A temporary fixing and processing method for small-sized packaging substrates
By combining a standard-sized carrier substrate with a thermally reversible phase change adhesive material on a small-sized packaging substrate, the problem of unstable fixation of small-sized substrates during photolithography is solved, achieving low-cost, damage-free rapid fixation and release, and improving photolithography accuracy and efficiency.
Patent Information
- Application Number
- CN202611308177.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-17
AI Technical Summary
Small-sized packaging substrates cannot be effectively adsorbed by the lithography machine's suction cup during the photolithography process, resulting in displacement, shifting, or detachment, which affects the photolithography accuracy and efficiency. Existing fixing methods are costly, have poor versatility, or are prone to damaging the substrate.
A standard-sized carrier substrate is combined with a thermally reversible phase change adhesive material. Rapid bonding and non-destructive separation of the substrate are achieved through thermal melting and room-temperature phase change. The carrier substrate is used to transfer small-sized substrates to be fixed by the chuck of the photolithography equipment.
It enables low-cost, non-destructive, and rapid fixation and release of small-sized packaging substrates, improves photolithography accuracy and efficiency, adapts to the processing of substrates of various specifications, and reduces the risk of substrate damage and processing costs.
Smart Images

Figure CN123124827A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of semiconductor processing technology, and specifically relates to a method for temporary fixing and processing of small-sized packaging substrates. Background Technology
[0002] In semiconductor packaging processes, packaging substrates of two inches and smaller are often processed using manual double-sided alignment lithography machines. Because these small packaging substrates are much smaller than the effective adsorption area of the lithography machine's chuck, the vacuum adsorption force of the chuck cannot effectively act on the substrate surface. Forcing the process can easily lead to substrate displacement, shifting, or even detachment during lithography, severely affecting the alignment accuracy, resulting in a high product scrap rate, and significantly reducing the lithography processing efficiency of small packaging substrates.
[0003] Existing methods for securing small-sized substrates primarily employ customized chucks, mechanical clamping, or temporary adhesives. Customized chucks require individual fabrication for substrates of different sizes, resulting in high costs, poor versatility, and an inability to adapt to various small-sized packaging substrates. Mechanical clamping can easily cause mechanical stress damage to the substrate edges, and the clamping area can obstruct the photolithography area, affecting the integrity of the photolithography pattern. Temporary adhesives, during curing and removal, easily leave residues that contaminate the substrate surface, and removal can damage the photolithography layer, failing to meet the requirements of high-precision photolithography processes. Therefore, there is an urgent need for a simple, reliable, non-destructive, and highly versatile method for photolithographically securing small-sized packaging substrates to overcome the shortcomings of existing technologies. Summary of the Invention
[0004] To address the problems of difficulty in processing and fixing small-sized packaging substrates and easy damage to the substrates in existing technologies, the purpose of this application is to provide a temporary fixing and processing method for small-sized packaging substrates, so as to achieve low-cost, non-damaging, and rapid temporary fixing and release of small-sized packaging substrates.
[0005] To achieve the above objectives, the technical solution adopted in this application is: a method for temporary fixing and processing of a small-size packaging substrate, comprising:
[0006] A standard-sized silicon wafer is provided as the carrier substrate;
[0007] A thermally reversible phase change adhesive material is coated on the surface of the carrier substrate;
[0008] The target substrate is placed on the surface of the carrier substrate coated with the thermally reversible phase change adhesive material. Heat is applied to melt the thermally reversible phase change adhesive material, and then the material is cooled and solidified to bond and fix the target substrate to the carrier substrate.
[0009] The carrier substrate on which the target substrate is fixed is placed in the processing equipment, and the carrier substrate is indirectly fixed by adsorbing the suction cup of the processing equipment, and the processing operation is performed on the target substrate;
[0010] After processing, the carrier substrate and the target substrate are cooled to room temperature to allow the thermally reversible phase change adhesive material to solidify again, and an external force is applied to separate the target substrate from the carrier substrate.
[0011] In this scheme, the size of the target substrate is smaller than the effective adsorption area of the suction cup of the processing equipment. By introducing a standard-sized carrier substrate as an intermediate carrier, the problem that small-sized target substrates cannot be directly and effectively adsorbed by the suction cup of the processing equipment is solved. At the same time, by utilizing the characteristics of thermally reversible phase change adhesive material to melt and bond under micro-heat and desorb under room temperature, a closed loop of thermal cycling process is constructed, thereby significantly reducing process cost and substrate damage risk while ensuring processing stability.
[0012] In one feasible embodiment, the thermally reversible phase change adhesive material is a low-melting-point thermally reversible phase change material, and the melting temperature of the low-melting-point thermally reversible phase change material is 45°C to 55°C; furthermore, the low-melting-point thermally reversible phase change material exhibits a molten flow dynamic when heated to above the melting temperature, and is solid at room temperature.
[0013] In this preferred embodiment, the melting temperature of the adhesive material is limited to a low range, so that the temporary bonding process can be triggered with only slight heating. This ensures that the adhesive material can melt quickly, avoids thermal damage to the packaging substrate or device structure caused by high temperature, and facilitates subsequent rapid cooling and desorption at room temperature.
[0014] In one feasible embodiment, the low-melting-point thermally reversible phase change material is a temporary bonding wax for semiconductors. This temporary bonding wax is a low-viscosity solid wax, free of conductive ion residues, and does not chemically react with the target substrate or the supporting substrate. The selection of the temporary bonding wax must meet semiconductor process compatibility requirements. Its low viscosity helps form an ultra-thin and uniform bonding layer, ensuring photolithographic alignment accuracy. The absence of conductive ion residues and chemical inertness ensure the cleanliness of the substrate surface and the reliability of its electrical properties after processing, preventing the introduction of additional contamination or defects.
[0015] In one feasible embodiment, the process of melting the thermally reversible phase change adhesive material by applying heat is to heat the carrier substrate using a constant temperature heating stage, so that the thermally reversible phase change adhesive material melts and then solidifies.
[0016] By utilizing a constant-temperature heating stage to provide a uniform and controllable heat source, the bonding material can be ensured to reach a molten state and rapidly complete interface wetting within a short time. Subsequently, it quickly enters the solidification and stabilization stage under constant temperature conditions or after the heat source is removed, thus improving bonding efficiency and process consistency. Heating the target substrate ensures that the heating range is limited to the area in contact between the target substrate and the bonding material, avoiding large-area heating that could cause the target substrate to slip.
[0017] In one feasible embodiment, the heating temperature is 50°C, and the heating time is 2 to 5 seconds. Controlling the process window temperature at 50°C, slightly higher than the material's melting point, ensures sufficient melting while allowing for a safety margin. The extremely short heating time reflects the core advantage of "micro-heating rapid bonding," significantly shortening the processing time per piece and adapting to rapid production needs.
[0018] In one feasible embodiment, the step of cooling the carrier substrate and the target substrate to room temperature to re-solidify the thermally reversible phase change adhesive material, and applying external force to separate the target substrate from the carrier substrate includes:
[0019] The thermally reversible phase change adhesive material is allowed to cool and solidify at room temperature, resulting in a decrease in adhesive strength.
[0020] A pushing force is applied to the edge of the target substrate to separate the target substrate from the carrier substrate.
[0021] During the cooling process at room temperature, the adhesive material changes from a molten state to a solid state. The thermal stress generated by volume shrinkage and the increased brittleness of the material itself work together to weaken the interfacial bonding force. At this time, only a slight pushing force is needed to achieve separation, without the need for high-cost and high-risk processes such as chemical solvent cleaning or laser peeling, thus ensuring the integrity and cleanliness of the packaging substrate surface.
[0022] In one feasible embodiment, the carrier substrate is also cleaned before being coated with the thermally reversible phase change adhesive material to remove surface dust, oil and impurities, ensuring that the surface of the carrier substrate is flat and clean.
[0023] In one feasible embodiment, coating the surface of the carrier substrate with a thermally reversible phase change adhesive material includes:
[0024] In a dust-free environment, the thermally reversible phase change adhesive material is uniformly coated on the surface of the carrier substrate using a scraping method, with a coating thickness of 5 μm to 10 μm.
[0025] In one feasible embodiment, the carrier substrate is a standard photolithography silicon wafer of 4-inch, 6-inch, 8-inch or 12-inch, and the surface flatness of the carrier substrate is less than or equal to 0.5μm.
[0026] In one feasible embodiment, the processing equipment is a photolithography machine, and the processing operation includes a double-sided alignment photolithography operation.
[0027] The temporary fixing and processing method for small-sized packaging substrates provided in this application has the following advantages compared with existing technologies: By transferring and fixing the packaging substrate through a carrier substrate and a thermally reversible phase change adhesive material, the problem that small-sized substrates cannot be directly fixed by vacuum chucks is solved. Simultaneously, by utilizing the reversible characteristics of the material between micro-thermal melting and room-temperature phase change, rapid temporary bonding is achieved without the need for complex debonding equipment. Rapid fixing and non-destructive release can be achieved, avoiding thermal damage, chemical contamination, and mechanical stress damage to the substrate caused by high temperatures, chemical solvents, or lasers. Only standard silicon wafers and conventional heating stages are required to adapt to the processing of various specifications of small-sized substrates, effectively improving processing efficiency and flexibility in small-batch, multi-variety production scenarios. Attached Figure Description
[0028] Figure 1 This is a flowchart of a method for temporarily fixing and processing a substrate according to an embodiment of this application. Specific Implementation
[0029] To illustrate the technical content, structural features, achieved objectives, and effects of the invention in detail, the technical solutions of the embodiments of this application will be described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. In the following description, for illustrative purposes, numerous specific details are set forth to provide a detailed description of various exemplary embodiments or implementations of the invention. However, various exemplary embodiments may also be implemented independently without these specific details or in one or more equivalent arrangements. Furthermore, the various exemplary embodiments may differ, but are not necessarily exclusive.
[0030] Conventional temporary bonding processes often require complex debonding steps such as high-temperature curing, laser lift-off, or chemical solvent dissolution. These processes are not only costly in terms of equipment and time-consuming, but also prone to damaging or contaminating the substrate surface due to chemical residues or mechanical stress during debonding. This makes it difficult to meet the demands of small-batch, multi-specification, and low-cost high-precision photolithography processing. Therefore, this application aims to provide a simple, reliable, and non-destructive solution for the temporary fixation and processing of small-sized packaging substrates.
[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application.
[0032] like Figure 1As shown, this embodiment provides a temporary fixing and processing method for small-sized packaging substrates. This method, through the combination of a carrier substrate transfer and a thermally reversible phase change material, provides a processing flow suitable for small-sized packaging substrates. It should be understood that this embodiment aims to illustrate the higher-level logic and functional implementation path of the method; specific material selection and process parameters can be varied and replaced without departing from this concept.
[0033] In step S100, a carrier substrate is provided. Specifically, in this application, the carrier substrate acts as a size conversion and intermediary carrier, and its core function is to provide a standard interface that can be stably adsorbed by the processing equipment. In practical applications, commonly used sizes are 4-inch, 6-inch, 8-inch, or 12-inch. The material and size of the carrier substrate are not limited to a specific type, as long as its surface flatness meets the processing accuracy requirements and can withstand the heat load in subsequent processes. For example, the carrier substrate can be a standard-sized silicon wafer, glass substrate, ceramic plate, or metal plate, etc. Its selection mainly depends on the suction cup specifications of the processing equipment and the process compatibility of the target substrate, rather than fixed material properties.
[0034] In step S200, a thermally reversible phase change adhesive material is coated onto the surface of the substrate. Specifically, a thermally reversible phase change adhesive material is a medium whose adhesive strength undergoes a reversible physical transformation with temperature changes. Unlike traditional permanent adhesives that require chemical curing or solvent dissolution for removal, this material exhibits a molten flow dynamic under specific thermal conditions to establish an adhesive interface, and returns to a solid state upon cooling to maintain fixation or reduce adhesive strength under specific conditions. Various coating methods can be employed, such as spin coating, blade coating, spray coating, or film lamination, as long as a continuous and controllable thickness adhesive layer can be formed on the substrate surface. If spin coating, blade coating, or spray coating is used, the coating temperature must be maintained above the melting point and kept constant to ensure the thermally reversible phase change adhesive material remains in a molten state and is uniformly coated. The key to this step is utilizing the physical phase change characteristics of the material to lay the material basis for subsequent non-destructive desorption and avoid introducing difficult-to-remove chemical residues.
[0035] In step S300, the target substrate is placed on the surface of a carrier substrate coated with a thermally reversible phase change adhesive material. Heat is applied to the target substrate to melt the thermally reversible phase change adhesive material. After the thermally reversible phase change adhesive material cools and solidifies again, the target substrate is bonded and fixed to the carrier substrate. This application specifically addresses the fixing of substrates that are too small to be effectively adsorbed directly by a vacuum chuck. When the target substrate size is smaller than the effective adsorption area of the chuck, direct adsorption can lead to air leakage, displacement, or even detachment. This application uses a carrier substrate as a transfer material, facilitating adsorption and fixation by the chuck of the processing equipment. During the bonding process, heat needs to be applied to trigger the melting phase change of the adhesive material, ensuring it fully wets the contact interface between the target substrate and the carrier substrate, thereby establishing a strong physical connection. This application chooses to directly apply heat to the carrier substrate, causing the adhesive material to melt rapidly. It should be understood that "applying heat" here is a functional action, and the heat source can be a constant-temperature heating platform, infrared radiation, or laser, etc. The heating duration and temperature profile should also be flexibly adjusted according to the thermal response characteristics of the material, as long as the material can be fully melted and the interface wetted. It should not be interpreted as being limited to a specific heating device or fixed time parameters. Thermally reversible phase change adhesives cool and solidify rapidly at room temperature. Therefore, after the thermally reversible phase change adhesive has cooled and solidified, the target substrate can be bonded and fixed to the carrier substrate.
[0036] In step S400, a carrier substrate with the target substrate fixed to it is placed in the processing equipment. At this time, the adhesive material is in a cured state, which can stably fix the target substrate. The carrier substrate is adsorbed by the suction cup of the processing equipment to indirectly fix the target substrate, and the target substrate is processed at room temperature. Specifically, the processing equipment can be any semiconductor manufacturing equipment equipped with a vacuum suction cup, such as a lithography machine, cleaning machine, inspection stage, or thin film deposition equipment. Since the size of the carrier substrate is adapted to the effective adsorption area of the suction cup, the vacuum suction can stably act on the carrier substrate, and the holding force is transferred to the target substrate without loss through the intermediate thermally reversible phase change adhesive layer, thereby achieving indirect high-precision fixation of small-sized substrates. This indirect fixation method not only solves the problem of difficulty in direct adsorption of small-sized substrates, but also avoids edge damage or occlusion problems that may be caused by mechanical clamping, ensuring the integrity and alignment accuracy of the processing area.
[0037] In step S500, after the processing is completed, the carrier substrate and the target substrate are left to cool at room temperature to allow the thermally reversible phase change adhesive material to undergo a physical phase change, and the target substrate and the carrier substrate are separated.
[0038] Traditional techniques often rely on high-temperature decomposition, laser ablation, or chemical solvent immersion to achieve debonding, which are complex processes and prone to damaging the substrate. In this embodiment, however, as the temperature drops to room temperature, the thermally reversible phase change adhesive material changes from a molten state to a solid state. During this physical phase change, microstructural changes such as volume shrinkage occur inside the material. These changes generate internal stress at the bonding interface and significantly reduce the interfacial adhesion force of the material. Only a slight external force (such as pushing, pulling, or shearing force) is required to achieve clean separation of the target substrate and the carrier substrate.
[0039] In one embodiment, the thermally reversible phase change adhesive is a low-melting-point thermally reversible phase change material with a melting temperature of 45°C to 55°C. This material exhibits a molten flow dynamic when heated above its melting temperature and is solid at room temperature. This temperature range is not arbitrarily chosen but is based on considerations of both "bonding reliability" and "thermal safety" in the processing of small-size packaging substrates. If the melting temperature is below 45°C, the material's stability at room temperature may be insufficient, and the high viscosity during bonding may lead to inadequate interfacial wetting, making it difficult to form sufficient bond strength to resist shear forces during processing. Conversely, if the melting temperature is above 55°C, although wettability improves, excessive heat may cause irreversible thermal damage to the target substrate (such as a packaging substrate containing an organic dielectric layer or a precision device structure), and will also prolong the time required for subsequent room-temperature cooling and desorption, reducing overall processing efficiency. Therefore, the temperature range of 45℃ to 55℃ ensures that the material can melt rapidly under micro-heat conditions and fully fill the micro-voids at the interface to achieve a strong bond, while also ensuring that the heat load during the processing is within a safe threshold and providing favorable conditions for subsequent rapid phase change desorption by using room temperature cooling.
[0040] Furthermore, to meet the cleanliness and electrical performance requirements of semiconductor packaging processes, the aforementioned low-melting-point thermally reversible phase change material is preferably a temporary bonding wax for semiconductors. This temporary bonding wax is a low-viscosity solid wax, free of conductive ion residues, and does not chemically react with the target substrate and the supporting substrate. The temporary bonding wax for semiconductors has extremely low melt viscosity, which allows it to easily form a uniform film with a thickness of only a few micrometers during coating. This avoids photolithographic focal length deviation and edge overflow problems caused by excessively thick or uneven adhesive layers, thereby ensuring high-precision alignment and pattern transfer. More importantly, its "no conductive ion residue" characteristic fundamentally eliminates the risk of sodium, potassium, and other mobile ions contaminating the substrate surface circuitry, preventing electrical failures such as device leakage or threshold voltage drift caused by ion migration. Its "chemical inertness" ensures that during the full thermal cycling process of bonding and debonding, the adhesive material will not undergo any chemical corrosion or cross-linking reaction with the metal wiring, passivation layer, or carrier substrate on the target substrate surface. This guarantees the original cleanliness and structural integrity of the substrate surface after separation, allowing it to directly enter the downstream packaging stage without complex cleaning and repair procedures. For semiconductor temporary bonding wax, commercially available antistatic water-soluble industrial solid wax products can be selected, which can automatically detach after curing.
[0041] In one embodiment, a constant-temperature heating stage is preferably used to apply heat to the carrier substrate, causing the thermally reversible phase change adhesive material to melt and solidify. Compared to non-contact heating methods such as hot air circulation or infrared radiation, the constant-temperature heating stage conducts heat through direct contact between the carrier substrate and the heating stage surface, resulting in extremely high heat transfer efficiency and temperature response speed. This ensures that heat penetrates the carrier substrate uniformly and acts on the thermally reversible phase change adhesive material layer in a very short time, effectively avoiding uneven bonding or thermal stress concentration on the substrate caused by local temperature differences. Simultaneously, the precise temperature control capability of the constant-temperature heating stage can stably maintain the heating temperature at the set value, preventing the decomposition of low-melting-point materials or damage to the target substrate due to temperature overshoot, providing a reliable thermal environment for subsequent rapid bonding.
[0042] More preferably, the heating temperature during the above heating process is 50°C, and the preset duration is 2 to 3 seconds, to achieve efficient and non-destructive temporary bonding. The 50°C heating temperature is set slightly higher than the lower limit of the melting temperature of the low-melting-point thermally reversible phase change material (45°C), and is located in the middle of its melting temperature range. This temperature is sufficient to allow the adhesive material to quickly reach a low-viscosity melt flow dynamic to fully fill the microscopic voids at the interface, while also preventing overheating and thermal damage to the target substrate. It should be understood that although this embodiment provides preferred parameters of 50°C and 2-3 seconds, in practical applications, these parameters can be adaptively adjusted according to the specific formulation of the thermally reversible phase change adhesive material, the coating thickness, and the thermal properties of the substrate, as long as instantaneous melting and rapid solidification of the material can be achieved.
[0043] Example 1
[0044] A manual double-sided alignment and photolithography fixation method for small-size packaging substrates, the specific steps of which are as follows:
[0045] 1. Select a 4-inch silicon wafer for photolithography as the substrate. Clean the surface of the silicon wafer with anhydrous ethanol and deionized water in sequence. After drying with nitrogen, ensure that the surface of the silicon wafer is free of impurities and has a flatness of ≤0.5μm.
[0046] 2. In a dust-free and clean environment, a temporary bonding wax for semiconductors is uniformly coated onto the surface of the silicon wafer using a scraping method. The coating thickness is controlled at 6μm to ensure that the wax layer is smooth, free of bubbles, and without any missed areas.
[0047] 3. Place the 1-inch encapsulation substrate stably on the wax-coated silicon wafer surface. After complete adhesion, heat the silicon wafer using a constant temperature heating table. The heating temperature is precisely controlled at 50℃ and heated for 2 seconds to melt and quickly solidify the solid wax, thus completing the bonding and fixing of the encapsulation substrate and the silicon wafer.
[0048] 4. The silicon wafer and the packaging substrate are fed into the double-sided alignment lithography machine. The silicon wafer is placed on the suction cup, and the vacuum adsorption is turned on to fix the silicon wafer, thereby realizing the positioning of the packaging substrate and performing double-sided alignment lithography.
[0049] 5. After photolithography is completed, remove the silicon wafer and the packaging substrate, let it stand at room temperature for 6 seconds to allow the wax layer to cool and solidify completely, then gently push one corner of the packaging substrate to successfully separate the packaging substrate from the silicon wafer. There is no wax residue or damage on the surface of the packaging substrate.
[0050] Testing showed that the packaging substrate fixed using this method had no displacement or shift during the photolithography process, the photolithography pattern alignment accuracy error was ≤0.5μm, and the substrate integrity rate was 100%.
[0051] Example 2
[0052] A manual double-sided alignment and photolithography fixation method for small-size packaging substrates, the specific steps of which are as follows:
[0053] 1. A 6-inch silicon wafer for photolithography is selected as the substrate and subjected to plasma cleaning to remove organic contaminants from the surface, ensuring the cleanliness of the silicon wafer surface;
[0054] 2. Apply industrial solid wax in a dust-free and clean environment to a thickness of 8μm, uniformly covering the effective bearing area of the silicon wafer;
[0055] 3. Place two 2-inch packaging substrates on the surface of the wax-coated silicon wafer and heat them at a constant temperature of 50°C for 3 seconds to achieve bonding and fixation of the packaging substrates;
[0056] 4. Place the silicon wafer and packaging substrate together in the photolithography machine, use a suction cup to hold the silicon wafer in place, and then perform the photolithography process;
[0057] 5. After photolithography, let it stand at room temperature for 8 seconds to complete the desorption of the packaging substrate. After cleaning, the silicon wafer can be reused for subsequent photolithography fixation of the packaging substrate.
[0058] This embodiment can simultaneously fix two 2-inch packaging substrates, with excellent fixation stability and a photolithography yield that is more than 30% higher than that of traditional adsorption methods.
[0059] The above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. The parameters regarding the selection of the substrate material, the melting temperature window of the thermally reversible phase change adhesive material, the specific duration of heating and cooling, and the coating thickness in the foregoing embodiments are merely illustrative descriptions provided to enable those skilled in the art to better understand the technical solution of this application, and are not intended to limit this application. Any person skilled in the art, within the scope of the technology disclosed in this application, can easily conceive of variations or substitutions based on the core concept of using thermally reversible physical phase change in conjunction with a substrate transfer to achieve non-destructive temporary fixation of small-sized substrates. For example, using other phase change materials with the same thermal response characteristics, adjusting the heat source form, or changing the mechanical stress application method should all be covered within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.
Claims
1. A method for temporary fixing and processing of a small-sized packaging substrate, characterized in that, include: A standard-sized silicon wafer is provided as the carrier substrate; A thermally reversible phase change adhesive material is coated on the surface of the carrier substrate; The target substrate is placed on the surface of the carrier substrate coated with the thermally reversible phase change adhesive material. Heat is applied to melt the thermally reversible phase change adhesive material, and then the material is cooled and solidified to bond and fix the target substrate to the carrier substrate. The carrier substrate on which the target substrate is fixed is placed in the processing equipment, and the carrier substrate is indirectly fixed by adsorbing the suction cup of the processing equipment, and the processing operation is performed on the target substrate; After processing, the carrier substrate and the target substrate are cooled to room temperature to allow the thermally reversible phase change adhesive material to solidify again, and an external force is applied to separate the target substrate from the carrier substrate.
2. The method according to claim 1, characterized in that, The thermally reversible phase change adhesive material is a low-melting-point thermally reversible phase change material, and the melting temperature of the low-melting-point thermally reversible phase change material is 45°C to 55°C; furthermore, the low-melting-point thermally reversible phase change material exhibits a molten flow dynamic when heated to above the melting temperature, and is solid at room temperature.
3. The method according to claim 2, characterized in that, The low-melting-point thermally reversible phase change material is a temporary bonding wax for semiconductors.
4. The method according to claim 2, characterized in that, The process of melting the thermally reversible phase change adhesive material by applying heat involves heating the carrier substrate using a constant temperature heating stage, which melts and then solidifies the thermally reversible phase change adhesive material.
5. The method according to claim 4, characterized in that, The heating temperature is 50°C, and the heating time is 2 to 5 seconds.
6. The method according to claim 1, characterized in that, The step of cooling the carrier substrate and the target substrate to room temperature to solidify the thermally reversible phase change adhesive material, and then applying external force to separate the target substrate from the carrier substrate includes: The thermally reversible phase change adhesive material is allowed to cool and solidify at room temperature, resulting in a decrease in adhesive strength. A pushing force is applied to the edge of the target substrate to separate the target substrate from the carrier substrate.
7. The method according to claim 1, characterized in that, The substrate is also cleaned before being coated with the thermally reversible phase change adhesive material.
8. The method according to claim 1, characterized in that, The step of coating the surface of the carrier substrate with a thermally reversible phase change adhesive material includes: uniformly coating the thermally reversible phase change adhesive material on the surface of the carrier substrate by a scraping method in a dust-free environment, with a coating thickness of 5μm to 10μm.
9. The method according to claim 1, characterized in that, The substrate is a standard photolithography silicon wafer of 4-inch, 6-inch, 8-inch or 12-inch, and the surface flatness of the substrate is less than or equal to 0.5μm.
10. The method according to claim 1, characterized in that, The processing equipment is a photolithography machine, and the processing operation includes a double-sided alignment photolithography operation.