A niobium oxide threshold device and a method of manufacturing the same

By using pulsed laser deposition to prepare a niobium oxide transformation layer in a niobium oxide threshold device, controlling the vacuum level and regulating the oxygen vacancy concentration, the problems of device consistency and durability were solved, and hardware support for high-precision neuromorphic information processing was realized.

CN123124672APending Publication Date: 2026-11-17HUBEI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611236720.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing niobium oxide threshold devices suffer from poor consistency and durability when used in neuronal functional applications, making it difficult to meet the needs of high-precision neuromorphic computing.

Method used

A niobium oxide transformation layer was prepared on the surface of the bottom electrode using pulsed laser deposition. The vacuum level of the chamber was controlled at 0.14~0.3 Pa. The oxygen vacancy concentration and thin film crystal structure in the niobium oxide transformation layer were adjusted to optimize the device performance.

Benefits of technology

It improves the consistency and durability of the device's switching voltage, keeps the device stable under long pulse stimulation, and shows no significant degradation in the switching current, providing a solid hardware foundation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124672A_ABST
    Figure CN123124672A_ABST
Patent Text Reader

Abstract

This invention provides a niobium oxide threshold device and its fabrication method. The niobium oxide threshold device of this invention includes a substrate, a bottom electrode, a niobium oxide transition layer, and a top electrode. The fabrication method of the niobium oxide transition layer is as follows: using Nb₂O₅ as the target material, a niobium oxide transition layer is prepared on the surface of the bottom electrode using pulsed laser deposition. During deposition, the vacuum degree in the chamber is 0.14~0.3 Pa. By controlling the oxygen vacancy concentration and the crystal phase structure in the thin film, the electrical performance of the device is optimized. By controlling the deposition temperature, the crystal phase of the thin film is improved. The orthorhombic Nb₂O₅ phase with high symmetry (T-Nb₂O₅) can effectively limit the formation and breakage paths of conductive wires, improving the consistency of its transition voltage. The niobium oxide threshold device provided by this invention achieves significant performance improvements in voltage consistency and durability, providing a solid hardware foundation for high-precision neuromorphic information processing and related large-scale integrated applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of microelectronic integrated circuit technology, and in particular to a niobium oxide threshold device and its fabrication method. Background Technology

[0002] With the explosive growth of data volume, current von Neumann architecture computers face increasingly severe performance challenges in processing massive amounts of data. Neuromorphic computing, inspired by the operating mechanisms of the biological brain, is considered one of the next-generation computing architectures that holds the promise of breaking through the "von Neumann" bottleneck. Artificial neurons, as the basic building blocks of this architecture, provide solid physical support for next-generation ultra-low-power neuromorphic intelligent systems due to their efficient hardware implementation capabilities. In terms of device selection, threshold devices, with their high integration and low power consumption, are considered the core building blocks for neuromorphic hardware. Among them, niobium oxide threshold devices, with their unique metal-insulator transition characteristics and better stability, have become the preferred choice for constructing this neuron model. However, existing niobium oxide devices still suffer from poor consistency and durability in neuronal functional applications. Summary of the Invention

[0003] To overcome the shortcomings of existing technologies, this invention provides a niobium oxide threshold device and its fabrication method. The method for fabricating the niobium oxide transition layer involves using Nb₂O₅ as the target material and employing pulsed laser deposition to prepare the niobium oxide transition layer on the surface of the bottom electrode. During deposition, the vacuum level within the chamber is maintained at 0.14–0.3 Pa. By controlling the oxygen vacancy concentration in the niobium oxide transition layer, this invention significantly improves device performance, including the consistency of the transition voltage and the durability of the device under long-pulse stimulation. The principle behind this is the optimization of the microstructure of the Nb₂O₅ region within the device, reducing the randomness of conductive filament growth, thereby optimizing the consistency of the transition voltage and exhibiting excellent durability. This invention provides strong hardware support for achieving high-precision neuromorphic information processing.

[0004] To achieve the above technical objectives, the present invention adopts the following technical solution:

[0005] In a first aspect, the present invention provides a niobium oxide threshold device, comprising:

[0006] Substrate;

[0007] The bottom electrode is located on the surface of the substrate;

[0008] A niobium oxide conversion layer is located on the surface of the bottom electrode;

[0009] The top electrode is located on the surface of the niobium oxide transformation layer;

[0010] The method for preparing the niobium oxide transformation layer is as follows:

[0011] Using Nb2O5 as the target material, a niobium oxide transformation layer was prepared on the surface of the bottom electrode by pulsed laser deposition. The vacuum degree in the chamber during deposition was 0.14~0.3 Pa.

[0012] Preferably, the bottom electrode is made of one of Ti, Pt, W or TiN;

[0013] The material of the top electrode is either Pt or Ti.

[0014] Preferably, the thickness of the bottom electrode is 100~300 nm;

[0015] The thickness of the niobium oxide transformation layer is 1~300 nm;

[0016] The thickness of the top electrode is 10~200nm.

[0017] Preferably, the top electrodes are arranged in an array on the surface of the niobium oxide transformation layer;

[0018] The top electrode has a circular or rectangular cross-section, with the radius of the circle being 0.05~0.5mm and the side length of the rectangle being 0.1~1mm.

[0019] Preferably, the substrate includes any one of Si substrate, Si / SiO2 substrate, Si / SiO2 / Ti substrate, c-plane sapphire substrate, magnesium oxide substrate, gallium oxide substrate, gallium nitride substrate, NSTO substrate, quartz glass substrate, r-plane sapphire substrate, and a-plane sapphire substrate.

[0020] Secondly, the present invention also provides a method for preparing the niobium oxide threshold device, comprising the following steps:

[0021] Fabricate the bottom electrode on the substrate;

[0022] A niobium oxide conversion layer is prepared on the surface of the bottom electrode;

[0023] A top electrode was fabricated on the surface of the niobium oxide transformation layer;

[0024] The method for preparing the niobium oxide transformation layer is as follows:

[0025] Using Nb2O5 as the target material, a niobium oxide transformation layer was prepared on the surface of the bottom electrode by pulsed laser deposition. The vacuum degree in the chamber during deposition was 0.14~0.3 Pa.

[0026] Preferably, when the niobium oxide transformation layer is prepared on the surface of the bottom electrode by pulsed laser deposition, the deposition temperature is 400~500℃ and the pulsed laser energy is 350~400 mJ.

[0027] Preferably, the top electrode is prepared by:

[0028] Using the material corresponding to the top electrode as the target material, the top electrode was prepared on the surface of the niobium oxide transformation layer by pulsed laser deposition.

[0029] The deposition temperature is 20~25℃, and the pulsed laser energy is 300~400 mJ.

[0030] Preferably, fabricating the bottom electrode on the substrate specifically includes:

[0031] The bottom electrode was fabricated on a substrate using pulsed laser deposition with the material corresponding to the bottom electrode as the target material.

[0032] The deposition temperature is 20~25℃, and the pulsed laser energy is 300~400 mJ.

[0033] The niobium oxide threshold device and its fabrication method of the present invention have the following advantages compared with the prior art:

[0034] The niobium oxide threshold device of the present invention includes a substrate, a bottom electrode, a niobium oxide transition layer, and a top electrode. The niobium oxide transition layer is prepared by using Nb₂O₅ as a target material and pulsed laser deposition on the surface of the bottom electrode. During deposition, the vacuum level in the chamber is 0.14~0.3 Pa. By controlling the oxygen vacancy concentration and crystal phase structure in the thin film, the electrical performance of the device is optimized. Specifically, by controlling the deposition oxygen pressure, the oxygen vacancy concentration in the niobium oxide transition layer is improved, optimizing the device's durability under long-pulse stimulation. Furthermore, by controlling the deposition temperature, the crystal phase of the thin film is improved. The orthorhombic Nb₂O₅ phase (T-Nb₂O₅) with high symmetry can effectively limit the formation and breakage paths of the conductive wire, improving its transition voltage consistency. The device of the present invention exhibits good consistency in 100 IV cycles, with the transition voltage dispersion rate remaining below 2%. The device of the present invention also exhibits good consistency after 10 IV cycles. 8 After several pulses, the device maintains a stable operating state, and during the pulse application process, the switching current of the device does not show significant degradation, and there are no abnormal fluctuations between the on-state and off-state currents. The niobium oxide threshold device provided by this invention achieves a significant performance improvement in voltage consistency and durability, providing a solid hardware foundation for high-precision neuromorphic information processing and related large-scale integrated applications. Attached Figure Description

[0035] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0036] Figure 1 This is a schematic diagram of the niobium oxide threshold device provided by the present invention;

[0037] Figure 2 This is a schematic diagram of the fabrication method of the niobium oxide threshold device provided by the present invention;

[0038] Figure 3 XPS analysis images of Nb in the niobium oxide transformation layers prepared in Examples 1-3 and Comparative Example 1;

[0039] Figure 4 XPS analysis images of O element in the niobium oxide transformation layers prepared in Examples 1-3 and Comparative Example 1;

[0040] Figure 5 The XRD patterns of the niobium oxide transformation layers prepared in Examples 1-3 and Comparative Example 1 are shown.

[0041] Figure 6 The following is a comparison of the Forming curves of the niobium oxide threshold devices prepared in Examples 1-3 and Comparative Example 1 of this invention;

[0042] Figure 7 The above are IV diagrams of the niobium oxide threshold devices prepared in Examples 1-3 and Comparative Example 1 of this invention;

[0043] Figure 8 The cumulative distribution diagram and dispersion coefficient of the switching voltage of the niobium oxide threshold devices prepared in Examples 1-3 and Comparative Example 1 are shown.

[0044] Figure 9 The durability diagrams show the niobium oxide threshold devices prepared in Examples 1-3 and Comparative Example 1. Detailed Implementation

[0045] The technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0046] It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of embodiments. Furthermore, in the description of this application, the term "comprising" means "including but not limited to". Various embodiments of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a rigid limitation on the scope of the invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single digits within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Additionally, whenever a numerical range is indicated herein, it means including any referenced number (fraction or integer) within the indicated range.

[0047] This invention provides a niobium oxide threshold device, such as... Figure 1 As shown, it includes:

[0048] Substrate 1;

[0049] Bottom electrode 2 is located on the surface of substrate 1;

[0050] Niobium oxide transformation layer 3 is located on the surface of bottom electrode 2;

[0051] Top electrode 4 is located on the surface of niobium oxide transformation layer 3;

[0052] The method for preparing the niobium oxide transformation layer is as follows:

[0053] Using Nb2O5 as the target material, a niobium oxide transformation layer was prepared on the surface of the bottom electrode by pulsed laser deposition. The vacuum degree in the chamber during deposition was 0.14~0.3 Pa.

[0054] Currently, traditional threshold switching devices still face many serious challenges in their journey towards large-scale integration and commercial application. Firstly, the operating voltage (threshold voltage (V)) remains a significant hurdle. th ) and holding voltage (V hold The high threshold voltage (TVP) results in high system power consumption. Secondly, the device exhibits significant fluctuations during multiple cycles, leading to poor device consistency and difficulty in achieving precise control. Furthermore, the device's durability is poor, and it is prone to degradation under long-pulse stimulation. Therefore, developing novel threshold devices that meet the requirements of high-precision neuromorphic computing has become a key technical challenge urgently needing to be solved in this field.

[0055] The niobium oxide threshold device fabricated in this invention, exhibiting high transition voltage consistency and durability, boasts advantages such as simple fabrication, low cost, and compatibility with modern CMOS processes. The fabrication method of the niobium oxide transition layer in this invention involves using Nb₂O₅ as the target material and employing pulsed laser deposition to prepare the niobium oxide transition layer on the surface of the bottom electrode. During deposition, the vacuum level in the chamber is maintained at 0.14~0.3 Pa. By controlling the oxygen vacancy concentration and crystal phase structure in the thin film, the electrical performance of the device is optimized. Specifically, by controlling the deposition oxygen pressure, the oxygen vacancy concentration in the niobium oxide transition layer is improved, optimizing the device's durability under long-pulse stimulation. Furthermore, by controlling the deposition temperature, the crystal phase of the thin film is improved. The highly symmetric orthorhombic Nb₂O₅ phase (T-Nb₂O₅) effectively limits the formation and breakage paths of the conductive wire, improving its transition voltage consistency. The device of this invention exhibits good consistency in 100 IV cycles, with the transition voltage dispersion rate remaining below 2%. In addition, to evaluate the long-term stability of the device, pulse durability tests were performed on the device deposited at 500℃. The device of this invention has undergone 10 8 After several pulses, the device maintains a stable operating state, and during the pulse application process, the switching current of the device does not show significant degradation, and there are no abnormal fluctuations between the on-state and off-state currents. The niobium oxide threshold device provided by this invention achieves a significant performance improvement in voltage consistency and durability, providing a solid hardware foundation for high-precision neuromorphic information processing and related large-scale integrated applications.

[0056] In some embodiments, the bottom electrode is made of one of Ti, Pt, W or TiN;

[0057] The top electrode is made of either Pt or Ti.

[0058] The substrate includes any one of the following: Si substrate, Si / SiO2 substrate, Si / SiO2 / Ti substrate, c-plane sapphire substrate, magnesium oxide substrate, gallium oxide substrate, gallium nitride substrate, NSTO substrate, quartz glass substrate, r-plane sapphire substrate, and a-plane sapphire substrate.

[0059] Preferably, the bottom electrode is Pt, which is a chemically stable noble metal with both high conductivity and strong corrosion resistance, making it an ideal choice for the bottom electrode of a threshold device; the substrate is a Si / SiO2 / Ti substrate; Ti, as an interface adhesion layer, has good adhesion to both Si and SiO2, which can effectively enhance the bonding force between the Pt layer and Si / SiO2, and prevent the Pt layer from falling off during subsequent processing or use; both Si and SiO2 have excellent thermal stability.

[0060] In some embodiments, the thickness of the bottom electrode is 100~300nm;

[0061] The thickness of the niobium oxide transformation layer is 1~300nm;

[0062] The thickness of the top electrode is 10~200nm.

[0063] In some embodiments, the top electrodes are arranged in an array on the surface of the niobium oxide conversion layer;

[0064] The top electrode cross-section is circular or rectangular, with a radius of 0.05~0.5mm for the circle and a side length of 0.1~1mm for the rectangle.

[0065] In some embodiments, the substrate includes any one of Si substrate, Si / SiO2 substrate, Si / SiO2 / Ti substrate, c-plane sapphire substrate, magnesium oxide substrate, gallium oxide substrate, gallium nitride substrate, NSTO substrate, quartz glass substrate, r-plane sapphire substrate, and a-plane sapphire substrate.

[0066] The niobium oxide threshold device of this invention achieves threshold switching of the niobium oxide conversion layer by applying an external voltage between the top and bottom electrodes. Specifically, external signal excitation is connected to both ends of the top and bottom electrodes to form a current loop. By regulating the external voltage and limiting the current, a resistance change condition is reached, enabling the switching between the high-resistance and low-resistance states of the niobium oxide threshold device, thereby completing the storage of information data. Furthermore, the relevant characteristics of neurons can be simulated under the action of external excitation, promoting the application of neuromorphic computing.

[0067] Based on the same inventive concept, the present invention also provides a method for fabricating the aforementioned niobium oxide threshold device, comprising the following steps:

[0068] Fabricate the bottom electrode on the substrate;

[0069] A niobium oxide conversion layer is prepared on the surface of the bottom electrode;

[0070] A top electrode was fabricated on the surface of the niobium oxide transformation layer;

[0071] The method for preparing the niobium oxide transformation layer is as follows:

[0072] Using Nb2O5 as the target material, a niobium oxide transformation layer was prepared on the surface of the bottom electrode by pulsed laser deposition. The vacuum degree in the chamber during deposition was 0.14~0.3 Pa.

[0073] In some embodiments, when a niobium oxide transformation layer is prepared on the surface of the bottom electrode using pulsed laser deposition, the deposition temperature is 400~500℃ and the pulsed laser energy is 350~400 mJ. Specifically, after deposition, the laser is turned off and the substrate is kept at the same temperature as the deposition temperature for 30 minutes. Then, the temperature is lowered to below 50℃, nitrogen gas is introduced to break the vacuum, the chamber is opened, and the substrate with the deposited niobium oxide transformation layer is removed. During the heat preservation process, sufficient time is provided for the thin film / solid phase reaction of the niobium oxide transformation layer, so that the chemical reaction can proceed fully and the crystal phase change can be more complete. At the same time, the material composition is homogenized, the internal film stress is released, and the intrinsic performance fluctuations caused by incomplete reaction, crystallization defects, and compositional inhomogeneity are eliminated.

[0074] In some embodiments, the top electrode is prepared as follows:

[0075] Using the material corresponding to the top electrode as the target material, the top electrode was prepared on the surface of the niobium oxide transformation layer by pulsed laser deposition.

[0076] The deposition temperature is 20~25℃, and the pulsed laser energy is 300~400 mJ.

[0077] In some embodiments, fabricating a bottom electrode on a substrate specifically includes:

[0078] The bottom electrode was fabricated on a substrate using pulsed laser deposition with the material corresponding to the bottom electrode as the target material.

[0079] The deposition temperature is 20~25℃, and the pulsed laser energy is 300~400 mJ.

[0080] In some embodiments, before fabricating the bottom electrode on the substrate, the substrate is cleaned. Specifically, the substrate is placed in a beaker, and an appropriate amount of acetone is poured in for cleaning. Since acetone is a volatile solution, it needs to be sealed with plastic wrap and then ultrasonically cleaned for 30 minutes. This step is mainly to remove impurities such as organic matter. After cleaning, the substrate is removed with tweezers and placed in another beaker. Anhydrous ethanol is poured in, and the substrate is cleaned twice. After sealing, it is ultrasonically cleaned for 20 minutes. This step is mainly to remove acetone and other surface contaminants. Finally, the substrate is placed in a beaker containing deionized water and ultrasonically cleaned for 10 minutes. After ultrasonic cleaning, it is dried.

[0081] Further reference Figure 2 As shown, the Si / SiO2 / Ti substrate is first cleaned, and then a bottom electrode Pt is fabricated on the Si / SiO2 / Ti substrate. A small amount of conductive silver paste is applied to the edge of the bottom electrode Pt to create an electrical contact channel. A niobium oxide transformation layer (i.e., NbO) is deposited on the portion of the bottom electrode Pt not coated with conductive silver paste. x(Functional layer); then a mask is placed on the niobium oxide conversion layer, and multiple holes adapted to the top electrode are opened on the mask. Ti is deposited on the niobium oxide conversion layer using the mask. After removing the mask and conductive silver paste, the top electrode Ti can finally be obtained on the niobium oxide conversion layer.

[0082] The following detailed embodiments further illustrate the niobium oxide threshold device and its fabrication method of this application. This section, in conjunction with specific embodiments, further explains the content of the present invention, but should not be construed as limiting the invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods, and equipment used in this invention are conventional reagents, methods, and equipment in the art.

[0083] Example 1

[0084] This embodiment provides a niobium oxide threshold device, including:

[0085] Substrate;

[0086] The bottom electrode is located on the substrate surface;

[0087] A niobium oxide conversion layer is located on the surface of the bottom electrode.

[0088] The top electrode is located on the surface of the niobium oxide transformation layer;

[0089] The bottom electrode is made of Pt and has a thickness of 200 nm.

[0090] The thickness of the niobium oxide transformation layer is 100 nm;

[0091] The top electrodes are arranged in an array on the niobium oxide transformation layer. The cross-section of the top electrode is circular with a radius of 0.2 mm. The material of the top electrode is Ti and the thickness of the top electrode is 50 nm.

[0092] The substrate is a Si / SiO2 / Ti substrate, with Si being p-type boron doped. <100> / <110> A single-crystal silicon wafer with dimensions of 10×10×0.5mm (i.e., 10mm in length, 10mm in width, and 0.5mm in thickness) is used to fabricate a 500nm SiO2 layer and a 50nm Ti layer sequentially on the wafer; the bottom electrode is located on the surface of the Ti layer.

[0093] The above-mentioned method for fabricating niobium oxide threshold devices includes the following steps:

[0094] S1. The substrate is ultrasonically cleaned with acetone for 30 min, ultrasonically cleaned with anhydrous ethanol for 20 min, and washed with deionized water for 10 min in sequence.

[0095] S2. A bottom electrode was prepared on a substrate using Pt as the target material and pulsed laser deposition method; wherein the deposition temperature was 25℃ and the pulsed laser energy was 350 mJ.

[0096] S3. Using Nb2O5 target material, a niobium oxide transformation layer was prepared on the surface of the bottom electrode by pulsed laser deposition. The vacuum degree in the chamber during deposition was 0.3 Pa, the deposition temperature was 500℃, and the pulsed laser energy was set to 350 mJ.

[0097] After deposition, the laser was turned off, the temperature was maintained at 500℃ for 30 minutes, then the temperature was lowered to below 50℃, nitrogen gas was introduced to break the vacuum, the chamber was opened and the substrate with a 100nm thick niobium oxide transformation layer was removed.

[0098] S4. Using Ti as the target material, a mask is set on the surface of the niobium oxide transformation layer. The mask has multiple holes adapted to the top electrode, and the radius of the holes is 0.2 mm. The top electrode is prepared on the surface of the niobium oxide transformation layer by pulsed laser deposition in a vacuum environment. The deposition temperature is 25℃ and the pulsed laser energy is 300 mJ.

[0099] Example 2

[0100] This embodiment provides a method for fabricating a niobium oxide threshold device similar to that in Embodiment 1, except that the method for fabricating the niobium oxide conversion layer is as follows: using a Nb2O5 target, a niobium oxide conversion layer is prepared on the surface of the bottom electrode by pulsed laser deposition. During deposition, the vacuum degree in the chamber is 0.3 Pa, the deposition temperature is 400 °C, and the pulsed laser energy is set to 350 mJ.

[0101] After deposition, the laser was turned off, the temperature was maintained at 400℃ for 30 minutes, then the temperature was lowered to below 50℃, nitrogen gas was introduced to break the vacuum, the chamber was opened and the substrate with a 100nm thick niobium oxide transformation layer was removed.

[0102] All other parameters are the same as those in Experiment 1.

[0103] Example 3

[0104] This embodiment provides a method for fabricating a niobium oxide threshold device similar to that in Embodiment 1, except that the method for fabricating the niobium oxide transformation layer is as follows: using a Nb2O5 target, a niobium oxide transformation layer is prepared on the surface of the bottom electrode by pulsed laser deposition. During deposition, the vacuum degree in the chamber is 0.14 Pa, the deposition temperature is 400 °C, and the pulsed laser energy is set to 350 mJ.

[0105] After deposition, the laser was turned off, the temperature was maintained at 400℃ for 30 minutes, then the temperature was lowered to below 50℃, nitrogen gas was introduced to break the vacuum, the chamber was opened and the substrate with a 100nm thick niobium oxide transformation layer was removed.

[0106] All other parameters are the same as those in Experiment 1.

[0107] Comparative Example 1

[0108] This embodiment provides a method for fabricating a niobium oxide threshold device similar to that in Embodiment 1, except that the niobium oxide transition layer is fabricated using a Nb₂O₅ target and pulsed laser deposition on the surface of the bottom electrode. During deposition, the chamber is in a vacuum environment (10⁻⁶ m² / 40⁻¹² ... -5 Pa), deposition temperature 400℃, pulsed laser energy set to 350 mJ;

[0109] After deposition, the laser was turned off, the temperature was maintained at 400℃ for 30 minutes, then the temperature was lowered to below 50℃, nitrogen gas was introduced to break the vacuum, the chamber was opened and the substrate with a 100nm thick niobium oxide transformation layer was removed.

[0110] All other parameters are the same as those in Experiment 1.

[0111] Performance testing

[0112] Figure 3 The images show XPS analysis of Nb in the niobium oxide transformation layers prepared in Examples 1-3 and Comparative Example 1; where Vacuum 400℃ represents Comparative Example 1, 0.14 Pa 400℃ represents Example 3, 0.30 Pa 400℃ represents Example 2, and 0.30 Pa 500℃ represents Example 1. Figures 4-9 They mean the same thing.

[0113] Figure 4 XPS analysis images of O element in the niobium oxide transformation layers prepared in Examples 1-3 and Comparative Example 1.

[0114] The relative Nb and O contents of the niobium oxide transformation layer prepared in Examples 1-3 and Comparative Example 1, Nb 5+ 、Nb 4+ 、Nb 2+ The relative contents of lattice O and vacant O are shown in Table 1 below:

[0115] Table 1 - Relative Nb and O contents of niobium oxide transformation layer in different embodiments

[0116]

[0117] Figure 3 and Figure 4 XPS analysis images of Nb and O under different deposition conditions are shown, illustrating the chemical states and contents of Nb and O. The atomic proportions of Nb in each valence state in the thin film prepared in Comparative Example 1 are as follows: 2+ Nb4+ Nb 5+ =45.45:30.63:23.92; the atomic ratio of lattice oxygen to oxygen vacancy in the oxygen element is 78.92:21.08. Other process conditions for Nb 3d5 / 2 The binding energy is significantly higher than that of Nb. 4+ 3d5 / 2 The binding energy positions indicate that the valence states of Nb in the film are predominantly tetravalent and pentavalent, therefore, no additional peak splitting is needed for the characteristic peak corresponding to divalent niobium. With the oxygen pressure increasing to 0.3 Pa, the Nb:O atomic ratio increased from 35.23:64.77 to 33.93:66.07, and the Nb in the film became... 4+ :Nb 5+ =57.25: 42.75; the atomic ratio of lattice oxygen to oxygen vacancy in oxygen element becomes 86.86: 13.14. In Example 1, the oxygen pressure is fixed at 0.3 Pa, and the temperature is increased to 500℃, the Nb:O ratio becomes 34.62: 65.38, Nb 4+ Nb 5+ =58.73: 41.27, lattice oxygen: oxygen vacancy=85.77:14.23.

[0118] Figure 5 The images show the XRD patterns of the niobium oxide transformation layers prepared in Examples 1-3 and Comparative Example 1.

[0119] from Figure 5 As can be seen from the XRD results, compared with the thin film prepared in Comparative Example 1, the thin film prepared in Example 1 has 2θ values ​​of 22.81° and 56.364°, which are the diffraction peaks of the (0 0 1) and (3 8 1) crystal planes of the orthorhombic Nb2O5 phase (T-Nb2O5). T-Nb2O5 has better lattice symmetry, and the open tunnel structure provides a uniform migration path for oxygen vacancies, which can effectively suppress the random growth of oxygen vacancy-type conductive wires, thereby improving the consistency of device cycling. Figure 5 The Pt peak in the middle is the Pt peak on the substrate.

[0120] The niobium oxide threshold devices prepared in Examples 1-3 and Comparative Example 1 were subjected to corresponding performance tests, all of which were performed on the Agilent B1500A semiconductor parameter analyzer platform. Specifically, the IV characteristics of the prepared niobium oxide threshold devices were tested. The niobium oxide threshold devices were placed on the probe stage of the Agilent B1500A semiconductor parameter analyzer, with the positive probe in close contact with the Ti top electrode and the negative probe in close contact with the Pt bottom electrode. A DC voltage of 0-8 V was applied to the Ti top electrode to perform the forming process. As shown in Figure 6, when the voltage was approximately 6 V, the resistance state of the niobium oxide threshold device prepared in Comparative Example 1 changed from an initial high-resistance state to a low-resistance state; this voltage is the forming voltage. The forming voltage of the device prepared in Example 1 was approximately 7 V.

[0121] Next, the formed niobium oxide threshold device was subjected to 100 cycles of alternating positive and negative scan voltages under a 2 mA current limit and a scan voltage ranging from 0 V to 1.5 V. The resulting IV curve is shown below. Figure 7 As shown. The device fabricated in Comparative Example 1 transitions from the off state to the on state when the voltage increases to 1.2 V. This voltage is the positive threshold voltage (V) of the device. th+ Subsequently, when the voltage across the device retraces from 1.5 V to 0 V, the current suddenly decreases when the voltage retraces to 0.9 V, indicating that the device has switched to the off state, corresponding to the forward holding voltage (V). hold+ The value is 0.9 V. The reverse voltage test pattern is the same as the forward voltage test. The negative threshold voltage (V) can be obtained from the IV curve. th- ) and negative holding voltage (V hold- The threshold switching voltage and holding voltage of the device prepared in Example 1 were -1.2 V and -0.9 V, respectively.

[0122] Figure 8 The cumulative distribution diagram and the dispersion coefficient of the switching voltage of the niobium oxide threshold devices prepared in Examples 1-3 and Comparative Example 1 are shown.

[0123] like Figure 8 As shown, the negative threshold voltage (V) of the device prepared in Comparative Example 1 th- ) and negative holding voltage (V hold- The coefficients of variation are 2.48% and 1.77% respectively, and the forward holding voltage (V) hold+ ), positive threshold voltage (V) th+ The coefficients of variation were 2.89% and 1.96%, respectively; while the negative threshold voltage (V) of the device prepared in Example 1 was... th- ) and negative holding voltage (V hold-The coefficients of variation are 1.23% and 0.29%, respectively, and the forward holding voltage (V) hold+ ), positive threshold voltage (V) th+ The coefficients of variation were 1.16% and 1.82%, respectively. Compared with the device prepared in Comparative Example 1, the device prepared in Example 1 had a smaller coefficient of variation in switching voltage, which indirectly proves the importance of crystal phase modulation for optimizing the consistency of switching voltage.

[0124] Figure 9 The image shows the durability of the niobium oxide threshold devices prepared in Examples 1-3 and Comparative Example 1. Figure 9 In the invention, ONCurrent refers to the on-state current, which is the current when the voltage is read. In this invention, it refers to the current limit set when testing the device. OffCurrent refers to the off-state current, which is the device current when the voltage is read at 1 / 2.

[0125] like Figure 9 As shown, the device prepared in Example 1 achieves a durability of 10. 8 This is significantly better than the device prepared in Comparative Example 1 (10). 5 (times). This significant comparative result fully demonstrates that by synergistically controlling deposition temperature and oxygen pressure, NbO deposition was successfully optimized. x The crystalline phase structure in the thin film improves the oxygen vacancy concentration, thereby effectively suppressing random overgrowth or breakage of the conductive wire during long-term, high-frequency switching processes, providing the device with excellent long-term operational reliability.

[0126] It is understood that the technical features of the above embodiments can be combined arbitrarily. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0127] The above are merely preferred embodiments of this application, and only specifically describe the technical principles of this application. These descriptions are only for explaining the principles of this application and should not be construed as limiting the scope of protection of this application in any way. Based on this explanation, any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application, as well as other specific embodiments of this application that can be conceived by those skilled in the art without creative effort, should be included within the scope of protection of this application.

Claims

1. A niobium oxide threshold device, characterized in that, include: Substrate; The bottom electrode is located on the surface of the substrate; A niobium oxide conversion layer is located on the surface of the bottom electrode; The top electrode is located on the surface of the niobium oxide transformation layer; The method for preparing the niobium oxide transformation layer is as follows: Using Nb2O5 as the target material, a niobium oxide transformation layer was prepared on the surface of the bottom electrode by pulsed laser deposition. The vacuum degree in the chamber during deposition was 0.14~0.3 Pa.

2. The niobium oxide threshold device as described in claim 1, characterized in that, The material of the bottom electrode is one of Ti, Pt, W or TiN; The material of the top electrode is either Pt or Ti.

3. The niobium oxide threshold device as described in claim 1, characterized in that, The thickness of the bottom electrode is 100~300nm; The thickness of the niobium oxide transformation layer is 1~300 nm; The thickness of the top electrode is 10~200nm.

4. The niobium oxide threshold device as described in claim 1, characterized in that, The top electrodes are arranged in an array on the surface of the niobium oxide transformation layer; The top electrode has a circular or rectangular cross-section, with the radius of the circle being 0.05~0.5mm and the side length of the rectangle being 0.1~1mm.

5. The niobium oxide threshold device as described in claim 1, characterized in that, The substrate includes any one of the following: Si substrate, Si / SiO2 substrate, Si / SiO2 / Ti substrate, c-plane sapphire substrate, magnesium oxide substrate, gallium oxide substrate, gallium nitride substrate, NSTO substrate, quartz glass substrate, r-plane sapphire substrate, and a-plane sapphire substrate.

6. A method for fabricating a niobium oxide threshold device as described in any one of claims 1 to 5, characterized in that, Includes the following steps: Fabricate the bottom electrode on the substrate; A niobium oxide conversion layer is prepared on the surface of the bottom electrode; A top electrode was fabricated on the surface of the niobium oxide transformation layer; The method for preparing the niobium oxide transformation layer is as follows: Using Nb2O5 as the target material, a niobium oxide transformation layer was prepared on the surface of the bottom electrode by pulsed laser deposition. The vacuum degree in the chamber during deposition was 0.14~0.3 Pa.

7. The method for fabricating the niobium oxide threshold device as described in claim 6, characterized in that, When a niobium oxide transformation layer is prepared on the surface of the bottom electrode using pulsed laser deposition, the deposition temperature is 400~500℃ and the pulsed laser energy is 350~400mJ.

8. The method for fabricating the niobium oxide threshold device as described in claim 6, characterized in that, The method for preparing the top electrode is as follows: Using the material corresponding to the top electrode as the target material, the top electrode was prepared on the surface of the niobium oxide transformation layer by pulsed laser deposition. The deposition temperature is 20~25℃, and the pulsed laser energy is 300~400 mJ.

9. The method for fabricating the niobium oxide threshold device as described in claim 6, characterized in that, Fabricating the bottom electrode on the substrate specifically includes: The bottom electrode was fabricated on a substrate using pulsed laser deposition with the material corresponding to the bottom electrode as the target material. The deposition temperature is 20~25℃, and the pulsed laser energy is 300~400 mJ.