Manufacturing methods of coating liquid, antireflective film and lens
By forming a multi-layer anti-reflective film using a coating liquid containing functional microparticles and adhesive components on a small lens, the problem of insufficient anti-reflective performance in the prior art is solved, achieving a highly efficient anti-reflective effect and wear resistance.
Patent Information
- Application Number
- CN202580027960.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-08-13
- Filing Date
- 2025-04-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing anti-reflective technologies still have room for improvement in terms of anti-reflective performance, especially in small lenses where it is difficult to achieve a highly effective anti-reflective effect.
A coating liquid containing functional microparticles, adhesive components, and solvents is used to form a multi-layer antireflective film on the lens surface. The low refractive index of the functional microparticles and the fixing effect of the adhesive, combined with appropriate heat treatment, form a stable antireflective layer.
It improves the anti-reflective performance of the lens, enhances its wear resistance and optical properties, and ensures effective anti-reflective performance on small lenses.
Smart Images

Figure CN123125513A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for manufacturing a coating liquid, an anti-reflective film, and a lens. Background Technology
[0002] Currently, there are known technologies for preventing or reducing light reflection from the surface of objects.
[0003] For example, Patent Document 1 describes a substrate on which a film is formed on the surface of a substrate, the film comprising hollow spherical silica-based microparticles and a coating matrix. The silica-based microparticles have cavities formed inside a porous outer shell, and these cavities contain a solvent or gas. Because the silica-based microparticles have a low refractive index, the coating also has a low refractive index, resulting in excellent anti-reflective properties.
[0004] Patent document 2 describes an antireflective film having a hard coating, a high-refractive-index layer, and a low-refractive-index layer on the surface of an organic film, starting from the lower layer side. The high-refractive-index layer is a synthetic resin-based thin film containing microparticles of metal oxides such as ZrO2. The synthetic resin is a UV- or electron beam-curing synthetic resin.
[0005] Patent Document 3 describes an antireflective laminate comprising a coating film, which is formed by a one-coat method using a coating composition in which low-refractive-index microparticles and medium to high-refractive-index microparticles are dispersed in an adhesive resin. The low-refractive-index microparticles are silica microparticles treated with a fluorine-based compound. As a result, due to the difference in specific gravity, the low-refractive-index microparticles are concentrated in the upper to middle portion of the coating film, while the medium to high-refractive-index microparticles are concentrated in the middle to lower portion.
[0006] Existing technical documents Patent documents Patent Document 1: Japanese Patent Application Publication No. 2001-233611 Patent Document 2: Japanese Patent Application Publication No. 2001-350001 Patent Document 3: Japanese Patent Application Publication No. 2007-272132 Summary of the Invention
[0007] The technical problem that the invention aims to solve The technologies described in Patent Documents 1 to 3, from the viewpoint of anti-reflective performance, still have room for further research. The object of the present invention is to provide a novel method for manufacturing a coating liquid, an anti-reflective film, and a lens that is advantageous from the viewpoint of anti-reflective performance.
[0008] Technical solutions for solving technical problems Item 1. A coating liquid for forming at least one antireflective film on a lens unit comprising a plurality of resin lenses. The aforementioned lens has an outer diameter of less than 20 mm. The above coating solution contains: Multiple functional microparticles have a refractive index lower than that of the lenses mentioned above; The adhesive component, which is an adhesive precursor, is capable of fixing the functional microparticles to each other in the antireflective film and fixing the antireflective film to the lens; and At least one solvent having a boiling point lower than that of the aforementioned adhesive components.
[0009] Item 2. The coating liquid as described in Item 1, wherein the lens unit comprises a lens having a center thickness of less than 1 mm.
[0010] Item 3. The coating liquid as described in Item 1 or 2, wherein the lens unit is built into a portable device.
[0011] Item 4. The coating liquid as described in any one of items 1 to 3, wherein the lens unit comprises a lens having at least one surface comprising an axisymmetric concave surface and a convex surface.
[0012] Item 5. The coating liquid as described in any one of items 1 to 4, wherein the first solvent comprises a solvent having a boiling point of 60°C or higher and 140°C or lower.
[0013] Item 6. The coating liquid as described in Item 5, further comprising a second solvent, The second solvent mentioned above has a boiling point above 150°C and a surface energy of more than 30 dyne / cm.
[0014] Item 7. The coating liquid as described in any one of items 1 to 6, wherein the mass ratio of the functional microparticles to the total mass of the functional microparticles and the adhesive component is 80% or more.
[0015] Item 8. The coating liquid as described in any one of items 1 to 7, wherein the deviation of the particle size of the functional microparticles is within ±20%.
[0016] Item 9. The coating liquid as described in any one of items 1 to 8, wherein the total mass ratio of the functional microparticles and the adhesive component to the coating liquid is 20% or less.
[0017] Item 10. The coating liquid as described in any one of items 1 to 9, wherein, The number of the aforementioned functional microparticles is as follows when the film is formed on the aforementioned lens: 3S / 2R and above, Wherein, S is the surface area of the lens to be coated with the coating liquid, and R is the diameter of the functional microparticles.
[0018] Item 11. The coating liquid as described in Item 10, wherein R is 55 ± 10 nm. The number of the above-mentioned functional microparticles is Below 3S / R.
[0019] Item 12. The coating liquid as described in any one of items 1 to 11, wherein the adhesive component is a composition having Si-OR (R represents an alkyl group having 1 to 4 carbon atoms) as the main component.
[0020] Item 13. The coating liquid as described in any one of items 1 to 12, wherein the solvent comprises a first solvent and a second solvent. The boiling point of the second solvent is higher than that of the first solvent.
[0021] Item 14. An antireflective film, formed by applying the coating liquid of any one of items 1 to 13 to the lenses described above, and then firing it at a temperature lower than the boiling point of the solvent.
[0022] Item 15. The antireflective film as described in Item 14, wherein R > 5r. Where R is the diameter of the aforementioned functional microparticles, and r is the cross-sectional diameter of the adhesive.
[0023] Item 16. The antireflective film as described in Item 14 or 15, wherein the aforementioned functional microparticles are stacked on the lens in a square-dense packing manner.
[0024] Item 17. The antireflective film as described in Item 16, wherein the refractive index is 1.16 or less.
[0025] Item 18. An antireflective film formed using any one of items 1 to 13, wherein the refractive index n is 1.16 or less.
[0026] Item 19. An antireflective film formed using any one of items 1 to 13, wherein the functional microparticles are stacked in two layers when fired at a temperature below the boiling point of the solvent.
[0027] Item 20. An optical thin film, which is an optical thin film on a light control component, wherein, The aforementioned optical film comprises microparticles and an adhesive that fixes the microparticles. The ratio of the above-mentioned adhesive to the above-mentioned particles is 0.5 or less by mass. The number of defects is less than 5.
[0028] Item 21. A method for manufacturing a lens, comprising: The step of coating a coating liquid onto the surface of a lens substrate, the coating liquid comprising: a plurality of functional microparticles having a refractive index lower than that of the lens substrate; an adhesive component capable of binding the functional microparticles and serving as an adhesive precursor; and a first solvent having a boiling point lower than that of the adhesive component; and The step of heating the above coating liquid to form an antireflective film.
[0029] Item 22. A method of manufacturing a lens as described in Item 21, wherein the lens substrate has at least one surface comprising an axisymmetric concave surface and a convex surface.
[0030] Item 23. A method of manufacturing a lens as described in Item 21 or 22, wherein the coating liquid further comprises a second solvent having a boiling point higher than that of the first solvent.
[0031] Item 24. A method of manufacturing a lens as described in any one of items 21 to 23, wherein the coating liquid further comprises at least one selected from a particle adhesion inhibitor or a dispersant.
[0032] Item 25. The method of manufacturing a lens as described in Item 24, further comprising the step of treating the formed antireflective film with at least one of plasma treatment, corona treatment, UV cleaning, high temperature treatment, organic cleaning, acid cleaning, and alkaline cleaning.
[0033] Invention Effects This invention is advantageous from the viewpoint of anti-reflective performance. Attached Figure Description
[0034] Figure 1 This is a cross-sectional view of a camera unit using the anti-reflective film of the present invention.
[0035] Figure 2 This is a cross-sectional view of the anti-reflective film.
[0036] Figure 3 This is a cross-sectional view showing another example of an anti-reflective film.
[0037] Figure 4 This is a cross-sectional view showing an example of a nozzle used for spray coating.
[0038] Figure 5 This is a diagram showing the lenses arranged on the surface before coating.
[0039] Figure 6 This is a cross-sectional view of the lens after the coating liquid composition has been applied.
[0040] Figure 7 This is a cross-sectional view showing another example of an anti-reflective film.
[0041] Figure 8The photograph was obtained by taking a cross-section of the antireflective film formed in Example 1 using SEM. Detailed Implementation
[0042] The following describes one embodiment of the coating liquid for the antireflective film of the present invention. In this embodiment, the application of the coating liquid to the lens included in the imaging unit will be described with reference to the accompanying drawings. The imaging unit and the antireflective film (optical thin film) will be described first, followed by the description of the coating liquid. Furthermore, Figure 1 This is a schematic diagram used to illustrate the various parts or features of a camera unit. The number, shape, size, arrangement of lenses, and distances between components are not accurately represented based on the actual configuration. Furthermore, Figure 1 For ease of explanation, three lenses (L1, L2, L3) are illustrated, but the present invention is not limited to this. It should be noted that the invention also includes cases with more than three lenses or fewer than three lenses.
[0043] <1. Camera Unit> Figure 1 This is a cross-sectional view of the camera unit according to this embodiment. The camera unit is installed in devices such as smartphones, tablet PCs, and laptop PCs (sometimes referred to as portable devices), and includes a lens unit 100, an image sensor (here, a solid-state image sensor) D, and a sensor substrate W on which the solid-state image sensor D is provided.
[0044] Lens unit 100 holds three or more lenses L1, L2, L3 (hereinafter referred to as the first to third lenses) separated by spacer 12 from the light incident side. Figure 1 The lenses are formed by stacking them sequentially (top side). Additionally, as shown in the figure, the surface of each lens is composed of curved surfaces.
[0045] The first lens L1 has a first upper lens surface 10A and a first lower lens surface 10B. More specifically, a convex first upper lens surface 10A is formed on the upper surface of the first lens L1, and a concave first lower lens surface 20A is formed on the lower surface. A black light-shielding film 14 is provided on the first lens L1 for the purpose of blocking light from the area of the first upper lens surface 10A other than the lens surface. Similarly, a black light-shielding film 14 is provided on the area of the first lower lens surface 20A other than the lens surface. The shape of the pattern of the black light-shielding film 14 is not limited, and the black light-shielding film 14 can be formed in a pattern with openings at the portions intersecting the optical axes of the two lenses 10A and 10B. The same black light-shielding film 14 is also provided on the second and third lenses L2 and 3. However, although the black masking film 14 is formed from the lens surface to the vicinity of the spacer 12 (described later), it is also formed from the lens surface to the vicinity of the spacer 12 (described later) and is separate from the spacer 12.
[0046] The second lens L2 has a second upper lens surface 20A and a second lower lens surface 20B. More specifically, a second upper lens surface 10B with a concave lens surface is formed on the upper surface of the second lens L2, and a second lower lens surface 20B with a convex shape is formed on the lower surface. A black light-shielding film 14 is provided in the area of the second upper lens surface 10B other than the lens surface, i.e., at the lens edge, on the light-incident side of the second lens L2. Figure 1 In the example shown, the black light-shielding film 14 is not provided on the lower surface of the second lens L2, but a patterned black light-shielding film 14 can also be provided on the area other than the lens surface of the second lower lens surface 20B.
[0047] The third lens L3 has a third upper lens surface 30A and a third lower lens surface 30B. More specifically, the third upper lens surface 30A, which has a lens surface with an aspherical or other curved shape, is formed on the upper surface of the third lens L3, and the third lower lens surface 30B, which also has a lens surface with an aspherical or other curved shape, is formed on the lower surface. In the region near the optical axis of the third upper lens surface 30A, it forms a convex surface symmetrical about the optical axis on the image side (upper side of the attached diagram), and in its peripheral region, it forms a concave surface symmetrical about the optical axis on the image side. On the other hand, the third lower lens surface 30B has a shape opposite to that of the third upper lens surface 30A. In lenses with this shape, because the peripheral region is concave, the coating liquid (described later) tends to accumulate in this region, preventing uniform film formation and posing a risk of not obtaining an effective reflection effect. To address this, as described later, for example, by using a solvent with a surface energy of 30 dyne / cm or higher, a uniform film can be formed. Furthermore, Figure 1 The aspherical shape of the third lens L3 shown is one example, but it can also be other shapes.
[0048] In addition, a black light-shielding film 14 is provided on both sides of the third lens L3, excluding the lens surfaces of each lens 30A and 30B.
[0049] The six lens surfaces 10A, 10B, 10C, 20A, 20B, 30A, and 30B are all formed in a shape that is rotationally symmetrical about the optical axis center. Each lens L1, L2, and L3 is supported by the spacer 12 in such a manner that the optical axes of all lens surfaces 10A, 10B, 10C, 20A, 20B, 30A, and 30B are aligned. It should also be noted that each lens is arranged with its own optical axis approximately aligned. Figure 1 The schematic diagram shown represents a cross section including its optical axis.
[0050] Furthermore, a sensor substrate W is disposed below the spacer 12. Therefore, the sensor substrate W is disposed at a distance from the third lens L3. For example, it is formed by cutting a wafer made of a semiconductor material such as silicon into a roughly rectangular shape when viewed from above. A solid-state imaging element D is disposed near the center of the sensor substrate W. The solid-state imaging element D is, for example, a CCD image sensor or a CMOS image sensor, which, after being chip-based, can be bonded to a semiconductor substrate on which wiring is formed. Alternatively, the solid-state imaging element D can be constructed by performing known film deposition processes, photolithography processes, etching processes, impurity addition processes, etc., on the sensor substrate W to form electrodes, insulating films, wiring, etc.
[0051] The spacer 12 is cylindrical, with three annular grooves 121 spaced axially on its inner circumferential surface. The outer peripheries of each lens L1, L2, and L3 are embedded into each groove 121, thereby holding each lens L1, L2, and L3 spaced apart within the spacer 12. Alternatively, the spacer 12 can be a component shaped to surround the solid-state imaging element D. By using the spacer 12 to surround the solid-state imaging element D and isolate it from the outside, light blocking can be achieved, preventing light other than that transmitted through the lenses from entering the solid-state imaging element D. Furthermore, by sealing the solid-state imaging element D from the outside, dust can be prevented from adhering to the solid-state imaging element D.
[0052] With the above configuration, the spacer 12 is designed such that the lens surfaces 10A, 10B, 20A, 20B, 30A, and 30B of the lenses L1, L2, and L3 image the subject onto the solid-state imaging element D.
[0053] Furthermore, the configuration of the spacer 12 is not particularly limited. As long as it can maintain a positional relationship between lenses L1, L2, and L3, or between lens L3 and sensor substrate W, at a predetermined distance, its shape is not particularly limited and can be appropriately modified. The spacer 12 can be joined to the lens area (the area where the lens functions) of each lens L1, L2, and L3. However, in addition to mounting each lens on one spacer as described above, spacers can also be installed between each lens L1, L2, and L3 to form a gap.
[0054] Alternatively, a housing can be provided to house the camera unit, which also holds the lens. In this case, the housing serves as a spacer. Alternatively, the outer periphery of the lens region can be made into a thick wall, which also serves as a spacer. Furthermore, the thick wall outside the lens region can be combined with a light-shielding film to achieve the function of a spacer.
[0055] An infrared cutoff filter or cover glass can also be placed between the lens module and the sensor substrate W. In this case, the position of each filter or cover glass is defined by a spacer or housing. If there are three or more lenses, the sensor substrate can be positioned outside the lowermost lens.
[0056] The camera unit configured as described above is reflowed and mounted onto a circuit board (not shown) built into a smartphone or similar device. Appropriate solder paste is pre-printed on the circuit board at the location where the camera unit is to be mounted. The camera unit is then placed there, and the circuit board containing the camera unit is subjected to heating treatment such as infrared irradiation or hot air blowing, thereby fusing the camera unit to the circuit board.
[0057] Each lens L1, L2, and L3 can be formed of resin. For example, ultraviolet-curable resin, thermosetting resin, or thermoplastic resin can be used as such resin. However, considering the reflow mounting of the aforementioned camera unit, a relatively high glass transition temperature is preferred, for example, 110°C or higher, and more preferably 250°C or higher.
[0058] As specific resins, propylene (methacrylic acid) resins, styrene resins, polycarbonate resins, polyolefin resins, cycloolefin resins, epoxy resins, polyethylene resins, polypropylene resins, ABS resins, polyamide resins, polyacetal resins, and polyethylene terephthalate resins can be used.
[0059] The black masking film 14 contains a black material. The black material can be a colorant, metal particles, or particles containing metal. For example, a black pigment or dye can be used as the colorant. The metal particles or particles containing metal can be selected from at least one of copper, silver, gold, platinum, tin, and alloys thereof.
[0060] After dissolving and dispersing the black material as described above in a solvent, a known additive such as a photopolymerization initiator is added to form a liquid black light-blocking film composition. Then, the black light-blocking film composition is patterned on a lens module using a known method to form the black shielding film 14 as described above. Alternatively, in addition to the patterning described above, a thin film-like black light-blocking film 14 may also be used.
[0061] In addition, the refractive index n of each lens under D-rays (wavelength 589.3 nm) SB For example, it can be 1.20 to 2.50, 1.30 to 2.30, or 1.35 to 2.00.
[0062] The wall thickness (center thickness) (H1, H2, H3) along the optical axis of each lens of L1, L2, and L3 is preferably 1 mm or less, and more preferably 0.5 mm or less. Furthermore, the outer diameter K of each lens is preferably 20 mm or less, and more preferably 10 mm or less.
[0063] <2. Coating liquid for antireflective film> In this embodiment, the coating liquid composition comprising the coating liquid includes at least microparticles, an adhesive precursor (adhesive component), and a solvent. The materials constituting the coating liquid composition will be described below.
[0064] <2-1. Particles> The microparticles (functional microparticles) can be either inorganic or organic. Inorganic microparticles include, for example, oxide microparticles and halide microparticles, especially oxide microparticles. Examples of oxide microparticles include silica microparticles, alumina microparticles, zirconium oxide microparticles, and titanium oxide microparticles. Oxide microparticles can be oxides containing multiple elements, such as aluminosilicate microparticles. Halide microparticles include, for example, chloride microparticles and fluoride microparticles. Examples of fluoride microparticles include magnesium fluoride microparticles and calcium fluoride microparticles. Organic microparticles can also be resin microparticles. Examples of resins contained in resin microparticles include (meth)acrylic resins, styrene resins, and polyurethane resins. However, in the case of membrane applications, such as plasma irradiation (plasma treatment) as described later, it is desirable for the microparticles to be inorganic.
[0065] Hollow microparticles can be used as microparticles, for example. Hollow microparticles are beneficial for achieving a low refractive index in antireflective films. Examples of hollow microparticles include silica hollow microparticles and magnesium fluoride hollow microparticles. Furthermore, microparticles can be those with internal voids, such as microparticles with voids exposed on the outside. Additionally, porous microparticles can also be used.
[0066] The average particle size is, for example, 10–300 nm, 10–200 nm, 10–150 nm, or, depending on the case, within the range of 10–100 nm. The average particle size can also be in the range of 15–100 nm, further within 20–100 nm, or 30–100 nm. The average particle size can also be in the range of 30–80 nm. The average particle size can be determined using a transmission electron microscope or a scanning electron microscope. This determination is performed by averaging the maximum particle size of 50 randomly selected particles. The average particle size described herein is based on the so-called primary particle size.
[0067] The deviation of the particle size is preferably ±20% or less, more preferably ±10% or less. More preferably, the deviation is within ±10% for particles that comprise 80% or more of all particles. The deviation of the average particle size can be measured using a transmission electron microscope or a scanning electron microscope. This measurement can be calculated by dividing the difference between the maximum and minimum particle sizes of any arbitrarily selected 50 particles by the average particle size.
[0068] The refractive index of the particles is less than the refractive index n of the lens. SB For example, the refractive index is 1.10 to 1.40, preferably 1.15 to 1.40, and even more preferably 1.17 to 1.35. Furthermore, the refractive index of the particle is not the refractive index of the material constituting the particle's outer shell, but rather the actual refractive index of the particle, including the effect of the hollow portion 'a'. The refractive index of the particle at a specific wavelength is sometimes well-known, or representative or average values can be obtained based on the approximate spherical size of the particle, the material or thickness of the particle's outer shell, etc., and can be calculated using, for example, the effective medium approximation method of the Bruggemann formula. Here, the refractive index of the particle is used as a representative value; any other refractive index value mentioned in this specification, unless otherwise specified, refers to the refractive index at D-rays (589.3 nm).
[0069] The number of functional microparticles contained in the antireflective film 2 can be set, for example, as follows: 3S / 2R or higher. Here, S is the surface area of the lens to be coated with the coating liquid, and R is the diameter of the particle. Furthermore, the particle diameter R is the average particle size value described above.
[0070] Therefore, as described later, the antireflective film 2 can be formed as a multilayer. To achieve a low refractive index, the microparticles are prone to peeling off. If the microparticles are arranged in a single layer, the optical properties (antireflective function) are impaired when a microparticle peels off. However, by stacking the microparticles in multiple layers, even if one microparticle peels off, the impact on the optical properties can be reduced.
[0071] When the diameter R of the particles is 55±10 nm, the number of particles can be set to... Below 3 S / R. Therefore, after film formation, the particles can be divided into two layers, with a film thickness of 90–130 nm depending on the particle size range. Within this range, an anti-reflection effect can be achieved in the visible light band through optical interference.
[0072] <2-2. Adhesives and their precursors> The adhesive serves to bond the microparticles together, attaching them to a substrate or other underlying structure (in this embodiment, a lens). The adhesive fixes the microparticles within the antireflective film, improving the film's abrasion resistance. The adhesive is added to the coating liquid composition in the form of a precursor. The adhesive may contain, for example, an oxide component, and more specifically, a metal oxide component. The adhesive precursor supplying the metal oxide component can be a metal alkoxide. The metal oxide component is provided by a method called the sol-gel process. For example, silane oxide provides the silica component through hydrolysis and polycondensation. The metal alkoxide is not limited to silane oxide; it may also be aluminum alkoxide, zirconium alkoxide, titanyl alkoxide, niobium alkoxide, tantalum alkoxide, etc. Furthermore, the boiling point of the adhesive precursor (adhesive component) is higher than that of the solvent described later.
[0073] The adhesive may also contain both a metal oxide component and an organic component. The organic component may be derived from a metal alkoxide, and more specifically, from an organic group bonded to the metal atoms constituting the metal alkoxide. That is, the adhesive may be an inorganic-organic composite containing both a metal oxide component and an organic component. An adhesive that is an inorganic-organic composite may, for example, be made from R… 2 n Si(OR 1 ) 4-n The silane oxide supply is shown. Here, R 1 It is an alkyl group having 1 to 4 carbon atoms, R 2 For the organic group that supplies the organic component to the adhesive, n is 1 or 2, particularly 1. R 2 There are no particular restrictions; it can be an aliphatic group, an aromatic group, or it can contain heteroatoms. R 2 It can be a hydrocarbon group with 1 to 10 carbon atoms, particularly an alkyl group with 1 to 10 carbon atoms, and further 1 to 4 carbon atoms. Adhesives called sesquioxanes are supplied from silane oxides (trialkoxysilanes) with n = 1.
[0074] If the adhesive precursor uses Si-OR as the main component as described above, although the detailed principle is unclear, the organic components volatilize after the antireflective film is formed, resulting in less organic content in the film. As a result, lens blurring can be suppressed.
[0075] The binder can be supplied by only one precursor, or by two or more precursors. An example of a combination of two precursors is an alkyltrialkoxysilane and a tetraalkoxysilane. Here, the number of carbon atoms in the alkyl group is not particularly limited; for example, it is 1 to 4 alkyl groups contained in the alkoxy group, and for example, it is 1 to 10 alkyl groups bonded to silicon atoms, particularly 1 to 4. A tetraalkoxysilane corresponds to a compound satisfying n=0 in the above general formula.
[0076] Metal alkoxides, such as silane oxides, can also be included in the coating liquid composition in the form of hydrolysates. The hydrolysates can be partially hydrolyzed. The binder precursor can also be a metal alkoxide or its hydrolysates, particularly alkoxysilanes or their hydrolysates.
[0077] <2-3. Ratio of adhesive precursor to microparticles> All ratios shown below are based on mass. Furthermore, these ratios are calculated based on the composition supplied to the membrane, not the precursor. Therefore, R in the above general formula, for example... 1 Differences will not affect the comparison. The ratio of microparticles to solid components (binder precursor and microparticles) in the coating liquid is preferably 80% or more, more preferably 90% or more, and particularly preferably 95% or more. As a result, the amount of binder between microparticles is reduced, enabling the formation of a flexible antireflective film.
[0078] Furthermore, the total mass ratio of functional microparticles and binder precursors to the coating liquid is preferably 20% or less, more preferably 10% or less. This increases the amount of solvent in the coating liquid, making it easier to create a porous structure in the antireflective film.
[0079] <2-4. Microparticle contact inhibitors> It is desirable to add a microparticle adhesion inhibitor to the coating liquid composition.
[0080] The particle adhesion inhibitor may, for example, have a boiling point of 300°C or higher, and more particularly 400°C or higher. The boiling point of the particle adhesion inhibitor is preferably higher than the curing temperature of the adhesive precursor. The curing temperature of the adhesive precursor is the highest temperature applied in the heating process used to generate the adhesive from the adhesive precursor. Furthermore, the boiling point of the particle adhesion inhibitor is preferably higher than that of the solvent. When the coating liquid composition contains multiple compounds as solvents, the particle adhesion inhibitor may have a boiling point higher than the boiling points of all the compounds contained as solvents. Additionally, as described later, when the coating liquid composition contains a first solvent and a second solvent, and the boiling point of the second solvent is higher than that of the first solvent, the boiling point of the particle adhesion inhibitor may be higher than that of the second solvent.
[0081] The particle adhesion inhibitor can have a viscosity of 1000 mPa·s or higher, 1200 mPa·s or higher, 1400 mPa·s or higher, 1600 mPa·s or higher, and more preferably 1800 mPa·s or higher. When the coating liquid composition contains multiple compounds as solvents, the particle adhesion inhibitor can have a viscosity higher than the combined viscosity of all the compounds contained as solvents. The relatively high viscosity of the particle adhesion inhibitor is particularly useful when coating the coating liquid composition onto curved surfaces. When the coating liquid composition contains a first solvent and a second solvent, and the viscosity of the second solvent is higher than the viscosity of the first solvent, the viscosity of the particle adhesion inhibitor can be higher than the viscosity of the second solvent. Furthermore, the viscosity can be measured at room temperature (25°C) using a vibratory viscometer (e.g., SEKONIC, probe: PR-10L, controller VM-10A). When the particle adhesion inhibitor contains a solvent, the viscosity measurement is performed after removing the solvent.
[0082] Particulate adhesion inhibitors can also be polymers, especially thermoplastic polymers. Particulate adhesion inhibitors can also be dispersants.
[0083] <2-5. Dispersants> It is desirable to add a dispersant selected from at least one of anionic polymeric dispersants and polymeric dispersants to the coating liquid composition. The dispersant can function as a particle adhesion inhibitor. The dispersant can have a boiling point as exemplified with respect to particle adhesion inhibitors. The dispersant can have a viscosity as exemplified with respect to particle adhesion inhibitors.
[0084] Anionic polymeric dispersants possess anionic groups, primarily carboxylate and sulfonate groups. Furthermore, they exhibit a polymeric molecular structure, meaning they contain repeating units. Anionic polymeric dispersants can be homopolymers or copolymers. Ideally, anionic polymeric dispersants should contain anionic groups within their repeating units.
[0085] Examples of anionic polymeric dispersants include polyacrylates, polystyrene sulfonates, styrene-maleic anhydride copolymers, olefin-maleic anhydride copolymers, acrylamide-acrylate copolymers, alginates, and carboxymethyl cellulose salts. Salts may be alkali metal salts such as sodium or potassium salts. Carboxylic acids derived from maleic anhydride may also exist in the form of sodium salts, etc.
[0086] Regarding polymeric dispersants, the average molecular weight is 2000 or higher, and the molecular weight is relatively larger than that of low-molecular-weight dispersants used as general surfactants, effectively acting on microparticles. The molecular weight of polymeric dispersants can also be 3000 or higher, 4000 or higher, 5000 or higher, 6000 or higher, 7000 or higher, 8000 or higher, 9000 or higher, and further, 10000 or higher. There is no particular upper limit to the molecular weight; for example, it can be below 200,000, and further, below 100,000. Polymeric dispersants can be anionic, nonionic, or cationic, with anionic or nonionic dispersants being preferred.
[0087] Examples of anionic polymeric dispersants are the same as those of anionic polymeric dispersants. Examples of nonionic polymeric dispersants include polyvinyl alcohol, polyethylene glycol, and polyacrylamide. Examples of cationic polymeric dispersants include polyethyleneimine and polyvinylimidazoline.
[0088] <2-6. Combination dosage of particulate close contact inhibitors> The amount of the particulate adhesion inhibitor or dispersant relative to the particulate matter, on a mass basis, can be 0.4 or more, 0.5 or more, 2 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, and further, 10 or more. There is no particular upper limit to this ratio, which can be 1000 or less, particularly 100 or less. Examples of this ratio are 4 or more but less than 100, 6 or more but less than 100, 8 or more but less than 100, and further, 10 or more but less than 100.
[0089] Like adhesives, particulate adhesion inhibitors or dispersants can maintain the spacing between particles. When a particulate adhesion inhibitor or dispersant is included, the ratio of the total amount of adhesive to the particulate adhesion inhibitor or dispersant relative to the particles is preferably 0.5 or more. This ratio is also described on a mass basis. This ratio can be 0.8 or more, 1.0 or more, 1.1 or more, 1.2 or more, 1.5 or more, 1.7 or more, and further 1.8 or more. There is no particular upper limit to this ratio; it can be 1000 or less, particularly 100 or less. Examples of this ratio are 0.5 or more but less than 100, and 1.0 or more but less than 100.
[0090] <2-7. Solvent> The solvent can consist of a single type of solvent, but preferably includes two or more solvents with different boiling points. The solvent may contain both an organic solvent, particularly a first solvent and a second solvent, which are polar organic solvents. When two solvents (the first solvent and the second solvent) are mainly used, the boiling point of the first solvent is preferably 60–150°C, more preferably 80–140°C, and particularly preferably 90–130°C. The boiling point of the second solvent is preferably above 150°C, more preferably above 165°C, and particularly preferably above 170°C. The boiling point of the second solvent can be below 280°C. An example of the boiling point of the second solvent is 150–280°C. When a particulate adhesion inhibitor or dispersant is included, the boiling point of the second solvent can be lower than the boiling point of the particulate adhesion inhibitor or dispersant. The difference between the boiling points of the first solvent and the second solvent can be, for example, 50–100°C.
[0091] The first solvent and the second solvent are expressed as a ratio of the second solvent to the first solvent, and are formulated in a manner that, on a mass basis, is less than 1, 0.8 or less, further less than 0.6, and particularly less than 0.4. The lower limit of this ratio can be 0.03 or more, 0.05, and further more than 0.07. For example, the ratio is 0.03 or more and 0.8 or less, 0.05 or more and 0.5 or less, and further more than 0.07 or 0.4 or less. These ratios are suitable for spray coating, particularly for coating liquid compositions applied to curved surfaces by spray coating.
[0092] The first and second solvents can be selected as a combination of solvents with excellent compatibility. Such a combination can be easily achieved, for example, by making both the first and second solvents alkoxy-containing alcohols.
[0093] As will be described later, the boiling point and surface energy of the solvent contained in the coating liquid composition are important during film formation. Since the boiling point of the first solvent is lower than that of the second solvent, it will evaporate before reaching the lens, for example, in the case of film formation by spray coating as described later. On the other hand, since the boiling point of the second solvent is higher than that of the first solvent, it reaches the lens as a droplet when sprayed from the nozzle. The droplets adhering to the lens then diffuse on the lens surface to form a film. In this case, if the surface energy of the second solvent is not high, the diffusion of the liquid will be insufficient, which may lead to defects such as uneven color. Therefore, it can be said that both the boiling point and surface energy of the second solvent are important properties. Specifically, the surface energy of the second solvent is preferably 30 dyne / cm or more, 35 dyne / cm or more, 40 dyne / cm or more, 45 dyne / cm or more, and more preferably 70 dyne / cm or more.
[0094] Solvents with high boiling points can be broadly categorized into: (A) those with larger molecular weights and higher boiling points, and (B) those with smaller molecular weights compared to (A), but stronger hydrogen bonds. Solvents in category (B) have higher surface energy, making them suitable for diffusion of liquids on lens surfaces. Representative solvents in category (A) include butoxyethanol (boiling point 171℃, surface energy 24.8 dyne / cm), while representative solvents in category (B) include propylene glycol 400 (boiling point 188℃, surface energy 71.6 dyne / cm).
[0095] Furthermore, in methods for determining the surface energy of a solvent, any conventional surface energy measurement method can be applied, regardless of its type. For example, it can also be determined by using a lubrication method to horizontally press a platinum ring against the liquid surface and then directly pulling it upwards. The force that balances the surface tension acting on the ring at the instant the platinum ring is about to detach from the liquid surface is then measured using a scale.
[0096] <2-8. Other ingredients> The coating liquid composition may further include tackifiers, thixotropic agents, surfactants, crosslinking agents, leveling agents, etc. Leveling agents improve the wettability of microparticles. The coating liquid composition may further include leveling agents. The leveling agent is preferably a low molecular weight surfactant, specifically an average molecular weight less than 2000.
[0097] <3. Anti-reflective film> Figure 2 This is a cross-sectional view of the anti-reflective coating stacked on the lens. For example... Figure 2 As shown, the antireflective film 2 is an example of a film disposed on the substrate 3 (each of the aforementioned lenses). The antireflective film 2 is formed of two layers of microparticles 21 fixed together by an adhesive 31. Furthermore, both the microparticles 21 and the substrate 3 are fixed together by the adhesive 31.
[0098] As described above, in the coating liquid of this embodiment, the mass of the solid component is relatively small compared to the solvent, and the mass of the binder is relatively small compared to the particles, thus enabling the antireflective film 2 to have a porous structure. For example, a porosity of 50% or more is preferably preferred for this porous structure.
[0099] The antireflective coating 2 has a refractive index n of 1.10 to 1.35. L1 And a thickness of 80nm to 150nm t L1 Based on this configuration, the anti-reflective film 2 can achieve high anti-reflective performance. Refractive index n L1 This is the refractive index under D-rays (wavelength 589.3 nm). Additionally, Figure 2 For ease of explanation, substrate 3 is described as flat, but it is actually a lens with a curved surface.
[0100] Regarding the antireflective film 2, for example, in the reflection spectrum that represents the wavelength of light with wavelengths from 300 nm to 1200 nm incident at an incident angle of 5°, and the reflectivity relative to that wavelength, the minimum reflectivity r in the range of 300 nm to 1200 nm is... min 300-1200 It can be below 1%. Reflectivity r min 300-1200 Ideally, it should be below 0.5%, and even more ideally below 0.2%. Unless otherwise specified, the reflectivity of antireflective films, etc., shall be set as the reflectivity calculated based on the reflection spectrum when light with wavelengths of 300 nm to 1200 nm is incident at an angle of 5°.
[0101] In antireflective film 2, the minimum reflectivity r in the wavelength range of 400nm to 800nm is... min 400-800 It is not limited to a specific value. Reflectivity r min 400-800 For example, below 0.5%. In this case, antireflective film 2 is more likely to achieve higher antireflective performance. Reflectivity r min 400-800 We hope it will be below 0.2%.
[0102] Regarding antireflective film 2, its reflectivity is below 2.5% in the wavelength range of 300nm to 1200nm. range / 2.5 It is not limited to a specific value. The range is λ. range / 2.5 For example, a wavelength of 400 nm or higher. Therefore, the anti-reflective coating 2 can more easily achieve higher anti-reflective performance. Range λ range / 2.5 It can be 450nm or higher, or 500nm or higher. Unless otherwise specified, the wavelength and wavelength range corresponding to the specified reflectance are also set as the wavelengths determined from the reflection spectrum.
[0103] Regarding antireflective film 2, its reflectivity is below 1.0% in the wavelength range of 300nm to 1200nm. range / 1.0 It is not limited to a specific value. The range is λ. range / 1.0 For example, a wavelength of 250 nm or higher. Therefore, the anti-reflective coating 2 can more easily achieve higher anti-reflective performance. Range λ range / 1.0 It can be 300nm or above, 350nm or above, or 400nm or above.
[0104] When the refractive index n of the substrate (lens) is... sb When the refractive index of the antireflective coating is n1, consider adjusting the optical thickness of the antireflective coating to 1 / 4 of the specified wavelength λ. In this case, n sb -n1 2The smaller the absolute value of the refractive index, the smaller the reflectivity at the wavelength λ corresponding to that refractive index. Therefore, from the viewpoint of reducing reflectivity, it is sometimes desirable for the antireflective film 2 to have a substantially low refractive index. In cases where a low refractive index is required for the antireflective film, it is advantageous for the antireflective film to contain hollow microparticles.
[0105] Figure 2 In the example, the substrate (lens) 3 is in direct contact with the antireflective film 2, but this is not a limitation; other films may be interposed between the substrate 3 and the antireflective film 2. Examples of other films include polyvinyl butyral resin (PVB). Furthermore, although the surface of the antireflective film 2 is exposed, this is not a limitation; the surface of the antireflective film 2 may also be covered by other layers.
[0106] Furthermore, when R is set as the diameter of the particles and r is set as the cross-sectional diameter of the adhesive, it is preferable that R > 5r (refer to...). Figure 2 Therefore, the amount of adhesive is reduced, thus enabling the antireflective film to have a porous structure. Furthermore, the cross-sectional diameter r of the adhesive is shown in the schematic diagram. Figure 2 As shown, when observing the cross-section of the membrane using a transmission electron microscope or a scanning electron microscope, the thickness can also be determined by measuring the maximum thickness of the portion where the particles are connected to each other. Alternatively, the thickness of the portions where identifiable particles are connected to each other can be measured within the field of view, and their average value can be set as the value of r.
[0107] Furthermore, the arrangement of particles in layers 21 and 22 is not particularly limited; for example, it can be set to a densest square filling. This allows the porosity to reach over 50%.
[0108] <4. Methods for forming anti-reflective coatings> The coating liquid composition of this embodiment can be used in various coating processes, but is particularly suitable for coating by spray coating. Spray coating is a known coating process in which the coating liquid composition is sprayed from a spray nozzle. In this embodiment, the lens being studied is small, and it is impossible to uniformly coat the coating liquid composition by methods such as spin coating; therefore, spray coating is suitable.
[0109] Compared to optical films formed through other coating processes, antireflective films formed by spray coating with a coating liquid composition containing microparticles, binder precursors, and solvents are more prone to micro-defects. One possible reason is the adhesion of microparticle aggregates. By using the aforementioned coating liquid composition, the generation of micro-defects is reduced, and in some cases, eliminated. Spray coating itself is a coating method with excellent mass production capabilities and can handle curved surfaces; it is also a coating process that allows for continuous film deposition on multiple substrates.
[0110] First, as described above, a black light-shielding film 14 is formed on the substrate 3. Next, after coating the substrate 3 with the coating liquid composition, it is fired, whereby the solvent evaporates, and an adhesive is generated from the adhesive precursor, forming an anti-reflective film. The firing temperature is below the boiling point of the solvent, for example, it can be set to 85–110°C, and the firing time can be set to, for example, 5–400 minutes. Since the lens of this embodiment is made of resin, the firing temperature cannot be high; therefore, it is set within the temperature range described above.
[0111] As described above, when the coating liquid composition contains the first solvent and the second solvent, the unevenness of the thickness of the formed antireflective film can be reduced when the coating liquid composition is applied to the substrate 3 by spray coating, but the detailed principle is unclear.
[0112] Furthermore, after the coating liquid composition is applied to the substrate, it gradually diffuses on the curved substrate 3 under the action of the second solvent. Subsequently, the second solvent evaporates during the firing process. Additionally, the adhesive can be made to hardly evaporate during the firing process. That is, if the metal alkoxide, as an adhesive precursor, is contained in the form of a hydrolysate, the adhesive precursor contained in the coating liquid composition can hardly evaporate during the firing process. Therefore, the controllability of the antireflective film formation is increased.
[0113] Alternatively, at least a portion of the particulate adhesion inhibitors or dispersants contained in the formed antireflective film can be removed subsequently. Specifically, the removal of particulate adhesion inhibitors or dispersants can be carried out through various treatments of the antireflective film. Examples of such treatments include plasma treatment, corona treatment, UV cleaning, high-temperature treatment, organic cleaning, acid cleaning, and alkaline cleaning. Plasma treatment can be carried out by irradiating oxidizing active species, such as oxygen plasma.
[0114] There are various methods for spray coating; one example is shown below. Figure 4 This is a cross-sectional view showing an example of a spray nozzle used for spray coating. For example... Figure 4 As shown, the spray nozzle has a receiving portion 91 for receiving the coating liquid composition, and an annular liquid flow path 93 extending from the receiving portion 91 toward the nozzle outlet 92. An air vortex (not shown) is provided in the liquid flow path 93 for causing the coating liquid composition to swirl within the liquid flow path 93. Therefore, the coating liquid composition sprayed from the outlet 92 through the liquid flow path 93 is sprayed downwards while swirling.
[0115] Additionally, an annular airflow path 94 extending toward the nozzle outlet 92 is formed on the outer side of the receiving section 91 and the liquid flow path 93. An air vortex (not shown) is provided in this airflow path 94 to cause the coating liquid composition to swirl within it. As a result, the air flowing through the airflow path 94 becomes a swirling flow, converging with the liquid flow path 93 from the outside near the outlet 92. Consequently, the coating liquid composition is pressed against the outside of the liquid flow path 93 by the swirling airflow, forming a thinner film that reaches the outlet 92. Then, the coating liquid composition is sprayed downwards while swirling from the outlet 92. The coating liquid composition sprayed from the outlet 92 through the airflow path 94 increases in outer diameter as it swirls downwards, coating the lens to be coated. For example, a nozzle manufactured by SHIMADA APPLI can be used as such a nozzle.
[0116] The distance from the nozzle outlet 92 of the spray nozzle 9 configured as described above to the lens to which the coating is to be applied is preferably 25 mm or more and 35 mm or less. Furthermore, the spray volume of the coating liquid composition per unit time is preferably 0.1 ml / min or more and 0.3 ml / min or less. Alternatively, the spray volume per unit time can be determined by collecting liquid sprayed from the spray nozzle over one minute and measuring its volume.
[0117] like Figure 4 As shown, in region N1, for example, which is 25-35 mm from the nozzle 92, the swirling flow of the coating liquid composition is stronger due to its proximity to the nozzle 92. Therefore, droplets forming the mist within the swirling flow are driven inwards by the swirling flow. Additionally, droplets flowing out to the outer side of the swirling flow are propelled further outwards by the swirling flow. That is, the propelled droplets do not adhere to the lens. Furthermore, droplets adhering to the lens diffuse into a film on the lens surface. Therefore, if a lens is positioned in region N1 and the coating liquid composition is applied, a suitable coating film can be formed.
[0118] On the other hand, the region N2, located 45-55 mm from the nozzle 92, has a weaker swirling flow of the coating liquid composition due to its distance from the nozzle 92. Therefore, it does not obstruct the flow of droplets forming the mist within the swirling flow to the outside of the swirling flow. Furthermore, droplets flowing to the outside of the swirling flow do not splash significantly further outward due to the weaker swirling flow, and may adhere to the lens. Therefore, if a lens is placed in this region N2 and the coating liquid composition is applied, uncontrolled droplets may adhere to the lens as splatter marks, potentially resulting in a defective product. Preferably, the number of such splatter marks (defects) is 5 or less.
[0119] like Figure 5As shown, when spray coating is applied to lens L, multiple lenses L (e.g., with a diameter of 5-20 mm) are arranged in a grid pattern on a mounting surface (e.g., a stage or tray) with a front-to-back and left-to-right spacing of 5-30 mm. The spray nozzle 9 moves sequentially over each lens to apply the coating. That is, the coating liquid composition is continuously applied to multiple lenses L. Therefore, there is a risk of problems arising, particularly when the height of the spray nozzle 9 is outside the aforementioned range or when the coating amount is small. Furthermore, the spacing or arrangement of the lenses L is not dominant compared to the appropriate height of the spray nozzle 9 and the coating amount; therefore, the arrangement is arbitrary and may not be grid-like. That is, taking the lens diameter or spacing as an example, the inventors have confirmed that as long as it is at least within this range, appropriate film formation can be achieved within the preferred range of the spray nozzle outlet height or spray amount.
[0120] (a) When the coating liquid composition has an appropriate coating amount and the spray nozzle is at a relatively high height (e.g., when the distance between the spray nozzle 9 and the lens L is 35 mm or more). In this case, the coating area of the coating liquid composition sprayed from the spray nozzle 9 becomes larger. Therefore, if the coating liquid composition is continuously applied to multiple lenses L, droplets of the coating liquid composition may sometimes adhere to the lenses L before coating. When these adhered droplets dry, they become splatter marks, and because the coating liquid composition is applied to them, the finished lenses L exhibit uneven discoloration, such as uneven color distribution. Similarly, if droplets adhere to the lenses L after coating, the same discoloration occurs.
[0121] However, if the height of the spray nozzle 9 is further increased to 60mm or more, the solvent evaporates more easily. Therefore, less liquid reaches the lens, and less flows to the center of the concave surface. As a result, although scattering marks are observed, uneven coloring is less likely to occur.
[0122] To prevent this discoloration, the following countermeasures can be taken.
[0123] (1) If a certain amount of particle adhesion inhibitor is added to the coating liquid composition in advance, it will prevent drying and reduce uneven discoloration even if a portion of the liquid composition is attached to the surface of the lens L before coating.
[0124] (2) The distance between the spray nozzle 92 and the lens L is set to the above-mentioned appropriate distance, thereby reducing the uneven color distribution.
[0125] (b) When the coating liquid composition has an appropriate coating amount and the spray nozzle height is low (e.g., when the distance between the spray nozzle 9 and the lens L is less than 25 mm). In this case, the film thickness of the coating liquid composition applied to lens L may become thicker. The reason is as follows.
[0126] (1) Because the distance between the spray nozzle 9 and the lens L is small, the coating area of the coating liquid composition becomes narrower. If the area of the coating area is small when the spray volume is constant, the film thickness will be thicker immediately after coating (after the coating liquid composition has just adhered to the lens L).
[0127] (2) Because the distance between the spray nozzle 9 and the lens L is small, the solvent contained in the coating liquid composition does not evaporate sufficiently. As a result, the film thickness becomes thicker immediately after coating.
[0128] Especially due to the curvature of the substrate such as the lens, in cases where, for example, a coating liquid composition is applied to the concave surface of the lens L, such as... Figure 6 As shown, the excess coating flows towards the bottom of the concave surface before drying, posing a risk of unacceptable deviations in film thickness. This may result in unsatisfactory refractive index or reflective properties, and also risks causing aesthetic problems, such as uneven color due to inconsistencies in the reflected hue. On the other hand, when the convex surface of lens L is coated with the coating liquid composition, the excess coating flows towards the periphery of the convex surface before drying, posing a risk of unacceptable deviations in film thickness. In (a) above, this phenomenon may occur when the coating liquid composition is applied in large quantities.
[0129] (c) Cases where the coating liquid composition has a low coating amount (e.g., coating amount less than 0.1 ml / min). In this case, the nozzle structure cannot control the ejection of a small amount of liquid, thus making coating impossible.
[0130] Furthermore, when the spray nozzle 9 is at a relatively high height with less adhesive, the antireflective film formed on the lens L becomes defective because the droplets of the coating liquid composition scatter around. On the other hand, to solve this technical problem, it is desirable to add a particulate aggregation inhibitor (a dispersant selected from at least one of anionic polymeric dispersants and polymeric dispersants). However, by rationalizing the height of the spray nozzle 9, a defect-free film can be produced even without adding the aforementioned aggregation inhibitor.
[0131] <5. Characteristics> The coating liquid according to this embodiment can achieve the following effects.
[0132] (1) Because it contains hollow microparticles with pores, it can form a porous antireflective film. As a result, a lower refractive index can be achieved.
[0133] (2) Because the ratio of microparticles to solid components (adhesive precursor and microparticles) in the coating liquid is low, the amount of adhesive between microparticles 21 is reduced, which can form a soft antireflective film. Therefore, even if the film is formed on a material with a large coefficient of thermal expansion, such as a resin lens, the antireflective film is not prone to cracking before and after the heat resistance test.
[0134] (3) Since the total mass of the microparticles and the binder precursor is relatively low relative to the mass of the coating liquid, the amount of solvent in the coating liquid increases. As a result, the antireflective film 2 is more likely to have a porous structure. That is, it is easier to form voids between adjacent microparticles, thus achieving a low refractive index.
[0135] <6. Examples of Variation> The present invention has been described above as one embodiment, but the present invention is not limited to the above embodiment, and various modifications can be made without departing from its spirit. In addition, the following variations can be appropriately combined.
[0136] (1) The lens unit of the antireflective film to be laminated in this invention is not particularly limited. Figure 1 This is just one example. That is, the lens unit targeted by this invention can be any lens unit formed by overlapping multiple resin lenses with an outer diameter of 20mm or less. Furthermore, the shape and number of each lens, and the form of the black light-blocking film, are not particularly limited and can be appropriately configured according to requirements. For example, it can be configured such that at least one curved surface constituting each lens has at least one inflection point.
[0137] (2) The antireflective film can also be constructed in multiple layers. For example, such as Figure 3 As shown, a second antireflective film 4 may also be provided between the aforementioned antireflective film (hereinafter referred to as the first antireflective film 2) and the substrate (lens) 3. The second antireflective film 4 has a plurality of hollow microparticles 21 dispersed inside the layer formed by the adhesive 41.
[0138] The refractive index of the second antireflective film 4 is greater than that of the first antireflective film 2, for example, it can be set to 1.30 to 1.25. In addition, the thickness of the second antireflective film 4 can be set to 5 nm to 150 nm, for example.
[0139] The hollow microparticles 21 and the adhesive 41 can be made of the same materials as those used in the first antireflective film 2. However, the second antireflective film 4 has fewer hollow microparticles 21 than the first antireflective film 2. As a result, the refractive index of the second antireflective film 4 can be higher than that of the first antireflective film 2.
[0140] To form the reflective film as described above, firstly, a second antireflective film 4 is formed on the substrate 3, and then a first antireflective film 2 is formed. The second antireflective film 4 can also be formed by spray coating in the same way as the first antireflective film 2.
[0141] (3) Figure 3 In the example, the antireflective film is formed as two layers, but it can also be like... Figure 7 The structure shown is formed in three or more layers. Figure 7 In the example, a five-layer antireflective film is formed. Hereinafter, these will sometimes be referred to as antireflective films 2, 5, 6, 7, and 8, from 1st to 5th. In the second antireflective film 5, approximately one layer of hollow microparticles 21 are bonded together by adhesive 31, similar to the first antireflective film 2. However, the number of hollow microparticles 21 is less than that in the first antireflective film 2. In the third antireflective film 6, a plurality of hollow microparticles 21 are dispersed in the layer formed by adhesive 61. The number of hollow microparticles 21 is less than that in the second antireflective film. Furthermore, voids 62 are also formed in the third antireflective film 6.
[0142] In the fourth antireflective film 7, a plurality of hollow microparticles 21 are dispersed in the layer formed by the adhesive 61. The number of hollow microparticles 21 is less than that in the third antireflective film 6. The fifth antireflective film 8 is a layer formed by the adhesive 71 and does not contain hollow microparticles.
[0143] As described above, the number of hollow particles contained in the antireflective film gradually decreases from the first antireflective film 2 to the fifth antireflective film. Consequently, the refractive index gradually increases from the first antireflective film 2 to the fifth antireflective film. More specifically, in this variation, it is preferable that the first antireflective film 2 is close to the refractive index of air, and the fifth antireflective film 8 is close to the refractive index of a lens.
[0144] The adhesives and hollow microparticles contained in each layer can be formed from the same materials as those contained in the first antireflective film 2. In addition, in order to form the above-mentioned antireflective film, the antireflective film can be formed on the substrate (lens) first by spray coating or the like in the order of the 5th, 4th, 3rd, 2nd and 1st layers.
[0145] If so Figure 3 and Figure 7 As shown, forming multiple anti-reflective films can improve anti-reflective performance.
[0146] Example The coating liquid and antireflective film of embodiments of the present invention will be described below. However, the present invention is not limited to the following embodiments.
[0147] (Formation of anti-reflective coating) A binder mixture was prepared by mixing tetraethoxysilane (TEOS), methyltriethoxysilane (MTES), and 0.3% formic acid in a mass ratio of 8.7:3.7:7.6. This mixture was then combined with microparticles, a dispersant, a leveling agent, a low-boiling-point solvent, and a high-boiling-point solvent to obtain the coating liquid compositions of Examples 1-7, as shown in Table 1. Table 2 shows the ratio of solid components in the coating liquid compositions and the ratio of microparticles to solid components. Solid components refer to the total mass of the binder mixture and the microparticles.
[0148] Next, the coating liquid composition is applied to the lens surface by spray coating. Then, the glass plate coated with the coating liquid composition is allowed to air dry for 10 minutes, followed by heating in an oven set to 85°C for 10 minutes to obtain the antireflective film. The thickness of the formed antireflective film is in the range of 50 nm to 350 nm.
[0149] The lenses are formed from cycloolefin resins (refractive index = 1.530 at the wavelength of D-rays (wavelength 589.3 nm), and are convex lenses with an outer diameter of 13 mm, a thickness of 0.5 mm, and an angle of 50 degrees near the outer periphery. Here, 100 lenses are arranged in a grid pattern with a spacing of 13 mm.
[0150] The raw materials used are as described below.
[0151] (i) Microparticles: Hollow silica microparticles, Balloon SIL (registered trademark) nanoparticles (Toyota Chemical Corporation, average particle size 55nm) (ii) Adhesive precursors: tetraethoxysilane (TEOS), methyltriethoxysilane (MTES), and tetraethyl orthosilicate in 0.3% aqueous solution (manufactured by Tama Chemical Industry Co., Ltd.) (iii) Particulate contact inhibitors (dispersants): • Styrene-maleic anhydride copolymer BYK-2013 (manufactured by BYK) ·2-Propanol (Kanto Chemical Manufacturing Premium Grade) Boiling point 82℃, surface energy 20.8 dyne / cm Methanol has a boiling point of 64℃ and a surface energy of 22.6 dyne / cm². • Acrylic copolymer Flowlen DOPA-35 (manufactured by Kyoeisha Chemicals) (iv) Low-boiling-point solvent (first solvent): 1M2P (1-methoxy-2-propanol), boiling point 120°C, surface energy 25.6 dyne / cm (manufactured by Tokyo Chemical Industry Co., Ltd.) (v-1) High-boiling-point solvents (second solvent): (represented as PG in the table) Propylene glycol 400 (manufactured by Fujifilm and Kogaku), boiling point 188°C, surface energy 71.6 dyne / cm (v-2) High-boiling-point solvent (second solvent): (represented by BE in the table) Butoxyethanol (manufactured by Fujifilm and Kohden Chemical Co., Ltd.) (boiling point 171°C, surface energy 24.8 dyne / cm) (vi) Leveling agent: polyether modified silicone, KP-341 (manufactured by Shin-Etsu Silicones) KP-341 (polyether-modified silicone) is a surfactant suitable as a leveling agent, with an average molecular weight of less than 2000.
[0152] [Table 1] (Unit: g) [Table 2] (Determination of refractive index) The refractive index was measured using an Olympus-manufactured USPM to determine the spectral reflectance in the visible light region of the film. Based on this spectral reflectance data, the film structure was simulated and fitted using optical film design software (TFCalc, manufactured by Hulinks Co., Ltd.), thereby obtaining the refractive index at the wavelength of D-rays (wavelength 589.3 nm). The refractive index of the antireflective films formed in Examples 1 to 7 was 1.16. Therefore, through these examples, it can be seen that a low-refractive-index antireflective film can be formed.
[0153] The cross-section of the antireflective film of Example 1 was observed using SEM, and the results obtained... Figure 8 .like Figure 5 As shown, regarding this antireflective film, when the microparticles are stacked into two layers, multiple voids were observed.
[0154] (A study on the conditions of the nozzle) The application of the coating liquid compositions of Examples 1 and 5 above onto lenses using the spray nozzles manufactured by SHIMAZU APPLI was investigated. A 7mm diameter lens made of cyclic olefin resin (refractive index = 1.530 at the wavelength of D-rays (wavelength 589.3nm)) was used as the coating target, and the coating liquid composition was applied to the concave surface of the lens. Furthermore, as described above, 100 lenses were arranged in a grid pattern with 13mm intervals, and the coating liquid composition was continuously applied. The following conditions (A to D) were set for the nozzle.
[0155] A: Nozzle height 60mm, spray volume 0.2ml / min; B: Nozzle height 30mm, spray volume 0.2ml / min; C: Nozzle height 10mm, spray volume 0.2ml / min; D: Nozzle height 30mm, spray volume 0.4ml / min.
[0156] The volume of liquid ejected per unit time is determined by collecting liquid ejected from the spray nozzle for 1 minute using the same method and conditions, and measuring its volume.
[0157] Then, according to the above conditions, the coating liquid composition was applied to the lens from the spray nozzle, and the appearance of each lens after drying was checked. In addition, the refractive index of each lens was measured. The appearance of the lenses was evaluated as follows.
[0158] (i) Defect In Examples 1 and 5, the number of defects (the number of fly-off marks mentioned above) was determined. The number of defects was determined by visually inspecting the obtained images using a laser microscope (OPTELICS HYBRID L7) manufactured by Lasertec Co., Ltd. at 20x magnification and counting the defects. The evaluation is as follows.
[0159] ◎5 or less; ○ Less than 20; △ Less than 50; More than 50.
[0160] (ii) Uneven color ◎The reflected color tone is uniform (there are no discoloration areas larger than φ0.1mm); △ The reflected color tone is uneven (there are discoloration areas larger than φ0.1mm).
[0161] The results are shown in Table 3. Under condition A, the spray nozzle height was very high, thus producing defects caused by splatter marks as described above. However, due to the easy evaporation of the solvent, the amount of liquid reaching the lens was reduced, and the color unevenness was reduced. Under condition C, almost no defects were observed, but the aforementioned film unevenness was produced, and a small amount of color unevenness was observed. Under condition D, the spray nozzle height was appropriate, but the spray volume was relatively large, thus producing film unevenness, and a small amount of color unevenness was observed.
[0162] On the other hand, under condition B, with appropriate nozzle height and spray volume, no defects or color unevenness were observed in Examples 1 and 5, and good film formation was achieved. Furthermore, while the solid content in the coating liquid composition differed in Examples 1 and 5, no difference was observed in this experiment. However, in Example 8, due to the use of a second solvent with a lower surface energy than in Examples 1 and 5, droplet diffusion was worse than in Examples 1 and 5, resulting in uneven and non-uniform color.
[0163] [Table 3] Symbol Explanation 2: Anti-reflective film; 21: Microparticles; 31: Adhesive.
Claims
1. A coating liquid for forming at least one antireflective film on a lens unit comprising a plurality of resin lenses, the coating liquid being characterized in that: The lens has an outer diameter of less than 20 mm. The coating liquid contains: Multiple functional microparticles having a refractive index lower than that of each of the lenses; An adhesive component, which is an adhesive precursor, is capable of fixing the functional microparticles to each other in the antireflective film and of fixing the antireflective film to the lens; and At least one first solvent having a boiling point lower than that of the adhesive component.
2. The coating liquid as described in claim 1, characterized in that: The lens unit comprises a lens having a center thickness of less than 1 mm.
3. The coating liquid as described in claim 1, characterized in that: The lens unit is built into the portable device.
4. The coating liquid as described in claim 1, characterized in that: The lens unit includes the following lenses. The lens has at least one surface comprising an axisymmetric concave surface and a convex surface.
5. The coating liquid as described in claim 1, characterized in that: The first solvent comprises a solvent having a boiling point of 60°C or higher and 140°C or lower.
6. The coating liquid as described in claim 5, characterized in that: It also contains a second solvent. The second solvent has a boiling point above 150°C and a surface energy of more than 30 dyne / cm.
7. The coating liquid as described in claim 1, characterized in that: The functional microparticles account for more than 80% of the total mass of the functional microparticles and the adhesive components.
8. The coating liquid as described in claim 1, characterized in that: The particle size deviation of the functional microparticles is within ±20%.
9. The coating liquid as described in claim 1, characterized in that: The total mass ratio of the functional microparticles and the adhesive components relative to the coating liquid is less than 20%.
10. The coating liquid as described in claim 1, characterized in that: The number of the functional microparticles is [number] when the film is formed on the lens. 3S / 2R and above, Wherein, S is the surface area of the lens to be coated with the coating liquid, and R is the diameter of the functional microparticles.
11. The coating liquid as described in claim 10, characterized in that: R is 55±10nm. The number of the functional microparticles is Below 3S / R.
12. The coating liquid as described in claim 1, characterized in that: The adhesive component uses a composition having Si-OR as the main component, wherein R represents an alkyl group having 1 to 4 carbon atoms.
13. The coating liquid as described in claim 1, characterized in that: The solvent comprises a first solvent and a second solvent. The boiling point of the second solvent is higher than that of the first solvent.
14. An anti-reflective film, characterized in that: It is formed by applying the coating liquid of claim 1 to each of the lenses and then firing them at a temperature below the boiling point of the solvent.
15. The antireflective film as described in claim 14, characterized in that: R > 5r, where R is the diameter of the functional microparticles and r is the cross-sectional diameter of the adhesive.
16. The antireflective film as described in claim 14, characterized in that: The functional microparticles are stacked on the lens in a square-dense packing manner.
17. The antireflective film as described in claim 14, characterized in that: The refractive index is below 1.
16.
18. An anti-reflective film, characterized in that: Formed using the coating liquid according to claim 1 or 2, wherein the refractive index n is 1.16 or less.
19. An anti-reflective film, characterized in that: The functional microparticles are formed using the coating liquid of claim 1 or 2 and, when fired at a temperature below the boiling point of the solvent, are stacked in two layers.
20. A method for manufacturing a lens, characterized in that, include: The step of applying a coating liquid to the surface of the lens substrate, the coating liquid comprising: a plurality of functional microparticles having a refractive index lower than that of the lens substrate, an adhesive component capable of binding the functional microparticles and serving as an adhesive precursor, and a first solvent having a boiling point lower than that of the adhesive component; and The step of heating the coating liquid to form an antireflective film.
21. The method for manufacturing a lens as described in claim 20, characterized in that: The lens substrate has at least one surface comprising an axisymmetric concave surface and a convex surface.
22. The method for manufacturing a lens as described in claim 20, characterized in that: The coating liquid also contains a second solvent having a boiling point higher than that of the first solvent.
23. The method for manufacturing a lens as described in claim 20, characterized in that: The coating liquid further comprises at least one selected from particle adhesion inhibitors and dispersants.
24. The method for manufacturing a lens as described in claim 23, characterized in that: It also includes the step of treating the formed antireflective film with at least one of plasma treatment, corona treatment, UV cleaning, high temperature treatment, organic cleaning, acid cleaning and alkaline cleaning.
Citation Information
Patent Citations
Silica-based microparticle, method for producing dispersion with the same, and base material with coating film
JP2001233611A
Antireflection film
JP2001350001A
Antireflection laminate and method for producing the same
JP2007272132A