A method for tungsten pore filling

By depositing a tungsten seed layer and performing nitrogen plasma source surface treatment on the semiconductor substrate, the problem of uneven tungsten layer surface was solved, thereby improving the flatness of the tungsten layer and increasing the yield.

CN123124778APending Publication Date: 2026-11-17CHENGDU ZIGUANG SEMICON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510614947.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing tungsten filling processes result in uneven tungsten layer surfaces when filling contact holes of varying depths in semiconductor substrates, increasing the stress of chemical mechanical polishing and making it difficult to control yield.

Method used

After depositing a tungsten seed layer and performing partial filling treatment on the surface of a semiconductor substrate, a nitrogen plasma source surface treatment is used to suppress the bulk tungsten layer deposition rate. The height difference is balanced by utilizing the difference in distance between the uneven surface and the nitrogen plasma source nozzle. Subsequently, bulk tungsten layer deposition and chemical mechanical polishing are performed.

Benefits of technology

It effectively balances the height difference of uneven surfaces, improves the flatness of the tungsten layer, reduces the difficulty of chemical mechanical polishing, and increases the yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124778A_ABST
    Figure CN123124778A_ABST
Patent Text Reader

Abstract

This disclosure relates to a method for tungsten-filled vias. After depositing a tungsten seed layer and performing partial filling on a substrate surface containing contact holes of varying depths, an uneven surface is formed on the partially filled substrate surface. Surface treatment with a nitrogen plasma source can suppress the tungsten deposition rate during the bulk tungsten layer deposition process. Because the higher portions of the uneven surface are closer to the nitrogen plasma source nozzle, the nitrogen plasma source surface treatment effect is better, and the tungsten deposition rate is slower; conversely, the lower portions of the uneven surface are farther from the nitrogen plasma source nozzle, resulting in a poorer nitrogen plasma source surface treatment effect and a faster tungsten deposition rate. Utilizing this characteristic, the height difference of the uneven surface can be balanced during the bulk tungsten layer deposition process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of semiconductor manufacturing, and more specifically, to a method for tungsten via filling. Background Technology

[0002] Existing tungsten filling processes can cause surface unevenness in the tungsten layer on semiconductor substrates when filling contact holes of varying depths. This unevenness not only increases the difficulty of subsequent chemical mechanical polishing (CMP) processes but also makes it challenging to control yield. Summary of the Invention

[0003] The purpose of this disclosure is to provide a method for tungsten filling holes to solve the problem in the prior art where contact holes of different depths in tungsten filling holes cause unevenness on the surface of the tungsten layer.

[0004] To achieve the above objectives, this disclosure provides a method for tungsten pore filling, the method comprising: S1. Provide a semiconductor substrate with a tungsten seed layer; S2. Partially fill the surface of the semiconductor substrate from step S1 to obtain a partially filled substrate; S3. Perform nitrogen plasma source surface treatment on the surface of the partially filled substrate to obtain a passivated surface substrate; S4. Perform a bulk tungsten layer deposition process on the surface of the passivated surface substrate to obtain a deposited tungsten substrate.

[0005] Optionally, the tungsten seed layer described in step S1 is prepared by a first chemical vapor deposition process; the precursor of the first chemical vapor deposition process includes a mixed component of WF6 and SiH4, a mixed component of WF6 and H2, or a mixed component of WF6 and B2H6, at a temperature of 250-450°C and a pressure of 5mTorr-300mTorr.

[0006] Optionally, the semiconductor substrate includes a first contact hole and a second contact hole with different depths; the depth of the first contact hole is greater than the depth of the second contact hole.

[0007] Optionally, step S2 includes: S21. A tungsten layer is deposited on the surface of the tungsten seed layer using a second chemical vapor deposition process. S22. Perform rapid annealing on the substrate obtained in step S21. S23. A tungsten layer is deposited on the surface of the substrate obtained in step S22 using a third chemical vapor deposition process to obtain the partially filled substrate.

[0008] Optionally, the conditions for the second chemical vapor deposition process include: the precursor includes WF6 and H2, the temperature is 250-450°C, and the pressure is 5 mTorr-300 mTorr; The conditions for the rapid annealing process include a temperature of 250-450℃; The conditions for the third chemical vapor deposition process include: the precursors include WF6 and H2, the temperature is 250-450℃, and the pressure is 5mTorr-300mTorr.

[0009] Optionally, the temperature of the nitrogen plasma source surface treatment in step S3 is 250-450°C.

[0010] Optionally, the bulk tungsten layer deposition process in step S4 is performed using a fourth chemical vapor deposition process; the precursors for the fourth chemical vapor deposition process include WF6 and H2, the temperature is 250-450℃, and the pressure is 5mTorr-300mTorr.

[0011] Optionally, the thickness of the tungsten seed layer is 5-10 nm.

[0012] Optionally, the ratio of the maximum thickness a of the tungsten layer on the surface of the partially filled substrate to the thickness c of the tungsten layer on the surface of the deposited tungsten substrate is (0.1-0.6):1.

[0013] Optionally, the method further includes: S5, performing chemical mechanical polishing on the surface of the deposited tungsten substrate.

[0014] By employing the above technical solution, after depositing a tungsten seed layer and performing partial filling treatment on the surface of a substrate containing contact holes of varying depths, an uneven surface is formed on the partially filled substrate. Surface treatment with a nitrogen plasma source can suppress the tungsten deposition rate during the bulk tungsten layer deposition process. Because the higher portions of the uneven surface are closer to the nitrogen plasma source nozzle, the nitrogen plasma source surface treatment effect is better, resulting in a slower tungsten deposition rate; conversely, the lower portions of the uneven surface are farther from the nitrogen plasma source nozzle, resulting in a poorer nitrogen plasma source surface treatment effect and a faster tungsten deposition rate. Utilizing this characteristic, the height difference of the uneven surface can be balanced during the bulk tungsten layer deposition process.

[0015] Other features and advantages of this disclosure will be described in detail in the following detailed description section. Attached Figure Description

[0016] The accompanying drawings are provided to further illustrate the present disclosure and form part of the specification. They are used together with the following detailed description to explain the present disclosure, but do not constitute a limitation thereof. In the drawings: Figure 1This is a flowchart of a tungsten pore-filling method disclosed herein.

[0017] Figure 2 This is a schematic diagram of a semiconductor substrate containing contact holes disclosed herein.

[0018] Figure 3 This is a schematic diagram of a semiconductor substrate with a barrier layer deposited on it.

[0019] Figure 4 This is a schematic diagram of a semiconductor substrate with a deposited tungsten seed layer disclosed herein.

[0020] Figure 5 This is a schematic diagram of a partially filled substrate disclosed herein.

[0021] Figure 6 This is a schematic diagram of a passivated surface substrate disclosed herein.

[0022] Explanation of reference numerals in the attached figures 1 Semiconductor substrate; 2 Gate; 3 First contact hole; 4 Second contact hole; 5 Barrier layer; 6 Tungsten seed layer; 7 Tungsten layer partially filling the substrate surface; 8 Bulk tungsten layer. Detailed Implementation

[0023] The specific embodiments of this disclosure will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit this disclosure.

[0024] In this disclosure, unless otherwise stated, directional terms such as "upper" and "lower" generally refer to the upper and lower positions of the device in its normal operating state, for example, as shown in the reference. Figure 1 In the drawing orientation, "inner" and "outer" refer to their relative to the outline of the device. Furthermore, the terms "first," "second," "third," and "fourth" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first," "second," "third," or "fourth" may explicitly or implicitly include one or more of that feature. In the description of this disclosure, "a plurality of" means two or more, unless otherwise explicitly specified.

[0025] like Figure 1 As shown, this disclosure provides a method for tungsten pore filling, the method comprising: S1. Provide a semiconductor substrate having a tungsten seed layer 6; S2. Partially fill the surface of the semiconductor substrate from step S1 to obtain a partially filled substrate; S3. Perform nitrogen plasma source surface treatment on the surface of the partially filled substrate to obtain a passivated surface substrate; S4. Perform a bulk tungsten layer deposition process on the surface of the passivated surface substrate to obtain a deposited tungsten substrate.

[0026] By employing the above technical solution, after depositing a tungsten seed layer and performing partial filling treatment on the surface of a substrate containing contact holes of varying depths, an uneven surface is formed on the partially filled substrate. Surface treatment with a nitrogen plasma source can suppress the tungsten deposition rate during the bulk tungsten layer deposition process. Because the higher portions of the uneven surface are closer to the nitrogen plasma source nozzle, the nitrogen plasma source surface treatment effect is better, resulting in a slower tungsten deposition rate; conversely, the lower portions of the uneven surface are farther from the nitrogen plasma source nozzle, resulting in a poorer nitrogen plasma source surface treatment effect and a faster tungsten deposition rate. Utilizing this characteristic, the height difference of the uneven surface can be balanced during the bulk tungsten layer deposition process.

[0027] In one embodiment, before step S1, the semiconductor substrate containing contact holes undergoes a contact hole etching post-processing and a barrier layer deposition process sequentially. The semiconductor substrate containing contact holes includes a semiconductor substrate 1 and a gate 2.

[0028] In one implementation, such as Figure 2 As shown, the semiconductor substrate containing contact holes includes first contact holes 3 and second contact holes 4 with different depths. In this embodiment, the different depths of the contact holes in the semiconductor substrate are caused by various factors, such as the first contact holes 3 and second contact holes 4 being located at different depths. Figure 2 As shown, the first contact hole 3 is opened in the region between two adjacent gates 2 and exposes the semiconductor substrate 1. The contact hole depth is relatively large here. The second contact hole 4 is opened above the gate 2 of the semiconductor. The contact hole depth is relatively small here.

[0029] In one embodiment, the post-etching treatment of the contact holes is a conventional choice in the art, and this application does not impose any special requirements. In this embodiment, after etching the contact holes, a post-etching treatment is used to remove residual etching byproducts and the native oxide layer, providing a clean surface for subsequent deposition. The post-etching treatment can employ wet cleaning and plasma treatment. Wet cleaning uses dilute hydrofluoric acid (DHF) or SC1 solution (NH4OH / H2O2 / H2O) to remove oxides from the substrate surface; plasma treatment can use Ar / H2 plasma to activate the surface to enhance adhesion.

[0030] In one embodiment, the barrier layer deposition process is a conventional choice in the art, and this application does not impose any special requirements. In this embodiment, such as Figure 3As shown, a barrier layer 5 is deposited on the substrate surface, which not only prevents tungsten from diffusing into the surrounding dielectric layer during tungsten via filling, thus avoiding short circuits or leakage, but also enhances the adhesion between tungsten and the exposed material, preventing peeling. The barrier layer 5 is formed by PVD or ALD deposition processes and is made of Ti and / or TiN.

[0031] In one embodiment, the tungsten seed layer 6 described in step S1 is fabricated using a first chemical vapor deposition process.

[0032] In one embodiment, the precursor of the first chemical vapor deposition process includes a mixed component of WF6 and SiH4, a mixed component of WF6 and B2H6, or a mixed component of WF6 and H2.

[0033] In one embodiment, the temperature of the first chemical vapor deposition process is 250-450°C, preferably 270-420°C; the pressure is 5 mTorr-300 mTorr, preferably 10 mTorr-200 mTorr. The time of the first chemical vapor deposition process can be flexibly set according to the thickness of the tungsten seed layer 6, as long as a tungsten seed layer 6 of suitable thickness can be deposited on the semiconductor substrate surface; further details are omitted here.

[0034] In one embodiment, the thickness of the tungsten seed layer 6 is 5-10 nm, preferably 6-9 nm.

[0035] In this embodiment, such as Figure 4 As shown, depositing a tungsten seed layer 6 on the surface of the semiconductor substrate provides a uniform seed layer for subsequent tungsten deposition, ensuring the uniformity and adhesion of the tungsten deposition. When the conditions of the first chemical vapor deposition process are within a suitable range, the tungsten seed layer 6 can be uniformly deposited on the surface of the semiconductor substrate. Depositing a tungsten seed layer 6 of appropriate thickness ensures, on the one hand, that the deposited tungsten seed layer 6 uniformly covers the substrate surface, avoiding voids or defects during subsequent tungsten deposition, and also ensures a stronger bond between the tungsten seed layer 6 and the barrier layer 5; on the other hand, it provides sufficient tungsten nucleation sites to promote conformal tungsten growth.

[0036] In one embodiment, the partial fill treatment described in this disclosure refers to staged filling rather than filling all at once; deep holes are gradually filled through multiple depositions and annealing processes to avoid the formation of voids or gaps in the holes due to excessively rapid filling at once. The partial fill treatment described in this disclosure includes a multi-stage vapor deposition process and an annealing process interspersed within the multi-stage vapor deposition process.

[0037] In one embodiment, step S2 includes: S21. A tungsten layer is deposited on the surface of the tungsten seed layer 6 using a second chemical vapor deposition process. S22. Perform rapid annealing on the substrate obtained in step S21. S23. A tungsten layer is deposited on the surface of the substrate obtained in step S22 using a third chemical vapor deposition process to obtain the partially filled substrate.

[0038] In this embodiment, tungsten is first deposited on the surface of the tungsten seed layer 6 using a second chemical vapor deposition process to partially fill the contact holes. The filling depth can be 30-80%, avoiding voids or defects caused by filling all at once. Rapid annealing of the substrate obtained in step S21 can repair film stress, reduce defects, and thus promote tungsten grain growth. After annealing, the substrate is then deposited with tungsten again using a third chemical vapor deposition process to fill the contact holes. Deposition continues for a period of time after filling to ensure complete sealing of the holes. At this point, the deposited tungsten forms an uneven tungsten layer on the substrate surface.

[0039] In one embodiment, the precursors used in the second chemical vapor deposition process include WF6 and H2.

[0040] In one embodiment, the conditions for the second chemical vapor deposition process include: a temperature of 250-450°C, preferably 270-420°C; and a pressure of 5 mTorr-300 mTorr, preferably 10 mTorr-200 mTorr. The time for the second chemical vapor deposition process can be flexibly set according to the filling depth, as long as a suitable depth of tungsten can be deposited in the contact hole; further details are omitted here.

[0041] In one embodiment, the rapid annealing process includes: heating to the annealing temperature, holding at that temperature for a certain time, and then cooling. The heating rate and holding time can be set according to the properties of the semiconductor substrate and actual production needs, which will not be elaborated here. The cooling process can be performed by purging with an inert gas or by natural cooling. The annealing temperature is 250-450℃, preferably 270-420℃.

[0042] In one embodiment, the precursors used in the third chemical vapor deposition process include WF6 and H2.

[0043] In one embodiment, the conditions for the third chemical vapor deposition process include: a temperature of 250-450°C, preferably 270-420°C; and a pressure of 5 mTorr-300 mTorr, preferably 10 mTorr-200 mTorr. The time for the third chemical vapor deposition process can be flexibly set according to the thickness of the deposited tungsten layer, as long as it is sufficient to fill the contact holes and deposit tungsten on the semiconductor substrate surface; further details are omitted here.

[0044] In one embodiment, the ratio of the maximum thickness a of the tungsten layer on the surface of the partially filled substrate to the thickness c of the tungsten layer on the surface of the deposited tungsten substrate is (0.1-0.6):1, preferably (0.2-0.5):1.

[0045] In the above embodiments, such as Figure 5 As shown, the tungsten layer 7 partially filling the substrate surface is uneven. The maximum thickness 'a' of the tungsten layer 7 partially filling the substrate surface refers to the vertical distance between the highest point of the tungsten layer and the surface of the barrier layer 5 of the semiconductor substrate; the minimum thickness 'b' of the tungsten layer 7 partially filling the substrate surface refers to the vertical distance between the lowest point of the tungsten layer and the surface of the barrier layer 5 of the semiconductor substrate. Figure 6 As shown, the thickness c of the tungsten layer on the surface of the deposited tungsten substrate refers to the thickness of the tungsten layer formed above the barrier layer 5 in steps S1-S4. Furthermore, when the ratio of the maximum thickness a of the tungsten layer on the surface of the filling substrate to the thickness c of the tungsten layer on the surface of the deposited tungsten substrate is appropriate, sufficient margin can be provided for subsequent bulk tungsten layer deposition, further improving the flatness of the tungsten layer on the surface of the deposited tungsten substrate.

[0046] In one embodiment, the plasma source for the nitrogen plasma source surface treatment is generated by remote plasma-excited N2. In this embodiment, the nitrogen free radicals generated by remote plasma-excited N2 passivate the surface of the tungsten layer in the partial fill process, which not only improves the quality of the tungsten layer but also enhances interfacial adhesion.

[0047] In one embodiment, the conditions for the nitrogen plasma source surface treatment are conventionally selected in the art, as long as they can passivate the tungsten layer surface of the partially filled substrate. In this embodiment, the conditions for nitrogen plasma source surface treatment mainly include the power of the nitrogen plasma source, temperature, treatment time, and the distance between the nozzle and the substrate. Using a nitrogen plasma source with appropriate power ensures that the N2 dissociation efficiency and nitrogen free radical concentration are at a suitable level, avoiding insufficient active nitrogen free radicals, substrate or film damage, and performance degradation caused by excessive ion generation. Using a suitable treatment temperature enhances the reactivity of nitrogen free radicals with the surface, preventing substrate performance degradation caused by nitrogen free radical diffusion and chemical reactions between nitrogen and the substrate. To avoid performance degradation due to temperature changes, the temperature can be matched to the tungsten deposition temperature; for example, the nitrogen plasma source surface treatment temperature is 250-450°C, preferably 270-420°C. Using a suitable treatment time ensures an appropriate depth of surface modification, further improving the passivation effect of the tungsten layer surface. When the nozzle is positioned appropriately, it can not only reduce ion bombardment but also retain highly reactive free radicals, thereby improving the passivation effect of the tungsten layer on the substrate surface. Furthermore, because the tungsten layer 7 partially fills the substrate surface and is uneven, the higher portions of the tungsten layer are closer to the nitrogen plasma source nozzle, resulting in better surface treatment and a slower tungsten deposition rate; conversely, the lower portions are farther from the nitrogen plasma source nozzle, leading to poorer surface treatment and a faster tungsten deposition rate. This characteristic can be utilized to balance the height difference of the tungsten layer during the bulk tungsten deposition process.

[0048] In one embodiment, a carrier gas can be added during the nitrogen plasma source surface treatment process to adjust plasma stability and free radical transport efficiency. The carrier gas is an inert gas, such as Ar. The flow rates and ratios of the carrier gas and the nitrogen plasma source can be flexibly adjusted according to actual production needs, which will not be elaborated upon here.

[0049] In one embodiment, the bulk tungsten layer 8 deposition in step S4 is performed using a fourth chemical vapor deposition process.

[0050] In one embodiment, the precursor for the fourth chemical vapor deposition process includes WF6 and H2.

[0051] In one embodiment, the conditions of the fourth chemical vapor deposition process include: a temperature of 250-450°C, preferably 270-420°C; and a pressure of 5 mTorr-300 mTorr, preferably 10 mTorr-200 mTorr. The time of the fourth chemical vapor deposition process is flexibly set according to the thickness of the tungsten layer deposited on the surface of the tungsten substrate, as long as it can compensate for part of the height difference of the substrate surface and allow the tungsten layer to be deposited to a suitable thickness. Further details are omitted here.

[0052] In this embodiment, by performing chemical vapor deposition on the surface of the passivated substrate, the tungsten deposition rate is lower in areas with greater height and higher in areas with less height. This characteristic can be utilized to gradually repair surface irregularities. Using appropriate chemical vapor deposition conditions can further enhance the repair effect on surface irregularities.

[0053] In one embodiment, step S4 further includes performing a bulk tungsten layer deposition process on the surface of the passivated surface substrate until the thickness of the tungsten layer on the substrate surface reaches the target thickness, and then stopping the bulk tungsten layer deposition process. The semiconductor substrate obtained at this time is the deposited tungsten substrate.

[0054] In this embodiment, the target thickness is determined based on the flatness of the tungsten layer on the surface of the deposited tungsten substrate. When the flatness of the tungsten layer on the surface of the deposited tungsten substrate meets the requirements, the thickness of the tungsten layer at this time is the target thickness. This target thickness is set according to actual production needs, and will not be elaborated further here.

[0055] In one embodiment, the method further includes: S5, performing chemical mechanical polishing on the surface of the deposited tungsten substrate. In this embodiment, chemical mechanical polishing of the surface of the deposited tungsten substrate can remove excess tungsten and flatten the surface. Chemical mechanical polishing is a conventional method in the art and will not be described in detail here.

[0056] The preferred embodiments of this disclosure have been described in detail above with reference to the accompanying drawings. However, this disclosure is not limited to the specific details of the above embodiments. Within the scope of the technical concept of this disclosure, various simple modifications can be made to the technical solutions of this disclosure, and these simple modifications all fall within the protection scope of this disclosure.

[0057] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, this disclosure will not describe the various possible combinations separately.

[0058] Furthermore, various different embodiments of this disclosure can be combined in any way, as long as they do not violate the spirit of this disclosure, they should also be regarded as the content disclosed in this disclosure.

Claims

1. A method of tungsten plug filling, characterized by, The method includes: S1. Provide a semiconductor substrate with a tungsten seed layer; S2. Partially fill the surface of the semiconductor substrate from step S1 to obtain a partially filled substrate; S3. Perform nitrogen plasma source surface treatment on the surface of the partially filled substrate to obtain a passivated surface substrate; S4. Perform a bulk tungsten layer deposition process on the surface of the passivated surface substrate to obtain a deposited tungsten substrate.

2. The method according to claim 1, characterized in that, The tungsten seed layer described in step S1 is prepared by a first chemical vapor deposition process; The precursor for the first chemical vapor deposition process includes a mixture of WF6 and SiH4, a mixture of WF6 and B2H6, or a mixture of WF6 and H2, at a temperature of 250-450℃ and a pressure of 5mTorr-300mTorr.

3. The method according to claim 1, characterized in that, The semiconductor substrate includes a first contact hole and a second contact hole of different depths; The depth of the first contact hole is greater than the depth of the second contact hole.

4. The method according to claim 1, characterized in that, Step S2 includes: S21. A tungsten layer is deposited on the surface of the tungsten seed layer using a second chemical vapor deposition process. S22. Perform rapid annealing on the substrate obtained in step S21. S23. A tungsten layer is deposited on the surface of the substrate obtained in step S22 using a third chemical vapor deposition process to obtain the partially filled substrate.

5. The method according to claim 4, characterized in that, The conditions for the second chemical vapor deposition process include: the precursors include WF6 and H2, the temperature is 250°C-450°C, and the pressure is 5 mTorr-300 mTorr; The conditions for the rapid annealing process include a temperature of 250°C-450°C. The conditions for the third chemical vapor deposition process include: the precursors include WF6 and H2, the temperature is 250-450℃, and the pressure is 5mTorr-300mTorr.

6. The method according to claim 1, characterized in that, The temperature for the nitrogen plasma source surface treatment in step S3 is 250-450℃.

7. The method according to claim 1, characterized in that, The bulk tungsten layer deposition process described in step S4 is performed using the fourth chemical vapor deposition process; The precursors for the fourth chemical vapor deposition process include WF6 and H2, with a temperature of 250-450℃ and a pressure of 5mTorr-300mTorr.

8. The method according to claim 1, characterized in that, The thickness of the tungsten seed layer is 5-10 nm.

9. The method according to claim 1, characterized in that, The ratio of the maximum thickness a of the tungsten layer on the surface of the partially filled substrate to the thickness c of the tungsten layer on the surface of the deposited tungsten substrate is (0.1-0.6):

1.

10. The method according to claim 5, characterized in that, The method also includes: S5. Perform chemical mechanical polishing on the surface of the deposited tungsten substrate.