A method for fabricating a semiconductor structure

By forming a barrier layer in the slope region of the semiconductor structure and then annealing it, the scratch problem caused by hump peeling was solved, improving the yield and processing quality.

CN123124776APending Publication Date: 2026-11-17SIEN (QINGDAO) INTEGRATED CIRCUITS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611490943.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the semiconductor manufacturing process, the humps at the edge of the wafer peel off during high-temperature annealing, causing scratches and affecting the yield. Existing technologies are unable to effectively solve this problem.

Method used

A barrier layer is formed in the sloping area and annealed to prevent hump spalling. The barrier layer in the flat area is then removed in the CMP process to avoid scratch formation.

Benefits of technology

This effectively avoids scratches caused by the peeling of the hump, improving the yield and processing quality of semiconductor structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124776A_ABST
    Figure CN123124776A_ABST
Patent Text Reader

Abstract

This application discloses a method for fabricating a semiconductor structure, comprising: providing an initial structure, wherein the initial structure includes a wafer and a patterned first mask layer, the wafer including a planar region and a ramp region located at the circumferential edge of the planar region, the first mask layer being located on the planar region, the first mask layer including an anti-reflective coating, the anti-reflective coating being partially located on the ramp region and forming a hump; etching the wafer using the first mask layer as a mask to form a trench on the upper part of the wafer; removing the first mask layer, wherein the hump is not completely removed; forming an isolation material layer in the trench and on the upper surface of the wafer, forming a barrier layer on the isolation material layer, and performing an annealing process; removing the barrier layer located above the planar region; and grinding the isolation material layer located above the planar region using a CMP process to form a shallow trench isolation in the trench. The technical solution of this application can effectively avoid hump shedding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of semiconductor technology, and more specifically to a method for fabricating a semiconductor structure. Background Technology

[0002] In chemical mechanical polishing (CMP) processes, defect control, morphology control, and thickness uniformity are all crucial, with scratch defects being a major concern. The introduction of scratches is primarily caused by the polishing pad, polishing disc, agglomerated polishing fluid particles, and leading particles.

[0003] With the mass production of advanced technology nodes such as 28nm and below, wafer edge processing has become increasingly important for improving yield performance. Peeling defects at wafer edges are a key factor affecting yield, caused by the complex thin film stacking at the silicon wafer edges, especially in the ramp region.

[0004] During photolithography, anti-reflective coating materials (such as Si-arc materials) accumulate in the slope region of the wafer, forming thick humps. These thick humps cannot be completely removed during etching and become residue. During subsequent thin film deposition and high-temperature annealing, the humps are prone to peeling off at high temperatures, extending to the front side of the wafer. This results in scratches during subsequent CMP (Chemical Mechanical Polishing) due to chemical and physical effects.

[0005] Therefore, improvements are needed to at least partially address the aforementioned problems. Summary of the Invention

[0006] The summary section introduces a series of simplified concepts, which will be further explained in detail in the detailed description section. The summary section of this invention is not intended to limit the key features and essential technical features of the claimed technical solution, nor is it intended to determine the scope of protection of the claimed technical solution.

[0007] To at least partially solve the above problems, according to a first aspect of the present invention, a method for fabricating a semiconductor structure is provided, comprising: An initial structure is provided, wherein the initial structure includes a wafer and a patterned first mask layer, the wafer including a planar region and a ramp region located at the circumferential edge of the planar region, the first mask layer being located on the planar region, the first mask layer including an anti-reflective coating, the anti-reflective coating being partially located on the ramp region and forming a hump; The wafer is etched using the first mask layer as a mask to form a trench on the upper part of the wafer; Remove the first mask layer, wherein the hump is not completely removed; An isolation material layer is formed in the trench and on the upper surface of the wafer, a barrier layer is formed on the isolation material layer, and then annealing is performed. Remove the barrier layer located above the planar region, while retaining the barrier layer located above the slope region; The insulating material layer located above the planar region is ground using a CMP process to form shallow trench isolation in the trench.

[0008] For example, the insulating material layer is made of silicon dioxide; The barrier layer is made of silicon nitride.

[0009] For example, removing the barrier layer located above the planar region includes: A patterned second mask layer is formed on the barrier layer, wherein the patterned second mask layer exposes the barrier layer located above the planar region and covers the barrier layer located above the slope region; The exposed barrier layer is removed by an etching process.

[0010] For example, the etching process is a wet etching process.

[0011] For example, the first mask layer includes a spin-coated carbon layer, an anti-reflective coating on the spin-coated carbon layer, and a photoresist layer on the anti-reflective coating.

[0012] According to a second aspect of the present invention, a method for fabricating a semiconductor structure is provided, comprising: An initial structure is provided, wherein the initial structure includes a wafer, a polishing stop layer, and a patterned first mask layer, the wafer including a planar region and a ramp region located at the circumferential edge of the planar region, the polishing stop layer being located on the planar region, the first mask layer being located on the polishing stop layer, the first mask layer including an anti-reflective coating, the anti-reflective coating being partially located on the ramp region and forming a hump; The grinding stop layer and the wafer are etched using the first mask layer as a mask to form a trench on the upper part of the wafer; Remove the first mask layer, wherein the hump is not completely removed; An isolation material layer is formed in the trench, on the grinding stop layer, and on the slope area; a barrier layer is formed on the isolation material layer; and annealing is performed. Remove the barrier layer located above the planar region, while retaining the barrier layer located above the slope region; The insulating material layer located above the grinding stop layer is ground using a CMP process to form shallow trench isolation in the trench.

[0013] For example, the wafer is made of silicon; The grinding stop layer is made of silicon nitride. The insulating material layer is made of silicon dioxide; The barrier layer is made of silicon nitride.

[0014] For example, removing the barrier layer located above the planar region includes: A patterned second mask layer is formed on the barrier layer, wherein the patterned second mask layer exposes the barrier layer located above the planar region and covers the barrier layer located above the slope region; The exposed barrier layer is removed by an etching process.

[0015] For example, the etching process is a wet etching process.

[0016] For example, the first mask layer includes a spin-coated carbon layer, an anti-reflective coating on the spin-coated carbon layer, and a photoresist layer on the anti-reflective coating.

[0017] According to the semiconductor structure fabrication method of the present invention, by first forming a barrier layer on the isolation material layer in the slope region and then performing annealing, the humps in the slope region can be effectively prevented from peeling off to the top of the planar region due to high temperature during annealing. Then, the barrier layer located above the planar region is removed and CMP process is performed, thereby effectively preventing scratches caused by the peeling off of humps during the CMP process. Attached Figure Description

[0018] The following figures are included as part of this application for understanding the application. The figures illustrate embodiments of the application and their descriptions, serving to explain the apparatus and principles of the application. In the figures, Figures 1A-1D These are cross-sectional schematic diagrams of the structures corresponding to each step of the semiconductor structure fabrication method in related technologies; Figure 2 This is a picture of a camel's hump. Figure 3 This is a schematic diagram illustrating the formation process of a camel hump. Figure 4 This is a schematic flowchart of a method for fabricating a semiconductor structure according to the first embodiment of this application; Figures 5A-5E This is a cross-sectional schematic diagram of the structure corresponding to each step of the semiconductor structure fabrication method according to the first embodiment of this application; Figure 6 This is a schematic flowchart of a method for fabricating a semiconductor structure according to a second embodiment of this application; Figures 7A-7E This is a cross-sectional schematic diagram of the structure corresponding to each step of the semiconductor structure fabrication method according to the second embodiment of this application.

[0019] Explanation of reference numerals in the attached figures: 10-Wafer, 11-Planar area, 12-Slope area, 13-Trench, 20-Mask layer, 21-Anti-reflective coating, 22-Hump, 30-Isolation material layer, 31-Shallow trench isolation, 40-Diluent, 50-Mixed transition layer; 100 - Wafer, 110 - Planar area, 111 - Trench, 120 - Sloping area, 200 - First mask layer, 210 - Anti-reflective coating, 211 - Hump, 220 - Spin-coated carbon layer, 230 - Photoresist layer, 240 - Polishing stop layer, 300 - Isolation material layer, 310 - Shallow trench isolation, 400 - Barrier layer, 500 - Second mask layer. Detailed Implementation

[0020] The following description provides numerous specific details to offer a more thorough understanding of this application. However, it will be apparent to those skilled in the art that this application can be practiced without one or more of these details. In other instances, certain technical features well-known in the art have not been described to avoid confusion with this application.

[0021] It should be understood that this application can be implemented in various forms and should not be construed as limited to the embodiments set forth herein. Rather, providing these embodiments will make the disclosure thorough and complete, and will fully convey the scope of this application to those skilled in the art. In the drawings, for clarity, the dimensions and relative dimensions of layers and regions may be exaggerated. The same reference numerals denote the same elements throughout.

[0022] It should be understood that although the terms first, second, third, etc., may be used to describe various elements, components, areas, layers, and / or parts, these elements, components, areas, layers, and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, area, layer, or part from another element, component, area, layer, or part. Therefore, without departing from the teachings of this application, the first element, component, area, layer, or part discussed below may be referred to as the second element, component, area, layer, or part.

[0023] Spatial relation terms such as "below," "under," "below," "under," "above," and "above" are used here for convenience to describe the relationship between one element or feature shown in the figure and other elements or features. It should be understood that, in addition to the orientation shown in the figure, spatial relation terms are intended to also include different orientations of devices in use and operation.

[0024] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of this application. When used herein, the singular forms “a,” “an,” and “the” are also intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the terms “comprising” and / or “including,” when used in this specification, identify the presence of the stated features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups. When used herein, the term “and / or” includes any and all combinations of the associated listed items.

[0025] Embodiments of the invention are described herein with reference to cross-sectional views that serve as schematic diagrams of preferred embodiments (and intermediate structures) of this application. Thus, variations in the shown shape are contemplated due to, for example, manufacturing techniques and / or tolerances. Therefore, embodiments of this application should not be limited to the specific shapes shown herein, but include shape deviations due to, for example, manufacturing processes. Consequently, the figures are substantially schematic, and their shapes are not intended to show the actual shape of the device and are not intended to limit the scope of this application.

[0026] See attached document Figures 1A-1D The methods for fabricating semiconductor structures in related technologies are explained.

[0027] First, see appendix Figure 1A An initial structure is provided, comprising a wafer 10 and a patterned mask layer 20. The wafer 10 includes a planar region 11 and a bevel region 12 located at the circumferential edge of the planar region 11. The mask layer 20 is located on the planar region 11 and includes an anti-reflective coating 21, which is partially located on the bevel region 12 and has a hump 22. (Appendix) Figure 2 The specific morphology of hump 22 is shown. See appendix. Figure 3The formation process of the hump 22 is as follows: After the anti-reflective coating 21 is formed in the slope region 12, it needs to undergo edge washing. During the edge washing process, the anti-reflective coating 21 comes into contact with the thinner 40 used in the edge washing process to form an intermediate mixing transition layer 50. The adhesion of the mixing transition layer 50 to the wafer 10 becomes poor, and the melt here is easy to spread on the wafer 10, so it is easy to push upwards to form the prototype of the hump 22. After the edge washing process is completed, it will be spun dry at high speed and dried, and the hump 22 is formed.

[0028] Then, see appendix. Figure 1B The wafer 10 is etched using the mask layer 20 as a mask to form a trench 13 on the upper part of the wafer 10. Afterward, the mask layer 20 is removed. In this process, the hump 22 is difficult to completely remove and will remain as a residue on the slope region 12 of the wafer 10.

[0029] Then, see appendix. Figure 1C An isolation material layer 30 is formed in the trench 13 and on the upper surface of the wafer 10, and then annealed to repair the damaged lattice and improve the film quality of the formed isolation material layer 30. During this process, the hump 22 is prone to peeling off to the surface of the isolation material layer 30 at the high temperature during annealing.

[0030] Then, see appendix. Figure 1D The isolation material layer 30 is polished using CMP process to form shallow trench isolation 31 in the trench 13. The humps 22 that peel off to the surface of the isolation material layer 30 are prone to forming scratches on the surface of the wafer 10 due to chemical and physical effects during the CMP process.

[0031] The following is a reference to the appendix. Figure 4 An exemplary description will be given of a method for fabricating a semiconductor structure according to the first embodiment of this application, which includes the following steps: S10: Provide an initial structure, wherein the initial structure includes a wafer and a patterned first mask layer, the wafer including a planar region and a ramp region located at the circumferential edge of the planar region, the first mask layer being located on the planar region, the first mask layer including an anti-reflective coating, the anti-reflective coating being partially located on the ramp region and forming a hump.

[0032] S11: Etch the wafer using the first mask layer as a mask to form a trench on the upper part of the wafer.

[0033] S12: Remove the first mask layer, where the hump is not completely removed.

[0034] S13: An isolation material layer is formed in the trench and on the upper surface of the wafer, a barrier layer is formed on the isolation material layer, and annealing is performed; S14: Remove the barrier layer located above the planar area, while retaining the barrier layer located above the slope area; S15: The isolation material layer located above the planar area is ground by CMP process to form shallow trench isolation in the trench.

[0035] According to the semiconductor structure fabrication method of the present application embodiment, by first forming a barrier layer on the isolation material layer in the slope region and then performing annealing, the humps in the slope region can be effectively prevented from peeling off onto the isolation material layer due to high temperature during annealing. After that, the barrier layer located above the planar region is removed and CMP process is performed, thereby effectively preventing scratches caused by hump peeling off during the CMP process.

[0036] The following is a reference to the appendix. Figures 5A-5E The method for preparing the semiconductor structure according to the first embodiment of this application (i.e., steps S10-S15 described above) will be described in detail.

[0037] In step S10, see Appendix Figure 5A This provides an initial structure. The initial structure includes a wafer 100 and a patterned first mask layer 200.

[0038] Wafer 100 includes a planar region 110 and a ramp region 120 located at the circumferential edge of the planar region 110. The planar region 110 is the central region of wafer 100, and its upper surface is horizontal when wafer 100 is placed horizontally. The upper surface of the ramp region 120 is inclined relative to the horizontal plane when wafer 100 is placed horizontally. For example, wafer 100 can be a silicon wafer or a wafer of other suitable materials (e.g., SiC, GaAs, InP, etc.).

[0039] The first mask layer 200 is located on the planar region 110. The first mask layer 200 includes an anti-reflection coating (ARC) 210, which is partially located on the ramp region 120 and has a hump 211. Exemplarily, the first mask layer 200 may include a spin-on-carbon (SOC) layer, the anti-reflection coating 210 located on the spin-on-carbon layer 220, and a photoresist layer 230 located on the anti-reflection coating 210. Exemplarily, the anti-reflection coating 210 may be a silicon-containing anti-reflection coating (Si-ARC layer). The hump 211 is a protruding portion located at the edge of the anti-reflection coating 210 on the ramp region 120, and its thickness is significantly greater than the thickness of the anti-reflection coating 210. The formation process of the hump 211 has been specifically described above and will not be repeated here.

[0040] In step S11, see Appendix Figure 5BThe wafer 100 is etched using the first mask layer 200 as a mask to form a trench 111 on the upper part of the wafer 100. Exemplarily, in this step, the wafer 100 can be etched using an anisotropic dry etching process.

[0041] In step S12, see Appendix Figure 5B The first mask layer 200 is removed. After the first mask layer 200 is removed, the upper surface of the planar region 110 is exposed. For example, when the first mask layer 200 includes a spin-coated carbon layer 220, an anti-reflective coating 210 on the spin-coated carbon layer 220, and a photoresist layer 230 on the anti-reflective coating 210, the photoresist layer 230 can be removed by a process such as plasma ashing, the anti-reflective coating 210 can be removed by a dry etching process, and the spin-coated carbon layer 220 can be removed by a process such as plasma ashing. Due to limitations of existing removal processes, when the anti-reflective coating 210 is removed, the hump 211 is usually difficult to completely remove and remains as a residue on the slope region 120 of the wafer 100. That is, in step S12, the hump 211 is not completely removed.

[0042] In step S13, see Appendix Figure 5CAn isolation material layer 300 is formed in the trench 111 and on the upper surface of the wafer 100, a barrier layer 400 is formed on the isolation material layer 300, and then annealing is performed. Specifically, an isolation material layer 300 is first formed in the trench 111 and on the upper surface of the wafer 100 (including the planar region 110 and the ramp region 120) using a deposition process such as HARP (High Aspect Ratio Process). The isolation material layer 300 is an insulating material and is used to form the Shallow Trench Isolation (STI) 310 in the subsequent process. Then, a barrier layer 400 is formed on the isolation material layer 300 using a deposition process such as CVD. The barrier layer 400 is used to prevent the humps 211 of the ramp region 120 from peeling off above the planar region 110 (i.e., peeling off above the barrier layer 400 located above the planar region 110) due to high temperature during the subsequent annealing process. The barrier layer 400 needs to be a material layer with relatively high hardness that can be stably maintained at the high temperature of annealing. Then, annealing is performed to repair the damaged lattice and improve the film quality of the formed isolation material layer 300. For example, the annealing process can be furnace tube annealing or rapid thermal annealing. Since a barrier layer 400 covers the slope region 120 during annealing, it effectively prevents the hump 211 from peeling off onto the planar region 110. For example, the insulating material layer 300 is made of silicon dioxide, and the barrier layer 400 is made of silicon nitride. On the one hand, silicon nitride has higher hardness and structural stability at high temperatures; therefore, annealing effectively prevents the hump 211 from peeling off onto the planar region 110 due to high temperatures. On the other hand, silicon dioxide has a higher abrasion selectivity than silicon nitride; therefore, in subsequent steps, the barrier layer 400 located above the slope region 120 does not need to be removed, allowing it to continue preventing the hump 211 from peeling off onto the planar region 110 and forming scratches during the CMP process.

[0043] In step S14, see Appendix Figure 5DThe barrier layer 400 above the planar region 110 is removed, exposing the isolation material layer 300 above the planar region 110, while retaining the barrier layer 400 above the ramp region 120. Specifically, a patterned second mask layer 500 (which may be, for example, a photoresist layer) is first formed on the barrier layer 400, wherein the patterned second mask layer 500 exposes the barrier layer 400 above the planar region 110 and covers the barrier layer 400 above the ramp region 120; then, the exposed barrier layer 400 is removed by an etching process. Exemplarily, this etching process can be a wet etching process. Since the etching of the barrier layer 400 is a large-area etching, and the pattern precision requirement is relatively low, a relatively low-cost and relatively simple wet etching process can be used. In some embodiments, this etching process can also be a dry etching process. Exemplarily, after the exposed barrier layer 400 is removed, the second mask layer 500 can be removed.

[0044] In step S15, see Appendix Figure 5E The isolation material layer 300 above the planar region 110 is ground using a CMP process to form a shallow trench isolation 310 in the trench 111. Specifically, the isolation material layer 300 above the planar region 110 is ground to the upper surface of the wafer 100 using a CMP process, and the remaining grinding material layer in the trench 111 is ground to form the shallow trench isolation 310. The isolation material layer 300 needs to have a relatively high grinding selectivity relative to the wafer 100 (e.g., a grinding selectivity greater than 5:1) so that the grinding can stop relatively accurately on the upper surface of the wafer 100. Since the aforementioned steps can effectively prevent the hump 211 of the ramp region 120 from peeling off to the upper surface of the planar region 110 due to high temperature during annealing, scratches will not be formed due to the peeling off of the hump 211 during the CMP process. For example, the isolation material layer 300 may have a relatively high abrasion selectivity (e.g., a abrasion selectivity greater than 5:1) relative to the barrier layer 400, so that the barrier layer 400 located above the ramp region 120 can be retained as much as possible during the abrasion process, so as to continue to prevent the hump 211 from peeling off above the planar region 110 and forming scratches in the CMP process.

[0045] The following is a reference to the appendix. Figure 6 An exemplary description will be given of a method for fabricating a semiconductor structure according to a second embodiment of this application, the method comprising the following steps: S20: Provide an initial structure, wherein the initial structure includes a wafer, a polishing stop layer and a patterned first mask layer, the wafer including a planar region and a ramp region located at the circumferential edge of the planar region, the polishing stop layer being located on the planar region, the first mask layer being located on the polishing stop layer, the first mask layer including an anti-reflective coating, the anti-reflective coating being partially located on the ramp region and forming a hump.

[0046] S21: Using the first mask layer as a mask, etch and grind the stop layer and the wafer to form a trench on the upper part of the wafer.

[0047] S22: Remove the first mask layer, where the hump is not completely removed.

[0048] S23: An isolation material layer is formed in the groove, on the grinding stop layer and on the slope area, a barrier layer is formed on the isolation material layer, and annealing is performed.

[0049] S24: Remove the barrier layer located above the planar area, while retaining the barrier layer located above the slope area.

[0050] S25: The isolation material layer above the grinding stop layer is ground by CMP process to form shallow trench isolation in the trench.

[0051] According to the semiconductor structure fabrication method of the present application embodiment, by first forming a barrier layer on the isolation material layer in the slope region and then performing annealing, the humps in the slope region can be effectively prevented from peeling off to the top of the planar region due to high temperature during annealing. Then, the barrier layer located above the planar region is removed and CMP process is performed, thereby effectively preventing scratches caused by the peeling off of humps during the CMP process.

[0052] The following is a reference to the appendix. Figures 7A-7E The method for preparing the semiconductor structure according to the second embodiment of this application (i.e., steps S20-S25 described above) will be described in detail.

[0053] In step S20, see Appendix Figure 7A This provides an initial structure. The initial structure includes a wafer 100, a polishing stop layer 240, and a patterned first mask layer 200.

[0054] Wafer 100 includes a planar region 110 and a ramp region 120 located at the circumferential edge of the planar region 110. The planar region 110 is the central region of wafer 100, and its upper surface is horizontal when wafer 100 is placed horizontally. The upper surface of the ramp region 120 is inclined relative to the horizontal plane when wafer 100 is placed horizontally. For example, wafer 100 can be a silicon wafer or a wafer of other suitable materials (e.g., SiC, GaAs, InP, etc.).

[0055] The grinding stop layer 240 is located on the planar region 110. The setting of the grinding stop layer 240 allows the subsequent CMP process to stop accurately at the grinding stop layer 240, thereby effectively preventing the wafer 100 from being over-grinded when the grinding selectivity of the isolation material layer 300 relative to the wafer 100 is relatively low.

[0056] The first mask layer 200 is located on the polishing stop layer 240. The first mask layer 200 includes an anti-reflective coating 210, which is partially located on the ramp region 120 and has a hump 211. For example, the first mask layer 200 may include a spin-coated carbon layer 220, an anti-reflective coating 210 located on the spin-coated carbon layer 220, and a photoresist layer 230 located on the anti-reflective coating 210. For example, the anti-reflective coating 210 may be a silicon-containing anti-reflective coating. The hump 211 is a protruding portion located at the edge of the anti-reflective coating 210 on the ramp region 120, and its thickness is significantly greater than the thickness of the anti-reflective coating 210. The formation process of the hump 211 has been specifically described above and will not be repeated here.

[0057] In step S21, see Appendix Figure 7B Using the first mask layer 200 as a mask, the polishing stop layer 240 and the wafer 100 are etched to form a trench 111 on the upper part of the wafer 100. Exemplarily, in this step, the polishing stop layer 240 and the wafer 100 can be etched by an anisotropic dry etching process.

[0058] In step S22, see Appendix Figure 7B The first mask layer 200 is removed. After the first mask layer 200 is removed, the upper surface of the grinding stop layer 240 is exposed. For example, when the first mask layer 200 includes a spin-coated carbon layer 220, an anti-reflective coating 210 on the spin-coated carbon layer 220, and a photoresist layer 230 on the anti-reflective coating 210, the photoresist layer 230 can be removed by a process such as plasma ashing, the anti-reflective coating 210 can be removed by a dry etching process, and the spin-coated carbon layer 220 can be removed by a process such as plasma ashing. Due to limitations of existing removal processes, when the anti-reflective coating 210 is removed, the hump 211 is usually difficult to remove completely and remains as a residue on the ramp region 120 of the wafer 100. That is, in step S22, the hump 211 is not completely removed.

[0059] In step S23, see Appendix Figure 7CAn isolation material layer 300 is formed in the groove 111, on the grinding stop layer 240 and on the slope area 120, a barrier layer 400 is formed on the isolation material layer 300, and then annealing is performed. Specifically, an isolation material layer 300 is first formed in the trench 111, on the grinding stop layer 240, and on the slope region 120 using a deposition process such as HARP. The isolation material layer 300 is an insulating material and is used to form the shallow trench isolation 310 later. Then, a barrier layer 400 is formed on the isolation material layer 300 using a deposition process such as CVD. The barrier layer 400 is used to prevent the humps 211 of the slope region 120 from peeling off above the planar region 110 (i.e., peeling off above the barrier layer 400 located above the planar region 110) due to high temperatures during the subsequent annealing process. The barrier layer 400 needs to be a material layer with relatively high hardness that can be stably maintained at the high temperature of annealing. Then, annealing is performed to repair the damaged lattice and improve the film quality of the formed isolation material layer 300. For example, the annealing process can be furnace tube annealing or rapid thermal annealing. Because a barrier layer 400 covers the slope region 120 during annealing, the hump 211 is effectively prevented from peeling off onto the planar region 110. For example, the wafer 100 is made of silicon, the polishing stop layer 240 is made of silicon nitride, the isolation material layer 300 is made of silicon dioxide, and the barrier layer 400 is made of silicon nitride. On the one hand, silicon nitride has higher hardness and structural stability at high temperatures; therefore, annealing can effectively prevent the hump 211 from peeling off onto the planar region 110 due to high temperatures. On the other hand, silicon dioxide has a higher polishing selectivity than silicon nitride; therefore, in subsequent steps, the barrier layer 400 located above the slope region 120 does not need to be removed, allowing it to continue preventing the hump 211 from peeling off onto the planar region 110 and forming scratches during the CMP process.

[0060] In step S24, see Appendix Figure 7DThe barrier layer 400 above the planar region 110 is removed, exposing the isolation material layer 300 above the planar region 110, while retaining the barrier layer 400 above the ramp region 120. Specifically, a patterned second mask layer 500 (which may be, for example, a photoresist layer) is first formed on the barrier layer 400, wherein the patterned second mask layer 500 exposes the barrier layer 400 above the planar region 110 and covers the barrier layer 400 above the ramp region 120; then, the exposed barrier layer 400 is removed by an etching process. Exemplarily, this etching process can be a wet etching process. Since the etching of the barrier layer 400 is a large-area etching, and the pattern precision requirement is relatively low, a relatively low-cost and relatively simple wet etching process can be used. In some embodiments, this etching process can also be a dry etching process. Exemplarily, after the exposed barrier layer 400 is removed, the second mask layer 500 can be removed.

[0061] In step S25, see Appendix Figure 7E The isolation material layer 300 above the planar region 110 is ground using a CMP process to form a shallow trench isolation 310 in the groove 111. Specifically, the isolation material layer 300 above the planar region 110 is ground down to the grinding stop layer 240 using a CMP process, and the remaining isolation material layer 300 is ground to form the shallow trench isolation 310. The isolation material layer 300 needs to have a relatively high grinding selectivity relative to the grinding stop layer 240 (e.g., a grinding selectivity greater than 5:1). Since the aforementioned steps can effectively prevent the hump 211 of the ramp region 120 from peeling off to the top of the planar region 110 due to high temperature during annealing, scratches will not be formed due to the peeling off of the hump 211 during the CMP process. For example, the isolation material layer 300 may have a relatively high abrasion selectivity (e.g., a abrasion selectivity greater than 5:1) relative to the barrier layer 400, so that the barrier layer 400 located above the ramp region 120 can be retained as much as possible during the abrasion process, so as to continue to prevent the hump 211 from peeling off above the planar region 110 and forming scratches in the CMP process.

[0062] Although exemplary embodiments have been described herein with reference to the accompanying drawings, it should be understood that the above exemplary embodiments are merely illustrative and are not intended to limit the scope of this application. Various changes and modifications can be made therein by those skilled in the art without departing from the scope and spirit of this application. All such changes and modifications are intended to be included within the scope of this application as claimed in the appended claims.

[0063] Numerous specific details are set forth in the specification provided herein. However, it will be understood that embodiments of this application may be practiced without these specific details. In some instances, well-known methods, structures, and techniques have not been shown in detail so as not to obscure the understanding of this specification.

[0064] Similarly, it should be understood that, in order to streamline this application and aid in understanding one or more of the various inventive aspects, features of this application may sometimes be grouped together in a single embodiment, figure, or description thereof in the description of exemplary embodiments of this application. However, this approach should not be construed as reflecting an intention that the claimed application requires more features than are expressly recited in each claim. Rather, as reflected in the corresponding claims, its inventive point lies in solving the corresponding technical problem with features fewer than all features of a single disclosed embodiment. Therefore, the claims following the detailed description are hereby expressly incorporated into that detailed description, wherein each claim itself is a separate embodiment of this application.

[0065] Those skilled in the art will understand that, apart from the mutual exclusion of features, all features disclosed in this specification (including the accompanying claims, abstract, and drawings) and all processes or units of any method or apparatus so disclosed can be combined in any combination. Unless otherwise expressly stated, each feature disclosed in this specification (including the accompanying claims, abstract, and drawings) may be replaced by an alternative feature serving the same, equivalent, or similar purpose.

[0066] Furthermore, those skilled in the art will understand that although some embodiments described herein include certain features but not others included in other embodiments, combinations of features from different embodiments are intended to be within the scope of this application and form different embodiments. For example, in the claims, any one of the claimed embodiments can be used in any combination.

[0067] It should be noted that the above embodiments are illustrative of this application and not restrictive of this application, and that those skilled in the art can devise alternative embodiments without departing from the scope of the appended claims.

Claims

1. A method of fabricating a semiconductor structure, characterized by, include: An initial structure is provided, wherein the initial structure includes a wafer and a patterned first mask layer, the wafer including a planar region and a ramp region located at the circumferential edge of the planar region, the first mask layer being located on the planar region, the first mask layer including an anti-reflective coating, the anti-reflective coating being partially located on the ramp region and forming a hump; The wafer is etched using the first mask layer as a mask to form a trench on the upper part of the wafer; Remove the first mask layer, wherein the hump is not completely removed; An isolation material layer is formed in the trench and on the upper surface of the wafer, a barrier layer is formed on the isolation material layer, and then annealing is performed. Remove the barrier layer located above the planar region, while retaining the barrier layer located above the slope region; The insulating material layer located above the planar region is ground using a CMP process to form shallow trench isolation in the trench.

2. The preparation method according to claim 1, characterized in that, The insulating material layer is made of silicon dioxide; The barrier layer is made of silicon nitride.

3. The preparation method according to claim 1 or 2, characterized in that, Removing the barrier layer located above the planar region includes: A patterned second mask layer is formed on the barrier layer, wherein the patterned second mask layer exposes the barrier layer located above the planar region and covers the barrier layer located above the slope region; The exposed barrier layer is removed by an etching process.

4. The preparation method according to claim 3, characterized in that, The etching process is a wet etching process.

5. The preparation method according to claim 1, characterized in that, The first mask layer includes a spin-coated carbon layer, an anti-reflective coating on the spin-coated carbon layer, and a photoresist layer on the anti-reflective coating.

6. A method of fabricating a semiconductor structure, characterized by, include: An initial structure is provided, wherein the initial structure includes a wafer, a polishing stop layer, and a patterned first mask layer, wherein the wafer includes a planar region and a ramp region located at the circumferential edge of the planar region, the polishing stop layer is located on the planar region, the first mask layer is located on the polishing stop layer, and the first mask layer includes an anti-reflective coating, the anti-reflective coating being partially located on the ramp region and forming a hump; The grinding stop layer and the wafer are etched using the first mask layer as a mask to form a trench on the upper part of the wafer; Remove the first mask layer, wherein the hump is not completely removed; An isolation material layer is formed in the trench, on the grinding stop layer, and on the slope area; a barrier layer is formed on the isolation material layer; and annealing is performed. Remove the barrier layer located above the planar region, while retaining the barrier layer located above the slope region; The insulating material layer located above the grinding stop layer is ground using a CMP process to form shallow trench isolation in the trench.

7. The preparation method according to claim 6, characterized in that, The wafer is made of silicon; The grinding stop layer is made of silicon nitride. The insulating material layer is made of silicon dioxide; The barrier layer is made of silicon nitride.

8. The preparation method according to claim 6 or 7, characterized in that, Removing the barrier layer located above the planar region includes: A patterned second mask layer is formed on the barrier layer, wherein the patterned second mask layer exposes the barrier layer located above the planar region and covers the barrier layer located above the slope region; The exposed barrier layer is removed by an etching process.

9. The preparation method according to claim 8, characterized in that, The etching process is a wet etching process.

10. The preparation method according to claim 6, characterized in that, The first mask layer includes a spin-coated carbon layer, an anti-reflective coating on the spin-coated carbon layer, and a photoresist layer on the anti-reflective coating.