A self-healing perovskite solar cell and its preparation method and photovoltaic module
By introducing choline chloride-urea eutectic additives into the perovskite precursor solution and forming a eutectic interface layer using a flash evaporation process, the problem of defect repair in perovskite solar cell applications is solved, photoelectric performance and stability are improved, and it is suitable for industrial production.
Patent Information
- Application Number
- CN202611484197.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, perovskite solar cells cannot effectively repair defects during application, leading to a decrease in photoelectric conversion efficiency and stability.
By introducing choline chloride-urea eutectic additives into the perovskite precursor composite solution, a discontinuous eutectic interface layer is formed at the perovskite grain boundaries through a flash evaporation process, thereby achieving passivation and self-repair of the perovskite light-absorbing layer.
It effectively improves the photoelectric conversion efficiency and stability of perovskite solar cells, can be prepared in an air environment, and has industrialization prospects.
Smart Images

Figure CN123124649A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of photovoltaic cell technology, and more specifically, to a self-healing perovskite cell, its preparation method, and a photovoltaic module. Background Technology
[0002] With the rapid development of photovoltaic technology, perovskite solar cells have attracted widespread attention due to their excellent photoelectric conversion efficiency and low-cost manufacturing process.
[0003] However, due to the inherent properties of perovskite materials, defects within them can trap charge carriers, leading to nonradiative recombination and reduced battery efficiency. Furthermore, defects in perovskite materials, under the influence of an electric field, can cause charged ions to accumulate at the interface, resulting in a doping effect that induces band bending, current density-voltage hysteresis, phase separation, and degradation of the perovskite or metal electrodes. The migration of defects in perovskite materials primarily occurs through grain boundaries; therefore, passivation of these grain boundaries is necessary to impede their migration pathways.
[0004] CN117082879A discloses a bifacial passivated perovskite solar cell, its preparation method, and a photovoltaic module. By stacking a first passivation layer and a second passivation layer on the front and back sides of the perovskite layer respectively, an exogenous ion-compensated passivation structure is formed. This enables exogenous ions to passivate vacancy defects inside the perovskite layer caused by ion migration, effectively repairing surface defects of the perovskite layer and solving the problem of energy level mismatch caused by direct contact between the charge transport materials of the first and second charge extraction layers and the perovskite layer.
[0005] CN118804611A discloses a passivation unit, fabrication method, and battery for a perovskite solar cell. By forming a directionally arranged dipole molecular layer between the perovskite layer and the passivation layer, an additional dipole electric field is introduced between the perovskite and the passivation layer using the inserted dipole layer, which promotes the transport of charge carriers from the perovskite to the passivation layer, thereby improving the conversion efficiency of the device based on the passivation defects of the passivation layer.
[0006] CN119546140A discloses a method for fabricating a perovskite solar cell and its structure. By introducing an interface passivation layer comprising a piperazine carboxylic acid compound, defects on the surface and at the grain boundaries of the first perovskite light-absorbing layer are effectively passivated, and the interface defect state density between the first perovskite light-absorbing layer and the first electron transport layer is reduced, thereby effectively suppressing the occurrence of nonradiative recombination. Furthermore, this interface passivation layer optimizes the band structure of the first perovskite light-absorbing layer, significantly improving carrier extraction efficiency, and thus greatly enhancing the overall performance of the perovskite solar cell.
[0007] The existing technical solutions can only passivate defects in perovskite materials at the initial stage, but cannot repair defects in perovskite solar cells during application.
[0008] Therefore, it is of great significance to provide a technical solution that can self-repair defects generated in the perovskite light-absorbing layer in applications. Summary of the Invention
[0009] This application provides a self-healing perovskite solar cell, its preparation method, and a photovoltaic module. During the preparation of the perovskite light-absorbing layer, a eutectic additive is introduced into the perovskite precursor composite solution. A discontinuous eutectic interface layer is formed at the perovskite grain boundaries and on the surface of the perovskite light-absorbing layer through flash evaporation. This effectively passivates grain boundary defects in the perovskite material. Furthermore, during cell operation, the eutectic interface layer transforms into a low-viscosity liquid state as the temperature rises, self-repairing defects and microcracks generated during the application of the perovskite light-absorbing layer, effectively improving the photoelectric conversion efficiency and stability of the perovskite solar cell.
[0010] In a first aspect, a method for preparing a self-healing perovskite solar cell is provided, the method comprising: A first carrier transport layer, a perovskite light-absorbing layer, a passivation layer, a second carrier transport layer, a transparent conductive layer, and a metal electrode are sequentially fabricated on the substrate surface; the method for fabricating the perovskite absorber layer includes: A perovskite precursor composite solution is spin-coated onto the surface of the first carrier transport layer, followed by flash evaporation and annealing to obtain the perovskite absorber layer. The perovskite precursor composite solution includes a perovskite precursor and a eutectic additive. The eutectic additive includes choline chloride and urea.
[0011] This invention introduces a choline chloride-urea eutectic additive into a perovskite precursor composite solution, combined with a spin-coating flash evaporation process. During flash evaporation, the solvent evaporates rapidly, and the perovskite precursor becomes supersaturated and quickly forms crystal nuclei for crystallization. The choline chloride-urea eutectic additive does not have time to diffuse into the perovskite lattice, but is pushed to the interface by the rapidly growing grains, accumulating at the grain boundaries of the perovskite material and forming a discontinuous ultrathin eutectic interface layer on the surface of the perovskite light-absorbing layer.
[0012] The eutectic interface layer can not only effectively passivate defects in the perovskite light-absorbing layer, but also act as a "grain boundary adhesive" to self-repair perovskite materials, significantly improving the photoelectric performance and stability of perovskite solar cells.
[0013] Furthermore, in this invention, the choline chloride-urea eutectic additive has moderate hygroscopicity, and the quaternary ammonium salt structure in choline chloride has antioxidant properties. Urea, as a reducing agent, can remove dissolved oxygen and oxidative free radicals in the perovskite precursor composite solution. Therefore, in the preparation method provided by this invention, the preparation of the perovskite absorber layer can be carried out in an air environment, rather than necessarily under inert gas protection, which has industrialization prospects.
[0014] In some embodiments, the method for preparing the perovskite precursor composite solution includes: Choline chloride and urea are mixed in a solvent and heated and stirred to obtain a eutectic solution; the eutectic solution is added to a perovskite precursor solution to obtain the perovskite precursor composite solution.
[0015] In some embodiments, the molar ratio of choline chloride to urea in the eutectic solution is 1:(2~3).
[0016] In some embodiments, the total concentration of choline chloride and urea in the eutectic solution is 25 g / L to 35 g / L.
[0017] In some embodiments, the concentration of the perovskite precursor in the perovskite precursor solution is 1.6 mol / L to 2.0 mol / L.
[0018] In some embodiments, the volume ratio of the eutectic solution to the perovskite precursor solution is (0.005~0.02):1, and the volume of both the eutectic solution and the perovskite precursor solution is in liters (L).
[0019] In some embodiments, the temperature of the heating and stirring is 60°C to 80°C.
[0020] In some embodiments, the solvent includes N,N-dimethylformamide.
[0021] In some embodiments, the rotation speed of the spin-coated perovskite precursor composite solution is 1500 rpm to 2500 rpm.
[0022] In some embodiments, the spin-coating time of the perovskite precursor composite solution is 5s to 9s.
[0023] In some embodiments, the flash evaporation includes evacuating the cavity to a pressure of 3 Pa to 10 Pa for 8 to 12 seconds.
[0024] In some embodiments, the annealing temperature is 90°C to 110°C.
[0025] In some embodiments, the annealing time is 10 min to 30 min.
[0026] In some embodiments, the self-healing perovskite solar cell is prepared in an air environment.
[0027] In some embodiments, the substrate includes any one of an FTO conductive glass substrate, an ITO conductive glass substrate, or a crystalline silicon substrate.
[0028] Secondly, the present invention provides a self-healing perovskite solar cell, the self-healing perovskite solar cell comprising a first carrier transport layer, a perovskite light-absorbing layer, a passivation layer, a second carrier transport layer, a transparent conductive layer, and a metal electrode, which are sequentially stacked on the surface of a substrate; the surface of the perovskite absorption layer adjacent to the passivation layer further includes an in-situ formed self-healing layer, the self-healing layer being discontinuously formed in-situ at the grain boundary edge of the surface perovskite grains.
[0029] In the perovskite solar cell provided by this invention, the choline chloride-urea eutectic additive is pushed to the interface between the perovskite light-absorbing layer and the passivation layer by the rapidly growing perovskite grains during the flash evaporation stage, forming a eutectic interface layer at the edge of the surface perovskite grains. This eutectic interface layer acts as a self-healing layer, effectively passivating defects in the perovskite material. At temperatures of 40°C to 60°C, it transforms into a low-viscosity liquid state, repairing micro-cracks caused by thermal expansion and contraction, thus achieving self-repair of micro-cracks and effectively improving the photoelectric performance and stability of the perovskite solar cell.
[0030] In some embodiments, the melting point of the self-healing layer is 40°C to 60°C.
[0031] Thirdly, the present invention provides a photovoltaic module comprising a self-healing perovskite cell as described in the second aspect. Attached Figure Description
[0032] Figure 1 This is a schematic diagram of the photovoltaic system provided in this application.
[0033] Figure 2 This is a schematic diagram of the photovoltaic module provided in this application.
[0034] Figure 3 This is an exploded view of the photovoltaic module provided in this application.
[0035] The accompanying drawings are not drawn to scale.
[0036] Figure label: 1000 - Photovoltaic system; 100 - Photovoltaic module; 110 - Frame; 120 - Front cover plate; 130 - First encapsulating film; 140 - Cell string layer; 150 - Second encapsulating film; 160 - Back cover plate; 170 - Junction box. Detailed Implementation
[0037] The descriptions of specific structures or functions implemented according to the concept of this application disclosed in this specification are merely illustrative examples for explaining embodiments based on the concept of this application. Those skilled in the art will understand that embodiments based on the concept of this application can have various variations and forms, and are not limited to the embodiments described in this specification, but also include various modifications, equivalents, or substitutions made within the scope of the purpose, concept, and technology of this application.
[0038] In the description of this application, it should be understood that the use of terms such as "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", and "circumferential" indicates the relative orientation or positional relationship between different components, and is only for the convenience of describing this application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.
[0039] Although the terms "first" or "second" may be used to describe various components or components, the components or components should not be limited by the terms. The terms above are used only for the purpose of distinguishing one component or component from another. For example, without departing from the scope of the claims according to the concept of this application, a first battery cell may be referred to as a second battery cell, and similarly, a second battery cell may be referred to as a first battery cell.
[0040] In this application, unless otherwise expressly specified and limited, the terms "connected," "fixed," "set," etc., should be interpreted broadly. For example, when one component is said to "connect" another component, it should be understood that it can be directly or indirectly connected to the other component, meaning that other components may also be present in between. Similarly, the terms "fixed" and "set" should be interpreted broadly in a similar way. Furthermore, the term "connected" can refer to a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can refer to the internal communication of two components or the interaction between two components, unless otherwise expressly limited. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances. In this application, unless otherwise expressly specified and limited, the description of "above" or "below" the second feature can mean that the first and second features are in direct contact, or that the first and second features are in indirect contact through an intermediate medium. Moreover, "above," "on top of," and "over" the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. The first feature being "below", "under", or "below" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.
[0041] To make the above-mentioned objectives, features and advantages of this application more apparent and understandable, the specific embodiments of this application will be described in detail below with reference to the accompanying drawings.
[0042] The self-healing perovskite solar cell (hereinafter referred to as the cell) provided in this application embodiment undergoes performance testing through the following process: I. Preparatory work before testing 1. Battery cell cleaning, including: Wipe the surface of the battery cells with ultrapure water, ethanol or isopropanol to remove fingerprints, dust and organic residues; After drying the solar cells with nitrogen, let them stand for 10 minutes to avoid surface contamination affecting their optical properties.
[0043] 2. Electrode contact inspection, including Electrical measurements of the solar cells were performed using a four-wire probe (Keithley 2400 series) to ensure that the contact resistance between the metal electrodes of the solar cells and the probe was <0.1Ω; Use silver paste or spring probes to secure the battery cells and avoid pressure damage.
[0044] 3. Stabilization treatment, including: Place the solar cells under standard lighting (1000W / m²). 2After aging for 1 hour, light-induced degradation (LID) is eliminated; The temperature of the solar cells was maintained at 25℃±0.5℃ using a constant temperature stage to avoid the impact of thermal effects on carrier mobility.
[0045] 4. Equipment calibration, including: The light source spectrum was calibrated using a standard reference cell to conform to the AM1.5G standard spectral conditions, with a calibration wavelength range of 300 nm to 1200 nm. The irradiance uniformity deviation in the test area does not exceed ±2%, and the measurement error of the temperature sensor used is less than ±0.1℃.
[0046] II. Testing Equipment and Conditions 1. Core equipment IV tester: Keysight B2900A series, with a voltage resolution of 0.1mV and a current resolution of 0.1μA; Solar simulator: Class AAA compliant, with selectable pulsed or steady-state light source (e.g., Wacom WXS-200S-20). Temperature control console: Temperature regulation is achieved based on a thermoelectric cooling (TEC) module, with a control accuracy of ±0.2℃; Spectral response instrument: equipped with a quantum efficiency (QE) testing system (such as Bentham PVE300).
[0047] 2. Standard Test Conditions (STC) Irradiance: 1000W / m 2 (AM1.5G standard spectrum); Temperature: 25℃±1℃ (real-time monitoring via TEC module); Light spot uniformity: The uniformity of the light spot covering the effective area of the battery is >95%.
[0048] III. Key Parameter Testing Procedures 1. Conversion efficiency (Eta), IV characteristics (Voc, Isc and FF), and stability testing Test equipment: solar simulator, IV tester and four-wire probe.
[0049] step: (1) Sample placement: Place the battery cell in the center of the light spot of the simulator, and use a light shield to block the edge of the battery cell by 5mm to avoid light leakage at the edge; (2) IV scan: Apply a scan voltage from -0.5V to Voc+0.5V through an IV tester, set the scan step size to 10mV, and record the IV characteristic curve of the battery simultaneously; (3) Parameter extraction: Extract the open-circuit voltage Voc (voltage when current = 0) and short-circuit current Isc (current when voltage = 0) from the IV curve; (4) Calculation of power and fill factor: Calculate the maximum power point (Pmax=Vmpp×Impp) and fill factor FF=Pmax / (Voc×Isc) on the IV curve; (5) Efficiency calculation: The conversion efficiency Eta = (Pmax / Pin) × 100% is calculated, where the incident light power Pin is calibrated by a calibrated standard cell; (6) Stability test: The solar cell is continuously run under standard test conditions to test the conversion efficiency Eta-100, Eta-500 and Eta-1000 for 100h, 500h and 1000h. The percentage of Eta-100, Eta-500 and Eta-1000 to Eta obtained in step (5) is calculated, and the photoelectric conversion efficiency retention rate for 100h, 500h and 1000h is obtained.
[0050] The researchers of this application have found that the existing technical solutions for passivating defects in perovskite materials can only passivate defects in perovskite materials during the preparation process, but cannot repair defects in perovskite solar cells during application.
[0051] Based on this, this application provides a self-healing perovskite battery and its preparation method, photovoltaic module and photovoltaic system. The self-healing perovskite battery introduces a eutectic additive into the perovskite precursor solution during the preparation of the perovskite light-absorbing layer. This not only passivates the defects of the perovskite material during the preparation process, but also enables the self-repair of defects and microcracks generated in the perovskite light-absorbing layer during application.
[0052] This application provides a method for preparing a self-healing perovskite solar cell, the method comprising: A first carrier transport layer, a perovskite light-absorbing layer, a passivation layer, a second carrier transport layer, a transparent conductive layer, and a metal electrode are sequentially fabricated on the substrate surface; the method for fabricating the perovskite absorber layer includes: A perovskite precursor composite solution is spin-coated onto the surface of the first carrier transport layer, followed by flash evaporation and annealing to obtain the perovskite absorber layer. The perovskite precursor composite solution includes a perovskite precursor and a eutectic additive. The eutectic additive includes choline chloride and urea.
[0053] In this invention, the perovskite precursor in the perovskite precursor solution comprises ABX3 material, wherein A includes FA. + MA + or Cs +B comprises any one or at least two of the following, wherein B includes a metal ion, and the metal ion includes Pb. 2+ Sn 2 + Or Ge 2+ Any one or at least two of the following; X includes a halide ion, said halide ion including I - ,Br - or Cl - Any one or at least two of them.
[0054] This invention introduces a choline chloride-urea eutectic additive into a perovskite precursor composite solution, combined with a spin-coating flash evaporation process. During flash evaporation, the solvent evaporates rapidly, and the perovskite precursor becomes supersaturated and quickly forms crystal nuclei for crystallization. The choline chloride-urea eutectic additive does not have time to diffuse into the perovskite lattice, but is pushed to the interface by the rapidly growing grains, accumulating at the grain boundaries of the perovskite material and forming a discontinuous ultrathin eutectic interface layer on the surface of the perovskite light-absorbing layer.
[0055] In the eutectic interface layer, the choline ions of choline chloride include -OH groups. These -OH groups can form strong coordination bonds with uncoordinated metal ions in the perovskite material, effectively locking the metal ions and eliminating deep-level defects. Similarly, the -C=O and -NH2 groups in urea can coordinate with metal ions and form hydrogen bonds with halide ions, stabilizing the crystal structure of the perovskite material. With the help of the eutectic additives, defects in the perovskite light-absorbing layer are effectively passivated, significantly improving the photoelectric performance and stability of perovskite solar cells.
[0056] The eutectic interface layer not only serves as a passivation agent but also acts as a "grain boundary adhesive" for self-repair of perovskite materials. Since perovskite solar cells heat up to above 40°C during operation, typically between 40°C and 60°C, the choline chloride-urea eutectic additive transforms into a low-viscosity liquid within this temperature range. This liquid can repair microscopic cracks caused by thermal expansion and contraction during application, further enhancing the stability of the perovskite solar cell.
[0057] Furthermore, in this invention, the choline chloride-urea eutectic additive has moderate hygroscopicity, enabling it to act as a 'humidity buffer' in the perovskite precursor composite solution. It preferentially forms a hydrogen bond network with intruding trace water molecules, thereby competitively inhibiting the direct reaction between water molecules and perovskite components. Moreover, the quaternary ammonium salt structure in choline chloride has antioxidant properties, which can inhibit the oxidation reaction of halide ions. Urea, as a reducing agent, can remove dissolved oxygen and oxidative free radicals in the perovskite precursor composite solution. The synergistic effect of the choline chloride-urea eutectic additive achieves in-situ antioxidant protection, ensuring the stoichiometry and phase purity of the perovskite film.
[0058] Therefore, the perovskite absorber layer prepared by the present invention can be prepared in an air environment, rather than necessarily under the protection of an inert gas, and has industrialization prospects.
[0059] In this invention, the first carrier transport layer and the second carrier transport layer are respectively one of the hole transport layer and the electron transport layer, and the first carrier transport layer and the second carrier transport layer are different.
[0060] In this embodiment, the hole transport layer is made of organic hole transport materials and / or inorganic hole transport materials. The organic hole transport materials include poly[4-(9H-carbazole-9-yl)butylphosphonic acid](Poly-4PACz), [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), and [4-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-4). The inorganic hole transport material comprises any one of PACz), 2,2',7,7'-tetratetra(N,N-p-methoxyaniline)-9,9'-spirodifluorene (Spiro-OMeTAD), poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid) (PEDOT:PSS) or poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), wherein the inorganic hole transport material comprises any one of NiO, Cu2O or MoO3.
[0061] In this embodiment, the method for preparing the hole transport layer is not particularly limited. For example, it is prepared by spin coating followed by annealing.
[0062] In this embodiment, the electron transport layer is made of organic electron transport materials and / or inorganic electron transport materials. The inorganic electron transport materials include any one of TiO2, ZnO, or SnO2, and the organic electron transport materials include any one of [6,6]-phenyl-C61-butyrate methyl ester (PCBM), 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP), C60, or graphene.
[0063] In this application embodiment, the preparation method of the electron transport layer is not particularly limited. Exemplarily, it is prepared by thermal evaporation coating, magnetron sputtering or atomic layer deposition.
[0064] In this embodiment, the material of the perovskite light-absorbing layer includes any one of MAPbI3, MAPbBr3, FAPbI3, CsPbI3, or CsPbBr3.
[0065] In this embodiment of the application, the material of the transparent conductive layer includes any one of indium tin oxide (ITO), indium zinc oxide (IZO), aluminum-doped zinc oxide (AZO), or indium cadmium oxide (ICO).
[0066] In the embodiments of this application, the method for preparing the transparent conductive layer is not particularly limited, but includes, for example, magnetron sputtering or atomic layer deposition.
[0067] In this embodiment, the gate electrode includes a metal electrode, exemplarily including a gold electrode, a silver electrode, or a copper electrode.
[0068] In the embodiments of this application, the method for preparing the gate electrode is not particularly limited. Exemplarily, a thermal evaporation coating method or a slurry coating method is used.
[0069] In some specific embodiments, the preparation method of the perovskite precursor composite solution includes: Choline chloride and urea are mixed in a solvent and heated and stirred to obtain a eutectic solution; the eutectic solution is added to a perovskite precursor solution to obtain the perovskite precursor composite solution.
[0070] In this invention, choline chloride and urea are dissolved in a solvent to prepare a homogeneous eutectic solution in advance, which is then added to the perovskite precursor solution to better exert the eutectic effect and achieve passivation and self-repair.
[0071] In this invention, the molar ratio of choline chloride to urea affects the passivation effect on perovskite materials. A suitable molar ratio is beneficial for the effective passivation of perovskite materials and the elimination of deep-level defects. The -OH group of choline chloride is key to forming strong coordination bonds with uncoordinated metal ions. If too much urea is added and too little choline chloride is added, there will be insufficient coordination sites, which is equivalent to reducing the "holding points for metal ions". The passivation effect on deep-level defects will be weakened. Furthermore, after deviating from the optimal eutectic ratio, the hydrogen bond network becomes loose and disordered, which will greatly reduce the stability of the eutectic solvent and worsen the repair effect on defects and microcracks generated during the subsequent application of perovskite solar cells.
[0072] In some specific embodiments, the molar ratio of choline chloride to urea in the eutectic solution is 1:(2~3), for example, it can be 1:2, 1:2.2, 1:2.4, 1:2.6, 1:2.8 or 1:3.
[0073] In some specific embodiments, the total concentration of choline chloride and urea in the eutectic solution is 25 g / L to 35 g / L, for example, it can be 25 g / L, 27 g / L, 29 g / L, 31 g / L, 33 g / L or 35 g / L.
[0074] In some specific embodiments, the concentration of the perovskite precursor in the perovskite precursor solution is 1.6 mol / L to 2.0 mol / L, for example, it can be 1.6 mol / L, 1.65 mol / L, 1.7 mol / L, 1.75 mol / L, 1.8 mol / L, 1.85 mol / L, 1.9 mol / L, 1.95 mol / L or 2.0 mol / L.
[0075] In some specific embodiments, the volume ratio of the eutectic solution to the perovskite precursor solution is (0.005~0.02):1, for example, it can be 0.005:1, 0.008:1, 0.01:1, 0.012:1, 0.015:1, 0.018:1 or 0.02:1. The unit of volume for both the eutectic solution and the perovskite precursor solution is L.
[0076] In some specific embodiments, the heating and stirring temperature is 60°C to 80°C, for example, it can be 60°C, 65°C, 70°C, 75°C or 80°C.
[0077] In some specific embodiments, the solvent includes N,N-dimethylformamide.
[0078] In some specific embodiments, the rotation speed of the spin-coated perovskite precursor composite solution is 1500 rpm to 2500 rpm, for example, it can be 1500 rpm, 1700 rpm, 1900 rpm, 2100 rpm, 2300 rpm or 2500 rpm.
[0079] In some specific embodiments, the spin-coating time of the perovskite precursor composite solution is 5s to 9s, for example, 5s, 6s, 7s, 8s or 9s.
[0080] In this invention, by controlling the pumping speed and time of flash evaporation, the perovskite crystals are rapidly nucleated and grown, and the choline chloride-urea eutectic additive is "squeezed" to the grain boundaries of the perovskite crystals and the surface of the perovskite light-absorbing layer, forming a discontinuous ultrathin eutectic interface layer, which repairs the microcracks generated during the use of the perovskite battery.
[0081] In some specific embodiments, the flash evaporation includes evacuating the cavity to a pressure of 3 Pa to 10 Pa in 8 to 12 seconds. The evacuation time can be, for example, 8 s, 9 s, 10 s, 11 s or 12 s, and the pressure in the cavity after evacuation can be, for example, 3 Pa, 4 Pa, 5 Pa, 6 Pa, 7 Pa, 8 Pa, 9 Pa or 10 Pa.
[0082] In some specific embodiments, the annealing temperature is 90℃~110℃, for example, it can be 90℃, 95℃, 100℃, 105℃ or 110℃.
[0083] In some specific embodiments, the annealing time is 10 min to 30 min, for example, it can be 10 min, 15 min, 20 min, 25 min or 30 min.
[0084] In some specific embodiments, the self-healing perovskite solar cell is prepared in an air environment.
[0085] In some specific embodiments, the substrate includes any one of FTO conductive glass substrate, ITO conductive glass substrate, or crystalline silicon substrate cell.
[0086] In this invention, when the substrate is a crystalline silicon base cell, an intermediate composite layer is prepared on the surface of the crystalline silicon base cell, and a first carrier transport layer is prepared on the surface of the intermediate composite layer to obtain a perovskite-crystalline silicon tandem cell, which realizes the absorption of sunlight in different wavelength bands and is beneficial to improving the photoelectric conversion efficiency.
[0087] The material of the intermediate composite layer is not particularly limited. For example, the material of the intermediate composite layer can be any one of SnO2, ITO, AZO or FTO.
[0088] The type of crystalline silicon bottom cell is not particularly limited. For example, a crystalline silicon bottom cell can be any one of TOPCon (Tunnel Oxide Passivated Contact) cell, HJT (Hetero junction with Intrinsic Thin-film) cell, or BC (Back Contact) cell.
[0089] According to some embodiments of this application, this application provides a self-healing perovskite solar cell, which includes a first carrier transport layer, a perovskite light-absorbing layer, a passivation layer, a second carrier transport layer, a transparent conductive layer, and a metal electrode, which are sequentially stacked on the surface of a substrate; the surface of the perovskite absorption layer adjacent to the passivation layer also includes an in-situ formed self-healing layer, which is discontinuously formed in-situ at the grain boundary edge of the surface perovskite grains.
[0090] In the perovskite solar cell provided by this invention, the choline chloride-urea eutectic additive is pushed to the interface between the perovskite light-absorbing layer and the passivation layer by the rapidly growing perovskite grains during the flash evaporation stage, forming a eutectic interface layer at the edge of the surface perovskite grains. This eutectic interface layer acts as a self-healing layer, effectively passivating defects in the perovskite material. At temperatures of 40°C to 60°C, it transforms into a low-viscosity liquid state, repairing micro-cracks caused by thermal expansion and contraction, thus achieving self-repair of micro-cracks and effectively improving the photoelectric performance and stability of the perovskite solar cell.
[0091] In some specific embodiments, the melting point of the self-healing layer is 40°C to 60°C, for example, it can be 40°C, 45°C, 50°C, 55°C or 60°C.
[0092] According to some embodiments of this application, this application provides a photovoltaic module, which includes the self-healing perovskite cell as provided in the foregoing embodiments of this application.
[0093] A photovoltaic (PV) module is a device that directly converts light energy into electrical energy through the photoelectric effect or photochemical effect. A PV module typically has a stacked encapsulation structure, comprising at least the following from the light-facing side to the back-light-facing side: a front cover, a first encapsulating film, a cell string layer, a second encapsulating film, and a back cover, as well as a frame surrounding the stacked structure and a junction box located on one side of the back cover.
[0094] The front cover can be made of a material with excellent light transmittance, impact resistance, corrosion resistance, and weather resistance, and may optionally include at least one of the following materials: tempered glass, plexiglass, transparent ceramics, organic fibers, or polymers. In some embodiments, the front cover may include at least one of an insulating barrier layer, a fluorinated weather-resistant layer, and a transition adhesive layer.
[0095] Back cover plates typically need to possess insulation, water resistance, aging resistance, weather resistance, and corrosion resistance. They may optionally include at least one composite back cover with tempered glass, acrylic glass, a metal back cover, or a PET film as the substrate. The PET-based composite back cover may, depending on the needs of different scenarios, include composite back covers, coated composite back covers, and co-extruded composite back covers. For example, composite back covers include polyvinyl fluoride / polyethylene terephthalate / polyvinyl fluoride (TPT) composite back covers, polyvinylidene fluoride / polyethylene terephthalate / polyvinylidene fluoride (KPK) composite back covers, and polyvinyl fluoride / polyethylene terephthalate / ethylene-vinyl acetate copolymer (TPE) composite back covers. Composite backsheets or polyvinylidene fluoride / polyethylene terephthalate / ethylene-vinyl acetate copolymer (KPE) composite backsheets, coated backsheets such as polyvinylidene fluoride / polyethylene terephthalate / coating (TPC) composite backsheets, polyvinylidene fluoride / polyethylene terephthalate (KPC) composite backsheets, or coating / polyethylene terephthalate / coating (CPC) composite backsheets, co-extruded composite backsheets, exemplary, for example, can be multilayer co-extruded polyolefin (PO) composite backsheets.
[0096] It is understandable that the material selection for the front cover and the back cover does not affect each other, and the same or different materials can be selected depending on the different application scenarios of the components (such as residential photovoltaics and building-integrated photovoltaics).
[0097] The first encapsulating film and the second encapsulating film may be selected from at least one of ethylene-vinyl acetate copolymer (EVA) film, polyvinyl octene coelastomer (POE) film, EVA-POE-EVA co-extruded film (EPE), PVB (polyvinyl butyral), polyethylene terephthalate (PET) film, or liquid silicone.
[0098] In some embodiments, the first and second encapsulating films may further include one or more functional additives selected from the group consisting of crosslinking agents, coupling agents, antioxidants, and ultraviolet absorbers, to improve the degree of crosslinking, weather resistance, adhesive strength, and anti-aging properties of the films. It is understood that the first and second encapsulating films may be made of the same or different materials.
[0099] The battery string layer comprises multiple battery strings, which can be combined in series, parallel, or series-parallel configurations to achieve current convergence and output. Furthermore, each battery string is formed by sequentially connecting multiple battery cells via connectors.
[0100] In some embodiments, at least a portion of the connector is electrically connected to the back electrode of a battery cell, and at least another portion of the connector is electrically connected to the front or back electrode of another battery cell to form a battery string. The connector may optionally include conductive elements such as solder strips, busbars, or metal clips.
[0101] The solar cell may include a semiconductor substrate, a first emitter of a first conductivity type, and a second emitter of a second conductivity type. It is understood that one of the first and second conductivity types is P-type, and the other is N-type. The semiconductor substrate may include an N-type silicon substrate or a P-type silicon substrate. N-type silicon substrates are typically formed by doping with Group V elements such as phosphorus, arsenic, or antimony, and have the characteristic that the majority charge carriers are electrons; P-type silicon substrates are typically formed by doping with Group III elements such as boron, gallium, or aluminum, and have the characteristic that the majority charge carriers are holes.
[0102] The solar cell can employ a grid line design with no main grid (OBB), multiple main grid (MBB), or super-multiple main grid (SMBB). In some embodiments, the grid line material can be selected as at least one of silver-based conductive paste or silver-coated copper composite paste. The paste uses highly conductive metal powder as the conductive substrate, and the substrate can be at least one of silver powder, copper powder, or silver-coated copper composite powder. To improve the ohmic contact performance, conductivity, and long-term weather resistance of the electrodes, a composite functional layer can be formed on the surface of the substrate or in the grid line structure. The functional layer material includes at least one of glass powder, organic carrier, nickel-based barrier layer, tin-based alloy layer, or anti-oxidation and corrosion-resistant coating.
[0103] It is understood that the solar cells can be at least one of perovskite solar cells or perovskite / crystalline silicon tandem solar cells.
[0104] In some embodiments, to improve welding performance, oxidation resistance and weather resistance, the material of the connector may preferably be a highly conductive metal material, such as at least one of silver, copper, tin, nickel or an alloy thereof.
[0105] In some embodiments, to balance conductivity and cost control requirements, the connector can be made of at least one of the following metal-clad composite materials: silver-plated copper, copper-plated silver, copper-plated aluminum, aluminum-plated copper, tin-plated copper, and nickel-plated copper. The electrical connection can be achieved through one of the following methods: laser welding, spot welding, bonding, ultrasonic welding, resistance welding, or brazing.
[0106] The frame surrounds the periphery of the stacked structure and is mostly made of aluminum alloy or steel alloy. In some embodiments, the frame may also be a fiberglass frame or a plastic frame. The inner side of the frame usually has grooves for filling with sealant to achieve a sealed bond with the stacked components formed by the front cover, the first encapsulation film, the battery string layer, the second encapsulation film, and the back cover, thereby blocking moisture and buffering external impacts.
[0107] In some implementations, the border can be assembled by connecting corner brackets.
[0108] The junction box is located on one side of the rear cover and is electrically connected to the terminals of the bus electrodes in the battery string layer via a lead-out busbar for energy extraction. The junction box typically includes a housing and cover made of weather-resistant insulating material, conductive connecting tabs inside the housing, and one or more bypass diodes. The bypass diodes are connected in parallel with sub-units of the battery string. The electrical leads of the junction box include photovoltaic-specific connectors and cables. The cables preferably use cross-linked polyethylene insulation and tinned copper core wires.
[0109] In some embodiments, the electrical components can be filled and encapsulated with potting compound to achieve insulation, heat conduction, moisture protection and fixation.
[0110] According to some embodiments of this application, this application provides a photovoltaic system, which includes photovoltaic modules as provided in the foregoing embodiments of this application.
[0111] Photovoltaic systems can be used in photovoltaic power plants, such as ground-mounted power plants, rooftop power plants, and water-based power plants. They can also be used in equipment or devices that generate electricity using solar energy, such as user solar power supplies, solar streetlights, solar cars, and solar buildings.
[0112] It is understandable that the application scenarios of photovoltaic (PV) systems are not limited to this; that is to say, PV systems can be applied in all fields that require solar energy for power generation. Taking a PV power generation system as an example, a PV system can include a PV array, a combiner box, and an inverter. The PV array can be an array combination of multiple PV modules; for example, multiple PV modules can form multiple PV arrays. The PV array is connected to the combiner box, which can collect the current generated by the PV array. The collected current flows through the inverter and is converted into AC power required by the mains power grid before being connected to the mains power grid to realize solar power supply.
[0113] The numerical range described in this application includes not only the listed point values, but also any point values between numerical ranges not listed. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values included in the range.
[0114] To make the technical solutions of the embodiments of this application clear, as follows: Figure 1 As shown, this application provides a photovoltaic system 1000, including a photovoltaic module 100. As... Figure 2 and Figure 3As shown, the photovoltaic module consists of a frame 110, a front cover plate 120, a first encapsulating film 130, a battery string layer 140, a second encapsulating film 150, and a back cover plate 160 stacked in sequence, as well as a junction box 170. The battery string layer 140 is made by connecting the self-healing perovskite battery provided in the specific embodiment of this application in series and parallel.
[0115] Example 1 This embodiment provides a method for preparing a self-healing perovskite solar cell, the method comprising: (1) Choline chloride and urea were dissolved in N,N-dimethylformamide according to a molar ratio of 1:2.5, and heated and stirred at 70°C to obtain a eutectic solution with a total concentration of 29 g / L of choline chloride and urea. (2) Prepare a Cs solution with a concentration of 1.8 mol / L. 0.05 FA 0.73 MA 0.22 Pb(I 0.77 Br 0.23 Add the eutectic solution prepared in step (1) to the solution to obtain the perovskite precursor composite solution, wherein the volume ratio of the eutectic solution to the perovskite precursor solution is 0.01:1. (3) Using TOPCon battery as substrate, a 10nm thick SnO2 layer is prepared on its surface as an intermediate composite layer by reactive plasma deposition. (4) A concentration of 1 mg / mL of poly-4pacz was spin-coated onto the surface of the SnO2 intermediate composite layer at a spin speed of 4000 rpm for 30 seconds. The layer was then heated at 100°C for 10 minutes to form a hole transport layer. (5) In an air environment, spin-coat the perovskite precursor composite solution obtained in step (2) on the surface of the hole transport layer. The spin-coating speed is 2000 rpm and the spin-coating time is 7s. Then, place it in a flash evaporator and evacuate it for 10s until the pressure inside the cavity is 5Pa. Anneal at 100℃ for 20min to form a perovskite light-absorbing layer. (6) Prepare a polyimide isopropanol solution with a concentration of 0.3 mg / mL, statically drop it onto the surface of the perovskite light-absorbing layer, rotate at 5000 rpm for 30 s to form a 3 nm passivation layer; (7) An 8 nm thick C60 was deposited on the surface of the passivation layer by thermal evaporation coating, and then 120 cycles of SnO2 were deposited by atomic layer deposition to obtain the electron transport layer. (8) A transparent conductive layer was obtained by sputtering a 40 nm thick IZO layer using magnetron sputtering. (9) An Ag electrode was deposited on the surface of the transparent conductive layer by thermal evaporation coating method, and the thickness of the Ag electrode was 120 nm.
[0116] Example 2 This embodiment provides a method for preparing a self-healing perovskite solar cell, the method comprising: (1) Choline chloride and urea were dissolved in N,N-dimethylformamide according to a molar ratio of 1:2, and heated and stirred at 60°C to obtain a eutectic solution with a total concentration of 25 g / L of choline chloride and urea. (2) Prepare a Cs solution with a concentration of 2.0 mol / L. 0.05 FA 0.73 MA 0.22 Pb(I 0.77 Br 0.23 Add the eutectic solution prepared in step (1) to the solution to obtain the perovskite precursor composite solution, wherein the volume ratio of the eutectic solution to the perovskite precursor solution is 0.02:1. (3)~(4) Same as Example 1; (5) In an air environment, spin-coat the perovskite precursor composite solution obtained in step (2) on the surface of the hole transport layer. The spin-coating speed is 1500 rpm and the spin-coating time is 5s. Then, place it in a flash evaporator and evacuate it for 8s until the pressure inside the cavity is 10Pa. Anneal at 90℃ for 30min to form a perovskite light-absorbing layer. (6)~(9) Same as Example 1.
[0117] Example 3 This embodiment provides a method for preparing a self-healing perovskite solar cell, the method comprising: (1) Choline chloride and urea were dissolved in N,N-dimethylformamide according to a molar ratio of 1:3, and heated and stirred at 80°C to obtain a eutectic solution with a total concentration of 35 g / L of choline chloride and urea. (2) Prepare a Cs solution with a concentration of 1.6 mol / L. 0.05 FA 0.73 MA 0.22 Pb(I 0.77 Br 0.23 Add the eutectic solution prepared in step (1) to the solution to obtain the perovskite precursor composite solution, wherein the volume ratio of the eutectic solution to the perovskite precursor solution is 0.005:1. (3)~(4) Same as Example 1; (5) In an air environment, spin-coat the perovskite precursor composite solution obtained in step (2) on the surface of the hole transport layer. The spin-coating speed is 2500 rpm and the spin-coating time is 9s. Then, place it in a flash evaporator and evacuate it for 12s until the pressure inside the cavity is 3Pa. Anneal at 110℃ for 10min to form a perovskite light-absorbing layer. (6)~(9) Same as Example 1.
[0118] Example 4 This embodiment provides a method for preparing a self-healing perovskite battery. Except for the molar ratio of choline chloride to urea of 1:2.3 in step (1), the preparation method is the same as in Example 1.
[0119] Example 5 This embodiment provides a method for preparing a self-healing perovskite battery. Except for the molar ratio of choline chloride to urea of 1:2.8 in step (1), the preparation method is the same as in Example 1.
[0120] Example 6 This embodiment provides a method for preparing a self-healing perovskite battery. Except for the molar ratio of choline chloride to urea of 1:4 in step (1), the preparation method is the same as in Example 1.
[0121] Example 7 This embodiment provides a method for preparing a self-healing perovskite battery. Except for the molar ratio of choline chloride to urea in step (1) being 1:1, the preparation method is the same as in Example 1.
[0122] Example 8 This embodiment provides a method for preparing a self-healing perovskite solar cell. Except for step (5), in which the spin-coated perovskite wet film is placed in a flash evaporator and a vacuum is drawn for 15 seconds until the pressure inside the cavity is 5 Pa, the preparation method is the same as in Example 1.
[0123] Example 9 This embodiment provides a method for preparing a self-healing perovskite solar cell. The preparation method is the same as in Example 1, except that the perovskite wet film obtained by spin coating is placed in a flash evaporator and a vacuum is drawn for 5 seconds until the pressure inside the chamber is 5 Pa.
[0124] Comparative Example 1 This comparative example provides a method for preparing a perovskite solar cell, wherein the preparation method omits step (1) and does not introduce Cs into step (2). 0.05 FA 0.73 MA 0.22 Pb(I 0.77 Br 0.23 Add the eutectic solution to the solution, and in step (5) spin-coat only Cs. 0.05 FA 0.73 MA 0.22 Pb(I 0.77 Br 0.23 Except for the solution 3, everything else is the same as in Example 1.
[0125] Comparative Example 2 This comparative example provides a method for preparing a perovskite solar cell. Except for step (5), in the process of spin-coating the perovskite precursor composite solution, the method is the same as in Example 1, except that in step (5), the perovskite precursor composite solution is first spin-coated at 1000 rpm for 10 s, then spin-coated at 5000 rpm for 30 s, and 180 μL of CB as an antisolvent is dropped onto the membrane 10 seconds before the end of the final program, and then annealed.
[0126] The open-circuit voltage (Voc), short-circuit current (Isc), fill factor (FF), and photoelectric conversion efficiency of the perovskite solar cells prepared in all the above embodiments and comparative examples are shown in Table 1. The photoelectric conversion efficiency retention rates after continuous operation for 100h, 500h, and 1000h are shown in Table 2.
[0127] Table 1 Table 2 Based on the test results of Examples 1 to 5 and Comparative Example 1 in Tables 1 and 2, this invention introduces choline chloride and urea in a suitable molar ratio as eutectic additives into the perovskite precursor composite solution. Combined with a spin-coating flash evaporation process, during the flash evaporation stage, the eutectic additives are pushed by the rapidly growing perovskite grains to the interface between the perovskite light-absorbing layer and the passivation layer, forming a eutectic interface layer at the edge of the perovskite grains on the surface of the perovskite light-absorbing layer. This eutectic interface layer acts as a self-healing layer, effectively passivating defects in the perovskite material, stabilizing the perovskite lattice, and significantly improving the photoelectric performance of the perovskite solar cell. Simultaneously, the self-healing layer transforms into a low-viscosity liquid state when the perovskite solar cell is heated to 40℃~60℃, repairing micro-cracks caused by thermal expansion and contraction, achieving self-repair of micro-cracks, improving the stability of the perovskite solar cell, and maintaining high photoelectric conversion efficiency even after long-term operation.
[0128] According to the test results of Examples 1, 6 and 7, if the molar ratio of choline chloride to urea deviates from the appropriate molar ratio, the passivation and lattice strengthening effect on the perovskite material will decrease. At the same time, the resulting eutectic interface layer structure will be loose and unnecessary, reducing the ability to repair defects and microcracks generated during application, resulting in a decrease in both the photoelectric performance and stability of the perovskite solar cell.
[0129] Based on the test results of Examples 1, 8, and 9, and Comparative Example 2, if the perovskite light-absorbing layer is prepared using the anti-solvent method instead of the flash evaporation method, choline chloride and urea will enter the crystal lattice during the perovskite crystallization process and will not be able to accumulate at the grain boundaries and on the surface of the perovskite light-absorbing layer, thus losing the self-healing ability of the perovskite solar cell. If the flash evaporation pumping speed is too slow, some eutectic additives will also enter the perovskite crystal lattice, resulting in too few eutectic additives accumulating at the grain boundaries and on the surface of the perovskite light-absorbing layer, leading to the inability to form a eutectic interface layer locally, thus weakening the self-healing ability of the perovskite solar cell. On the other hand, if the flash evaporation pumping speed is too fast, the perovskite nucleation and growth rate will be too fast, generating a large number of defects inside the crystal, resulting in a decrease in the photoelectric performance of the perovskite solar cell.
[0130] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A method for preparing a self-healing perovskite solar cell, characterized in that, The preparation method includes: A first carrier transport layer, a perovskite light-absorbing layer, a passivation layer, a second carrier transport layer, a transparent conductive layer, and a metal electrode are sequentially fabricated on the substrate surface. The method for preparing the perovskite absorber layer includes: A perovskite precursor composite solution is spin-coated onto the surface of the first carrier transport layer, flash-evaporated, and annealed to obtain the perovskite absorber layer. The perovskite precursor composite solution includes a perovskite precursor and a eutectic additive; the eutectic additive includes choline chloride and urea.
2. The preparation method according to claim 1, characterized in that, The preparation method of the perovskite precursor composite solution includes: Choline chloride and urea are mixed in a solvent and heated and stirred to obtain a eutectic solution; the eutectic solution is added to a perovskite precursor solution to obtain the perovskite precursor composite solution.
3. The preparation method according to claim 2, characterized in that, In the eutectic solution, the molar ratio of choline chloride to urea is 1:(2~3); And / or, in the eutectic solution, the total concentration of choline chloride and urea is 25 g / L to 35 g / L; And / or, in the perovskite precursor solution, the concentration of the perovskite precursor is 1.6 mol / L to 2.0 mol / L; And / or, the volume ratio of the eutectic solution to the perovskite precursor solution is (0.005~0.02):1, and the volume of the eutectic solution and the perovskite precursor solution is in liters (L).
4. The preparation method according to claim 2 or 3, characterized in that, The heating and stirring temperature is 60℃~80℃; And / or, the solvent includes N,N-dimethylformamide.
5. The preparation method according to any one of claims 1 to 4, characterized in that, The rotation speed of the spin-coated perovskite precursor composite solution is 1500 rpm to 2500 rpm. And / or, the spin-coating time of the perovskite precursor composite solution is 5s~9s; And / or, the flash evaporation includes evacuating the cavity to a pressure of 3 Pa to 10 Pa for 8 to 12 seconds.
6. The preparation method according to any one of claims 1 to 5, characterized in that, The annealing temperature is 90℃~110℃; And / or, the annealing time is 10 min to 30 min.
7. The preparation method according to any one of claims 1 to 6, characterized in that, The self-healing perovskite solar cell was prepared in an air environment; And / or, the substrate includes any one of FTO conductive glass substrate, ITO conductive glass substrate, or crystalline silicon substrate.
8. A self-healing perovskite solar cell, characterized in that, The self-healing perovskite solar cell includes a first carrier transport layer, a perovskite light-absorbing layer, a passivation layer, a second carrier transport layer, a transparent conductive layer, and a metal electrode, which are sequentially stacked on the surface of a substrate. The surface of the perovskite absorption layer adjacent to the passivation layer also includes an in-situ formed self-healing layer, which is discontinuously formed in-situ at the grain boundary edges of the surface perovskite grains.
9. The self-healing perovskite solar cell as described in claim 8, characterized in that, The melting point of the self-healing layer is 40℃~60℃.
10. A photovoltaic module, characterized in that, The photovoltaic module includes the self-healing perovskite cell as described in claim 8 or 9.
Citation Information
Patent Citations
Double-sided passivated perovskite cell, preparation method thereof and photovoltaic module
CN117082879A
Preparation method and structure of perovskite battery
CN119546140A