thickness H52 of the first transparent conductive layer 412 on the side surface of the substrate 10 is 3 nm to 6 nm, which may be, for example, 3 nm, 1 nm, 3.5 nm, 4 nm, 4.5 nm, 5 nm, 5.5 nm or 6 nm, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.

[0120] In some preferred embodiments, the second transparent conductive layer 42 on the second surface of the substrate 10 may be formed by a PVD (Physical Vapor Deposition) process, and the thickness H61 of the second transparent conductive layer 42 is 60 nm to 120 nm, which may be, for example, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm or 120 nm, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.

[0121] In other embodiments of the present application, the first transparent conductive layer 41 may also be deposited only on the first surface of the substrate 10, while the second transparent conductive layer 42 is deposited on the first surface and the side surface of the substrate 10.

[0122] In this application, a transparent conductive layer with a thickness of 3nm to 6nm is formed on the doped stack on the side of the substrate. The thicker transparent conductive layer can further improve the side passivation effect, and at the same time can prevent water vapor from entering the doped stack and the intrinsic stack, which would lead to passivation deterioration, thereby improving the reliability of photovoltaic cells.

[0123] In some embodiments of this application, references Figure 2 and combined Figure 4 As shown, the second intrinsic layer 222, the first intrinsic layer 212, the first doped layer 312, the second doped layer 322 and the first transparent conductive layer 412 are stacked sequentially in the direction away from the side of the substrate 10, and the transparent conductive layer contains oxygen, and the oxygen concentration of each film layer on the side of the substrate gradually increases in the direction away from the side of the substrate 10.

[0124] Preferably, the first intrinsic layer 212 covers the entire second intrinsic layer 22 along the thickness direction of the substrate 10, the first doped layer 312 covers the entire first intrinsic layer 21 along the thickness direction of the substrate 10, the second doped layer 322 covers the entire first doped layer 31 along the thickness direction of the substrate 10, and the first transparent conductive layer 412 covers the entire second doped layer 32 along the thickness direction of the substrate 10.

[0125] In some other embodiments of this application, the order of the second intrinsic layer 222 and the first intrinsic layer 212 on the side of the substrate 10 can be interchanged. At the same time, the outermost transparent conductive layer can also be the second transparent conductive layer on the second surface of the substrate 10, which will not be described in detail here.

[0126] In some embodiments of this application, the first electrode 51 and the second electrode 52 are grid line electrodes, which are prepared by screen printing using conductive paste and then dried and cured.

[0127] In some embodiments of this application, the conductive paste is a low-temperature silver paste, a silver-copper paste, or a pure copper paste; the drying temperature is 100℃~200℃, for example, it can be 100℃, 120℃, 140℃, 160℃, 180℃ or 200℃, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable; the curing temperature is 150℃~230℃, for example, it can be 150℃, 170℃, 190℃, 210℃ or 230℃, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0128] It is worth noting that, in order to ensure the performance of the photovoltaic cell and the passivation performance of the first and second surfaces, the total thickness H11+H21 of the first intrinsic layer 211 and the second intrinsic layer 221 along the substrate thickness direction must be less than the total thickness H31+H41 of the first doped layer 311 and the second doped layer 321 along the substrate thickness direction. However, to simplify the process, each film layer on the side of the substrate 10 and each film layer on the first or second surface of the substrate 10 are prepared using a one-step deposition process. After conventional deposition, the thickness H12+H22 of the intrinsic stack on the side of the substrate 10 will be less than the thickness H32+H42 of the doped stack. Such a thinner intrinsic stack has a weaker passivation effect on the side, while a thicker doped stack will aggravate edge leakage. In order to make the thickness H12+H22 of the intrinsic stack greater than the thickness H32+H42 of the doped stack in the deposition process of each film layer, the applicant has further optimized the preparation process, which is described in detail below.

[0129] Combination Figures 2 to 5 As shown, this application provides a method for preparing a photovoltaic cell, comprising the following steps:

[0130] A substrate 10 is provided, the substrate 10 including a first surface and a second surface disposed opposite to each other, and a plurality of side surfaces;

[0131] A first intrinsic layer 21 is deposited on a first surface and a side surface of a substrate 10, and a second intrinsic layer 22 is deposited on a second surface and a side surface of a substrate 10. The first intrinsic layer 21 and the second intrinsic layer 22 overlap at at least one side surface of the substrate to form an intrinsic stack.

[0132] A first doped layer 31 is deposited on a first intrinsic layer 21 on a first surface and side surface of a substrate 10, and a second doped layer 32 is deposited on a second intrinsic layer 22 on a second surface and side surface of a substrate 10. The first doped layer 31 and the second doped layer 32 overlap at least one side surface of the substrate 10 to form a doped stack. The first doped layer has the same doping type as the substrate, and the second doped layer has the opposite doping type to the substrate.

[0133] A first transparent conductive layer 41 is deposited on the first doped layer 31 on the first surface and side surface of the substrate 10, and a second transparent conductive layer 42 is deposited on the second doped layer 32 on the second surface of the substrate 10.

[0134] A first electrode 51, which is in electrical contact with the first doped layer 31, is prepared on the first transparent conductive layer 41, and a second electrode 52, which is in electrical contact with the second doped layer 32, is prepared on the second transparent conductive layer 42.

[0135] In some embodiments of this application, both the first intrinsic layer 21 and the second intrinsic layer 22 are deposited using a PECVD process. To increase the thickness of the first intrinsic layer 21 and the second intrinsic layer 22 on the side of the substrate 10, an independently positioned first carrier plate is used to support the substrate 10, exposing more of the side surface of the substrate 10 to the coating atmosphere. Simultaneously, a low-frequency and low-power RF (Radio Frequency) power supply is used to excite the plasma, thereby depositing a thicker intrinsic layer on the side of the substrate 10. Preferably, in the PECVD process for depositing the first intrinsic layer 21 and / or the second intrinsic layer 22, the power supply frequency is 13.56 MHz and the power density is 100 W / m². 2 ~600W / m 2 For example, it could be 100W / m 2 200W / m 2 300W / m 2 400W / m 2 500W / m 2 Or 600W / m 2 The values ​​are not limited to those listed; other unlisted values ​​within the range also apply.

[0136] To increase the thickness of the intrinsic layer on the substrate sidewall, the substrate sidewall is exposed during the PECVD process, with only limiting elements used to constrain the substrate. (See reference...) Figure 6 , Figure 7 As shown, in some embodiments of this application, the first carrier plate 60 supports the substrate 10 using an independent limiting method. The first carrier plate 60 includes a first frame 61, a plurality of first support members 62 located within the first frame, and a plurality of limiting members 63 spaced apart on the frame. The top of the first frame 61 is flush with the top of the first support members 62. The first frame 61 is squarely distributed, and each frame is provided with at least one limiting member 63. Thus, during PECVD deposition, the sides of the substrate 10 are only shielded at the positions of the limiting members 63, while the remaining areas are exposed to the coating atmosphere, which is beneficial for depositing a thicker intrinsic layer.

[0137] For example, in the PECVD process for depositing the first intrinsic layer 21, an RF power source is used to excite the plasma with a power density of 100 W / m². 2 ~600W / m 2 The introduced gas is silane and hydrogen, with a flow rate ratio of silane to hydrogen of 1:(1~5). The chamber pressure is 0.4 Torr~0.7 Torr. The thickness of the first intrinsic layer 211 on the first surface is 4nm~6.5nm, and the thickness of the first intrinsic layer 212 on the side of the substrate 10 is 0.5nm~3nm.

[0138] For example, in the PECVD process for depositing the second intrinsic layer 22, an RF power source is used to excite the plasma with a power density of 100 W / m². 2 ~500W / m 2 The introduced gas is silane and hydrogen, with a flow rate ratio of silane to hydrogen of 1:(1~20). The chamber pressure is 0.4 Torr~0.7 Torr. The thickness of the second intrinsic layer 221 on the second surface is 5nm~7nm, and the thickness of the second intrinsic layer 222 on the side of the substrate 10 is 0.5nm~3nm.

[0139] In some embodiments of this application, both the first doped layer 31 and the second doped layer 32 are deposited using a PECVD process. To reduce the thickness of the first doped layer 31 and the second doped layer 32 on the side of the substrate 10, a stepped-limited second carrier plate is used to support the substrate 10, so that a smaller area of ​​the side of the substrate 10 is exposed to the coating atmosphere. Simultaneously, a high-frequency and high-power VHF (Very High Frequency) power supply is used to excite the plasma, thereby depositing a thinner doped layer on the side of the substrate 10. Preferably, in the PECVD process for depositing the first doped layer 31 and / or the second doped layer 32, the power supply frequency is 27MHz~100MHz, and the power density is 1500W / m². 2 ~5000W / m 2 For example, it could be 1500W / m 2 2000W / m 2 2500W / m 2 3000W / m 2 3500W / m 2 4000W / m 2 4500W / m 2 Or 5000W / m 2 The values ​​are not limited to those listed; other unlisted values ​​within the range also apply.

[0140] To reduce the thickness of the doped layer on the substrate sidewalls, the substrate sidewalls are not required in the PECVD process. (See reference...) Figure 8 , Figure 9 As shown, in some embodiments of this application, the second carrier plate 70 supports the substrate 10 in a stepped limiting manner. The second carrier plate 70 includes a second frame 71 and a plurality of second support members 72 located within the first frame 71. The second frame 71 has a receiving portion 711 facing inward, and the bottom of the receiving portion 711 is flush with the top of the second support member 72. The second frame 71 is squarely distributed, and the distance between the sidewalls of two relative receiving portions 711 is slightly larger than the size of the substrate 10. Thus, during PECVD deposition, the second frame 71 blocks the reactive gas, thereby depositing a thinner doped layer on the side of the substrate 10.

[0141] For example, in the PECVD process for depositing the first doped layer 31, a VHF power supply is used to excite the plasma with a power density of 1500 W / m. 2 ~5000W / m 2 The introduced gas is silane, hydrogen and a first dopant gas (e.g. phosphine). The flow rate ratio of silane to hydrogen is 1:(150~300), the flow rate ratio of the first dopant gas to silane is 1:(2~4), the chamber pressure is 3 Torr~6 Torr, the thickness of the first doped layer 311 on the first surface is 20nm~30nm, and the thickness of the first doped layer 312 on the side of the substrate 10 is 0.5nm~1.5nm.

[0142] For example, in the PECVD process for depositing the second doped layer 32, a VHF power supply is used to excite the plasma with a power density of 3000 W / m. 2 ~5000W / m 2 The introduced gas is silane, hydrogen, and a second dopant gas (e.g., borane). The flow rate ratio of silane to hydrogen is 1:(150~350), and the flow rate ratio of the second dopant gas to silane is 1:(0.5~5). The chamber pressure is 3 Torr~5 Torr. The thickness of the second doped layer 321 on the second surface is 25nm~35nm, and the thickness of the second doped layer 322 on the side of the substrate 10 is 0.5nm~1nm.

[0143] In this application, the power density P d For P d =P / A, where P is the power of the power supply (RF or VHF), and A is the electrode area. Taking a parallel-plate PECVD equipment as an example, the lower electrode is used to place the substrate, the power supply is applied between the upper and lower electrodes, and the electrode area refers to the area of ​​the lower electrode. In a specific PECVD equipment, the electrode area A is a fixed value, and the power density P can be controlled by adjusting the power supply power P. d .

[0144] In some embodiments of this application, both the first transparent conductive layer 41 and the second transparent conductive layer 42 are transparent conductive oxide layers (TCO), which are deposited using PVD (physical vapor deposition) or magnetron sputtering processes. The first transparent conductive layer 41 is located on the first surface and side surface of the substrate 10, while the second transparent conductive layer 42 is located only on the second surface of the substrate 10. When depositing the second transparent conductive layer 42, the back side is shielded by an edge design using a carrier disk, with a specific shielding area of ​​0.45mm to 0.65mm around the perimeter.

[0145] For example, the transparent conductive oxide layer is made of ITO (99.5%:0.5%)wt. The thickness of the first transparent conductive layer 411 on the first surface is 60nm~120nm, the thickness of the first transparent conductive layer 412 on the side of the substrate 10 is 3nm~6nm, the thickness of the second transparent conductive layer 42 on the second surface is 60nm~120nm, and the carrier concentration of the transparent conductive oxide layer is 2E20cm⁻¹. -3 ~3E20cm -3 Mobility 60cm 2 / Vs~80cm 2 / Vs.

[0146] In some embodiments of this application, a second intrinsic layer 22 may be deposited first on the second surface and side surface of the substrate 10, and then a first intrinsic layer 21 and a first doped layer 31 may be deposited sequentially on the first surface and side surface of the substrate 10. Next, a second doped layer 32 may be deposited on the second surface and side surface of the substrate 10, and finally a first transparent conductive layer 41 and a second transparent conductive layer 42 may be deposited. At this time, the second intrinsic layer, the first intrinsic layer, the first doped layer, the second doped layer and the first transparent conductive layer are sequentially stacked on the side surface of the substrate 10.

[0147] In some other embodiments of this application, a first intrinsic layer 21 may be deposited on the first surface and side surface of the substrate 10, followed by a second intrinsic layer 22 deposited on the second surface and side surface of the substrate 10, then a first doped layer 31 deposited on the first surface and side surface of the substrate 10, then a second doped layer 32 deposited on the second surface and side surface of the substrate 10, and finally a first transparent conductive layer 41 and a second transparent conductive layer 42 deposited. In this case, the first intrinsic layer, the second intrinsic layer, the first doped layer, the second doped layer and the first transparent conductive layer are sequentially stacked on the side surface of the substrate 10.

[0148] The present application will be further described below with reference to specific embodiments.

[0149] Example 1:

[0150] Photovoltaic cell parameters in this embodiment Figure 2 As shown, it includes:

[0151] Base 10;

[0152] The first intrinsic layer 21 and the second intrinsic layer 22 are located on the second surface and the side surface of the substrate 10, respectively. The first intrinsic layer 21 is located on the first surface and the side surface of the substrate 10, and the first intrinsic layer 21 and the second intrinsic layer 22 overlap on at least one side surface of the substrate to form an intrinsic stack.

[0153] A first doped layer 31 and a second doped layer 32, wherein the first doped layer 31 is located on the first intrinsic layer 21 and the second doped layer 32 is located on the second intrinsic layer 22, and the first doped layer 31 and the second doped layer 32 overlap on at least one side of the substrate 10 to form a doped stack.

[0154] A first transparent conductive layer 41 and a second transparent conductive layer 42, wherein the first transparent conductive layer 41 is located on the first surface and side surface of the substrate 10, and the second transparent conductive layer 42 is located on the second surface of the substrate 10;

[0155] The first electrode 51 and the second electrode 52 are located on the first transparent conductive layer 41 and are in electrical contact with the first doped layer 31, and the second electrode 52 is located on the second transparent conductive layer 42 and are in electrical contact with the second doped layer 32.

[0156] The photovoltaic cell preparation method in this embodiment specifically includes the following steps:

[0157] 1. A substrate 10 is provided, the substrate 10 including a first surface, a second surface and multiple side surfaces.

[0158] For example, in this embodiment, the substrate 10 is an N-type monocrystalline silicon substrate with a resistivity of 0.5 Ω·cm to 3 Ω·cm and a thickness of 100 μm to 130 μm.

[0159] 2. Cleaning and flocking.

[0160] The surface of substrate 10 is cleaned by a mixture of KOH and H2O2. Then, the surface of substrate 10 is rough polished with KOH solution. Next, a pyramid textured structure is formed on the first surface, second surface and side surface of substrate 10 by using KOH solution with alcohol and anisotropic etching of single crystal silicon.

[0161] 3. The second intrinsic layer 22 was deposited.

[0162] The texturized substrate 10 is placed on the first carrier plate 60 in the PECVD chamber, and a second intrinsic layer 22 is deposited on the second surface and side surface of the substrate 10 using the PECVD process.

[0163] The PECVD process uses an RF power source to excite the plasma, with a power density of 100 W / m³. 2 ~500W / m 2 The introduced gas is silane and hydrogen, with a flow rate ratio of silane to hydrogen of 1:(1~20). The chamber pressure is 0.4 Torr~0.7 Torr. The thickness H21 of the second intrinsic layer 221 on the second surface of the substrate 10 is 6 nm, and the thickness H22 of the second intrinsic layer 222 on the side surface of the substrate 10 is 2 nm.

[0164] 4. The first intrinsic layer 21 was deposited.

[0165] After the second intrinsic layer 22 is prepared, the substrate 10 is flipped over on the first carrier plate 60, and the first intrinsic layer 21 is deposited on the first surface and side surface of the substrate 10 using the PECVD process.

[0166] The PECVD process uses an RF power source to excite the plasma, with a power density of 100 W / m³. 2 ~600W / m 2 The introduced gas is silane and hydrogen, with a flow rate ratio of silane to hydrogen of 1:(1~5). The chamber pressure is 0.4 Torr~0.7 Torr. The thickness H11 of the first intrinsic layer 211 on the first surface of the substrate 10 is 5.5 nm, and the thickness H12 of the first intrinsic layer 212 on the side surface of the substrate 10 is 2 nm. The first intrinsic layer 212 on the side surface of the substrate 10 is stacked on the second intrinsic layer 222.

[0167] 5. Deposit the first doped layer 31.

[0168] The substrate 10, after the preparation of the first intrinsic layer 21, is placed on the second carrier plate 70, and the first doped layer 31 is deposited on the first surface and side surface of the substrate 10 using the PECVD process.

[0169] The PECVD process uses a VHF power source to excite the plasma, with a power density of 1500 W / m³. 2 ~5000W / m 2 The introduced gases are silane, hydrogen, and phosphine. The flow ratio of silane to hydrogen is 1:(150~300), the flow ratio of phosphine to silane is 1:(2~4), the chamber pressure is 3 Torr~6 Torr, the thickness H31 of the first doped layer 311 on the first surface of the substrate 10 is 20 nm, and the thickness H32 of the first doped layer 312 on the side surface of the substrate 10 is 0.5 nm.

[0170] 6. Deposit the second doped layer 32.

[0171] The substrate 10, after the first doped layer 31 is prepared, is flipped onto the second carrier plate 70, and the second doped layer 32 is deposited on the second surface and side surface of the substrate 10 using a PECVD process.

[0172] The PECVD process uses a VHF power source to excite the plasma, with a power density of 3000 W / m³. 2 ~5000W / m 2The introduced gases are silane, hydrogen, and borane. The flow rate ratio of silane to hydrogen is 1:(150~350), and the flow rate ratio of borane to silane is 1:(0.5~5). The chamber pressure is 3 Torr~5 Torr. The thickness H41 of the second doped layer 321 on the second surface of the substrate 10 is 25 nm, and the thickness H42 of the second doped layer 322 on the side surface of the substrate 10 is 0.5 nm. The first doped layer 312 and the second doped layer 322 on the side surface of the substrate 10 are sequentially stacked on the first intrinsic layer 212.

[0173] 7. Deposit a transparent conductive layer.

[0174] A first transparent conductive layer 41 and a second transparent conductive layer 42 are prepared on the first doped layer 31 and the second doped layer 32 respectively using PVD process.

[0175] The transparent conductive oxide layer is made of ITO (99.5%:0.5%)wt. The thickness H51 of the first transparent conductive layer 411 on the first surface of the substrate 10 is 60 nm, the thickness H52 of the first transparent conductive layer 412 on the side surface of the substrate 10 is 3 nm, the thickness H61 of the second transparent conductive layer 42 is 75 nm, and the carrier concentration of the transparent conductive oxide layer is 2E20cm⁻¹. -3 ~3E20cm -3 Mobility 60cm 2 / Vs~80cm 2 / Vs.

[0176] In this embodiment, the thickness of the intrinsic stacked layer on the side of the substrate is 4 nm (H12+H22), the thickness of the doped stacked layer on the side of the substrate is 1 nm (H32+H42), and the thickness of the transparent conductive layer on the side of the substrate is 3 nm. The side morphology of the substrate is as follows: Figure 10 As shown in the figure, the side of the base has a pyramidal velvet structure, and the outermost black film layer is the test protective film.

[0177] Example 2:

[0178] The structure and fabrication method of the photovoltaic cell in this embodiment are roughly the same as those in Embodiment 1. The difference is that the thickness H11 of the first intrinsic layer 211 on the first surface of the substrate 10 is 6.5 nm, the thickness H12 of the first intrinsic layer 212 on the side surface of the substrate 10 is 2.5 nm, the thickness H21 of the second intrinsic layer 221 on the second surface of the substrate 10 is 7 nm, and the thickness H22 of the second intrinsic layer 222 on the side surface of the substrate 10 is 2.5 nm.

[0179] In this embodiment, the thickness of the intrinsic stack on the side of the substrate, H12+H22, is 5 nm, the thickness of the doped stack on the side of the substrate, H32+H42, is 1 nm, and the thickness of the transparent conductive layer on the side of the substrate is 3 nm.

[0180] Example 3:

[0181] The structure and preparation method of the photovoltaic cell in this embodiment are roughly the same as those in Embodiment 1. The difference is that the thickness H41 of the second doped layer 321 on the second surface of the substrate 10 is 30 nm, and the thickness H42 of the second doped layer 322 on the side of the substrate 10 is 0.7 nm.

[0182] In this embodiment, the thickness of the intrinsic stack on the substrate side is 4 nm (H12+H22), the thickness of the doped stack on the substrate side is 1.2 nm (H32+H42), and the thickness of the transparent conductive layer on the substrate side is 3 nm.

[0183] Example 4:

[0184] The structure and preparation method of the photovoltaic cell in this embodiment are roughly the same as those in Embodiment 1. The difference is that the thickness H31 of the first doped layer 311 on the first surface of the substrate 10 is 25 nm, and the thickness H32 of the first doped layer 312 on the side of the substrate 10 is 1 nm.

[0185] In this embodiment, the thickness of the intrinsic stack on the substrate side is 4 nm (H12+H22), the thickness of the doped stack on the substrate side is 1.5 nm (H32+H42), and the thickness of the transparent conductive layer on the substrate side is 3 nm.

[0186] Example 5:

[0187] The structure and fabrication method of the photovoltaic cell in this embodiment are roughly the same as those in Embodiment 1. The difference is that the thickness H31 of the first doped layer 311 on the first surface of the substrate 10 is 25 nm, the thickness H32 of the first doped layer 312 on the side surface of the substrate 10 is 1 nm, the thickness H41 of the second doped layer 321 on the second surface of the substrate 10 is 30 nm, and the thickness H42 of the second doped layer 322 on the side surface of the substrate 10 is 0.7 nm.

[0188] In this embodiment, the thickness of the intrinsic stack on the substrate side is 4 nm (H12+H22), the thickness of the doped stack on the substrate side is 1.7 nm (H32+H42), and the thickness of the transparent conductive layer on the substrate side is 3 nm.

[0189] Example 6:

[0190] The structure and preparation method of the photovoltaic cell in this embodiment are roughly the same as those in Embodiment 1. The difference is that the thickness H51 of the first transparent conductive layer 411 on the first surface of the substrate 10 is 75 nm, and the thickness H52 of the first transparent conductive layer 412 on the side of the substrate 10 is 4 nm.

[0191] In this embodiment, the thickness of the intrinsic stack on the substrate side is 4 nm (H12+H22), the thickness of the doped stack on the substrate side is 1.7 nm (H32+H42), and the thickness of the transparent conductive layer on the substrate side is 4 nm.

[0192] Comparative Example 1:

[0193] The photovoltaic cells in this comparative example Figure 1 As shown, there are no membrane structures on the sides of substrate 10.

[0194] Comparative Example 2:

[0195] In this comparative example, the structure and fabrication method of the photovoltaic cell are largely the same as in Example 1. The difference lies in that, after the first intrinsic layer 21 and the second intrinsic layer 22 are deposited on the first and second surfaces of the substrate 10 respectively using a PECVD process, a stacked film of the first and second intrinsic layers is deposited on the side surface of the substrate 10. In this comparative example, the thickness H12+H22 of the intrinsic stacked film on the side surface of the substrate is 0.8 nm, the thickness H32+H42 of the doped stacked film on the side surface of the substrate is 1 nm, and the thickness of the transparent conductive layer on the side surface of the substrate is 3 nm.

[0196] The electrical performance of the photovoltaic cells in each embodiment and comparative example was tested, and the results are shown in the table below:

[0197] Table 1: Photovoltaic Cell Electrical Performance Data

[0198]

[0199] As shown in Table 1, the sides of photovoltaic cells are passivated and protected by intrinsic and doped layers. Controlling the thickness of the intrinsic layer to be greater than that of the doped layer improves the side passivation effect, while the thinner doped layer reduces edge leakage current. Ultimately, this significantly improves the cell's open-circuit voltage (Voc), fill factor (FF), pseudo-fill factor (pFF), and cell efficiency (EFF). Furthermore, the transparent conductive layer on the sides ensures that the doped and intrinsic layers are protected from moisture damage, guaranteeing the side passivation effect of the cell.

[0200] The photovoltaic cells in the above embodiments and comparative examples are illustrated using heterojunction (HJT) cells as an example. In a heterojunction cell, the first intrinsic layer and the first doped layer are located on the first surface of the substrate, and the second intrinsic layer and the second doped layer are located on the second surface of the substrate. In other embodiments, the photovoltaic cell can also be other types of cells, such as back contact heterojunction cells (HBC). In a back contact heterojunction cell, the first intrinsic layer and the first doped layer, as well as the second intrinsic layer and the second doped layer, are all located on the second surface of the substrate (i.e., the back side or the backlight side). The side films in the back contact heterojunction cell are exactly the same as in the above embodiments, and will not be described in detail here.

[0201] It is worth noting that in a back-contact heterojunction cell, all PN junctions are concentrated on the back side of the cell, with only field passivation performed on the front side. Photogenerated carriers need to be transported vertically to the PN junctions on the back side for collection. The P / N doped layer is deposited around the side of the substrate, exposing both N and P doped layers simultaneously. Side recombination directly dissipates a large number of photogenerated carriers, resulting in an open-circuit voltage V. OC The losses are more pronounced than in conventional heterojunction cells, and lateral leakage channels are more easily formed. Therefore, leakage and lateral recombination caused by the P / N doped layer deposited around the sides in back-contact heterojunction cells become key bottlenecks restricting performance. In this application, by optimizing the structure and thickness of the side film, the parasitic lateral leakage caused by back-contact heterojunction cells can be suppressed, and the open-circuit voltage Vo can be significantly reduced. OC This reduces losses and thus improves photoelectric conversion efficiency.

[0202] Of course, this application is not limited to the heterojunction cells and back-contact heterojunction cells mentioned above. Any technical solution that improves the passivation effect of the side and reduces edge leakage by optimizing the side passivation stack and intrinsic stack is within the scope of protection of this application.

[0203] This application also provides a photovoltaic module, comprising: a plurality of the aforementioned photovoltaic cells connected in series to form a photovoltaic cell string; an interconnecting member electrically connected to the aforementioned photovoltaic cells to connect the aforementioned photovoltaic cells to form a photovoltaic cell string; and an encapsulation layer covering the surface of the plurality of photovoltaic cells.

[0204] In some embodiments of this application, the interconnecting components can be solder ribbons, metal wires, conductive tapes, etc.; the encapsulation layer can include a backplate, encapsulating film, cover plate, etc., to improve the stability of the photovoltaic cell string. The cover plate is located on the front of the photovoltaic cell string, and the backplate is located on the back of the photovoltaic cell string, both serving a protective function; the adhesive film is the adhesive film between the photovoltaic cell string and the cover plate and backplate, serving a bonding and fixing function, and must be made of a transparent material.

[0205] In some examples, the encapsulating film can be an organic encapsulating film such as polyvinyl butyral (PVB) film, ethylene-vinyl acetate copolymer (EVA) film, polyvinyl octene elastomer (POE) film, or polyethylene terephthalate (PET) film. In some examples, the cover or backing plate can be a light-transmitting film layer such as a glass cover or a plastic cover.

[0206] It will be apparent to those skilled in the art that this disclosure is not limited to the details of the exemplary embodiments described above, and that this disclosure can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of this disclosure is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within this disclosure. No reference numerals in the claims should be construed as limiting the scope of the claims.

[0207] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A photovoltaic cell, characterized in that, The photovoltaic cell includes: A substrate, the substrate including a substrate surface and a plurality of substrate side surfaces, the substrate surface including a first surface and a second surface disposed opposite to each other; A first intrinsic layer and a second intrinsic layer, wherein the first intrinsic layer is located on a first surface or a second surface of the substrate, the second intrinsic layer is located on a first surface or a second surface of the substrate, and the first intrinsic layer and the second intrinsic layer overlap at least one side of the substrate to form an intrinsic stack. A first doped layer and a second doped layer, wherein the first doped layer is located on the first intrinsic layer, the second doped layer is located on the second intrinsic layer, and the first doped layer and the second doped layer overlap at least one side of a substrate to form a doped stack, wherein the first doped layer has the same doping type as the substrate, and the second doped layer has the opposite doping type to the substrate; The first electrode and the second electrode are in electrical contact, the first electrode is in electrical contact with the first doped layer, and the second electrode is in electrical contact with the second doped layer; In at least a portion of the overlapping region on the side of the substrate, the thickness of the intrinsic stack is greater than the thickness of the doped stack.

2. The photovoltaic cell according to claim 1, characterized in that, In at least a partial overlapping region on the side surface of the substrate, the thickness of the intrinsic stack is 3 nm to 6 nm; and / or, In at least a portion of the overlapping region on the side of the substrate, the thickness of the doped stack is 1 nm to 2.5 nm.

3. The photovoltaic cell according to claim 1 or 2, characterized in that, The total thickness of the first intrinsic layer and the second intrinsic layer along the substrate thickness direction is less than the total thickness of the first doped layer and the second doped layer along the substrate thickness direction.

4. The photovoltaic cell according to claim 3, characterized in that, The total thickness of the first intrinsic layer and the second intrinsic layer along the substrate thickness direction is 9 nm to 13.5 nm; and / or, The total thickness of the first doped layer and the second doped layer along the thickness direction of the substrate is 45 nm to 65 nm.

5. The photovoltaic cell according to claim 1, characterized in that, The first intrinsic layer on the substrate surface and sidewalls is prepared using a one-step deposition process. The thickness of the first intrinsic layer on the substrate surface along the substrate thickness direction is 4 nm to 6.5 nm, and the thickness of the first intrinsic layer in the intrinsic stack is 0.5 nm to 3 nm; and / or, The second intrinsic layer on the substrate surface and the substrate side surface is prepared by a one-step deposition process. The thickness of the second intrinsic layer on the substrate surface is 5nm~7nm, and the thickness of the second intrinsic layer in the intrinsic stack is 0.5nm~3nm.

6. The photovoltaic cell according to claim 1, characterized in that, The first doped layer on the substrate surface and the substrate side surface is prepared by a one-step deposition process. The thickness of the first doped layer on the substrate surface is 20 nm to 30 nm, and the thickness of the first doped layer on the substrate side surface is 0.5 nm to 1.5 nm; and / or, The second doped layer on the substrate surface and the substrate side surface is prepared by a one-step deposition process. The thickness of the second doped layer on the substrate surface is 25nm~35nm, and the thickness of the second doped layer on the substrate side surface is 0.5nm~1nm.

7. The photovoltaic cell according to claim 1, characterized in that, The second intrinsic layer, the first intrinsic layer, the first doped layer, and the second doped layer are stacked sequentially in a direction away from the side surface of the substrate; or, The first intrinsic layer, the second intrinsic layer, the first doped layer, and the second doped layer are stacked sequentially in a direction away from the side surface of the substrate.

8. The photovoltaic cell according to claim 1, characterized in that, The first intrinsic layer and the second intrinsic layer are located on the first surface and the second surface of the substrate, respectively; or, Both the first intrinsic layer and the second intrinsic layer are located on the first surface or the second surface of the substrate.

9. The photovoltaic cell according to claim 1, characterized in that, The first intrinsic layer is an intrinsic amorphous silicon layer; and / or, The second intrinsic layer is an intrinsic amorphous silicon layer; and / or, The first doped layer is any one of amorphous silicon, microcrystalline silicon, or nanocrystalline silicon; and / or, The second doped layer is any one of amorphous silicon doped layer, microcrystalline silicon doped layer, or nanocrystalline silicon doped layer; and / or, The substrate is an N-type crystalline silicon substrate, the first doped layer is an N-type doped layer, and the second doped layer is a P-type doped layer; and / or, The surface of the substrate has a light-trapping velvet structure.

10. The photovoltaic cell according to claim 1, characterized in that, The photovoltaic cell also includes: A first transparent conductive layer and a second transparent conductive layer, wherein the first transparent conductive layer is at least partially located on the first doped layer, and the second transparent conductive layer is at least partially located on the second doped layer.

11. The photovoltaic cell according to claim 10, characterized in that, The first transparent conductive layer or the second transparent conductive layer covers the doped stack on the side of the substrate.

12. The photovoltaic cell according to claim 11, characterized in that, The thickness of the first transparent conductive layer on the substrate surface is 60 nm to 120 nm; and / or, The thickness of the second transparent conductive layer on the substrate surface is 60nm~120nm; and / or, The thickness of the first or second transparent conductive layer on the side of the substrate is 3nm to 6nm.

13. The photovoltaic cell according to claim 11, characterized in that, The first transparent conductive layer and the second transparent conductive layer are transparent conductive oxide layers, and the oxygen concentration of each film layer on the side of the substrate gradually increases in the direction away from the side of the substrate.

14. A method for preparing a photovoltaic cell, characterized in that, The preparation method includes the following steps: A substrate is provided, the substrate including a substrate surface and a substrate side surface, the substrate surface including a first surface and a second surface disposed opposite to each other; A first intrinsic layer is deposited on the substrate surface and the substrate sidewalls, and a second intrinsic layer is deposited on the substrate surface and the substrate sidewalls. The first and second intrinsic layers are deposited using a PECVD process with a power density of 100 W / m². 2 ~600W / m 2 The first intrinsic layer and the second intrinsic layer overlap at at least one side of the substrate to form an intrinsic stack; A first doped layer is deposited on the first intrinsic layer on the substrate surface and the substrate side surface, and a second doped layer is deposited on the second intrinsic layer on the substrate surface and the substrate side surface. The first doped layer and the second doped layer overlap at at least one substrate side surface to form a doped stack. The first doped layer and the second doped layer are deposited using a PECVD process with a power density of 1500 W / m². 2 ~5000W / m 2 ; A first electrode that is in electrical contact with the first doped layer is prepared on the first doped layer, and a second electrode that is in electrical contact with the second doped layer is prepared on the second doped layer. In at least a portion of the overlapping region on the side of the substrate, the thickness of the intrinsic stack is greater than the thickness of the doped stack.

15. The method for preparing a photovoltaic cell according to claim 14, characterized in that, In the PECVD process for depositing the first intrinsic layer and / or the second intrinsic layer, the substrate sidewalls are exposed to increase the thickness of the first intrinsic layer and / or the second intrinsic layer on the substrate sidewalls.

16. The method for preparing a photovoltaic cell according to claim 14, characterized in that, A first intrinsic layer is deposited on the first surface and the side surface of the substrate, and a second intrinsic layer is deposited on the second surface and the side surface of the substrate; A first doped layer is deposited on the first intrinsic layer on the first surface and side surface of the substrate, and a second doped layer is deposited on the second intrinsic layer on the second surface and side surface of the substrate.

17. The method for preparing a photovoltaic cell according to claim 16, characterized in that, The first doped layer is deposited before the second doped layer; and / or, The second intrinsic layer is deposited before the first intrinsic layer.

18. The method for preparing a photovoltaic cell according to claim 14, characterized in that, The preparation method further includes: A first transparent conductive layer is deposited on the first doped layer on the substrate surface and the substrate side surface, wherein the thickness of the first transparent conductive layer on the substrate surface is 60 nm to 120 nm, and the thickness of the first transparent conductive layer on the substrate side surface is 3 nm to 6 nm; and / or, A second transparent conductive layer is deposited on the second doped layer on the surface of the substrate, and the thickness of the second transparent conductive layer on the surface of the substrate is 60 nm to 120 nm.

19. A photovoltaic module comprising a plurality of cell strings, wherein the cell strings include at least one photovoltaic cell as described in any one of claims 1 to 13 or at least one photovoltaic cell prepared by any one of claims 14 to 18.