Method for producing fiber reinforcements containing fluorinated copolymers
By using electrospinning with low-boiling-point solvents such as γ-valerol, the problems of health risks and insufficient β-phase content have been solved, enabling the effective use of high β-phase PVDF fiber webs in new energy applications.
Patent Information
- Application Number
- CN202580027704.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-29
- Filing Date
- 2025-04-29
- Publication Date
- 2026-11-17
AI Technical Summary
The solvents used in existing electrospinning technologies, such as DMAC, DMF, and NMP, are harmful to health and make it difficult to obtain a high proportion of β-phase PVDF fibers to improve their ferroelectric properties. Therefore, they cannot be effectively used as polymer electrolyte mechanical reinforcements for new energy applications such as fuel cells and battery packs.
PVDF copolymer fibers are produced by electrospinning using a mixture of γ-valerol and other low-boiling-point solvents such as acetone, dimethyl carbonate, methyl ethyl ketone, or 2-methyltetrahydrofuran as solvents, forming a fiber web with a high β-phase content.
It provides a more environmentally friendly solvent system, increases the proportion of the β phase in the fiber network, enhances its ferroelectric properties, and is suitable as a polymer electrolyte mechanical reinforcement in the new energy field.
Smart Images

Figure CN123125375A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for producing fibrous webs / webs by electrospinning a solution of a fluoropolymer, the fibrous web comprising fibers based on copolymers of repeating units derived from vinylidene fluoride (VDF). The invention also relates to fibrous webs obtainable by this method. Finally, the invention relates to fibrous webs intended for various applications in the field of new energy, particularly as mechanical reinforcements for polymeric electrolytes in fuel cells, electrolyzers, and battery packs. Background Technology
[0002] Electrospinning is an electrohydrodynamic method that allows the production of polymer nanofibers from a solution of one or more polymers by applying a high electrostatic field. The resulting submicron diameter fibers accumulate to form a fibrous web.
[0003] Submicron-diameter poly(vinylidene fluoride-copoly-hexafluoropropylene) (P(VDF-HFP)) fibers are used in various fields, such as new energy, due to their chemical resistance and good heat resistance. Currently, the main solvents used in the electrospinning of P(VDF-HFP) are N,N-dimethylacetamide (DMAC), dimethylformamide (DMF), and N-methylpyrrolidone (NMP), which are harmful to health and classified as Substances of Very High Concern (SVHC) by the European Chemicals Agency (ECHA). DMF, NMP, and DMAC are labeled "H360D - May harm an unborn fetus." Therefore, they are considered CMR solvents (carcinogenic, mutagenic, or reproductively toxic).
[0004] P(VDF-HFP) is a semi-crystalline thermoplastic copolymer that exhibits a complex structure depending on the chain conformation, attributed to five crystalline phases: α, β, γ, δ, and e. The β phase is the most polar phase and exhibits piezoelectric, thermoelectric, and ferroelectric properties.
[0005] Kundu et al. The publication “On the relevance of the polar β-phase of poly(vinylidene fluoride) for high-performance lithium-ion battery separators”, The Journal of Physical Chemistry, 2017, vol. 47, p. 121, describes how the presence of the β-phase in PVDF homopolymer and / or copolymer films is particularly advantageous for their application as battery separators, because materials with high β-phase content have higher polarity, thereby promoting lithium-ion migration into the separator.
[0006] Andrew et al. The publication "Effect of electrospinning on the ferroelectric phase content of polyvinylidene difluoride fibers", Langmuir, 2008, vol. 24, no. 3, pp. 670-672 describes the electrospinning of a solution of PVDF homopolymer in DMF. By varying certain parameters of the method, specifically the concentration of PVDF homopolymer in the solution and the voltage applied during electrospinning, the authors successfully obtained a network of PVDF homopolymer fibers with a crystallinity of 49% to 58%, and a β phase percentage of up to 75% in the crystalline phase. Therefore, the obtained fibers have a β phase content of 37% to 47% by weight, relative to the weight of the fibers.
[0007] To improve the durability of electrospinning technology, low toxicity and bio-based solvents (i.e., alternative green solvents) constitute a suitable strategy.
[0008] In document WO 2021 / 255389, the applicant describes a method for producing nonwoven webs of PVDF homopolymer or copolymer fibers by electrospinning a solution or homopolymer dispersion, wherein the solution or homopolymer dispersion comprises at least 15% by weight of dimethyl sulfoxide and at least one second liquid having a pressure of 7 MPa. 1 / 2 Up to 15 MPa 1 / 2 Hansen solubility parameter δ p And a boiling point strictly above 100 °C. DMSO is a green solvent with a melting point of 18 °C, which limits its use in room-temperature processing methods (such as electrospinning) due to the risk of polymer solution gelation.
[0009] It is still necessary to provide an electrospinning method using a liquid carrier that is not considered carcinogenic, mutagenic, or reproductively toxic by virtue of its composition.
[0010] An electrospinning method is also required, which provides a means of obtaining a fibrous web with a high proportion of β phase (relative to the weight of the fiber) in order to improve the ferroelectric properties of the web.
[0011] A method is also needed to provide a way to obtain fibrous networks intended to be used as mechanical reinforcements for polymer electrolytes in new energy applications (fuel cells, electrolyzers, and battery packs).
[0012] Another object of the present invention (at least according to some embodiments) is to provide an electrospinning method that provides a means of obtaining a fibrous web having a high proportion of β phase (relative to the weight of the fiber) in order to improve the ferroelectric properties of the web. Summary of the Invention
[0013] The present invention relates to a method for producing a nonwoven web of PVDF copolymer fibers by electrospinning a solution comprising the fluoropolymer dissolved in a mixture of solvents, characterized in that the mixture comprises a first solvent and a second solvent, the first solvent being γ-valerol (GVL) and the second solvent being a mixture of solvents or a pure solvent having a boiling point below 100 °C.
[0014] Typically, the second solvent is selected from acetone, dimethyl carbonate (DMC), methyl ethyl ketone (MEK), 2-methyltetrahydrofuran (2MTHF), or mixtures thereof.
[0015] Advantageously, none of the components of the solution used to dissolve the PVDF copolymer are considered to be carcinogenic, mutagenic, or reproductively toxic (CMR).
[0016] According to one embodiment, the solution has a Brinell viscosity of 50 to 3000 cP, preferably 75 to 1500 cP, and more preferably 80 to 500 cP at 20 °C, as measured according to standard ASTM D1238-13. According to one embodiment, the PVDF copolymer accounts for 6% to 25% by weight, preferably 10% to 21% by weight, relative to the total weight of the solution.
[0017] PVDF copolymers are copolymers having repeating units derived from VDF and at least one repeating unit derived from monomers other than VDF, wherein the other monomers are selected from the following list: vinyl fluoride (VF), tetrafluoroethylene (TFE), trifluoroethylene (TrFE), vinyl chlorofluoroethylene (CFE), dichlorofluoroethylene, trichlorofluoroethylene (CTFE), dichlorodifluoroethylene, trichlorofluoroethylene, hexafluoropropylene (HFP), trifluoropropylene, tetrafluoropropylene, trichlorofluoropropylene, hexafluoroisobutylene, perfluorobutylethylene, pentafluoropropylene, perfluoroethers, especially perfluoroalkyl vinyl ethers, ethylene, acrylic monomers, methacrylic monomers, and mixtures thereof.
[0018] According to one embodiment, the fluorinated copolymer is a P(VDF-HFP) copolymer.
[0019] The present invention also relates to a fibrous web that can be obtained by electrospinning, the P(VDF-HFP) web being characterized by a crystallinity of 29% to 34% (a degree determined by DSC from the melting enthalpy of P(VDF-HFP) at 104.5 J / g) and a percentage of the β phase in the crystalline phase between 41% and 69% (a content determined by infrared spectroscopy).
[0020] The present invention also relates to the use of the PVDF copolymer fiber network as a mechanical reinforcement for polymer electrolytes in fuel cells, electrolyzers and battery packs.
[0021] This invention overcomes the shortcomings of existing technologies. Electrospinning of PVDF copolymers using γ-valerol is a more sustainable and improved approach for producing fluoropolymer fiber webs. γ-valerol is a biomass-derived, sustainable solvent and is not classified as a reproductively toxic CMR solvent. Attached Figure Description
[0022] Figure 1 A reactor is schematically shown for preparing an electrospinning solution intended for use in the method according to the invention.
[0023] Figure 2 The image shows a scanning electron microscope (SEM) image of a fiber web obtained by electrospinning according to the invention, the fiber web being obtained from a mixture of γ-valerol and acetone solvent (see embodiments according to the invention). Detailed Implementation
[0024] All ranges listed in this patent application include endpoints unless otherwise stated.
[0025] The fluorinated copolymer used in the method according to the invention is based on repeating units derived from vinylidene fluoride (VDF). The proportion of repeating units derived from VDF is at least 50 mol%, relative to the total number of moles of repeating units in the fluorinated polymer.
[0026] According to some embodiments, the fluorinated copolymer comprises at least 60 mol%, or at least 70 mol%, or at least 75 mol%, or at least 80 mol%, or at least 85 mol%, or at least 90 mol%, or at least 95 mol% of units derived from VDF. The term "polymer" refers to a polymer obtained by copolymerizing at least two chemically different monomers (referred to as comonomers).
[0027] The copolymer has repeating units derived from VDF and at least one repeating unit derived from monomers other than VDF, wherein the comonomers are selected from the following list: vinyl fluoride (VF), tetrafluoroethylene (TFE), trifluoroethylene (TrFE), vinyl chlorofluoroethylene (CFE), dichlorofluoroethylene, trichlorofluoroethylene (CTFE), dichlorodifluoroethylene, trichlorofluoroethylene, hexafluoropropylene (HFP), trifluoropropylene, tetrafluoropropylene, trichlorofluoropropylene, hexafluoroisobutylene, perfluorobutylethylene, pentafluoropropylene, perfluoroethers, especially perfluoroalkyl vinyl ethers, ethylene, acrylic monomers, methacrylic monomers, and mixtures thereof.
[0028] It should be clearly understood that all geometric isomers of the fluorinated compounds mentioned above are included in the above terminology, such as: 1,1-chlorofluoroethylene (1,1-CFE), 1,2-chlorofluoroethylene (1,2-CFE), 1,2-dichloro-1,2-difluoroethylene, 1,1-dichloro-1,1-difluoroethylene and 1,1,2-trichloro-2-fluoroethylene, 3,3,3-trifluoropropylene, 2-chloro-3,3, 3-Trifluoropropene (1233xf), 1-chloro-3,3,3-trifluoropropene (1233zd), 1,3,3,3-tetrafluoropropene, 2,3,3,3-tetrafluoropropene (or 1234yf), 3-chloro-2,3,3-trifluoropropene (or 1233yf), 3-chloro-3,3,3-trifluoropropene, 1,1,3,3,3-pentafluoropropene or 1,2,3,3,3-pentafluoropropene.
[0029] Among perfluoroalkyl vinyl ethers, those of the general formula can be mentioned: R f -O-CF-CF2, R f It is an alkyl group, preferably a C1 to C4 alkyl group, and for example, methyl vinyl ether (MVE) or isopropyl vinyl ether (PVE).
[0030] According to certain variants, the fluorinated copolymer is a mixture of one or more copolymers selected from the following: P(VDF-TrFE), P(VDF-HFP), P(VDF-TFE), P(VDF-TrFE-CFE), P(VDF-TrFE-CTFE), P(VDF-TFE-CFE), and P(VDF-TFE-CTFE).
[0031] According to one embodiment, the fluoropolymer is a P(VDF-HFP) copolymer. The P(VDF-HFP) advantageously has a molar proportion of 5% to 35% repeating units derived from HFP.
[0032] Fluoropolymer solution
[0033] The fluoropolymer solution comprises the polymer dissolved in a mixture of solvents, the mixture comprising a first solvent and a second solvent, the first solvent being γ-valerolactone (GVL) and the second solvent being a mixture of solvents or a pure solvent having a boiling point below 100 °C.
[0034] Advantageously, the second solvent is selected from acetone, dimethyl carbonate (DMC), methyl ethyl ketone (MEK), 2-methyltetrahydrofuran (2MTHF), or mixtures thereof.
[0035] The solvent mixture can dissolve the polymer to form a true solution (i.e., a single-phase or homogeneous solution at the molecular level); in this way, it is easier to obtain nonwoven webs of PVDF copolymer fibers with a high proportion of β phase.
[0036] The mass content of the first solvent is between 10% and 70%, preferably between 30% and 50%, relative to the weight of the solution. The mass content of the PVDF copolymer is between 6% and 25%, preferably between 10% and 21%, relative to the weight of the solution.
[0037] The preparation of electrospinning solutions involves dissolving PVDF copolymers in a solvent mixture.
[0038] According to one implementation method, such as Figure 1 As shown, a first solvent and a second solvent (or a mixture of solvents) are introduced into an 8 L jacketed vertical reactor equipped with a three-bladed propeller stirrer and a condenser. The PVDF copolymer, in powder form, is slowly introduced into the solvent under mechanical stirring. Dissolution is carried out under heating conditions and with stirring at temperatures between 30 and 70 °C.
[0039] The hydrodynamic conditions depend on the type of agitator used. Agitators that promote axial flow are particularly preferred. Agitation time is typically from 30 minutes to 24 hours. Agitation time is preferably less than or equal to 12 hours, more preferably less than or equal to 6 hours, and most preferably less than or equal to 4 hours.
[0040] According to one embodiment, the PVDF copolymer in powder form is dissolved in a mixture of solvents at a temperature between 30 and 70°C for a time range of 1 to 5 hours.
[0041] When all particles have dissolved and the solution is clear, electrospinning can be performed on the electrospinning solution.
[0042] According to some embodiments, the solution (correspondingly a uniform dispersion) has a Brookfield viscosity of 50 to 3000 cP, preferably 75 to 1500 cP, and more preferably 80 to 500 cP at a measurement temperature of 20 °C to 25 °C, preferably 20 °C. To measure the Brookfield viscosity, a Brookfield viscometer (e.g., DV II+ PRO) can be used.
[0043] Electrospinning method
[0044] The present invention relates to a method for producing a nonwoven web of PVDF copolymer fibers by electrospinning the solution described above to form the web.
[0045] The term "fiber" is understood to refer to filamentous elements that are typically described by their diameter and length.
[0046] "Nonwoven fiber webs" are understood to refer specifically to fibrous assemblies obtained by assembling fibers without weaving or knitting. An additional definition has been proposed by EDANA (…). European Disposables and Nonwovens Association, European Disposable Products and Nonwovens Association According to standard EN ISO 9092, it means a sheet made of single fibers that are directly or randomly oriented and bonded by friction, cohesion or adhesion.
[0047] According to one embodiment, the electrospinning method is implemented using an electrospinning apparatus, which may be a needle, thread or cable, cylinder, disc or rotating disc, cone, spiral or pyramidal system, or other system capable of producing fibers under the influence of an electric field. The apparatus includes an electrospinning solution tank and a system for supplying the solution to the electrospinning apparatus at a controlled flow rate. The electrospinning apparatus is connected to a positive high-voltage generator. A metal collecting electrode is placed opposite the electrospinning apparatus and connected to a negative high-voltage generator or ground. The voltage difference during electrospinning generates an electric field. Multiple filaments of the solution are generated at the electrospinning apparatus under the influence of this field and guided to the collecting electrode. Whip movement between the electrospinning apparatus and the collecting electrode causes solvent evaporation. Solid PVDF copolymer fibers are deposited on a substrate placed above the collecting electrode.
[0048] Several parameters of the method can be adjusted to obtain a web with advantageous properties, particularly a web of fibers having desired dimensions, a substantially uniform appearance, and minimizing the presence of polymer beads. The electrospinning parameters are specifically: - Voltage on the electrospinning device: between 1 kV and 80 kV; - Voltage on the collecting electrode: between 0 kV and -40 kV; - The distance between the electrospinning device and the collecting electrode: between 1 cm and 50 cm; - Flow rate of polymer solution: between 0.1 g / min and 20 g / min; - The speed of the rolling belt: between 0.01 m / min and 15 m / min; - The relative humidity of the air in the electrospinning room is between 0% and 50%. - Indoor air temperature: between 10 °C and 40 °C.
[0049] The fibrous web enters the drying oven at the exit of the electrospinning chamber. The oven temperature is between 25 °C and 70 °C. The fibrous web is then cooled to ambient temperature (25 °C). This drying step can, where appropriate, evaporate residual solvent and optionally increase the crystallinity of the fluoropolymer, and thus improve its ferroelectric properties.
[0050] The electrospun fiber web has a crystallinity of 29% to 34% (the degree of crystallinity determined by differential scanning calorimetry (DSC) from the enthalpy of fusion of P(VDF-HFP) at 104.5 J / g).
[0051] The percentage of β phase in the crystalline phase is between 41% and 69% (content determined by Fourier transform infrared spectroscopy or FTIR spectroscopy). The fibers have different weight contents of β phase, and the maximum content relative to the weight of the fiber, calculated by multiplying the degree of crystallinity by the percentage of β phase in the crystalline phase, is 21% for the fibrous web produced from a mixture of acetone and γ-valerolactone P(VDF-HFP).
[0052] According to certain embodiments, the β-phase weight content (relative to the weight of the fiber) measured in PVDF copolymer fibers electrospun from γ-valerol is higher than that of PVDF copolymer fibers electrospun from other more sustainable solvents and those assessed by conventional CMR. More specifically, the percentage of this β-phase in the crystalline phase is higher than that obtained from fiber webs produced from a mixture of P(VDF-HFP) in acetone and dimethyl sulfoxide.
[0053] These noteworthy properties are also advantageous in piezoelectric applications.
[0054] According to certain embodiments, the elastic modulus E' measured on an ion exchange membrane reinforced with a fibrous web prepared from a PVDF copolymer electrospun from γ-valerol is greater than the elastic modulus of a PVDF copolymer fibrous web electrospun from other more sustainable solvents and conventional CMR-evaluated. More specifically, this elastic modulus is greater than that obtained with an ion exchange membrane reinforced with a fibrous web produced from a mixture of acetone and P(VDF-HFP) in dimethyl sulfoxide.
[0055] These noteworthy properties are also advantageous in applications as mechanical reinforcements for polymer electrolytes, which are ion-exchange polymer membranes in electrolyzers or fuel cells, or polymer separators in battery packs.
[0056] Depending on the operating conditions of the electrospinning method, and especially the distance between electrodes, voltage, and solution flow rate, the diameter of electrospun PVDF copolymer fibers can be less than 200 nm.
[0057] Applications of PVDF copolymer fiber networks
[0058] According to one embodiment, the present invention relates to the use of the PVDF copolymer fiber network described above as a mechanical reinforcement for a polymer electrolyte. The polymer electrolyte may be an ion-exchange polymer membrane in a fuel cell or electrolyzer.
[0059] According to one embodiment, the present invention relates to the use of the PVDF copolymer fiber mesh described above as a mechanical reinforcement of a polymer electrolyte, wherein the electrolyte is a polymer separator in a battery pack.
[0060] Depending on the selected electrospinning conditions, PVDF copolymer fiber webs are produced with a thickness varying between 1 and 200 µm, preferably between 2 and 100 µm, and a basis weight ranging from 0.5 g / m² to 100 g / m², preferably from 1 g / m² to 50 g / m², for use in the new energy field, particularly as mechanical reinforcements for polymer electrolytes in fuel cells, electrolyzers, and battery packs.
[0061] The mesh is composed of PVDF copolymer fibers and has a basis weight that varies depending on the application.
[0062] Example
[0063] exist Figure 1An electrospinning solution containing 14 wt% P (VDF-HFP, with 10% HFP), 43 wt% acetone, and 43 wt% γ-valerolactone was prepared in the reactor described herein. First, γ-valerolactone and acetone were introduced into the reactor. Powdered P (VDF-HFP) was slowly introduced into the solvent mixture under cold conditions and with mechanical stirring at 300 rpm. A temperature-controlled bath was opened at 50 °C and dissolution was carried out under hot conditions and stirring for 2 to 3 hours. When all particles had dissolved and the solution was clear, the electrospinning solution was ready for electrospinning.
[0064] The prepared fluoropolymer solution was electrospun using the following electrospinning parameters: - The flow rate of the polymer solution = 3 g / min; - The rotational speed of the electrospinning device = 11,000 rpm; -Electrode distance = 18 cm; - Relative humidity = 15%; -Air temperature = 30 °C.
[0065] The obtained fibrous network was characterized by scanning microscopy, such as in... Figure 2 As shown in the figure, the measured average fiber diameter is 136 + / - 75 nm.
[0066] The fiber web was electrospun in a second electrospinning apparatus using different solvent mixtures. The degree of crystallinity was determined by measuring the enthalpy of fusion ΔH, which was obtained by integrating the melting peak on a DSC thermogram. mea Compared with the literature value ΔH of 100% crystalline PVDF lit (104.5 J / g) was obtained by comparison. The following formula is used to calculate the relative crystallinity X. C : [Formula 1]
[0067] The percentage of the β phase in the crystalline phase of the PVDF copolymer was determined by interpreting the spectrum obtained by Fourier transform infrared spectroscopy (FTIR).
[0068] The results obtained (crystallization) X C The degree of β phase, the percentage of β phase in the crystalline phase of P(VDF-HFP), and the weight content of β phase in the powder and fiber network are shown in Table 1.
[0069] [Table 1]
[0070] The fibers contain β phases with varying weight contents, with the maximum content obtained relative to the weight of the fibers being 21% for a fibrous web produced from a mixture of acetone and γ-valerolactone containing P(VDF-HFP).
[0071] The obtained fibrous network was impregnated with 20% by weight of Nafion concentrated alcohol / water dispersion (NafionTMD2020CS). To do this, the Nafion dispersion was poured onto a glass plate and the fibrous network was gently deposited onto the wet surface. The membrane was then placed in an oven preheated to 120 °C. After drying for 2 hours, the enhanced ion exchange membrane was separated from the glass plate in a water bath and then dried at ambient temperature for 24 hours.
[0072] Dynamic mechanical analysis (DMA) was used on a mechanical testing bench to characterize the viscoelastic behavior of ion exchange membranes reinforced with fiber meshes. This apparatus can be used to calculate the elastic modulus E'. Samples were heated to temperatures varying from 20 to 150 °C at a rate of 4 °C / min.
[0073] The results are shown in Table 2.
[0074] [Table 2]
[0075] Ion exchange membranes reinforced with different P(VDF-HFP) fiber meshes have different elastic moduli E', with the highest temperature modulus measured on ion exchange membranes reinforced with fiber meshes produced from a mixture of acetone and γ-valerolactone P(VDF-HFP).
Claims
1. A method for producing a nonwoven web of poly(vinylidene fluoride) (PVDF) copolymer fibers by electrospinning a solution, wherein the solution comprises the PVDF copolymer dissolved in a mixture of solvents, characterized in that... The mixture comprises a first solvent and a second solvent, the first solvent being γ-valerolactone, and the second solvent being a solvent mixture or a pure solvent having a boiling point below 100 °C, the second solvent being selected from acetone, dimethyl carbonate, methyl ethyl ketone, 2-methyltetrahydrofuran, or mixtures thereof.
2. The production method according to claim 1, wherein the mass content of the first solvent is between 10% and 70%, preferably between 30% and 50%, relative to the weight of the solution.
3. The production method according to any one of claims 1 and 2, wherein the mass content of the PVDF copolymer is between 6% and 25%, preferably between 10% and 21%, relative to the weight of the solution.
4. The production method according to any one of claims 1 to 3, wherein the PVDF copolymer has at least 50 mol% of repeating units derived from vinylidene fluoride (VDF) relative to the total number of moles of repeating units of the PVDF copolymer, and at least one repeating unit derived from monomers other than VDF, wherein the comonomer is selected from the following list: vinyl fluoride (VF), tetrafluoroethylene (TFE), trifluoroethylene (TrFE), vinyl chlorofluoroethylene (CFE), dichlorofluoroethylene, trichlorofluoroethylene (CTFE), dichlorodifluoroethylene, trichlorofluoroethylene, hexafluoropropylene (HFP), trifluoropropylene, tetrafluoropropylene, trichlorofluoropropylene, hexafluoroisobutylene, perfluorobutylethylene, pentafluoropropylene, perfluoroethers, especially perfluoroalkyl vinyl ethers, ethylene, acrylic monomers, methacrylic monomers, and mixtures thereof.
5. The production method according to any one of claims 1 to 4, wherein the solution has a Brinell viscosity of 50 to 3000 cP, preferably 75 to 1500 cP, and more preferably 80 to 500 cP at 20 °C, as measured according to standard ASTM D1238-13.
6. The production method according to any one of claims 1 to 5, wherein the PVDF copolymer is a poly(vinylidene fluoride-copolymer-hexafluoropropylene) (P(VDF-HFP)) copolymer.
7. The production method according to claim 6, wherein the P(VDF-HFP) has a molar ratio of 5% to 35% of repeating units derived from HFP.
8. The production method according to any one of claims 1 to 7, wherein the PVDF copolymer in powder form is dissolved in a solvent mixture at a temperature of 30 to 70 °C for 1 to 5 h.
9. The production method according to any one of claims 1 to 8, implemented by means of an apparatus comprising: an electrospinning solution tank, a system for supplying the electrospinning solution to an electrospinning apparatus connected to a positive high voltage generator, and a metal collecting electrode placed opposite the electrospinning apparatus and connected to a negative high voltage generator or grounded.
10. The method of claim 9, wherein at the outlet of the electrospinning chamber, the PVDF copolymer fibers undergo a drying step in an oven at an oven temperature between 25 °C and 70 °C.
11. A network obtainable by the method of any one of claims 1 to 10, wherein the PVDF copolymer fiber network is characterized by a crystallinity of 29% to 34% and a percentage of β phase in the crystalline phase between 41% and 69%.
12. Use of the mesh according to claim 11 as a mechanical reinforcement for polymer electrolytes in fuel cells, electrolyzers and battery packs, wherein the mesh has a thickness ranging from 1 to 200 µm, preferably from 2 µm to 100 µm, and a basis weight ranging from 0.5 g / m² to 100 g / m², preferably from 1 g / m² to 50 g / m².
13. The use as a mechanical reinforcement for a polymer electrolyte according to claim 12, wherein the polymer electrolyte is an ion-exchange polymer membrane in a fuel cell.
14. The use as a mechanical reinforcement of a polymer electrolyte according to claim 12, wherein the polymer electrolyte is an ion-exchange polymer membrane in an electrolyzer.
15. The use as a mechanical reinforcement for a polymer electrolyte according to claim 12, wherein the polymer electrolyte is a polymer separator in a battery pack.
Citation Information
Patent Citations
Method for producing an assembly of fibres comprising a fluorinated polymer made from vdf
WO2021255389A1