Semiconductor structure, method for forming it, and method for optimizing silicon nitride layer profile
By optimizing the thickness and profile of the SiN layer through cyclic deposition, etching, and nitriding processes, the unwanted sidewall deposition problem in conventional deposition processes is solved, achieving uniform and reliable SiN layer formation within the gaps, thus improving the isolation and protection of the device.
Patent Information
- Application Number
- CN202610652874.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-05-13
- Publication Date
- 2026-11-17
AI Technical Summary
When conventional deposition processes deposit a sufficient thickness of SiN at the bottom of the gaps in the substrate, unwanted sidewall or overhang depositions can easily occur, resulting in poor device isolation, reliability, and protection.
By cyclically performing deposition, etching, and nitriding processes, an amorphous silicon layer is formed and converted into a silicon nitride layer. Combined with a post-etching process, the thickness and profile of the SiN layer are optimized to ensure that the SiN layer within the gaps reaches the target bottom thickness.
This technology enables the formation of a uniform and reliable SiN layer within the gap, providing electrostatic discharge protection and field oxide etch barrier, thereby improving the isolation and protection of the device.
Smart Images

Figure CN123124681A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to semiconductor processing, and more specifically, to forming a silicon nitride (SiN) layer within a gap in a substrate. Background Technology
[0002] Conventional deposition processes typically face limitations in depositing sufficient SiN thickness at the bottom of gaps in the substrate without causing unwanted sidewall or overhang deposition. These drawbacks hinder effective device isolation, reliability, and protection. Summary of the Invention
[0003] A method is provided for forming a semiconductor structure including a silicon nitride (SiN) layer. The method includes performing a deposition process to deposit an amorphous silicon (a-Si) layer on a substrate including gaps, and performing an etching process on the a-Si layer. The method further includes performing a nitriding process to convert at least a portion of the a-Si layer into a SiN layer, and repeating the deposition, etching, and nitriding processes until a target bottom thickness of the SiN layer within the gaps is achieved.
[0004] In some embodiments, the target bottom thickness of the SiN layer within the gap is in the range of 150 Å to 300 Å. In some embodiments, the method further includes performing a post-etching process after achieving the target bottom thickness of the SiN layer within the gap. In some embodiments, dilute hydrofluoric acid (DHF) or phosphoric acid (H3PO4) is used during the post-etching process to refine the profile of the SiN layer. In some embodiments, the post-etching process is performed until the sidewall width of the SiN layer within the gap is less than 30 Å. In some embodiments, the post-etching process is performed at approximately 250°C.
[0005] In some embodiments, a CCP plasma is used to perform a deposition process. The CCP plasma is generated using a gas mixture at an RF frequency in the range of about 1 MHz to 100 MHz (e.g., 13.56 MHz). The gas mixture includes a silicon-containing gas selected from silane (SiH4), disilane (Si2H6), hydrosilane, silicon halide, or organosilicon compounds, and one or more other gases including hydrogen (H2), helium (He), and argon (Ar). In some embodiments, a CCP plasma is used to perform an etching process. The CCP plasma is generated using a gas mixture including hydrogen (H2), helium (He), and argon (Ar) at an RF frequency in the range of about 1 MHz to 100 MHz (e.g., 13.56 MHz). In some embodiments, a CCP plasma is used to perform a nitriding process. The CCP plasma is generated using a gas mixture including nitrogen (N2), ammonia (NH3), hydrogen (H2), and helium (He) at an RF frequency in the range of about 1 MHz to 100 MHz (e.g., 13.56 MHz). In some embodiments, the etching process and the nitriding process are performed in the same reaction chamber.
[0006] A method for optimizing the profile of a silicon nitride (SiN) layer is provided. The method includes performing multiple cycles of an a-Si deposition process, an H2 etching process, and a nitriding process. The method also includes measuring the thickness of the resulting SiN layer after each cycle. Furthermore, the method includes adjusting process parameters to achieve a desired SiN layer thickness.
[0007] In some embodiments, process parameters include deposition time, etching duration, and nitriding temperature. In some embodiments, the method further includes performing a DHF post-etching process or an H3PO4 post-etching process to further refine the profile of the SiN layer. In some embodiments, measurements are performed using a real-time thickness measurement system. In some embodiments, the profile of the SiN layer is monitored using a transmission electron microscope (TEM). In some embodiments, the cycle is repeated at least 10 times. In some embodiments, the cycle is repeated at least 20 times.
[0008] A semiconductor structure is provided. The semiconductor structure includes a silicon substrate and a bottom SiN film, the bottom SiN film having a thickness greater than 150 Å and being formed on the silicon substrate using a cyclic deposition-etch-nitridation process.
[0009] In some embodiments, the silicon substrate includes a plurality of gaps, and a bottom SiN film is formed within each gap. In some embodiments, the semiconductor structure further includes a gate structure formed on the silicon substrate and adjacent to the bottom SiN film. Attached Figure Description
[0010] This disclosure can be more fully understood by referring to the detailed description and embodiments in conjunction with the accompanying drawings. It should be noted that the various features may not be drawn to scale. In fact, for clarity of discussion, the dimensions of the various features may be arbitrarily increased or decreased, and the various features may be drawn schematically.
[0011] Figures 1A to 1G Exemplary steps of a method for forming a silicon nitride (SiN) layer within a gap in a substrate, according to some embodiments, are shown.
[0012] Figure 2A The process flow of the deposition process according to some embodiments is shown.
[0013] Figure 2B The process flow of the etching process according to some embodiments is shown.
[0014] Figure 2C A process flow diagram of a nitriding process according to some embodiments is shown.
[0015] Figure 3 A system that can perform the method according to some embodiments is shown.
[0016] Figure 4 A flowchart of a method for forming a semiconductor structure including a SiN layer according to some embodiments is shown.
[0017] Figure 5 A flowchart of a method for optimizing the profile of a SiN layer according to some embodiments is shown. Detailed Implementation
[0018] The following description provides various embodiments or examples for implementing different features of this disclosure. Additionally, spatial relative terms may be used in the following description to describe the arrangement of various features. These spatial relative terms are for the convenience of describing the positional relationship between one feature and another as shown in the accompanying drawings. These spatial relative terms are intended to cover different orientations of the device in use or operation, in addition to those shown in the drawings. The device may be oriented in other ways (rotated 90 degrees or in other orientations), and the spatial relative terms used in the following description may be interpreted accordingly. For example, if the device in the drawings were upside down, the "above" feature would become the "below" feature.
[0019] For example, in the following description, the first feature being formed "on", "above", or "below" the second feature can include embodiments in which the first feature and the second feature are formed in direct contact, and can also include embodiments in which an additional feature can be formed between the first feature and the second feature such that the first feature and the second feature are not in direct contact.
[0020] In the following description, the terms “comprising,” “including,” “having,” etc., shall be interpreted as meaning “including but not limited to…”. Therefore, when the terms “comprising,” “including,” “having,” etc., are used, they specify the presence of a corresponding feature, area, step, operation, and / or element, and do not exclude the presence of other features, areas, steps, operations, and / or elements.
[0021] As used herein, the term "substrate" can refer to any one or more underlying materials that can be used to form or on which devices, circuits, or films are formed. A substrate may comprise a bulk material, such as silicon (e.g., single-crystal silicon), other group IV materials (e.g., germanium), or compound semiconductor materials (e.g., group III-V or II-VI semiconductors), and may comprise one or more layers overlying or underlying the bulk material. Furthermore, a substrate may include various features such as gaps (e.g., recesses or vias), lines, or protrusions, such as lines with gaps formed therebetween, formed on or within at least a portion of the layers or bulk material of the substrate. For example, one or more features may have an aspect ratio of about 1:1, 1:3, 1:10, 1:100, or greater, or any range thereof. In some examples, one or more features may include a gap structure comprising a bottom and one or more sidewalls. In some examples, one or more sidewalls may not be straight, such that the width of the gap structure is non-uniform in depth. In some examples, one or more sidewalls may have a convex shape. In some examples, one or more sidewalls may protrude below the opening of the gap structure. In some examples, the gap structure may have a neck at the opening of the gap structure.
[0022] As used herein, the term "film" refers to a layer extending in a direction perpendicular to the thickness direction. As used herein, the term "layer" refers to a material of a certain thickness formed on a surface and can be synonymous with a film or non-film structure. A film or layer may consist of discrete single films or layers or multiple films or layers having certain properties, and the boundaries between adjacent films or layers may or may not be clear, and may or may not be established based on the physical, chemical and / or any other properties, formation processes or sequences and / or functions or purposes of adjacent films or layers. A layer or film may be continuous or discontinuous. Furthermore, a single film or layer may be formed using one or more deposition cycles and / or one or more deposition and processing cycles.
[0023] As used herein, the term "structure" can refer to a device structure that is partially or fully fabricated. For example, a structure can be a substrate or a substrate having one or more layers and / or features formed thereon.
[0024] As used herein, the term “chemical vapor deposition” can refer to any process in which a substrate is exposed to one or more volatile precursors that react and / or decompose on the substrate surface to produce the desired deposition.
[0025] As used herein, the term "atomic layer deposition" (ALD) can refer to a vapor-phase deposition process in which deposition cycles, preferably multiple consecutive cycles, are performed in a processing chamber. Typically, during each cycle, a precursor is chemisorbed onto the deposition surface (e.g., a substrate surface or a previously deposited lower layer surface, such as material from a previous ALD cycle), forming a monolayer or sub-monolayer that is not readily reactive with another precursor (i.e., a self-limiting reaction). Subsequently, if desired, a reactant (e.g., another precursor or reactive gas) can be introduced into the processing chamber to convert the chemisorbed precursor into the desired material on the deposition surface. Typically, this reactant is capable of further reacting with the precursor. Furthermore, a purging step can be used during each cycle to remove excess precursor from the processing chamber and / or excess reactant and / or reaction byproducts from the processing chamber after the conversion of the chemisorbed precursor. Furthermore, the term atomic layer deposition as used herein is also intended to include processes specified by related terms, such as chemical vapor deposition, atomic layer epitaxy (ALE), molecular beam epitaxy (MBE), gas-source MBE or organometallic MBE, and chemical beam epitaxy when performed with alternating pulses of a precursor composition, a reactive gas, and a purge gas (e.g., an inert carrier gas).
[0026] As used herein, the term "cyclic deposition process" can refer to a vapor-phase deposition process in which deposition cycles (typically multiple consecutive deposition cycles) are performed in a processing chamber. Cyclic deposition processes can include cyclic plasma-enhanced CVD, ALD, and / or plasma-enhanced ALD (PEALD) processes. A cyclic deposition process may include one or more cycles, each cycle comprising plasma activation of precursors, reactants, and / or inert gases in any combination.
[0027] As used herein, the term “continuous” can refer to a discrete physical or chemical structure that does not break the vacuum, has no interruption as a timeline, has no material intervention step, has no change in processing conditions, immediately follows as the next step, or, in some embodiments and depending on the circumstances, has no intervention between the two structures except for the two structures themselves.
[0028] In this disclosure, any two numbers of a variable may constitute a feasible range of the variable, and any range indicated may include or exclude endpoints. Furthermore, any value of the indicated variable (whether or not it is indicated by “about”) may refer to an exact value or an approximate value and includes equivalents, and in some embodiments may refer to an average, median, representative value, multi-value, etc.
[0029] When using (e.g., RF) plasma, low RF frequencies (LF) can be below 1 MHz or between 430 kHz and 1 MHz or between approximately 40 kHz and 800 kHz, high RF frequencies (HF) can be greater than 1 MHz or between 13 and 100 MHz or between approximately 13.56 MHz and 27 MHz, and very high RF frequencies (VHF) can be greater than 27 MHz, greater than 30 MHz, greater than 40 MHz, greater than 60 MHz or between approximately 30 MHz and 5 GHz.
[0030] Please refer to Figures 1A to 1G as well as Figures 2A to 2C . Figures 1A to 1G Exemplary steps of a method for forming a silicon nitride (SiN) layer (e.g., 235, 236, 245, or 245') within a gap 110 of a substrate 100, according to some embodiments, are shown. The substrate 100 may be a wafer, such as a silicon wafer. Other substrates may also be used, such as multilayer or gradient substrates. In some embodiments, the semiconductor material of the substrate 100 may include silicon; germanium; compound semiconductors including silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, and / or indium antimonide; alloy semiconductors including SiGe, GaAsP, AlInAs, AlGaAs, GaInAs, GaInP, and / or GaInAsP; or combinations thereof. The gap 110 may be a trench or via in the substrate 100.
[0031] The method includes a deposition process 210, an etching process 220, and a nitriding process 230, as well as an optional post-etching process 240. Figure 2A A process flow diagram of deposition process 210 according to some embodiments is shown. Figure 2B The process flow of etching process 220 according to some embodiments is shown. Figure 2C A process flow diagram of nitriding process 230 according to some embodiments is shown.
[0032] The deposition process 210 may also be referred to as an a-Si deposition process because it forms an amorphous silicon (a-Si) layer 215. In some embodiments, the deposition process 210 is performed using a CCP plasma generated with a gas mixture at an RF frequency in the range of about 1 MHz to 100 MHz (e.g., 13.56 MHz). The gas mixture includes silicon-containing gases selected from silanes (SiH4), disilanes (Si2H6), hydrosilanes, silicon halides, or organosilicon compounds, and one or more additional gases including hydrogen (H2), helium (He), and argon (Ar). Specifically, the deposition process 210 may include multiple stages, including a feed stage 211, an RF turn-on stage 212, and a post-purge stage 213. In some embodiments, the duration of the deposition process 210 ranges from about 10 seconds to 120 seconds. In some embodiments, the deposition process 210 is performed for less than 60 seconds. In some embodiments, the deposition process 210 is performed for about 10 seconds, 20 seconds, or 30 seconds.
[0033] A silicon-containing gas (e.g., SiH4) is introduced at the start of feed stage 211, flows continuously through RF turn-on stage 212, and stops at the start of post-purge stage 213. Various gases, He, H2, and Ar, are continuously supplied throughout all three stages (i.e., feed stage 211, RF turn-on stage 212, and post-purge stage 213). During feed stage 211, the RF power is off. The RF power is turned on during RF turn-on stage 212 and off again at the start of post-purge stage 213. The pressure remains constant throughout the deposition process 210. In other words, the deposition process 210 begins with a silicon-containing gas and various gas streams, and RF power is applied only during the intermediate stage (i.e., RF turn-on stage 212) to activate deposition. Post-purge stage 213 continues the gas flow only to remove residual gases. The pressure remains stable throughout all stages.
[0034] The formed a-Si layer 215 includes a top thickness 215T on the top surface of the substrate 100, a sidewall width 215S lining the sidewalls of the gap 110, and a bottom thickness 215B at the bottom of the gap 110. In some embodiments, the top thickness 215T of the a-Si layer 215 is greater than 150 Å. In some embodiments, the sidewall width 215S of the a-Si layer 215 is greater than 35 Å. In some embodiments, the bottom thickness 215B of the a-Si layer 215 is greater than 50 Å.
[0035] Next, etching process 220 is performed. Etching process 220 can be a wet etching process. Etching process 220 can also be referred to as an H2 etching process because it requires hydrogen plasma. Etching process 220 etches the a-Si layer 215 to form the etched a-Si layer 225. In some embodiments, CCP plasma is used to perform etching process 220, which is generated using a gas mixture comprising hydrogen (H2), helium (He), and argon (Ar) at an RF frequency in the range of about 1 MHz to 100 MHz (e.g., 13.56 MHz). Specifically, etching process 220 may include multiple stages, including a feed stage 221, an RF turn-on stage 222, and a post-purge stage 223. In some embodiments, etching process 220 lasts for more than 50 seconds. In some embodiments, etching process 220 lasts for about 60 to 110 seconds. In some embodiments, etching process 220 lasts for about 100 seconds.
[0036] H2 is continuously supplied from feed stage 221 through post-purge stage 223. Similar to the H2 supply, He and Ar (inert gases or carrier gases) are also continuously supplied in all three stages (i.e., feed stage 221, RF on stage 222, and post-purge stage 223) to help stabilize the plasma and assist in purging. During feed stage 221 and post-purge stage 223, the RF power is off. The RF power is turned on only during RF on stage 222. The RF power activates the plasma. The pressure remains constant in all three stages (i.e., feed stage 221, RF on stage 222, and post-purge stage 223), thus providing a stable environment.
[0037] The etched a-Si layer 225 includes a top thickness 225T on the top surface of the substrate 100, a sidewall width 225S lining the sidewalls of the gap 110, and a bottom thickness 225B at the bottom of the gap 110. The top thickness 225T of the etched a-Si layer 225 is less than the top thickness 215T of the a-Si layer 215, the sidewall width 225S of the etched a-Si layer 225 is less than the sidewall width 215S of the a-Si layer 215, and the bottom thickness 225B of the etched a-Si layer 225 is less than or equal to the bottom thickness 215B of the a-Si layer 215, because the etching process 220 removes at least a portion of the a-Si layer 215.
[0038] Furthermore, the etching process 220 primarily etches the top region of the a-Si layer 215. Therefore, in some embodiments, the difference between the top thickness 225T and the top thickness 215T of the etched a-Si layer 225 is greater than the difference between the bottom thickness 225B and the bottom thickness 215B of the etched a-Si layer 225. In some embodiments, the difference between the sidewall width 225S and the sidewall width 215S of the etched a-Si layer 225 may also be greater than the difference between the bottom thickness 225B and the bottom thickness 215B of the etched a-Si layer 225.
[0039] Next, a nitriding process 230 is performed. The nitriding process 230 converts at least a portion of the etched a-Si layer 225 into a SiN layer 235. In some embodiments, the nitriding process 230 is performed using CCP plasma, which is generated using a gas mixture comprising nitrogen (N2), ammonia (NH3), hydrogen (H2), and helium (He) at an RF frequency in the range of about 1 MHz to 100 MHz (e.g., 13.56 MHz). Specifically, the nitriding process 230 may include multiple stages, including a feed stage 231, an RF turn-on stage 232, and a post-purge stage 233. In some embodiments, the duration of the nitriding process 230 ranges from about 10 seconds to 400 seconds. In some embodiments, the nitriding process 230 is performed for less than 200 seconds. In some embodiments, the nitriding process 230 is performed for about 50 seconds, 100 seconds, or 150 seconds. In some embodiments, the nitriding process 230 is performed at a temperature between 100°C and 600°C. In some embodiments, the nitriding process 230 is carried out at about 400°C.
[0040] Nitrogen reactants (used for nitriding), such as N2 and NH3, are continuously supplied from feed stage 231 through post-purge stage 233. Similar to the nitrogen reactant supply, H2, He, and Ar (carrier gas) are also continuously supplied in all three stages (i.e., feed stage 231, RF on stage 232, and post-purge stage 233), contributing to plasma stabilization and purging. During feed stage 231 and post-purge stage 233, the RF power is off. The RF power is turned on only during RF on stage 232. The RF power activates the plasma to initiate the nitriding reaction. Pressure remains constant in all three stages (i.e., feed stage 231, RF on stage 232, and post-purge stage 233), thus providing a stable environment.
[0041] The SiN layer 235 includes a top thickness 235T on the top surface of the substrate 100, a sidewall width 235S on the sidewalls of the gap 110, and a bottom thickness 235B at the bottom of the gap 110. As the nitriding process 230 converts a-Si into SiN, the top thickness 235T, the sidewall width 235S, and the bottom thickness 235B of the SiN layer 235 are respectively greater than or equal to the top thickness 225T, the sidewall width 225S, and the bottom thickness 225B of the etched a-Si layer 225.
[0042] In some embodiments, the deposition process 210, the etching process 220, and the nitriding process 230 are repeated in multiple cycles (e.g., 5-30 cycles) until a SiN layer 236 with a bottom thickness 236B greater than the target bottom thickness is formed, such as... Figure 1E As shown. The SiN layer 236 also includes a top thickness 236T on the top surface of the substrate 100 and a sidewall width 236S on the sidewalls of the gap 110. The top thickness 236T, the sidewall width 236S, and the bottom thickness 236B of the SiN layer 236 are greater than or equal to the top thickness 235T, the sidewall width 235S, and the bottom thickness 235B of the SiN layer 235, respectively.
[0043] In some embodiments, the target bottom thickness of the SiN layer 236 within the gap 110 is greater than 150 Å. That is, the deposition process 210, etching process 220, and nitriding process 230 are performed until the bottom thickness 236B of the SiN layer 236 exceeds 150 Å. In some embodiments, the target bottom thickness of the SiN layer 236 within the gap 110 is greater than 100 Å. That is, the deposition process 210, etching process 220, and nitriding process 230 are performed until the bottom thickness 236B of the SiN layer 236 exceeds 100 Å. In some embodiments, the target bottom thickness of the SiN layer 236 within the gap 110 is in the range of 150 Å to 300 Å.
[0044] A relatively thick bottom SiN layer can be particularly advantageous for electrostatic discharge (ESD) protection, field oxide etch barrier layers, and other dielectric applications requiring protection at the bottom of narrow features, such as substrate gaps. For example, in some embodiments, the SiN layer 236 can be used as a protective structure in an ESD protection scheme or as a barrier layer during the field oxide etch process. The combination of deposition, selective etching, and nitriding enables the formation of a bottom-thickened SiN profile.
[0045] In some embodiments, the cycle is repeated at least 10 times. In some embodiments, the cycle is repeated at least 20 times. The number of cycles may depend on the desired target bottom thickness of the SiN layer 236 within the gap 110 (e.g., 100 Å, 150 Å, or 150 Å to 300 Å), the a-Si deposition rate during deposition process 210, the etching rate during etching process 220, and the conversion efficiency during nitriding process 230. This cyclic method allows for precise control of the SiN deposition distribution, particularly when achieving a relatively thick bottom portion of the SiN layer, while minimizing over-deposition on the top and sidewall regions.
[0046] It should be noted that the thickness of the resulting SiN layer (e.g., the sidewall width 235S of SiN layer 235 and / or the bottom thickness 235B of SiN layer 235) can be measured after each cycle, and process parameters can be adjusted accordingly to better achieve the desired thickness of the SiN layer. Process parameters include temperature, pressure, a-Si deposition rate, deposition time, etching duration, cycle repeatability, plasma parameters, chamber conditions, etc. In some embodiments, a real-time thickness measurement system is used for measurement. In some embodiments, a transmission electron microscope (TEM) is used to monitor the profile of the SiN layer.
[0047] This process allows for precise control of film growth by measuring the SiN layer thickness (e.g., the sidewall width 235S of SiN layer 235 and / or the bottom thickness 235B of SiN layer 235) after each cycle. Furthermore, real-time adjustment of process parameters such as temperature, pressure, deposition rate, and etch duration allows for dynamic process tuning to achieve optimal results. In addition, real-time monitoring and parameter tuning contribute to consistent layer formation across cycles, improve process repeatability and film uniformity, and result in more reliable and predictable yields.
[0048] A resulting semiconductor structure is provided. The semiconductor structure includes a silicon substrate (e.g., substrate 100) and a bottom SiN film (e.g., the bottom region of SiN layer 236), the bottom SiN film having a thickness greater than 150 Å and formed on the silicon substrate using a cyclic deposition-etch-nitridation process. In some embodiments, the silicon substrate includes a plurality of gaps, and the bottom SiN film is formed within each gap. In some embodiments, the semiconductor structure may further include a gate structure formed on the silicon substrate and adjacent to the bottom SiN film.
[0049] In some embodiments, after achieving the target bottom thickness of the SiN layer 236 within the gap 110, a post-etching process 240 can be performed to form the SiN layer. Figure 1F 245 or Figure 1G(245' in the original text). The post-etching process 240 can refine the contour of the SiN layer 236. The post-etching process 240 can be a wet etching process. In some embodiments, the post-etching process 240 may be referred to as a DHF post-etching process because DHF is used in the post-etching process 240. In some embodiments, a 200:1 DHF solution is used. In some embodiments, the post-etching process 240 may be referred to as an H3PO4 post-etching process because H3PO4 is used in the post-etching process 240. In some embodiments, an H3PO4 solution with a concentration of about 85% is used. In some embodiments, the post-etching process 240 is performed for more than 50 seconds. In some embodiments, the post-etching process 240 is performed for about 100 seconds to 300 seconds. In some embodiments, the post-etching process 240 is performed for about 100 seconds, about 150 seconds, or about 200 seconds. In some embodiments, the post-etching process 240 is performed at a temperature between 100°C and 500°C. In some embodiments, the post-etching process 240 is performed at about 250°C.
[0050] like Figure 1F As shown, the SiN layer 245 includes a top thickness 245T on the top surface of the substrate 100, a sidewall width 245S lining the sidewalls of the gap 110, and a bottom thickness 245B at the bottom of the gap 110. The top thickness 245T is less than the top thickness 236T of the SiN layer 236, the sidewall width 245S is less than the sidewall width 236S of the SiN layer 236, and the bottom thickness 245B is less than or equal to the bottom thickness 236B of the SiN layer 236 because the post-etching process 240 removes at least a portion of the SiN layer 236. In some embodiments, after performing the post-etching process 240, the bottom thickness 245B of the SiN layer 245 within the gap 110 remains greater than the target bottom thickness. In some embodiments, after performing the post-etching process 240, the bottom thickness 245B of the SiN layer 245 remains greater than 150 Å. In some embodiments, after performing the post-etching process 240, the bottom thickness 245B of the SiN layer 245 is greater than 100 Å.
[0051] Furthermore, the post-etching process 240 primarily etches the top and / or sidewall regions of the SiN layer 236. Therefore, in some embodiments, the difference between the top thickness 245T of the SiN layer 245 and the top thickness 236T of the SiN layer 236 is greater than the difference between the bottom thickness 245B of the SiN layer 245 and the bottom thickness 236B of the SiN layer 236. In some embodiments, the difference between the sidewall width 245S of the SiN layer 245 and the sidewall width 236S of the SiN layer 236 may also be greater than the difference between the bottom thickness 245B of the SiN layer 245 and the bottom thickness 236B of the SiN layer 236.
[0052] In some embodiments, post-etching process 240 is performed until the top thickness 245T of the SiN layer 245 on the top surface of the substrate 100 is reduced to less than 100 Å. In some embodiments, post-etching process 240 is performed until the top thickness 245T of the SiN layer 245 on the top surface of the substrate 100 is reduced to about 30 Å. In some embodiments, post-etching process 240 is performed until the sidewall width 245S of the SiN layer 245 within the gap 110 is reduced to less than 30 Å. In some embodiments, post-etching process 240 is performed until the sidewall width 245S of the SiN layer 245 within the gap 110 is reduced to about 20 Å.
[0053] In some embodiments, a post-etching process 240 is performed until the SiN layer 245' is selectively formed at the bottom of the gap 110 without forming any substantial thickness on the top surface of the substrate 100 or along the sidewalls of the gap 110, such as Figure 1G As shown.
[0054] The SiN layer 245' includes a bottom thickness 245'B at the bottom of the gap 110. The bottom thickness 245'B is less than or equal to the bottom thickness 236B of the SiN layer 236. In some embodiments, after performing the post-etching process 240, the bottom thickness 245'B of the SiN layer 245' within the gap 110 remains greater than the target bottom thickness. In some embodiments, after performing the post-etching process 240, the bottom thickness 245'B of the SiN layer 245' remains greater than 150 Å. In some embodiments, after performing the post-etching process 240, the bottom thickness 245'B of the SiN layer 245' is greater than 100 Å.
[0055] The deposition process 210, etching process 220, nitriding process 230, and post-etching process 240 can be repeated in multiple cycles (e.g., 5-30 cycles). Alternatively, the post-etching process 240 can be performed only once after several cycles of the deposition process 210, etching process 220, and nitriding process 230 have been completed. In this case, the deposition process 210, etching process 220, and nitriding process 230 are repeated, followed by a single post-etching process 240.
[0056] In some embodiments, all processes (i.e., deposition process 210, etching process 220, nitriding process 230, and post-etching process 240) are performed in situ without exposing the substrate 100 to air. That is, all processes (i.e., deposition process 210, etching process 220, nitriding process 230, and post-etching process 240) are performed in the same reaction chamber. In some embodiments, deposition process 210 and etching process 220 are performed in the same reaction chamber. In some embodiments, etching process 220 and nitriding process 230 are performed in the same reaction chamber.
[0057] Next, please refer to Figure 3 . Figure 3 A system 300 is shown in which the method can be performed according to some embodiments. The system 300 can be used to perform the methods described herein and / or form semiconductor structures as described herein.
[0058] In the illustrated example, system 300 includes one or more reaction chambers 302, a precursor gas source 304, a nitrogen reactant gas source 306, a purge gas source 308, an exhaust source 310, and a controller 312. The reaction chamber 302 can include any suitable reaction chamber, such as a CVD chamber, an ALD chamber, or a PEALD reaction chamber. Although shown as a single reaction chamber 302, system 300 can include any suitable number of reaction chambers, such as a first reaction chamber configured to deposit an a-Si layer, a second reaction chamber configured to perform an etching process on the a-Si layer, and a third reaction chamber configured to perform a nitriding process to convert at least a portion of the a-Si layer into a SiN layer. The first, second, and third reaction chambers can enable high-vacuum isolation and automated wafer transfer.
[0059] Precursor gas source 304 may include a container and one or more precursors as described herein—alone or mixed with one or more carrier gases (e.g., inert gases). Nitrogen reactant gas source 306 may include a container and one or more nitrogen reactants as described herein—alone or mixed with one or more carrier gases. Purge gas source 308 may include one or more inert gases as described herein. Although three gas sources 304, 306, and 308 are shown, system 300 may include any suitable number of gas sources. Gas sources 304, 306, and 308 may be coupled to reaction chamber 302 via lines 314, 316, and 318, each of which may include a flow controller, valve, heater, etc. Exhaust source 310 may include one or more vacuum pumps.
[0060] Controller 312 includes electronic circuitry and software to selectively operate valves, manifolds, heaters, pumps, and other components included in system 300. Such circuitry and components operate to introduce precursors, reactants, and purge gases from corresponding sources 304, 306, and 308. Controller 312 can control the timing of gas pulse sequences, the temperature of the substrate and / or reaction chamber, the pressure within the reaction chamber, and various other operations to provide appropriate operation of system 300. Controller 312 may include control software to electrically or pneumatically control valves to control the inflow and outflow of precursors, reactants, and purge gases from reaction chamber 302. Controller 312 may include modules, such as software or hardware components, to perform certain tasks. Modules may advantageously be configured to reside on addressable storage media of the control system and configured to perform one or more processes.
[0061] Other configurations for performing this method are possible, including different numbers and types of precursor and reactant sources, as well as purge gas sources. Furthermore, it should be understood that numerous arrangements of valves, conduits, precursor sources, and purge gas sources exist to achieve the goal of selectively supplying gases to the reaction chamber 302. Additionally, for the sake of simplicity and to illustrate the system schematically, many components have been omitted, and these components may include, for example, various valves, manifolds, purifiers, heaters, containers, vents, and / or bypasses. For example, an RF power supply capable of operating at 13.56 MHz may be coupled to the reaction chamber 302.
[0062] During operation of system 300, a substrate (e.g., substrate 100) is transferred from, for example, a substrate transport system to reaction chamber 302. Once the substrate is transferred to reaction chamber 302, one or more gases (e.g., precursors, reactants, carrier gases, and / or purge gases) from gas sources 304, 306, and 308 are introduced into reaction chamber 302.
[0063] Next, please refer to Figure 4 . Figure 4 A flowchart of a method 400 for forming a semiconductor structure including a SiN layer according to some embodiments is shown. Method 400 includes multiple operations 410-470. In operation 410, a substrate having gaps is provided in a reaction chamber. In operation 420, a deposition process (e.g., deposition process 210) is performed to deposit an a-Si layer. In operation 430, an etching process (e.g., etching process 220) is performed on the a-Si layer. In operation 440, a nitriding process (e.g., nitriding process 230) is performed to convert at least a portion of the a-Si layer into a SiN layer. In operation 450, if a target bottom thickness of the SiN layer within the gaps is achieved, method 400 proceeds to operation 460, where a post-etching process (e.g., post-etching process 240) is performed on the SiN layer. Alternatively, method 400 (operation 470) can be terminated if the target bottom thickness of the SiN layer within the gaps is achieved. If the target bottom thickness of the SiN layer within the gaps is not achieved, method 400 returns to operation 420.
[0064] Next, please refer to Figure 5 . Figure 5A flowchart of a method 500 for optimizing the profile of a SiN layer according to some embodiments is shown. Method 500 includes multiple operations 510-540. In operation 510, a substrate with gaps is provided in a reaction chamber. In operation 520, multiple cycles of an a-Si deposition process, an H2 etching process, and a nitriding process are performed to form a SiN layer within the gaps. In some embodiments, the number of cycles is between 5 and 30. In operation 530, the thickness of the resulting SiN layer is measured after each cycle. In some embodiments, the measurement is performed using a real-time thickness measurement system. In operation 540, based on the measurement results, process parameters are adjusted to achieve a desired thickness of the SiN layer. In some embodiments, process parameters include temperature, pressure, a-Si deposition rate, deposition time, etching duration, cycle repetition, plasma parameters, chamber conditions, etc.
[0065] In summary, a method is provided for forming a semiconductor structure including a SiN layer within a gap in a substrate. The method includes cyclic deposition of a-Si, etching of the a-Si with hydrogen plasma (primarily thinning the top and sidewall regions while retaining the bottom), and conversion of the a-Si to SiN by nitriding. The method may also include an optional post-etching process to refine the SiN layer, selectively thinning the top and sidewalls while maintaining the bottom thickness. The deposition-etch-nitriding cycle is repeated multiple times (e.g., 5-30 cycles) to gradually build up the bottom thickness of the SiN layer. This allows the formation of SiN layers with a target bottom thickness greater than 100 Å or 150 Å, and in some embodiments, up to 300 Å or greater.
[0066] The cycling process enables the formation of a thick bottom SiN layer, which is particularly advantageous for electrostatic discharge (ESD) protection, field oxide etch barrier layers, and other dielectric applications requiring robust protection at the bottom of narrow features, such as substrate gaps. The number of cycles and process parameters can be adjusted to meet specific requirements. In some embodiments, a real-time thickness measurement system is used to monitor film growth, thereby enhancing process reliability and predictability. Furthermore, all processes can be performed in situ without exposing the substrate to air, thus minimizing contamination.
[0067] The foregoing has outlined features of several embodiments, enabling those skilled in the art to better understand various aspects of this disclosure. Those skilled in the art should understand that they can readily use this disclosure as the basis for designing or modifying other processes and structures to achieve the same purposes and / or advantages as the embodiments described below. Those skilled in the art should also recognize that such equivalent constructions do not depart from the spirit and scope of this disclosure, and that various changes, substitutions, and alterations can be made in the following description without departing from the spirit and scope of this disclosure.
Claims
1. A method for forming a semiconductor structure including a silicon nitride (SiN) layer, the method comprising: A deposition process is performed to deposit an amorphous silicon (a-Si) layer on a substrate including gaps; An etching process is performed on the a-Si layer; A nitriding process is performed to convert at least a portion of the a-Si layer into a SiN layer; as well as Repeat the deposition, etching, and nitriding processes until the target bottom thickness of the SiN layer within the gaps is achieved.
2. The method according to claim 1, wherein, The target bottom thickness of the SiN layer within the gap is in the range of 150 Å to 300 Å.
3. The method of claim 1, further comprising performing a post-etching process after achieving the target bottom thickness of the SiN layer within the gap.
4. The method according to claim 3, wherein, Dilute hydrofluoric acid (DHF) or phosphoric acid (H3PO4) is used in the post-etching process to refine the contour of the SiN layer.
5. The method according to claim 3, wherein, Perform the post-etching process until the sidewall width of the SiN layer within the gap is less than 30 Å.
6. The method according to claim 3, wherein, The post-etching process is performed at approximately 250°C.
7. The method according to claim 1, wherein, The deposition process is performed using CCP plasma, which is generated using a gas mixture at an RF frequency in the range of about 1 MHz to 100 MHz. The gas mixture contains a silicon-containing gas selected from silane (SiH4), disilane (Si2H6), hydrosilane, silicon halide, or organosilicon compounds, as well as one or more other gases including hydrogen (H2), helium (He), and argon (Ar).
8. The method according to claim 1, wherein, The etching process is performed using CCP plasma, which is generated using a gas mixture comprising hydrogen (H2), helium (He) and argon (Ar) at RF frequencies in the range of 1 MHz to 100 MHz.
9. The method according to claim 1, wherein, The nitriding process is performed using CCP plasma, which is generated using a gas mixture comprising nitrogen (N2), ammonia (NH3), hydrogen (H2), and helium (He) at RF frequencies in the range of 1 MHz to 100 MHz.
10. The method according to claim 1, wherein, The etching process and the nitriding process are performed in the same reaction chamber.
11. A method for optimizing the profile of a silicon nitride (SiN) layer, the method comprising: Multiple cycles of a-Si deposition, H2 etching, and nitriding processes are performed. The thickness of the resulting SiN layer was measured after each of the multiple cycles; as well as Adjust process parameters to achieve the desired thickness of the SiN layer.
12. The method according to claim 11, wherein, The process parameters include deposition time, etching duration, and nitriding temperature.
13. The method of claim 11 further comprises performing a DHF post-etching process or an H3PO4 post-etching process to further refine the contour of the SiN layer.
14. The method according to claim 11, wherein, The measurement was performed using a real-time thickness measurement system.
15. The method according to claim 11, wherein, The contours of the SiN layer were monitored using transmission electron microscopy (TEM).
16. The method according to claim 11, wherein, The cycle is repeated at least 10 times.
17. The method according to claim 11, wherein, The cycle is repeated at least 20 times.
18. A semiconductor structure comprising: silicon substrate; as well as A bottom SiN film is formed on a silicon substrate using a cyclic deposition-etch-nitridation process, wherein the bottom SiN film is greater than 150 Å.
19. The semiconductor structure according to claim 18, wherein, The silicon substrate includes multiple gaps, and the bottom SiN film is formed within each gap.
20. The semiconductor structure of claim 18 further includes a gate structure formed on the silicon substrate and adjacent to the bottom SiN film.