A method for controlling perovskite solar cells with polyvinylpyrrolidone
By using polyvinylpyrrolidone to regulate the self-assembled monolayer of 4PADCB in perovskite solar cells, the problem of interface defects caused by the easy aggregation of self-assembled monolayers was solved, and higher open-circuit voltage, fill factor and photoelectric conversion efficiency were achieved.
Patent Information
- Application Number
- CN202611368084.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-17
AI Technical Summary
Self-assembled monolayers tend to aggregate in perovskite solar cells, leading to uneven interface coverage, leakage channels, and interface recombination centers, which affect the open-circuit voltage, fill factor, and operational stability of the device.
A self-assembled monolayer material, 4PADCB, containing carbazole and phosphonic acid anchoring groups, was used. Through the coordination of the carbonyl group of the lactam in polyvinylpyrrolidone with the phosphonic acid group of 4PADCB, the formation of polymer intercalation state was promoted, the intermolecular π-π aggregation was inhibited, and the material coordinated with Pb-related species in the perovskite precursor at the buried interface, thereby improving the interfacial wettability and crystallinity.
This achieves continuous and flat coverage of the hole-selective layer, reduces leakage current channels and interface recombination, improves open-circuit voltage, fill factor and photoelectric conversion efficiency, and enhances the stability and performance of the device.
Smart Images

Figure CN123124645A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of interface engineering technology for perovskite solar cells, and more particularly to a method for controlling perovskite solar cells using polyvinylpyrrolidone. Background Technology
[0002] Inverted pin-structured perovskite solar cells offer advantages such as low-temperature solution processing, compatibility with tandem cells, and suitability for large-area fabrication. Using carbazole-based self-assembled monolayers as hole-selective contacts can replace traditional thick polymer hole transport layers, reducing parasitic absorption and series resistance. Furthermore, the formation of interfacial dipoles on transparent conductive oxide surfaces using phosphonic acid anchoring groups has garnered significant attention.
[0003] However, self-assembled monolayer molecules typically possess rigid conjugated carbazole structures and amphiphilic characteristics, making them prone to self-aggregation in precursor solutions. During the adsorption and drying process on the substrate, these aggregates can form localized island-like coverage, expose the conductive substrate, and create discontinuous buried contacts. This leads to leakage channels, interfacial recombination centers, and energy level mismatches, limiting the device's open-circuit voltage, fill factor, and operational stability.
[0004] Existing improvement strategies often employ small-molecule co-adsorbents, inorganic interfacial layers, or redesigned self-assembled monolayer molecules, but these frequently introduce new resistance barriers or disrupt the homogeneity of the molecular layer. Polymers, with their flexible backbones and abundant functional groups, hold promise for regulating the aggregation state of monolayer molecules in solution; however, the formation of continuous polymer layers can hinder hole transport.
[0005] Therefore, how to confine the polymer within the molecular layer while maintaining charge-selective contact and simultaneously improve the perovskite buried interface remains a pressing technical problem to be solved. Summary of the Invention
[0006] The purpose of this invention is to overcome the problems of the prior art and provide a method for controlling perovskite solar cells with polyvinylpyrrolidone, which solves the technical problems of easy aggregation of 4PADCB self-assembled monolayers, uneven coverage, and many defects at the perovskite buried interface above.
[0007] The above objectives are achieved through the following technical solutions: A method for controlling perovskite solar cells using polyvinylpyrrolidone includes the following steps: Step S1: Dissolve polyvinylpyrrolidone and 4PADCB, a self-assembled monolayer material containing carbazole and phosphonic acid anchoring groups, in an alcohol solvent to obtain a PVP / 4PADCB precursor solution. Step S2: The PVP / 4PADCB precursor solution obtained in step S1 is applied to the surface of a transparent conductive substrate, and after spin coating and annealing, a hole-selective layer of PVP-assisted assembly is formed on the transparent conductive substrate. Step S3: Prepare a perovskite absorber layer on the hole-selective layer obtained in step S2; Step S4: On the perovskite absorber layer obtained in step S3, a surface passivation layer, an electron transport layer, a buffer layer, and a metal electrode are formed sequentially to obtain a perovskite solar cell; The polyvinylpyrrolidone is dispersed in the 4PADCB self-assembled monolayer, and the lactam carbonyl group of the polyvinylpyrrolidone is located at the buried interface between the hole-selective layer and the perovskite absorber layer.
[0008] Furthermore, in the solution system of step S1 and the hole-selective layer formed in step S2, the lactam carbonyl group of the polyvinylpyrrolidone coordinates with the phosphonic acid group of the 4PADCB, promoting the formation of a polymer intercalation state, so that the polyvinylpyrrolidone chain segment is located between adjacent carbazole groups, and inhibiting the π-π aggregation between the 4PADCB molecules.
[0009] Further, in step S1, the concentrations of the 4PADCB and the polyvinylpyrrolidone in ethanol are both 1.0 mg / mL; the polyvinylpyrrolidone is K15 with a weight-average molecular weight of 8,000 to 12,000; and the transparent conductive substrate is indium tin oxide conductive glass.
[0010] Furthermore, in step S2, the spin coating speed is 3000 rpm, the spin coating time is 30 s, the annealing temperature is 100℃, and the annealing time is 10 min.
[0011] Furthermore, the perovskite precursor used in step S3 to prepare the perovskite absorber layer includes FAI, CsI, PbI2, and MACl, and the main component of the formed perovskite absorber layer is FAI. 0.95 Cs 0.05 PbI3; the perovskite precursor comprises an excess of 7 mol% PbI2 and 9 mol% MACl relative to the nominal perovskite concentration.
[0012] Furthermore, the solvent for the perovskite precursor is a mixed solvent of DMF and DMSO, with a volume ratio of DMF to DMSO of 4:1; the concentration of the perovskite precursor is 1.5M.
[0013] Further, step S3 involves a two-step spin-coating process to prepare the perovskite absorber layer, including: The first step involves a rotation speed of 1000 rpm, a time of 10 seconds, and an acceleration of 500 rpm·s.-1 ; The second step involves a rotation speed of 4000 rpm, a time of 50 seconds, and an acceleration of 1000 rpm·s. -1 ; Add 150 μL of chlorobenzene antisolvent 20 seconds before the end of the second spin coating step, and anneal at 100 °C for 30 min.
[0014] Further, in step S4, the surface passivation layer is formed of tetraethylammonium chloride (TEACl); the electron transport layer includes C 60 The buffer layer comprises copper bath chelate (BCP); the metal electrode comprises a silver electrode.
[0015] Furthermore, at the buried interface, the lactam carbonyl group of the polyvinylpyrrolidone can coordinate with Pb-related species in the perovskite absorber layer, which helps to reduce the defect state density at the buried interface.
[0016] Furthermore, after completing the fabrication according to steps S1 to S4, the resulting perovskite solar cell has the following device structure: glass / ITO / PVP+4PADCB / perovskite / TEACl / C. 60 / BCP / Ag.
[0017] This invention provides a method for regulating perovskite solar cells using polyvinylpyrrolidone (PVP). This method utilizes the coordination between the PPVP lactam carbonyl group and the phosphonic acid group of 4PADCB, along with the steric hindrance of the polymer backbone, to inhibit 4PADCB aggregation, promoting continuous and flat hole-selective layer formation. By controlling the amount of PPVP added, the formation of a continuous insulating polymer layer is avoided. Residual carbonyl groups at the buried interface can coordinate with Pb-related species, helping to improve precursor wetting and perovskite crystallization, reducing device leakage and non-radiative recombination at the interface, thereby improving open-circuit voltage, fill factor, and photoelectric conversion efficiency. Compared with existing technologies, this invention offers the following technical advantages: (1) PVP reduces the large-scale aggregation of 4PADCB in solution through carbonyl-phosphonic acid coordination and steric hindrance of polymer backbone, promotes uniform anchoring and continuous coverage of 4PADCB molecules on ITO surface, thereby suppressing local leakage channels.
[0018] (2) The carbonyl group of residual PVP can coordinate with Pb-related species, which helps to improve the wettability of precursors and the ability to passivate defects at the buried interface, promotes the uniform nucleation and ordered crystallization of perovskite at the bottom interface, and reduces non-radiative recombination.
[0019] (3) The contact layer of PVP-assisted assembly has low leakage current, maintainable electrochemical accessibility and energy level position closer to the perovskite valence band, which can improve the open circuit voltage and fill factor of the device without introducing a continuous insulating barrier layer.
[0020] (4) In this embodiment, the champion photoelectric conversion efficiency of the PVP auxiliary device is 25.95%, which is higher than the comparative example of 25.23%; the open circuit voltage and fill factor are improved simultaneously. Attached Figure Description
[0021] Figure 1 This is a schematic diagram of the molecular structures of PVP and 4PADCB in the method for regulating perovskite solar cells according to the present invention. Figure 2 Fourier transform infrared spectra of PVP, 4PADCB, and PVP / 4PADCB in the method for controlling perovskite solar cells according to the present invention. Figure 3 The dynamic light scattering particle size distribution of 4PADCB and PVP / 4PADCB precursor solutions in the method for controlling perovskite solar cells according to the present invention is shown in the figure. Figure 4 This is a comparison of the contact angles at the interface of the perovskite precursor with and without PVP in the method for controlling perovskite solar cells with polyvinylpyrrolidone (PVP) as described in this invention. Figure 5 This is a comparison chart of representative JV curves and photovoltaic parameters of devices without and with PVP in the method for controlling perovskite solar cells using polyvinylpyrrolidone (PVP) as described in this invention. Figure 6 The graphs show the SCLC curves of hole-single-carrier devices with and without PVP in the method for regulating perovskite solar cells according to the present invention. Figure 7 This is a flowchart of a method for controlling perovskite solar cells using polyvinylpyrrolidone according to the present invention. Detailed Implementation
[0022] The present invention will now be described in further detail with reference to the accompanying drawings and embodiments. The described embodiments are merely some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] like Figure 7As shown, this method provides a way to regulate perovskite solar cells using polyvinylpyrrolidone (PVP). After adding PPVP to the 4PADCB precursor solution, its lactam carbonyl groups can coordinate with the phosphonic acid groups of 4PADCB. The flexible PPVP backbone simultaneously provides steric hindrance, promoting the formation of smaller mixed assemblies and inhibiting the aggregation of large-sized 4PADCB. After spin-coating, the phosphonic acid groups of 4PADCB can more fully form PO-In anchoring bonds with the hydroxyl sites on the ITO surface, resulting in a more continuous, flat, and hole-selective contact layer.
[0024] The amount of polyvinylpyrrolidone added needs to be controlled to promote its dispersion in the 4PADCB assembly and avoid the formation of a continuous insulating polymer layer; if the concentration of polyvinylpyrrolidone is too high, it may form an insulating barrier and hinder hole transport, while if the concentration is too low, it may not be enough to inhibit the aggregation of 4PADCB molecules.
[0025] Unlike methods that only regulate self-assembled monolayers, the polyvinylpyrrolidone (PVP) in this invention does not completely detach from the interface during subsequent film formation. The residual PPVP dispersed in the hole-selective layer can coordinate with Pb-related species in the perovskite precursor via its carbonyl group, which helps improve the wetting of the precursor at the buried interface, regulates initial nucleation and crystallization, and reduces Pb-related defects. Simultaneously, controlling the amount of PPVP avoids the formation of a continuous insulating layer.
[0026] The technical solution of the present invention includes: firstly, cleaning and surface activation of a transparent conductive substrate; spin-coating a PVP / 4PADCB precursor solution onto the transparent conductive substrate and annealing to obtain a hole-selective layer; then preparing a perovskite absorber layer and a surface passivation layer; finally depositing an electron transport layer, a buffer layer and a metal electrode to obtain an inverted perovskite solar cell.
[0027] Specifically, the execution steps are as follows: Step S1: Dissolve polyvinylpyrrolidone and 4PADCB, a self-assembled monolayer material containing carbazole and phosphonic acid anchoring groups, in an alcohol solvent to obtain a PVP / 4PADCB precursor solution. Step S2: The PVP / 4PADCB precursor solution obtained in step S1 is applied to the surface of a transparent conductive substrate, and after spin coating and annealing, a hole-selective layer of PVP-assisted assembly is formed on the transparent conductive substrate. Step S3: Prepare a perovskite absorber layer on the hole-selective layer obtained in step S2; Step S4: On the perovskite absorber layer obtained in step S3, a surface passivation layer, an electron transport layer, a buffer layer, and a metal electrode are formed sequentially to obtain a perovskite solar cell; The polyvinylpyrrolidone is dispersed in the 4PADCB self-assembled monolayer, and the lactam carbonyl group of the polyvinylpyrrolidone is located at the buried interface between the hole-selective layer and the perovskite absorber layer. In this embodiment, ethanol was used as the solvent for the PVP / 4PADCB precursor solution, and the concentrations of both 4PADCB and polyvinylpyrrolidone were 1.0 mg / mL. The polyvinylpyrrolidone used was an Adamas product, CAS No. 9003-39-8, K15, with a weight-average molecular weight of 8,000 to 12,000, and was reagent grade. This formulation achieved polymer-assisted dispersion adjustment while maintaining 4PADCB as the hole-selective contact host.
[0028] In this embodiment, the perovskite absorber layer can be made of FA. 0.95 Cs 0.05 The PbI3 system. The perovskite precursor was prepared in a DMF / DMSO mixed solvent, and a dense absorber layer was formed after two-step spin coating, chlorobenzene antisolvent-assisted crystallization, and annealing.
[0029] As a specific embodiment of this solution, the transparent conductive substrate used in this embodiment is ITO conductive glass. The self-assembled monolayer material used is 4PADCB, the polymer control material is polyvinylpyrrolidone (PVP), the perovskite precursor raw materials used include FAI, CsI, PbI2, and MACl, and the electron transport material is C 60 The buffer material is BCP, the passivation material is TEACl, and the top electrode material is Ag.
[0030] The general fabrication method for perovskite solar cells provided in this embodiment is as follows: 1. Substrate cleaning and surface activation: The ITO conductive glass was ultrasonically cleaned once in a cleaning agent solution, twice in distilled water, once in isopropanol, and twice in ethanol, each time for 15 minutes; after drying, it was treated with ultraviolet ozone for 15 minutes to obtain a clean substrate with surface hydroxyl sites.
[0031] 2. Preparation of PVP-assisted self-assembled monolayer: 4PADCB was dissolved in ethanol to prepare a 1.0 mg / mL solution; 1.0 mg of polyvinylpyrrolidone was added to 1.0 mL of the 4PADCB solution to obtain a PVP / 4PADCB precursor solution with both components having a concentration of 1.0 mg / mL. The precursor solution was spin-coated onto an ITO substrate at 3000 rpm for 30 s, followed by annealing at 100 °C for 10 min to form a PVP-assisted assembled 4PADCB hole-selective layer.
[0032] 3. Preparation of the perovskite absorber layer: FAI, CsI, PbI2, and MACl are dissolved in a DMF / DMSO mixed solvent to obtain a perovskite precursor solution; this solution is spin-coated onto the hole-selective layer, and an antisolvent is added dropwise at the end of the spin-coating process, followed by annealing to form the perovskite absorber layer. This process allows the carbonyl groups of polyvinylpyrrolidone to coordinate with Pb-related species at the interface, which helps promote uniform crystallization at the bottom interface.
[0033] 4. Post-processing and top electrode fabrication: A TEACl solution was spin-coated onto the surface of the perovskite absorber layer to form a passivation layer; subsequently, C was deposited sequentially via thermal evaporation. 60 BCP and Ag were used to obtain glass / ITO / PVP+4PADCB / perovskite / TEACl / C. 60 Solar cells with a BCP / Ag structure.
[0034] Example 1: PVP-assisted 4PADCB hole-selective layer and perovskite solar cell The first step is to prepare the PVP / 4PADCB precursor solution. Dissolve 1.0 mg of 4PADCB in 1.0 mL of ethanol to obtain a 1.0 mg / mL 4PADCB solution. Add 1.0 mg of polyvinylpyrrolidone (Adamas, CAS 9003-39-8, K15, weight average molecular weight 8,000 to 12,000, reagent grade) to this solution and stir until clear and homogeneous to obtain a 1.0 mg / mL PVP / 4PADCB precursor solution.
[0035] The second step is to prepare the hole-selective layer. The PVP / 4PADCB precursor solution is spin-coated at 3000 rpm onto the surface of a cleaned and UV-ozone-treated ITO substrate for 30 s, and then annealed at 100 °C for 10 min to obtain the PVP-assisted assembled 4PADCB hole-selective layer.
[0036] The third step involved preparing the perovskite absorber layer. 245.1 mg FAI, 19.5 mg CsI, 739.9 mg PbI2, and 9.1 mg MACl were dissolved in 800 μL DMF and 200 μL DMSO to obtain a 1.5 M perovskite precursor solution, in which PbI2 was in 7 mol% excess relative to the nominal perovskite concentration, and the MACl content was 9 mol%. This solution was then spin-coated at 1000 rpm for 10 s with an acceleration of 500 rpm·s. -1 Then spin coat at 4000 rpm for 50 seconds with an acceleration of 1000 rpm·s. -1 150 μL of chlorobenzene was added 20 seconds before the end of the second spin coating step, followed by annealing at 100 °C for 30 min to form a perovskite absorber layer.
[0037] The fourth step involves preparing the passivation layer, electron transport layer, and electrode. A 4 mg / mL TEACl isopropanol solution was spin-coated at 3000 rpm for 30 seconds and annealed at 100 °C for 5 minutes; subsequently, it was thermally evaporated at 17 nm. 60 4nm BCP and 100nm Ag were used to obtain the complete device.
[0038] Comparative Example 1: 4PADCB hole-selective layer and perovskite solar cell without PVP The only difference from Example 1 is that: polyvinylpyrrolidone is not added to the hole-selective layer precursor solution, and 1 mg / mL 4 PADCB ethanol solution is directly spin-coated onto the surface of the ITO substrate; the preparation steps of the remaining perovskite absorber layer, passivation layer, electron transport layer and electrode are the same as in Example 1.
[0039] This comparative example is used to isolate device differences caused by PVP-assisted modulation under otherwise identical preparation conditions. The judgment that PVP did not form a continuous thick insulating layer is also combined with the near-insulating conductivity response after PVP film formation alone, the electrochemical accessibility maintained by PVP-assisted contacts, and the series of PVP dosage results.
[0040] Interface control mechanism and performance verification like Figure 1 As shown, the lactam carbonyl group of polyvinylpyrrolidone can coordinate with the phosphonic acid group of 4PADCB, and together with the steric hindrance provided by the polyvinylpyrrolidone backbone, it inhibits the self-aggregation of carbazole molecules.
[0041] like Figure 2 The image shows the Fourier transform infrared spectra of PVP, 4PADCB, and PVP / 4PADCB; the P=O vibrational peak of 4PADCB is observed at 1227.9 cm⁻¹. -1 Moved to 1213.4cm -1 The P-OH vibration peak is at 1001.8 cm⁻¹. -1 Moved to 994.7cm -1 The carbonyl peak of polyvinylpyrrolidone is at 1659.5 cm⁻¹. -1 Moved to 1678.7cm -1 The coordinated shift of the phosphonate-related vibrational peak to lower wavenumbers and the carbonyl peak to higher wavenumbers supports coordination between the lactam carbonyl group and the phosphonate group.
[0042] like Figure 3 The figure shows the dynamic light scattering particle size distribution of 4PADCB and PVP / 4PADCB precursor solutions. After the addition of polyvinylpyrrolidone, the large particle size distribution peak of the 4PADCB precursor solution was significantly weakened, indicating that polyvinylpyrrolidone can inhibit the aggregation of 4PADCB.
[0043] XPS and conductive atomic force microscopy tests showed that after polyvinylpyrrolidone-assisted assembly, polyvinylpyrrolidone-related C=O components could be observed in the contact layer, and high-current hot spots were significantly reduced; the surface Rq and Ra decreased from 2.162 nm and 1.661 nm to 1.419 nm and 1.136 nm, respectively, indicating the formation of a smoother and more continuous molecular layer contact.
[0044] like Figure 4 The figure shows a comparison of the contact angles at the interface between the perovskite precursor without PVP and with PVP. The contact angle of the polyvinylpyrrolidone-assisted interface with the perovskite precursor decreased from 45.4° to 11.7°, indicating improved wettability of the buried interface. The carbonyl group of polyvinylpyrrolidone undergoes a red shift after the introduction of PbI2, supporting Lewis acid-base coordination between the carbonyl oxygen and Pb-related species; this interaction helps reduce Pb-related defects at the bottom interface and promotes perovskite crystallization.
[0045] Polyvinylpyrrolidone-assisted perovskite films exhibit clearer buried interface diffraction characteristics and more uniform morphology; the root mean square roughness Rq of its upper surface is reduced from 40.94 nm to 32.96 nm, the fast decay components of transient absorption are 335 ps and 331 ps, respectively, and the slow decay component is extended from 3644 ps to 5235 ps, an increase of 43.7%, indicating that trap-assisted nonradiative recombination is suppressed.
[0046] like Figure 5 The figure shows a comparison of representative JV curves and photovoltaic parameters for devices without and with PVP. Under the same device structure, the top parameters for the control device are: Jsc = 25.61 mA / cm², Voc = 1.167 V, FF = 84.44%, and PCE = 25.23%; the top parameters for the PVP-assisted device are: Jsc = 25.67 mA / cm², Voc = 1.185 V, FF = 85.42%, and PCE = 25.95%.
[0047] like Figure 6 The figure shows the SCLC curves of hole single-carrier devices without PVP and with PVP. After adding polyvinylpyrrolidone, the trap filling limit voltage decreased from 0.594V to 0.390V, a reduction of 34.3%, further supporting the role of polyvinylpyrrolidone-assisted regulation in reducing trap-related defects and non-radiative recombination.
[0048] The above description is merely illustrative of the embodiments of the present invention and is not intended to limit the present invention. For those skilled in the art, any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for controlling perovskite solar cells using polyvinylpyrrolidone, characterized in that, Includes the following steps: Step S1: Dissolve polyvinylpyrrolidone and 4PADCB, a self-assembled monolayer material containing carbazole and phosphonic acid anchoring groups, in an alcohol solvent to obtain a PVP / 4PADCB precursor solution. Step S2: The PVP / 4PADCB precursor solution obtained in step S1 is applied to the surface of a transparent conductive substrate, and after spin coating and annealing, a hole-selective layer of PVP-assisted assembly is formed on the transparent conductive substrate. Step S3: Prepare a perovskite absorber layer on the hole-selective layer obtained in step S2; Step S4: On the perovskite absorber layer obtained in step S3, a surface passivation layer, an electron transport layer, a buffer layer, and a metal electrode are formed sequentially to obtain a perovskite solar cell; The polyvinylpyrrolidone is dispersed in the 4PADCB self-assembled monolayer, and the lactam carbonyl group of the polyvinylpyrrolidone is located at the buried interface between the hole-selective layer and the perovskite absorber layer.
2. The method for controlling perovskite solar cells using polyvinylpyrrolidone according to claim 1, characterized in that, In the solution system of step S1 and the hole-selective layer formed in step S2, the lactam carbonyl group of polyvinylpyrrolidone coordinates with the phosphonic acid group of 4PADCB, promoting the formation of polymer intercalation state, so that the polyvinylpyrrolidone chain segment is located between adjacent carbazole groups, and inhibiting the π-π aggregation between 4PADCB molecules.
3. The method for controlling perovskite solar cells using polyvinylpyrrolidone according to claim 1, characterized in that, In step S1, the concentrations of the 4PADCB and the polyvinylpyrrolidone in ethanol are both 1.0 mg / mL; the polyvinylpyrrolidone is K15 with a weight-average molecular weight of 8,000 to 12,000; and the transparent conductive substrate is indium tin oxide conductive glass.
4. The method for controlling perovskite solar cells using polyvinylpyrrolidone according to claim 1, characterized in that, In step S2, the spin coating speed is 3000 rpm and the spin coating time is 30 s; the annealing temperature is 100℃ and the annealing time is 10 min.
5. The method for controlling perovskite solar cells using polyvinylpyrrolidone according to claim 1, characterized in that, The perovskite precursor used in step S3 to prepare the perovskite absorber layer includes FAI, CsI, PbI2, and MACl, and the main component of the formed perovskite absorber layer is FAI. 0.95 Cs 0.05 PbI3; the perovskite precursor comprises an excess of 7 mol% PbI2 and 9 mol% MACl relative to the nominal perovskite concentration.
6. The method for controlling perovskite solar cells using polyvinylpyrrolidone according to claim 5, characterized in that, The solvent for the perovskite precursor is a mixture of DMF and DMSO, with a volume ratio of DMF to DMSO of 4:1; the concentration of the perovskite precursor is 1.5M.
7. The method for controlling perovskite solar cells using polyvinylpyrrolidone according to claim 1, characterized in that, Step S3 involves a two-step spin-coating process to prepare the perovskite absorber layer, including: The first step involves a rotation speed of 1000 rpm, a time of 10 seconds, and an acceleration of 500 rpm·s. -1 ; The second step involves a rotation speed of 4000 rpm, a time of 50 seconds, and an acceleration of 1000 rpm·s. -1 ; Add 150 μL of chlorobenzene antisolvent 20 seconds before the end of the second spin coating step, and anneal at 100 °C for 30 min.
8. The method for controlling perovskite solar cells using polyvinylpyrrolidone according to claim 1, characterized in that, In step S4, the surface passivation layer is formed of tetraethylammonium chloride (TEACl); the electron transport layer includes C 60 The buffer layer comprises copper bath chelate (BCP); the metal electrode comprises a silver electrode.
9. A method for controlling perovskite solar cells using polyvinylpyrrolidone according to claim 1, characterized in that, At the buried interface, the lactam carbonyl group of the polyvinylpyrrolidone can coordinate with Pb-related species in the perovskite absorber layer, which helps to reduce the defect state density of the buried interface.
10. A method for controlling perovskite solar cells using polyvinylpyrrolidone according to any one of claims 1-9, characterized in that, After completing the fabrication according to steps S1 to S4, the resulting perovskite solar cell has the following device structure: glass / ITO / PVP+4PADCB / perovskite / TEACl / C. 60 / BCP / Ag.