Resin laminated film

By employing a specific composition of an infrared radiation layer and a light reflection layer in the radiation cooling material, the problems of temperature rise, low electromagnetic wave transmittance, and contamination are solved, achieving efficient radiation cooling and high reflectivity, thus improving the cooling performance of the material.

CN123125103APending Publication Date: 2026-11-17OSAKA GAS CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202480088656.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-02-27
Filing Date
2024-12-16
Publication Date
2026-11-17

Smart Images

  • Figure CN123125103A_ABST
    Figure CN123125103A_ABST
Patent Text Reader

Abstract

It exhibits high cooling capacity under direct sunlight, while also exhibiting high electromagnetic wave transmittance, and prevents the reduction in radiative cooling performance caused by pores in the resin material and the reduction in cooling performance due to pore contamination. The light-reflecting layer (B) has multiple pores K and is composed of a second resin, while the infrared radiation layer (J) is composed of a first resin. This first resin emits thermal radiation energy at wavelengths of 8 μm to 13 μm that is greater than the absorbed solar energy. The infrared radiation layer (J) contains fewer pores than the light-reflecting layer (B), and the laminated resin layer (M) comprising the light-reflecting layer (B) and the infrared radiation layer (J) has a wavelength-average (arithmetic average) light reflectance of 80% or more at wavelengths of 400 nm to 800 nm, a wavelength-average (arithmetic average) light reflectance of 70% or more at wavelengths of 800 nm to 1200 nm, and a wavelength-average emissivity of 43% or more at wavelengths of 8 μm to 13 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin laminated film comprising: an infrared radiating layer that radiates infrared light from a radiating surface; and a light reflecting layer located on the side of the infrared radiating layer opposite to the side where the radiating surface is located. Background Technology

[0002] As a conventional example of a composite cooling raw material utilizing the radiation cooling phenomenon, there are examples of materials that are constructed by stacking the following layers: an infrared radiation layer that radiates infrared light from a radiation surface; and a light reflection layer located on the side of the infrared radiation layer opposite to the side where the radiation surface is located (for example, see Patent Document 1).

[0003] In order to dissipate heat into space through radiative cooling and to cool objects under direct sunlight, it is important to have both high solar reflectivity and high infrared emissivity.

[0004] Existing technical documents Patent documents Patent Document 1: Japanese Patent Publication No. 2018-526599 Patent Document 2: Japanese Patent Publication No. 2022-528289 Patent Document 3: International Publication No. 2018 / 062541. Summary of the Invention

[0005] The problem that the invention aims to solve Current methods for radiative cooling of raw materials achieve high reflectivity of sunlight by using thin metal films to reflect sunlight. However, the use of thin metal films leads to increased absorption, which becomes a major cause of increased raw material temperature under direct sunlight. Furthermore, there are other issues: the low radio wave transmittance of thin metal films makes it difficult for communication equipment to function when enclosed in a space.

[0006] In addition, if a metal thin film is used as a reflective layer, the following issues arise: when the surface is damaged and the metal layer is exposed, corrosion will begin from the metal layer, and the metal layer will be colored through oxidation, which will easily reduce the reflectivity.

[0007] In addition, if a metal thin film is used as a reflective layer, the following problem exists: since metal oxides can easily turn colored even in trace amounts, the degree of reflectivity reduction during deterioration is greater compared to reflective layers made of resin.

[0008] Furthermore, there are also radiation-cooled raw materials that improve solar reflectivity by making the resin porous (see Patent Document 2). In the case of such radiation-cooled raw materials, when the porous material is exposed on the outside, it is easily contaminated by rainwater, etc. When the outermost surface of the radiation-cooled raw material is contaminated, even if the dirt absorbs sunlight, the radiation-cooled raw material itself will not heat up because the thermal contact between the dirt and the radiation-cooled raw material is small. However, when the interior of the porous material is contaminated, the heat converted from sunlight cannot escape due to the dirt, and therefore the raw material will be significantly heated. As described above, from the point of view of dirt, there is a need for radiation-cooled raw materials that avoid the state of the porous material being exposed on the surface.

[0009] Furthermore, there are radiation-cooling raw materials that effectively utilize the porous material itself as a radiation layer (see Patent Document 3). However, such radiation-cooling raw materials struggle to maximize radiation-cooling capacity in atmospheric window regions. Examples of porousable raw materials include polyethylene terephthalate, polypropylene, polyethylene, and polyethylene naphthalate, but making them porous reduces the amount of material contributing to radiation; therefore, increasing the thickness is necessary to achieve greater radiation-cooling capacity. Radiation-cooling raw materials are designed to cool the adhered object; increasing the resin layer, especially a porous resin layer, hinders the radiation-cooling capacity of the raw material. From this perspective, designs that use the porous resin layer itself for radiation impede cooling the object.

[0010] Furthermore, when using porous materials to enhance radiation capacity, the poor thermal conductivity caused by porosity leads to the following problem: the temperature of the object being cooled cannot be transferred to the resin at the outermost surface, resulting in insufficient cooling of the object. Additionally, when multiple layers of porous resin containing air are stacked to form a mille-feuille-like structure, the emissivity tends to decrease compared to a non-multilayered structure. This is because, as an optical multilayer film structure, a photonic bandgap structure is formed, increasing reflectivity. Therefore, effectively using porous resin layers not only as reflective layers but also as radiative layers is not ideal for cooling structures that enhance radiation-cooled raw materials.

[0011] The purpose of this invention is to provide a resin laminated film that exhibits high cooling capacity under direct sunlight, high radio wave transmittance, and prevents the reduction in radiative cooling performance caused by the presence of pores in the resin material and the reduction in cooling performance caused by pore contamination.

[0012] Methods for solving problems The resin laminate used to achieve the above objectives is a resin laminate having the following layers: An infrared radiating layer that radiates infrared light from a radiating surface; and a light-reflecting layer located on the opposite side of the infrared radiating layer from the radiating surface. Its characteristics are constituted in the following aspects: The light-reflecting layer has multiple pores and is composed of a second resin. The infrared radiation layer is composed of a first resin that emits thermal radiation energy at wavelengths from 8 μm to 13 μm that is greater than the absorbed solar energy. The number of pores in the infrared radiation layer is less than the number of pores in the light reflection layer. The laminated resin layer comprising the light-reflecting layer and the infrared-radiating layer has a wavelength-average (arithmetic average) light reflectance of 80% or more at wavelengths from 400 nm to 800 nm, a wavelength-average (arithmetic average) light reflectance of 70% or more at wavelengths from 800 nm to 1200 nm, and a wavelength-average emissivity of 43% or more at wavelengths from 8 μm to 13 μm.

[0013] Based on the above-described features, firstly, since no metal thin film is used as a light-reflecting layer, the absorption rate of sunlight can be suppressed, thereby suppressing the temperature rise of the resin laminate compared to a configuration that uses a metal thin film as a light-reflecting layer. Furthermore, because the radio wave transmittance is relatively high, communication using the wireless communication device can be well maintained even when the resin material film with the above-described features is surrounding a wireless communication device.

[0014] Moreover, infrared radiation layers with their radiating surfaces facing the atmosphere are typically configured such that the pores in the infrared radiation layer are fewer than those in the light reflection layer, and more preferably, the pores in the infrared radiation layer are essentially zero. This makes them less susceptible to contamination by rainwater and other contaminants, and effectively prevents dirt from absorbing sunlight and heating the infrared radiation layer.

[0015] Furthermore, by forming a structure that makes the porosity of the infrared radiation layer substantially zero, the volume ratio of the first resin material that contributes to radiation in the radiation cooling layer can be sufficiently ensured, thereby ensuring sufficient radiation cooling capacity. Moreover, thermal conductivity can be improved, making it easier for heat from the object being cooled to be transferred to the radiation surface, thus expecting an enhanced cooling effect.

[0016] Furthermore, since it is possible to achieve a configuration in which a photonic bandgap structure is substantially not formed inside the first resin layer constituting the infrared radiation layer, the emissivity of the infrared radiation layer can be increased.

[0017] In addition to the structure described so far, by forming a light-reflecting layer from a second resin having multiple pores, the inventors confirmed through experiments described later that the following resin laminate film can be achieved: the wavelength-average (arithmetic average) reflectance of the laminated resin layer incorporating the light-reflecting layer and the infrared radiation layer is 80% or more for wavelengths from 400 nm to 800 nm, the wavelength-average (arithmetic average) reflectance of the light-reflecting layer from 800 nm to 1200 nm is 70% or more, and the wavelength-average emissivity at wavelengths from 8 μm to 13 μm is 43% or more.

[0018] It should be noted that, as mentioned above, in laminated resin layers with a wavelength-average (arithmetic mean) reflectance of over 80% for wavelengths from 400nm to 800nm ​​and over 70% for wavelengths from 800nm ​​to 1200nm, the absence of metal also has an impact, resulting in the light-reflecting layer absorbing only about 2% of solar energy. Consequently, at midday in summer, the solar energy absorbed by the light-reflecting layer can reach 20W / m². 2 Below the left and right sides, radiative cooling can be performed even better.

[0019] As described above, a resin laminated film can be realized that exhibits high cooling capacity under direct sunlight, high electromagnetic transmittance, and prevents the reduction in radiative cooling performance caused by the presence of pores in the resin material and the reduction in cooling performance caused by pore contamination.

[0020] The resin laminated film is further characterized by the following aspects: The infrared radiation layer contains filler in the first resin.

[0021] As explained so far, the infrared radiation layer with the radiating surface facing the atmosphere is usually composed of a first resin layer without pores, in order to improve antifouling properties, radiative cooling capacity, and heat transfer in the direction intersecting the radiating surface. However, by including fillers in the first resin as described above, the infrared radiation layer can also achieve a certain degree of light reflection performance by utilizing the difference in refractive index between the first resin layer and the fillers.

[0022] Therefore, in addition to utilizing the solar reflection layer, the infrared radiation layer can also provide solar reflection, thus maintaining the overall reflectivity of the raw materials at a high level.

[0023] The resin laminated film is further characterized by the following aspects: The thickness of the second resin is more than 10 μm and less than 500 μm.

[0024] As described above, by setting the thickness of the second resin in the light-reflecting layer to 10 μm or more, the reflectivity required for radiative cooling can be well ensured by utilizing a light-reflecting layer composed of a second resin with multiple pores. Furthermore, by setting it to 500 μm or less, the heat insulation effect generated by the second resin having pores containing air or the like is kept below a certain level, ensuring that the cooling performance of the object being cooled is at least adequate. Incidentally, if it is 500 μm or more, from a rigidity point of view, it is difficult to follow the bend when the material is applied to a curved section, or the material will be damaged if forced to follow it, which is not ideal. Additionally, during roll-to-roll processing, if the thickness is too thick, the amount of raw material that can be produced at one time will be reduced, which is also not ideal.

[0025] That is, by selecting an appropriate material as the second resin with multiple pores and setting the thickness of the second resin to be more than 10 μm and less than 500 μm, by setting such a light-reflecting layer together with an infrared radiation layer, the following functions can be achieved: the wavelength-average (arithmetic average) reflectance of light with wavelengths from 400 nm to 800 nm is more than 80%, and the wavelength-average (arithmetic average) reflectance of light with wavelengths from 800 nm to 1200 nm is more than 70%.

[0026] It should be noted that the thickness of the light-reflecting layer is preferably 50~300um, and more preferably 75~200um.

[0027] As a further feature of resin laminated films, The thickness of the first resin is preferably 10 μm or more and 500 μm or less.

[0028] In particular, according to the resin laminate film of the present invention, since the first resin of the infrared radiating layer does not contain multiple pores, it can exhibit high radiation performance compared to an infrared radiating layer containing pores. Therefore, even when a relatively thin film layer with a thickness of 500 μm is produced, the required radiation performance can be well ensured. Incidentally, if the thickness is 500 μm or more, from a rigidity point of view, it is difficult to follow the bend when the raw material is applied to a bending section, or if it is forced to follow, the material will be damaged, which is not ideal. In addition, during roll-to-roll processing, if the thickness is too thick, the amount of raw material that can be produced at one time will be reduced, which is also not ideal.

[0029] In addition, by ensuring a thickness of 10 μm or more, the emissivity can be adequately ensured, and even if there are unevennesses on the surface of the light-reflecting layer caused by multiple pores contained in the second resin, it is difficult to reflect the unevenness on the radiating surface of the infrared radiating layer, thus effectively suppressing dirt adhesion to the radiating surface.

[0030] The resin laminated film is further characterized by the following aspects: The refractive index of the pores in the second resin is less than that of the second resin. The arithmetic mean pore size is greater than 0.1 μm and less than 3.0 μm.

[0031] As described above, the second resin of the preferred light-reflecting layer has a pore with a refractive index lower than that of the second resin, and the arithmetic mean pore size is 0.1 μm or more and 3.0 μm or less.

[0032] The inventors have confirmed that when the arithmetic mean aperture of the pores is set to multiple arithmetic mean apertures in the range of 0.1 μm to 3.0 μm, good light reflectivity can be achieved at wavelengths of 400 nm to 800 nm and 800 nm to 1200 nm.

[0033] It should be noted that, in this invention, the arithmetic mean pore diameter refers to the pore diameter obtained by arithmetically averaging the shortest inner diameter of the pores. Furthermore, regarding the shape, it can be not only spherical, but also a flat structure with short and long sides, a polyhedral structure, etc.

[0034] The resin laminated film is further characterized by the following aspects: The volume percentage of the pores in the light-reflecting layer is more than 0.1% and less than 60%.

[0035] As described above, the inventors have confirmed that by setting the volume ratio of the pores in the light-reflecting layer, the reflectivity of the light-reflecting layer can be made to the arithmetic mean reflectivity mentioned above.

[0036] It should be noted that, more preferably, the volume ratio of the pores in the light-reflecting layer is more than 1% and less than 50% by volume, and the volume ratio of the pores in the light-reflecting layer is more than 10% and less than 40% by volume.

[0037] If the porosity exceeds 60% by volume, the thermal conductivity decreases, leading to heat storage in systems with internal heat sources, which is undesirable from a heat dissipation perspective. Furthermore, a porosity exceeding 60% by volume also results in reduced strength.

[0038] Furthermore, when the volume percentage of pores is less than 0.1% by volume, it is difficult to sufficiently increase the reflectivity even if efforts are made to improve the average particle size or the configuration of the pores.

[0039] Furthermore, the laminated resin layer preferably has an arithmetic mean reflectance of 84% or more for wavelengths from 400 nm to 800 nm, and an arithmetic mean reflectance of 75% or more for wavelengths from 800 nm to 1200 nm. More preferably, the arithmetic mean reflectance of the laminated resin layer is 88% or more for wavelengths from 400 nm to 800 nm, and 80% or more for wavelengths from 800 nm to 1200 nm.

[0040] The resin laminated film is further characterized by the following aspects: The wavelength-average (arithmetic average) light transmittance of the laminated resin layer at wavelengths from 400 nm to 800 nm is greater than 1% and less than 12%.

[0041] According to the present invention, since the wavelength-average, i.e., the arithmetic average transmittance of light with wavelengths from 400 nm to 800 nm is 1% or more and less than 12%, both the first resin of the infrared radiation layer and the second resin of the light reflection layer can transmit light with wavelengths from 400 nm to 800 nm well, and the reflectivity of the laminated resin layer is well increased in the form of light reflection at the boundary between the second resin of the light reflection layer and the pores.

[0042] In other words, it can reduce the absorption rate in the laminated resin layers. Furthermore, by having a light transmittance of over 1%, it ensures good light transmission when used outdoors, which is advantageous in this respect.

[0043] Furthermore, the laminated resin layer preferably has an average emissivity of 70% or more at wavelengths of 8 μm to 13 μm, and more preferably, the laminated resin layer has an average emissivity of 85% or more at wavelengths of 8 μm to 13 μm.

[0044] The resin laminated film is further characterized by the following aspects: The second resin contains filler.

[0045] As described above, the second resin forming the light-reflecting layer contains not only the multiple pores described so far, but also filler. As a result, light can be reflected not only at the boundary between the second resin and the pores, but also at the boundary between the second resin and the filler. Therefore, even if the volume ratio of the pores to the second resin is relatively low in order to ensure a certain degree of thermal conductivity, or if the thickness is controlled to be thin, a high arithmetic mean reflectance can be maintained.

[0046] The resin laminated film is further characterized by the following aspects: The filler is selected from any one or more of the following: titanium dioxide, glass microspheres, silica, heavy calcium carbonate powder, barium sulfate, zinc sulfate, aluminum silicate, heavy calcium carbonate, alumina, zinc oxide, zirconium oxide, cerium oxide, lanthanum oxide, rhodium oxide, magnesium oxide, and barium titanate. Furthermore, they can be porous.

[0047] By including the aforementioned filler in the first resin forming the infrared radiation layer or the second resin forming the light reflection layer, a good light reflectivity can be achieved as a whole in the laminated resin layer.

[0048] It should be noted that the inventors have confirmed that, in particular, when any one or more of titanium dioxide, glass microspheres, silicon dioxide, heavy calcium carbonate powder, barium sulfate, zinc sulfate, aluminum silicate, heavy calcium carbonate, aluminum oxide, zinc oxide, zirconium oxide, cerium oxide, lanthanum oxide, rhodium oxide, magnesium oxide, and barium titanate are used as fillers, as a laminated resin layer, the wavelength-average (arithmetic mean) reflectance of light with wavelengths from 400 nm to 800 nm and the wavelength-average (arithmetic mean) reflectance of light with wavelengths from 800 nm to 1200 nm can exhibit a high reflectance that can appropriately perform the function of radiative cooling.

[0049] Furthermore, the second resin of the light-reflecting layer preferably comprises at least one of the following: polyethylene terephthalate, polypropylene, polyethylene, polyethylene naphthalate, polyvinyl chloride, polyvinylidene chloride, polyvinyl fluoride, polyvinylidene fluoride, polymethyl methacrylate, and polycarbonate. More preferably, the first resin forming the infrared radiation layer comprises at least one of the following: polyethylene terephthalate, polyethylene naphthalate, polyvinyl chloride, polyvinylidene chloride, polyvinyl fluoride, polyvinylidene fluoride, and polymethyl methacrylate.

[0050] It should be noted that the details will be discussed later, such as... Figure 2 As shown, in resins with carbon-fluorine bonds (CF), the absorption coefficients attributed to CHF and CF2 extend significantly across a broad wavelength range within the atmospheric window, from 8 μm to 13 μm, with a particularly high absorption coefficient at 8.6 μm. Furthermore, regarding the wavelength band of sunlight, there is no significant absorption coefficient at wavelengths with higher energy intensities, from 0.3 μm to 2.5 μm.

[0051] Furthermore, in resins containing carbon-chlorine bonds (C-Cl), the absorption coefficient caused by the C-Cl stretching vibration appears in a broad wavelength band centered at 12 μm with a half-value width of 1 μm or more. Additionally, in the case of vinyl chloride resins, due to the electron-withdrawing effect of chlorine, the absorption coefficient of the bending vibration (variable-angle vibration) of CH from the olefins contained in the main chain appears around 10 μm.

[0052] The inventors also considered the characteristics related to these absorptions and chose the material of the first resin mentioned above.

[0053] The first resin preferably comprises at least one of polyvinyl chloride, polyvinylidene chloride, and polyvinylidene fluoride.

[0054] In particular, regarding the wavelengths at which resin materials with carbon-fluorine bonds (CF) exhibit absorption coefficients in the ultraviolet to visible region, if the bond energies of the CC, CH, and CF bonds in the basic structural part, represented by polyvinylidene fluoride (PVDF), are calculated, they are 4.50 eV, 4.46 eV, and 5.05 eV, respectively. These correspond to wavelengths of 0.275 μm, 0.278 μm, and 0.246 μm, respectively, indicating the absorption of light at these wavelengths.

[0055] Therefore, from the viewpoint of absorbing ultraviolet rays in the first resin of the infrared radiation layer and reducing the amount of ultraviolet rays transmitted through the light reflection layer, polyvinylidene fluoride or polyvinylidene fluoride is preferably used as the first resin.

[0056] The resin laminated film is further characterized by the following aspects: The first resin contains an ultraviolet absorber. The wavelength-average, or arithmetic mean, reflectance of the ultraviolet light in the infrared radiation layer with wavelengths from 340 nm to 400 nm is less than 50%.

[0057] Based on the above-mentioned features, since the first resin forming the infrared radiation layer contains an ultraviolet absorber, and the wavelength average (arithmetic mean) reflectance of the ultraviolet light in the wavelength range of 340nm to 400nm of the infrared radiation layer is less than 50%, ultraviolet light can be appropriately absorbed by the ultraviolet absorber, while ultraviolet light is not easily reflected. This reduces the amount of ultraviolet light transmitted through the first resin forming the infrared radiation layer and the second resin forming the light reflection layer, and effectively suppresses the deterioration of the first resin layer and the second resin layer caused by ultraviolet light.

[0058] The resin laminated film is further characterized by the following aspects: The light-reflecting layer and the infrared-radiating layer are connected by a connecting layer composed of at least one of adhesives, binders, and glues, wherein the connecting layer is contained within the laminated resin layers. The connecting layer comprises at least one of filler and hollow particles.

[0059] In particular, as described above, by including fillers or hollow particles with an arithmetic mean particle size of about 0.1 μm to 5 μm in the bonding layer, the reflectivity of light in the ultraviolet to visible region can be increased, and the thickness of the laminated resin layer (especially the light reflective layer) used to obtain the desired reflectivity can be reduced.

[0060] The resin laminated film is further characterized by the following aspects: The pores of the second resin are flat in shape.

[0061] Based on the above-mentioned features, since it can have multiple layers with different refractive indices, it is easier to induce light reflection compared to the case where the pores are non-flat structures at the same thickness. This gives it the advantage of being able to easily improve reflectivity even at the same thickness.

[0062] The resin laminated films described so far can be configured as follows: On the side of the light-reflecting layer opposite to the infrared radiation layer, there is a resin layer for bonding.

[0063] Therefore, resin laminates can be appropriately bonded to other materials that are the objects of adhesion, thus effectively achieving a cooling effect on various materials. Attached Figure Description

[0064] [ Figure 1 [ ] is a diagram illustrating an embodiment of the resin laminated film.

[0065] [ Figure 2 [ ] is a diagram illustrating another embodiment of the resin laminated film.

[0066] [ Figure 3 [ ] is a graph showing the relationship between the absorption coefficient of the resin material and the wavelength band.

[0067] [ Figure 4 [This is a graph showing the relationship between the light absorption rate of the resin material and the wavelength.]

[0068] [ Figure 5 [ ] is a graph showing the emissivity spectrum of vinyl chloride resin.

[0069] [ Figure 6 [ ] is a graph showing the emissivity spectrum of vinylidene chloride resin.

[0070] [ Figure 7 [This is a graph showing the emissivity spectrum of polyethylene terephthalate resin.]

[0071] [ Figure 8 [ ] is a graph showing the relationship between the temperature of the radiating surface and the temperature of the light-reflecting layer.

[0072] [ Figure 9 [This is a graph showing the light absorption spectrum of polyethylene terephthalate resin.] Detailed Implementation

[0073] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings.

[0074] (Basic composition of resin laminated films) like Figure 1 As shown, the resin laminated film CP has the following layers in a laminated state: an infrared radiation layer J that radiates infrared light IR from the radiation surface H, and a light reflection layer B located on the side of the infrared radiation layer J opposite to the side where the radiation surface H is located; and is formed in a film shape.

[0075] That is, the resin laminated film CP is configured as a radiation cooling film.

[0076] The light-reflecting layer B has multiple pores K and is composed of a second resin. The infrared radiation layer J is composed of a first resin that emits thermal radiation energy at wavelengths from 8 μm to 13 μm that is greater than the absorbed solar energy. The infrared radiation layer J contains fewer pores K than the light-reflecting layer B. The infrared radiation layer J is a layer that is substantially free of pores K.

[0077] Furthermore, the laminated resin layer M, which incorporates the light-reflecting layer B and the infrared radiation layer J, is configured such that: the wavelength-average (arithmetic average) reflectance of light with wavelengths from 400 nm to 800 nm is 80% or more; the wavelength-average (arithmetic average) reflectance of light with wavelengths from 800 nm to 1200 nm is 70% or more; and the wavelength-average emissivity at wavelengths from 8 μm to 13 μm is 43% or more.

[0078] It should be noted that, in this specification, the laminated resin layer M refers to the concept of a connecting layer S that also includes the light-reflecting layer B and the infrared radiation layer J.

[0079] More preferably, in the laminated resin layer M, the wavelength-average (arithmetic mean) reflectance of light with wavelengths from 400 nm to 800 nm is 84% ​​or more, and the wavelength-average (arithmetic mean) reflectance of light with wavelengths from 800 nm to 1200 nm is 75% or more; in the laminated resin layer M, the wavelength-average (arithmetic mean) reflectance of light with wavelengths from 400 nm to 800 nm is 88% or more, and the wavelength-average (arithmetic mean) reflectance of light with wavelengths from 800 nm to 1200 nm is 80% or more.

[0080] Furthermore, the laminated resin layer M is more preferably characterized by an average wavelength emissivity of 70% or more at wavelengths of 8 μm to 13 μm, and even more preferably by an average wavelength emissivity of 85% or more.

[0081] Incidentally, by selecting materials with a greater difference in refractive index for the infrared radiation layer J, the connecting layer S, and the light reflection layer B, the reflectivity can be improved. As an example, the infrared radiation layer can be made of polyvinylidene chloride containing TiO2, the connecting layer S can be made of acrylic adhesive, and the light reflection layer B can be made of PET with multiple pores.

[0082] By possessing this characteristic, the laminated resin layer M can suppress the absorbed solar energy to below 2%, achieving a solar energy absorption of 20 W / m² during midday summer in Japan. 2 about.

[0083] It should be noted that in this embodiment, light L refers to light including ultraviolet light, visible light, and infrared light. If we describe these as light with wavelengths that are electromagnetic waves, then it includes electromagnetic waves with wavelengths of 10nm to 20000nm (electromagnetic waves of 0.01μm to 20μm).

[0084] The solar spectrum exists in the range of wavelengths from 300 nm to 4000 nm. The intensity increases with increasing wavelength from 400 nm, especially in the range of 500 nm to 1800 nm.

[0085] In addition, in this embodiment, the laminated resin layer M is configured such that the wavelength-average (arithmetic average) transmittance of light with a wavelength of 400 nm to 800 nm is 1% or more and 12% or less.

[0086] Therefore, the resin laminate CP is configured such that a portion of the light L incident on the resin laminate CP is reflected on the radiating surface H of the infrared radiating layer J; and the light (sunlight, etc.) that passes through the infrared radiating layer J in the light L incident on the resin laminate CP is reflected on the light reflecting layer B and escapes to the outside from the radiating surface H.

[0087] Furthermore, it is configured such that: through the infrared radiation layer J, the heat input (e.g., heat input generated by heat conduction from the object to be cooled (not shown) located on the side opposite to the side where the infrared radiation layer J is located) to the resin laminate CP is converted into infrared light IR and radiated, thereby cooling the object to be cooled.

[0088] That is, the resin laminate CP is configured to reflect the light L that is irradiated onto the resin laminate CP, and to radiate the heat transfer to the resin laminate CP (e.g., heat transfer from the atmosphere, heat transfer from the object being cooled) to the outside in the form of infrared light IR.

[0089] In addition, it is configured such that the infrared radiation layer J and the light reflection layer B are made flexible, and the resin laminate CP (radiative cooling film) is made flexible.

[0090] It should be noted that the light-reflecting layer B and the infrared radiation layer J are connected by a connecting layer S composed of at least one of adhesives, binders, and glues. Although not illustrated, this connecting layer S, by including at least one of fillers and hollow particles, can improve the reflectivity of light in the ultraviolet-visible region, thereby reducing the thickness of the laminated resin layer M (especially the light-reflecting layer) used to obtain the desired reflectivity. Here, the filler or hollow particles are suitably materials with an arithmetic mean particle size of approximately 0.1 μm or more and about 5 μm or less. As the filler, materials obtained by granulating any one or more of the following can be suitably used: titanium dioxide, glass microspheres, silica, heavy calcium carbonate powder, barium sulfate, zinc sulfate, aluminum silicate, heavy calcium carbonate, aluminum oxide, zinc oxide, zirconium oxide, cerium oxide, lanthanum oxide, rhodium oxide, magnesium oxide, and barium titanate.

[0091] This can improve the light reflectivity in the ultraviolet to visible region and reduce the thickness of the laminated resin layer M (especially the light reflective layer B) used to obtain the desired reflectivity.

[0092] In addition, the resin laminate CP is used to implement a radiation cooling method that radiates infrared light IR from the radiation surface H on the side opposite to the surface of the infrared radiation layer J that is in contact with the light reflection layer B. Specifically, the radiation cooling method is implemented by facing the sky with the radiation surface H facing the sky and radiating infrared light IR from the sky-facing radiation surface H.

[0093] (Infrared radiation layer) The first resin forming the infrared radiation layer J contains an ultraviolet absorber. The infrared radiation layer J preferably has an arithmetic mean reflectance of 50% or less, representing an ultraviolet reflectance with a wavelength of 340 nm to 400 nm. Suitable ultraviolet absorbers include benzotriazole-based, triazine-based, or hindered amine stabilizers, benzophenone-based, cyanoacrylate-based, salicylate-based, and oxaloyl aniline-based absorbers. Benzotriazole-based, triazine-based, or hindered amine stabilizers are particularly preferred because they can absorb ultraviolet light up to the longer wavelengths.

[0094] It should be noted that the first resin preferably contains at least one of the following: polyethylene terephthalate, polyethylene naphthalate, polyvinyl chloride, polyvinylidene chloride, polyvinylidene fluoride, polyvinylidene fluoride, polymethyl methacrylate, and more preferably contains at least one of polyvinyl chloride, polyvinylidene chloride, and polyvinylidene fluoride.

[0095] In the first resin that forms the infrared radiation layer J, a colorless resin material containing carbon-fluorine bonds (CF), carbon-chlorine bonds (C-Cl), carbon-oxygen bonds (CO), ester bonds (R-COO-R), ether bonds (COC bonds), and benzene rings can be used.

[0096] Regarding their respective resin materials (excluding carbon-oxygen bonds), the wavelength regions with absorption coefficients within the atmospheric window are as follows: Figure 3 As shown.

[0097] According to Kirchhoff's laws, emissivity (ε) equals light absorptivity (A). Light absorptivity can be obtained from the absorption coefficient (α) using the relationship A = 1 - exp(-αt) (hereinafter referred to as the light absorptivity relationship). It should be noted that t is the film thickness.

[0098] That is, by adjusting the thickness of the infrared radiation layer J, greater thermal radiation can be obtained in the wavelength band with a higher absorption coefficient. In the case of outdoor radiative cooling, materials with a higher absorption coefficient in the wavelength band of atmospheric window, i.e., wavelengths from 8 μm to 13 μm, can be used.

[0099] In addition, to suppress the absorption of sunlight, materials with no absorption coefficient or a small absorption coefficient in the wavelength range of 0.3 μm to 4 μm, especially 0.4 μm to 2.5 μm, can be used. From the relationship between absorption coefficient and absorptivity, it can be seen that the light absorptivity (radiative power) varies depending on the film thickness of the resin material.

[0100] In order to achieve a temperature lower than the surrounding atmosphere through radiative cooling under sunlight, if a material with a large absorption coefficient in the wavelength band of the atmospheric window and almost no absorption coefficient in the wavelength band of sunlight is selected, then by adjusting the film thickness, a state can be formed in which sunlight is hardly absorbed, but a large amount of thermal radiation is emitted from the atmospheric window, that is, the output caused by radiative cooling is greater than the input of sunlight.

[0101] Regarding carbon-fluorine bonds (CF), the absorption coefficients caused by CHF and CF2 extend significantly across a broad wavelength range of 8 μm to 13 μm within the atmospheric window, with a particularly large absorption coefficient at 8.6 μm. Furthermore, regarding the wavelength band of sunlight, there is no significant absorption coefficient at wavelengths with higher energy intensities, from 0.3 μm to 2.5 μm.

[0102] Examples of resin materials containing carbon-fluorine bonds (CF) include: Polyvinylidene fluoride (PVDF) is a partially fluorinated resin.

[0103] It should be noted that polyvinylidene fluoride (PVDF) may sometimes be referred to as PVDF resin below, but both terms refer to the same material. The same applies to other resins.

[0104] Regarding the carbon-chlorine bond (C-Cl), the absorption coefficient caused by the C-Cl stretching vibration appears in a wide band with a half-value width of more than 1 μm centered at a wavelength of 12 μm.

[0105] In addition, examples of resin materials include polyvinyl chloride (PVC) and vinylidene chloride resin (PVDC). In the case of vinyl chloride resin, due to the electron-withdrawing effect of chlorine, the absorption coefficient of the bending vibration of CH from the olefin contained in the main chain appears to be around 10 μm.

[0106] Regarding ester bonds (R-COO-R) and ether bonds (COC bonds), they exhibit absorption coefficients in the wavelength range of 7.8 μm to 9.9 μm. Furthermore, the carbon-oxygen bonds contained in ester and ether bonds show strong absorption coefficients in the wavelength range of 8 μm to 10 μm.

[0107] If a benzene ring is introduced into the side chain of a hydrocarbon resin, a broad absorption is observed in the wavelength range of 8.1 μm to 18 μm due to the vibration of the benzene ring itself or the vibration of surrounding elements caused by the influence of the benzene ring.

[0108] Resins containing these bonds include polyethylene terephthalate resin, polyethylene naphthalate resin, and polymethyl methacrylate resin.

[0109] (Examination of light absorption) The absorption of light in the ultraviolet-visible region, i.e., sunlight absorption, of resin materials possessing the aforementioned bonds and functional groups was investigated. The origin of absorption from ultraviolet to visible light is electronic transitions that facilitate bonding. The absorption in this wavelength region can be determined by calculating the bond energy.

[0110] First, consider the wavelengths at which resin materials with carbon-fluorine (CF) bonds exhibit absorption coefficients in the ultraviolet to visible region. If we calculate the bond energies of the C-C, CH, and CF bonds in the basic structural unit, exemplified by polyvinylidene fluoride (PVDF), they are 4.50 eV, 4.46 eV, and 5.05 eV, respectively. These correspond to wavelengths of light absorbed at 0.275 μm, 0.278 μm, and 0.246 μm.

[0111] Since the solar spectrum only contains long wavelengths greater than 0.300 μm, the use of fluoropolymers results in almost no absorption of ultraviolet, visible, or near-infrared radiation from sunlight. It should be noted that ultraviolet radiation is defined as short wavelengths less than 0.400 μm, visible light as the range of 0.400 μm to 0.800 μm, near-infrared light as the range of 0.800 μm to 3 μm, mid-infrared light as the range of 3 μm to 8 μm, and far-infrared light as long wavelengths greater than 8 μm.

[0112] Regarding the carbon-chlorine bond (C-Cl), the bond energy between carbon and chlorine in alkenes is 3.28 eV, with a wavelength of 0.378 μm. Therefore, it absorbs a large amount of ultraviolet light from sunlight, but has almost no absorption in the visible region.

[0113] The absorption spectrum of a 100 μm thick vinyl chloride resin from the ultraviolet to the visible region is as follows: Figure 4 As shown, light absorption increases on the short wavelength side, where the wavelength is less than 0.38 μm.

[0114] The absorption spectrum of a 100 μm thick vinylidene chloride resin from the ultraviolet to the visible region is as follows: Figure 4 As shown, some increase in the absorption spectrum can be observed on the short wavelength side, where the wavelength is less than 0.4 μm.

[0115] Resins containing ester bonds (R-COO-R), ether bonds (COC bonds), and benzene rings include methyl methacrylate resin, polyethylene terephthalate resin, and polyethylene naphthalate resin. For example, the C / C bond energy of acrylic resin is 3.93 eV, absorbing short-wavelength sunlight with wavelengths less than 0.315 μm, but exhibiting almost no absorption in the visible region.

[0116] As an example of a resin material containing these bonds and functional groups, the absorption spectrum of a 5 mm thick methyl methacrylate resin from the ultraviolet to the visible region is as follows: Figure 4 As shown. It should be noted that the methyl methacrylate resin exemplified is a common commercially available product, which contains benzotriazole-based ultraviolet absorbers.

[0117] Because the plate is 5mm thick, the wavelength with the smallest absorption coefficient becomes larger. On the short-wavelength side (less than 0.38μm) with a wavelength greater than 0.315, the light absorption increases.

[0118] As an example of a resin material possessing these bonds and functional groups, the absorption spectrum of a 40 μm thick polyethylene terephthalate resin from the ultraviolet to the visible region is as follows: Figure 4 As shown.

[0119] As shown in the figure, the absorption rate increases closer to the wavelength of 0.315 μm, and the absorption rate increases sharply at the wavelength of 0.315 μm. It should be noted that, similar to methyl methacrylate resin, as the thickness increases, the absorption rate from the absorption end of the C-C bonds increases on the longer wavelength side, which is slightly longer than 0.315 μm, and the absorption rate of ultraviolet light also increases.

[0120] The infrared radiation layer J can be made of a resin material with the aforementioned emissivity (light emissivity) and light absorption characteristics. It can be a single-layer film of a single resin material, a multilayer film of multiple resin materials, a single-layer film of a resin material made by blending multiple resin materials, or a multilayer film of a resin material made by blending multiple resin materials.

[0121] It should be noted that blends also include copolymers such as alternating copolymers, random copolymers, block copolymers, and graft copolymers; and modified products obtained by substituting side chains.

[0122] (Emissivity of vinyl chloride resin and vinylidene chloride resin) Figure 5 In this example, the emissivity of vinyl chloride resin (PVC) in an atmospheric window is shown as a representative example of resins with carbon-chlorine bonds. Additionally, Figure 6 The emissivity of vinylidene chloride resin (PVDC) in the atmospheric window is shown.

[0123] Regarding the carbon-chlorine bond, the absorption coefficient caused by the C-Cl stretching vibration appears in a broad band with a half-value width of more than 1 μm centered at a wavelength of 12 μm.

[0124] Furthermore, in the case of vinyl chloride resin, due to the electron-withdrawing effect of chlorine, the absorption coefficient of the bending vibration of CH from the olefin contained in the main chain appears to be around 10 μm. The same applies to vinylidene chloride resin.

[0125] Due to these effects, the average emissivity of a 10 μm thick film is 43% at wavelengths between 8 μm and 13 μm, falling within the specified range of 43% or higher. As shown in the figure, if the film thickness increases, the emissivity in the atmospheric window region will increase.

[0126] (Emissivity of polyethylene terephthalate resin) Figure 7 In this study, as a representative example of resins with ester bonds or benzene rings, the emissivity of polyethylene terephthalate resin in an atmospheric window is shown.

[0127] Regarding the ester bond, an absorption coefficient is observed in the wavelength range of 7.8 μm to 9.9 μm. Furthermore, the carbon-oxygen bonds contained within the ester bond exhibit a strong absorption coefficient in the wavelength range of 8 μm to 10 μm. If a benzene ring is introduced into the side chain of the hydrocarbon resin, a broad absorption is observed in the wavelength range of 8.1 μm to 18 μm due to the vibrations of the benzene ring itself or the vibrations of surrounding elements influenced by the benzene ring.

[0128] Due to these effects, the average emissivity of a 10 μm thick film is 71% at wavelengths between 8 μm and 13 μm, falling within the specified range of over 40% at average wavelengths. As shown in the figure, if the film thickness increases, the emissivity in the atmospheric window region will increase.

[0129] (Surface temperature of the light-reflecting layer and the infrared-radiating layer) Thermal radiation from the atmospheric window of the infrared radiation layer J occurs near the surface of the resin material.

[0130] according to Figure 5 In the case of vinyl chloride resin, even if the thickness exceeds 100 μm, the thermal radiation in the atmospheric window region hardly increases. That is, in the case of vinyl chloride resin, the thermal radiation in the atmospheric window is generated in the part within a depth of about 100 μm from the surface, and the radiation in the deeper part cannot escape to the outside.

[0131] Depend on Figure 6 It can be seen that vinylidene chloride resin is the same as vinyl chloride resin.

[0132] according to Figure 7 In the case of polyethylene terephthalate resin, even with a thickness exceeding 125 μm, thermal radiation in the atmospheric window region hardly increases. That is, in the case of polyethylene terephthalate resin, thermal radiation in the atmospheric window is generated in the portion approximately 100 μm deep from the surface, and radiation from deeper portions cannot escape to the outside.

[0133] As described above, thermal radiation from the atmospheric window region generated from the surface of the resin material is generated in the portion within a depth of approximately 100 μm from the surface. If the resin thickness is increased to above that, the thermal state of the resin laminate after radiative cooling is insulated by the resin material, which does not contribute to thermal radiation.

[0134] Ideally, an infrared radiating layer J is constructed using a first resin that does not absorb sunlight at all, and this infrared radiating layer J is fabricated on a light-reflecting layer B. In this case, sunlight is absorbed only at the light-reflecting layer B of the resin layer stack CP.

[0135] The thermal conductivity of resin materials is typically around 0.2 W / m / K. If this thermal conductivity is taken into account in the calculation, when the thickness of the infrared radiation layer J exceeds 20 mm, the temperature of the cooling surface (the side of the light reflection layer B opposite to the side where the infrared radiation layer J is located) will increase.

[0136] Even if an ideal resin material exists that does not absorb sunlight at all, the thermal conductivity of the first resin in the infrared radiation layer J is typically around 0.2 W / m·K. Therefore, if... Figure 8As shown, if the thickness exceeds 20 mm, the light-reflecting layer B will be heated by sunlight, and the object to be cooled, located on the side of the light-reflecting layer B, will also be heated. Therefore, the thickness of the first resin in the infrared radiation layer J needs to be less than 20 mm.

[0137] It should be noted that, Figure 8 This is a graph showing the surface temperature of the radiating surface H and the temperature of the light-reflecting layer B of a resin laminated film (radiative cooling film), calculated under the assumption of a clear summer daytime in western Japan. Sunlight intensity is set to AM1.5, and the average daytime solar radiation intensity in summer is set to 350 W / m². 2 The energy density is calculated as follows: The ambient temperature is 30°C, and the radiant energy varies with temperature, but is 100W at 30°C. This calculation assumes no solar absorption in the infrared radiation layer J. A windless state is assumed, and the convective heat transfer rate is 5W / m². 2 / K.

[0138] (Regarding the light absorption of hydrocarbon-based resins) When the resin material (first resin, second resin) is a resin with a hydrocarbon as the main chain having one or more carbon-chlorine bonds, carbon-oxygen bonds, ester bonds, ether bonds, or benzene rings, in addition to the ultraviolet absorption caused by covalent bond electrons mentioned above, absorption based on bond bending or stretching vibrations will also be observed in the near-infrared region.

[0139] Specifically, the fundamental frequency absorptions of CH3, CH2, and CH transitions to the first excited state are observed at wavelengths of 1.6 μm to 1.7 μm, 1.65 μm to 1.75 μm, and 1.7 μm, respectively. Furthermore, the fundamental frequency absorptions of the combination of CH3, CH2, and CH are observed at wavelengths of 1.35 μm, 1.38 μm, and 1.43 μm, respectively. Moreover, the overtones of CH2 and CH transitions to the second excited state are observed near a wavelength of 1.24 μm. The fundamental frequencies of CH bond bending and stretching are distributed across a broad wavelength range of 2 μm to 2.5 μm.

[0140] In addition, when ester bonds (R-COO-R) or ether bonds (COC) are present, there is a large light absorption near the wavelength of 1.9 μm.

[0141] The light absorption rate caused by these factors will be small and insignificant if the resin film thickness is thin, but will be large if the film thickness is thick.

[0142] Figure 9 The paper describes the relationship between light absorption rate and solar spectrum when the film thickness of polyethylene terephthalate resin with ester bonds and benzene rings is varied.

[0143] As shown in the figure, whenever the film thickness increases by 25 μm, 125 μm, and 500 μm, the light absorption in the long-wavelength region with wavelengths greater than 1.5 μm, caused by their respective vibrations, increases.

[0144] Furthermore, absorption increases not only at longer wavelengths but also across the entire light absorption spectrum from the ultraviolet to the visible region. This is due to the expansion of the light absorption end caused by chemical bonds.

[0145] When the film thickness is thin, the light absorption rate increases at the wavelength with the maximum absorption coefficient. However, if the film thickness increases, according to the above-mentioned light absorption rate relationship, the weak absorption coefficient with an extended absorption end will appear as an absorption rate. Therefore, if the film thickness increases, the light absorption will increase from the ultraviolet region to the visible region.

[0146] Regarding reflectivity, if the wavelength-average (arithmetic mean) reflectivity of light with wavelengths from 400nm to 800nm ​​is above 80%, and the wavelength-average (arithmetic mean) reflectivity of light with wavelengths from 800nm ​​to 1200nm is above 43%, and if the absorbed energy of sunlight has a wavelength-average emissivity of above 43% at wavelengths from 8μm to 13μm, then relative to solar energy 350W / m 2 Absorption can be suppressed to 85W / m 2 Around. Based on this, if the emissivity is above 43%, then in good atmospheric conditions, relative to 200W / m²... 2 The radiation from the left and right sides can emit 85W / m 2 The energy can thus exhibit radiative cooling function. In other words, the laminated resin layer comprising the light-reflecting layer and the infrared-radiating layer preferably has a wavelength-average (arithmetic average) reflectance of 80% or more for wavelengths from 400 nm to 800 nm, a wavelength-average (arithmetic average) reflectance of 70% or more for wavelengths from 800 nm to 1200 nm, and a wavelength-average emissivity of 43% or more for wavelengths from 8 μm to 13 μm.

[0147] The light-reflecting layer B exhibits reflectivity exceeding 80% in the wavelength range of 400nm to 800nm, and over 70% in the wavelength range of 800nm ​​to 1200nm. This allows the solar energy absorbed by the radiative cooling device (radiative cooling film) within the light-reflecting layer B to be suppressed to below 25%, meaning that the absorbed solar energy at midday in summer can be around 85W. Furthermore, under conditions of high humidity, the atmospheric window narrows, but even when radiation decreases to, for example, 125W / m², the absorption rate can still be reduced. 2 Under these conditions, as long as the emissivity is above 70%, it can still release more energy than solar energy, which is ideal.

[0148] As mentioned above, in the summer in the lowlands of Japan, the maximum infrared radiation in the wavelength band of the atmospheric window is around 160W under good atmospheric conditions at 30°C, and is usually around 125W.

[0149] If the first resin forming the infrared radiation layer J and the second resin forming the light reflection layer B are both identified as polyethylene terephthalate resins, which are hydrocarbon-based resins, then with a film thickness of 500 μm for each, the sum of the solar light absorption of the stacked resin layers M (the infrared radiation layer J and the light reflection layer B) is 176 W / m. 2 .

[0150] As described above, when both the first resin forming the infrared radiation layer J and the second resin forming the light reflection layer B are hydrocarbon-based polyethylene terephthalate resins, if the film thickness of the infrared radiation layer J and the light reflection layer B is 500 μm or more, that is, if the film thickness of the laminated resin layer M is 1000 μm or more, the radiative cooling performance cannot be achieved.

[0151] In other words, the thickness of the first resin in the infrared radiating layer J and the thickness of the second resin in the light reflecting layer B are preferably 500 μm or less. It should be noted that the thickness of the first resin in the infrared radiating layer J and the thickness of the second resin in the light reflecting layer B are preferably 10 μm or more, and the lower limit of this film thickness is determined from the viewpoint of ensuring infrared emissivity and light reflectivity.

[0152] (Regarding the light absorption of blended resins) When the resin materials (first resin and second resin) are resin materials made by blending a resin with a carbon-fluorine bond as the main chain and a resin with a hydrocarbon as the main chain, light absorption in the near-infrared region caused by CH, CH2, CH3, etc. will be observed depending on the proportion of the blended resin with a hydrocarbon as the main chain.

[0153] When carbon-fluorine bonds are the main component, the light absorption in the near-infrared region caused by hydrocarbons is reduced, so from the viewpoint of thermal conductivity, the thickness can be increased to an upper limit of 20 mm. However, when the blended hydrocarbon resin is the main component, it is necessary to make the thickness of the first resin and the second resin each less than 500 μm.

[0154] Blends of fluoropolymers and hydrocarbons also include substances in which the fluoropolymer is replaced by a hydrocarbon, or alternating copolymers of fluoropolymers and hydrocarbon monomers, random copolymers, block copolymers, and graft copolymers.

[0155] Depending on the molecular weight and proportion of the substituted hydrocarbon side chains, near-infrared light absorption caused by CH, CH2, CH3, etc., will be observed. When the monomers introduced in the form of side chains or copolymers are low molecular weight, or when the density of the introduced monomers is low, the near-infrared light absorption caused by hydrocarbons becomes smaller. Therefore, from the point of view of thermal conductivity, the thickness can be increased to a limit of 20 mm.

[0156] When a high molecular weight hydrocarbon is introduced as a side chain or comonomer of a fluoropolymer, the thickness of the first resin and the second resin must be less than 500 μm.

[0157] (Regarding the thickness of the infrared radiation layer) From the perspective of practical applications of resin laminated films (CP), a thinner infrared radiation layer (J) is preferable. The thermal conductivity of resin materials is generally lower than that of metals or glass. For effective cooling of the object, the thickness of the infrared radiation layer (J) should be at the necessary minimum. The thicker the infrared radiation layer (J), the greater the thermal radiation from the atmospheric window; however, if a certain thickness is exceeded, the thermal radiation energy in the atmospheric window will saturate.

[0158] While the saturated film thickness depends on the resin material, in the case of fluoropolymers, approximately 300 μm is sufficient for adequate saturation. Therefore, from a thermal conductivity perspective, it is desirable to keep the film thickness below 300 μm, rather than below 500 μm. Furthermore, even though thermal radiation is not yet saturated, sufficient thermal radiation can be obtained in the atmospheric window region even with a thickness of around 100 μm. The thinner the thickness, the higher the thermal conductivity, and the more effectively the temperature of the object being cooled can be reduced; therefore, in the case of fluoropolymers, a thickness of around 100 μm or less is preferable.

[0159] The absorption coefficients from carbon-silicon bonds, carbon-chlorine bonds, carbon-oxygen bonds, ester bonds, and ether bonds are greater than those caused by CF bonds. Of course, from the point of view of thermal conductivity, it is desirable to keep the film thickness below 300 μm rather than below 500 μm, but if the film thickness is further reduced to improve thermal conductivity, a greater radiative cooling effect can be expected.

[0160] In the case of resins containing carbon-chlorine bonds, carbon-oxygen bonds, ester bonds, ether bonds, and benzene rings, even a thickness of 100 μm is saturated, and even a thickness of 50 μm provides sufficient thermal radiation in the atmospheric window region. Since the thinner the resin material, the higher the thermal conductivity, and the more effectively the temperature of the object being cooled is reduced, in the case of resins containing carbon-chlorine bonds, carbon-oxygen bonds, ester bonds, ether bonds, and benzene rings, if the thickness is less than 50 μm, the thermal insulation decreases, allowing for effective cooling of the object being cooled. In the case of carbon-chlorine bonds, if the thickness is less than 100 μm, the object being cooled can be effectively cooled.

[0161] The effect of thinning is not merely to reduce thermal insulation and facilitate the transfer of heat and cold. It also lies in suppressing the absorption of near-infrared light from CH, CH2, and CH3 by resins containing carbon-chlorine bonds, carbon-oxygen bonds, ester bonds, and ether bonds. Thinning reduces the absorption of sunlight caused by these bonds, thus improving the cooling capacity of the resin laminate film (CP).

[0162] Based on the above viewpoints, in the case of resins containing carbon-chlorine bonds, carbon-oxygen bonds, ester bonds, ether bonds, and benzene rings, if the thickness is less than 50 μm, they can more effectively exert a radiative cooling effect under sunlight.

[0163] In the case of carbon-silicon bonds, even with a thickness of 50 μm, thermal radiation is saturated in the atmospheric window region, and even with a thickness of 10 μm, sufficient thermal radiation is obtained in the atmospheric window region. Since a thinner infrared radiation layer J results in a higher thermal conductivity and more effectively reduces the temperature of the object being cooled, in the case of resins containing carbon-silicon bonds, a thickness of less than 10 μm reduces thermal insulation, effectively cooling the object. Thinning further reduces the absorption of sunlight, thus improving the cooling capacity of the resin laminate CP.

[0164] Based on the above viewpoints, in the case of resins containing carbon-silicon bonds, if the thickness is less than 10 μm, the radiative cooling effect under sunlight can be more effective.

[0165] It should be noted that, as described later, resin is also used as the light-reflecting layer B in the resin laminated film CP involved in this embodiment. In the following text, although this light-reflecting layer B contains pores K in a certain volume ratio, a certain amount of thermal radiation is still expected. Taking this into account, the thickness of the aforementioned infrared radiation layer J is preferably further reduced.

[0166] (Details of the light-reflecting layer) Regarding the light-reflecting layer B, the refractive index of the second resin forming the light-reflecting layer is different from the refractive index of the internal material of the plurality of pores K contained in the second resin, thereby having the above-mentioned reflective properties (as reflective properties of the laminated resin layer M).

[0167] Specifically, the second resin of the light-reflecting layer B preferably comprises at least one of the following: polyethylene terephthalate, polypropylene, polyethylene, polyethylene naphthalate, polyvinyl chloride, polyvinylidene chloride, polyvinyl fluoride, polyvinylidene fluoride, polymethyl methacrylate, and polycarbonate. Conversely, polyimide or phenolic plastics (Bakelite) are not ideal as the second resin of the light-reflecting layer B because the resin itself is easily colored and its reflectivity is easily reduced.

[0168] Furthermore, the pores K of the second resin in the light-reflecting layer B can contain various gases or fluids, and are suitable for containing air. The refractive index of the pores K (more specifically, the gases or fluids contained in the pores K) is lower than that of the second resin.

[0169] Furthermore, the arithmetic mean pore diameter of the pores K is preferably 0.1 μm or more and 3.0 μm or less. It should be noted that, in this embodiment, the arithmetic mean pore diameter refers to the arithmetic mean of the minimum inner diameters of the pores K.

[0170] The shape of the pore K can be spherical or elliptical, but from the viewpoint of improving light reflectivity, a flat shape is preferred. More preferably, the long axis of the pore K extends in the direction along the film surface (radiating surface H) of the resin laminate CP.

[0171] Furthermore, the volume percentage of pores K in the light-reflecting layer B is preferably 0.1% or more and 60% or less, more preferably 1% or more and 50% or less, and even more preferably 10% or more and 40% or less.

[0172] Furthermore, based on in-depth research conducted by the inventors, the thickness of the second resin in the light-reflecting layer B is preferably 10 μm or more and 500 μm or less. By ensuring that the thickness of the second resin in the light-reflecting layer B is 10 μm or more, the reflectivity required for radiative cooling can be well ensured by utilizing the light-reflecting layer B composed of a second resin having multiple pores K. In addition, by ensuring that the thickness is 500 μm or less, the thermal insulation effect provided by the second resin having pores K containing air, etc., is less than a certain level, ensuring that the cooling performance of the object being cooled is at least a certain level. It should be noted that the thickness of the second resin in the light-reflecting layer B is preferably 50 to 300 μm, and more preferably 75 to 200 μm. If the thickness reaches 500 μm or more, the thermal conductivity in the thickness direction decreases and the thermal insulation is enhanced. Therefore, when applied to shells or the like with internal heat sources, the heat storage capacity inside the shell increases, which is not preferred from the viewpoint of thermal radiation.

[0173] It should be noted that, as a resin laminated film CP, such as Figure 2 As shown, fillers F (F1, F2) may also be included in the first resin forming the infrared radiation layer J and the second resin forming the light reflection layer B. The fillers F (F1, F2) may be configured to be included in at least one of the first resin forming the infrared radiation layer J and the second resin forming the light reflection layer B.

[0174] The filler F (F1, F2) can be any one or more of the following: titanium oxide, glass microspheres, silicon dioxide, heavy calcium carbonate powder, barium sulfate, zinc sulfate, aluminum silicate, heavy calcium carbonate, aluminum oxide, zinc oxide, zirconium oxide, cerium oxide, lanthanum oxide, rhodium oxide, magnesium oxide, barium titanate. The filler F1 contained in the first resin and the filler F2 contained in the second resin can be different materials.

[0175] (Experimental Results) For the examples and comparative examples of the laminated resin films described so far, various tests were conducted regarding antifouling properties, ultraviolet reflectivity, reflectivity at wavelengths of 400 nm to 800 nm, reflectivity at wavelengths of 800 nm to 1200 nm, transmittance at wavelengths of 400 nm to 800 nm, infrared emissivity, thermal conductivity, xenon weather resistance, and electromagnetic wave transmittance. The results are shown in Tables 1 to 4 below. In the test results shown in the tables, the underlined portions indicate that the conditions for each test were not met.

[0176] Incidentally, Tables 1 through 4 also show various conditions under which the membranes of the Examples and Comparative Examples are constructed.

[0177] Regarding stain resistance, a one-month outdoor exposure test was conducted in Osaka City, and the color difference ΔE before and after use was used for evaluation. A ΔE < 2.0 was defined as high (good) stain resistance. It should be noted that the color difference ΔE refers to the "CIEDE2000 color difference" based on JIS Z8781.

[0178] Ultraviolet reflectance was evaluated using the arithmetic mean of reflectance at wavelengths from 340 nm to 400 nm, measured by a UV-2600 ultraviolet-visible spectrometer (manufactured by Shimadzu Corporation). A reflectance of 50% or less was defined as meeting the condition (low ultraviolet reflectance).

[0179] The reflectance at wavelengths from 400 nm to 800 nm was evaluated using the arithmetic mean of the reflectance at wavelengths from 400 nm to 800 nm as measured by a UV-2600 UV-Vis spectrometer (manufactured by Shimadzu Corporation). A reflectance of 80% or higher was defined as meeting the condition (high reflectance at wavelengths from 400 nm to 800 nm).

[0180] The reflectance at wavelengths from 800 nm to 1200 nm was evaluated using the arithmetic mean of the reflectance at wavelengths from 800 nm to 1200 nm as measured by a UV-2600 ultraviolet-visible spectrometer (manufactured by Shimadzu Corporation). A reflectance of 70% or higher was defined as meeting the condition (high reflectance at wavelengths from 800 nm to 1200 nm).

[0181] The transmittance at wavelengths from 400 nm to 800 nm was evaluated using the arithmetic mean of the transmittance at wavelengths from 400 nm to 800 nm as measured by a UV-2600 UV-Vis spectrometer (manufactured by Shimadzu Corporation). A transmittance of 1% or more was defined as meeting the condition (high transmittance at wavelengths from 400 nm to 800 nm).

[0182] Infrared emissivity was evaluated using the arithmetic mean of emissivity measured with an FT-IR IRTracer-100 (manufactured by Shimadzu Corporation) at wavelengths from 8 μm to 13 μm. A condition was defined as meeting the requirement of high reflectivity at wavelengths from 400 nm to 800 nm when the emissivity was 70% or higher.

[0183] Thermal conductivity was measured using the laser flash method as defined in JIS R1611, and a thermal conductivity of 0.3 W / m·K or higher was defined as high (good) thermal conductivity.

[0184] Regarding xenon weather resistance, in the xenon weather resistance test defined by JIS K5600, under an environment with a black panel temperature (BPT) of 63°C, exposure to ultraviolet radiation with an intensity of 180 W / m 2 The samples were subjected to ultraviolet light for 3000 hours, and the color difference ΔE before and after the test was measured. The case where ΔE < 2.0 was defined as high weather resistance (good).

[0185] Regarding radio wave transmittance, the KEC method of the Kansai Electronics Industry Promotion Center (KEC) was used to measure the radio wave transmittance at 800MHz. A transmittance of less than 10dB was defined as high (good) radio wave transmittance.

[0186] It should be noted that in the table, PET refers to polyethylene terephthalate, PEN refers to polyethylene naphthalate, PVC refers to polyvinyl chloride, PVDC refers to polyvinylidene chloride, PVDF refers to polyvinylidene fluoride, and PP refers to polypropylene.

[0187] Regarding the sample preparation of Example 1, a thin film of polyvinyl chloride resin containing TiO2 was formed by calendering, and then laminated with a PET film containing TiO2 by dry lamination.

[0188] Table 1 Table 2 Table 3 Table 4 As shown in the above experimental results, in the resin laminated film CP involved in Examples 1 to 16 of the present invention, results were obtained that met the specified conditions for antifouling properties, ultraviolet reflectivity, reflectivity at wavelengths of 400nm to 800nm, reflectivity at wavelengths of 800nm ​​to 1200nm, transmittance at wavelengths of 400nm to 800nm, infrared emissivity, thermal conductivity, xenon weather resistance, and electromagnetic wave transmittance.

[0189] On the other hand, in Comparative Examples 1 to 4, since a relatively large number of pores K were formed on the infrared radiation layer J, which serves as the surface layer, the conditions for anti-fouling were not met, and dirt easily adhered to it.

[0190] In Comparative Examples 1 and 5, since a second resin as the light-reflecting layer B was not provided, the relevant conditions for reflectivity at wavelengths of 400 nm to 800 nm and 800 nm to 1200 nm were not met, resulting in a decrease in reflectivity.

[0191] In Comparative Example 6, since PET coated with metallic silver was used as the light reflective layer B, the transmittance condition of 400 nm to 800 nm was not met, resulting in poor light transmission, and the condition of radio wave transmittance was also not met.

[0192] Furthermore, it is believed that in Comparative Examples 1 and 5, a second resin as the light-reflecting layer B was not provided, therefore the infrared emissivity did not meet the requirements. It is speculated that the second resin as the light-reflecting layer B contributes to the infrared emissivity to a certain extent. Regarding Comparative Examples 2 and 4, it is speculated that because multiple pores K were provided in the relatively thin 100 μm infrared radiating layer J, the infrared emissivity requirements were not met.

[0193] In Comparative Examples 3 and 4, the overall thermal conductivity of the raw material is reduced because the resin layer with pores K is thicker, thus failing to meet the thermal conductivity requirement. In Comparative Examples 1 to 5, the PET has insufficient resistance to ultraviolet light and will yellow when evaluating xenon weather resistance, thus failing to meet the xenon weather resistance requirement.

[0194] (Other implementation methods) (1) The radiating surface H of the infrared radiating layer J described above may also be constructed with a protective layer (not shown). This protective layer may be made of materials such as fluorine (resin) or fluorinated acrylic (resin), and its thickness is preferably about 0.1 μm or more and about 100 μm or less. Polyethylene or polypropylene, which have low emissivity in the atmospheric window, may also be used as this material.

[0195] This protective layer has anti-fouling or anti-scratch functions and acts as a sacrificial layer.

[0196] (2) A bonding resin layer may also be provided on the side of the reflective layer B opposite to the infrared radiation layer J. As an example, the bonding resin layer may be a bonding layer made of polyvinyl chloride, thereby being suitable for bonding with membrane materials made of polyvinyl chloride, tarpaulin, and steel plates.

[0197] The following shows a specific configuration example of connecting a resin layer laminate (CPCP) to other materials using a bonding resin layer.

[0198] As one example of its application, it can be combined with membrane materials. By using a bonding resin layer to bond a general membrane material to a resin laminate (CP), a membrane material with cooling properties can be produced.

[0199] In this case, the resin layer used as the bonding layer for the resin laminate CP can be a bonding layer made of acrylic resin or resins such as polyurethane, silicone, vinyl chloride, vinylidene chloride, etc.

[0200] If it is a membrane material with resin laminated film CP, it can be sewn or heat-fused, and can be effectively used in buildings or tents, sunshades, truck tarpaulins, etc.

[0201] As one example of its application, it can be combined with a resin waterproof sheet. By using a bonding resin layer to bond a general resin waterproof sheet (e.g., "New Best-proof", manufactured by Ryūki Ryūki K.K.) to a resin laminate CP, a resin waterproof sheet with cooling properties can be produced.

[0202] In this case, the resin layer used as the bonding layer for the resin laminate CP can be a bonding layer made of acrylic resin or resins such as polyurethane, silicone, vinyl chloride, vinylidene chloride, etc.

[0203] If it is a resin waterproof sheet with resin laminate CP, it can be heat-fused and can be effectively used for roof waterproofing of buildings.

[0204] As one example of its application, it can be combined with asphalt waterproofing sheets. By using a bonding resin layer to connect a general asphalt waterproofing sheet to a resin layer laminate (CP), an asphalt waterproofing sheet with cooling properties can be produced.

[0205] In this case, the resin layer used as the bonding layer for the resin laminate CP can be a bonding layer made of acrylic resin or resins such as polyurethane, silicone, vinyl chloride, vinylidene chloride, polyester, etc.

[0206] It should be noted that, in the case of using a resin laminated membrane CP without a bonding resin layer, the asphalt waterproofing sheet and the resin laminated membrane CP can also be configured to be directly bonded by heat melting at least one of the asphalt waterproofing sheet and the resin laminated membrane CP.

[0207] If it is an asphalt waterproof sheet with resin-coated laminated film (CP), it can be adhered to building materials such as metal roofs, concrete roofs, and slate roofs, and can be effectively used for building cooling.

[0208] As one example of its application, it can be combined with clothing fabrics. By using a bonding resin layer to bond ordinary clothing fabrics with a resin laminate (CP), clothing fabrics with cooling properties can be produced.

[0209] In this case, the resin layer used as the bonding layer for the resin laminate CP can be a bonding layer made of acrylic resin or resins such as polyurethane, silicone, vinyl chloride, vinylidene chloride, polyester, etc.

[0210] It should be noted that, when using a resin laminate film CP without a bonding resin layer, the fabric and the resin laminate film CP can also be configured to be directly bonded by heat melting at least one of the fabric and the resin laminate film CP.

[0211] By using this fabric with resin-coated laminated film (CP) to make and effectively utilize clothing, it is expected to improve the feeling of heat outdoors or prevent heatstroke.

[0212] As one example of its application, it can be combined with magnetic sheets. By using a bonding resin layer to connect a general magnetic sheet to a resin layer laminate (CP), a magnetic sheet with cooling properties can be produced.

[0213] In this case, the resin layer used as the bonding layer for the resin laminate CP can be a bonding layer made of acrylic resin or resins such as polyurethane, silicone, vinyl chloride, vinylidene chloride, polyester, etc.

[0214] It should be noted that, in the case of using a resin laminate CP without a connecting resin layer, the magnetic sheet and the resin laminate CP can also be directly connected by melting the resin laminate CP with heat.

[0215] By applying this magnetic sheet with resin laminate CP to metal adhesion surfaces (such as metal casings) under outdoor sunlight, it can be effectively used for cooling the adhesion surface.

[0216] As one example of its application, it can be combined with metal sheets. By using a bonding resin layer to bond a general metal sheet (such as SUS or aluminum alloy sheet) to a resin laminate (CP), a metal sheet with cooling properties can be produced.

[0217] In this case, the resin layer used as the bonding layer for the resin laminate CP can be a bonding layer made of acrylic resin or resins such as polyurethane, silicone, vinyl chloride, vinylidene chloride, polyester, etc.

[0218] It should be noted that, when using a resin laminate CP without a bonding resin layer, the metal plate and the resin laminate CP can also be directly bonded by heat melting the resin laminate CP.

[0219] If this type of metal sheet with resin laminate CP is processed to make metal roofs or metal walls and applied to buildings, buildings with high cooling efficiency can be achieved.

[0220] As one example of its application, it can be combined with slate slabs. By using a bonding resin layer to connect a general slate slab to a resin laminate (CP), a slate slab with cooling properties can be produced.

[0221] In this case, the resin layer used as the bonding layer for the resin laminate CP can be a bonding layer made of acrylic resin or resins such as polyurethane, silicone, vinyl chloride, vinylidene chloride, polyester, etc.

[0222] It should be noted that, in the case of using a resin laminate CP without a connecting resin layer, the slate slab and the resin laminate CP can also be directly connected by melting the resin laminate CP with heat.

[0223] If slate slabs with resin laminated film (CP) are processed to make slate roofs or slate walls and applied to buildings, buildings with high cooling efficiency can be achieved.

[0224] As one example of its application, it can be combined with tiles. By using a bonding resin layer to connect ordinary tiles to a resin layer laminate (CP), tiles with cooling properties can be produced.

[0225] In this case, the resin layer used as the bonding layer for the resin laminate CP can be suitably made of acrylic resin or polyurethane, silicone, vinyl chloride, vinylidene chloride, polyester, or other resins.

[0226] If this type of tile with resin laminate film CP is applied to buildings, buildings with high cooling efficiency can be achieved.

[0227] As one example of its application, it can be combined with concrete slabs. By using a bonding resin layer to connect a general concrete slab with a resin laminate (CP), a concrete slab with cooling properties can be produced.

[0228] In this case, the resin layer used as the bonding layer for the resin laminate CP can be a bonding layer made of acrylic resin or resins such as polyurethane, silicone, vinyl chloride, vinylidene chloride, polyester, etc.

[0229] If this type of concrete slab with resin laminated film CP is processed to make concrete roofs or concrete walls and applied to buildings, buildings with high cooling efficiency can be achieved.

[0230] As one example of its application, it can be combined with siding boards. By using a bonding resin layer to connect a general siding board to a resin layer laminate (CP), a siding board with cooling properties can be produced.

[0231] In this case, the resin layer used as the bonding layer for the resin laminate CP can be a bonding layer made of acrylic resin or resins such as polyurethane, silicone, vinyl chloride, vinylidene chloride, polyester, etc.

[0232] It should be noted that, when using a resin laminate CP without a bonding resin layer, the exterior wall panel and the resin laminate CP can also be directly bonded by heat melting the resin laminate CP.

[0233] If these exterior wall panels with resin laminates (CP) are processed to manufacture walls and applied to buildings, buildings with high cooling efficiency can be achieved.

[0234] As one example of its application, it can be combined with a resin board. By using a bonding resin layer to connect a general resin board to a resin layer laminate (CP), a resin board with cooling properties can be produced.

[0235] In this case, the resin layer used as the bonding layer for the resin laminate CP can be a bonding layer made of acrylic resin or resins such as polyurethane, silicone, vinyl chloride, vinylidene chloride, polyester, etc.

[0236] It should be noted that, when using a resin laminate CP without a connecting resin layer, the resin board and the resin laminate CP can also be configured to be directly connected by heat melting at least one of the resin board or the resin laminate CP.

[0237] If a resin plate with a resin laminate CP is processed to make a shell, a shell with high outdoor cooling efficiency can be achieved.

[0238] It should be noted that the configurations disclosed in the above embodiments (including other embodiments, the same below) can be combined with the configurations disclosed in other embodiments as long as they do not cause contradictions. In addition, the embodiments disclosed in this specification are only examples, and the embodiments of the present invention are not limited thereto. Appropriate changes can be made without departing from the purpose of the present invention.

[0239] Industrial applicability The resin laminate of the present invention can be effectively used as a resin laminate that can exert high cooling capacity under direct sunlight, while also exhibiting high radio wave transmittance, and can prevent the reduction of radiative cooling performance when pores are formed in the resin material and the reduction of cooling performance due to pore contamination.

[0240] Symbol Explanation B: Light-reflecting layer CP: Resin laminated film F: Packing material H: Radiation surface IR: Infrared light J: Infrared radiation layer K: Porosity M: Laminated resin layer S: Connector layer.

Claims

1. A resin laminate film comprising: an infrared radiating layer that radiates infrared light from a radiating surface; and a light-reflecting layer located on the side of the infrared radiating layer opposite to the side containing the radiating surface. The light-reflecting layer has multiple pores and is composed of a second resin. The infrared radiation layer is composed of a first resin that emits thermal radiation energy at wavelengths from 8 μm to 13 μm that is greater than the absorbed solar energy. The number of pores in the infrared radiation layer is less than the number of pores in the light reflection layer. The laminated resin layer comprising the light-reflecting layer and the infrared-radiating layer has a wavelength-average (arithmetic average) light reflectance of 80% or more at wavelengths from 400 nm to 800 nm, a wavelength-average (arithmetic average) light reflectance of 70% or more at wavelengths from 800 nm to 1200 nm, and a wavelength-average emissivity of 43% or more at wavelengths from 8 μm to 13 μm.

2. The resin laminated film according to claim 1, wherein, The infrared radiation layer contains filler in the first resin.

3. The resin laminated film according to claim 1 or 2, wherein, The thickness of the second resin is more than 10 μm and less than 500 μm.

4. The resin laminated film according to claim 1 or 2, wherein, The thickness of the first resin is more than 10 μm and less than 500 μm.

5. The resin laminated film according to claim 1 or 2, wherein, The refractive index of the pores in the second resin is less than that of the second resin. The arithmetic mean pore size is greater than 0.1 μm and less than 3.0 μm.

6. The resin laminated film according to claim 1 or 2, wherein, The volume percentage of the pores in the light-reflecting layer is more than 0.1% and less than 60%.

7. The resin laminated film according to claim 1 or 2, wherein, The volume percentage of the pores in the laminated resin layer is more than 1% by volume and less than 50% by volume.

8. The resin laminated film according to claim 1 or 2, wherein, The volume percentage of the pores in the laminated resin layer is 10% or more and 40% or less.

9. The resin laminated film according to claim 1 or 2, wherein, The wavelength-average (arithmetic mean) reflectance of the laminated resin layer at wavelengths of 400nm to 800nm ​​is above 88%, and the wavelength-average (arithmetic mean) reflectance at wavelengths of 800nm ​​to 1200nm is above 80%.

10. The resin laminated film according to claim 1 or 2, wherein, The wavelength-average (arithmetic average) light transmittance of the laminated resin layer at wavelengths from 400 nm to 800 nm is greater than 1% and less than 12%.

11. The resin laminated film according to claim 1 or 2, wherein, The average wavelength emissivity of the laminated resin layer at wavelengths from 8 μm to 13 μm is over 70%.

12. The resin laminated film according to claim 1 or 2, wherein, The second resin contains filler.

13. The resin laminated film according to claim 2, wherein, The filler is any one or more of the following: titanium dioxide, glass microspheres, silicon dioxide, heavy calcium carbonate powder, barium sulfate, zinc sulfate, aluminum silicate, heavy calcium carbonate, aluminum oxide, zinc oxide, zirconium oxide, cerium oxide, lanthanum oxide, rhodium oxide, magnesium oxide, and barium titanate.

14. The resin laminated film according to claim 12, wherein, The filler is any one or more of the following: titanium dioxide, glass microspheres, silicon dioxide, heavy calcium carbonate powder, barium sulfate, zinc sulfate, aluminum silicate, heavy calcium carbonate, aluminum oxide, zinc oxide, zirconium oxide, cerium oxide, lanthanum oxide, rhodium oxide, magnesium oxide, and barium titanate.

15. The resin laminated film according to claim 1 or 2, wherein, The second resin comprises at least one of the following: polyethylene terephthalate, polypropylene, polyethylene, polyethylene naphthalate, polyvinyl chloride, polyvinylidene chloride, polyvinyl fluoride, polyvinylidene fluoride, polymethyl methacrylate, and polycarbonate.

16. The resin laminated film according to claim 1 or 2, wherein, The first resin comprises at least one of the following: polyethylene terephthalate, polyethylene naphthalate, polyvinyl chloride, polyvinylidene chloride, polyvinylidene fluoride, polyvinylidene fluoride, and polymethyl methacrylate.

17. The resin laminated film according to claim 1 or 2, wherein, The first resin comprises at least one of polyvinyl chloride, polyvinylidene chloride, and polyvinylidene fluoride.

18. The resin laminated film according to claim 1 or 2, wherein, The first resin contains an ultraviolet absorber. The wavelength-average, or arithmetic mean, reflectance of the ultraviolet light in the infrared radiation layer with wavelengths from 340 nm to 400 nm is less than 50%.

19. The resin laminated film according to claim 1 or 2, wherein, The light-reflecting layer and the infrared-radiating layer are connected by a connecting layer composed of at least one of adhesives, bonding agents, and glues. The connecting layer is contained within the laminated resin layers.

20. The resin laminated film according to claim 19, wherein, The connecting layer comprises at least one of filler and hollow particles.

21. The resin laminated film according to claim 1 or 2, wherein, The pores of the second resin are flat in shape.

22. The resin laminated film according to claim 1 or 2, wherein, A bonding resin layer is provided on the side of the light-reflecting layer opposite to the infrared radiation layer side.

Citation Information

Patent Citations

  • Systems and methods for radiative cooling and heating

    JP2018526599A

  • Composite cooling film and article containing the same

    JP2022528289A

  • Laminate structure

    WO2018062541A1