A method for fabricating a semiconductor structure
By forming a low-resistivity surface on the first side of the substrate and channeling the charge during the etching process, the problem of arc discharge breaking down the insulating film layer in high-power plasma etching processes is solved, and a more reliable etching process is achieved.
Patent Information
- Application Number
- CN202610703654.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-20
- Publication Date
- 2026-11-17
AI Technical Summary
In high-power plasma etching, plasma charges accumulate on the insulating film layer, resulting in a strong potential difference between the insulating film layer and the covering metal layer, which easily leads to arc discharge and subsequent breakdown of the insulating film layer.
A low-resistivity surface electrically connected to the active substrate is formed on the first side of the substrate. A portion of the insulating layer is removed by an anisotropic etching process to expose the conductor layer. During the etching process, the charge is guided to the active substrate to avoid the formation of a potential difference.
This effectively reduces the potential difference between the insulating layer and the conductor layer, avoids arc discharge and breakdown of the insulating layer, and improves the reliability of the etching process.
Smart Images

Figure CN123124678A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor technology, and more specifically to a method for fabricating a semiconductor structure. Background Technology
[0002] 3D technology has provided new solutions for the post-Moore's Law era of semiconductors. With the accumulation of 3D vertical device stacking layers, High Power Plasma (HPP) technology, characterized by high selectivity deep hole etching and deep hole filling capabilities, has been introduced.
[0003] HPP etching can achieve high selectivity etching. However, during HPP etching, plasma charges tend to accumulate on the insulating film layer, forming a strong potential difference with the metal layer wrapped by the insulating film layer. This can easily lead to arcing, causing the insulating film layer to break down.
[0004] Therefore, improvements are needed to at least partially address the aforementioned problems. Summary of the Invention
[0005] The summary section introduces a series of simplified concepts, which will be further explained in detail in the detailed description section. The summary section of this invention is not intended to limit the key features and essential technical features of the claimed technical solution, nor is it intended to determine the scope of protection of the claimed technical solution.
[0006] To at least partially solve the above problems, according to a first aspect of the present invention, a method for fabricating a semiconductor structure is provided, comprising: A substrate is provided, the substrate including an interconnect layer on a first side and an active substrate on a second side, the interconnect layer including an insulating layer and a conductor layer covered by the insulating layer, at least a portion of the conductor layer being electrically connected to the active substrate; A low-resistivity surface electrically connected to the active substrate is formed on the first side of the substrate, wherein the conductivity of the low-resistivity surface is greater than or equal to the conductivity of the active substrate. An anisotropic etching process is performed from the first side to remove a portion of the insulating layer, exposing the conductor layer.
[0007] For example, the active substrate includes a wafer, and the low-resistivity surface is formed in a region of the substrate corresponding to the edge of the wafer.
[0008] For example, an active device is formed in the active substrate, and the conductor layer includes at least a first conductive layer and a second conductive layer. The first conductive layer is located between the second conductive layer and the active substrate, and the first conductive layer is electrically connected to the active device. The substrate includes a first region, a second region, and a third region, which are arranged along the center to edge direction of the wafer. The first region and the second region each have the conductor layer. In the first region, the first conductive layer and the second conductive layer are electrically connected. In the second region, the first conductive layer and the second conductive layer are mutually insulated. The third region includes the crystal edge and the insulating layer located on a first side of the crystal edge. The exposure of the conductor layer includes: exposing the surface of the first side of the second conductive layer.
[0009] For example, before forming a low-resistivity surface electrically connected to the active substrate on the first side of the substrate, the fabrication method further includes: The substrate is trimmed until the first side exposes the active substrate, wherein the trimming width is 0.3mm-1.2mm.
[0010] For example, the trimming process includes at least one of dry etching, wet chemical etching, laser trimming, mechanical polishing, and chemical mechanical polishing.
[0011] For example, the active substrate includes a doped region and an epitaxial layer, the epitaxial layer being located between the doped region and the interconnect layer, and the conductivity of the epitaxial layer being lower than the conductivity of the doped region; Wherein, the first side of the substrate after the trimming process exposes the doped region, and the low-resistivity surface includes the surface of the doped region exposed by the trimming process.
[0012] For example, forming a low-resistivity surface electrically connected to the active substrate on the first side of the substrate includes: Ion implantation is performed on the first side of the active substrate exposed after trimming to form a doped region in the trimmed area; The doping type of the doped region is not opposite to that of the active substrate, and the doping concentration of the doped region is not lower than that of the active substrate.
[0013] For example, the ion implantation of the active substrate exposed after trimming includes: A photoresist layer is spin-coated onto the first side of the trimmed substrate; The photoresist layer is subjected to edge washing to at least partially expose the active substrate exposed after edge trimming. Ion implantation is performed on the active substrate using the photoresist layer as a mask.
[0014] For example, when performing edge washing on the photoresist layer, the edge washing width is 0.3mm-1.2mm.
[0015] For example, the anisotropic etching process performed from the first side to remove a portion of the insulating layer includes: After ion implantation, the photoresist layer is patterned; Using the patterned photoresist layer as a mask, the anisotropic etching process is performed from the first side to remove a portion of the insulating layer.
[0016] For example, forming a low-resistivity surface electrically connected to the active substrate on the first side of the substrate includes: A doped semiconductor layer is grown on the first side surface of the active substrate exposed after trimming. The doped semiconductor layer is in contact with the active substrate to form an electrical connection. The conductivity type of the doped semiconductor layer is not opposite to that of the active substrate, and the conductivity of the doped semiconductor layer is not lower than that of the active substrate.
[0017] According to the semiconductor structure fabrication method of the present invention, by forming a low-resistivity surface electrically connected to the active substrate on the first side of the substrate, the charge acting on the edge of the substrate during anisotropic etching can be guided to the active substrate, thereby charging the active substrate and the conductor layer electrically connected to the active substrate. This effectively reduces the potential difference between the insulating layer and the conductor layer covered by the insulating layer, avoiding arc discharge and preventing the insulating layer from being broken down. Attached Figure Description
[0018] The following figures are included as part of this application for understanding the application. The figures illustrate embodiments of the application and their descriptions, serving to explain the apparatus and principles of the application. In the figures, Figure 1 This is a schematic flowchart of a method for fabricating a semiconductor structure according to an embodiment of this application; Figures 2A-2E This is a cross-sectional schematic diagram of the structure corresponding to each step of the semiconductor structure fabrication method according to an embodiment of this application; Figure 3 This is a cross-sectional schematic diagram of a portion of the steps in a method for fabricating a semiconductor structure according to another embodiment of this application; Figure 4 This is a cross-sectional schematic diagram of a portion of the steps in a method for fabricating a semiconductor structure according to another embodiment of this application.
[0019] Explanation of reference numerals in the attached figures: 100 - Substrate, 101 - First region, 102 - Second region, 103 - Third region, 110 - Insulating layer, 111 - Silicon oxide layer, 112 - Silicon nitride layer, 120 - Conductor layer, 121 - First conductive layer, 122 - Second conductive layer, 130 - Active substrate, 1301 - Doped region, 1302 - Epitaxial layer, 131 - Wafer, 132 - Active device; 200 - Photoresist layer; 300-doped region; 400-doped semiconductor layer; a - Low-resistivity surface, d - Trimming width. Detailed Implementation
[0020] The following description provides numerous specific details to offer a more thorough understanding of this application. However, it will be apparent to those skilled in the art that this application can be practiced without one or more of these details. In other instances, certain technical features well-known in the art have not been described to avoid confusion with this application.
[0021] It should be understood that this application can be implemented in various forms and should not be construed as limited to the embodiments set forth herein. Rather, providing these embodiments will make the disclosure thorough and complete, and will fully convey the scope of this application to those skilled in the art. In the drawings, for clarity, the dimensions and relative dimensions of layers and regions may be exaggerated. The same reference numerals denote the same elements throughout.
[0022] It should be understood that although the terms first, second, third, etc., may be used to describe various elements, components, areas, layers, and / or parts, these elements, components, areas, layers, and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, area, layer, or part from another element, component, area, layer, or part. Therefore, without departing from the teachings of this application, the first element, component, area, layer, or part discussed below may be referred to as the second element, component, area, layer, or part.
[0023] Spatial relation terms such as "below," "under," "below," "under," "above," and "above" are used here for convenience to describe the relationship between one element or feature shown in the figure and other elements or features. It should be understood that, in addition to the orientation shown in the figure, spatial relation terms are intended to also include different orientations of devices in use and operation.
[0024] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of this application. When used herein, the singular forms “a,” “an,” and “the” are also intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the terms “comprising” and / or “including,” when used in this specification, identify the presence of the stated features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups. When used herein, the term “and / or” includes any and all combinations of the associated listed items.
[0025] Embodiments of the invention are described herein with reference to cross-sectional views that serve as schematic diagrams of preferred embodiments (and intermediate structures) of this application. Thus, variations in the shown shape are contemplated due to, for example, manufacturing techniques and / or tolerances. Therefore, embodiments of this application should not be limited to the specific shapes shown herein, but include shape deviations due to, for example, manufacturing processes. Consequently, the figures are substantially schematic, and their shapes are not intended to show the actual shape of the device and are not intended to limit the scope of this application.
[0026] See attached document Figure 1 An exemplary method for fabricating a semiconductor structure according to an embodiment of this application will be described, the method comprising the following steps: S10: Provide a substrate, the substrate including an interconnect layer on a first side and an active substrate on a second side, the interconnect layer including an insulating layer and a conductor layer covered by the insulating layer, at least a portion of the conductor layer being electrically connected to the active substrate.
[0027] S20: A low-resistivity surface electrically connected to the active substrate is formed on the first side of the substrate, wherein the conductivity of the low-resistivity surface is greater than or equal to the conductivity of the active substrate.
[0028] S30: Perform an anisotropic etching process from the first side to remove a portion of the insulating layer and expose the conductor layer.
[0029] Anisotropic etching processes include plasma-assisted etching (PAL) processes. During PAL processes, a large amount of charge adheres to the surface of the insulating layer. According to the semiconductor structure fabrication method of this application, by forming a low-resistivity surface electrically connected to the active substrate on the first side of the substrate, the charge acting on the substrate edge during anisotropic etching can be guided to the active substrate, charging the active substrate and the conductor layer electrically connected to the active substrate. This effectively reduces the potential difference between the surface of the insulating layer and the conductor layer covered by the insulating layer, preventing arc discharge and thus avoiding insulation layer breakdown. When the conductor layer includes multiple conductive layers, the semiconductor structure fabrication method of this application can also prevent the insulation layer between conductive layers from breaking down during the PAL process.
[0030] The following is a reference to the appendix. Figures 2A-2E A method for fabricating a semiconductor structure according to an embodiment of this application (i.e., steps S10-S30 described above) will be described in detail.
[0031] In step S10, see Appendix Figure 2A A substrate 100 is provided, the substrate 100 including components located on the first side ( Figure 2A The interconnect layer on the upper side and the interconnect layer on the second side (in the middle) Figure 2A The active substrate 130 is located on the lower side of the active substrate 130. The interconnect layer includes an insulating layer 110 and a conductor layer 120 covered by the insulating layer 110, at least a portion of which is electrically connected to the active substrate 130. Exemplarily, in this embodiment, the insulating layer 110 includes alternating layers of silicon oxide 111 and silicon nitride 112.
[0032] In one example, the active substrate 130 refers to a semiconductor substrate in which an active device 132 (such as a transistor, diode, etc.) is integrated, that is, an active device 132 is formed in the active substrate 130. In this embodiment, the active substrate 130 includes a wafer 131, which is the main body of the active substrate 130. The wafer 131 may be, for example, a silicon wafer or a wafer made of other suitable materials that is not insulating.
[0033] In one example, the conductor layer 120 may include a first conductive layer 121 and a second conductive layer 122. The first conductive layer 121 is located between the second conductive layer 122 and the active substrate 130, and is electrically connected to the active device 132. An insulating layer 110 is provided between the first conductive layer 121 and the second conductive layer 122, and between the first conductive layer 121 and the active substrate 130. The first conductive layer 121 and the second conductive layer 122 are patterned conductive layers, which may be metal layers or other suitable conductive material layers. For example, the first conductive layer 121 is electrically connected to the active device 132 through a conductive via. For example, the first conductive layer 121 or the second conductive layer 122 is used to form conductive wiring, conductive vias, or pads; this application does not specifically limit the application to these methods.
[0034] In one example, substrate 100 includes a first region 101, a second region 102, and a third region 103, which are located along the center-to-edge direction of wafer 131 (i.e., Figure 2AArranged from left to right. Both the first region 101 and the second region 102 have a conductor layer 120. In the first region 101, the first conductive layer 121 and the second conductive layer 122 are electrically connected, for example, through a conductive via. The first conductive layer 121 is electrically connected to the active device 132. In the second region 102, the first conductive layer 121 and the second conductive layer 122 are insulated from each other, separated by an insulating layer 110. The second conductive layer is a floating conductive layer. The first conductive layer 121 is electrically connected to the active device 132. The second conductive layers 122 in the first region 101 and the second region 102 are insulated from each other. The third region 103 includes a crystal edge and an insulating layer 110 located on a first side of the crystal edge. For the substrate 100 in this embodiment, if a large amount of plasma charge accumulates on the surface of the insulating layer 110, and the substrate 100 is wrapped by the insulating layer 110 and has a floating potential, on the one hand, the insulating layer 110 will have a large potential difference with the substrate, thereby forming a strong potential difference with the conductor layer 120 that is close to the surface of the insulating layer 110 and electrically connected to the substrate, which will cause the insulating layer 110 to be at risk of being broken down by an electric arc; on the other hand, as etching proceeds, the insulating layer 110 on the first side of the second conductive layer 122 is completely removed or its thickness is reduced to a certain extent, and the plasma charge will enter the second conductive layer 122 to make the second conductive layer 122 charged. The charged second conductive layer 122 in the second region 102 forms a strong potential difference with the first conductive layer 121 that is at a floating potential, which will cause the insulating layer 110 between the first conductive layer 121 and the second conductive layer 122 in the second region 102 to be at risk of breakdown.
[0035] In step S20, a low-resistivity surface a, electrically connected to the active substrate 130, is formed on the first side of the substrate 100. The conductivity of the low-resistivity surface a is greater than or equal to the conductivity of the active substrate 130. The low-resistivity surface a can be horizontal, inclined, or vertical relative to the first side surface of the substrate 100; this application does not specifically limit this. It should be noted that the conductivity of the low-resistivity surface a refers to the conductivity of the bulk material to which the low-resistivity surface a belongs.
[0036] In one example, before forming a low-resistivity surface a electrically connected to the active substrate 130 on the first side of the substrate 100, see Appendix Figure 2B The substrate 100 is trimmed until the active substrate 130 is exposed on the first side, wherein the trimming width d is 0.3mm-1.2mm. The trimming process forms a stepped structure at the edge of the first side of the substrate 100, with the active substrate 130 exposed at the bottom of the step. The trimming width d is along the direction from the center to the edge of the wafer 131 (i.e.,...). Figure 2B On the inner edge of the step (from left to right) Figure 2B The left edge of the middle section) and the outermost edge of wafer 131 (i.e. Figure 2B The distance between the right edge and the edge. Exposing the active substrate through trimming allows for better connection of the low-resistivity surface a and ensures that the low-resistivity surface a has sufficient area. For example, the bottom surface of the step formed by the trimming is lower than the upper surface of the active substrate 130, and in the thickness direction of the active substrate 130 (i.e.,...) Figure 2B The distance between the active substrate 130 and the upper surface of the active substrate 130 in the vertical direction is greater than or equal to 5 μm, so that the active substrate 130 can be better exposed.
[0037] Edge trimming is a critical process in semiconductor manufacturing for shaping, defect removal, and performance optimization of the wafer edge / bevel. Exemplarily, edge trimming may include at least one of dry etching, wet chemical etching, laser trimming, mechanical grinding, and chemical mechanical polishing. Exemplarily, edge trimming is performed only in the third region 103.
[0038] In one example, after trimming the base 100, see the appendix. Figure 2C , Figure 2D A low-resistivity surface a is formed on the trimmed area of the first side of the substrate 100, which is electrically connected to the active substrate 130.
[0039] In one example, the low-resistivity surface a comprises the surface of the active substrate 130 that has been trimmed and exposed. Accordingly, the active substrate 130 comprises a doped or undoped single-crystal silicon wafer, and the conductivity of the low-resistivity surface a is the same as that of the active substrate 130.
[0040] In one example, forming the low-resistivity surface a further includes ion implantation on a first side of the active substrate 130 exposed after trimming, to form a doped region 300 in the trimmed area. The low-resistivity surface a is the surface of the doped region 300, which has low resistance and high conductivity. The doping type of the doped region 300 is not opposite to the doping type of the active substrate 130. For example, when the active substrate 130 is a doped substrate (e.g., N-type or P-type doped single-crystal silicon), the doping type of the doped region 300 is the same as that of the active substrate 130. When the active substrate 130 is an undoped substrate (e.g., undoped single-crystal silicon), the doping type of the doped region 300 can be N-type or P-type, but is not limited thereto, as long as ion implantation can increase the conductivity of the doped region 300 to a level not lower than that of the active substrate, and the doped region 300 does not form a conductive barrier with the active substrate (e.g., forming a reverse-biased junction on the charging path from the conductive surface to the active substrate). The doping concentration of the doped region 300 is not lower than the doping concentration of the active substrate 130. That is, when the active substrate 130 includes a doped body region 1301 and an epitaxial layer 1302 located on the doped body region 1301 (the doping concentration of the epitaxial layer 1302 is lower than the doping concentration of the doped body region 1301), the doping concentration of the doped region 300 is greater than or equal to the doping concentration of the doped body region 1301, and the doped region 300 is electrically connected to the doped body region 1301. When the active substrate 130 is undoped single-crystal silicon (or other suitable substrate material) or lightly doped single-crystal silicon (or other suitable substrate material), the doping concentration of the doped region 300 is greater than the doping concentration of the active substrate 130. Therefore, the conductivity of the low-resistivity surface a (i.e., the surface of the doped region 300) is greater than or equal to the conductivity of the active substrate 130. In this embodiment, since a low-resistivity surface a is formed in the trimmed area, and the doped region 300 is formed at the edge of the wafer 131, that is, the low-resistivity surface a is formed in the region of the substrate 100 corresponding to the edge of the wafer 131. Thus, the idle space of the edge can be effectively utilized without occupying the effective area of the wafer 131.
[0041] Specifically, first, see the appendix. Figure 2CA photoresist layer 200 is spin-coated onto the first side of the trimmed substrate 100, covering the first side surface of the substrate 100. Then, the photoresist layer 200 is subjected to an edge-washing process to at least partially expose the active substrate 130 exposed after the edge-washing process. This edge-washing process is also known as EBR (Edge Bead Removal). Exemplarily, the edge-washing process can be solvent wet edge-washing, plasma dry edge-washing, or laser edge-washing. Generally, the edge-washing process can remove photoresist from a certain annular area at the edge of the substrate 100, and the range of the edge-washing process is usually preset by the process equipment performing the edge-washing process. For example, when performing edge washing on the photoresist layer 200, the edge washing width can be 0.3mm-1.2mm. It should be noted that the edge washing width mentioned here refers to the edge washing range preset by the process equipment performing the edge washing process. The edge washing range can be a range of 0.3mm-1.2mm from the edge of the wafer 131 towards the center of the wafer 131, so as to effectively expose the active substrate 130 exposed after the edge trimming process.
[0042] Then, see appendix. Figure 2D Ion implantation is performed on the active substrate 130 using the photoresist layer 200 as a mask to form a doped region 300. Exemplarily, ion implantation can be performed using a High Current Implantation (HCI) ion implantation process to form the doped region 300. The interconnect layer is blocked by the photoresist layer 200 and therefore will not be implanted with ions. Exemplarily, ion implantation can be P-type implantation (preferably with B, Ge, or In), with an implantation dose greater than or equal to 10⁻⁶. 20 cm -3 The implantation energy is less than 5 keV. By implanting a large dose of low-energy ions, a highly conductive doped region 300 can be formed on the surface of the active substrate 130.
[0043] In step S30, see Appendix Figure 2E An anisotropic etching process is performed from the first side to remove a portion of the insulating layer 110, exposing the conductor layer 120.
[0044] Specifically, after ion implantation, the photoresist layer 200 is first patterned. That is, the photoresist layer 200 is subjected to photolithography steps such as exposure and development to pattern the photoresist layer 200.
[0045] Then, using the patterned photoresist layer 200 as a mask, an anisotropic etching process is performed from the first side to remove a portion of the insulating layer 110, exposing the conductor layer 120. Exemplarily, this anisotropic etching process can be an HPP etching process or other similar dry etching processes that generate a large amount of plasma charge. Exemplarily, in this embodiment, an anisotropic etching process is performed from the first side to remove a portion of the insulating layer 110, exposing the surface of the second conductive layer 122 on the first side to achieve electrical lead-out of the second conductive layer 122. For example, the second conductive layer 122 includes pads or conductive wiring, or the second conductive layer 122 includes conductive vias, or the second conductive layer 122 includes pads or conductive wiring, and conductive vias located on the side of the pads or conductive wiring away from the active substrate. The recesses formed by the patterned etching of the insulating layer 110 expose the conductor layer 120. For example, conductive material can be filled into the recesses to form electrical lead-out of the conductor layer 120.
[0046] However, it is not limited to this. After ion implantation, the photoresist layer 200 can be removed, and an anisotropic etching process can be performed on the entire surface to expose the conductor layer 120. The specific settings can be configured according to actual needs.
[0047] According to the semiconductor structure fabrication method of the application embodiment, by forming a low-resistivity surface a (similar to a lightning rod) electrically connected to the active substrate 130 on the first side of the substrate 100, the charge acting on the edge of the substrate 100 during dry etching can be guided to the active substrate 130, charging the active substrate and the conductor layer 120 electrically connected to the active substrate. On the one hand, this avoids the formation of a strong potential difference between the surface of the insulating layer 110 and the conductor layer 120 near the surface of the insulating layer 110, thus avoiding arc discharge and breakdown of the insulating layer 110. On the other hand, it avoids the formation of a strong potential difference between the first conductive layer 121 and the second conductive layer 122 in the second region 102, thus avoiding breakdown of the insulating layer 110 between the first conductive layer 121 and the second conductive layer 122.
[0048] In another embodiment of this application, the method for fabricating the semiconductor structure includes steps S10-S30 as described above. Step S10 is the same as in the above embodiment (see above and appendix). Figure 2A (This will not be repeated here.)
[0049] In step S20, the substrate 100 is first trimmed until the active substrate 130 is exposed on the first side, wherein the trimming width d is 0.3mm-1.2mm. The specific process is the same as in the above embodiment (see above and appendix). Figure 2B (This will not be repeated here.)
[0050] Then, see appendix. Figure 3A doped semiconductor layer 400 is grown on the first side surface of the active substrate 130 exposed after trimming. The low-resistivity surface a is the surface of the doped semiconductor layer 400, which has low resistance and high conductivity. The doped semiconductor layer 400 contacts the active substrate 130 to form an electrical connection. The conductivity type of the doped semiconductor layer 400 is not opposite to that of the active substrate 130; that is, when the active substrate 130 is a doped substrate (e.g., N-type or P-type doped single-crystal silicon), the doping type of the doped semiconductor layer 400 is the same as that of the active substrate 130; when the active substrate 130 is an undoped substrate (e.g., undoped single-crystal silicon), the doping type of the doped semiconductor layer 400 can be either N-type or P-type. The conductivity of the doped semiconductor layer 400 is not lower than that of the active substrate 130. That is, when the active substrate 130 includes a doped region 1301 and an epitaxial layer 1302 located on the doped region 1301 (the doping concentration of the epitaxial layer 1302 is lower than the doping concentration of the doped region 1301), the doping concentration of the doped semiconductor layer 400 is greater than or equal to the doping concentration of the doped region 1301. When the active substrate 130 is undoped single-crystal silicon (or other suitable substrate material) or lightly doped single-crystal silicon (or other suitable substrate material), the doping concentration of the doped semiconductor layer 400 is greater than that of the active substrate 130. Therefore, the conductivity of the low-resistivity surface a (i.e., the surface of the doped semiconductor layer 400) is greater than or equal to the conductivity of the active substrate 130. In this embodiment, the edge of wafer 131 is exposed by trimming, and a doped semiconductor layer 400 is formed on the edge of wafer 131. That is, a low-resistivity surface a is formed on the region of substrate 100 corresponding to the edge of wafer 131. Thus, the unused space of the edge can be effectively utilized without occupying the effective area of wafer 131.
[0051] For example, the doped semiconductor layer 400 can be formed by, for example, a selective epitaxial growth process or a lift-off process, whichever is appropriate for those skilled in the art.
[0052] In step S30, a patterned photoresist layer is first formed on a first side of the substrate 100, exposing a portion of the insulating layer 110 and at least a portion of the low-resistivity surface a. Then, using the patterned photoresist layer as a mask, an anisotropic etching process is performed from the first side to remove a portion of the insulating layer 110, exposing the conductor layer 120. Exemplarily, this anisotropic etching process can be an HPP etching process or other similar dry etching processes that generate a large amount of plasma charge. Exemplarily, in this embodiment, an anisotropic etching process is performed from the first side to remove a portion of the insulating layer 110, exposing the surface of the first side of the second conductive layer 122 to achieve electrical lead-out of the second conductive layer 122. For example, the second conductive layer 122 includes pads or conductive wiring, or the second conductive layer 122 includes conductive vias, or the second conductive layer 122 includes pads or conductive wiring, and conductive vias located on the side of the pads or conductive wiring away from the active substrate.
[0053] However, it is not limited to this. After ion implantation, the photoresist layer 200 can be removed, and an anisotropic etching process can be performed on the entire surface to expose the conductor layer 120. The specific settings can be configured according to actual needs.
[0054] According to the semiconductor structure fabrication method of the application embodiment, by forming a low-resistivity surface a (similar to a lightning rod) electrically connected to the active substrate 130 on the first side of the substrate 100, the charge acting on the edge of the substrate 100 during dry etching can be guided to the active substrate 130, charging the active substrate and the conductor layer 120 electrically connected to the active substrate. On the one hand, this avoids the formation of a strong potential difference between the surface of the insulating layer 110 and the conductor layer 120 near the surface of the insulating layer 110, thus avoiding arc discharge and breakdown of the insulating layer 110. On the other hand, it avoids the formation of a strong potential difference between the first conductive layer 121 and the second conductive layer 122 in the second region 102, thus avoiding breakdown of the insulating layer 110 between the first conductive layer 121 and the second conductive layer 122.
[0055] In another embodiment of this application, the method for fabricating the semiconductor structure includes the steps S10-S30 described above. Step S10 is the same as in the above embodiment and will not be repeated here.
[0056] In this embodiment, the active substrate 130 in the substrate 100 includes a doped region 1301 and an epitaxial layer 1302. That is, the wafer 131 includes a doped region 1301 and an epitaxial layer 1302. The epitaxial layer 1302 is located between the doped region 1301 and the interconnect layer. The conductivity of the epitaxial layer 1302 is lower than that of the doped region 1301, that is, the doping concentration of the epitaxial layer 1302 is lower than that of the doped region 1301.
[0057] See appendix Figure 4In step S20, the substrate 100 is trimmed until the active substrate 130 is exposed on the first side, wherein the trimming width d is 0.3 mm to 1.2 mm. The trimmed substrate 100 exposes a doped region 1301 on the first side, and a low-resistivity surface a electrically connected to the active substrate 130 is formed on the first side of the substrate 100. The low-resistivity surface a includes the surface of the doped region 1301 exposed by the trimming process.
[0058] In step S30, a patterned photoresist layer is first formed on a first side of the substrate 100, exposing a portion of the insulating layer 110 and at least a portion of the low-resistivity surface a. Then, using the patterned photoresist layer as a mask, an anisotropic etching process is performed from the first side to remove a portion of the insulating layer 110, exposing the conductor layer 120. Exemplarily, this anisotropic etching process can be an HPP etching process or other similar dry etching processes that generate a large amount of plasma charge. Exemplarily, in this embodiment, an anisotropic etching process is performed from the first side to remove a portion of the insulating layer 110, exposing the surface of the first side of the second conductive layer 122 to achieve electrical lead-out of the second conductive layer 122. For example, the second conductive layer 122 includes pads or conductive wiring, or the second conductive layer 122 includes conductive vias, or the second conductive layer 122 includes pads or conductive wiring, and conductive vias located on the side of the pads or conductive wiring away from the active substrate.
[0059] However, this is not the only example. In another example, the first side of the trimmed substrate 100 exposes the doped region 1301. Forming a low-resistivity surface a electrically connected to the active substrate 130 on the first side of the substrate 100 further includes ion implantation of the exposed doped region 1301. The method and effect of ion implantation have been described above and will not be repeated here. Furthermore, the photoresist layer 200 can be removed after ion implantation, and an anisotropic etching process can be performed on the entire surface to expose the conductor layer 120, which can be specifically set according to actual needs.
[0060] According to the semiconductor structure fabrication method of the application embodiment, by forming a low-resistivity surface a (similar to a lightning rod) electrically connected to the active substrate 130 on the first side of the substrate 100, the charge acting on the edge of the substrate during dry etching can be guided to the active substrate 130, charging the active substrate and the conductor layer 120 electrically connected to the active substrate. On the one hand, this avoids the formation of a strong potential difference between the surface of the insulating layer 110 and the conductor layer 120 near the surface of the insulating layer 110, thus avoiding arc discharge and breakdown of the insulating layer 110. On the other hand, it avoids the formation of a strong potential difference between the first conductive layer 121 and the second conductive layer 122 in the second region 102, thus avoiding breakdown of the insulating layer 110 between the first conductive layer 121 and the second conductive layer 122.
[0061] In an embodiment not shown, forming a low-resistivity surface a includes forming a low-resistivity refractory metal silicide on the exposed crystal edge surface after trimming. The low-resistivity surface a may also include the surface of the refractory metal silicide.
[0062] Although exemplary embodiments have been described herein with reference to the accompanying drawings, it should be understood that the above exemplary embodiments are merely illustrative and are not intended to limit the scope of this application. Various changes and modifications can be made therein by those skilled in the art without departing from the scope and spirit of this application. All such changes and modifications are intended to be included within the scope of this application as claimed in the appended claims.
[0063] Numerous specific details are set forth in the specification provided herein. However, it will be understood that embodiments of this application may be practiced without these specific details. In some instances, well-known methods, structures, and techniques have not been shown in detail so as not to obscure the understanding of this specification.
[0064] Similarly, it should be understood that, in order to streamline this application and aid in understanding one or more of the various inventive aspects, features of this application may sometimes be grouped together in a single embodiment, figure, or description thereof in the description of exemplary embodiments of this application. However, this approach should not be construed as reflecting an intention that the claimed application requires more features than are expressly recited in each claim. Rather, as reflected in the corresponding claims, its inventive point lies in solving the corresponding technical problem with features fewer than all features of a single disclosed embodiment. Therefore, the claims following the detailed description are hereby expressly incorporated into that detailed description, wherein each claim itself is a separate embodiment of this application.
[0065] Those skilled in the art will understand that, apart from the mutual exclusion of features, all features disclosed in this specification (including the accompanying claims, abstract, and drawings) and all processes or units of any method or apparatus so disclosed can be combined in any combination. Unless otherwise expressly stated, each feature disclosed in this specification (including the accompanying claims, abstract, and drawings) may be replaced by an alternative feature serving the same, equivalent, or similar purpose.
[0066] Furthermore, those skilled in the art will understand that although some embodiments described herein include certain features but not others included in other embodiments, combinations of features from different embodiments are intended to be within the scope of this application and form different embodiments. For example, in the claims, any one of the claimed embodiments can be used in any combination.
[0067] It should be noted that the above embodiments are illustrative of this application and not restrictive of this application, and that those skilled in the art can devise alternative embodiments without departing from the scope of the appended claims.
Claims
1. A method for fabricating a semiconductor structure, characterized in that, include: A substrate is provided, the substrate including an interconnect layer on a first side and an active substrate on a second side, the interconnect layer including an insulating layer and a conductor layer covered by the insulating layer, at least a portion of the conductor layer being electrically connected to the active substrate; A low-resistivity surface electrically connected to the active substrate is formed on the first side of the substrate, wherein the conductivity of the low-resistivity surface is greater than or equal to the conductivity of the active substrate. An anisotropic etching process is performed from the first side to remove a portion of the insulating layer, exposing the conductor layer.
2. The preparation method according to claim 1, characterized in that, The active substrate includes a wafer, and the low-resistivity surface is formed in the region of the substrate corresponding to the edge of the wafer.
3. The preparation method according to claim 2, characterized in that, An active device is formed in the active substrate, and the conductor layer includes at least a first conductive layer and a second conductive layer. The first conductive layer is located between the second conductive layer and the active substrate, and the first conductive layer is electrically connected to the active device. The substrate includes a first region, a second region, and a third region, which are arranged along the center to edge direction of the wafer. The first region and the second region each have the conductor layer. In the first region, the first conductive layer and the second conductive layer are electrically connected. In the second region, the first conductive layer and the second conductive layer are mutually insulated. The third region includes the crystal edge and the insulating layer located on a first side of the crystal edge. The exposure of the conductor layer includes: exposing the surface of the first side of the second conductive layer.
4. The preparation method according to claim 2, characterized in that, Before forming a low-resistivity surface electrically connected to the active substrate on the first side of the substrate, the fabrication method further includes: The substrate is trimmed until the first side exposes the active substrate, wherein the trimming width is 0.3mm-1.2mm.
5. The preparation method according to claim 4, characterized in that, The trimming process includes at least one of dry etching, wet chemical etching, laser trimming, mechanical polishing, and chemical mechanical polishing.
6. The preparation method according to claim 4, characterized in that, The active substrate includes a doped region and an epitaxial layer, the epitaxial layer being located between the doped region and the interconnect layer, and the conductivity of the epitaxial layer being lower than the conductivity of the doped region; Wherein, the first side of the substrate after the trimming process exposes the doped region, and the low-resistivity surface includes the surface of the doped region exposed by the trimming process.
7. The preparation method according to claim 4 or 6, characterized in that, The formation of a low-resistivity surface electrically connected to the active substrate on the first side of the substrate includes: Ion implantation is performed on the first side of the active substrate exposed after trimming to form a doped region in the trimmed area; The doping type of the doped region is not opposite to that of the active substrate, and the doping concentration of the doped region is not lower than that of the active substrate.
8. The preparation method according to claim 7, characterized in that, The step of ion implantation into the active substrate exposed after trimming includes: A photoresist layer is spin-coated onto the first side of the trimmed substrate; The photoresist layer is subjected to edge washing to at least partially expose the active substrate exposed after edge trimming. Ion implantation is performed on the active substrate using the photoresist layer as a mask.
9. The preparation method according to claim 8, characterized in that, When performing edge washing on the photoresist layer, the edge washing width is 0.3mm-1.2mm.
10. The preparation method according to claim 8, characterized in that, The anisotropic etching process performed from the first side to remove a portion of the insulating layer includes: After ion implantation, the photoresist layer is patterned; Using the patterned photoresist layer as a mask, the anisotropic etching process is performed from the first side to remove a portion of the insulating layer.
11. The preparation method according to claim 4, characterized in that, The formation of a low-resistivity surface electrically connected to the active substrate on the first side of the substrate includes: A doped semiconductor layer is grown on the first side surface of the active substrate exposed after trimming. The doped semiconductor layer is in contact with the active substrate to form an electrical connection. The conductivity type of the doped semiconductor layer is not opposite to that of the active substrate, and the conductivity of the doped semiconductor layer is not lower than that of the active substrate.