sintered body

By adding specific elements and controlling the crystallite diameter in zirconia sintered bodies, the problems of impact resistance and light-blocking properties of thin zirconia sintered bodies were solved, achieving high impact resistance and light opacity, and improving design flexibility.

CN123125183APending Publication Date: 2026-11-17TOSOH CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202580028847.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-23
Filing Date
2025-04-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing zirconia sintered bodies are difficult to simultaneously possess high impact resistance and light-shielding properties in thin shapes, and their light transmittance leads to design compromises.

Method used

By adding stabilizing elements such as yttrium, lanthanum, neodymium, gadolinium, erbium, and ytterbium to zirconia sintered bodies, combined with niobium, alumina, iron, cobalt, and zinc, the crystallite diameter is controlled within the range of 25 nm to 100 nm, forming spinel-type metal oxides, thereby improving light-shielding properties and impact resistance.

Benefits of technology

It has been achieved that sintered zirconia bodies with a thickness of less than 0.5 mm can maintain high impact resistance while being opaque, thus improving design flexibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125183A_ABST
    Figure CN123125183A_ABST
Patent Text Reader

Abstract

This invention provides a zirconia sintered body that exhibits high impact resistance even in thin shapes with a thickness of less than 0.5 mm, and high light-shielding properties that prevent the substrate from being visible. It contains stabilizing elements, niobium, alumina, and iron, cobalt, and zinc as pigment components, and has a crystallite diameter of 25 nm or more and 100 nm or less, calculated from the XRD peaks of the (111) facet of tetragonal zirconia.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to sintered bodies, and more particularly to sintered bodies that are impact-resistant and light-shielding and are mainly composed of zirconium oxide. Background Technology

[0002] Zirconia-based sintered bodies (zirconia sintered bodies) possess not only high strength and toughness but also high aesthetic appeal. Therefore, their application in decorative uses, such as exterior components for watches and portable electronic devices, is under investigation. Particularly in the application of zirconia sintered bodies in mobile and wearable devices such as smartphones and smartwatches, lightweight designs are required. Therefore, high strength and impact resistance that prevent cracking even in thin shapes are essential.

[0003] As a material with impact resistance in a thin shape, composite materials (laminated materials) have been proposed, which are made by laminating zirconia sintered bodies with synthetic resins, fiber-reinforced plastics, etc. For example, Patent Document 1 reports a composite plate made by combining a zirconia matrix with a polymer material. It is reported that the thickness of the composite plate is less than 1 mm, and the height at which it breaks when a 20g steel ball is dropped on it is more than 40 cm, demonstrating high impact resistance.

[0004] Existing technical documents Patent documents Patent Document 1: Japanese Patent Application Publication No. 2014-54780 Patent Document 2: Japanese Patent Application Publication No. 2020-180048 Summary of the Invention

[0005] The problem that the invention aims to solve Patent Document 1 describes a composite plate that requires layering zirconia-based ceramic components with resin materials, complicating the manufacturing process. Therefore, a material with high impact resistance even in a thin shape is required, even if only a zirconia sintered body is used. Furthermore, when thin outer components are made solely from zirconia sintered bodies, the translucency of zirconia allows the base component to be seen through the top of the outer component, impairing design. Patent Document 2 discloses incorporating alumina and titanium dioxide as light-shielding materials to adjust the translucency of dental zirconia sintered bodies. However, when such zirconia sintered bodies are made into a shape with a thickness of 0.5 mm or less (thin shape), the base component is visible. Moreover, since alumina has low toughness, the fracture toughness of the zirconia sintered body decreases with increasing alumina content, resulting in reduced impact resistance.

[0006] The present invention provides a zirconia sintered body that has high impact resistance even in thin shapes with a thickness of less than 0.5 mm, and has light-shielding properties that prevent the base component from being exposed.

[0007] Methods for solving problems That is, the present invention is as described in the claims; in addition, the gist of the present invention is as follows.

[0008] [1] A zirconia sintered body comprising stabilizing elements, niobium, alumina, and iron, cobalt and zinc as pigment components, wherein the crystallite diameter of the zirconia sintered body, calculated from the peak of the XRD belonging to the (111) plane of tetragonal zirconia, is 25 nm or more and 100 nm or less.

[0009] [2] According to the zirconia sintered body of [1], wherein at least a portion of the pigment component forms a spinel-type metal oxide.

[0010] [3] The zirconia sintered body according to [1] or [2], wherein the stabilizing element comprises at least one selected from calcium, yttrium, lanthanum, neodymium, gadolinium, erbium and ytterbium, and the content of the stabilizer is more than 2.0 mol% and less than 5.5 mol%.

[0011] [4] The zirconia sintered body according to any one of [1] to [3], wherein the niobium content is 0.1% by mass or more and 3.0% by mass or less.

[0012] [5] The zirconia sintered body according to any one of [1] to [4], wherein the alumina content is greater than 0% by mass and less than 30% by mass.

[0013] [6] The zirconia sintered body according to any one of [1] to [5], wherein, in terms of oxides, the iron content is 0.1% by mass or more and 5% by mass or less, the cobalt content is 0.1% by mass or more and 3% by mass or less, and the zinc content is 0.05% by mass or more and 1% by mass or less.

[0014] [7] The zirconia sintered body according to any one of [1] to [6], wherein the peaks at the (400) facets of the tetragonal zirconia are 2 θ 2 with the peak of the (004) plane belonging to tetragonal zirconia θ The difference is more than 1.54°.

[0015] [8] A zirconia sintered body according to any one of [1] to [7], wherein the lightness L of the zirconia sintered body is Those aged 40 and above and 65 and below.

[0016] [9] A zirconia sintered body as described in any one of [1] to [8], wherein the total light transmittance of the zirconia sintered body when the thickness is 0.5 mm is less than 0.1%.

[0017]

[10] A zirconium oxide powder comprising stabilizing elements, niobium, aluminum oxide, and iron, cobalt, and zinc as pigment components. The stabilizer content is 2.0 mol% or more and 5.5 mol% or less, the niobium content is 0.1 wt% or more and 3.0 wt% or less, and the alumina content is greater than 0 wt% and 30 wt% or less. The zirconia powder has a BET specific surface area of ​​5.0 m². 2 / g or more and 17m 2 / g or less.

[0018]

[11] The zirconium oxide powder according to

[10] , wherein the pigment component is contained in the zirconium oxide powder in the form of a spinel-type metal oxide comprising iron, cobalt and zinc.

[0019]

[12] The zirconium oxide powder according to

[10] or

[11] , wherein the zirconium oxide powder, in terms of oxides, has an iron content of 0.1% by mass or more and 5% by mass or less, a cobalt content of 0.1% by mass or more and 3% by mass or less, and a zinc content of 0.05% by mass or more and 1% by mass or less.

[0020]

[13] The zirconium oxide powder according to any one of

[10] to

[12] , wherein the 10% particle size D10 in the cumulative particle size distribution of the powder is 0.15. μ m or more and 0.5 μ The particle size is below 1 μm, and 90% of the particles have a D90 of 0.5 μm. μ m or more and 1.3 μ Below m.

[0021]

[14] A component comprising any one of the following: [1] to [9] sintered zirconium oxide. Attached Figure Description

[0022] Figure 1 This is a schematic diagram of the falling ball test apparatus.

[0023] Figure 2 This is a schematic diagram of the sample used in the falling ball test.

[0024] Figure 3 This is a schematic diagram illustrating the ball-dropping test.

[0025] Figure 4A This is a photograph of the appearance of the zirconia sintered body of Comparative Example 4.

[0026] Figure 4B This is a photograph of the appearance of the zirconia sintered body of Comparative Example 4 (the translucent appearance of the sintered body).

[0027] Figure 5 This is a photograph of the appearance of the zirconia sintered body in Example 9 (the sintered body is opaque). Detailed Implementation

[0028] The following description illustrates an example of an embodiment of the present invention. The present invention includes any combination of the components and parameters disclosed in this specification; furthermore, the range of any combination of the upper and lower limits of the values ​​disclosed in this specification is also included in the present invention.

[0029] (Sintered body) This embodiment is a zirconia sintered body containing stabilizing elements, niobium, alumina, and iron, cobalt, and zinc as pigment components, with a crystallite diameter of 25 nm or more and 100 nm or less calculated from the XRD peaks of the (111) plane of tetragonal zirconia (hereinafter also referred to as "the sintered body of this embodiment"). Furthermore, the sintered body of this embodiment is a zirconia sintered body containing niobium, alumina, and iron, cobalt, and zinc as pigment components, with a crystallite diameter of 25 nm or more and 100 nm or less calculated from the XRD peaks of the (111) plane of tetragonal zirconia, and containing stabilizing elements. By including niobium, alumina, and iron, cobalt, and zinc as pigment components—elements already known for addition to zirconia sintered bodies—and satisfying this configuration, a zirconia sintered body with high impact resistance and shielding properties that prevent the substrate material from penetrating is obtained. The sintered body of this embodiment is a sintered body containing zirconium oxide with stabilizing elements. It is a sintered body with zirconium oxide containing stabilizing elements as the main phase, and further, it is a sintered body with the highest proportion (especially the mass proportion) of zirconium oxide in the composition of the sintered body. It is a so-called zirconium oxide sintered body. The stabilizing element is an element that has the function of stabilizing zirconium oxide. The stabilizing element contained in the sintered body of this embodiment is preferably selected from one or more of calcium (Ca), magnesium (Mg), scandium (Sc), lanthanum (La), yttrium (Y), neodymium (Nd), cerium (Ce), gadolinium (Gd), erbium (Er) and ytterbium (Yb); selected from one or more of calcium, yttrium, lanthanum, neodymium, gadolinium, erbium and ytterbium; selected from one or more of yttrium, lanthanum, neodymium, gadolinium and erbium; selected from at least one of yttrium and erbium; or yttrium.

[0030] The sintered body of this embodiment may contain two or more stabilizing elements. In this case, the stabilizing elements may be selected from two or more of calcium, magnesium, scandium, lanthanum, yttrium, neodymium, cerium, gadolinium, erbium, and ytterbium. Preferably, it is a combination of yttrium and other stabilizing elements (hereinafter, when the sintered body contains this combination of stabilizing elements, the stabilizing elements other than yttrium are also referred to as "secondary stabilizing elements"). The secondary stabilizing elements contained in the sintered body of this embodiment are preferably selected from one or more of calcium, magnesium, scandium, lanthanum, neodymium, cerium, gadolinium, erbium, and ytterbium. More preferably, they are selected from one or more of lanthanum, erbium, and neodymium. Even more preferably, they are selected from one or more of lanthanum, erbium, or neodymium. Erbium is even more preferred.

[0031] The content of stabilizing elements (hereinafter also referred to as "stabilizing element amount," and when the stabilizing element is yttrium, etc., it is also referred to as "yttrium amount," etc.) is sufficient to stabilize the crystal phase of zirconia. Examples of stabilizing element amounts include greater than 0 mol%, 1.5 mol% or more, 2.0 mol% or more, or 2.5 mol% or more, and less than 8.5 mol%, 5.5 mol% or less, 4.0 mol% or less, 3.4 mol% or less, or 3.2 mol% or less. By setting the stabilizing element amount to 2.0 mol% or more and 5.5 mol% or less, the zirconia in the sintered body is mainly composed of tetragonal zirconia. Preferably, the stabilizing element amount of the sintered body in this embodiment is greater than 0 mol% and less than 8.5 mol%, 1.5 mol% or more and 5.5 mol% or less, 2.0 mol% or more and 4.0 mol% or less, 2.5 mol% or more and 4.0 mol% or less, or 2.5 mol% or more and 3.2 mol% or less.

[0032] When the sintered body contains secondary stabilizing elements, the total content of one or more secondary stabilizing elements (hereinafter also referred to as "amount of secondary stabilizing elements") may be greater than 0 mol%, 0.05 mol% or more, or 0.10 mol% or more, 0.20 mol% or more, or 1.0 mol% or more, and less than 5.5 mol%, 4.0 mol% or less, 3.0 mol% or less, or 1.9 mol% or less. The amount of secondary stabilizing elements is preferably greater than 0 mol% and less than 5.5 mol%, 0.05 mol% or more and 4.0 mol% or less, or 0.10 mol% or more and 3.0 mol% or less, 0.20 mol% or more and 1.9 mol% or less, or 1.0 mol% or more and 1.9 mol% or less.

[0033] The content of each stabilizing element is arbitrary, provided that the total content of the stabilizing elements meets the above-mentioned amount of stabilizing elements. Examples of the content of each stabilizing element include the following: Yttrium content can be greater than 0 mol%, 1.0 mol% or more, 1.5 mol% or more, 2.0 mol% or more, or 2.5 mol% or more, and less than 4.0 mol%, 3.5 mol% or less, 3.0 mol% or less, or less than 3.0 mol%, preferably greater than 0 mol% and less than 4.0 mol%, 1.0 mol% or more and 3.5 mol% or less, 1.5 mol% or more and 3.0 mol% or less, or 2.5 mol% or more and 3.0 mol% or less.

[0034] When the secondary stabilizing element is erbium, the amount of erbium can be greater than 0 mol%, greater than 0.03 mol%, or greater than 1.0 mol%, and less than 4.0 mol%, less than 3.0 mol%, less than 2.0 mol%, or less than 1.9 mol%, preferably greater than 0 mol% and less than 4.0 mol%, greater than 0.01 mol% and less than 3.0 mol%, greater than 0.03 mol% and less than 2.0 mol%, or greater than 1.0 mol% and less than 1.9 mol%.

[0035] When neodymium is the secondary stabilizing element, the amount of neodymium can be greater than 0 mol%, greater than 0.01 mol%, greater than 0.03 mol%, greater than 0.2 mol%, or greater than 0.25 mol%, and less than 4.0 mol%, less than 3.0 mol%, less than 2.0 mol%, less than 0.5 mol%, or less than 0.4 mol%. More preferably, it is greater than 0 mol% and less than 4.0 mol%, greater than 0.01 mol% and less than 2.0 mol%, greater than 0.03 mol% and less than 0.5 mol%, or greater than 0.09 mol% and less than 0.4 mol%.

[0036] When the secondary stabilizing element is lanthanum, the amount of lanthanum can be greater than 0 mol%, greater than 0.01 mol%, greater than 0.03 mol%, or greater than 0.1 mol%, and less than 4.0 mol%, less than 3.0 mol%, less than 2.0 mol%, or less than 0.5 mol%. More preferably, it is greater than 0 mol% and less than 4.0 mol%, greater than 0.01 mol% and less than 0.5 mol%, or greater than 0.1 mol% and less than 0.5 mol%.

[0037] In this embodiment, "amount of stabilizing elements" is the ratio (mol%) of the total amount of stabilizing elements converted from oxides to the total amount of stabilizing elements converted from zirconium oxide and oxides. In addition, "amount of secondary stabilizing elements" is the ratio (mol%) of the total amount of secondary stabilizing elements converted from oxides to the total amount of secondary stabilizing elements converted from zirconium oxide and oxides.

[0038] The sintered body of this embodiment contains niobium (Nb). By including niobium, it is expected that the impact resistance and light-shielding properties of the sintered body will be improved. The niobium content (hereinafter also referred to as "niobium content") can be greater than 0% by mass, greater than 0.1% by mass, 0.5% by mass or more, or 1.0% by mass or more, and less than 3.0% by mass, less than 2.5% by mass, or less than 2.0% by mass. In addition, the niobium content can be greater than 0% by mass and less than 3.0% by mass, more than 1.0% by mass and less than 2.5% by mass, or more than 1.5% by mass and less than 2.0% by mass. The form of niobium contained in the sintered body of this embodiment is arbitrary. For example, niobium can be contained in the sintered body as niobium oxide (Nb2O5) particles, i.e., second-phase particles, without solid dissolution. Part or all of the niobium can be dissolved in zirconium oxide, or it can react with oxides other than zirconium oxide in the sintered body to form a composite oxide.

[0039] In this embodiment, the niobium content is the ratio of the mass of niobium to the total mass of zirconium oxide, stabilizing elements, niobium, aluminum, and pigment components.

[0040] The powder in this embodiment contains alumina (Al2O3). The alumina content (hereinafter also referred to as "alumina content") can be greater than 0% by mass and less than 30% by mass. By including alumina (i.e., the alumina content is greater than 0% by mass), a dense sintered body can be easily obtained even at lower temperatures. To improve shielding properties, the alumina content is preferably 0% by mass or more, greater than 0% by mass, 0.005% by mass or more, 0.05% by mass or more, 0.1% by mass or more, 0.25% by mass or more, 0.5% by mass or more, or 1% by mass or more. On the other hand, to improve mechanical properties, such as static strength, the alumina content can be less than 30% by mass, less than 20% by mass, less than 10% by mass, less than 5% by mass, or less than 2% by mass. The alumina content of the sintered body in this embodiment can be greater than 0% by mass and less than 20% by mass, or more than 0.1% by mass and less than 10% by mass.

[0041] Alumina can be included as at least one of alumina particles and aluminum-containing composite oxide particles, and further as alumina particles, i.e., second-phase particles, and a portion of it can be dissolved in zirconium oxide.

[0042] The sintered body of this embodiment includes iron, cobalt, and zinc as pigment components. The pigment components in the sintered body refer to components (elements) that have the function of coloring the sintered body. Therefore, the sintered body can exhibit any hue different from the original hue of zirconium oxide. In particular, by including iron, cobalt, and zinc in the pigment components, in addition to improving the opacity of the sintered body, a dense sintered body is easily obtained even when sintering at a lower temperature. It should be noted that the aforementioned stabilizing elements sometimes also include elements that have the function of coloring the sintered body. However, for convenience, in the calculation of the composition in this embodiment, these stabilizing elements are not included in the pigment components but are calculated as stabilizing elements. Examples of stabilizing elements that have the function of coloring the sintered body include neodymium, cerium, and erbium.

[0043] The iron, cobalt and zinc contents of the sintered body in this embodiment (hereinafter, their respective contents are also referred to as "iron content", "cobalt content" and "zinc content") are preferably the following amounts.

[0044] The iron content can be 0.10% by mass or more, preferably 0.20% by mass or more, 0.30% by mass or more, or 0.50% by mass or more, and can be 5.0% by mass or less, preferably 4.5% by mass or less, 3.0% by mass or less, or 2.0% by mass or less. Further, the iron content can be 0.10% by mass or more and 5.0% by mass or less, more preferably 0.20% by mass or more and 4.5% by mass or less, 0.30% by mass or more and 3.0% by mass or less, or 0.50% by mass or more and 2.0% by mass or less.

[0045] The amount of cobalt can be 0.10% by mass or more, preferably 0.20% by mass or more or 0.25% by mass or more, and can be 3.0% by mass or less, preferably 2.0% by mass or less, 1.5% by mass or less or 1.0% by mass or less. Furthermore, the amount of cobalt can be 0.10% by mass or more and 3.0% by mass or less, and more than 0.20% by mass or less and 2.0% by mass or less, 0.25% by mass or more and 1.5% by mass or less, or 0.25% by mass or more and 1.0% by mass or less.

[0046] The zinc content can be 0.05% by mass or more, preferably 0.10% by mass or more, and can be 1.0% by mass or less, preferably 0.70% by mass or less or 0.50% by mass or less. Furthermore, the zinc content can be 0.05% by mass or more and 1.0% by mass or less, preferably 0.10% by mass to 0.70% by mass, and more preferably higher than 0.10% by mass and 0.50% by mass or less.

[0047] The sintered body of this embodiment may further contain pigment components other than iron, cobalt, and zinc (hereinafter also referred to as "other pigment component amounts"). As other pigment components, compounds containing metallic elements are preferred, and further, transition metal elements and compounds containing them are preferred. Specific examples of pigment components other than iron, cobalt, and zinc include one or more elements selected from vanadium (V), manganese (Mn), nickel (Ni), and copper (Cu), and compounds containing one or more of these elements, as well as oxides containing one or more of these elements. The sintered body of this embodiment may contain chromium (Cr) as a pigment component, but from an environmental perspective, it is preferable not to contain chromium.

[0048] As a pigment component, for example, by sintering a substance in which pigment is mixed in zirconia powder, it is possible to include a coloring element derived from the pigment powder or a compound containing the coloring element as a pigment component in the zirconia sintered body.

[0049] In this embodiment, the pigment component in the sintered body preferably consists of a portion or all of a spinel-type metal oxide. By forming a portion or all of the pigment component into a spinel-type metal oxide, in addition to improved opacity, the hue is more easily stabilized. The spinel-type metal oxide is represented by AB₂O₄, where A and B are preferably selected from one or more of Mg, Ca, Sr, Y, La, Gd, V, Mn, Fe, Co, Ni, Cu, Zn, and Al; more preferably, it is represented by AB₂O₄, where A and B are selected from one or more of Mg, Ca, Sr, Y, Gd, Fe, Co, Ni, Zn, and Al. When the spinel-type metal oxide in the sintered body of this embodiment is represented by AB₂O₄, it can contain multiple elements at sites A and B. When multiple elements are contained at sites A and B, the composition ratio of each element at site A and site B is arbitrary. Specific spinel-type metal oxides include one or more selected from CoAl2O4, ZnFe2O4, MgFe2O4, CoFe2O4, NiFe2O4, Co(Fe,Al)2O4, and (Co,Zn)(Fe,Al)2O4.

[0050] In this embodiment, regarding whether the pigment component forms a spinel-type metal oxide, based on the powder X-ray diffraction (hereinafter also referred to as XRD) pattern of the zirconia powder of this embodiment, it is determined by the 2 planes corresponding to the spinel-type metal oxide (311). θ The presence of a peak at 36.3±0.5 can be used for confirmation.

[0051] In this embodiment, the X-ray diffraction pattern of the sintered body when the pigment component forms a spinel-type metal oxide can be determined by using a conventional crystallization analysis X-ray diffraction apparatus (e.g., Ultima IV, manufactured by RIGAKU).

[0052] The following conditions can be cited as test conditions.

[0053] X-ray source: CuK α ray( λ =0.15418nm) Tube voltage: 45kV Tube current: 40mA Measurement mode: Continuous scanning Scanning speed: 4° / minute Step size: 0.02° Measurement range: 2 θ =32° and above and 40° and below Goniometer: radius 185mm As the test specimen, a sintered body in the shape of a circular plate with a diameter of 20 mm and a thickness of 1.0 mm was used, and the surface to be evaluated was mirror-polished (surface roughness Ra ≤ 0.02). μ The method involves irradiating the polished surface with X-rays to measure the surface (m).

[0054] The content of other pigment components in the sintered body of this embodiment (hereinafter also referred to as "amount of other pigment components," and in the case of other pigment components such as manganese, also referred to as "amount of manganese," etc.) can be arbitrary as long as it is within the range of exerting the effect of the present invention. It is preferably greater than 0% by mass, 0.001% by mass or more, 0.005% by mass or more, 0.01% by mass or more, 0.05% by mass or more, or 0.1% by mass or more, and preferably 5.0% by mass or less, 3.5% by mass or less, 3.0% by mass or less, 1.0% by mass or less, or 0.7% by mass or less. In addition, examples of other pigment component amounts include 0% by mass or more and 5.0% by mass or less, 0.01% by mass or more and 3.0% by mass or less, 0.1% by mass or more and 1.0% by mass or less, or 0.1% by mass or more and 0.7% by mass or less.

[0055] The sintered body of this embodiment may contain one or more additives selected from silicon dioxide (SiO2), titanium dioxide (TiO2), and gallium oxide (Ga2O3). By including such additives, a sintered body with desired mechanical properties can be produced. The content of the additive (hereinafter also referred to as "amount of additive") may be 0% by mass or more, 0.5% by mass or more, or 1.0% by mass or more, and may be 5.0% by mass or less or 2.5% by mass or less. In addition, the amount of additive may be 0% by mass or more and 5.0% by mass or less, or 1.0% by mass or more and 2.5% by mass or less.

[0056] In this embodiment, the niobium, alumina, pigment components, and additives in the sintered body can be contained in the sintered body in any form. They can be contained in the form of compounds, and further in the form of composite oxides and at least one of oxides. Alternatively, they can be contained in part or all of them by solid dissolution in zirconium oxide.

[0057] In this embodiment, the amounts of niobium, alumina, pigment, other pigments, and additives are the ratios (mass%) of the mass of each of the niobium, alumina, pigment, other pigments, and additives (calculated as oxides) to the total mass of zirconium oxide and the metal elements (calculated as oxides).

[0058] Examples of oxide conversions in this embodiment include: calcium as CaO, magnesium as MgO, scandium as Sc2O3, yttrium as Y2O3, lanthanum as La2O3, neodymium as Nd2O3, cerium as CeO2, gadolinium as Gd2O3, erbium as Er2O3, ytterbium as Yb2O3, niobium as Nb2O5, aluminum as Al2O3, silicon as SiO2, gallium as Ga2O3, vanadium as V2O5, chromium as Cr2O3, iron as Fe2O3, cobalt as Co3O4, manganese as Mn3O4, nickel as NiO, copper as CuO, and zinc as ZnO.

[0059] The sintered body of this embodiment may contain unavoidable impurities such as hafnium oxide (HfO2). In this embodiment, the content of each component in the sintered body can be calculated by treating hafnium oxide as zirconium oxide (ZrO2) and calculating their values.

[0060] For example, the composition (content of each component) of the sintered body of this embodiment, which includes alumina and niobium, as pigment components iron, cobalt and zinc, and zirconia sintered body (the same applies to the powder described later) containing gadolinium and yttrium as stabilizing elements, can be calculated as follows.

[0061] Pigment composition [mass %] = {(Fe2O3+Co3O4+ZnO) / (Gd2O3+Y2O3+ZrO2+Nb2O5+Mn3O4+Al2O3+Fe2O3 +Co3O4+ZnO)}×100 Iron content [mass %] = {Fe2O3 / (Gd2O3+Y2O3+ZrO2)} +Nb2O5+Al2O3+Fe2O3+Co3O4+ZnO)}×100 Cobalt content [mass %] = {Co3O4 / (Gd2O3+Y2O3+ZrO2)} +Nb2O5+Al2O3+Fe2O3+Co3O4+ZnO)}×100 Zinc content [mass %] = {ZnO / (Gd2O3 + Y2O3 + ZrO2)} +Nb2O5+Al2O3+Fe2O3+Co3O4+ZnO)}×100 Alumina content [mass %] = {Al2O3 / (Gd2O3+Y2O3+ZrO2)} +Nb2O5+Al2O3+Fe2O3+Co3O4+ZnO)}×100 Niobium content [mass%] = {Nb2O5 / (Gd2O3+Y2O3+ZrO2)} +Nb2O5+Al2O3+Fe2O3+Co3O4+ZnO)}×100 Stabilizing element amount [mol%] = {(Gd₂O₃ + Y₂O₃) / (Gd₂O₃ + Y₂O₃ + ZrO₂) × 100 Amount of secondary stabilizing elements [mol%] = {(Gd₂O₃) / } (Gd₂O₃ + Y₂O₃ + ZrO₂) × 100 Gadolinium content [mol%] = {(Gd2O3) / (Gd₂O₃ + Y₂O₃ + ZrO₂) × 100 Yttrium content [mol%] = {(Y₂O₃) / (Gd₂O₃ + Y₂O₃ + ZrO₂) × 100 In this embodiment, the crystallite diameter (hereinafter referred to as "Dt" or simply "crystal diameter") of the sintered body, calculated from the XRD peaks belonging to the (111) plane of tetragonal zirconia, is 25 nm or more and 100 nm or less. By having Dt within the above range, the impact resistance of the zirconia sintered body is improved. Dt is preferably 25 nm or more, 30 nm or more, or 40 nm or more; furthermore, Dt is preferably 90 nm or less, 85 nm or less, or 80 nm or less. Examples of Dt in this embodiment include 25 nm or more and 90 nm or less, 30 nm or more and 85 nm or less, or 40 nm or more and 80 nm or less.

[0062] One reason why the sintered body of this embodiment possesses high impact resistance and high light-shielding properties by including niobium, manganese, and alumina and satisfying the aforementioned Dt is as follows: That is, by including manganese and alumina, it is possible to easily improve the Dt value for impact resistance. t Sintering was carried out under specific conditions, and the interaction between manganese and niobium promoted niobium segregation in the sintered body. It is believed that by promoting niobium segregation, a state conducive to zirconia phase transformation is formed. As a result, despite the presence of alumina, which reduces impact resistance, a zirconia sintered body with high impact resistance and high light-shielding properties is achieved. Furthermore, it is believed that when Dt is greater than 100 nm, the grain diameter of the sintered body increases, making it easier to form large pores as defects in the sintered body, thus reducing impact resistance.

[0063] As described below, the XRD peaks attributable to the (111) plane of tetragonal zirconia, in CuK α In XRD measurements using X-rays as the radiation source, as in 2 θ =30±0.5° with an XRD peak at the apex for determination. Therefore, D t It can also be considered as being based on CuK α In XRD measurements using X-rays as the source, the values ​​measured in 2... θ =30±0.5° is the diameter of the crystallite calculated from the XRD peak with the apex.

[0064] D t The XRD pattern of the zirconia sintered body can be obtained using the following formula.

[0065] Dt=K λ / Btcos θ t(1) In equation (1), Dt is the crystallite diameter (nm) calculated from the peak of the XRD of the (111) plane of tetragonal zirconia, and K is the Scherrer constant (K=1). λ Bt is the wavelength of the X-rays used in the XRD measurement (0.15418 nm), and Bt is the width (rad) of the peak attributable to the (111) plane of tetragonal zirconia. θ t is the Bragg angle (rad) of the peak attributable to the (111) plane of tetragonal zirconia.

[0066] It should be noted that the XRD peaks belonging to the (111) plane of tetragonal zirconia and the XRD peaks belonging to the (111) plane of cubic zirconia were measured repeatedly. In this specification, no distinction is made between the XRD peaks belonging to the (111) plane of tetragonal zirconia and the XRD peaks belonging to the (111) plane of cubic zirconia; the repeated peaks are treated as XRD peaks belonging to the (111) plane of tetragonal zirconia.

[0067] In this embodiment, the crystallite diameter of the zirconia sintered body, calculated from the XRD peaks belonging to the (111) facet of tetragonal zirconia, is preferably 25 nm or more and 90 nm or less, more preferably 30 nm or more and 85 nm or less, and more preferably 40 nm or more and 80 nm or less. By having the crystallite diameter calculated from the XRD peaks belonging to the (111) facet of tetragonal zirconia fall within the above-mentioned range, the impact resistance of the zirconia sintered body is improved.

[0068] In this embodiment, the X-ray diffraction pattern of the sintered body containing the XRD peaks belonging to the (111) plane of tetragonal zirconia can be determined by a conventional crystallographic X-ray diffraction apparatus (e.g., Ultima IV, manufactured by RIGAKU).

[0069] The following conditions can be cited as test conditions.

[0070] X-ray source: CuK α ray( λ =0.15418nm) Tube voltage: 45kV Tube current: 40mA Measurement mode: Continuous scanning Scanning speed: 4° / minute Step size: 0.02° Measurement range: 2 θ =26° and above and 33° and below Goniometer: radius 185mm As the test specimen, a sintered body in the shape of a circular plate with a diameter of 20 mm and a thickness of 1.0 mm was used, and the surface to be evaluated was mirror-polished (surface roughness Ra ≤ 0.02). μ The method involves irradiating the polished surface with X-rays to measure the surface (m).

[0071] In the above XRD pattern determination, the following 2 θ The XRD peak with a peak can be regarded as the XRD peak belonging to each crystal plane of zirconium oxide in this embodiment.

[0072] XRD peaks corresponding to the (111) plane of monoclinic zirconia: 2 θ =31±0.5° XRD peaks corresponding to the (11-1) plane of monoclinic zirconia: 2 θ =28±0.5° XRD peaks corresponding to the (111) plane of tetragonal zirconia: 2 θ =30±0.5° The patterns obtained by the above XRD pattern determination can be analyzed using the comprehensive powder X-ray analysis software "PDXL" (manufactured by RIGAKU Co., Ltd.). Through analysis, the width (rad) of each peak and the area intensity of each peak can be calculated.

[0073] The sintered body of this embodiment contains tetragonal zirconia (i.e., the zirconia crystal phase comprises a tetragonal crystal phase), and preferably is mainly composed of tetragonal zirconia. "Zirconium oxide is mainly composed of tetragonal zirconia" means that the zirconia crystal phase is mainly composed of tetragonal zirconia, and the zirconia crystal phase is 50% or more tetragonal. In this embodiment, the sintered body preferably has 50% or more or 60% or more tetragonal zirconia crystal phase, and more preferably 100% or less or 90% or less tetragonal zirconia crystal phase.

[0074] Furthermore, the zirconia crystal phase contained in the sintered body of this embodiment may include at least one of cubic and monoclinic crystal phases, in addition to the tetragonal crystal phase. That is, the zirconia contained in the sintered body of this embodiment may be composed of at least one of cubic zirconia and monoclinic zirconia, as well as tetragonal zirconia. In other words, the zirconia crystal phase contained in the sintered body of this embodiment may be composed of at least one of tetragonal, cubic, and monoclinic crystal phases. It should be noted that, for convenience, in this embodiment, the zirconia crystal phase is considered to be composed of one or more of tetragonal, cubic, and monoclinic crystal phases (i.e., the zirconia is composed of one or more of tetragonal, cubic, and monoclinic zirconia).

[0075] In this embodiment, the sintered body is preferably characterized by the peak of the XRD pattern at the center of the sintered body belonging to the (400) plane of tetragonal crystal (tetragonal zirconia) at the 2 θ The peak of the XRD peak at the (004) plane of tetragonal zirconia is 2 θ The difference (hereinafter also referred to as "2") θ The difference () is preferably 1.55° or higher. By making 2 θ An impact resistance of 1.55° or higher improves the impact resistance. θ The preferred deviation is 1.55° or higher, 1.57° or higher, or 1.60° or higher; examples include 3.0° or lower, 2.5° or lower, 2.2° or lower, or 2.0° or lower. The sintered body of this embodiment has 2... θ Differences can be categorized as 1.55° or higher and 3.0° or lower, 1.57° or higher and 2.5° or lower, or 1.60° or higher and 2.0° or lower.

[0076] In this embodiment, the X-ray diffraction pattern containing the XRD peaks belonging to the tetragonal (004) and (400) planes of the zirconia sintered body can be measured using the same method as the XRD measurement described above, except that the measurement conditions are set as follows.

[0077] X-ray source: CuK α ray( λ =0.15418nm) Tube voltage: 45kV Tube current: 40mA Measurement mode: Continuous scanning Scanning speed: 2° / minute Step size: 0.02° Measurement range: 2 θ =72° and above and 76° and below Goniometer: radius 185mm In the above XRD pattern measurement, the XRD peaks of each crystal plane of zirconia belonging to the central portion of the zirconia sintered body of this embodiment are defined as follows: θ The XRD peak with a apex is used for determination.

[0078] XRD peaks corresponding to the (004) plane of tetragonal zirconia: 2 θ =72.5±0.5° XRD peaks corresponding to the (400) plane of tetragonal zirconia: 2 θ =74.5±0.5° The patterns obtained by the above XRD pattern determination can be analyzed using the comprehensive powder X-ray analysis software "PDXL" (manufactured by RIGAKU Co., Ltd.). Specifically, background removal and CuK-based analysis are performed using the "PDXL" program. α 2 rays ( λ =1.5443 After removing the XRD peaks of ), the positions (°) of each peak corresponding to the (004) and (400) planes of tetragonal zirconia were detected.

[0079] The sintered body of this embodiment conforms to CIE 1976 (L). a b Lightness (L) in a color space Preferably, the lightness L of the sintered body in this embodiment is 35 or higher and 60 or lower. Preferably, the value is 35 or higher, 38 or higher, or 40 or higher, and more preferably 60 or lower, 55 or lower, 50 or lower, or 48 or lower. Therefore, even when a thin sintered body is formed, such as a sintered body with a sample thickness of 0.5 mm, it is easy to have shielding properties.

[0080] The CIE1976 (L) standard for the sintered body of this embodiment a b ) Chromaticity a in color space and b It is arbitrary; a can be given as an example. For values ​​above -10 and below 10, b It is above -10 and below 10.

[0081] Brightness L and chromaticity a and b It can be measured using a conventional spectrophotometer (such as CM-700d, manufactured by Konica Minolta) based on the JIS Z8722 method. As for lightness (L)... and chromaticity a and b The measurement conditions can be summarized as follows. The measurement only needs to be set to use a black plate as the background (so-called black background measurement).

[0082] Light source: D65 light source Angle of view: 10° Measurement method: SCI As the test specimen, a sintered body in the shape of a circular plate with a diameter of 20 mm and a thickness of 1.8 mm was used, and the surface to be evaluated was mirror-polished (surface roughness Ra ≤ 0.02). μ The hue can be evaluated using the area (m). Additionally, a diameter of 10mm can be used as an example of an effective area for hue evaluation.

[0083] The zirconia sintered body of this embodiment is impact-resistant, meaning it is not easily damaged by impact, especially when formed into a thin shape. Specifically, an example is shown where a 0.5mm thick sintered body of this embodiment is bonded to an ultra-hard plate. In a drop ball impact test where a steel ball (23mm in diameter, material: bearing steel SUJ2) weighing 25g, 50g, or 95g is dropped naturally from a height of 100cm, the sample is unlikely to crack or suffer other damage. Furthermore, the sintered body of this embodiment is preferably one that does not break when subjected to a drop ball test in which a SUJ2 steel ball with a diameter of 23 mm and a mass of 95 g is dropped naturally from a height of 100 cm three times with a sample thickness of 0.5 ± 0.05 mm. More preferably, it does not break when subjected to a drop ball test in which a SUJ2 steel ball with a diameter of 23 mm and a mass of 25 g is dropped three times, a SUJ2 steel ball with a diameter of 23 mm and a mass of 50 g is dropped three times, and a SUJ2 steel ball with a diameter of 23 mm and a mass of 95 g is dropped naturally from a height of 100 cm three times in sequence with a sample thickness of 0.5 ± 0.05 mm.

[0084] Regarding "damage" in the ball drop test, damage is considered to have occurred when the sintered body is divided or cracked due to the natural fall of the steel ball.

[0085] The zirconia sintered body of this embodiment has high light-shielding properties. For example, it is preferable to have the following light-shielding properties: when a stack consisting of the sintered body of this embodiment and a base member is formed, the base member does not show through when viewed from the sintered body of this embodiment along the stacking direction.

[0086] To achieve such light-blocking properties, when the thickness of the sintered body sample in this embodiment is 0.5 ± 0.05 mm, the total light transmittance (hereinafter also referred to as "total light transmittance") relative to the D65 light source is preferably 10% or less, 1% or less, or less than 0.1%. A lower total light transmittance means higher light-blocking properties. The total light transmittance is preferably 0%, but the total light transmittance of the sintered body in this embodiment can be 0% or more, greater than 0%, or greater than 0.01%, and examples include 0% or more and less than 10%, 0% or more and less than 1%, 0% or more and less than 0.1%, or greater than 0% and less than 0.1%.

[0087] In this embodiment, the total transmittance is a value measured using a conventional haze meter (e.g., NDH4000, manufactured by Nippon Denshoku Co., Ltd.) under the following conditions, based on the method of JIS K 7361-1.

[0088] Measurement light source: D65 light source Sample thickness: 0.5 ± 0.05 mm Sample diameter: 20mm Surface roughness: Ra≤0.02 μ m Total transmittance refers to the ratio of the combined intensity of diffuse and linearly transmitted light to the intensity of incident light, and they have the following relationship.

[0089] Incident light = reflected light + (diffuse transmitted light + linearly transmitted light) The shape of the sintered body in this embodiment can be selected from one or more shapes chosen from spherical, substantially spherical, elliptical, plate-like, cylindrical, cubic, cuboid, polyhedral, and substantially polyhedral. Furthermore, any shape suitable for achieving various intended purposes is acceptable.

[0090] The sintered body of this embodiment can be applied to the uses of conventional zirconia sintered bodies, particularly those selected from one or more of structural materials, optical materials, and dental materials. It can be used as a covering layer for accessories such as decorative items, watches, and housings, and as an outer component for portable electronic devices such as mobile phones, requiring highly machined components. Due to its impact resistance, it is particularly preferred for portable applications where drops and collisions are likely to occur.

[0091] (powder) The sintered body of this embodiment can be manufactured by molding and sintering raw material powder having the same composition. As a preferred sintering body powder of this embodiment, examples include zirconium oxide powder containing stabilizing elements, niobium, alumina, and iron, cobalt, and zinc as pigment components; the stabilizer content is 2.0 mol% or more and 5.5 mol% or less; the niobium content is 0.1 wt% or more and 3.0 wt% or less; the alumina content is greater than 0% and 30 wt% or less; and the BET specific surface area is 5.0 m² / s. 2 / g or more and 17.0m 2 / g or less.

[0092] The powder in this embodiment is a zirconium oxide powder containing stabilizing elements. Stabilizing elements are elements that have the function of stabilizing zirconium oxide. The stabilizing elements contained in the powder of this embodiment are preferably selected from one or more of calcium, magnesium, scandium, lanthanum, yttrium, neodymium, cerium, gadolinium, erbium, and ytterbium. More preferably, they are selected from one or more of yttrium, lanthanum, neodymium, gadolinium, erbium, and ytterbium; more preferably, they are selected from one or more of yttrium, lanthanum, neodymium, gadolinium, and erbium; or from one or more of yttrium, lanthanum, and neodymium; or from one or more of yttrium and neodymium; or from one or more of yttrium and lanthanum; or from one or more of yttrium and erbium. The powder in this embodiment may contain two or more of the stabilizing elements. In this case, the stabilizing elements may be selected from two or more of calcium, magnesium, scandium, lanthanum, yttrium, neodymium, cerium, gadolinium, erbium, and ytterbium, preferably a combination of yttrium and other stabilizing elements (secondary stabilizing elements). The secondary stabilizing elements contained in the sintered body of this embodiment are preferably selected from one or more of calcium, magnesium, scandium, lanthanum, neodymium, cerium, gadolinium, erbium, and ytterbium, more preferably from one or more of lanthanum, erbium, and neodymium, even more preferably from one or more of lanthanum, erbium, or neodymium, and even more preferably from erbium.

[0093] In this embodiment, the amount of stabilizing element in the powder is simply the amount that stabilizes the crystal phase of zirconia. Examples of stabilizing element amounts include greater than 0 mol%, 1.5 mol% or more, 2.0 mol% or more, 2.5 mol% or more, and less than 8.5 mol%, 5.5 mol% or less, 4.0 mol% or less, 3.4 mol% or less, or 3.2 mol%. Other examples of stabilizing element amounts in the powder of this embodiment include greater than 0 mol% and less than 8.5 mol%, 1.5 mol% or more and 5.5 mol% or less, 2.0 mol% or more and 4.0 mol% or less, 2.5 mol% or more and 4.0 mol% or less, or 2.5 mol% or more and 3.2 mol% or less. When the powder in this embodiment contains a secondary stabilizing element, the amount of the secondary stabilizing element in the powder can be greater than 0 mol%, 0.05 mol% or more, 0.10 mol% or more, 0.20 mol% or more, or 1.0 mol% or more, and less than 5.5 mol%, 4.0 mol% or less, 3.0 mol% or less, or 1.9 mol% or less. Preferably, the amount of the secondary stabilizing element is greater than 0 mol% and less than 5.5 mol%, 0.05 mol% or more and 4.0 mol% or less, 0.10 mol% or more and 3.0 mol% or less, 0.20 mol% or more and 1.9 mol% or less, or 1.0 mol% or more and 1.9 mol% or less.

[0094] As long as the total content of stabilizing elements meets the above-mentioned amount of stabilizing elements, the content of each stabilizing element is arbitrary, and the following contents can be exemplified.

[0095] Examples of yttrium content include greater than 0 mol%, greater than 1.0 mol%, greater than 1.5 mol%, greater than 2.0 mol%, or greater than 2.5 mol%, and less than 4.0 mol%, less than 3.5 mol%, less than 3.0 mol%, or less than 3.0 mol%, preferably greater than 0 mol% and less than 4.0 mol%, greater than 1.0 mol% and less than 3.5 mol%, greater than 1.5 mol% and less than 3.0 mol%, or greater than 2.5 mol% and less than 3.0 mol%.

[0096] When the secondary stabilizing element is erbium, the amount of erbium can be greater than 0 mol%, greater than 0.03 mol%, or greater than 1.0 mol%, and less than 4.0 mol%, less than 3.0 mol%, less than 2.0 mol%, or less than 1.9 mol%, preferably greater than 0 mol% and less than 4.0 mol%, greater than 0.01 mol% and less than 3.0 mol%, greater than 0.03 mol% and less than 2.0 mol%, or greater than 1.0 mol% and less than 1.9 mol%.

[0097] When neodymium is the secondary stabilizing element, the amount of neodymium can be greater than 0 mol%, greater than 0.01 mol%, greater than 0.03 mol%, greater than 0.09 mol%, greater than 0.2 mol%, or greater than 0.25 mol%, and less than 4.0 mol%, less than 3.0 mol%, less than 2.0 mol%, less than 0.5 mol%, or less than 0.4 mol%. More preferably, it is greater than 0 mol% and less than 4.0 mol%, greater than 0.01 mol% and less than 2.0 mol%, greater than 0.03 mol% and less than 0.5 mol%, or greater than 0.09 mol% and less than 0.4 mol%.

[0098] When the secondary stabilizing element is lanthanum, the amount of lanthanum can be greater than 0 mol%, greater than 0.01 mol%, greater than 0.03 mol%, or greater than 0.1 mol%, and less than 4.0 mol%, less than 3.0 mol%, less than 2.0 mol%, or less than 0.5 mol%. More preferably, it is greater than 0 mol% and less than 4.0 mol%, greater than 0.01 mol% and less than 0.5 mol%, or greater than 0.1 mol% and less than 0.5 mol%.

[0099] The powder in this embodiment contains niobium. By including niobium, it is expected to improve the impact resistance and light-shielding properties of the resulting sintered body. The niobium content can be greater than 0% by mass, greater than 0.1% by mass, 0.5% by mass or more, or 1.0% by mass or more, and less than 3.0% by mass, less than 2.5% by mass, or less than 2.0% by mass. Furthermore, examples of niobium content include greater than 0% by mass and less than 3.0% by mass, preferably more than 1.0% by mass and less than 3.0% by mass, or more than 1.0% by mass and less than 2.5% by mass.

[0100] The powder in this embodiment contains alumina. Examples of alumina content include greater than 0% by mass and less than 30% by mass. By including alumina (i.e., alumina content greater than 0% by mass), the sintered body of this embodiment can be obtained by sintering at a lower temperature. Furthermore, by having an alumina content of less than 30% by mass, the mechanical properties of the sintered body, such as static strength, are easily improved. Examples of alumina content include greater than 0% by mass and less than 30% by mass. By including alumina, a dense sintered body can be easily obtained even at lower temperatures. To improve shielding properties, the alumina content is preferably 0% by mass or more, greater than 0% by mass, 0.005% by mass or more, 0.05% by mass or more, 0.1% by mass or more, 0.25% by mass or more, 0.5% by mass or more, or 1% by mass or more. On the other hand, to improve mechanical properties, such as static strength, the alumina content can be less than 30% by mass, less than 20% by mass, less than 10% by mass, less than 5% by mass, or less than 2% by mass. Examples of alumina content in the sintered body of this embodiment include greater than 0% by mass and less than 20% by mass, or greater than 0.1% by mass and less than 10% by mass.

[0101] The powder of this embodiment contains iron, cobalt, and zinc as pigment components. The pigment components in the powder of this embodiment refer to components that have the function of coloring the sintered body. Therefore, the sintered body can exhibit any hue different from the original hue of zirconium oxide. In particular, by including iron, cobalt, and zinc in the pigment components, in addition to improving the opacity of the sintered body, a dense sintered body is easily obtained even when sintering at a lower temperature. It should be noted that even if the aforementioned stabilizing elements have the function of coloring the sintered body, their content is not included in the pigment components, but is calculated as elements included as stabilizing elements. For example, neodymium, cerium, and erbium are elements that have the function of coloring the sintered body, but their content is not included in the pigment components, but is calculated as elements included as stabilizing elements.

[0102] The iron content can be 0.10% by mass or more, preferably 0.20% by mass or more, 0.30% by mass or more, or 0.50% by mass or more, and can be 5.0% by mass or less, preferably 4.5% by mass or less, 3.0% by mass or less, or 2.0% by mass or less. Further, the iron content can be 0.10% by mass or more and 5.0% by mass or less, more preferably 0.20% by mass or more and 4.5% by mass or less, 0.30% by mass or more and 3.0% by mass or less, or 0.50% by mass or more and 2.0% by mass or less.

[0103] The amount of cobalt can be 0.10% by mass or more, preferably 0.20% by mass or more or 0.25% by mass or more, and can be 3.0% by mass or less, preferably 2.0% by mass or less, 1.5% by mass or less or 1.0% by mass or less. Furthermore, the amount of cobalt can be 0.10% by mass or more and 3.0% by mass or less, and more than 0.20% by mass or less and 2.0% by mass or less, 0.25% by mass or more and 1.5% by mass or less, or 0.25% by mass or more and 1.0% by mass or less.

[0104] The zinc content can be 0.05% by mass or more, preferably 0.10% by mass or more, and can be 1.0% by mass or less, preferably 0.70% by mass or less or 0.50% by mass or less. Further, the zinc content can be 0.05% by mass and 1.0% by mass or less, preferably 0.10% by mass and 0.70% by mass or less, and more preferably greater than 0.10% by mass and 0.50% by mass or less.

[0105] The powder of this embodiment may further contain pigment components other than iron, cobalt, and zinc. As pigment components other than iron, cobalt, and zinc, compounds containing metallic elements are preferred, more preferably transition metal elements and compounds containing them. Specifically, pigment components other than iron, cobalt, and zinc are more preferably one or more elements selected from vanadium, manganese, nickel, and copper, and compounds containing one or more of them, and more preferably oxides containing one or more of them. The sintered body of this embodiment may contain chromium as a pigment component, but from an environmental perspective, it is preferable not to contain chromium.

[0106] The content of other pigment components in the powder of this embodiment is arbitrary, but preferably greater than 0% by mass, 0.001% by mass or more, 0.005% by mass or more, 0.01% by mass or more, 0.05% by mass or more, or 0.1% by mass or more, and more preferably 5.0% by mass or less, 3.5% by mass or less, or 3.0% by mass or less. Furthermore, the amount of other pigment components is preferably greater than 0% by mass and less than 5.0% by mass, greater than 0.001% by mass and less than 3.5% by mass, or greater than 0.005% by mass and less than 3.0% by mass.

[0107] In addition to niobium, alumina, and pigment components, the powder of this embodiment may also contain one or more additives selected from silicon dioxide, titanium dioxide, and gallium oxide. By including such additives, a sintered body with the desired mechanical properties can be obtained.

[0108] The powder in this embodiment may contain unavoidable impurities such as hafnium oxide. In this embodiment, the content of each component in the sintered body can be calculated simply by treating hafnium oxide as zirconium oxide and calculating their values.

[0109] In this embodiment, the niobium, alumina, pigment components, other pigment components, and additives in the powder can be contained in the powder in any form. They can be contained in the form of compounds, and further in the form of composite oxides and at least one of oxides. Alternatively, they can be contained in part or all of them by solid dissolution in zirconium oxide.

[0110] In this embodiment, part or all of the pigment component in the powder can form a spinel-type metal oxide. By forming a spinel-type metal oxide in part or all of the pigment component, in addition to improved opacity, the hue is more easily stabilized. The spinel-type metal oxide is preferably represented by AB₂O₄, where A and B are each selected from one or more of Mg, Ca, Sr, Y, La, Gd, V, Mn, Fe, Co, Ni, Cu, Zn, and Al; more preferably, it is represented by AB₂O₄, where A and B are each selected from one or more of Mg, Ca, Sr, Y, Gd, Fe, Co, Ni, Zn, and Al. When represented by AB₂O₄, the spinel-type metal oxide contained in the powder of this embodiment can contain multiple elements at sites A and B. In the case where multiple elements are contained at sites A and B, the composition ratio of each element at site A and site B is arbitrary. Specific spinel-type metal oxides include one or more selected from CoAl2O4, ZnFe2O4, MgFe2O4, CoFe2O4, NiFe2O4, Co(Fe,Al)2O4, and (Co,Zn)(Fe,Al)2O4.

[0111] The powder in this embodiment has a BET specific surface area of ​​5.0 m². 2 / g or more and 17.0m 2 / g or less. The BET specific surface area of ​​the powder in this embodiment is preferably 6.0 m². 2 / g or more and 16m 2 / g or less, 7.0m 2 / g or more and 14.0m 2 / g or less, or 8.0m 2 / g or more and 12.0m 2 / g or less. By keeping the BET specific surface area within this range, sintered bodies with crystallite diameters of 25nm or more and 100nm or less can be easily obtained.

[0112] In this embodiment, the BET specific surface area of ​​the powder is determined by the BET1-point method, which is based on JIS R 1626-1996. A conventional automated flow-type specific surface area measuring device (e.g., Flowsorb III 2305, manufactured by Shimadzu Corporation) is used, and nitrogen (N2) is used as the adsorbent. Prior to measurement, the powder is pretreated by being treated at 250°C under a vacuum atmosphere for 2 hours.

[0113] In this embodiment, the powder preferably has a cumulative particle size distribution in which 10% of the particle size D10 is 0.15. μ m or more and 0.50 μ The particle size is below 1 μm, and 90% of the cumulative particle size distribution of the powder has a D90 of 0.50. μ m or more and 1.30 μ Below 10 nm. D10 and D90 are both indicators representing the distribution of secondary particle size in powder. It is believed that by using D10 and D90 within this range, the stability of tetragonal zirconium oxide in the sintered body is controlled, resulting in the easy acquisition of sintered bodies with crystallite diameters Dt of 25 nm or more and 100 nm or less.

[0114] The powder in this embodiment can be exemplified by having a D10 of 0.15. μ m or more and 0.50 μ Below m, 0.20 μ m or more and 0.48 μ Less than m, or 0.30 μ m or more and 0.46 μ Below 10 μm. The preferred particle size D10 is 0.15 μm. μ m or more, 0.20 μ m or more or 0.30 μ m or more, and 0.50 μ Below m, 0.48 μ Below m or 0.46 μ Below m. If D10 decreases, the tetragonal crystals of zirconium oxide in the sintered body become unstable, and the crystallite diameter tends to decrease.

[0115] Furthermore, the powder of this embodiment can be exemplified as having a D90 of 0.50. μ m or more and 1.5 μ Below m, 0.50 μ m or more and 1.3 μ Below m, 0.525 μ m or more and 1.25 μBelow m, 0.55 μ m or more and 1.2 μ Less than m, or 0.55 μ m or more and less than 1.0 μ m. A more preferred particle size D90 for 90% of particles is 0.50. μ m or more, greater than 0.50 μ m, 0.525 μ m or more, 0.55 μ m or more, preferably 1.5 m. μ Below m, 1.3 μ Below m, 1.2 μ m or less than 1.0 μ m. When D90 increases, the tetragonal crystals of zirconium oxide in the sintered body become unstable, and the crystallite diameter tends to decrease.

[0116] In this embodiment, D10 and D90 can be determined from the cumulative particle size distribution curve obtained by measurement using the HRA mode of a conventional Microtrac particle size analyzer (e.g., device name: MT3000II, manufactured by Microtrac BEL). To disperse the agglomeration of powder particles, a slurry made by suspending the powder sample in pure water can be pretreated using an ultrasonic homogenizer or similar device before measurement. Furthermore, a dispersant (e.g., sodium hexametaphosphate) can be used when preparing the slurry.

[0117] The powder of this embodiment may contain a molding aid. By including the molding aid, the molded article obtained by molding according to this embodiment has high strength. The molding aid is any molding aid that can be applied to ceramic powder used in dry pressure molding, and thereby improves the properties of the molded article obtained by dry pressure molding of ceramic powder. Examples of such molding aids include one or more selected from polyethylene glycol resin, polyvinyl alcohol resin, polyvinylpyrrolidone resin, and acrylic resin. Specific molding aids include, for example, one or more selected from AS-1100, AS-1800, and AS-2000 (all product names, manufactured by Toa Synthetic Co., Ltd.).

[0118] The powder in this embodiment can be a granulated powder (hereinafter also referred to as "powder particles"). Examples of powder particles include those with an average particle size of 30 mm. μ m or more and 80 μ Below m, further to 50 λ m or more and 60 θ Below m and with a bulk density of 1.00 g / cm³ 3 Above and 1.50 g / cm 3 The following is further: 1.10 g / cm³ 3Above and 1.45g / cm 3 the following.

[0119] (Powder manufacturing method) The manufacturing method is arbitrary as long as the powder of this embodiment can be obtained. As an example of the manufacturing method of the powder of this embodiment, a manufacturing method including the following steps can be given: heat-treating a composition containing a zirconia sol containing crystalline zirconia with monoclinic zirconia as the main phase and a stabilizing element source at a temperature of 600°C or higher and 1250°C or lower to produce a pre-calcined powder (hereinafter also referred to as the "powder pre-calcination step"); and pulverizing the pre-calcined powder, niobium source, alumina source, iron source, cobalt source and zinc source (hereinafter also referred to as the "pulverization step").

[0120] A composition comprising a zirconia sol containing crystalline zirconia with monoclinic zirconia as the main phase and a stabilizing element source (hereinafter also referred to as the "raw material composition") is supplied to the powder pre-calcination process.

[0121] The method for manufacturing zirconia sol containing crystalline zirconia with monoclinic zirconia as the main phase is arbitrary, and at least one of hydrothermal synthesis and hydrolysis methods can be exemplified. In the hydrothermal synthesis method, a coprecipitate obtained by mixing zirconium salt and alkali in the presence of a solvent is heat-treated at 100°C to 200°C to obtain zirconia sol. Alternatively, in the hydrolysis method, zirconia sol can be obtained by heating zirconium salt in the presence of a solvent, which hydrolyzes the zirconium salt. Thus, zirconia sol can be exemplified by zirconia sol obtained by at least one of hydrothermal synthesis and hydrolysis methods, preferably zirconia sol obtained by hydrolysis. Zirconium salts can be used as precursors in the method for manufacturing zirconia sol. Zirconium salts can be selected from one or more of zirconium oxychloride, zirconium nitrate, zirconium chloride, and zirconium sulfate, preferably at least one of zirconium nitrate and zirconium oxychloride, and more preferably zirconium oxychloride.

[0122] A pre-calcined powder, serving as a precursor for zirconium oxide powder, is obtained through a powder pre-calcination process. The zirconium oxide raw material composition may contain at least one of a niobium source and an alumina source.

[0123] The stabilizing element source can be at least one of an oxide of the stabilizing element and a compound containing the stabilizing element as a precursor. Examples include one or more selected from oxides, hydroxides, oxychlorides, chlorides, acetates, nitrates, and sulfates that are precursors of the oxide of the stabilizing element, preferably at least one of chlorides and nitrates. (Hereinafter, when the stabilizing element is yttrium or the like, the stabilizing element source will also be referred to as "yttrium source," etc.). The content of the stabilizing element source in the raw material composition need only be equal to the amount of stabilizing element in the target sintered body.

[0124] The yttrium source can be any one of yttrium oxide and yttrium compounds that are precursors thereto, and can be selected from yttrium chloride, yttrium oxide and yttrium carbonate, with yttrium chloride being preferred.

[0125] The erbium source can be any one of erbium oxide and erbium compounds that are its precursors, and can be selected from erbium chloride, erbium oxide and erbium carbonate, with erbium oxide being preferred.

[0126] The neodymium source can be any one of neodymium oxide and a neodymium compound as a precursor, and can be selected from one or more of neodymium chloride, neodymium oxide, neodymium hydroxide and neodymium carbonate, with neodymium oxide being preferred.

[0127] The niobium source can be any one of niobium oxide and a compound that is a precursor thereof. Examples include one or more of germanium hydroxides, chlorides, alkoxides, nitrates, oxalates, and sulfates that are precursors of niobium oxide. Preferably, it is selected from one or more of niobium oxide, germanium hydroxides, and alkoxides that are precursors of niobium oxide. The content of the niobium source in the raw material composition only needs to be equal to the niobium content of the target sintered body.

[0128] The alumina source is at least one of alumina and an aluminum-containing compound as a precursor thereto, preferably selected from aluminum chloride, aluminum sulfate, aluminum nitrate, aluminum hydroxide, alumina sol, and alumina. The content of the alumina source in the raw material composition need only be equal to the alumina content of the target sintered body.

[0129] As a zirconium oxide source, zirconium oxide can be used instead of a zirconium oxide sol containing zirconium oxide as a monoclinic crystal, or zirconium oxide containing a stabilizing element can be used. Examples of zirconium oxide containing a stabilizing element include yttrium-stabilized zirconium oxide. When using zirconium oxide containing a stabilizing element, the method for containing the stabilizing element in the zirconium oxide is arbitrary. For example, the following method can be used: mixing a hydrated zirconium oxide sol with a stabilizing element source of equal content to the target stabilizing element, drying, pre-calcining, and washing with water.

[0130] Furthermore, niobium-containing stabilized zirconia, which contains niobium and stabilizing elements, can also be used as zirconia. When using niobium-containing stabilized zirconia, the method for incorporating niobium into the zirconia is arbitrary. Examples include: mixing hydrated zirconia sol, a stabilizing element source, and a niobium source, followed by drying, pre-firing, and washing; or mixing hydrated zirconia sol and a stabilizing element source, followed by drying, pre-firing, and then mixing with a niobium source for pre-firing.

[0131] The mixing method is arbitrary, preferably at least one of dry mixing and wet mixing, more preferably wet mixing, and even more preferably wet mixing using ball milling.

[0132] In the powder pre-calcination process, heat treatment is performed at 500°C or higher and 1250°C or lower, and further at 600°C or higher and 1250°C or lower. By heat treatment at 500°C or higher, powder that is easily densified under atmospheric pressure sintering can be obtained. On the other hand, by heat treatment at 1250°C or lower, powder that is easily dispersed by pulverization is more readily obtained. The heat treatment time can be appropriately varied depending on the heat treatment temperature, the amount of zirconia raw material composition supplied for treatment, and the characteristics of the heat treatment furnace; for example, 30 minutes or more and 6 hours or less can be used. The rate of heating to the heat treatment temperature has almost no effect on the obtained pre-calcined powder; for example, a rate of heating of 50°C / hour or higher and 1000°C / hour or less can be used.

[0133] The atmosphere for heat treatment is arbitrary and can be selected from any of the following: oxidizing atmosphere, reducing atmosphere, inert gas atmosphere and vacuum atmosphere, preferably an oxidizing atmosphere, and more preferably an atmospheric atmosphere.

[0134] The raw material composition supplied for the powder pre-calcination process only needs to contain the above-mentioned zirconium oxide sol and stabilizing element source, and all or part of the stabilizing element source can be dissolved in the zirconium oxide sol. For example, by mixing and hydrolyzing the zirconium salt with the stabilizing element source, or by mixing the zirconium salt, the stabilizing element source and the alkali to form a coprecipitate, at least a portion of the stabilizing element source can be readily dissolved in zirconium oxide.

[0135] In the pulverization process, the pre-sintered powder is pulverized. Zirconia with low stabilizing element content is prone to cracking and defects during sintering. In contrast, pulverizing the pre-sintered powder can easily improve the yield during sintering.

[0136] The pulverization method is arbitrary, as long as it is at least one of wet pulverization and dry pulverization, with wet pulverization being preferred. Specifically, wet pulverization can be exemplified by one or more selected from ball mills and continuous media stirred mills, with ball mills being preferred.

[0137] The powder supplied for the pulverizing process can be pre-calcined powder or a mixed powder containing pre-calcined powder, niobium source, alumina source, iron source, cobalt source, and zinc source. Alternatively, the alumina source, iron source, cobalt source, and zinc source can be pre-reacted with the raw materials to form a composite oxide.

[0138] The iron source is at least one of iron oxide and an iron-containing compound as a precursor thereto, and may be selected from one or more of ferric chloride, iron oxide and iron hydroxide, with iron oxide being preferred.

[0139] The cobalt source is at least one of iron oxide and a cobalt-containing compound as a precursor thereto, and may be selected from one or more of cobalt chloride, cobalt oxide and cobalt hydroxide, preferably cobalt oxide.

[0140] The zinc source is at least one of zinc oxide and zinc-containing compounds that are precursors thereto, and may be selected from zinc chloride, zinc oxide and zinc hydroxide, with zinc oxide being preferred.

[0141] In addition to the powders mentioned above, the powders supplied for the pulverizing process can also be mixed powders containing pigment components.

[0142] Examples of pulverization conditions using ball milling include: mixing pre-calcined powder with a solvent (e.g., at least one of water and alcohol, or water) to prepare a slurry with a powder-to-slurry mass ratio of 30% to 60% by mass for the pulverization process; and pulverizing using zirconia balls with a diameter of 0.5 mm to 15 mm as the pulverizing medium. The pulverization time can be adjusted appropriately according to the amount of pre-calcined powder to be processed, for example, 5 hours to 100 hours.

[0143] Zirconia powder is obtained by wet pulverization followed by drying using any method. Examples of drying conditions include atmospheric atmosphere and temperatures above 110°C and below 200°C.

[0144] To improve the workability of the powder, the powder manufacturing method may include a step of granulating the powder (hereinafter also referred to as the "granulation step"). Granulation can be carried out by any method, such as spray granulation of a slurry formed by mixing powder and solvent. The solvent is at least one of water and alcohol, preferably water.

[0145] (Manufacturing method of sintered body) The manufacturing method of the sintered body in this embodiment is arbitrary, and a manufacturing method having a step of sintering the powder of this embodiment can be exemplified. The powder can be supplied in any form in the above-described step (hereinafter also referred to as the "sintering step"), and considering the thermal shrinkage caused by sintering, a shape that can obtain the shape of the target sintered body is preferred. For example, it can be provided for sintering after forming a molded body (pressed powder), or the molded body can be pre-fired to form a pre-fired body for sintering.

[0146] In the method for manufacturing the sintered body according to this embodiment, a step of forming powder into a molded body (pressed powder body) may be included (hereinafter also referred to as the "forming step").

[0147] In addition to the powder of this embodiment, the raw materials used for molding may also be a powder slurry formed by slurrying the powder of this embodiment, or a powder composite containing the powder of this embodiment and a binder. The binder can be any organic binder used in ceramic molding, and examples include one or more selected from acrylic resins, polyolefin resins, waxes, and plasticizers. Specific examples of binders include one or more selected from AS-1100, AS-1800, and AS-2000 (all product names, manufactured by Toa Gosei Co., Ltd.).

[0148] As for the content of the binder, examples can be given of a binder content in the volume of the molded article that is 25% by volume or more and 65% by volume or less at room temperature. Furthermore, examples can be given of a binder content greater than 0% by mass and 10% by mass in 100% by mass of the molded article. By including the binder, the shape stability of the obtained molded article can be improved.

[0149] Considering the shrinkage caused by heat treatment such as sintering, the shape of the molded body can be any shape corresponding to the target, such as one or more selected from spherical, approximately spherical, elliptical, disc-shaped, cylindrical, cubic, cuboid, polyhedral, and approximately polyhedral shapes. Furthermore, any shape corresponding to the target is acceptable.

[0150] The molding method can use a known molding method that can form the powder of this embodiment into a pressed powder, preferably one or more selected from uniaxial compression molding, isostatic pressing, injection molding, extrusion molding, rotary granulation, slip casting and casting, more preferably at least one of uniaxial compression molding and isostatic pressing, further preferably at least one of cold isostatic pressing and uniaxial compression molding (powder compression molding), and even more preferably cold isostatic pressing is performed after uniaxial compression molding.

[0151] Before sintering, there may be a process of pre-firing the molded body to obtain a pre-fired body (hereinafter also referred to as the "pre-firing process"). By pre-firing the molded body, a pre-fired body from which the binder has been removed from the molded body can be obtained. "Pre-fired body" refers to a composition composed of fused particles, which is a composition that retains at least a portion of the shape of the powder particles and has a structure in which the particles embrace each other.

[0152] The conditions for the pre-firing process can be arbitrary as long as the sintered body of this embodiment can be obtained through the subsequent sintering process. Examples include heat treatment based on a temperature at which densification of the molded body is not performed. Specifically, examples include heat treatment performed in an atmospheric atmosphere at a temperature of 400°C or higher and less than 1100°C.

[0153] The sintering process sintersects the molded body or pre-sintered body to obtain a sintered body. The sintering method can be any method of sintering, and examples include one or more methods selected from atmospheric pressure sintering, pressure sintering, and vacuum sintering, as well as other known sintering methods. As a preferred sintering method, atmospheric pressure sintering can be performed, and sintering is carried out solely by atmospheric pressure sintering. Therefore, the sintered body of this embodiment can be obtained as a so-called atmospheric pressure sintered body. Atmospheric pressure sintering refers to a method in which no external force is applied to the material being sintered (e.g., powder, molded body, or pre-sintered body) during sintering, and sintering is carried out solely by heating.

[0154] Regarding the conditions for atmospheric pressure sintering, the holding temperature (sintering temperature) for the sintering process is 1050°C or higher and 1600°C or lower, preferably 1100°C or higher and 1550°C or lower, 1100°C or higher and 1500°C or lower, 1150°C or higher and 1500°C or lower, 1200°C or higher and 1500°C or lower, or 1250°C or higher and 1450°C or lower. When the sintering temperature is within this range, it is easy to obtain sintered bodies with a crystallite diameter of 25 nm or higher and 100 nm or lower. The sintering temperature is preferably higher than the pre-sintering temperature. Furthermore, as the sintering atmosphere, at least one of an atmospheric atmosphere and an oxygen atmosphere can be cited, with an atmospheric atmosphere being preferred. The heating rate is 20°C / hour or more or 75°C / hour or more. Examples of heating rates include 5000°C / hour or less, 500°C / hour or less, or 200°C / hour or less. Examples of heating rates include 20°C / hour or more and 500°C / hour or 75°C / hour or more and 200°C / hour or less. The sintering time can be appropriately set according to the amount and size of the material to be sintered and the characteristics of the sintering furnace. For example, the holding time at the aforementioned sintering temperature can be 0.3 hours or more, 0.5 hours or more, or 1 hour or more. Examples of holding times include 20 hours or less, 10 hours or less, or 5 hours or less. Examples of holding times include 0.5 hours or more and 20 hours or less, or 0.5 hours or more and 15 hours or less.

[0155] It should be noted that the metal elements and their contents do not change substantially in the molding process, the pre-firing process, and the sintering process. Therefore, in this embodiment, the composition of the metal components (inorganic substances) in the powder and the molded body, pre-firing body, and sintered body obtained therefrom can be regarded as the same.

[0156] Example The present invention will now be specifically described through examples. However, the present invention is not limited to these examples.

[0157] (BET specific surface area) The BET specific surface area of ​​the powder was determined by the BET 1-point method, which is based on JIS R 1626-1996 and uses a conventional automated flow-type specific surface area measuring device (device name: FlowSorb III2305, manufactured by Shimadzu Corporation) and nitrogen (N2) as the adsorbent. Prior to the measurement, the powder was pretreated by drying it under vacuum at 250°C for 2 hours.

[0158] (D10 and D90) The cumulative particle size distribution curve was obtained by measuring using the HRA mode of a standard Microtrac particle size analyzer (device name: MT3000II, manufactured by MicrotracBEL). D10 and D90 were then determined based on the obtained cumulative particle size distribution curve. Prior to measurement, the powder was suspended in pure water with added dispersant (sodium hexametaphosphate) and dispersed using an ultrasonic homogenizer for 10 minutes as a pretreatment.

[0159] (Crystal diameter: Dt) The XRD pattern of the sintered body sample was obtained using a conventional X-ray diffraction apparatus (Ultima IV, manufactured by RIGAKU) under the following conditions.

[0160] X-ray source: CuK α ray( μ =0.15418nm) Tube voltage: 45kV Tube current: 40mA Measurement mode: Continuous scanning Scanning speed: 4° / minute Step size: 0.02° Measurement range: 2 μ =26° and above and 33° and below Goniometer: radius 185mm Using the XRD pattern of the obtained sintered body, the crystallite diameter D, calculated from the peaks of the XRD belonging to the (111) plane of tetragonal zirconia, is obtained according to Equation (1). t (nm). It should be noted that the X-ray irradiation surface for measuring the sample is as follows: after removing the burnt skin surface (i.e., the burnt skin surface) by grinding 0.3 mm along the depth direction on the surface of the freshly sintered body, the sample is then subjected to grinding using sandpaper, with an average particle size of 3... θ Grinding of diamond slurry at m, and utilizing 0.03 θ The polished surface is obtained by mirror polishing the colloidal silica in the order of grinding m.

[0161] (2) λ Difference) In addition, 2 was obtained from the XRD pattern obtained by the same method except that the XRD measurement was performed under the following conditions. θ Difference.

[0162] X-ray source: CuK α ray( λ =1.5418nm) Tube voltage: 45kV Tube current: 40mA Measurement mode: Continuous scanning Scanning speed: 2° / minute Step size: 0.02° Measurement range: 2 θ =72° and above and 76° and below Goniometer: radius 185mm For the patterns obtained by the above XRD measurements, background removal and CuK-based analysis were performed using the comprehensive powder X-ray analysis software "PDXL". α 2 lines ( θ After removing the XRD peak of (1.5443), the peak values ​​of the XRD peaks corresponding to the (004) and (400) planes of tetragonal zirconia were determined. λ and 2 θ Difference.

[0163] (Confirmation of the formation of spinel-type metal oxides) The XRD pattern of the sintered body sample was obtained using a conventional X-ray diffraction apparatus (Ultima IV, manufactured by RIGAKU) under the following conditions.

[0164] X-ray source: CuK α ray( θ =0.15418nm) Tube voltage: 45kV Tube current: 40mA Measurement mode: Continuous scanning Scanning speed: 4° / minute Step size: 0.02° Measurement range: 2 μ =32° and above and 40° and below Goniometer: radius 185mm The pattern obtained from the above XRD measurement was analyzed using the comprehensive powder X-ray analysis software "PDXL" to confirm whether there were 2 corresponding to the (111) facet of the spinel-type metal oxide. μ The peak is 36.3° ± 0.5°.

[0165] (tone) The hue of the sintered body samples was determined using a method based on JIS Z 8722. Measurements were performed using a standard spectrophotometer (CM-700d, manufactured by Konica Minolta) against a black background with a black plate on the back. The measurement conditions are as follows.

[0166] Light source: D65 light source Angle of view: 10° Measurement method: SCI The sintered body specimens were circular plates with a diameter of 20 mm and a thickness of 1.8 mm. One surface of the sintered body specimen was mirror-polished (Ra ≤ 0.02). μ The surface is used as the evaluation surface to evaluate the hue (m). The effective area for hue evaluation is set to a diameter of 10 mm.

[0167] (Total transmittance) The total transmittance of the sintered body samples was determined using a method based on JIS K 7361-1. Measurements were performed using a standard haze meter (NDH4000, manufactured by Nippon Denshoku Co., Ltd.) equipped with a D65 light source. The sintered body samples were set with a thickness of 0.5 ± 0.05 mm and a diameter of 20 mm, with a surface roughness Ra ≤ 0.02. μ The mirror polishing process is performed on both sides using the m method.

[0168] (Steel ball drop test) The sintered body sample was ground into a disc shape with a diameter of 36 mm and a thickness of 0.5 mm. For both surfaces of the disc-shaped sintered body sample (the 36 mm diameter surface; the main surface), automatic grinding was performed using sandpaper, with an average particle size of 3... Figures 1-3 Automatic grinding of diamond slurry with a diameter of m, and the use of 0.03 μ The colloidal silica of m was automatically polished to a mirror finish to obtain the test sample. A schematic diagram of the falling ball test is shown below. μ To prevent the test piece from breaking, after applying repair tape 2 (thickness: 0.05 mm) to one main surface of the test specimen 1, the test specimen 1 is positioned on a 10 mm thick ultra-hard plate 3 (MAST-FB10, Takeuchi Profiles Research Institute, HRA: 93.5) with the side of the test specimen 1 with repair tape 2 in contact with the ultra-hard plate 3. Repair tape 2 is then applied to the ends of the test specimen 1 and the ultra-hard plate 3, thereby fixing the test specimen 1 to the ultra-hard plate 3. The ultra-hard plate 3 with the test specimen 1 attached is positioned so that the steel ball 4 (material: bearing steel SUJ2) falls near the center of the test specimen 1 after it is fixed to the ultra-hard plate 3. A transparent vinyl chloride tube 5 (Φ30 mm) is fixed using a clamp 6. A level is used to fix the transparent vinyl chloride tube 5 perpendicular to the ultra-hard plate 3.

[0169] Then, the steel ball 4 is allowed to fall freely from a height of 100 cm through the inside of the transparent vinyl chloride tube 5. The initial configuration is to place the steel ball 4 on the iron rod 7, with the iron rod 7 inserted horizontally into the hole 8 located 100 cm from the upper surface of the test sample 1 in the transparent vinyl chloride tube 5. The steel ball 4 is then dropped. The iron rod 7 is then removed, allowing the steel ball to fall freely. The steel ball 4 is allowed to fall freely without contacting the inner wall of the transparent vinyl chloride tube 5 during its descent. To prevent the steel ball 4 from bouncing back and falling again after free fall, thus preventing contact with the test sample 1, a hole 10 is made in the transparent vinyl chloride tube 5 at a height of approximately 5 cm from the upper surface of the test sample 1, into which the iron rod 9 (Φ5mm, 4cm) is inserted. When the rebounding steel ball 4 reaches a height of 5 cm or more, the iron rod 9 is inserted into the hole 10 to stop the steel ball 4 from falling freely again.

[0170] If no damage is confirmed by the drop ball test, the drop ball test is repeated. The drop ball test is repeated in the following order: three times with a 25g steel ball, three times with a 50g steel ball, and three times with a 95g steel ball.

[0171] Example 1 3 mol% yttrium-stabilized zirconium oxide (TZ-3YS, manufactured by Tosoh Corporation), niobium oxide powder (manufactured by Fujifilm and Koko Pure Chemical Industries Co., Ltd.), aluminum oxide (AKP-30, manufactured by Sumitomo Chemical), and spinel-type oxide pigments containing zinc, cobalt, and iron were mixed in accordance with the composition shown in Table 1 to obtain a mixed powder. Pure water was added to the obtained mixed powder to prepare a mixed slurry. This mixed slurry was pulverized using a ball mill with 10 mm diameter zirconium oxide pellets as the pulverizing medium, with D10 and D90 values ​​shown in Table 1, to obtain a pulverized slurry. The obtained pulverized slurry was dried at 110°C under atmospheric conditions, and then sieved to remove aggregates with a diameter greater than 180 mm. θ The powder of this embodiment is obtained by producing coarse particles of m.

[0172] Examples 2 and 3 Except for using the mixed powder with the composition shown in Table 1, the powders of Examples 2 and 3 were obtained using the same method as in Example 1.

[0173] Examples 4 to 7 The powders of Examples 4 to 7 were obtained by using the mixed powders with the composition shown in Table 1 and by ball milling with zirconia balls of 2 mm in diameter as the grinding medium, in the manner described in Table 1.

[0174] Example 8 A zirconium oxychloride aqueous solution was hydrolyzed to obtain hydrated zirconium oxide sol. Yttrium chloride was added to the hydrated zirconium at a concentration of 2.5 mol% and mixed. The mixture was then pre-calcined at 1150 °C for 2 hours under atmospheric conditions to obtain yttrium-stabilized zirconium oxide pre-calcined powder.

[0175] The obtained yttrium-stabilized zirconia pre-calcined powder was mixed with niobium oxide powder (manufactured by Fujifilm and Koujun Pharmaceutical Co., Ltd.), alumina (AKP-30, manufactured by Sumitomo Chemical), zinc oxide (manufactured by Kishida Chemical), and spinel-type oxide pigments containing cobalt and iron to obtain a mixed powder. Pure water was added to the obtained mixed powder to prepare a mixed slurry. The mixed slurry was ball-milled using zirconia balls with a diameter of 2 mm as the grinding medium to achieve D10 and D90 values ​​as listed in Table 1, resulting in a pulverized slurry. The pulverized slurry was dried at 110°C under atmospheric conditions, and then sieved to remove aggregates with a diameter greater than 180 mm. μ The powder of this embodiment is obtained by producing coarse particles of m.

[0176] Comparative Example 1 The powder of this comparative example was obtained using the same method as in Example 1, except that niobium oxide was not added.

[0177] Comparative Example 2 Except that TZ-3Y (manufactured by Tosoh Corporation) was used instead of TZ-3YS (manufactured by Tosoh Corporation) as 3 mol% yttrium oxide stabilized zirconium oxide, the powder of this comparative example was obtained by the same method as in Example 4. The composition and properties of the powders of these examples and comparative examples are shown in Table 1.

[0178] [Table 1]

[0179] (Preparation of sintered bodies) Example 9 The powder from Example 1 was subjected to die pressing at a pressure of 50 MPa and cold isostatic pressing (CIP) at a pressure of 196 MPa to form a molded body. The resulting molded body was then sintered at atmospheric pressure at 1400 °C to obtain a sintered body of this example with the following composition: 2.0 wt% niobium, 0.5 wt% iron, 0.25 wt% cobalt, 0.11 wt% zinc, 0.14 wt% alumina, and 3.0 mol% yttrium. The sintering conditions are described below.

[0180] Heating rate: 100℃ / h Sintering temperature: 1400℃ Sintering temperature holding time: 1 hour Cooling rate: 200℃ / h Examples 10 to 17, and Comparative Examples 3 and 4 Except for changing the powder and sintering temperature as shown in Table 2, the sintered bodies of each example or comparative example were obtained using the same method as in Example 9.

[0181] [Table 2]

[0182] In this embodiment and comparative example, the sintered bodies were all dark gray or black.

[0183] Table 3 shows the hues of Examples 9 to 17, and Comparative Examples 3 and 4.

[0184] [Table 3]

[0185] In any embodiment or comparative example, the formation of spinel-type metal oxides in the sintered body was confirmed by XRD patterning.

[0186] In Table 3, in the ball drop test, cases where no damage occurred are marked as "〇", and cases where damage occurred are marked as "×". Based on this, the number of times the steel ball fell when damage occurred is recorded in parentheses.

[0187] The sintered body of Comparative Example 4, prepared using powder from Comparative Example 1 that does not contain niobium, has a (-2) θ If the difference is less than 1.55°, the steel ball will break when dropped once in the drop test, confirming insufficient impact resistance.

[0188] In addition, it was confirmed that the specific surface area using BET was 17m². 2 / g or higher and D90 is 1.3 μ The crystallite diameter Dt of the sintered body of Comparative Example 5, prepared from powder of Comparative Example 2 (m or more), is less than 25 nm and 2 Figure 4A The difference is less than 1.54°.

[0189] Furthermore, it was confirmed that the sintered body of Comparative Example 5 cracked when a 25g steel ball was dropped once in the drop ball test, indicating insufficient impact resistance.

[0190] On the other hand, it contains stabilizing elements, niobium, alumina, iron, cobalt, and zinc, and has a BET specific surface area of ​​5.0 m². 2 / g or more and 17m 2 Below / g, and D90 is 1.3 Figure 4BZirconia powders from Examples 1 to 8 (with a diameter of less than m) were used to obtain sintered zirconia bodies from Examples 9 to 17, containing stabilizing elements, niobium, alumina, iron, cobalt, and zinc, with a crystallite diameter Dt of 25 nm or more and 100 nm or less. It was confirmed that the sintered body did not break when dropped three times by steel balls weighing 25 g to 50 g, demonstrating high impact resistance. Furthermore, it was confirmed that the transmittance at a thickness of 0.5 mm was 0%, indicating high shielding efficiency.

[0191] Furthermore, the sintered body of Comparative Example 4 (using powder: Comparative Example 1) which does not contain niobium oxide differs from the sintered body of Example 9 (using powder: same as Example 1) which contains 2.0% by mass of niobium oxide, and has a transmittance as high as 0.2%.

[0192] Using a commercially available LED lamp (manufactured by Sanwa Supply Co., Ltd., 800-LED028) as the light source, and with 0.5 mm thick sintered bodies of Comparative Example 4 and Example 9 mounted on a shielding plate with a 1 cm diameter hole, photographs are shown respectively. Figure 5 , Figure 4A as well as Figure 4B .

[0193] The sintered body of Comparative Example 4, with a transmittance of 0.2%, is as follows: Figure 5 and ​ As shown, the holes in the shielding plate can be observed through the upper surface of the sintered body. On the other hand, the sintered body of Example 9, with a transmittance of 0%, as shown... ​ As shown, the holes in the shielding plate cannot be observed from the upper surface of the sintered body, indicating high shielding performance.

[0194] The entire contents of the specification, claims, drawings, and abstract of Japanese Patent Application No. 2024-69543, filed on April 23, 1963, are incorporated herein by reference and are incorporated as a disclosure of the specification of this invention.

[0195] Explanation of reference numerals in the attached figures 1: Test sample 2: Repair tape 3: Ultra-hard board 4: Steel ball 5: Transparent polyvinyl chloride pipe 6: Fixture 7: Iron bar 8: Hole.

Claims

1. A zirconia sintered body, characterized in that, Include: Stabilizing elements, niobium, alumina, and iron, cobalt, and zinc as pigment components, The crystallite diameter of the zirconia sintered body, calculated from the XRD peaks of the (111) plane of tetragonal zirconia, is greater than 25 nm and less than 100 nm.

2. The zirconia sintered body according to claim 1, wherein, At least a portion of the pigment components forms a spinel-type metal oxide.

3. The zirconia sintered body according to claim 1 or 2, wherein, The stabilizing element includes one or more selected from calcium, yttrium, lanthanum, neodymium, gadolinium, erbium and ytterbium, and the content of the stabilizer is more than 2.0 mol% and less than 5.5 mol%.

4. The sintered zirconium oxide body according to any one of claims 1 to 3, wherein, The niobium content is above 0.1% by mass and below 3.0% by mass.

5. The sintered zirconium oxide body according to any one of claims 1 to 4, wherein, The manganese content is 0.5% by mass or more and 2.0% by mass or less.

6. The zirconia sintered body according to any one of claims 1 to 5, wherein, The alumina content is greater than 0% by mass and less than 30% by mass.

7. The zirconia sintered body according to any one of claims 1 to 6, wherein, The peak of the (400) facet of tetragonal zirconia is 2 θ 2 with the peak of the (004) plane belonging to tetragonal zirconia θ The difference is more than 1.54°.

8. The sintered zirconium oxide body according to any one of claims 1 to 7, wherein, The brightness L of the zirconia sintered body Those aged 40 and above and 65 and below.

9. The zirconia sintered body according to any one of claims 1 to 8, wherein, The total light transmittance of the zirconia sintered body is less than 0.1% when the thickness is 0.5 mm.

10. A zirconium oxide powder, characterized in that, Include: Stabilizing elements, niobium, alumina, and iron, cobalt, and zinc as pigment components, The stabilizer content is 2.0 mol% or more and 5.5 mol% or less, the niobium content is 0.1 wt% or more and 3.0 wt% or less, and the alumina content is greater than 0 wt% and 30 wt% or less. The zirconia powder has a BET specific surface area of ​​5.0 m². 2 / g or more and 17m 2 / g or less.

11. The zirconium oxide powder according to claim 10, wherein, The pigment components are contained in the zirconium oxide powder in the form of spinel-type metal oxides containing iron, cobalt, and zinc.

12. The zirconium oxide powder according to claim 10 or 11, wherein, The zirconium oxide powder, in terms of oxide content, has an iron content of 0.1% to 5% by mass, a cobalt content of 0.1% to 3% by mass, and a zinc content of 0.05% to 1% by mass.

13. The powder according to any one of claims 10 to 12, wherein, The 10% particle size D10 in the cumulative particle size distribution of the powder is 0.

15. μ m or more and 0.5 μ The particle size is below 1 μm, and 90% of the particles have a D90 of 0.5 μm. μ m or more and 1.3 μ Below m.

14. A component, characterized in that, The sintered body comprising any one of claims 1 to 9.

Citation Information

Patent Citations

  • Laminate

    JP2014054780A

  • Zirconia composition, zirconia calcined body and zirconia sintered body, and dental product

    JP2020180048A

  • Game machine

    JP2024069543A