A wide-bandgap perovskite solar cell based on guanidine hydrochloride synergistic passivation, its fabrication method and application

By using a biguanide hydrochloride passivation layer in perovskite solar cells, the defect problem of perovskite thin films was solved, resulting in high-efficiency and high-stability perovskite solar cells and improved carrier extraction and transport performance.

CN123124566APending Publication Date: 2026-11-17NANKAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610979266.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing perovskite solar cells suffer from numerous defects during fabrication due to lattice distortion and loss of volatile components, affecting carrier transport efficiency and device stability. Furthermore, existing passivating agents are prone to desorption or degradation under high temperatures or light exposure, making it difficult to achieve high efficiency and high stability.

Method used

Using biguanide hydrochloride as a passivation material, it forms a multifunctional passivation layer by strongly coordinating with uncoordinated lead ions on the perovskite surface and filling halogen vacancies, thereby improving battery efficiency and stability.

Benefits of technology

It significantly reduces surface defects in perovskite thin films, inhibits halide ion migration, improves open-circuit voltage and power conversion efficiency, and enhances device stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124566A_ABST
    Figure CN123124566A_ABST
Patent Text Reader

Abstract

A wide-bandgap perovskite solar cell based on guanidine hydrochloride synergistic passivation, its fabrication method, and its application are disclosed, relating to the field of solar cell technology. The solar cell structure, from bottom to top, comprises a glass substrate, a transparent electrode, a hole transport layer, a perovskite light-absorbing layer, a passivation layer, an electron transport layer, a buffer layer, and a metal electrode. The guanidine hydrochloride passivation layer material provided by this invention can react with uncoordinated Pb in the perovskite. 2+ By coordinating and filling halogen vacancies and forming a hydrogen bond network, the surface defects of perovskite films are significantly reduced, the film quality is improved, and thus the open-circuit voltage and photoelectric conversion efficiency of perovskite solar cells are significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solar cell technology, specifically to a wide-bandgap perovskite solar cell using biguanide hydrochloride as a synergistic passivation material and its preparation method. Background Technology

[0002] Perovskite solar cells, as outstanding representatives of third-generation thin-film solar cells, have achieved a leapfrog development in photoelectric conversion efficiency (PCE) from an initial 3.8% to over 27% in just over a decade, thanks to their excellent photoelectric properties, such as high absorption coefficient, long carrier diffusion length, and continuously tunable bandgap, demonstrating enormous commercial potential. However, perovskite materials are essentially ionic crystals. During the preparation of polycrystalline thin films using low-cost solution methods, rapid solvent evaporation and runaway crystallization kinetics inevitably lead to a large amount of lattice distortion inside and on the surface of the film. These defects not only limit the carrier transport efficiency but are also key physical factors that cause devices to encounter bottlenecks on the path to high efficiency.

[0003] At the surface and grain boundaries of perovskite films, large amounts of uncoordinated lead ions (Pb) are typically formed due to lattice truncation and the loss of volatile components (such as methylamine cations or iodine). 2+ Dangling bonds and halogen vacancies. These sites form nonradiative recombination centers in the band gap, causing significant energy dissipation of photogenerated carriers before they reach the electrodes, thus significantly reducing the device's open-circuit voltage (V). OC Furthermore, these defect sites are often chemically unstable weak points that readily adsorb water molecules from the environment or react with oxygen, triggering chemical degradation of the perovskite structure from the outside in and exacerbating ion migration, severely weakening the long-term stability of the battery under real-world service conditions.

[0004] To address these challenges, surface passivation technology has become a core process for improving the overall performance of perovskite solar cells. While current research has explored various organic amine salts, polymers, or small-molecule electrolytes as passivating agents, many materials suffer from limited functionality, often only targeting one type of defect (cation or anion). Furthermore, some passivating agents are prone to desorption or degradation under high temperatures or light exposure. Therefore, developing a multifunctional passivation material with multi-site synergistic passivation capabilities—capable of effectively anchoring metal cations through strong coordination, enhancing lattice stability through ion filling and hydrogen bonding networks, and exhibiting good chemical compatibility—is of paramount scientific and economic value for the industrial application of high-efficiency, high-stability perovskite solar cells. Summary of the Invention

[0005] The purpose of this invention is to provide a wide-bandgap perovskite solar cell passivated with biguanide hydrochloride and its preparation method. The abundant highly electronegative nitrogen-containing functional groups (imino and amino groups) in the biguanide molecule bind to uncoordinated lead ions on the perovskite surface, while chloride ions fill halogen vacancies, thereby synergistically improving the cell's efficiency and stability.

[0006] To achieve the above-mentioned objectives, the present invention provides the following technical solution:

[0007] This invention provides a perovskite solar cell, the structure of which, from bottom to top, includes a transparent electrode substrate, a hole transport layer, a perovskite light absorption layer, a passivation layer, an electron transport layer, a buffer layer, and a metal electrode.

[0008] The passivation material is guanidine hydrochloride, and its structural formula is shown below:

[0009]

[0010] The passivation material has the molecular formula C2H7N5·HCl.

[0011] The passivating agent is dissolved in an organic solvent and spin-coated onto the surface of the perovskite light-absorbing layer.

[0012] Preferably, the perovskite solar cell is a PIN-type perovskite solar cell;

[0013] The perovskite solar cell is a single-junction perovskite solar cell; or a perovskite / crystalline silicon tandem solar cell.

[0014] The perovskite solar cell has a wide bandgap of 1.60 eV or more.

[0015] Preferably, the perovskite material is an organic-inorganic hybrid multi-halogen mixed perovskite material.

[0016] Preferably, the underlying substrate includes one or more of transparent glass, flexible PET substrate, and flexible PEN substrate.

[0017] Preferably, the transparent electrode can be one or more of the following: FTO transparent electrode, ITO transparent electrode, IZO transparent electrode, IZrO transparent electrode, AZO transparent electrode, and oxide-metal-oxide multilayer composite transparent electrode.

[0018] Preferably, the hole transport layer is PTAA, Poly-TPD, Spiro-TTB, PEDOT:PSS, P3HT, a self-assembled monolayer, CuSCN, or NiO. x One or more of organic or inorganic hole transport materials;

[0019] The self-assembled monolayer includes one or more of (2-(9H-carbazole-9-yl)ethyl)phosphonic acid (2PACz), (2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl)phosphonic acid (MeO-2PACz), and (4-(3,6-dimethyl-9H-carbazole-9-yl)butyl)phosphonic acid (Me-4PACz).

[0020] Preferably, the electron transport layer is SnO2, TiO2, ZnO, PCBM, or C. 60 One or more of other electron transport materials such as fullerene derivatives.

[0021] Preferably, the buffer layer is one or more of BCP, PEI, ZnO, SnO2, Al2O3, SiO2, LiF and MgF2;

[0022] Preferably, the metal electrode material is one or more of Ag, Au, Cu, and Al, and the thickness is 80~120 nm.

[0023] This invention provides a method for preparing a perovskite solar cell, characterized in that,

[0024] Step 1: Pretreatment of transparent conductive substrate;

[0025] Step 2: Prepare a hole transport layer on the surface of the pretreated transparent conductive substrate;

[0026] Step 3: Coat the perovskite precursor solution onto the surface of the hole transport layer to prepare the perovskite light absorption layer.

[0027] Step 4: Spin-coat the passivating agent onto the surface of the perovskite light-absorbing layer to prepare the passivation layer;

[0028] Step 5: Spin-coat an electron transport material onto the surface of the interface passivation layer to prepare an electron transport layer;

[0029] Step 6: Prepare a buffer layer on the surface of the electron transport layer;

[0030] Step 7: Prepare a metal electrode on the surface of the buffer layer;

[0031] The passivating agent has the structural formula of the biguanide hydrochloride described above in this invention.

[0032] In this invention, the perovskite absorber layer is prepared by a blade coating method, wherein the blade coating speed is 5~15 mm / s, the nitrogen purging speed is 5~15 mm / s, and the blade coating time is 10~30 s;

[0033] The annealing temperature is 100~150℃, and the annealing time is 10~60 min.

[0034] In this invention, the passivation layer preparation method includes:

[0035] Biguanide hydrochloride was dissolved in an organic solvent to obtain a mixed slurry;

[0036] The organic solvent is one or more of chlorobenzene, ethyl acetate, isopropanol, and anisole;

[0037] The mixed slurry is coated onto the surface of the perovskite absorber layer at a coating speed of 5-15 mm / s; the annealing temperature is 50-100℃ and the annealing time is 10-30 min.

[0038] Advantages and positive effects of the present invention:

[0039] 1. The present invention proposes a method for preparing a perovskite passivation layer, which involves dissolving biguanide hydrochloride in an organic solvent and then depositing it onto the surface of a perovskite light-absorbing layer. This method can significantly reduce surface defects in wide-bandgap perovskite films, inhibit halide ion migration, and significantly improve the efficiency and stability of perovskite solar cells.

[0040] 2. The biguanide hydrochloride described in this invention can optimize the energy level structure of perovskite solar cells, promote electron extraction and transport, and significantly improve the open-circuit voltage of perovskite solar cells. Attached Figure Description

[0041] Figure 1 This is a schematic diagram of the structure of the perovskite solar cell provided by the present invention.

[0042] Figure 2 The JV curve of the perovskite solar cell described in Example 1 of this invention;

[0043] Figure 3 The JV curve of the perovskite solar cell described in Example 2 of this invention;

[0044] Figure 4 The JV curve of the perovskite solar cell described in Example 3 of this invention;

[0045] Figure 5 The JV curve of the perovskite solar cell described in Comparative Example 1 of this invention; Detailed Implementation

[0046] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments, nor do they limit the content and scope of protection of the present invention. Where specific experimental steps or conditions are not specified in the embodiments, they can be performed according to the conventional experimental steps or conditions described in the literature in the art. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.

[0047] Example 1

[0048] The PIN-type perovskite solar cell provided in this embodiment has a bandgap of approximately 1.68 eV, and its structure is as follows: Figure 1 As shown, from bottom to top, it includes: transparent glass, ITO, Me-4PACz (hole transport layer), perovskite light absorption layer, biguanide hydrochloride (passivation layer), PCBM (electron transport layer), BCP (buffer layer), and silver electrode.

[0049] The method for fabricating a PIN-type perovskite solar cell in this embodiment includes the following steps:

[0050] Step 1, Transparent Electrode Pretreatment: Clean the ITO conductive glass in sequence with detergent, deionized water, and isopropanol, then dry it with nitrogen and treat it with ultraviolet ozone.

[0051] Step 2, Preparation of hole transport layer: Transfer the pretreated ITO conductive glass to an N2 glove box and spin-coat the ITO surface with Me-4PACz solution as a hole transport layer.

[0052] Step 3, Preparation of perovskite light-absorbing layer: (1) Preparation of 1.6 MCs in DMF / NMP (9 / 1:v / v) co-solvent x FA 1-x Pb(I y Br 1-y (2) The obtained perovskite precursor solution was scraped onto the surface of the hole transport layer at a scraping speed of 9 mm / s, a nitrogen purging speed of 5 mm / s, and a scraping time of 15 s; (3) The obtained wet film was annealed at 130 ℃ for 30 min to obtain the perovskite light absorption layer.

[0053] Step 4, prepare the passivation layer: (1) Dissolve 0.2 mg of biguanide hydrochloride in 1 mL of organic solvent (ethanol) to form a passivating agent; (2) Spin coat the passivating agent onto the surface of the perovskite light absorption layer at a spin coating speed of 4000 rpm / min; (3) Anneal the obtained film at 100 °C for 5 min.

[0054] Step 5, prepare the electron transport layer: spin-coat a chlorobenzene solution (20 mg / ml) of PCBM onto the surface of the interface passivation layer as the electron transport layer at a spin-coating speed of 2000 rpm / min.

[0055] Step 6, Prepare the buffer layer: Spin-coat a BCP isopropanol solution (0.5 mg / ml) as a buffer layer on the surface of the electron transport layer at a spin-coating speed of 5000 rpm / min.

[0056] Step 7, Prepare the metal electrode: Prepare a silver electrode on the surface of the buffer layer.

[0057] Step 8, Photovoltaic performance testing: The effective area of ​​the perovskite solar cell device prepared by the above method is 0.08875 cm². 2 At 100 mW / cm 2 Measurements were taken under illumination (AM 1.5G), with a scanning range from 1.3 V to 0 V and a scanning step size of 0.02 V.

[0058] The JV characteristic curves of the obtained perovskite solar cells are as follows: Figure 2 As shown, by Figure 2 It can be seen that the open-circuit voltage of the perovskite solar cell is 1.229 V, the fill factor is 82.92%, and the short-circuit current density is 20.88 mA / cm². 2 The power conversion efficiency is 21.32%.

[0059] Example 2

[0060] The PIN-type perovskite solar cell provided in this embodiment has a bandgap of approximately 1.68 eV, and its structure is as follows: Figure 1 As shown, from bottom to top, it includes: transparent glass, ITO, Me-4PACz (hole transport layer), perovskite light absorption layer, biguanide hydrochloride (passivation layer), PCBM (electron transport layer), BCP (buffer layer), and silver electrode.

[0061] The method for fabricating a PIN-type perovskite solar cell in this embodiment includes the following steps:

[0062] Step 1, Transparent Electrode Pretreatment: Clean the ITO conductive glass in sequence with detergent, deionized water, and isopropanol, then dry it with nitrogen and treat it with ultraviolet ozone.

[0063] Step 2, Preparation of hole transport layer: Transfer the pretreated ITO conductive glass to an N2 glove box and spin-coat the ITO surface with Me-4PACz solution as a hole transport layer.

[0064] Step 3, Preparation of perovskite light-absorbing layer: (1) Preparation of 1.6 MCs in DMF / NMP (9 / 1:v / v) co-solventx FA 1-x Pb(I y Br 1-y (2) The obtained perovskite precursor solution was scraped onto the surface of the hole transport layer at a scraping speed of 9 mm / s, a nitrogen purging speed of 5 mm / s, and a scraping time of 15 s; (3) The obtained wet film was annealed at 130 ℃ for 30 min to obtain the perovskite light absorption layer.

[0065] Step 4, prepare the passivation layer: (1) Dissolve 0.5 mg of biguanide hydrochloride in 1 mL of organic solvent (ethanol) to form a passivating agent; (2) Spin coat the passivating agent onto the surface of the perovskite light absorption layer at a spin coating speed of 4000 rpm / min; (3) Anneal the obtained film at 100 °C for 5 min.

[0066] Step 5, prepare the electron transport layer: spin-coat a chlorobenzene solution (20 mg / ml) of PCBM onto the surface of the interface passivation layer as the electron transport layer at a spin-coating speed of 2000 rpm / min.

[0067] Step 6, Prepare the buffer layer: Spin-coat a BCP isopropanol solution (0.5 mg / ml) as a buffer layer on the surface of the electron transport layer at a spin-coating speed of 5000 rpm / min.

[0068] Step 7, Prepare the metal electrode: Prepare a silver electrode on the surface of the buffer layer.

[0069] Step 8, Photovoltaic performance testing: The effective area of ​​the perovskite solar cell device prepared by the above method is 0.08875 cm². 2 At 100 mW / cm 2 Measurements were taken under illumination (AM 1.5G), with a scanning range from 1.3 V to 0 V and a scanning step size of 0.02 V.

[0070] The JV characteristic curves of the obtained perovskite solar cells are as follows: Figure 3 As shown, by Figure 3 It is known that the open-circuit voltage of the perovskite solar cell is 1.245 V, the fill factor is 84.11%, and the short-circuit current density is 21.20 mA / cm². 2 The power conversion efficiency is 22.23%.

[0071] Example 3

[0072] The PIN-type perovskite solar cell provided in this embodiment has a bandgap of approximately 1.68 eV, and its structure is as follows: Figure 1As shown, from bottom to top, it includes: transparent glass, ITO, Me-4PACz (hole transport layer), perovskite light absorption layer, biguanide hydrochloride (passivation layer), PCBM (electron transport layer), BCP (buffer layer), and silver electrode.

[0073] The method for fabricating a PIN-type perovskite solar cell in this embodiment includes the following steps:

[0074] Step 1, Transparent Electrode Pretreatment: Clean the ITO conductive glass in sequence with detergent, deionized water, and isopropanol, then dry it with nitrogen and treat it with ultraviolet ozone.

[0075] Step 2, Preparation of hole transport layer: Transfer the pretreated ITO conductive glass to an N2 glove box and spin-coat the ITO surface with Me-4PACz solution as a hole transport layer.

[0076] Step 3, Preparation of perovskite light-absorbing layer: (1) Preparation of 1.6 MCs in DMF / NMP (9 / 1:v / v) co-solvent x FA 1-x Pb(I y Br 1-y (2) The obtained perovskite precursor solution was scraped onto the surface of the hole transport layer at a scraping speed of 9 mm / s, a nitrogen purging speed of 5 mm / s, and a scraping time of 15 s; (3) The obtained wet film was annealed at 130 ℃ for 30 min to obtain the perovskite light absorption layer.

[0077] Step 4, prepare the passivation layer: (1) Dissolve 0.8 mg of biguanide hydrochloride in 1 mL of organic solvent (ethanol) to form a passivating agent; (2) Spin coat the passivating agent onto the surface of the perovskite light absorption layer at a spin coating speed of 4000 rpm / min; (3) Anneal the obtained film at 100 °C for 5 min.

[0078] Step 5, prepare the electron transport layer: spin-coat a chlorobenzene solution (20 mg / ml) of PCBM onto the surface of the interface passivation layer as the electron transport layer at a spin-coating speed of 2000 rpm / min.

[0079] Step 6, Prepare the buffer layer: Spin-coat a BCP isopropanol solution (0.5 mg / ml) as a buffer layer on the surface of the electron transport layer at a spin-coating speed of 5000 rpm / min.

[0080] Step 7, Prepare the metal electrode: Prepare a silver electrode on the surface of the buffer layer.

[0081] Step 8, Photovoltaic performance testing: The effective area of ​​the perovskite solar cell device prepared by the above method is 0.08875 cm². 2At 100 mW / cm 2 Measurements were taken under illumination (AM 1.5G), with a scanning range from 1.3 V to 0 V and a scanning step size of 0.02 V.

[0082] The JV characteristic curves of the obtained perovskite solar cells are as follows: Figure 4 As shown, by Figure 4 It can be seen that the open-circuit voltage of the perovskite solar cell is 1.241 V, the fill factor is 81.31%, and the short-circuit current density is 21.18 mA / cm². 2 The power conversion efficiency is 21.41%.

[0083] Comparative Example 1

[0084] The comparative example provides a PIN-type perovskite solar cell with a band gap of approximately 1.68 eV, which, from bottom to top, includes: transparent glass, ITO, Me-4PACz (hole transport layer), perovskite light absorption layer, PCBM (electron transport layer), BCP (buffer layer), and silver electrode.

[0085] To further compare the technical solution of the present invention and its beneficial effects, the perovskite solar cell prepared is prepared in a manner that is roughly the same as that in Example 1, except that step 4, the preparation of the passivation layer, is omitted in this comparative example.

[0086] The JV characteristic curves of the obtained perovskite solar cells are as follows: Figure 5 As shown, by Figure 5 It is known that the open-circuit voltage of the perovskite solar cell is 1.224 V, the fill factor is 80.62%, and the short-circuit current density is 20.40 mA / cm². 2 The power conversion efficiency is 20.17%.

[0087] In summary, this invention, by preparing a biguanide hydrochloride passivation layer, results in perovskite films with fewer surface defects, significantly improving carrier extraction and transport. Perovskite solar cells prepared using this method ultimately achieve higher open-circuit voltage and photoelectric conversion efficiency. This method is simple to operate, easy to implement, and has good reproducibility, showing promising application prospects in the fabrication of large-area perovskite solar cells and modules.

[0088] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A perovskite solar cell, characterized in that, The solar cell structure, from bottom to top, includes a transparent conductive substrate, a hole transport layer, a perovskite light absorption layer, a passivation layer, an electron transport layer, a buffer layer, and a metal electrode. The passivation layer is guanidine hydrochloride, which is deposited on the surface of the perovskite light-absorbing layer. The structural formula of guanidine hydrochloride is: The molecular formula is C2H7N5·HCl.

2. The perovskite solar cell as described in claim 1, characterized in that, The perovskite solar cell is a PIN-type perovskite solar cell. The perovskite solar cell is a single-junction perovskite solar cell or a perovskite / crystalline silicon tandem solar cell. The perovskite solar cell has a wide bandgap of 1.60 eV or more. The perovskite material is an organic-inorganic hybrid multi-halogen mixed perovskite material.

3. The perovskite solar cell as described in claim 1, characterized in that, The transparent electrode is one or more of the following: FTO transparent electrode, ITO transparent electrode, IZO transparent electrode, IZrO transparent electrode, AZO transparent electrode, and oxide-metal-oxide multilayer composite transparent electrode.

4. The perovskite solar cell as described in claim 1, characterized in that, The hole transport layer is composed of PTAA, Poly-TPD, Spiro-TTB, PEDOT:PSS, P3HT, self-assembled monolayer, CuSCN, or NiO. x One or more of organic or inorganic hole transport materials; The self-assembled monolayer includes one or more of the following: (2-(9H-carbazole-9-yl)ethyl)phosphonic acid, (2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl)phosphonic acid, and (4-(3,6-dimethyl-9H-carbazole-9-yl)butyl)phosphonic acid self-assembled monolayers.

5. The perovskite solar cell as described in claim 1, characterized in that, The electron transport layer is SnO2, TiO2, ZnO, PCBM, or C. 60 One or more of fullerene derivative electron transport materials; The buffer layer is one or more of BCP, PEI, ZnO, SnO2, Al2O3, SiO2, LiF or MgF2.

6. The perovskite solar cell as described in claim 1, characterized in that, The metal electrode material is one or more of Ag, Au, Cu, and Al, and has a thickness of 80~120 nm.

7. The perovskite solar cell as described in claim 1, characterized in that, The underlying substrate is one or more of transparent glass, flexible PET substrate, and flexible PEN substrate.

8. The method for preparing a perovskite solar cell according to any one of claims 1-7, characterized in that, Step 1: Pretreatment of transparent conductive substrate; Step 2: Prepare a hole transport layer on the surface of the pretreated transparent conductive substrate; Step 3: Coat the perovskite precursor solution onto the surface of the hole transport layer to prepare the perovskite light absorption layer. Step 4: Spin-coat the passivating agent onto the surface of the perovskite light-absorbing layer to prepare the passivation layer; Step 5: Spin-coat an electron transport material onto the surface of the interface passivation layer to prepare an electron transport layer; Step 6: Prepare a buffer layer on the surface of the electron transport layer; Step 7: Prepare a metal electrode on the surface of the buffer layer; The passivating agent has the following structural formula: The molecular formula is C2H7N5·HCl; By utilizing the abundant highly electronegative nitrogen-containing functional groups imino and amino in the biguanide molecule, they can bind to uncoordinated lead ions on the perovskite surface, while chloride ions are used to fill halogen vacancies, thus synergistically improving the efficiency and stability of the battery.

9. The method for preparing a perovskite solar cell as described in claim 8, characterized in that, The perovskite absorber layer is prepared by a blade coating method, wherein the blade coating speed is 5~15 mm / s, the nitrogen purging speed is 5~15 mm / s, and the blade coating time is 10~30s. The annealing temperature is 100~150℃, and the annealing time is 10~60 min.

10. The method for preparing a perovskite solar cell as described in claim 8, characterized in that, The method for preparing the passivation layer includes: Biguanide hydrochloride was dissolved in an organic solvent to obtain a mixed slurry; The organic solvent is one or more of chlorobenzene, ethyl acetate, methanol, ethanol, isopropanol, and anisole; The mixed slurry was coated onto the surface of the perovskite absorber layer and then annealed. The coating speed is 5~15 mm / s; the annealing temperature is 50~100℃; and the annealing time is 10~30 min.