Semiconductor structure and its formation method

By forming a stress buffer layer and a stress compensation layer on the back of the wafer, the problem of stress directly acting on the device area in wafer warpage compensation in the prior art is solved, thereby improving stress uniformity and mechanical reliability, and is suitable for ultra-thin wafers in three-dimensional packaging.

CN123124683APending Publication Date: 2026-11-17SWAYSURE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611259217.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the current wafer warpage compensation process of 3D packaging, the front-side thin film stress directly acts on the device area, affecting the electrical performance of the transistor. Furthermore, the uniformity of the thin film stress is difficult to guarantee, which limits the process window. In particular, it is difficult to meet the warpage correction requirements in high aspect ratio stacking scenarios.

Method used

A stress buffer layer and a stress compensation layer are formed on the back side of the wafer. The stress in the stress buffer layer is opposite to the direction of the initial stress and is less than the preset stress. The stress in the stress compensation layer is opposite to the direction of the initial stress and is the preset stress. The sum of the two stresses is less than or equal to the initial stress. A smooth stress transition is achieved through a multi-layer stress gradient structure to avoid stress abrupt changes.

Benefits of technology

It achieves uniformity of wafer stress, avoids the impact of direct stress abrupt changes on device layers, ensures the mechanical reliability and electrical performance of the wafer, and is suitable for stress compensation of ultra-thin wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124683A_ABST
    Figure CN123124683A_ABST
Patent Text Reader

Abstract

A semiconductor structure and a method for forming the same are disclosed. The method includes: providing a wafer including a front side and a back side opposite to each other, wherein a device layer is formed on the front side of the wafer; detecting initial stress on the wafer; forming a stress buffer layer covering the back side of the wafer, wherein the stress in the stress buffer layer is opposite in direction to the initial stress and is less than a preset stress; and forming a stress compensation layer on the stress buffer layer, wherein the stress in the stress compensation layer is opposite in direction to the initial stress and is equal to the preset stress, wherein the sum of the stresses in the stress buffer layer and the stress compensation layer is less than or equal to the initial stress. This disclosure ensures stress uniformity of the wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of semiconductor manufacturing, and more particularly to a semiconductor structure and a method for forming the same. Background Technology

[0002] In 3D (3-Dimentional) packaging technology, wafer bonding is a key process for achieving vertical interconnection of multi-layer chips. Wafer bow (BOW) control, as a necessary step before bonding, directly affects bonding quality and stacking yield. With the continuous increase in the number of stacked layers in devices such as 3D NAND flash memory and high-bandwidth memory (HBM), warpage compensation is required for each wafer layer before bonding.

[0003] Existing warpage compensation processes typically involve dielectric deposition and chemical mechanical polishing (CMP) on the front side of the wafer, using stress in the front-side thin film to control the wafer morphology. However, the stress in the front-side thin film directly affects the device region, potentially negatively impacting transistor electrical performance. Furthermore, the front-side deposition is limited by the presence of device patterns, making it difficult to guarantee the uniformity of film stress, which in turn restricts the CMP process window. Summary of the Invention

[0004] This disclosure provides a semiconductor structure and a method for forming the same, which helps to ensure the stress uniformity of the wafer.

[0005] To address the aforementioned problems, this disclosure provides a method for forming a semiconductor structure, comprising: providing a wafer including a front side and a back side opposite to each other, wherein a device layer is formed on the front side of the wafer; detecting the initial stress of the wafer; forming a stress buffer layer covering the back side of the wafer, wherein the stress in the stress buffer layer is opposite in direction to the initial stress and is less than a preset stress; and forming a stress compensation layer on the stress buffer layer, wherein the stress in the stress compensation layer is opposite in direction to the initial stress and is equal to the preset stress, wherein the sum of the stresses in the stress buffer layer and the stress compensation layer is less than or equal to the initial stress.

[0006] Optionally, in the step of forming a stress buffer layer covering the back side of the wafer, the material of the stress buffer layer includes silicon oxide with tetraethyl orthosilicate as a precursor; in the step of forming a stress compensation layer on the stress buffer layer, the material of the stress compensation layer includes silicon oxide with tetraethyl orthosilicate as a precursor.

[0007] Optionally, the thickness of the wafer is less than or equal to 100 μm.

[0008] Optionally, before forming a stress compensation layer on the stress buffer layer, the method further includes: forming a stress gradient layer covering the stress buffer layer, wherein the stress of the stress gradient layer is opposite in direction to the initial stress and increases from a first stress to a second stress as the thickness increases, the first stress being greater than the stress of the stress buffer layer, and the second stress being less than the preset stress; in the step of forming a stress compensation layer on the stress buffer layer, the stress compensation layer covers the stress gradient layer, and the sum of the stresses of the stress buffer layer, the stress gradient layer, and the stress compensation layer is less than or equal to the initial stress.

[0009] Optionally, in the step of forming a stress gradient layer covering the stress buffer layer, the material of the stress gradient layer includes silicon oxide with tetraethyl orthosilicate as a precursor.

[0010] Optionally, in the step of forming the stress gradient layer covering the stress buffer layer, the stress gradient layer is formed using a plasma-enhanced chemical vapor deposition process, and during the deposition process, the high-frequency power is set to increase incrementally.

[0011] Optionally, after forming a stress compensation layer on the stress buffer layer, the method further includes: forming a stress relief layer covering the stress compensation layer, wherein the stress in the stress relief layer is opposite in direction to the initial stress and is less than the stress in the stress buffer layer, or the stress relief layer has no stress; the stress relief layer is located away from the surface of the wafer to form a bonding surface.

[0012] Optionally, in the step of forming a stress relief layer covering the stress compensation layer, the material of the stress relief layer includes silicon oxide with tetraethyl orthosilicate as a precursor.

[0013] Optionally, after forming a stress compensation layer on the stress buffer layer, the process further includes annealing the stress buffer layer and the stress compensation layer.

[0014] This disclosure also provides a semiconductor structure, including: a wafer, including a front side and a back side opposite to each other, the wafer having an initial stress, and a device layer formed on the front side of the wafer; a stress buffer layer covering the back side of the wafer, the stress in the stress buffer layer being opposite in direction to the initial stress and less than a preset stress; and a stress compensation layer located on the stress buffer layer, the stress in the stress compensation layer being opposite in direction to the initial stress and being the preset stress, the sum of the stresses in the stress buffer layer and the stress compensation layer being less than or equal to the initial stress.

[0015] Optionally, the stress buffer layer is made of silicon oxide with tetraethyl orthosilicate as a precursor; the stress compensation layer is made of silicon oxide with tetraethyl orthosilicate as a precursor.

[0016] Optionally, the thickness of the wafer is less than or equal to 100 μm.

[0017] Optionally, a stress gradient layer is further formed between the stress buffer layer and the stress compensation layer. The stress in the stress gradient layer is opposite in direction to the initial stress and increases from a first stress to a second stress as the thickness increases. The first stress is greater than the stress in the stress buffer layer, and the second stress is less than the preset stress. The sum of the stresses in the stress buffer layer, the stress gradient layer, and the stress compensation layer is less than or equal to the initial stress.

[0018] Optionally, the material of the stress gradient layer includes silicon oxide with tetraethyl orthosilicate as a precursor.

[0019] Optionally, a stress relief layer is also formed on the stress compensation layer, wherein the stress in the stress relief layer is opposite in direction to the initial stress and is less than the stress in the stress buffer layer, or the stress relief layer has no stress; the stress relief layer is located away from the surface of the wafer to form a bonding surface.

[0020] Optionally, the stress relief layer may be made of silicon oxide with tetraethyl orthosilicate as a precursor.

[0021] Compared with the prior art, the technical solution of the present disclosure has the following advantages: In the formation method provided in this embodiment, a device layer is formed on the front side of the wafer, and a stress buffer layer and a stress compensation layer are formed on the back side of the wafer to balance the initial stress of the wafer. The device layer on the front side of the wafer is not affected. The stress of the stress buffer layer is opposite in direction to the initial stress and is less than a preset stress. The stress of the stress compensation layer is opposite in direction to the initial stress and is a preset stress. The sum of the stresses of the stress buffer layer and the stress compensation layer is less than or equal to the initial stress. That is, the stress buffer layer and the stress compensation layer together perform stress compensation on the wafer based on the initial stress. The stress compensation layer has a higher stress. As the main film layer for balancing the initial stress of the wafer, the stress of the stress buffer layer is between the initial stress of the wafer and the high stress of the stress compensation layer, realizing a smooth stress transition. This helps to avoid the stress abrupt change caused by jumping directly from the wafer to the higher stress of the stress compensation layer, thereby achieving better stress compensation on the wafer based on the initial stress and ensuring the stress uniformity of the wafer. Attached Figure Description

[0022] Figures 1 to 7 This is a schematic diagram of the structure corresponding to each step in one embodiment of the method for forming a semiconductor structure disclosed herein; Figure 8 This is a schematic diagram of one embodiment of the semiconductor structure disclosed herein. Detailed Implementation

[0023] As the background technology indicates, in wafer warpage compensation processes, existing techniques typically involve dielectric deposition and chemical mechanical polishing on the front side of the wafer, using front-side thin-film stress to control the wafer morphology. However, front-side thin-film stress directly affects the device region, potentially negatively impacting transistor electrical performance. Furthermore, front-side deposition is limited by the presence of device patterns, making it difficult to guarantee thin-film stress uniformity, thus restricting the process window. Moreover, existing warpage compensation techniques primarily employ single-layer thin-film structures, which have limited stress compensation capabilities, making it difficult to meet the demands of significant warpage correction in high aspect ratio stacking scenarios.

[0024] To address the aforementioned technical problems, this disclosure provides a method for forming a semiconductor structure, comprising: providing a wafer, including a front side and a back side opposite to each other, wherein a device layer is formed on the front side of the wafer; detecting the initial stress of the wafer; forming a stress buffer layer covering the back side of the wafer, wherein the stress in the stress buffer layer is opposite in direction to the initial stress and is less than a preset stress; forming a stress compensation layer on the stress buffer layer, wherein the stress in the stress compensation layer is opposite in direction to the initial stress and is a preset stress, and the sum of the stresses in the stress buffer layer and the stress compensation layer is less than or equal to the initial stress.

[0025] In this embodiment, a device layer is formed on the front side of the wafer, and a stress buffer layer and a stress compensation layer are formed on the back side of the wafer to balance the initial stress of the wafer. The device layer on the front side of the wafer is not affected. The stress in the stress buffer layer is opposite in direction to the initial stress and is less than a preset stress. The stress in the stress compensation layer is opposite in direction to the initial stress and is a preset stress. The sum of the stresses in the stress buffer layer and the stress compensation layer is less than or equal to the initial stress. That is, the stress buffer layer and the stress compensation layer together perform stress compensation on the wafer based on the initial stress. The stress compensation layer has a higher stress. As the main film layer for balancing the initial stress of the wafer, the stress in the stress buffer layer is between the initial stress of the wafer and the high stress of the stress compensation layer, realizing a smooth stress transition. This helps to avoid the stress abrupt change caused by jumping directly from the wafer to the higher stress of the stress compensation layer, thereby achieving better stress compensation on the wafer based on the initial stress and ensuring the stress uniformity of the wafer.

[0026] To make the above-mentioned objects, features and advantages of this disclosure more apparent and understandable, specific embodiments of this disclosure will be described in detail below with reference to the accompanying drawings.

[0027] Figures 1 to 7 This is a schematic diagram of the structure corresponding to each step in one embodiment of the method for forming a semiconductor structure disclosed herein.

[0028] refer to Figure 1 A wafer 100 is provided, including a front side 100a and a back side 100b opposite to each other, wherein a device layer 110 is formed on the front side of the wafer 100.

[0029] Wafer 100 is used as a physical carrier and substrate for the fabrication of semiconductor structures.

[0030] For example, in some embodiments, wafer 100 is typically a monocrystalline silicon wafer.

[0031] Specifically, wafer 100 includes a front side 100a and a back side 100b that are opposite to each other. The front side 100a is typically used to form devices, while the back side 100b is typically used to provide mechanical support during manufacturing and to serve as a processing surface for thinning and interconnection in subsequent packaging stages.

[0032] In some embodiments, the thickness of wafer 100 is less than or equal to 100 μm.

[0033] The thickness of wafer 100 is less than or equal to 100 μm, that is, wafer 100 has a small thickness and is usually an ultra-thin wafer. Ultra-thin wafers have extremely low mechanical strength, and the residual stress in the front 100a device layer 110 can cause wafer 100 to warp more severely. This method is particularly suitable for the formation method disclosed herein to compensate for the stress of ultra-thin wafers.

[0034] In some embodiments, a device layer 110 is formed on the front side of the wafer 100.

[0035] Device layer 110 is used to implement the basic functions of the semiconductor structure.

[0036] refer to Figure 2 Before subsequent detection of the initial stress of wafer 100, a protective layer 120 is formed to cover the device layer 110.

[0037] The protective layer 120 is used to protect the device layer 110 on the front side 100a of the wafer 100 from damage during subsequent processes on the back side 100b of the wafer 100.

[0038] In some embodiments, in the step of forming a protective layer 120 covering the device layer 110, the protective layer 120 is a peelable photoresist or a temporary bonding adhesive, which makes it easy to remove the protective layer 120 subsequently and has little impact on the device layer 110.

[0039] Continue to refer to Figure 2 The initial stress of wafer 100 was detected.

[0040] The initial stress of wafer 100 is detected, and wafer warpage (BOW) compensation is then performed on wafer 100 based on the initial stress.

[0041] Specifically, in some embodiments, the initial stress of wafer 100 can be detected from the back side 100b of wafer 100 or from the front side 100a of wafer 100, and there is no limitation on this.

[0042] As an example, in some embodiments, the initial stress of wafer 100 is detected by the back surface 100b of wafer 100, and the amount and direction of compensation required for the back surface 100b can be determined by the curvature method.

[0043] Specifically, in some embodiments, the direction of the initial stress can be tensile stress, that is, the wafer 100 can have a shape with a concave center and an upturned edge. The direction of the initial stress can also be compressive stress, that is, the wafer 100 can also have a shape with a convex center and an upturned edge.

[0044] Continue to refer to Figure 2 Before forming the stress buffer layer covering the back side 100b of wafer 100, the process also includes cleaning and activating the back side 100b of wafer 100.

[0045] The back side 100b of wafer 100 is cleaned and plasma activated to remove contaminants and the natural oxide layer, and to activate the surface dangling bonds. This provides a clean, chemically active, and strongly adhesive wafer 100 surface for subsequent processes (forming a stress buffer layer covering the back side 100b of wafer 100), ensuring mechanical reliability.

[0046] As an example, in some embodiments, standard cleaning solutions SC1 (Standard Clean 1) and SC2 (Standard Clean 2) are used to clean the back side 100b of wafer 100, and a plasma activation process is used to activate the back side 100b of wafer 100, wherein the plasma is oxygen plasma or nitrogen plasma, the power is 200W to 500W, and the time is 10s to 30s.

[0047] refer to Figure 3 A stress buffer layer 210 is formed covering the back side 100b of the wafer 100. The stress in the stress buffer layer 210 is opposite in direction to the initial stress and is less than the preset stress.

[0048] The preset stress is a stress value preset based on the initial stress, such that after the stress compensation layer with the preset stress is formed, the sum of the stresses of the stress buffer layer and the stress compensation layer is less than or equal to the initial stress.

[0049] The stress in the stress buffer layer 210 is opposite in direction to the initial stress and is less than the preset stress. That is, the stress buffer layer 210 is used to compensate for the stress of the wafer 100. The stress in the stress buffer layer 210 is between the initial stress of the wafer 100 and the high stress of the subsequently formed stress compensation layer, so as to achieve a smooth stress transition. This helps to avoid the stress abrupt change caused by jumping directly from the wafer 100 to the subsequently formed higher stress compensation layer.

[0050] In some embodiments, in the step of forming a stress buffer layer 210 covering the back side 100b of the wafer 100, the material of the stress buffer layer 210 includes silicon oxide with tetraethyl orthosilicate (TEOS) as a precursor.

[0051] The stress buffer layer 210 is formed by using silicon oxide with tetraethyl orthosilicate as a precursor, which makes the stress of the stress buffer layer 210 adjustable, low temperature compatible and mature in process, and easy to form a stress buffer layer 210 with flexible stress control based on preset stress.

[0052] Specifically, in some embodiments, in the step of forming a stress buffer layer 210 covering the back side 100b of the wafer 100, the stress buffer layer 210 is made of medium-density (MD) silicon dioxide with tetraethyl orthosilicate as a precursor.

[0053] The stress buffer layer 210 formed by medium-density silicon oxide with tetraethyl orthosilicate as a precursor has moderate stress, which enables the stress buffer layer 210 to achieve a good stress smooth transition between the wafer 100 and the subsequently formed stress compensation layer, and helps to prevent the stress of the stress buffer layer 210 from being too high, which would lead to a sudden stress change between the wafer 100 and the stress buffer layer 210.

[0054] As an example, in some embodiments, a stress buffer layer 210 covering the back side 100b of wafer 100 is formed using plasma-enhanced chemical vapor deposition (PECVD) at a deposition temperature of 360°C to 400°C. The stress of the formed stress buffer layer 210 is -50 MPa to -80 MPa (i.e., compressive stress), and the thickness of the stress buffer layer 210 is 0.2 μm to 0.5 μm.

[0055] In other embodiments, in the step of forming a stress buffer layer covering the back side of the wafer, the material of the stress buffer layer may also be silicon oxide with silane as a precursor, silicon oxide with tetramethylsilane as a precursor, silicon nitride, or silicon oxynitride.

[0056] refer to Figure 4 Before the stress compensation layer is formed on the stress buffer layer 210, the method further includes: forming a stress gradient layer 220 covering the stress buffer layer 210. The stress in the stress gradient layer 220 is opposite to the direction of the initial stress and increases from the first stress to the second stress as the thickness increases. The first stress is greater than the stress in the stress buffer layer 210, and the second stress is less than the preset stress.

[0057] The stress gradient layer 220 is used together with the stress buffer layer 210 to perform stress compensation on the wafer 100. The stress of the stress gradient layer 220 is opposite to the direction of the initial stress and increases from the first stress to the second stress as the thickness increases, so as to achieve a gradual stress smooth transition from the stress buffer layer 210 to the stress compensation layer formed subsequently.

[0058] In some embodiments, in the step of forming a stress gradient layer 220 covering the stress buffer layer 210, the material of the stress gradient layer 220 includes silicon oxide with tetraethyl orthosilicate as a precursor.

[0059] The stress gradient layer 220 is formed by using silicon oxide with tetraethyl orthosilicate as a precursor, which makes the stress of the stress gradient layer 220 adjustable, low temperature compatible and mature in process, and easy to form a stress gradient layer 220 with flexible stress control based on preset stress.

[0060] In some embodiments, in the step of forming the stress gradient layer 220 covering the stress buffer layer 210, the stress gradient layer 220 is formed by plasma-enhanced chemical vapor deposition, and during the deposition process, the high-frequency power is set to increase.

[0061] In plasma-enhanced chemical vapor deposition (PECVD), the lower the high-frequency power, the more porous the deposited film layer and the lower the stress of the film layer; the higher the high-frequency power, the more compact the deposited film layer and the greater the stress of the film layer. Therefore, during the deposition process, the high-frequency power is set to increase gradually, so that as the deposition thickness increases, the stress of the stress gradient layer 220 gradually increases from the first stress to the second stress.

[0062] As an example, in some embodiments, a stress gradient layer 220 covering the stress buffer layer 210 is formed by plasma-enhanced chemical vapor deposition at a deposition temperature of 350°C to 390°C, an initial high-frequency power of 400W corresponding to a stress of approximately -60MPa (i.e., compressive stress), and a final high-frequency power of 700W corresponding to a stress of approximately -120MPa (i.e., compressive stress). The rate of change of the high-frequency power is 10 W / min to 30 W / min, and the deposition thickness of the stress gradient layer 220 is 0.8 μm to 1.2 μm.

[0063] In other embodiments, in the step of forming the stress gradient layer covering the stress buffer layer, the material of the stress gradient layer may also be silicon oxide with silane as a precursor, silicon oxide with tetramethylsilane as a precursor, silicon nitride, or silicon oxynitride.

[0064] Continue to refer to Figure 4 Before forming a stress compensation layer on the stress buffer layer 210, the process also includes planarizing the stress gradient layer 220.

[0065] The stress gradient layer 220 is planarized to provide a better process platform for the subsequent formation of the stress compensation layer, so that the stress compensation layer and the stress gradient layer 220 are firmly bonded together, ensuring mechanical reliability.

[0066] Specifically, in some embodiments, a chemical mechanical polishing process is used to planarize the stress gradient layer 220.

[0067] As an example, in some embodiments, the stress gradient layer 220 is planarized, such that the thickness of the stress gradient layer 220 is 0.6 μm to 0.8 μm.

[0068] refer to Figure 5 A stress compensation layer 230 is formed on the stress buffer layer 210. The stress in the stress compensation layer 230 is opposite in direction to the initial stress and is a preset stress. The sum of the stresses in the stress buffer layer 210 and the stress compensation layer 230 is less than or equal to the initial stress.

[0069] The stress compensation layer 230 is used together with the stress buffer layer 210 to perform stress compensation on the wafer 100. The stress of the stress compensation layer 230 is opposite in direction to the initial stress and is a preset stress. The sum of the stresses of the stress buffer layer 210 and the stress compensation layer 230 is less than or equal to the initial stress. That is, the stress compensation layer 230 is the main film layer for stress compensation on the wafer 100.

[0070] In some embodiments, a device layer 110 is formed on the front side 100a of the wafer 100. A stress buffer layer 210 and a stress compensation layer 230 are formed on the back side 100b of the wafer 100 to balance the initial stress of the wafer 100. The device layer 110 on the front side 100a of the wafer 100 is not affected. The stress in the stress buffer layer 210 is opposite in direction to the initial stress and less than a preset stress. The stress in the stress compensation layer 230 is opposite in direction to the initial stress and equal to a preset stress. The sum of the stresses in the stress buffer layer 210 and the stress compensation layer 230 is less than or equal to the initial stress. In other words, the stress... The buffer layer 210 and the stress compensation layer 230 together perform stress compensation on the wafer 100 based on the initial stress. The stress compensation layer 230 has a higher stress. As the main film layer for balancing the initial stress of the wafer 100, the stress of the stress buffer layer 210 is between the initial stress of the wafer 100 and the high stress of the stress compensation layer 230, so as to achieve a smooth stress transition. This helps to avoid the stress abrupt change caused by jumping directly from the wafer 100 to the higher stress of the stress compensation layer 230. Thus, it is possible to achieve better stress compensation on the wafer 100 based on the initial stress, thereby ensuring the stress uniformity of the wafer 100.

[0071] In some embodiments, in the step of forming a stress compensation layer 230 on the stress buffer layer 210, the material of the stress compensation layer 230 includes silicon oxide with tetraethyl orthosilicate as a precursor.

[0072] The stress compensation layer 230 is formed by using silicon oxide with tetraethyl orthosilicate as a precursor, which makes the stress of the stress compensation layer 230 adjustable, low temperature compatible and mature in process, and easy to form a stress compensation layer 230 with flexible stress control based on preset stress.

[0073] Specifically, in some embodiments, in the step of forming a stress compensation layer 230 on the stress buffer layer 210, the material of the stress compensation layer 230 is high stress (HS) silicon dioxide with tetraethyl orthosilicate as a precursor.

[0074] The stress compensation layer 230 formed from silicon oxide with tetraethyl orthosilicate as a precursor has high stress, which enables the stress compensation layer 230 to compensate for the stress of wafer 100 to a large extent and achieve stress balance of wafer 100.

[0075] As an example, in some embodiments, a stress compensation layer 230 is formed on the stress buffer layer 210 using plasma-enhanced chemical vapor deposition at a deposition temperature of 300°C to 350°C. The stress of the formed stress compensation layer 230 is -250 MPa to -350 MPa (i.e., compressive stress), and the thickness of the stress compensation layer 230 is 0.8 μm to 1.2 μm.

[0076] In other embodiments, in the step of forming a stress compensation layer on the stress buffer layer, the material of the stress compensation layer may also be silicon oxide with silane as a precursor, silicon oxide with tetramethylsilane as a precursor, silicon nitride, or silicon oxynitride.

[0077] In some embodiments, in the step of forming a stress compensation layer 230 on the stress buffer layer 210, the stress compensation layer 230 covers the stress gradient layer 220, and the sum of the stresses of the stress buffer layer 210, the stress gradient layer 220 and the stress compensation layer 230 is less than or equal to the initial stress.

[0078] The stress buffer layer 210, the stress gradient layer 220 and the stress compensation layer 230 together perform stress compensation on the wafer 100.

[0079] Specifically, the stress buffer layer 210, the stress gradient layer 220, and the stress compensation layer 230 constitute a multi-layer stress gradient structure from lower stress to higher stress, realizing a gradual gradient transition of stress, which is beneficial for flexibly adapting to the compensation stress based on the initial stress and avoiding stress abrupt changes.

[0080] Continue to refer to Figure 5Before the stress relief layer covering the stress compensation layer 230 is formed, the process also includes: planarizing the stress compensation layer 230.

[0081] The stress compensation layer 230 is planarized to provide a better process platform for the subsequent formation of the stress relief layer, so that the stress relief layer and the stress compensation layer 230 are firmly bonded together, ensuring mechanical reliability.

[0082] Specifically, in some embodiments, a chemical mechanical polishing process is used to planarize the stress compensation layer 230.

[0083] As an example, in some embodiments, the stress compensation layer 230 is planarized, such that the thickness of the stress compensation layer 230 is 0.6 μm to 0.8 μm.

[0084] It should be noted that in the steps of forming the stress buffer layer 210, the stress gradient layer 220 and the stress compensation layer 230 on the back side 100a of wafer 100, TEOS silicon oxide material is used. The coefficient of thermal expansion (CTE) of the TEOS silicon oxide film matches that of the silicon substrate (wafer 100). Therefore, even if a thick film of more than 20 μm is deposited, edge delamination will not occur. Moreover, its deposition temperature is relatively low (300°C to 420°C), which can avoid thermal warping of ultrathin wafers.

[0085] refer to Figure 6 After the stress compensation layer 230 is formed on the stress buffer layer 210, the method further includes: forming a stress relief layer 240 covering the stress compensation layer 230, wherein the stress in the stress relief layer 240 is opposite in direction to the initial stress and is less than the stress in the stress buffer layer 210, or the stress relief layer 240 has no stress.

[0086] The stress relief layer 240 is used to release surface stress and improve surface quality after the formation of multiple film layers (stress buffer layer 210, stress gradient layer 220 and stress compensation layer 230).

[0087] In some embodiments, the stress relief layer 240 is located away from the surface of the wafer 100 for forming a bonding surface.

[0088] A low-stress or near-zero-stress stress relief layer 240 is deposited on the stress compensation layer 230 to form a bonding surface, which can release surface stress and thus improve the bonding interface quality.

[0089] In some embodiments, in the step of forming a stress relief layer 240 covering the stress compensation layer 230, the material of the stress relief layer 240 includes silicon oxide with tetraethyl orthosilicate as a precursor.

[0090] The stress relief layer 240 is formed using silicon oxide with tetraethyl orthosilicate as a precursor. This allows for stress controllability, low-temperature compatibility, and a mature process. It is easy to form a stress relief layer 240 with flexible stress control based on a preset stress. Furthermore, other films can be bonded to the stress relief layer 240. In heterogeneous integration bonding (e.g., Si / SiC, Si / GaN), TEOS silicon oxide can serve as a bonding medium layer. After planarization, it has extremely high surface flatness (Ra<0.2nm) and is stress-stable under high-temperature bonding conditions of 400°C, making it less prone to bonding bubbles. At the same time, in the wafer reconstruction process of 3D integrated circuit (3D IC), the back-side TEOS silicon oxide also functions as a stress compensation layer and a laser debonding barrier layer, which can improve the debonding yield to over 99%.

[0091] Specifically, in some embodiments, in the step of forming the stress relief layer 240 covering the stress compensation layer 230, the material of the stress relief layer 240 is medium-density silicon oxide with tetraethyl orthosilicate as a precursor.

[0092] The stress relief layer 240 formed from medium-density silicon dioxide with tetraethyl orthosilicate as a precursor can achieve low stress, or even near-zero stress, which allows the stress relief layer 240 to better release surface stress, thereby improving the bonding interface quality.

[0093] As an example, in some embodiments, a stress relief layer 240 covering the stress compensation layer 230 is formed by plasma-enhanced chemical vapor deposition at a deposition temperature of 360°C to 400°C. The stress of the stress relief layer 240 is -30 MPa to -50 MPa (i.e., compressive stress), and the thickness of the stress relief layer 240 is 0.05 μm to 0.2 μm.

[0094] In other embodiments, in the step of forming the stress relief layer covering the stress compensation layer, the material of the stress relief layer may also be silicon oxide with silane as a precursor, silicon oxide with tetramethylsilane as a precursor, silicon nitride, or silicon oxynitride.

[0095] It should be noted that after the stress relief layer 240 covering the stress compensation layer 230 is formed, the sum of the stresses of the stress buffer layer 210, the stress gradient layer 220, the stress compensation layer 230 and the stress relief layer 240 is less than or equal to the initial stress. The stress buffer layer 210, the stress gradient layer 220, the stress compensation layer 230 and the stress relief layer 240 can be used together to perform stress compensation on the wafer 100.

[0096] Continue to refer to Figure 6Before annealing the stress buffer layer 210 and the stress compensation layer 230, the stress relief layer 240 is further planarized.

[0097] The stress relief layer 240 is planarized to provide a better bonding platform for subsequent bonding on the stress relief layer 240, making the bonding of the stress relief layer 240 with other film layers more stable.

[0098] Specifically, in some embodiments, a chemical mechanical polishing process is used to planarize the stress relief layer 240.

[0099] As an example, in some embodiments, the stress relief layer 240 is planarized, such that the thickness of the stress relief layer 240 is 0.03 μm to 0.15 μm and the surface roughness Ra is ≤0.3 nm.

[0100] Continue to refer to Figure 6 After the stress buffer layer 230 is formed on the stress compensation layer 210, the process further includes annealing the stress buffer layer 210 and the stress compensation layer 230.

[0101] Stress is generated and accumulated during the process. If it is not released by annealing, the stress will affect the device over time during subsequent use. Annealing the stress buffer layer 210 and the stress compensation layer 230 can further balance the stress and release the stress accumulated during the process, thereby further balancing the stress in the semiconductor structure.

[0102] Specifically, in some embodiments, the stress buffer layer 210, stress gradient layer 220, stress compensation layer 230 and stress relief layer 240 are annealed to release the stress accumulated during the process of forming the stress buffer layer 210, stress gradient layer 220, stress compensation layer 230 and stress relief layer 240.

[0103] As an example, in some embodiments, the annealing parameters for the stress buffer layer 210 and the stress compensation layer 230 are: a temperature of 350°C to 400°C, a time of 30 min to 60 min, and a heating / cooling rate of ≤5°C / min.

[0104] refer to Figure 7 After annealing the stress buffer layer 210 and the stress compensation layer 230, the process also includes removing the protective layer 120.

[0105] Remove the protective layer 120 to expose the device layer 110, in preparation for subsequent processes.

[0106] It should be noted that, in some embodiments, after removing the protective layer 120, wafer warpage value can be detected to verify the stress compensation effect.

[0107] It should also be noted that any one of the stress buffer layer 210, stress gradient layer 220, stress compensation layer 230 and stress relief layer 240 can be used as an insulating dielectric layer to form the back interconnect wiring layer of wafer 100.

[0108] Figure 8 This is a schematic diagram of one embodiment of the semiconductor structure disclosed herein.

[0109] refer to Figure 8 The semiconductor structure includes: a wafer 100, including a front side 100a and a back side 100b opposite to each other, the wafer 100 having initial stress, and a device layer 110 formed on the front side 100a of the wafer 100; a stress buffer layer 210 covering the back side 100b of the wafer 100, the stress of the stress buffer layer 210 being opposite in direction to the initial stress and less than a preset stress; and a stress compensation layer 230 located on the stress buffer layer 210, the stress of the stress compensation layer 230 being opposite in direction to the initial stress and being a preset stress, the sum of the stresses of the stress buffer layer 210 and the stress compensation layer 230 being less than or equal to the initial stress.

[0110] Wafer 100 is used as a physical carrier and substrate for the fabrication of semiconductor structures.

[0111] For example, in some embodiments, wafer 100 is typically a monocrystalline silicon wafer.

[0112] Specifically, wafer 100 includes a front side 100a and a back side 100b that are opposite to each other. The front side 100a is typically used to form devices, while the back side 100b is typically used to provide mechanical support during manufacturing and to serve as a processing surface for thinning and interconnection in subsequent packaging stages.

[0113] In some embodiments, the wafer 100 has an initial stress, which is used to compensate for wafer warpage based on the initial stress.

[0114] In some embodiments, the thickness of wafer 100 is less than or equal to 100 μm.

[0115] The thickness of wafer 100 is less than or equal to 100 μm, that is, wafer 100 has a small thickness and is usually an ultra-thin wafer. Ultra-thin wafers have extremely low mechanical strength, and the residual stress in the front 100a device layer 110 can cause wafer 100 to warp more severely. This method is particularly suitable for the formation method disclosed herein to compensate for the stress of ultra-thin wafers.

[0116] In some embodiments, a device layer 110 is formed on the front side of the wafer 100.

[0117] Device layer 110 is used to implement the basic functions of the semiconductor structure.

[0118] In some embodiments, the semiconductor structure further includes a stress buffer layer 210 covering the back side 100b of the wafer 100, wherein the stress in the stress buffer layer 210 is opposite in direction to the initial stress and is less than the preset stress.

[0119] The preset stress is a stress value preset based on the initial stress, such that after the stress compensation layer with the preset stress is formed, the sum of the stresses of the stress buffer layer and the stress compensation layer is less than or equal to the initial stress.

[0120] The stress in the stress buffer layer 210 is opposite in direction to the initial stress and is less than the preset stress. That is, the stress buffer layer 210 is used to compensate for the stress of the wafer 100. The stress in the stress buffer layer 210 is between the initial stress of the wafer 100 and the high stress of the subsequently formed stress compensation layer, so as to achieve a smooth stress transition. This helps to avoid the stress abrupt change caused by jumping directly from the wafer 100 to the subsequently formed higher stress compensation layer.

[0121] In some embodiments, the stress buffer layer 210 is made of silicon oxide with tetraethyl orthosilicate as a precursor.

[0122] The stress buffer layer 210 is formed by using silicon oxide with tetraethyl orthosilicate as a precursor, which makes the stress of the stress buffer layer 210 adjustable, low temperature compatible and mature in process, and easy to form a stress buffer layer 210 with flexible stress control based on preset stress.

[0123] Specifically, in some embodiments, the stress buffer layer 210 is made of medium-density (MD) silicon dioxide with tetraethyl orthosilicate as a precursor.

[0124] The stress buffer layer 210 formed by medium-density silicon oxide with tetraethyl orthosilicate as a precursor has moderate stress, which enables the stress buffer layer 210 to achieve a good stress smooth transition between the wafer 100 and the subsequently formed stress compensation layer, and helps to prevent the stress of the stress buffer layer 210 from being too high, which would lead to a sudden stress change between the wafer 100 and the stress buffer layer 210.

[0125] In other embodiments, the stress buffer layer may also be made of silicon oxide with silane as a precursor, silicon oxide with tetramethylsilane as a precursor, silicon nitride, or silicon oxynitride.

[0126] In some embodiments, a stress gradient layer 220 is further formed between the stress buffer layer 210 and the stress compensation layer 230. The stress in the stress gradient layer 220 is opposite in direction to the initial stress and increases from a first stress to a second stress as the thickness increases. The first stress is greater than the stress in the stress buffer layer 210, and the second stress is less than the preset stress.

[0127] The stress gradient layer 220 is used together with the stress buffer layer 210 to perform stress compensation on the wafer 100. The stress of the stress gradient layer 220 is opposite to the direction of the initial stress and increases from the first stress to the second stress as the thickness increases, so as to achieve a gradual stress smooth transition from the stress buffer layer 210 to the stress compensation layer formed subsequently.

[0128] In some embodiments, the material of the stress gradient layer 220 includes silicon oxide with tetraethyl orthosilicate as a precursor.

[0129] The stress gradient layer 220 is formed by using silicon oxide with tetraethyl orthosilicate as a precursor, which makes the stress of the stress gradient layer 220 adjustable, low temperature compatible and mature in process, and easy to form a stress gradient layer 220 with flexible stress control based on preset stress.

[0130] In other embodiments, in the step of forming the stress gradient layer covering the stress buffer layer, the material of the stress gradient layer may also be silicon oxide with silane as a precursor, silicon oxide with tetramethylsilane as a precursor, silicon nitride, or silicon oxynitride.

[0131] In some embodiments, the semiconductor structure further includes a stress compensation layer 230 located on the stress buffer layer 210, wherein the stress of the stress compensation layer 230 is opposite in direction to the initial stress and is a preset stress, and the sum of the stresses of the stress buffer layer 210 and the stress compensation layer 230 is less than or equal to the initial stress.

[0132] The stress compensation layer 230 is used together with the stress buffer layer 210 to perform stress compensation on the wafer 100. The stress of the stress compensation layer 230 is opposite in direction to the initial stress and is a preset stress. The sum of the stresses of the stress buffer layer 210 and the stress compensation layer 230 is less than or equal to the initial stress. That is, the stress compensation layer 230 is the main film layer for stress compensation on the wafer 100.

[0133] In some embodiments, a device layer 110 is formed on the front side 100a of the wafer 100. A stress buffer layer 210 and a stress compensation layer 230 are formed on the back side 100b of the wafer 100 to balance the initial stress of the wafer 100. The device layer 110 on the front side 100a of the wafer 100 is not affected. The stress in the stress buffer layer 210 is opposite in direction to the initial stress and less than a preset stress. The stress in the stress compensation layer 230 is opposite in direction to the initial stress and equal to a preset stress. The sum of the stresses in the stress buffer layer 210 and the stress compensation layer 230 is less than or equal to the initial stress. In other words, the stress... The buffer layer 210 and the stress compensation layer 230 together perform stress compensation on the wafer 100 based on the initial stress. The stress compensation layer 230 has a higher stress. As the main film layer for balancing the initial stress of the wafer 100, the stress of the stress buffer layer 210 is between the initial stress of the wafer 100 and the high stress of the stress compensation layer 230, so as to achieve a smooth stress transition. This helps to avoid the stress abrupt change caused by jumping directly from the wafer 100 to the higher stress of the stress compensation layer 230. Thus, it is possible to achieve better stress compensation on the wafer 100 based on the initial stress, thereby ensuring the stress uniformity of the wafer 100.

[0134] In some embodiments, the material of the stress compensation layer 230 includes silicon oxide with tetraethyl orthosilicate as a precursor.

[0135] The stress compensation layer 230 is formed by using silicon oxide with tetraethyl orthosilicate as a precursor, which makes the stress of the stress compensation layer 230 adjustable, low temperature compatible and mature in process, and easy to form a stress compensation layer 230 with flexible stress control based on preset stress.

[0136] Specifically, in some embodiments, the stress compensation layer 230 is made of high-stress (HS) silicon dioxide with tetraethyl orthosilicate as a precursor.

[0137] The stress compensation layer 230 formed from silicon oxide with tetraethyl orthosilicate as a precursor has high stress, which enables the stress compensation layer 230 to compensate for the stress of wafer 100 to a large extent and achieve stress balance of wafer 100.

[0138] In other embodiments, the material of the stress compensation layer may also be silicon oxide with silane as a precursor, silicon oxide with tetramethylsilane as a precursor, silicon nitride, or silicon oxynitride.

[0139] In some embodiments, the stress buffer layer 210, the stress gradient layer 220, and the stress compensation layer 230 are stacked sequentially, and the sum of the stresses of the stress buffer layer 210, the stress gradient layer 220, and the stress compensation layer 230 is less than or equal to the initial stress.

[0140] The stress buffer layer 210, the stress gradient layer 220 and the stress compensation layer 230 together perform stress compensation on the wafer 100.

[0141] Specifically, the stress buffer layer 210, the stress gradient layer 220, and the stress compensation layer 230 constitute a multi-layer stress gradient structure from lower stress to higher stress, realizing a gradual gradient transition of stress, which is beneficial for flexibly adapting to the compensation stress based on the initial stress and avoiding stress abrupt changes.

[0142] In some embodiments, a stress relief layer 240 is also formed on the stress compensation layer 230, wherein the stress of the stress relief layer 240 is opposite in direction to the initial stress and is less than the stress of the stress buffer layer 210, or the stress relief layer 240 has no stress.

[0143] The stress relief layer 240 is used to release surface stress and improve surface quality after the formation of multiple film layers (stress buffer layer 210, stress gradient layer 220 and stress compensation layer 230).

[0144] In some embodiments, the stress relief layer 240 is located away from the surface of the wafer 100 for forming a bonding surface.

[0145] A low-stress or near-zero-stress stress relief layer 240 is deposited on the stress compensation layer 230 to form a bonding surface, which can release surface stress and thus improve the bonding interface quality.

[0146] In some embodiments, the material of the stress relief layer 240 includes silicon oxide with tetraethyl orthosilicate as a precursor.

[0147] The stress relief layer 240 is formed using silicon oxide with tetraethyl orthosilicate as a precursor. This allows for stress controllability, low-temperature compatibility, and a mature process. It is easy to form a stress relief layer 240 with flexible stress control based on a preset stress. Furthermore, other films can be bonded to the stress relief layer 240. In heterogeneous integration bonding (e.g., Si / SiC, Si / GaN), TEOS silicon oxide can serve as a bonding medium layer. After planarization, it has extremely high surface flatness (Ra<0.2nm) and is stress-stable under high-temperature bonding conditions of 400°C, making it less prone to bonding bubbles. At the same time, in the wafer reconstruction process of 3D IC, the back-side TEOS silicon oxide also functions as a stress compensation layer and a laser debonding barrier layer, which can improve the debonding yield to over 99%.

[0148] Specifically, in some embodiments, the stress relief layer 240 is made of medium-density silicon dioxide with tetraethyl orthosilicate as a precursor.

[0149] The stress relief layer 240 formed from medium-density silicon dioxide with tetraethyl orthosilicate as a precursor can achieve low stress, or even near-zero stress, which allows the stress relief layer 240 to better release surface stress, thereby improving the bonding interface quality.

[0150] In other embodiments, the stress relief layer may also be made of silicon oxide with silane as a precursor, silicon oxide with tetramethylsilane as a precursor, silicon nitride, or silicon oxynitride.

[0151] It should be noted that the sum of the stresses of the stress buffer layer 210, stress gradient layer 220, stress compensation layer 230 and stress relief layer 240 is less than or equal to the initial stress. The stress buffer layer 210, stress gradient layer 220, stress compensation layer 230 and stress relief layer 240 can be used together to perform stress compensation on the wafer 100.

[0152] It should also be noted that the semiconductor structure of this embodiment can be formed using the formation method of the aforementioned embodiments, or it can be formed using other methods.

[0153] While the above disclosure is provided, it is not limited thereto. Any person skilled in the art may make various alterations and modifications without departing from the spirit and scope of this disclosure; therefore, the scope of protection of this disclosure shall be determined by the scope defined in the claims.

Claims

1. A method for forming a semiconductor structure, characterized in that, include: A wafer is provided, including a front side and a back side opposite to each other, wherein a device layer is formed on the front side of the wafer; Detect the initial stress of the wafer; A stress buffer layer is formed covering the back side of the wafer, wherein the stress in the stress buffer layer is opposite in direction to the initial stress and is less than a preset stress; A stress compensation layer is formed on the stress buffer layer, wherein the stress in the stress compensation layer is opposite in direction to the initial stress and is the preset stress, and the sum of the stresses in the stress buffer layer and the stress compensation layer is less than or equal to the initial stress.

2. The forming method as described in claim 1, characterized in that, In the step of forming a stress buffer layer covering the back side of the wafer, the material of the stress buffer layer includes silicon oxide with tetraethyl orthosilicate as a precursor; In the step of forming a stress compensation layer on the stress buffer layer, the material of the stress compensation layer includes silicon oxide with tetraethyl orthosilicate as a precursor.

3. The forming method as described in claim 2, characterized in that, The thickness of the wafer is less than or equal to 100 μm.

4. The forming method as described in claim 1, characterized in that, Before forming a stress compensation layer on the stress buffer layer, the method further includes: forming a stress gradient layer covering the stress buffer layer, wherein the stress of the stress gradient layer is opposite in direction to the initial stress and increases from a first stress to a second stress as the thickness increases, wherein the first stress is greater than the stress of the stress buffer layer and the second stress is less than the preset stress; In the step of forming a stress compensation layer on the stress buffer layer, the stress compensation layer covers the stress gradient layer, and the sum of the stresses of the stress buffer layer, the stress gradient layer, and the stress compensation layer is less than or equal to the initial stress.

5. The forming method as described in claim 4, characterized in that, In the step of forming a stress gradient layer covering the stress buffer layer, the material of the stress gradient layer includes silicon oxide with tetraethyl orthosilicate as a precursor.

6. The forming method as described in claim 4, characterized in that, In the step of forming the stress gradient layer covering the stress buffer layer, the stress gradient layer is formed by plasma-enhanced chemical vapor deposition, and during the deposition process, the high-frequency power is set to increase.

7. The forming method as described in claim 1, characterized in that, After forming a stress compensation layer on the stress buffer layer, the method further includes: forming a stress relief layer covering the stress compensation layer, wherein the stress in the stress relief layer is opposite in direction to the initial stress and is less than the stress in the stress buffer layer, or the stress relief layer has no stress. The stress relief layer is located away from the surface of the wafer to form a bonding surface.

8. The forming method as described in claim 7, characterized in that, In the step of forming a stress relief layer covering the stress compensation layer, the material of the stress relief layer includes silicon oxide with tetraethyl orthosilicate as a precursor.

9. The forming method as described in claim 1, characterized in that, After forming a stress compensation layer on the stress buffer layer, the process further includes annealing the stress buffer layer and the stress compensation layer.

10. A semiconductor structure, characterized in that, include: A wafer, including a front side and a back side opposite to each other, the wafer having initial stress, and a device layer formed on the front side of the wafer; A stress buffer layer is applied to the back side of the wafer, wherein the stress in the stress buffer layer is opposite in direction to the initial stress and is less than a preset stress; A stress compensation layer is located on the stress buffer layer. The stress in the stress compensation layer is opposite in direction to the initial stress and is the preset stress. The sum of the stresses in the stress buffer layer and the stress compensation layer is less than or equal to the initial stress.

11. The semiconductor structure as claimed in claim 10, characterized in that, The stress buffer layer is made of silicon dioxide with tetraethyl orthosilicate as a precursor. The stress compensation layer is made of silicon oxide with tetraethyl orthosilicate as a precursor.

12. The semiconductor structure as claimed in claim 11, characterized in that, The thickness of the wafer is less than or equal to 100 μm.

13. The semiconductor structure as described in claim 10, characterized in that, A stress gradient layer is also formed between the stress buffer layer and the stress compensation layer. The stress in the stress gradient layer is opposite to the direction of the initial stress and increases from the first stress to the second stress as the thickness increases. The first stress is greater than the stress in the stress buffer layer, and the second stress is less than the preset stress. The sum of the stresses in the stress buffer layer, the stress gradient layer, and the stress compensation layer is less than or equal to the initial stress.

14. The semiconductor structure as described in claim 13, characterized in that, The material of the stress gradient layer includes silicon oxide with tetraethyl orthosilicate as a precursor.

15. The semiconductor structure as claimed in claim 10, characterized in that, A stress relief layer is also formed on the stress compensation layer. The stress in the stress relief layer is opposite in direction to the initial stress and is less than the stress in the stress buffer layer. Alternatively, the stress relief layer may not have any stress. The stress relief layer is located away from the surface of the wafer to form a bonding surface.

16. The semiconductor structure as claimed in claim 15, characterized in that, The stress relief layer is made of silicon dioxide with tetraethyl orthosilicate as a precursor.