A method for fabricating a semiconductor device and the semiconductor device.

By defining a high-resistivity region and reducing the height difference before etching, damage to the high-resistivity layer is avoided, thus solving the damage problem during the etching of contact holes and improving the performance and stability of semiconductor devices.

CN123124677APending Publication Date: 2026-11-17CHENGDU ZIGUANG SEMICON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510638712.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

High-resistivity devices are susceptible to damage during the etching of contact holes, affecting the quality and performance of semiconductor devices.

Method used

First, the high-resistivity region in the first interlayer dielectric layer is etched out to form a high-resistivity layer. Then, the unwanted parts are removed to reduce the height difference between the high-resistivity layer and other devices. Contact holes are formed by chemical mechanical polishing to avoid damaging the high-resistivity layer.

Benefits of technology

This improves the quality of the high-resistivity layer, enhances the performance and stability of semiconductor devices, and expands the operating window for contact hole etching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124677A_ABST
    Figure CN123124677A_ABST
Patent Text Reader

Abstract

This invention relates to a method for fabricating a semiconductor device and the semiconductor device itself. The method includes the following steps: providing a semiconductor substrate, the semiconductor substrate including an active region, and forming a first interlayer dielectric layer on the semiconductor substrate; photolithographically etching a high-resistivity region of the first interlayer dielectric layer until the upper surface of the semiconductor substrate in the high-resistivity region is exposed, forming an opening; depositing a high-resistivity layer, and depositing a second interlayer dielectric layer on the high-resistivity layer such that the second interlayer dielectric layer fills the opening; removing the second interlayer dielectric layer and the high-resistivity layer outside the high-resistivity region; sequentially depositing a third interlayer dielectric layer, an amorphous carbon layer, and a nitrogen-free dielectric anti-reflective layer; and forming desired contact holes in the high-resistivity region and non-high-resistivity region, respectively. The method provided by this invention reduces the height difference between the high-resistivity layer and other devices, obtaining a wider etching process window.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductors, specifically relating to a method for preparing a semiconductor device and the semiconductor device itself. Background Technology

[0002] During the fabrication of semiconductor devices, the active regions of transistors (including the source, drain, and gate) are filled with conductive material through contact holes to form metal plugs and form electrical connections with the metal layer.

[0003] High-resistivity devices are commonly used in circuits for voltage division and current limiting, and TiN is generally used as the high-resistivity structure. Because TiN is thickness-sensitive, its thickness is usually thin to obtain high-resistivity devices. In existing technologies, high-resistivity devices are typically fabricated by first etching the interlayer dielectric layer, and then contact holes are simultaneously etched in both the active region and the high-resistivity device region. However, the etching process of the contact holes can easily damage the high-resistivity device. Summary of the Invention

[0004] The purpose of this invention is to reduce damage to high-resistance structures when opening contact holes.

[0005] To achieve the above objectives, the present invention provides a method for fabricating a semiconductor device, the method comprising the following steps: A semiconductor substrate is provided, the semiconductor substrate including an active region, and a first interlayer dielectric layer is formed on the semiconductor substrate; Etch the high-resistivity region of the first interlayer dielectric layer until the upper surface of the semiconductor substrate in the high-resistivity region is exposed, forming an opening; A high-resistivity layer is deposited to form a high-resistivity layer, and a second interlayer dielectric layer is deposited on the high-resistivity layer such that the second interlayer dielectric layer fills the opening; Remove the second interlayer dielectric layer and the high-resistivity layer outside the high-resistivity region; The third interlayer dielectric layer, the amorphous carbon layer, and the nitrogen-free dielectric antireflective layer are deposited sequentially. The required contact holes are formed in the high-resistance region and the non-high-resistance region respectively.

[0006] Optionally, the high-resistivity layer is made of TiN; the thickness of the high-resistivity layer is 46-50 Å.

[0007] Optionally, the second interlayer dielectric layer and the high-resistivity layer outside the high-resistivity region are removed by chemical mechanical polishing, and a first high-resistivity layer and a vertical second high-resistivity layer located on the semiconductor substrate and located on both sides of the first high-resistivity layer are formed in the high-resistivity region; the length of the first high-resistivity layer is 90-110 nm; and the height of the second high-resistivity layer is 45-55 nm.

[0008] Optionally, the materials of the first interlayer dielectric layer, the second interlayer dielectric layer, and the third interlayer dielectric layer are each TEOS; the thickness of the first interlayer dielectric layer is 45-55 nm.

[0009] Optionally, the method for forming the contact hole includes the following steps: spin-coating photoresist onto the upper surface of the nitrogen-free dielectric antireflective layer, baking and curing it, defining the pattern of the contact hole on the photoresist by exposure and development, and forming the desired contact hole by etching; the method for forming the contact hole is dry etching or wet etching, preferably dry etching; preferably, the conditions for dry etching include: a CF4 flow rate of 95-105 sccm, a source RF power of 650-750 W, and a chamber pressure of 18-22 torr.

[0010] Optionally, the method further includes: after forming the contact hole, removing the amorphous carbon layer and the nitrogen-free dielectric antireflective layer, and filling the contact hole with metal to form a metal plug.

[0011] A second aspect of the present invention provides a semiconductor device comprising a semiconductor substrate, an interlayer dielectric layer on the semiconductor substrate, and a high-resistivity layer located in a high-resistivity region of the interlayer dielectric layer; the semiconductor substrate having an active region, wherein the high-resistivity region is located in the interlayer dielectric layer separately from the active region; The high-resistivity layer includes a first high-resistivity layer in the horizontal direction and a second high-resistivity layer in the vertical direction located on both sides of the first high-resistivity layer, and the first high-resistivity layer is located on the semiconductor substrate; The high-resistivity region of the interlayer dielectric layer is provided with a contact hole, and the contact hole communicates with the upper surface of the first high-resistivity layer.

[0012] Optionally, the length of the first high-resistivity layer is 90-110 nm; and the height of the second high-resistivity layer is 45-55 nm.

[0013] Optionally, the high-resistivity layer is made of TiN; the thickness of the high-resistivity layer is 46-50 Å.

[0014] Optionally, the interlayer dielectric layer includes a TEOS layer located on the semiconductor substrate; preferably, the thickness of the TEOS layer is 950-1050 nm.

[0015] Through the above technical solution, the present invention first etches a high-resistance layer defining the high-resistance region in the first interlayer dielectric layer, and then removes the unwanted parts of the high-resistance layer after forming the high-resistance layer. This reduces the height difference between the high-resistance layer and other devices, obtains a wider process window, avoids damage to the high-resistance layer when opening contact holes, thereby ensuring the quality of the high-resistance layer and improving the performance and stability of semiconductor devices.

[0016] Other features and advantages of the present invention will be described in detail in the following detailed description section. Attached Figure Description

[0017] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used together with the following detailed description to explain the invention, but do not constitute a limitation thereof. In the drawings: Figure 1 This is a schematic diagram of the structure of a semiconductor device obtained by implementing the contact hole process using existing technology.

[0018] Figures 2 to 5 These are schematic diagrams illustrating the semiconductor device formation process in some embodiments of the present invention. Detailed Implementation

[0019] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.

[0020] Fabricating a high-resistivity layer is an essential process in semiconductor manufacturing. Figure 1 This is a schematic diagram of the structure of a semiconductor device obtained by a common fabrication process. The general fabrication method is to form a high-resistivity layer sequentially above the interlayer dielectric layer TEOS layer.

[0021] Contact vias are typically used to connect front-end of line (FEOL) and back-end of line (BEOL) processes to transmit electrical signals generated by transistors to the metal interconnect layer. Tungsten is generally used as the filler material in contact via processes.

[0022] An inter-layer dielectric (ILD) is formed between the transistor device and the first metal using a dielectric material, which achieves electrical isolation while also reducing the parasitic capacitance between the metal and the substrate.

[0023] The semiconductor substrate provided by the present invention includes a substrate and a memory device and / or logic device located on the substrate. Specifically, the semiconductor substrate includes an active region formed by an active region isolation structure, for example, a silicon substrate and a CMOS device located on the silicon substrate, and a layer of phosphosilicate glass (PSG) formed by High Density Plasma Chemical Vapor Deposition (HDPCVD) is formed on the CMOS device to absorb and fix ions and block water vapor.

[0024] Figure 1 A schematic diagram of a semiconductor device obtained by implementing a contact hole process in the prior art is provided. For example... Figure 1 As shown, the semiconductor device includes a semiconductor substrate and an interlayer dielectric layer 201, an amorphous carbon layer 205, and a nitrogen-free dielectric antireflective layer 206 sequentially stacked on the semiconductor substrate. The semiconductor substrate 100 has an active region, and a high-resistance structure is located in the high-resistance region within the interlayer dielectric layer. In the direction from the semiconductor substrate to the amorphous carbon layer, the high-resistance structure includes a TiN layer 202, a SiN layer 203, and a B-OX layer 204 sequentially stacked, and a contact hole 207 is formed in the high-resistance region.

[0025] Existing methods for fabricating high-resistivity devices typically involve forming tetraethyl orthosilicate (TEOS) as an interlayer dielectric layer on a phosphosilicate glass substrate. The height of this dielectric layer is then adjusted using a chemical mechanical polishing (CMP) process, followed by the sequential formation of a TiN layer, a SiN layer, and a B-OX layer on top of the dielectric layer. Subsequently, photoresist is spin-coated, retaining the photoresist in the high-resistivity region, and the TiN, SiN, and B-OX layers outside the high-resistivity region are etched away. After growing the interlayer dielectric layer (using TEOS), contact holes are formed in both the high-resistivity and active regions. After forming the contact holes, an amorphous carbon layer and a nitrogen-free dielectric antireflective layer are removed. However, due to the height difference between the high-resistivity and active regions (typically 400 Å), forming contact holes in the high-resistivity region can easily damage the TiN layer, even when a SiN layer is stacked on top of it, affecting the quality and performance of the semiconductor device and increasing the difficulty of forming the contact holes.

[0026] A first aspect of the present invention provides a method for fabricating a semiconductor device, the method comprising the following steps: A semiconductor substrate is provided, the semiconductor substrate including an active region, and a first interlayer dielectric layer is formed on the semiconductor substrate; Etch the high-resistivity region of the first interlayer dielectric layer until the upper surface of the semiconductor substrate in the high-resistivity region is exposed, forming an opening; A high-resistivity layer is deposited to form a high-resistivity layer, and a second interlayer dielectric layer is deposited on the high-resistivity layer such that the second interlayer dielectric layer covers and fills the opening; Remove the second interlayer dielectric layer and the high-resistivity layer outside the high-resistivity region; The third interlayer dielectric layer, the amorphous carbon layer, and the nitrogen-free dielectric antireflective layer are deposited sequentially. The required contact holes are formed in the high-resistance region and the non-high-resistance region respectively.

[0027] This invention first etches and defines the high-resistance region in the first interlayer dielectric layer, and then removes the unwanted parts of the high-resistance layer after it is formed. This reduces the height difference between the high-resistance layer and other devices, and prevents damage to the high-resistance layer when making contact holes, thereby ensuring the quality of the high-resistance layer and improving the performance and stability of semiconductor devices.

[0028] Figures 2 to 5 These are schematic diagrams illustrating the semiconductor device formation process in some embodiments of the present invention.

[0029] refer to Figure 2 A semiconductor substrate 100 is provided, the semiconductor substrate 100 including an active region. Further, the semiconductor substrate 100 includes a substrate and a device located on the substrate. Specifically, Figure 2 In the schematic diagram shown, the semiconductor substrate includes a silicon substrate, on which a metal gate is formed. A source / drain structure is formed between the metal gates, and the source / drain structure is located in the silicon substrate with a height lower than the metal gate. A first interlayer dielectric layer 310 is formed on the semiconductor substrate 100. The high-resistivity region of the first interlayer dielectric layer 310 is etched until the upper surface of the semiconductor substrate in the high-resistivity region is exposed, forming an opening.

[0030] The material of the first interlayer dielectric layer is TEOS.

[0031] In some embodiments, the thickness of the first interlayer dielectric layer is 45-55 nm.

[0032] The first interlayer dielectric layer of this invention is preferably tetraethyl orthosilicate (TEOS), which can be grown using plasma-enhanced chemical vapor deposition (PECVD). After the first interlayer dielectric layer is formed, its surface is planarized by chemical mechanical polishing (CMP), and its height is adjusted to the desired height. Specifically, the desired height of the first interlayer dielectric layer is obtained by controlling the CMP time.

[0033] Photoresist is spin-coated onto the first interlayer dielectric layer after polishing, and the high-resistivity regions are removed by development to define the high-resistivity regions. The first interlayer dielectric layer is then etched to remove the high-resistivity regions until the upper surface of the semiconductor substrate is exposed. That is, an opening is formed in the high-resistivity region of the first interlayer dielectric layer. The etching method defining the high-resistivity region can be dry etching or wet etching.

[0034] refer to Figure 3 A high-resistivity layer 320 is deposited to form a high-resistivity layer, and a second interlayer dielectric layer 330 is deposited on the high-resistivity layer, such that the second interlayer dielectric layer 330 fills the high-resistivity region. Specifically, a high-resistivity layer 320 is deposited to form a high-resistivity layer 320 on the device surface and the high-resistivity region of the semiconductor substrate, and a second interlayer dielectric layer 330 is formed by depositing on the high-resistivity layer 320, such that the second interlayer dielectric layer fills the opening.

[0035] In some embodiments of the present invention, the material of the high-resistivity layer 320 may be selected from TiN, TaN, TiO2, WN, and WSi. For example, in some preferred embodiments of the present invention, the material of the high-resistivity layer is preferably TiN.

[0036] The thickness of the high-resistivity layer 320 can be 46-50 Å, for example, 46 Å, 47 Å, 48 Å, 49 Å, 50 Å, or any value within the aforementioned range. In some preferred embodiments of the present invention, the high-resistivity layer is made of TiN and has a thickness of 48 Å.

[0037] In some embodiments of the present invention, the high-resistivity TiN layer can be formed by physical vapor deposition or chemical vapor deposition.

[0038] The material of the second interlayer dielectric layer 330 is preferably TEOS. Specifically, the material of the second interlayer dielectric layer 330 can be a TEOS layer grown by LPCVD or PECVD.

[0039] refer to Figure 4 The second interlayer dielectric layer and the high-resistivity layer outside the high-resistivity region are removed. Specifically, the second interlayer dielectric layer and the high-resistivity layer outside the high-resistivity region are removed by a chemical mechanical polishing process, and a first high-resistivity layer 321 and vertical second high-resistivity layers 322 located on both sides of the first high-resistivity layer 321 are formed in the high-resistivity region on the semiconductor substrate.

[0040] In some embodiments of the present invention, the length of the first high-resistivity layer 321 is 90-110 nm, for example, it can be 90 nm, 92 nm, 94 nm, 95 nm, 96 nm, 98 nm, 100 nm, 102 nm, 104 nm, 105 nm, 106 nm, 108 nm, 110 nm, or any value within the aforementioned range. To control the uniformity of the high-resistivity layer film and ensure the reliability of the device, the length of the first high-resistivity layer is preferably 95-105 nm.

[0041] By etching openings for forming a high-resistivity layer in the first interlayer dielectric layer, and then forming the first high-resistivity layer through a planarization process, damage to the first high-resistivity layer can be avoided during chemical mechanical polishing due to the height difference between the first high-resistivity layer and the high-resistivity layer outside the high-resistivity region. In some embodiments of the present invention, the height of the second high-resistivity layer is 45-55 nm, for example, it can be 45 nm, 46 nm, 47 nm, 48 nm, 49 nm, 50 nm, 51 nm, 52 nm, 53 nm, 54 nm, 55 nm, or any value within the aforementioned range. That is, the present invention reduces the height difference between the first high-resistivity layer and the semiconductor substrate, significantly increasing the operating window of the contact hole etching process. To further improve the device performance, the height of the second high-resistivity layer is preferably 47-53 nm.

[0042] refer to Figure 5 The third interlayer dielectric layer 340, the amorphous carbon layer (APF) 350, and the nitrogen-free dielectric antireflective layer 360 are deposited sequentially; then the required contact holes are formed in the high-resistance region and the non-high-resistance region, respectively.

[0043] Specifically, the third interlayer dielectric layer 340 is preferably a TEOS layer formed by PECVD growth. The amorphous carbon layer (APF) 350 and the nitrogen-free dielectric antireflective layer (NFDARC) can be formed by subatmospheric chemical vapor deposition (SACVD).

[0044] In some embodiments of the present invention, the method of forming the contact hole includes the following steps: Photoresist is spin-coated onto the upper surface of the nitrogen-free dielectric antireflective layer. After baking and curing, the pattern of contact holes is defined on the photoresist by exposure and development, and the required contact holes are formed by etching.

[0045] In some embodiments of the present invention, the method for forming the contact hole can be dry etching or wet etching. In some specific embodiments, dry etching is used to form the contact hole, for example, by using plasma formed from fluorine-containing gases such as CHF3 or CF4 to bombard and remove the dielectric layer in areas without photoresist coverage, forming a contact hole with a high aspect ratio. The bottom width of the contact hole in the vertical cross-section is smaller than the top width of the contact hole, and the bottom width of the contact hole is the designed width.

[0046] In some specific embodiments of the present invention, the conditions for dry etching include: a CF4 flow rate of 95-105 sccm, a source RF power of 650-750 W, and a chamber pressure of 18-22 torr.

[0047] like Figure 5 As shown, the contact hole 371 formed in the high-resistivity region extends to the upper surface of the first high-resistivity layer 321. The contact holes formed in the non-high-resistivity region include a contact hole 372 extending to the upper surface of the metal gate and a contact hole 373 extending to the upper surface of the source / drain structure. When the contact holes are formed, a larger operating window is provided for forming the contact holes because the height difference between the high-resistivity region and the non-high-resistivity region (including the metal gate and the source / drain structure) is reduced.

[0048] In some embodiments of the present invention, the method further includes: after forming the contact hole, removing the amorphous carbon layer and the nitrogen-free dielectric antireflective layer, and filling the contact hole with metal to form a metal plug. The amorphous carbon layer and the nitrogen-free dielectric antireflective layer can be removed using methods known in the art after forming the contact hole or during the formation of the metal plug.

[0049] A second aspect of the present invention provides a semiconductor device, such as Figure 5 The semiconductor device shown includes a semiconductor substrate 100, an interlayer dielectric layer on the semiconductor substrate 100, and a high-resistance layer located in a high-resistance region of the interlayer dielectric layer; the semiconductor substrate 100 has an active region, and the high-resistance region is located in the interlayer dielectric layer differently from the active region; The high-resistivity layer includes a first high-resistivity layer 321 in the horizontal direction and a second high-resistivity layer 322 in the vertical direction located on both sides of the first high-resistivity layer 321, and the first high-resistivity layer 321 is located on the semiconductor substrate 100; a contact hole 371 is provided in the high-resistivity region of the interlayer dielectric layer, and the contact hole 371 communicates with the first high-resistivity layer 321.

[0050] The length of the first high-resistivity layer 321 can be 90-110 nm; the height of the second high-resistivity layer 322 can be 45-55 nm. Preferably, the length of the first high-resistivity layer 321 can be 95-105 nm; and the height of the second high-resistivity layer 322 can be 47-53 nm.

[0051] The high-resistivity layer can be made of TiN; the thickness of the high-resistivity layer is 46-50 Å. The TiN high-resistivity layer has a suitable thickness to ensure the stability of the device's resistance value.

[0052] Among them, such as Figure 5 As shown, the interlayer dielectric layer includes a TEOS layer located on the semiconductor substrate. The amorphous carbon layer 350 and the nitrogen-free dielectric antireflective layer 360 are removed after the contact holes are formed or in subsequent processes.

[0053] In some embodiments of the present invention, the thickness of the TEOS layer can be 950-1050 nm.

[0054] Understandably, the above methods also include processes such as annealing to improve device performance and stability.

[0055] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.

[0056] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.

[0057] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.

Claims

1. A method for fabricating a semiconductor device, characterized in that, The method includes the following steps: A semiconductor substrate is provided, the semiconductor substrate including an active region, and a first interlayer dielectric layer is formed on the semiconductor substrate; Photolithography and etching are performed on the high-resistivity region of the first interlayer dielectric layer until the upper surface of the semiconductor substrate in the high-resistivity region is exposed, forming an opening; A high-resistivity layer is deposited to form a high-resistivity layer, and a second interlayer dielectric layer is deposited on the high-resistivity layer such that the second interlayer dielectric layer fills the opening; Remove the second interlayer dielectric layer and the high-resistivity layer outside the high-resistivity region; The third interlayer dielectric layer, the amorphous carbon layer, and the nitrogen-free dielectric antireflective layer are deposited sequentially. The required contact holes are formed in the high-resistance region and the non-high-resistance region respectively.

2. The method according to claim 1, wherein, The high-resistivity layer is made of TiN; The thickness of the high-resistivity layer is 46-50 Å.

3. The method according to claim 1, wherein, The second interlayer dielectric layer and the high-resistivity layer outside the high-resistivity region are removed by chemical mechanical polishing process, and a first high-resistivity layer and a vertical second high-resistivity layer located on the semiconductor substrate are formed in the high-resistivity region. The length of the first high-resistivity layer is 90-110 nm; The height of the second high-resistivity layer is 45-55 nm.

4. The method according to claim 1, wherein, The materials of the first interlayer dielectric layer, the second interlayer dielectric layer, and the third interlayer dielectric layer are all TEOS; The thickness of the first interlayer dielectric layer is 45-55 nm.

5. The method according to claim 1, wherein, The method for forming the contact hole includes the following steps: Photoresist is spin-coated onto the upper surface of the nitrogen-free dielectric antireflective layer. After baking and curing, the pattern of contact holes is defined on the photoresist by exposure and development, and the required contact holes are formed by etching. The method for forming the contact hole is dry etching or wet etching, preferably dry etching; Preferably, the dry etching conditions include: a CF4 flow rate of 95-105 sccm, a source RF power of 650-750W, and a chamber pressure of 18-22 torr.

6. The method according to claim 1, wherein, The method further includes: after forming the contact hole, removing the amorphous carbon layer and the nitrogen-free dielectric antireflective layer, and filling the contact hole with metal to form a metal plug.

7. A semiconductor device, characterized in that, The semiconductor device includes a semiconductor substrate, an interlayer dielectric layer on the semiconductor substrate, and a high-resistivity layer located in a high-resistivity region of the interlayer dielectric layer; the semiconductor substrate has an active region, and the high-resistivity region is located in the interlayer dielectric layer differently from the active region; The high-resistivity layer includes a first high-resistivity layer in the horizontal direction and a second high-resistivity layer in the vertical direction located on both sides of the first high-resistivity layer, and the first high-resistivity layer is located on the semiconductor substrate; The high-resistivity region of the interlayer dielectric layer is provided with a contact hole, and the contact hole communicates with the upper surface of the first high-resistivity layer.

8. The semiconductor device according to claim 7, wherein, The length of the first high-resistivity layer is 90-110 nm; The height of the second high-resistivity layer is 45-55 nm.

9. The semiconductor device according to claim 7 or 8, wherein, The high-resistivity layer is made of TiN; The thickness of the high-resistivity layer is 46-50 Å.

10. The semiconductor device according to claim 7, wherein, The interlayer dielectric layer includes a TEOS layer located on the semiconductor substrate; Preferably, the thickness of the TEOS layer is 950-1050 nm.