Method for forming self-aligned pattern, semiconductor device and method for forming the same
By setting silicon oxynitride thin film layers with different oxygen-nitrogen ratios in the self-aligned dual patterning process, the micro-load effect caused by insufficient etching selectivity is solved, and the critical size uniformity of the self-aligned pattern and the improvement of the electrical performance of the semiconductor device are achieved.
Patent Information
- Application Number
- CN202611111913.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-24
- Publication Date
- 2026-11-17
AI Technical Summary
In the self-aligned dual patterning process, insufficient etching selectivity of the silicon oxynitride thin film layer leads to micro-load effect, which affects the uniformity of local critical dimensions after hard mask pattern transfer, and thus affects the electrical performance of semiconductor devices.
By setting silicon oxynitride thin films of the same type but different oxygen-nitrogen ratios in the first and second material layers in the stack to be etched, a natural etching selectivity barrier is constructed by utilizing the difference in oxygen-nitrogen ratio. This ensures that the selectivity of the etching process for the second and first material layers is greater than a preset threshold, thus avoiding over-etching of the underlying material layers.
It effectively eliminates the micro-load effect, ensures the critical dimension uniformity of the self-aligned pattern, and improves the accuracy of hard mask pattern transfer and the electrical performance of semiconductor devices.
Smart Images

Figure CN123124765A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor technology, and to, but is not limited to, a method for forming a self-aligned pattern, a semiconductor device, and a method for forming the same. Background Technology
[0002] With the development of semiconductor technology, Self-Aligned Double Patterning (SADP) is commonly used in the patterning of high-density semiconductor devices such as phase-change memories (PCMs). In the SADP process, to ensure the final device performance, it is necessary to control the local critical dimension uniformity (LCDU) after hard mask pattern transfer. However, in PCM manufacturing, SADP typically requires the use of dielectric thin films such as silicon oxynitrides (SiON) as the mask structure for pattern transfer. In the stack to be etched, the same type of SiON thin film material is often deposited above and below the intermediate carbon layer. When performing removal processes such as mandrel etching after deposition, the etching rate difference between the two adjacent SiON thin films is small due to their similar physicochemical properties. This results in the etching selectivity between the two SiON thin films not being effectively increased during the etching process.
[0003] Due to insufficient interlayer etching selectivity, excessive etching occurs on the lower film during the removal of the upper film, leading to a micro-loading effect between adjacent spaces. This micro-loading effect results in poor local critical dimension uniformity (LCDU) after subsequent hard mask pattern transfer (HM transfer), thus affecting the electrical performance of the device. Therefore, a self-aligned pattern formation method is still needed to improve the micro-loading effect during etching and enhance the critical dimension uniformity of the pattern. Summary of the Invention
[0004] This application provides a method for forming a self-aligned pattern, a semiconductor device, and the method thereof, which can effectively reduce the load effect of adjacent patterns during the etching process and improve the critical dimension uniformity of the final self-aligned pattern.
[0005] The technical solution of this application embodiment is implemented as follows: This application provides a method for forming a self-aligned pattern, comprising: sequentially forming a first material layer, an intermediate carbon layer, a second material layer, and a core mold layer on a stack to be etched; wherein the first material layer and the second material layer have the same type of material, and the oxygen-nitrogen ratio of the first material layer and the second material layer is different; based on the core mold pattern of the core mold layer, etching the second material layer and the intermediate carbon layer to form a patterned stack; the patterned stack includes the second material layer and the intermediate carbon layer; forming a sidewall material layer on the surface of the patterned stack; etching the horizontal sidewall material layer to form a sidewall structure located outside the patterned stack; removing the patterned stack by an etching process to form the self-aligned pattern; wherein the etching process has an etching selectivity ratio between the second material layer and the first material layer that is greater than a preset etching selectivity ratio threshold.
[0006] In the above scheme, the materials of the first material layer and the second material layer are silicon oxynitride.
[0007] In the above scheme, the step of sequentially forming a first material layer, an intermediate carbon layer, a second material layer, and a core mold layer on the stack to be etched includes: sequentially forming a silicon oxynitride layer having a first concentration of oxygen atoms or a first concentration of nitrogen atoms, the intermediate carbon layer, the second material layer having a basic concentration of oxygen atoms and nitrogen atoms, and the core mold layer on the stack to be etched; the first concentration is greater than the basic concentration.
[0008] In the above scheme, the step of sequentially forming a first material layer, an intermediate carbon layer, a second material layer, and a core mold layer on the stack to be etched includes: sequentially forming a first material layer having a basic concentration of oxygen atoms and nitrogen atoms, the intermediate carbon layer, a silicon oxynitride layer having a second concentration of oxygen atoms or nitrogen atoms, and the core mold layer on the stack to be etched; the second concentration is greater than the basic concentration.
[0009] In the above scheme, the step of sequentially forming a first material layer, an intermediate carbon layer, a second material layer, and a core mold layer on the stack to be etched includes: sequentially forming a silicon oxynitride layer with a third concentration of oxygen atoms, the intermediate carbon layer, a silicon oxynitride layer with a fourth concentration of nitrogen atoms, and the core mold layer on the stack to be etched; or, sequentially forming a silicon oxynitride layer with a fifth concentration of nitrogen atoms, the intermediate carbon layer, a silicon oxynitride layer with a sixth concentration of oxygen atoms, and the core mold layer on the stack to be etched; wherein the third concentration, the fourth concentration, the fifth concentration, and the sixth concentration are all greater than a specific base concentration.
[0010] In the above scheme, etching the sidewall material layer in the horizontal direction to form a sidewall structure located outside the patterned stack includes: etching the sidewall material layer in the horizontal direction, retaining the sidewall material layer perpendicular to the surface of the stack to be etched, and forming a sidewall structure located outside the patterned stack.
[0011] In the above scheme, the preset etching selectivity threshold is used to define the etching selectivity critical value for removing the second material layer and retaining the first material layer during the process of removing the patterned stack.
[0012] In the above scheme, after removing the patterned stack, the method further includes: using the self-aligned pattern as a mask, performing hard mask pattern transfer on the stack to be etched to form a hard mask pattern.
[0013] This application provides a method for forming a semiconductor device, wherein the method employs the self-aligned pattern forming method described in any one of the above claims to form a self-aligned pattern and perform pattern transfer.
[0014] This application provides a semiconductor device, which is prepared using the semiconductor device formation method described above.
[0015] The above solution has the following beneficial effects: In this embodiment, a first material layer and a second material layer formed of the same type of material are provided in the stack to be etched, and the oxygen-nitrogen ratio of the first material layer and the second material layer are specifically made different. The difference in the oxygen-nitrogen ratio endows the same type of material with different etching rate characteristics, thereby successfully constructing a natural barrier boundary in the process of removing the patterned stack. At the same time, when removing the patterned stack containing part of the second material layer and part of the intermediate carbon layer by etching process, the above-mentioned difference in oxygen-nitrogen ratio makes the etching selectivity ratio of the second material layer and the first material layer greater than the preset etching selectivity ratio threshold. This high selectivity etching operation that meets the threshold requirement provides sufficient physical protection for the bottom first material layer, and can effectively ensure that the upper second material layer is removed accurately while the lower first material layer is preserved without damage. Furthermore, by widening the etching selectivity between layers of similar materials, the micro-loading effect at the spacing between adjacent patterns and the excessive erosion defects of the underlying structure are effectively avoided. The removal scheme based on the high etching selectivity ensures the high consistency and integrity of the preserved structural morphology, thereby ensuring the high fidelity of the target pattern boundary and ultimately improving the local critical dimension uniformity of the formed self-aligned pattern. Attached Figure Description
[0016] Figure 1A This is a schematic cross-sectional view of the structure after the core mold layer is formed in the related technology; Figure 1B This is a schematic diagram of the cross-sectional view of the structure after patterned layering is formed in related technologies; Figure 1C This is a schematic cross-sectional view of the structure after the sidewall material layer has been formed in the relevant technology; Figure 1D This is a schematic diagram of the structural cross-section after the sidewall material layer is etched to form the sidewall in the related technology; Figure 1E This is a schematic cross-sectional view of the structure after removing the pattern of the second material layer in the related technology; Figure 1F This is a schematic diagram of the cross-sectional structure after etching the first material layer in related technologies; Figure 2 This is a schematic flowchart of a method for forming a self-aligned pattern provided in an embodiment of this application; Figure 3A This is a schematic cross-sectional view of the structure after the core mold layer is formed in the first embodiment of this application; Figure 3B This is a schematic cross-sectional view of the structure after the patterned stack is formed in the first embodiment of this application; Figure 3C This is a schematic cross-sectional view of the structure after the sidewall material layer is formed in the first embodiment of this application; Figure 3D This is a schematic cross-sectional view of the structure after the sidewall structure is formed in the first embodiment of this application; Figure 3E This is a schematic cross-sectional view of the structure after removing the pattern of the second material layer in the first embodiment of this application; Figure 3F This is a schematic cross-sectional view of the structure after completely removing the patterned overlays to form a self-aligned pattern in the first embodiment of this application; Figure 4A This is a schematic cross-sectional view of the structure after the core mold layer is formed in the second embodiment of this application; Figure 4B This is a schematic cross-sectional view of the structure after the patterned stack is formed in the second embodiment of this application; Figure 4C This is a schematic cross-sectional view of the structure after the sidewall material layer is formed in the second embodiment of this application; Figure 4D This is a schematic cross-sectional view of the structure after the sidewall structure is formed in the second embodiment of this application; Figure 4E This is a schematic cross-sectional view of the structure after removing the pattern of the second material layer in the second embodiment of this application; Figure 4F This is a schematic cross-sectional view of the structure after completely removing the patterned overlays to form a self-aligned pattern in the second embodiment of this application. Detailed Implementation
[0017] To make the objectives, technical solutions, and advantages of this application clearer, the application will be further described in detail below with reference to the accompanying drawings. The described embodiments should not be regarded as limitations on this application. All other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0018] In the accompanying drawings, for clarity, the dimensions of layers, areas, and elements, as well as their relative dimensions, may be exaggerated. The same reference numerals denote the same elements throughout.
[0019] It should be understood that when an element or layer is referred to as "on," "adjacent to," "connected to," or "coupled to" other elements or layers, it may be directly on, adjacent to, connected to, or coupled to other elements or layers, or there may be intervening elements or layers. Conversely, when an element is referred to as "directly on," "directly adjacent to," "directly connected to," or "directly coupled to" other elements or layers, there are no intervening elements or layers. It should be understood that although the terms first, second, third, etc., may be used to describe various elements, components, areas, layers, and / or portions, these elements, components, areas, layers, and / or portions should not be limited by these terms. These terms are only used to distinguish one element, component, area, layer, or portion from another element, component, area, layer, or portion. Therefore, without departing from the teachings of the embodiments of this application, the first element, component, area, layer, or portion discussed below may be referred to as a second element, component, area, layer, or portion. And when a second element, component, area, layer, or portion is discussed, it does not indicate that the embodiments of this application necessarily contain a first element, component, area, layer, or portion.
[0020] Spatial relation terms such as “below,” “under,” “below,” “below,” “above,” “above,” etc., are used herein for convenience of description to describe the relationship between one element or feature shown in the figure and other elements or features. It should be understood that, in addition to the orientation shown in the figure, spatial relation terms are intended to also include different orientations of the device in use and operation. For example, if the device in the figure is flipped, then the element or feature described as “below” or “below” other elements or features will be oriented “above” other elements or features. Therefore, the exemplary terms “below” and “under” can include both upper and lower orientations. The device may be otherwise oriented (rotated 90 degrees or otherwise) and the spatial descriptive terms used herein will be interpreted accordingly.
[0021] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the embodiments of this application. When used herein, the singular forms “a,” “an,” and “the” are also intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the terms “compose” and / or “comprising,” when used in this specification, identify the presence of the stated features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups. When used herein, the term “and / or” includes any and all combinations of the associated listed items.
[0022] To fully understand the embodiments of this application, detailed steps and structures will be presented in the following description to illustrate the technical solutions of the embodiments of this application. Preferred embodiments of this application are described in detail below; however, in addition to these detailed descriptions, the embodiments of this application may have other implementation methods.
[0023] Among related technologies, Self-Aligned Double Patterning (SADP) offers the ability to overcome optical resolution limitations and significantly increase pattern density compared to traditional single-exposure lithography. By generating sidewalls on the sidewalls of the mandrel pattern and removing the mandrel, SADP can halve the pattern spacing within the capabilities of existing lithography equipment, thus finding widespread application in the pattern fabrication of high-density semiconductor devices such as phase-change memories. The core mask structure of SADP typically includes a mandrel layer, sidewall material layers, and underlying multilayer hard mask dielectrics. To form extremely fine micro-circuit arrays, related technologies typically form the aforementioned composite thin films sequentially on the layers to be etched, then form sidewalls through deposition and etch-back processes, selectively etch away excess sacrificial layer material, and finally use the remaining sidewall structure as a self-aligned pattern to achieve precise hard mask pattern transfer to the next layer.
[0024] Figures 1A to 1F This is a schematic diagram of the process flow for Self-Aligned Double Patterning (SADP) technology in related fields. For example... Figure 1A As shown, the layers to be etched using the SADP process, from bottom to top, are: a silicon nitride (SiN) layer 101, a diamond-like carbon (DLC) layer 102, a first material layer 103, a spin-coated carbon (SOC) layer 104, and a second material layer 105. The first material layer 103 and the second material layer 105 are of the same material type. A patterned mandrel layer 106 is formed on the second material layer 105. Figure 1BAs shown, using the core mold layer 106 as a mask, the pattern is transferred to the underlying second material layer 105 and spin-coated carbon layer 104 through an etching process. After etching, the second material layer pattern 105a and the spin-coated carbon layer pattern 104a are formed. Figure 1C As shown, an oxide film of uniform thickness (ALD oxide) is deposited on the surface and sides of the second material layer pattern 105a and the spin-coated carbon layer pattern 104a, as well as on the exposed surface of the first material layer 103, using atomic layer deposition (ALD) technology. This film is referred to as the sidewall material layer 107. Figure 1D As shown, the sidewall material layer 107 formed in the previous step is etched using an etching process. After etching, the horizontal sidewall material layer 107 parallel to the surface direction of the stack is etched away. Due to the geometric effect of the pattern sidewalls, the sidewall material deposited on both sides of the second material layer pattern 105a and the spin-coated carbon layer pattern 104a will remain, forming vertical sidewalls 108 (spacers). Figure 1E As shown, the second material layer pattern 105a between the sidewalls 108 is removed by an etching process. During this process, the etching needs to stop at the bottom first material layer 103. However, since the second material layer 105 and the first material layer 103 are both of the same type of material with similar physicochemical properties, their etching selectivity cannot be effectively differentiated. Therefore, when removing the second material layer pattern 105a, it is very easy to cause varying degrees of over-etching to the underlying first material layer 103, resulting in a micro-loading effect between adjacent spaces. Finally, as... Figure 1F As shown, the residual spin-coated carbon layer pattern 104a is removed. Then, using the remaining sidewall 108 as a mask, the underlying first material layer 103 is etched, transferring the pattern to the first material layer 103 and exposing the underlying diamond-like carbon layer 102. However, due to the micro-loading effect generated between adjacent spaces during the previous mandrel etching process, this directly leads to poor local critical dimension uniformity (LCDU) after hard mask pattern transfer (HM transfer), thus affecting the electrical performance of the final device.
[0025] Therefore, embodiments of this application provide a method for forming a self-aligned pattern, such as... Figure 2 As shown, the procedure includes the following steps S101 to S105: S101, a first material layer, an intermediate carbon layer, a second material layer and a core mold layer are sequentially formed on the stack to be etched.
[0026] Here, the first material layer and the second material layer are made of the same type of material, but the oxygen-nitrogen ratio of the first material layer and the second material layer is different.
[0027] In some embodiments, the materials of the first and second material layers are silicon oxynitrides. To clearly illustrate the complete formation process of the self-aligned pattern of this application, the following describes... Figures 3A to 3F Please provide a detailed explanation.
[0028] In some embodiments, step S101 can be implemented by: sequentially forming a silicon oxynitride layer having a first concentration of oxygen atoms or a first concentration of nitrogen atoms, an intermediate carbon layer, a second material layer having a basic concentration of oxygen atoms and nitrogen atoms, and a core mold layer on the stack to be etched.
[0029] like Figure 3A As shown, on the etchable stack consisting of a silicon nitride layer 201, a diamond-like carbon layer 202, etc., a silicon oxynitride layer 203 with a first concentration of oxygen atoms or a first concentration of nitrogen atoms is sequentially formed, followed by an intermediate carbon layer 204, a second material layer 205 with a basic concentration of oxygen atoms and nitrogen atoms, and a patterned core mold layer 206. It is worth noting that the basic concentration refers to the standard stoichiometry of a conventional silicon oxynitride layer in semiconductor manufacturing (i.e., the oxygen and nitrogen atom concentrations determined under conventional deposition ratios). A first concentration greater than the basic concentration means that the percentage of oxygen atoms inside the silicon oxynitride layer 203 is higher than the basic oxygen atom concentration in the second material layer 205 by adjusting deposition process parameters (e.g., gas flow rate ratio), thus achieving an oxygen-rich state (O-Rich); or the percentage of nitrogen atoms inside the silicon oxynitride layer 203 is higher than the basic nitrogen atom concentration in the second material layer 205, thus achieving a nitrogen-rich state (N-Rich).
[0030] By setting the aforementioned concentration difference, the second material layer 205 maintains the conventional properties of the base concentration, while the silicon oxynitride layer 203 is in an oxygen-rich or nitrogen-rich state at the first concentration. This results in the silicon oxynitride layer 203 and the second material layer 205, although both belong to silicon oxynitrides, having completely different properties, thereby widening the etching selectivity ratio between the two similar films in the subsequent reactive ion etching environment.
[0031] S102, based on the core pattern of the core mold layer, the second material layer and the intermediate carbon layer are etched to form a patterned stack.
[0032] Here, the patterned stack includes a portion of the second material layer and a portion of the intermediate carbon layer. Specifically, as shown... Figure 3BAs shown, the core mold layer 206 is used as a mask to etch downwards to form a patterned stack containing a second material layer pattern 205a and an intermediate carbon layer pattern 204a. The core mold layer 206 is usually consumed or removed in this process.
[0033] S103, forming a sidewall material layer on the surface of the patterned stack.
[0034] like Figure 3C As shown, an atomic layer deposition technique can be used to conformally deposit a thin film of uniform thickness on the top surface and sidewalls of the second material layer pattern 205a and the intermediate carbon layer pattern 204a, as well as on the surface of the exposed silicon oxynitride layer 203, as a sidewall material layer 207.
[0035] S104, etch the horizontal sidewall material layer to form a sidewall structure located outside the patterned stack.
[0036] In some embodiments, step S104 can be implemented by etching the sidewall material layer in the horizontal direction, retaining the sidewall material layer perpendicular to the surface of the stack to be etched, thus forming a sidewall structure located outside the patterned stack. For example... Figure 3D As shown, the sidewall material layer 207 is etched by anisotropic etching process, removing the sidewall material in the horizontal direction parallel to the surface of the silicon oxynitride layer 203. The sidewall material deposited on both sides of the patterned stack is retained, forming a vertical sidewall 208.
[0037] S105 uses an etching process to remove patterned layers to form a self-aligned pattern.
[0038] Here, the etching process selectivity ratio between the second material layer and the first material layer is greater than a preset etching selectivity ratio threshold. The preset etching selectivity ratio threshold is used to define the critical etching selectivity ratio value for removing the second material layer while retaining the first material layer during the removal of the patterned stack.
[0039] Specifically, such as Figure 3EAs shown, the second material layer pattern 205a between the sidewalls 208 can be removed using a mandrel pull process. Since the second material layer pattern 205a uses a base concentration of silicon oxynitride, while the exposed silicon oxynitride layer 203 below uses a first concentration (oxygen-rich or nitrogen-rich) of silicon oxynitride, the difference in composition results in completely different etching rates for the two. A high etching selectivity that meets the preset etching selectivity threshold ensures that when removing the upper second material layer pattern 205a, the exposed silicon oxynitride layer 203 at the bottom of the adjacent space is protected from over-etching and remains intact, thus avoiding the micro-loading effect caused by similar etching rates in different pattern density regions.
[0040] In some embodiments, after step S105, the following operations may be performed: using a self-aligned pattern as a mask, a hard mask pattern transfer is performed on the stack to be etched to form a hard mask pattern.
[0041] like Figure 3F As shown, the intermediate carbon layer pattern 204a can be further removed. At this point, the patterned stack is completely removed, leaving only sidewalls 208 on the silicon oxynitride layer 203. These sidewalls 208 constitute the desired self-aligned pattern. Subsequently, using the remaining sidewalls 208 as a mask, the underlying stack to be etched (such as the silicon oxynitride layer 203, diamond-like carbon layer 202, etc.) can be etched downwards to achieve hard mask pattern transfer. Thanks to the elimination of the micro-load effect in step S105, the surface morphology of the silicon oxynitride layer 203 is completely protected during the core removal process, thereby enabling the pattern obtained after the final hard mask pattern transfer to have excellent local critical dimension uniformity (LCDU).
[0042] As can be seen from the above implementation process, the self-aligned pattern formation method provided in this application's embodiments uses process control to make the upper and lower layers of the same material (such as silicon oxynitride) have different compositions, utilizing the difference in oxygen and nitrogen concentrations to construct a natural etching selectivity barrier. Based on this same inventive concept, in order to adapt to the process requirements of different process nodes or specific production equipment, this application's embodiments also provide two other implementation methods: namely, during the film formation process of the material layer, a second material layer with a higher concentration of oxygen or nitrogen atoms is generated by controlling the process conditions (second implementation method); or a first material layer and a second material layer with a significant difference in oxygen-nitrogen ratio are directly generated during the deposition stage (third implementation method), thereby achieving the same inventive objective. These two implementation methods will be described in detail below.
[0043] First, combined Figures 4A to 4FThe second implementation method will be described in detail below. In some embodiments, the above step S101 can be implemented in the following way: on the stack to be etched, a first material layer having a basic concentration of oxygen atoms and nitrogen atoms, an intermediate carbon layer, a silicon oxynitride layer having a second concentration of oxygen atoms or nitrogen atoms, and a core mold layer are formed sequentially.
[0044] like Figure 4A As shown, on the etchable stack consisting of a silicon nitride layer 301, a diamond-like carbon layer 302, etc., a first material layer 303 maintaining the basic concentration is sequentially formed, an intermediate carbon layer 304 is formed, a silicon oxynitride layer 305 is formed, and a patterned core mold layer 306 is formed. Here, during the film formation process, the concentration of oxygen or nitrogen atoms inside the silicon oxynitride layer 305 (i.e., the second concentration) is controlled to be greater than the basic concentration by controlling the process conditions, thereby presenting an oxygen-rich or nitrogen-rich state.
[0045] like Figures 4B to 4D As shown, the subsequent patterned layering and sidewall structure formation process is basically the same in principle and process as the first implementation method mentioned above, and is briefly described here: Figure 4B As shown (corresponding to step S102), the core mold layer 306 is used as a mask for etching downwards to transfer the pattern to the underlying material layer, thereby forming a patterned stack containing a second material layer pattern 305a and an intermediate carbon layer pattern 304a. The core mold layer 306 is typically consumed or removed during this etching process. Figure 4C As shown (corresponding to step S103), a thin film of uniform thickness is conformally deposited on the top surface and sidewalls of the second material layer pattern 305a and the intermediate carbon layer pattern 304a, as well as on the exposed surface of the first material layer 303, using a deposition technique, as the sidewall material layer 307. Figure 4D As shown (corresponding to step S104), the sidewall material layer 307 is etched back using an anisotropic etching process, removing the horizontal sidewall material and retaining the material on both sides of the patterned stack, thereby forming the vertical sidewall 308. Figure 4E As shown (corresponding to step S105), the second material layer pattern 305a between the sidewalls 308 is removed by an etching process. During this process, because the upper second material layer pattern 305a has a higher second concentration (oxygen-rich or nitrogen-rich state) during film formation, the etching rate changes significantly compared to conventional materials with a base concentration, while the exposed first material layer 303 below maintains its base concentration. Therefore, this etching process can also achieve an etching selectivity greater than a preset threshold, selectively removing the upper second material layer pattern 305a, thereby ensuring the complete preservation of the exposed first material layer 303 below, effectively avoiding the micro-loading effect caused by over-etching in areas with different pattern densities. Figure 4FAs shown, after removing the second material layer pattern 305a, the intermediate carbon layer pattern 304a is further removed. At this point, only the sidewalls 308 remain on the first material layer 303, and these sidewalls 308 constitute the desired self-aligned pattern. Subsequently, using the remaining sidewalls 308 as a mask, the underlying first material layer 303 and the even deeper diamond-like carbon layer 302 are sequentially etched downwards to achieve hard mask pattern transfer. Also thanks to the complete protection of the surface morphology of the first material layer 303, the pattern obtained after hard mask pattern transfer exhibits good critical dimension uniformity.
[0046] Furthermore, the third implementation method will be described in detail. In some embodiments, step S101 can be implemented by sequentially forming a silicon oxynitride layer with a third concentration of oxygen atoms, an intermediate carbon layer, a silicon oxynitride layer with a fourth concentration of nitrogen atoms, and a core mold layer on the stack to be etched; or, sequentially forming a silicon oxynitride layer with a fifth concentration of nitrogen atoms, an intermediate carbon layer, a silicon oxynitride layer with a sixth concentration of oxygen atoms, and a core mold layer on the stack to be etched.
[0047] In the third implementation, the third, fourth, fifth, and sixth concentrations are all greater than a specific base concentration. This process directly generates two film layers in opposing states (one significantly oxygen-rich and the other significantly nitrogen-rich) during the film formation stage, without retaining the base concentration material layer. Since oxygen-rich silicon oxynitrides and nitrogen-rich silicon oxynitrides exhibit drastically different physicochemical etching preferences in the etching system, this bidirectional configuration strategy maximizes the difference in etching selectivity between the first and second material layers. Therefore, during the subsequent removal of the patterned stack, the widest possible etching process window is obtained, allowing the upper second material layer to be selectively removed while ensuring the underlying structure is adequately protected, thereby optimizing the local critical dimension uniformity (LCDU) after the final hard mask pattern transfer to the optimal level. The subsequent patterning and pattern transfer processes are the same as in the aforementioned embodiments and will not be repeated here.
[0048] The self-aligned pattern formation method provided in this application provides a method for forming a first material layer and a second material layer made of the same type of material (such as silicon oxynitride) in the stack to be etched. During the film formation stage, the first and second material layers are controlled by the process to achieve different oxygen and nitrogen concentrations. This allows similar thin film materials to have drastically different etching rate characteristics, overcoming the limitation in related technologies where the etching selectivity cannot be effectively differentiated due to similar materials in the upper and lower layers. This successfully constructs a natural etching barrier boundary during the removal of the patterned stack. Specifically, this application can either unidirectionally generate a single material layer with a higher concentration of oxygen or nitrogen atoms, providing a flexible and highly compatible implementation path; or it can bidirectionally configure the first and second material layers to be in oxygen-rich and nitrogen-rich states, respectively. In the actual process of removing the patterned stack, the high etch selectivity that meets the preset threshold requirement ensures that the etching process can accurately etch away the upper second material layer while retaining the exposed first material layer below. This eliminates the micro-loading effect caused by similar etching rates in areas with different pattern densities (such as the bottom of adjacent gaps). This not only ensures the high consistency and integrity of the retained sidewall structure and the morphology of the bottom first material layer, but also ensures high fidelity of the target pattern boundary during subsequent hard mask pattern transfer using a self-aligned pattern as a mask. This improves the local critical dimension uniformity (LCDU) after hard mask pattern transfer, thereby effectively improving the electrical performance and reliability of the final fabricated semiconductor device.
[0049] This application also provides a method for forming a semiconductor device, which uses the above-described method for forming a self-aligned pattern to form a self-aligned pattern and then performs pattern transfer.
[0050] This application also provides a semiconductor device, which is prepared using the semiconductor device formation method described above.
[0051] It should be understood that the phrase "an embodiment" or "one embodiment" throughout the specification means that a specific feature, structure, or characteristic related to the embodiment is included in at least one embodiment of this disclosure. Therefore, "in one embodiment" or "one embodiment" appearing throughout the specification does not necessarily refer to the same embodiment. Furthermore, these specific features, structures, or characteristics can be combined in any suitable manner in one or more embodiments. It should be understood that in the various embodiments of this disclosure, the sequence numbers of the above-described processes do not imply a sequential order of execution; the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this disclosure. The sequence numbers of the above-described embodiments are for descriptive purposes only and do not represent the superiority or inferiority of the embodiments.
[0052] The above description is merely an embodiment of this disclosure and is not intended to limit the scope of protection of this disclosure. Any modifications, equivalent substitutions, and improvements made within the spirit and scope of this disclosure are included within the scope of protection of this disclosure.
Claims
1. A method for forming a self-aligned pattern, characterized in that, include: A first material layer, an intermediate carbon layer, a second material layer, and a core mold layer are sequentially formed on the stack to be etched; wherein the first material layer and the second material layer have the same type of material, and the oxygen-nitrogen ratio of the first material layer and the second material layer is different; Based on the core pattern of the core mold layer, the second material layer and the intermediate carbon layer are etched to form a patterned stack; the patterned stack includes a portion of the second material layer and a portion of the intermediate carbon layer; A sidewall material layer is formed on the surface of the patterned stack; The sidewall material layer in the horizontal direction is etched to form a sidewall structure located outside the patterned stack; The patterned stack is removed by an etching process to form the self-aligned pattern; wherein the etching process has an etching selectivity ratio between the second material layer and the first material layer that is greater than a preset etching selectivity ratio threshold.
2. The method according to claim 1, characterized in that, The materials of the first material layer and the second material layer are silicon oxynitrides.
3. The method according to claim 2, characterized in that, The process of sequentially forming a first material layer, an intermediate carbon layer, a second material layer, and a core mold layer on the etchable stack includes: On the etchable stack, a silicon oxynitride layer having a first concentration of oxygen atoms or a first concentration of nitrogen atoms, the intermediate carbon layer, the second material layer having a basic concentration of oxygen atoms and nitrogen atoms, and the core mold layer are formed sequentially; the first concentration is greater than the basic concentration.
4. The method according to claim 2, characterized in that, The process of sequentially forming a first material layer, an intermediate carbon layer, a second material layer, and a core mold layer on the etchable stack includes: On the etchable stack, a first material layer having a basic concentration of oxygen and nitrogen atoms, an intermediate carbon layer, a silicon oxynitride layer having a second concentration of oxygen or nitrogen atoms, and a core mold layer are sequentially formed; the second concentration is greater than the basic concentration.
5. The method according to claim 2, characterized in that, The process of sequentially forming a first material layer, an intermediate carbon layer, a second material layer, and a core mold layer on the etchable stack includes: On the stack to be etched, a silicon oxynitride layer with a third concentration of oxygen atoms, the intermediate carbon layer, a silicon oxynitride layer with a fourth concentration of nitrogen atoms, and the core mold layer are sequentially formed; or, On the etchable stack, a silicon oxynitride layer with a fifth concentration of nitrogen atoms, the intermediate carbon layer, a silicon oxynitride layer with a sixth concentration of oxygen atoms, and the core mold layer are formed sequentially. The third, fourth, fifth, and sixth concentrations are all greater than a specific base concentration.
6. The method according to claim 1, characterized in that, The sidewall material layer etched horizontally forms a sidewall structure located outside the patterned stack, including: The sidewall material layer located in the horizontal direction is etched, while the sidewall material layer perpendicular to the surface of the stack to be etched is retained, forming a sidewall structure located outside the patterned stack.
7. The method according to any one of claims 1 to 6, characterized in that, The preset etching selectivity threshold is used to define the etching selectivity critical value for removing the second material layer and retaining the first material layer during the process of removing the patterned stack.
8. The method according to any one of claims 1 to 6, characterized in that, After removing the patterned overlay, the method further includes: Using the self-aligned pattern as a mask, the hard mask pattern is transferred to the stack to be etched to form a hard mask pattern.
9. A method for forming a semiconductor device, characterized in that, The method employs the self-aligned pattern formation method according to any one of claims 1 to 8 to form a self-aligned pattern and perform graphic transfer.
10. A semiconductor device, characterized in that, The semiconductor device is prepared using the semiconductor device formation method described in claim 9.