An epitaxial structure for visible light communication and its fabrication method, and a MicroLED chip.
By introducing multiple GaN barrier layers and AlGaN insertion layers into the GaN-based MicroLED epitaxial structure, the problems of insufficient electron overflow and polarization field shielding are solved, the uniformity of carrier distribution and modulation bandwidth are improved, and efficient data transmission is achieved.
Patent Information
- Application Number
- CN202611291783.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing technology, GaN-based MicroLED epitaxial structures suffer from insufficient electron overflow and polarization field shielding under high modulation bandwidth requirements, resulting in uneven carrier distribution and affecting data transmission rate.
A multilayer GaN barrier structure is adopted, with the Si doping concentration decreasing layer by layer along the epitaxial direction. An AlGaN insertion layer is introduced into the GaN barrier layer to form a distributed electron reflection barrier. Electron overflow is suppressed and the polarization electric field is shielded through the quantum mechanical resonant reflection mechanism.
The overlap rate of the carrier wavefunction was improved, the modulation bandwidth was increased by 3dB, the efficiency roll-off under high current density was reduced, and efficient data transmission was achieved.
Smart Images

Figure CN123124526A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor device technology, and in particular to an epitaxial structure and its fabrication method for visible light communication, and a MicroLED chip. Background Technology
[0002] Visible light communication (VLC) technology utilizes the ultra-high spectrum resources of 400THz to 800THz to achieve wireless data transmission and is considered a key complementary technology to 6G communication. MicroLEDs, with their micrometer-scale size, nanosecond-level response speed, and high brightness, have become the ideal emission light source for VLC systems. The modulation bandwidth directly determines how quickly an LED can respond to changes in electrical signals, thus limiting the system's maximum data transmission rate.
[0003] To achieve high modulation bandwidth, GaN-based MicroLED epitaxial structures commonly employ a "thin well, thin barrier" strategy. While thinning the quantum barrier can promote hole tunneling into the deep quantum well, improve carrier distribution uniformity, and increase recombination rate, it also brings two serious side effects: First, the ability of the ultrathin barrier to confine electrons is significantly reduced, leading to increased electron overflow at high current densities and worsening efficiency roll-off; second, simply relying on thinning the barrier cannot effectively shield strong polarization fields, and there is a physical ceiling to improving the electron-hole wavefunction overlap rate.
[0004] In existing technologies, while uniform Si doping of the potential barrier can partially shield the polarization electric field, uniform doping also reduces the barrier's ability to block electrons. Furthermore, excessively high doping concentrations can introduce impurity scattering and non-radiative recombination centers. Although traditional p-type aluminum nitride electron blocking layers (EBLs) can effectively block electron leakage, the polarization difference between them and p-type GaN creates a strong hole accumulation barrier at the interface between the electron blocking layer and the multi-quantum well layer, severely hindering hole injection and resulting in extremely uneven carrier distribution.
[0005] The existing technology has the following specific defects: (1) Uniform doping barrier cannot simultaneously achieve polarization field shielding and electron confinement: high concentration uniform doping shields the polarization field but reduces the height of the electron barrier; low concentration doping maintains electron confinement but does not provide sufficient polarization field shielding.
[0006] (2) The dual negative effects of traditional electron blocking layers: electron blocking layers both hinder hole injection and increase junction capacitance, which are particularly prominent in high-speed modulation scenarios.
[0007] (3) The contradiction between electron leakage and modulation bandwidth in ultrathin barrier systems: thinning the barrier increases the bandwidth but exacerbates electron leakage, and the two cannot be achieved at the same time. Summary of the Invention
[0008] The purpose of this invention is to overcome the shortcomings of the prior art. This invention provides an epitaxial structure and preparation method for visible light communication, as well as a MicroLED chip. The resulting epitaxial structure has a thin total thickness, effectively suppresses electron overflow under high current density, and does not hinder hole injection.
[0009] To address the aforementioned issues, this invention proposes an epitaxial structure for visible light communication, comprising a substrate, and a buffer layer, a U-type GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer sequentially stacked along the epitaxial direction on the substrate. The multi-quantum-well layer comprises InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction; The GaN barrier layer includes GaN sublayers stacked along the epitaxial direction, and the Si doping concentration of the multiple GaN sublayers decreases layer by layer along the epitaxial direction; The GaN barrier layer has an AlGaN insertion layer, which is disposed between any two GaN sublayers.
[0010] As an improvement to the above technical solution, the multi-quantum well layer includes InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction, with a period number of 3 to 8; The InGaN well layer is undoped, with an In content of 0.18~0.28 and a thickness of 1nm~2.5nm. The GaN barrier layer has a thickness of 3nm~6nm, and the ratio of the thickness of the GaN barrier layer to the thickness of the InGaN well layer is 1.5~3.
[0011] As an improvement to the above technical solution, the Si doping concentration of the multilayer GaN sublayer decreases linearly along the epitaxial direction, and the Si doping concentration of the GaN sublayer is 0~8×10⁻⁶. 18 atoms / cm 3 The Si doping concentration of the multilayer GaN barrier decreases periodically along the epitaxial direction, and the Si doping concentration of the GaN barrier decreases by 3% to 10% between two adjacent periods.
[0012] As an improvement to the above technical solution, the GaN barrier layer is formed by stacking three GaN sublayers, and the GaN barrier layer includes a first GaN sublayer, a second GaN sublayer and a third GaN sublayer stacked sequentially along the epitaxial direction; The Si doping concentration of the first GaN sublayer is 3 × 10⁻⁶. 18 atoms / cm 3 ~8×10 18 atoms / cm 3 ; The Si doping concentration of the second GaN sublayer is 1×10⁻⁶. 18 atoms / cm3 ~3×10 18 atoms / cm 3 ; The Si doping concentration of the third GaN sublayer is 5 × 10⁻⁶. 17 atoms / cm 3 ~2×10 18 atoms / cm 3 ; Alternatively, the third GaN sublayer may not be doped.
[0013] As an improvement to the above technical solution, the Al composition content of the AlGaN insertion layer is 0.05~0.2, the thickness is 0.5nm~1.5nm, and the AlGaN insertion layer is located at 1 / 3~2 / 3 of the thickness of the GaN barrier layer.
[0014] Accordingly, the present invention also provides a method for fabricating an epitaxial structure for visible light communication, comprising the following steps: Provide substrate; A buffer layer is deposited on the substrate; A U-shaped GaN layer is deposited on the buffer layer; An N-type GaN layer is deposited on the U-type GaN layer; A multi-quantum-well layer is deposited on the N-type GaN layer; An electron blocking layer is deposited on the multi-quantum-well layer; A P-type GaN layer is deposited on the electron blocking layer; The multi-quantum-well layer comprises InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction; The GaN barrier layer includes GaN sublayers stacked along the epitaxial direction, and the Si doping concentration of the multiple GaN sublayers decreases layer by layer along the epitaxial direction; The GaN barrier layer has an AlGaN insertion layer, which is disposed between any two GaN sublayers.
[0015] As an improvement to the above technical solution, the method for preparing the GaN barrier layer includes the following steps: TMGa is introduced as a Ga source, NH3 as a nitrogen source, and SiH4 as a Si dopant. The flow rate of SiH4 is linearly adjusted to form multiple GaN sublayers, and the Si doping concentration of the multiple GaN sublayers decreases along the epitaxial direction. When the GaN barrier layer grows to 1 / 3 to 2 / 3 of the preset thickness, the introduction of SiH4 and TMGa is interrupted, and TMAl and TEGa are introduced instead to form the AlGaN insertion layer. After the AlGaN insertion layer is formed, TMGa and SiH4 are continued to be introduced, and the flow rate of SiH4 is continuously adjusted linearly to form multiple GaN sublayers.
[0016] As an improvement to the above technical solution, the multi-quantum well layer includes InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction, with a period number of 3 to 8; The InGaN well layer is undoped, with an In content of 0.18~0.28 and a thickness of 1nm~2.5nm. The GaN barrier layer has a thickness of 3nm~6nm, and the ratio of the thickness of the GaN barrier layer to the thickness of the InGaN well layer is 1.5~3. The Si doping concentration of the multilayer GaN sublayer decreases linearly along the epitaxial direction, and the Si doping concentration of the GaN sublayer is 0~8×10⁻⁶. 18 atoms / cm 3 The Si doping concentration of the multilayer GaN barrier decreases periodically along the epitaxial direction, and the Si doping concentration of the GaN barrier decreases by 3% to 10% between two adjacent periods.
[0017] As an improvement to the above technical solution, the Al composition content of the AlGaN insertion layer is 0.05~0.2, and the thickness is 0.5nm~1.5nm.
[0018] Accordingly, the present invention also provides a MicroLED chip, including the epitaxial structure for visible light communication described in the above technical solution; The MicroLED chip has a 3dB modulation bandwidth greater than 2.0GHz.
[0019] The implementation of this invention has the following beneficial effects: The multi-quantum well layer of the epitaxial structure for visible light communication of the present invention includes InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction; the GaN barrier layer includes GaN sub-layers stacked along the epitaxial direction, the Si doping concentration of the multiple GaN sub-layers decreases layer by layer along the epitaxial direction, and the GaN barrier layer has an AlGaN insertion layer, which is disposed between any two GaN sub-layers.
[0020] First, since the Si doping concentration of the GaN barrier layer decreases along the epitaxial direction, the highly doped section near the substrate effectively shields the polarization electric field and promotes hole tunneling, while the low-doped section near the P-type GaN layer maintains a sufficient confinement barrier for electrons. At the same time, the ultrathin aluminum nitride insertion layer forms a sharp electron reflection barrier in each barrier, which generates a multi-level distributed blockage of electron overflow through the quantum mechanical resonance reflection effect, thereby increasing the overlap rate of the electron-hole wave function and effectively improving the 3dB modulation bandwidth.
[0021] Secondly, the GaN barrier layer in each growth cycle has an AlGaN insertion layer. Because the distributed electron reflection barrier formed by the ultrathin aluminum nitride insertion layer in each barrier creates a multi-level blockage of electron overflow, rather than relying on a single thick electron blocking layer, the electron leakage under high current density is suppressed through a multi-level quantum reflection mechanism, and the efficiency roll-off is reduced at the same current density.
[0022] Finally, the AlGaN insertion layer in each cycle acts as an electron barrier, dispersing the electron reflection function into the AlGaN insertion layer inside each barrier, rather than concentrating it in a thick electron barrier layer. This effectively blocks electron leakage while maintaining the overall ultrathin structure, avoiding the obstruction of hole injection by the electron barrier layer. Attached Figure Description
[0023] Figure 1 This is a schematic diagram of an epitaxial structure for visible light communication according to an embodiment of the present invention; Figure 2 This is a schematic diagram of the structure of a multi-quantum well layer according to an embodiment of the present invention; Figure 3 This is a schematic diagram of the structure of a GaN barrier layer according to an embodiment of the present invention; Figure 4 This is a schematic diagram of the GaN barrier layer in another embodiment of the present invention. Detailed Implementation
[0024] To make the objectives, technical solutions, and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings.
[0025] See Figures 1 to 3 As shown, this embodiment of the invention provides an epitaxial structure for visible light communication, including a substrate 100, and a buffer layer 200, a U-type GaN layer 300, an N-type GaN layer 400, a multiple quantum well layer 500, an electron blocking layer 600 and a P-type GaN layer 700 sequentially stacked on the substrate 100 along the epitaxial direction.
[0026] This invention improves the GaN barrier layer 520 of the multi-quantum well layer 500 to enhance electron blocking capability without increasing the thickness of the electron blocking layer 600, and without hindering hole injection.
[0027] Specifically, the multi-quantum well layer 500 includes an InGaN well layer 510 and a GaN barrier layer 520 periodically stacked along the epitaxial direction; The GaN barrier layer 520 includes GaN sublayers 521 stacked along the epitaxial direction, and the Si doping concentration of the multiple GaN sublayers 521 decreases layer by layer along the epitaxial direction. The GaN barrier layer 520 has an AlGaN insertion layer 521, and the AlGaN insertion layer 522 is disposed between any two GaN sublayers 521.
[0028] First, the GaN barrier layer 520 includes GaN sublayers 521 stacked along the epitaxial direction, and the Si doping concentration of the multilayer GaN sublayers 521 decreases layer by layer along the epitaxial direction. Since the Si doping concentration near the substrate 100 is a high-doped region that effectively shields the polarization electric field and promotes hole tunneling, and the side near the electron blocking layer 600 is a low-doped region that maintains a sufficient confinement barrier for electrons, while the ultrathin AlGaN insertion layer 522 forms a sharp electron reflection barrier in each barrier, generating a multi-level distributed barrier against electron overflow through the quantum mechanical resonant reflection effect, thereby increasing the overlap rate of the electron-hole wave function and improving the 3dB modulation bandwidth.
[0029] Secondly, the GaN barrier layer 520 in each growth cycle has an AlGaN insertion layer 522. Since the distributed electron reflection barrier formed by the ultrathin aluminum nitride insertion layer in each barrier creates a multi-level blockage of electron overflow, instead of relying on a single thick electron blocking layer 600, the electron leakage under high current density is suppressed through a multi-level quantum reflection mechanism, and the efficiency roll-off is reduced at the same current density.
[0030] Finally, the AlGaN insertion layer 522 in each cycle acts as an electron barrier, dispersing the electron reflection function into the AlGaN insertion layer 522 inside each barrier, rather than concentrating it in a thick electron barrier layer 600. This effectively blocks electron leakage while maintaining the overall ultra-thin structure, avoiding the obstruction of hole injection by the electron barrier layer 600.
[0031] Preferably, the multi-quantum well layer 500 includes InGaN well layers 510 and GaN barrier layers 520 periodically stacked along the epitaxial direction, with a period number of 3 to 8; the period number can be 3, 4, 5, 6, 7, or 8.
[0032] The InGaN well layer 510 is undoped, with an In content of 0.18~0.28 and a thickness of 1nm~2.5nm. The GaN barrier layer 520 has a thickness of 3nm~6nm, and the ratio of the thickness of the GaN barrier layer 520 to the thickness of the InGaN well layer 510 is 1.5~3.
[0033] The In content of the InGaN well layer 510 can be 0.18, 0.22, 0.24, 0.25, 0.27, or 0.28, but is not limited to these. The thickness of the InGaN well layer 510 can be 1 nm, 1.2 nm, 1.5 nm, 1.8 nm, 1.9 nm, 2.2 nm, 2.4 nm, or 2.5 nm, but is not limited to these. The thickness of the GaN barrier layer 520 can be 3 nm, 3.7 nm, 4.2 nm, 4.7 nm, 4.9 nm, 5.3 nm, 5.8 nm, or 6 nm, but is not limited to these. The ratio of the thickness of the GaN barrier layer 520 to the thickness of the InGaN well layer 510 can be 1.5, 1.8, 1.9, 2.3, 2.5, 2.8, or 3, but is not limited to these.
[0034] The thickness ratio of the GaN barrier layer 520 to the InGaN well layer 510 is 1.5 to 3, providing an effective electronic barrier, suppressing electron leakage and overflow, and reducing efficiency roll-off. Simultaneously, the thin barrier layer allows holes to be transported to the deep quantum well via quantum tunneling, improving the uniformity of carrier spatial distribution and enhancing recombination rate and modulation bandwidth.
[0035] If the ratio is less than 1.5, the GaN barrier layer 520 is too thin, resulting in a lower barrier height. Electrons are prone to overflow under high injection current, exacerbating nonradiative recombination and efficiency roll-off, leading to power degradation. The thin barrier provides insufficient shielding against the polarization field, increasing electron leakage current and reducing modulation bandwidth due to carrier imbalance, thus limiting data transmission rate. If the ratio is greater than 3, the GaN barrier layer 520 is too thick, forming a high barrier that hinders hole tunneling to the deep quantum well, worsening conductor distribution uniformity, reducing recombination rate, and decreasing modulation bandwidth. The thick barrier layer increases the quantum well region capacitance, introducing signal delay under high-frequency modulation and limiting the maximum data transmission rate; it may also amplify the polarization electric field, reduce wavefunction overlap, and decrease luminous efficiency.
[0036] More preferably, the Si doping concentration of the multilayer GaN sublayer 521 decreases linearly along the epitaxial direction, and the Si doping concentration of the GaN sublayer 521 is 0~8×10⁻⁶. 18 atoms / cm 3 The Si doping concentration of the multilayer GaN barrier layer 520 decreases periodically along the epitaxial direction, and the Si doping concentration of the GaN barrier layer 520 decreases by 3% to 10% between two adjacent periods.
[0037] The Si doping concentration of the GaN sublayer 521 is 0~8×10⁻⁶. 18 atoms / cm 3The high doping concentration near the N-type GaN layer 400 can significantly neutralize the strong polarization charge, weaken the quantum confinement Stark effect, and improve the electron-hole wave function overlap rate; while the low or no Si doping concentration of the GaN sublayer 521 near the electron blocking layer 600 maintains the barrier height and avoids electron blocking ability.
[0038] The Si doping concentration of the GaN barrier layer 520 decreases periodically to achieve gradual control of the polarization field in the multi-quantum well layer 500, thus avoiding carrier transport imbalance caused by sudden changes in the electric field at the interface.
[0039] The Si doping concentration decreases by less than 3% in adjacent GaN barrier layers 520, and the difference in barrier height between adjacent quantum wells is too small to effectively establish a gradual electric field gradient, thus weakening the polarization field shielding effect. The Si doping concentration decreases by more than 10% in adjacent GaN barrier layers 520, and the abrupt change in barrier height forms a carrier transport barrier, resulting in electrons accumulating in the N-type GaN layer 400 and holes being blocked in the electron blocking layer 600, thus worsening the uniformity of carrier distribution.
[0040] In another embodiment of the invention, see Figure 4 As shown, the GaN barrier layer 520 is formed by stacking three GaN sublayers 521. The GaN barrier layer 520 includes a first GaN sublayer 521a, a second GaN sublayer 521b, and a third GaN sublayer 521c stacked sequentially along the epitaxial direction. The Si doping concentration of the first GaN sublayer 521a is 3 × 10⁻⁶. 18 atoms / cm 3 ~8×10 18 atoms / cm 3 ; The Si doping concentration of the second GaN sublayer 521b is 1×10⁻⁶. 18 atoms / cm 3 ~3×10 18 atoms / cm 3 ; The Si doping concentration of the third GaN sublayer 521c is 5 × 10⁻⁶. 17 atoms / cm 3 ~2×10 18 atoms / cm 3 ; Alternatively, the third GaN sublayer 521c may not be doped.
[0041] The Si doping concentration of the first GaN sublayer 521a can be 3 × 10⁻⁶. 18 atoms / cm 3 4×10 18atoms / cm 3 5×10 18 atoms / cm 3 6×10 18 atoms / cm 3 7×10 18 atoms / cm 3 8×10 18 atoms / cm 3 However, it is not limited to this.
[0042] The Si doping concentration of the second GaN sublayer 521b can be 1×10⁻⁶. 18 atoms / cm 3 1.2×10 18 atoms / cm 3 1.7×10 18 atoms / cm 3 1.9×10 18 atoms / cm 3 2.3×10 18 atoms / cm 3 2.7×10 18 atoms / cm 3 3×10 18 atoms / cm 3 However, it is not limited to this.
[0043] The Si doping concentration of the third GaN sublayer 521c can be 5 × 10⁻⁶. 17 atoms / cm 3 7×10 17 atoms / cm 3 9×10 17 atoms / cm 3 1.2×10 18 atoms / cm 3 1.7×10 18 atoms / cm 3 1.9×10 18 atoms / cm 3 2×10 18 atoms / cm 3 However, it is not limited to this.
[0044] More preferably, the Al composition content of the AlGaN insertion layer 522 is 0.05~0.2, the thickness is 0.5nm~1.5nm, and the AlGaN insertion layer 522 is located at 1 / 3~2 / 3 of the thickness of the GaN barrier layer 520.
[0045] The Al content of the AlGaN insertion layer 522 can be 0.05, 0.07, 0.09, 0.12, 0.14, 0.18, or 0.2%, but is not limited thereto. The thickness of the AlGaN insertion layer 522 can be 0.5 nm, 0.7 nm, 0.9 nm, 1.1 nm, 1.2 nm, 1.3 nm, 1.4 nm, or 1.5 nm, but is not limited thereto.
[0046] The Al content of the AlGaN insertion layer 522 is 0.05~0.2%, ensuring sufficient conduction band step, improving electron confinement capability, and suppressing electron leakage. Simultaneously, it avoids the introduction of strong lattice mismatch due to high Al content, preventing an increase in interface dislocations. When the Al content of the AlGaN insertion layer 522 is less than 0.05%, electron mobility decreases; when the Al content of the AlGaN insertion layer 522 is greater than 0.2%, interface roughness scattering is enhanced, and carrier mobility decreases.
[0047] The AlGaN insertion layer 522 has a thickness of 0.5 nm to 1.5 nm, which can balance polarization field shielding and carrier transport. If the thickness of the AlGaN insertion layer 522 is less than 0.5 nm, the polarization shielding will be insufficient; if the thickness of the AlGaN insertion layer 522 is greater than 1.5 nm, the interface barrier will be increased, hindering hole injection.
[0048] The AlGaN insertion layer 522 is located in the middle of the GaN barrier layer 520, forming a symmetrical barrier structure. More preferably, the AlGaN insertion layer 522 is located at 1 / 2 of the GaN barrier layer 520.
[0049] Accordingly, the present invention also provides a method for fabricating an epitaxial structure for visible light communication, comprising the following steps: Provide substrate; The substrate may be sapphire, but is not limited to it; A buffer layer is deposited on the substrate; A low-temperature GaN buffer layer was deposited on the substrate using the MOCVD method. The growth pressure in the reaction chamber was 100 torr to 200 torr, NH3 and TMGa were introduced, the growth temperature was 500℃ to 700℃, and the deposition thickness was 20nm to 50nm. A U-shaped GaN layer is deposited on the buffer layer; NH3 is introduced as the nitrogen source and TMGa is introduced as the Ga source. The growth temperature is 950℃~1100℃ and the growth pressure is 100 torr~300 torr. A three-dimensional island growth layer and a two-dimensional merged growth layer are deposited and grown sequentially to complete the deposition of the U-shaped GaN layer. An N-type GaN layer is deposited on the U-type GaN layer; The growth temperature was 1000℃~1100℃, the growth pressure was 100 torr~300 torr, NH3 and TMGa were introduced at a flow rate of 300 sccm~600 sccm, and SiH4 was introduced as an n-type dopant at a flow rate of 100 sccm~300 sccm. The Si doping concentration was 5×10⁻⁶. 18 atoms / cm 3 A Si-doped N-type GaN current-spreading layer with a thickness of 3000 nm to 4000 nm was grown. A multi-quantum-well layer is deposited on the N-type GaN layer; An electron blocking layer is deposited on the multi-quantum-well layer; The temperature is 880℃~1050℃, 100 torr~300 torr, NH3, TMGa and TMAl are introduced, and CP2Mg is introduced as Mg dopant to form the electron blocking layer; A P-type GaN layer is deposited on the electron blocking layer; The temperature is 900℃~1150℃, 100 torr~300 torr, and NH3, TMGa and CP2Mg are introduced to deposit the P-type GaN layer; The multi-quantum-well layer comprises InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction; The GaN barrier layer includes GaN sublayers stacked along the epitaxial direction, and the Si doping concentration of the multiple GaN sublayers decreases layer by layer along the epitaxial direction; The GaN barrier layer has an AlGaN insertion layer, which is disposed between any two GaN sublayers.
[0050] Preferably, TMGa is introduced as the Ga source, NH3 as the nitrogen source, and SiH4 as the Si dopant. The flow rate of SiH4 is linearly adjusted to form multiple GaN sublayers, and the Si doping concentration of the multiple GaN sublayers decreases along the epitaxial direction. When the GaN barrier layer grows to 1 / 3 to 2 / 3 of the preset thickness, the introduction of SiH4 and TMGa is interrupted, and TMAl and TEGa are introduced instead to form the AlGaN insertion layer. After the AlGaN insertion layer is formed, TMGa and SiH4 are continued to be introduced, and the flow rate of SiH4 is continuously adjusted linearly to form multiple GaN sublayers.
[0051] Preferably, the multi-quantum well layer comprises InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction, with a period number of 3 to 8; The InGaN well layer is undoped, with an In content of 0.18~0.28 and a thickness of 1nm~2.5nm. The GaN barrier layer has a thickness of 3nm~6nm, and the ratio of the thickness of the GaN barrier layer to the thickness of the InGaN well layer is 1.5~3. The Si doping concentration of the multilayer GaN sublayer decreases linearly along the epitaxial direction, and the Si doping concentration of the GaN sublayer is 0~8×10⁻⁶. 18 atoms / cm 3 The Si doping concentration of the multilayer GaN barrier decreases periodically along the epitaxial direction, and the Si doping concentration of the GaN barrier decreases by 3% to 10% between two adjacent periods.
[0052] Preferably, the Al composition content of the AlGaN insertion layer is 0.05~0.2, and the thickness is 0.5nm~1.5nm.
[0053] Accordingly, the present invention also provides a MicroLED chip, including the aforementioned epitaxial structure for visible light communication; The MicroLED chip has a 3dB modulation bandwidth greater than 2.0GHz.
[0054] The present invention will be further described below with reference to specific embodiments.
[0055] Example 1 This embodiment provides an epitaxial structure for visible light communication, including a substrate, and a buffer layer, a U-type GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer and a P-type GaN layer sequentially stacked on the substrate along the epitaxial direction; The multiple quantum well layer comprises InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction, with a period number of 6; The InGaN well layer is undoped, has an In content of 0.23, and a thickness of 1.8 nm. The thickness of the GaN barrier layer is 4.5 nm; The thickness ratio of the GaN barrier layer to the InGaN well layer is 2.5; The GaN barrier layer comprises multiple GaN sublayers, and the Si doping concentration of the multiple GaN sublayers varies from 8 × 10⁻⁶ along the epitaxial direction. 18 atoms / cm 3 Decrease to 5×10 17 atoms / cm 3 ; The GaN barrier layer has an AlGaN insertion layer located at 1 / 4 of the thickness of the GaN barrier layer; the AlGaN insertion layer has a thickness of 1 nm and an Al content of 0.1%.
[0056] This invention also provides a method for fabricating an epitaxial structure for visible light communication, comprising the following steps: Provide substrate; A buffer layer is deposited on the substrate; A U-shaped GaN layer is deposited on the buffer layer; An N-type GaN layer is deposited on the U-type GaN layer; A multi-quantum-well layer is deposited on the N-type GaN layer; An electron blocking layer is deposited on the multi-quantum-well layer; A P-type GaN layer is deposited on the electron blocking layer; The method for preparing the GaN barrier layer includes the following steps: TMGa is introduced as a Ga source, NH3 as a nitrogen source, and SiH4 as a Si dopant. The flow rate of SiH4 is linearly adjusted to form multiple GaN sublayers, and the Si doping concentration of the multiple GaN sublayers decreases along the epitaxial direction. When the GaN barrier layer grows to 1 / 3 to 2 / 3 of the preset thickness, the introduction of SiH4 and TMGa is interrupted, and TMAl and TEGa are introduced instead to form the AlGaN insertion layer. After the AlGaN insertion layer is formed, TMGa and SiH4 are continued to be introduced, and the flow rate of SiH4 is continuously adjusted linearly to form multiple GaN sublayers.
[0057] Example 2 The difference between this embodiment and Embodiment 1 is that: The multiple quantum well layer comprises InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction, with a period number of 6; The InGaN well layer is undoped, has an In content of 0.18, and a thickness of 2 nm. The thickness of the GaN barrier layer is 3 nm; The thickness ratio of the GaN barrier layer to the InGaN well layer is 1.5; The GaN barrier layer comprises multiple GaN sublayers, and the Si doping concentration of the multiple GaN sublayers increases from 3 × 10⁻⁶ along the epitaxial direction. 18 atoms / cm 3 Decrease to 2×10 17 atoms / cm 3 ; The GaN barrier layer has an AlGaN insertion layer located at 1 / 3 of the thickness of the GaN barrier layer; the AlGaN insertion layer has a thickness of 1.5 nm and an Al content of 0.2%.
[0058] Example 3 The difference between this embodiment and Embodiment 1 is that: The multiple quantum well layer comprises InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction, with a period number of 6; The InGaN well layer is undoped, has an In content of 0.28, and a thickness of 2 nm. The thickness of the GaN barrier layer is 6 nm; The thickness ratio of the GaN barrier layer to the InGaN well layer is 3; The GaN barrier layer comprises multiple GaN sublayers, and the Si doping concentration of the multiple GaN sublayers increases from 3 × 10⁻⁶ along the epitaxial direction. 18 atoms / cm 3 Decrease to 2×10 17 atoms / cm 3 ; The GaN barrier layer has an AlGaN insertion layer located at 1 / 2 of the thickness of the GaN barrier layer; the AlGaN insertion layer has a thickness of 1.5 nm and an Al content of 0.2%.
[0059] Example 4 The difference between this embodiment and Embodiment 1 is that: The GaN barrier layer is composed of three GaN sublayers stacked together, and the GaN barrier layer includes a first GaN sublayer, a second GaN sublayer and a third GaN sublayer stacked sequentially along the epitaxial direction; The Si doping concentration of the first GaN sublayer is 5 × 10⁻⁶. 18 atoms / cm 3 ; The Si doping concentration of the second GaN sublayer is 3 × 10⁻⁶. 18 atoms / cm 3 ; The Si doping concentration of the third GaN sublayer is 1×10⁻⁶. 18 atoms / cm 3 ; The GaN barrier layer includes an AlGaN insertion layer located at 1 / 3 of the thickness of the GaN barrier layer; the AlGaN insertion layer has a thickness of 1 nm and an Al content of 0.1%. Furthermore, the total Si doping concentration of the GaN barrier layer decreases by 6% in two adjacent growth cycles.
[0060] Example 5 The difference between this embodiment and embodiment 4 is that: The total Si doping concentration of the GaN barrier layer decreases by 12% in two adjacent growth cycles.
[0061] Comparative Example 1 The difference between this comparative example and Example 1 is as follows: The GaN barrier layer can be a single layer or multiple layers, and all multiple GaN barrier layers are uniformly doped layers. The Si doping concentration of the GaN barrier layer is 5 × 10⁻⁶. 18 atoms / cm 3 Furthermore, the AlGaN insertion layer is not provided in the GaN barrier layer.
[0062] Comparative Example 2 The difference between this comparative example and Example 1 is as follows: The AlGaN insertion layer is not provided in the GaN barrier layer.
[0063] Performance testing: Examples 1 to 5, and Comparative Examples 1 to 2, were fabricated into 80μm × 80μm MicroLED chips, and the current density was 300A / cm². 2 The test chip's optical output power increase (%) and efficiency roll-off (%) were measured. The optical output power increase was calculated based on Comparative Example 1.
[0064] The performance test results are shown in the table below.
[0065]
[0066] As can be seen from Examples 1 to 5 and Comparative Example 1, the Si doping concentration of the GaN barrier layer decreases along the epitaxial direction. The highly doped section near the substrate effectively shields the polarization electric field and promotes hole tunneling, while the low-doped section near the P-type GaN layer maintains a sufficient confinement barrier for electrons, thereby increasing the overlap rate of the electron-hole wave function, effectively improving the optical output power of the chip and reducing the efficiency roll-off.
[0067] As can be seen from Comparative Example 2, the AlGaN insertion layer in each cycle acts as an electron barrier, resulting in a reduced efficiency roll-off at the same current density.
[0068] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention.
Claims
1. An epitaxial structure for visible light communication, characterized in that, It includes a substrate, and a buffer layer, a U-type GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer and a P-type GaN layer sequentially stacked on the substrate along the epitaxial direction; The multi-quantum-well layer comprises InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction; The GaN barrier layer includes GaN sublayers stacked along the epitaxial direction, and the Si doping concentration of the multiple GaN sublayers decreases layer by layer along the epitaxial direction; The GaN barrier layer has an AlGaN insertion layer, which is disposed between any two GaN sublayers.
2. The epitaxial structure for visible light communication as described in claim 1, characterized in that, The multiple quantum well layer comprises InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction, with a period number of 3 to 8; The InGaN well layer is undoped, with an In content of 0.18~0.28 and a thickness of 1nm~2.5nm; the GaN barrier layer has a thickness of 3nm~6nm, and the ratio of the thickness of the GaN barrier layer to the thickness of the InGaN well layer is 1.5~3.
3. The epitaxial structure for visible light communication as described in claim 1 or 2, characterized in that, The Si doping concentration of the multilayer GaN sublayer decreases linearly along the epitaxial direction, and the Si doping concentration of the GaN sublayer is 0~8×10⁻⁶. 18 atoms / cm 3 The Si doping concentration of the multilayer GaN barrier decreases periodically along the epitaxial direction, and the Si doping concentration of the GaN barrier decreases by 3% to 10% between two adjacent periods.
4. The epitaxial structure for visible light communication as described in claim 3, characterized in that, The GaN barrier layer is composed of three GaN sublayers stacked together, and the GaN barrier layer includes a first GaN sublayer, a second GaN sublayer and a third GaN sublayer stacked sequentially along the epitaxial direction; The Si doping concentration of the first GaN sublayer is 3 × 10⁻⁶. 18 atoms / cm 3 ~8×10 18 atoms / cm 3 ; The Si doping concentration of the second GaN sublayer is 1×10⁻⁶. 18 atoms / cm 3 ~3×10 18 atoms / cm 3 ; The Si doping concentration of the third GaN sublayer is 5 × 10⁻⁶. 17 atoms / cm 3 ~2×10 18 atoms / cm 3 ; Alternatively, the third GaN sublayer may not be doped.
5. The epitaxial structure for visible light communication as described in claim 3, characterized in that, The Al composition content of the AlGaN insertion layer is 0.05~0.2, and the thickness is 0.5nm~1.5nm. The AlGaN insertion layer is located at 1 / 3~2 / 3 of the thickness of the GaN barrier layer.
6. A method for fabricating an epitaxial structure for visible light communication as described in any one of claims 1 to 5, characterized in that, Includes the following steps: Provide substrate; A buffer layer is deposited on the substrate; A U-shaped GaN layer is deposited on the buffer layer; An N-type GaN layer is deposited on the U-type GaN layer; A multi-quantum-well layer is deposited on the N-type GaN layer; An electron blocking layer is deposited on the multi-quantum-well layer; A P-type GaN layer is deposited on the electron blocking layer; The multi-quantum-well layer comprises InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction; The GaN barrier layer includes GaN sublayers stacked along the epitaxial direction, and the Si doping concentration of the multiple GaN sublayers decreases layer by layer along the epitaxial direction; The GaN barrier layer has an AlGaN insertion layer, which is disposed between any two GaN sublayers.
7. The method for fabricating an epitaxial structure for visible light communication as described in claim 6, characterized in that, The method for preparing the GaN barrier layer includes the following steps: TMGa is introduced as a Ga source, NH3 as a nitrogen source, and SiH4 as a Si dopant. The flow rate of SiH4 is linearly adjusted to form multiple GaN sublayers, and the Si doping concentration of the multiple GaN sublayers decreases along the epitaxial direction. When the GaN barrier layer grows to 1 / 3 to 2 / 3 of the preset thickness, the introduction of SiH4 and TMGa is interrupted, and TMAl and TEGa are introduced instead to form the AlGaN insertion layer. After the AlGaN insertion layer is formed, TMGa and SiH4 are continued to be introduced, and the flow rate of SiH4 is continuously adjusted linearly to form multiple GaN sublayers.
8. The method for fabricating an epitaxial structure for visible light communication as described in claim 7, characterized in that, The multiple quantum well layer comprises InGaN well layers and GaN barrier layers periodically stacked along the epitaxial direction, with a period number of 3 to 8; The InGaN well layer is undoped, with an In content of 0.18~0.28 and a thickness of 1nm~2.5nm. The GaN barrier layer has a thickness of 3nm~6nm, and the ratio of the thickness of the GaN barrier layer to the thickness of the InGaN well layer is 1.5~3. The Si doping concentration of the multilayer GaN sublayer decreases linearly along the epitaxial direction, and the Si doping concentration of the GaN sublayer is 0~8×10⁻⁶. 18 atoms / cm 3 The Si doping concentration of the multilayer GaN barrier decreases periodically along the epitaxial direction, and the Si doping concentration of the GaN barrier decreases by 3% to 10% between two adjacent periods.
9. The method for fabricating an epitaxial structure for visible light communication as described in claim 7, characterized in that, The Al composition content of the AlGaN insertion layer is 0.05~0.2, and the thickness is 0.5nm~1.5nm.
10. A MicroLED chip, characterized in that, Includes the epitaxial structure for visible light communication as described in any one of claims 1 to 5; The MicroLED chip has a 3dB modulation bandwidth greater than 2.0GHz.