Disk substrate

By optimizing the shape of the outer periphery of the disk substrate and controlling the position and size of the recesses and protrusions, the problem of magnetic head collision failure was solved, and the magnetic recording area was expanded and the stability was improved.

CN123125646APending Publication Date: 2026-11-17HOYA CORPORATION +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580028933.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-29
Filing Date
2025-04-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, the unevenness of the outer peripheral edge of the disk substrate is confined to an extremely narrow area when expanding the magnetic recording area, which increases the risk of magnetic head collision failure and limits the expansion of the magnetic recording area.

Method used

By controlling the shape of the outer peripheral edge of the disk substrate, ensuring that the maximum depression point is below 0.90R and the fitted circle radius is above 80μm, and controlling the radial distance of the maximum protrusion point and the fitted circle radius, the steepness of the depression and the magnetic recording area are reduced.

Benefits of technology

It effectively reduces the risk of magnetic head collision failure, improves the stability and read/write performance of the magnetic head during seek operations, and expands the magnetic recording area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125646A_ABST
    Figure CN123125646A_ABST
Patent Text Reader

Abstract

A disk substrate capable of expanding the magnetic recording area is provided. The disk substrate 1 includes annular main surfaces 11a and 11b and an outer peripheral edge surface 12. In a cross-section taken along the radial and thickness directions of the disk substrate 1, the main surface 11a has a protrusion CV extending upward in the thickness direction and a recess CC located radially inward relative to the protrusion CV and extending downward in the thickness direction. The radial distance from the center C to the maximum recess point CC1 is less than 0.90R, and at the maximum recess point CC1, the recess depth of the recess CC is the largest in the downward direction in the thickness direction, where R represents the radius of the disk substrate 1.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to a magnetic disk substrate for a magnetic recording medium. BACKGROUND

[0002] In recent years, a glass substrate and an aluminum alloy substrate have been used as a magnetic disk substrate for an HDD. A manufacturing process of a glass magnetic disk substrate, for example, includes a main surface polishing process performed on a main surface of a glass plate cut into a ring shape. In the main surface polishing process, the front and back main surfaces of the ring-shaped glass plate are pressed to be sandwiched between polishing pads, and the ring-shaped glass plate and the polishing pads are moved relative to each other while a polishing liquid containing a polishing abrasive is supplied, thereby polishing the main surfaces. At this time, on a portion of the main surface near an outer peripheral edge surface (hereinafter also referred to as an "outer peripheral edge portion"), a protrusion called a skijump (a state in which the portion of the main surface near the outer peripheral edge surface protrudes outward in a thickness direction of the glass plate with respect to other portions of the main surface) or a depression called a roll-off (a state in which the portion of the main surface near the outer peripheral edge surface is recessed inward in the thickness direction of the glass plate with respect to other portions of the main surface) can be generated. In addition, with respect to the protrusion, a recess can be generated on an inner side in the radial direction.

[0003] On the other hand, in recent years, with an increase in storage capacity and a demand for higher recording density of each magnetic recording medium (magnetic disk) 1, a flying height of a magnetic head with respect to a magnetic recording layer of the magnetic recording medium has been reduced. That is, a distance between the magnetic recording layer of the magnetic recording medium and a recording / reproducing element of the magnetic head has been shortened. In this case, when the protrusion is present on the main surface of the glass substrate, a head crash failure can occur in which, for example, the magnetic head with the reduced flying height collides with the protrusion.

[0004] For this reason, in recent years, in the outer peripheral edge portion of the main surface, the protrusion height and the depression depth are reduced, and the protrusion and the depression are shifted to an outside of a magnetic recording area, thereby expanding and flattening the magnetic recording area (see Patent Literature 1).

[0005] LIST OF CITATIONS

[0006] PATENT LITERATURE

[0007] [Patent Literature 1]: JP 2010-073289 A SUMMARY

[0008] PROBLEMS TO BE SOLVED BY THE INVENTION

[0009] However, when unevenness, such as protrusions and depressions, is shifted as far outward as possible on the main surface to expand the magnetic recording area, the unevenness is confined to a very narrow region at the outer peripheral edge of the main surface, and it has been found that steep unevenness forms at the outer peripheral edge of the main surface. In this case, due to the risk of head collision failures, the portion of the outer peripheral edge of the main surface where such unevenness occurs cannot be used as a magnetic recording area, thus limiting the expansion of the magnetic recording area.

[0010] The present invention was made in view of the above-mentioned problems, and its object is to provide a disk substrate capable of expanding the magnetic recording area.

[0011] Technical solution

[0012] According to one aspect of the present invention, a disk substrate is provided, comprising: A pair of annular main surfaces; and outer peripheral edge surface, In a cross-section taken along the radial and thickness directions of the substrate, at least one of the pair of main surfaces has a protrusion extending upward in the thickness direction and a recess located radially inward relative to the protrusion and extending downward in the thickness direction. The radial distance from the center of the substrate to the maximum depression point is less than 0.90R. At the maximum depression point, the depression depth of the depression in the downward direction of the thickness direction is the largest, where R represents the radius of the substrate.

[0013] In a disk substrate according to one aspect of the present invention, the radius of the fitted circle based on the maximum depression point can be 80 m or more.

[0014] In a disk substrate according to one aspect of the present invention, the absolute value of the radial distance between the maximum depression point and the center of the fitted circle based on the maximum depression point can be less than 1.00 mm.

[0015] In a disk substrate according to one aspect of the present invention, the radial distance from the center of the substrate to the maximum protrusion point can be less than 0.98R, at which the protrusion height in the upward direction of the thickness direction is the maximum.

[0016] In a disk substrate according to one aspect of the present invention, the radius of the fitted circle based on the maximum protrusion point can be 15 m or more.

[0017] Beneficial effects of the present invention

[0018] According to the present invention, a magnetic disk substrate capable of expanding the magnetic recording area can be provided. Attached Figure Description

[0019] [ Figure 1 (a) is a perspective view showing an example of a disk substrate according to this embodiment. Figure 1 (b) is a diagram showing an example of the cross-sectional shape of the outer peripheral edge surface of the disk substrate according to this embodiment, and [ Figure 1 (c) is a diagram showing an example of the cross-sectional shape of the inner peripheral edge surface of the disk substrate according to this embodiment.

[0020] [ Figure 2 [Illustration] is a diagram showing a recess and a protrusion on a main surface of a disk substrate according to this embodiment, near its outer peripheral edge, and a fitted circle based on the maximum recess point of the recess.

[0021] [ Figure 3 [Illustration] is a diagram showing a recess and a protrusion on a main surface of a disk substrate according to this embodiment, near its outer peripheral edge, and a fitted circle based on the maximum protrusion point of the protrusion. Detailed Implementation

[0022] First, the disk substrate 1 according to this embodiment will be described.

[0023] like Figure 1 As shown in (a), the disk substrate 1 has an annular shape with a circular hole formed in the center.

[0024] The disk substrate 1 includes a pair of opposing main surfaces 11a and 11b, an outer peripheral edge surface 12, and an inner peripheral edge surface 13 defining a circular hole at its center. The main surface 11a has two circles centered at the center C of the disk substrate 1 as its inner and outer edges. The main surface 11b has the same shape as the main surface 11a and also has two circles centered at the center C of the disk substrate 1 as its inner and outer edges. The outer peripheral edge surface 12 connects the outer edges of the main surfaces 11a and 11b. The inner peripheral edge surface 13 connects the inner edges of the main surfaces 11a and 11b.

[0025] like Figure 1 As shown in (b), the main surfaces 11a and 11b and the outer peripheral edge surface 12 are connected by chamfered surfaces 12a and 12b, respectively.

[0026] like Figure 1 As shown in (c), the main surfaces 11a and 11b and the inner peripheral edge surface 13 are connected by chamfered surfaces 13a and 13b, respectively.

[0027] The size of the disk substrate 1 is not particularly limited; for example, its size can be suitable for disks with a nominal diameter of 2.5 inches or more (e.g., 2.5 inches, 3.5 inches, 5 inches, etc.). When the disk substrate is used for a disk with a nominal diameter of 2.5 inches, for example, the outer diameter of the disk substrate 1 is 55 mm to 70 mm, the diameter of the circular hole in the center is 20 mm, and the thickness of the disk substrate 1 is 0.3 mm to 0.8 mm. When the disk substrate is used for a disk with a nominal diameter of 3.5 inches, for example, the outer diameter of the disk substrate 1 is 85 mm to 100 mm, the diameter of the circular hole in the center is 25 mm, and the thickness of the disk substrate 1 is 0.3 mm to 0.8 mm. To increase the number of disks installed in each HDD, a smaller thickness is preferred, and a thickness is more preferably 0.5 mm or less, even more preferably 0.45 mm or less, and even more preferably 0.40 mm or less.

[0028] In the following description, an example of a method for manufacturing a disk substrate 1 according to this embodiment will be explained. Examples of materials for the disk substrate 1 include aluminosilicate glass, soda-lime glass, borosilicate glass, and aluminum-magnesium alloy having a NiP alloy film on its surface. Among these, amorphous aluminosilicate glass can be suitably used because it can be chemically strengthened as needed and can provide a disk substrate 1 with excellent flatness and high strength of the main surfaces 11a and 11b.

[0029] When a glass plate is used as the substrate of the disk substrate 1, the glass plate can be manufactured, for example, by float glass or overflow down-draw process, or by pressing a glass block using a mold. Methods for forming the glass plate into a ring shape include scribing the glass plate with a known scribing tool and then splitting the glass plate along the scribing lines, or irradiating the glass plate with a laser to form a circular defect and separating the glass plate along the circular defect.

[0030] Edge surface treatment, including edge grinding and edge polishing processes, is performed on the outer and / or inner peripheral edge surfaces of a glass plate formed into a ring shape. In the edge grinding process, for example, a form grinding wheel is used to form a chamfered surface. The form grinding wheel has a generally cylindrical shape and includes grooves along its outer peripheral surface. By pressing the edge surface of the glass plate against the grooves while rotating both the form grinding wheel and the glass plate cut into a ring shape, the edge surface of the glass plate can be ground to obtain an edge surface shape corresponding to the shape of the grooves. The edge grinding process can be performed in two stages: coarse grinding and fine grinding. For example, electroplated diamond grinding wheels with different grain sizes can be used as the first and second stage grinding wheels. In the edge polishing process, for example, a mirror finish is achieved on the outer and / or inner peripheral edge surfaces after the edge grinding process by brush polishing. At this time, a polishing slurry containing fine particles such as cerium oxide or zirconium oxide as loose abrasive particles is used. Polishing the edge surfaces can prevent thermal asperities and the precipitation of sodium and potassium ions that cause corrosion.

[0031] After the above edge surface treatment, the main surface grinding process, main surface polishing process, and cleaning process are carried out.

[0032] In the main surface grinding process, a double-sided grinding apparatus equipped with a planetary gear mechanism is used to grind the main surface of the annular glass plate. The amount of material removed by grinding is, for example, a few micrometers to about 100 μm. The double-sided grinding apparatus includes an upper platen and a lower platen, and the glass plate is held between the upper and lower platens. The main surface is ground by moving the glass plate and the platen relative to each other. As the platen, a platen with fixed abrasive grains attached thereto can be used. The fixed abrasive grains include abrasive particles such as diamond bonded to their surface with resin. Note that the main surface grinding process can be omitted.

[0033] In the main surface polishing process, the main surface of the annular glass plate is mirror-polished. The amount of material removed by polishing is, for example, about 0.1 μm to 50 μm. The main surface polishing aims to remove scratches and strain remaining on the main surface from previous processes, reduce ripples, micro-ripples, and surface roughness, and provide a mirror finish to the main surface. The surface roughness after the main surface polishing process, expressed as an arithmetic mean roughness (Ra) measured by AFM (atomic force microscopy), is preferably less than 0.15 nm. For the main surface polishing, a polishing slurry containing, for example, cerium oxide abrasive particles or zirconium oxide abrasive particles (particle size: D50 of about 0.5 μm to 2 μm) or silica abrasive particles (particle size: D50 of about 10 nm to 100 nm) as loose abrasive particles is used. The main surface polishing process can be performed in two or more stages.

[0034] The main surface polishing process can be performed using a known double-sided polishing apparatus equipped with a planetary gear mechanism, similar to the main surface grinding process described above. The double-sided polishing apparatus includes an upper and lower pressure plate made of cast iron, and a carrier holding the substrate between the upper and lower pressure plates. A polishing pad is attached to each surface of the upper and lower pressure plates (the contact surface with the substrate).

[0035] In a double-sided polishing apparatus, a substrate is held between an upper and lower pressure plate by a carrier and is clamped between the upper and lower pressure plates under a predetermined processing pressure (load). While polishing slurry is supplied at a predetermined supply rate between the polishing pad and the glass substrate on the upper pressure plate side and between the polishing pad and the glass substrate on the lower pressure plate side, the upper and lower pressure plates rotate about their central axes in opposite directions. As a result, the front and rear surfaces of the substrate slide against the surfaces of the opposing polishing pads, and both main surfaces of the substrate are polished simultaneously.

[0036] The following section will detail the case where the main surface polishing process is divided into a first polishing process and a second polishing process. The second polishing process is performed after the first polishing process.

[0037] (First polishing process)

[0038] As a polishing slurry, a slurry containing cerium oxide with a D50 of 0.5 μm to 2 μm as loose abrasive particles can be used. Although the type of polishing pad and other processing conditions also have an impact, it is mainly due to the effect of the polishing slurry containing this cerium oxide that a protrusion (skip shape) is formed at the outer peripheral edge of the main surface. In addition, a recess (recess) can be formed on the inner peripheral side of the protrusion.

[0039] As a polishing pad, a polyurethane pad with a hardness (Asker C) of 80 or higher can be used (a relatively hard polyurethane polishing pad with a foamed structure and not suede-like). The foamed polyurethane resin preferably has a hardness of 0.3 g / cm³. 3 Up to 1.0 g / cm 3 The density and compression ratio are 0.5% to 3.0%. Furthermore, the opening diameter of the foam pores is preferably 30 μm to 200 μm.

[0040] The polishing pad can be pre-impregnated with 10 to 35 (by weight) of a polishing material made of zirconium oxide and / or cerium oxide. By doing so, a new surface is easily and continuously formed, making it easier to achieve a uniform polishing effect throughout, even with prolonged polishing at low polishing rates. Grooves with a width of 0.5 mm to 3.0 mm and a depth of 0.5 mm to 2.0 mm can be formed on the surface of the polishing pad. These grooves can be formed, for example, in a grid pattern with intervals of 10 mm to 50 mm. This facilitates the supply of polishing fluid to the central periphery of the substrate's main surface.

[0041] The load applied to the main surface of the substrate during polishing can be set, for example, to 20 g / cm². 2 Up to 200 g / cm 2 Within a certain range. The polishing rate can be, for example, from 0.1 μm / min to 1.0 μm / min. The amount of material removed in the first polishing process, in terms of the equivalent thickness of the substrate, can be, for example, from 10 μm to 50 μm (5 μm to 25 μm on one surface).

[0042] Here, the processing conditions of the first polishing process and the shape of the outer peripheral edge are generally related as follows: (1) the greater the amount of material removed, the higher the protrusion becomes, and the deeper the recess on the inner peripheral side becomes; and (2) the lower the load applied to the main surface of the substrate or the slower the polishing rate, the more the radial position of the maximum protrusion point of the protrusion and the maximum recess point of the recess shifts towards the inner peripheral side.

[0043] (Second polishing process)

[0044] As a polishing slurry for the second polishing process, a slurry containing loose abrasive particles of silicon dioxide (D50) with a diameter of 10 nm to 100 nm can be used. Polishing with a silicon dioxide-containing slurry can create an edge-sagging shape (descending shape) at the outer peripheral edge of the substrate's main surface. Alternatively, when polishing with a silicon dioxide-containing slurry, edge sagging (descending) is more likely to occur at the outer peripheral edge of the substrate's main surface.

[0045] As a polishing pad, a soft suede-type polishing pad containing polyurethane foam with a hardness (Asker C) of 60 to 80 can be used. The load applied to the main surface of the substrate during polishing can be set, for example, to 20 g / cm². 2 Up to 150 g / cm 2 Within this range. Furthermore, the amount of material removed in the second polishing process, in terms of the equivalent thickness of the substrate, can be, for example, 0.5 μm to 4 μm (0.25 μm to 2 μm on one surface).

[0046] Here, the processing conditions of the second polishing process and the shape of the outer peripheral edge are generally related as follows. However, when the protrusions and recesses have already been formed by the first polishing process, the amount of material removed in the second polishing process is relatively small, so it is generally not possible to expect a change (effect) comparable to that in the first polishing process. (3) The greater the amount of material removed, the lower the protrusion becomes, and the shallower the recess on the inner peripheral side becomes. (4) The lower the load applied to the main surface of the substrate or the slower the polishing rate, the more the radial position of the maximum protrusion point of the protrusion and the maximum recess point of the recess shifts towards the inner peripheral side.

[0047] Furthermore, by appropriately adjusting the various polishing conditions of the first and / or second polishing processes described above, and by monitoring and providing feedback on the shape of the outer peripheral edge of the substrate after the polishing process using the method described later, the shape of the outer peripheral edge can be controlled to a desired shape. That is, by optimizing the various polishing conditions of the first and / or second polishing processes, the disk substrate of the present invention can be obtained.

[0048] The disk is manufactured by forming at least a magnetic layer on the main surfaces 11a and 11b of the disk substrate 1 manufactured by the above-described process. For example, a vertical disk can be manufactured by forming an adhesion layer, a soft magnetic layer, a seed layer, a second bottom layer, a magnetic layer (recording layer), and a protective layer sequentially on the surface of the substrate using a single-wafer sputtering apparatus or the like, and then forming a lubricating layer.

[0049] Next, taking the main surface 11a as an example, the shape of the outer peripheral edge of the main surfaces 11a and 11b of the disk substrate 1 according to this embodiment will be described. Figure 2 and 3 It is a diagram showing a cross section along the radial and thickness directions at the outer radial edge portion of the main surface 11a (hereinafter also referred to as the "profile" or "measurement profile"). Figure 2 and 3 The disk substrate 1 shown has a radius of 48.5 mm (i.e., a diameter of 97 mm) and a thickness of 0.5 mm. The radius of the disk substrate 1 refers to the distance from the center C of the disk substrate 1 to the outer peripheral edge surface 12.

[0050] Using MicroXAM (KLA) and analysis software, such as Figure 2 and 3 The shape of the outer peripheral edge shown is measured. The main measurement conditions are as follows. Note that noise is appropriately removed to make the measured profile a smooth curve.

[0051] Measurement radius: 38.5 mm to 48.5 mm (Multiple measurements are performed while offsetting the measurement position in the radial direction, so that adjacent rectangular measurement areas overlap by 30%, and then the data are merged) Number of measurement points in the radial direction (resolution): 65 points (one pitch is approximately 0.156 mm) Inclination correction of the measurement profile: Inclination correction is performed so that the straight line passing through two points with radii of 40.0 mm and 45.0 mm on the measurement profile becomes horizontal. Various measurements calculated from the profile (e.g., the positions of the maximum indentation point and the maximum protrusion point, and the radius of the fitted circle) are obtained through the following process: for a main surface (one main surface of a single disk), the shape of the outer peripheral edge is measured in four directions (0°, 90°, 180° and 270° with the center of the substrate as the origin), the values ​​for each profile are calculated, and the four values ​​obtained are averaged.

[0052] like Figure 2 and 3 As shown, the outer diameter edge of the main surface 11a has a protrusion CV extending upward in the thickness direction and a recess CC located radially inward relative to the protrusion CV and extending downward in the thickness direction. Here, "upward" in the thickness direction refers to the direction away from the center of the thickness direction of the disk substrate 1, and "downward" in the thickness direction refers to the direction toward the center of the thickness direction of the disk substrate 1.

[0053] like Figure 2As shown, when the point with the greatest recess depth in the downward direction of the thickness direction of the recessed portion CC is defined as the maximum recess point CC1, the radial distance from the center C of the disk substrate 1 to the maximum recess point CC1 is, for example, 41.5 mm to 43.5 mm. That is, the radial distance from the center C of the disk substrate 1 to the maximum recess point CC1 can be expressed as approximately 0.856R to 0.897R, where R represents the radius of the disk substrate 1. The radial distance from the center C of the disk substrate 1 to the maximum recess point CC1 is more preferably 0.89R or less, more preferably 0.88R or less, even more preferably 0.87R or less, and particularly preferably 0.86R or less. On the other hand, the slower the polishing rate of the first polishing and / or the second polishing, the closer the maximum recess point CC1 is to the center C of the disk substrate 1; however, if the polishing rate is too slow, the productivity decreases. Therefore, the lower limit is preferably, for example, 0.83R, and more preferably 0.84R or more.

[0054] Furthermore, on the main surface 11a, when a virtual circle passing through the maximum depression point CC1 and two points CC2 and CC3 located 1 mm inward and outward respectively from the maximum depression point CC1 in the radial direction are defined as the fitted circle CCC with the maximum depression point CC1 as the reference, the radius RCC of the fitted circle CCC with the maximum depression point CC1 as the reference is calculated to be, for example, 80 m or more. The radius and center coordinates of the fitted circle can be calculated from the coordinates of the three points. The radius RCC, as... Figure 2 and 3 The shape of the outer peripheral edge of the main surface shown can be obtained by performing the main surface polishing process in two or more stages while adjusting the conditions.

[0055] As described above, in recent technologies, the height of protrusions and the depth of depressions are reduced at the outer peripheral edge of the main surface, and the protrusions and depressions are offset to the outside of the magnetic recording area, thereby expanding the magnetic recording area and flattening it. However, when such protrusions and depressions are offset as far outward as possible on the main surface in order to expand the magnetic recording area, the protrusions and depressions are confined to a very narrow area at the outer peripheral edge of the main surface, and it has been found that steep protrusions and depressions are formed at the outer peripheral edge of the main surface, in other words, protrusions and depressions with a large slope. In this case, there are limitations in expanding the magnetic recording area. Therefore, the inventors of the present invention have discovered that when the maximum depression point CC1 is located at a radial position of less than 0.90R (where R represents the radius of the disk substrate 1), problems during disk read and / or write (hereinafter referred to as "R / W") are reduced, and the magnetic recording area can be further expanded radially outward. Although the mechanism by which the maximum indentation point CC1 is located radially below 0.90R to reduce problems during R / W is not yet fully understood, it is speculated that the embossed pattern is elongated radially, making it less likely for contact to occur between the read / write head and the disk.

[0056] As described above, in recent years, in response to the increasing demand for higher recording capacity and higher recording density per disk, the distance between the magnetic recording layer of the disk and the R / W element of the head has been further reduced. For example, in heads employing thermal flying height control, it is necessary to maintain a constant flying height of the R / W element from the disk surface (i.e., the distance between the disk surface and the R / W element) by controlling the protrusion of the R / W element at high speed. However, when the aforementioned skid shape appears on the main surface of the disk substrate, this control becomes difficult, and the R / W element may come into physical contact with the skid, or even without physical contact, the flying height of the R / W element may become unstable, leading to R / W errors. Therefore, the inventors of this invention have discovered that when the radius RCC of the fitted circle CCC based on the maximum indentation point CC1 is greater than or equal to a predetermined value, the stability of the head during seek operations is improved, and the aforementioned problems are reduced. While the mechanism of this effect is not yet fully understood, it is speculated that the presence of a recess CC with an appropriate radius of curvature allows centrifugal force to act on the read / write head during high-speed seek operations, thereby enabling the read / write head to move stably along the wall of the recess CC. In this regard, in the disk substrate 1 of this embodiment, since the radius RCC of the fitted circle CCC based on the maximum recess point CC1 is calculated to be, for example, 80 m or more, the stability of the read / write head during seek operations is improved, and problems can be reduced. If the radius RCC of the fitted circle CCC is too small, the flight characteristics of the read / write head will deteriorate. Therefore, the radius RCC of the fitted circle CCC is preferably 50 m or more. On the other hand, if the radius RCC of the fitted circle CCC is too large, the effect of improving the stability of the read / write head during seek operations tends to decrease. Therefore, the radius RCC of the fitted circle CCC is preferably 400 m or less, more preferably 300 m or less.

[0057] Furthermore, it is preferable that the absolute value of the radial distance between the maximum depression point CC1 and the center CC0 of the fitted circle CCC based on the maximum depression point CC1 is 1.00 mm or less. If the center CC0 of the fitted circle CCC is located radially inward relative to the maximum depression point CC1 and the absolute value exceeds 1 mm, the slope towards the apex of the protrusion becomes too steep, thereby increasing the load on the seek operation and potentially increasing the frequency of seek operation errors during long-term operation. On the other hand, if the center CC0 of the fitted circle CCC is located radially outward of the maximum depression point CC1 and the absolute value exceeds 1 mm, the slope towards the center of the disk becomes too steep, thereby increasing the load on the seek operation and potentially increasing the frequency of seek operation errors during long-term operation.

[0058] On the other hand, such as Figure 3As shown, when the point where the protrusion height of the protrusion CV reaches its maximum in the upward direction of the thickness direction is defined as the maximum protrusion point CV1, the radial distance from the center C of the disk substrate 1 to the maximum protrusion point CV1 is preferably about 47.53 mm or less. That is, the radial distance from the center C of the disk substrate 1 to the maximum protrusion point CV1 is preferably about 0.98R or less, where R represents the radius of the disk substrate 1. When the radial distance from the center C of the disk substrate 1 to the maximum protrusion point CV1 is 0.98R or less, the slope on the outer periphery of the maximum protrusion point CV1 becomes gentler, thereby reducing the possibility of the R / W element contacting the disk at the outermost circumferential portion, which is advantageous. For the same reason, the radial distance is more preferably 0.97R or less. On the other hand, if the polishing rate of the first polishing and / or the second polishing is reduced by moving the maximum protrusion point CV1 toward the center C side of the disk substrate 1, the productivity will decrease. Therefore, the lower limit is preferably set to 0.93R.

[0059] Furthermore, on the main surface 11a, when a virtual circle passing through the maximum protrusion point CV1 and two points CV2 and CV3 located at radial distances of 0.5 mm inward and outward respectively from the maximum protrusion point CV1 are defined as the fitted circle CCV based on the maximum protrusion point CV1, the radius RCV of the fitted circle CCV based on the maximum protrusion point CV1 is preferably 15 m or more. When the radius RCV of the fitted circle CCV is 15 m or more, even if the read / write head moves at high speed in the radial direction to cross the maximum protrusion point CV1 during seek operations, the R / W element is less likely to move away from the disk surface, thereby reducing the possibility of R / W errors, which is advantageous. For the same reason, the radius RCV of the fitted circle CCV based on the maximum protrusion point CV1 is more preferably 20 m or more. On the other hand, if the polishing rate of the first polishing and / or the second polishing is reduced in order to increase the radius RCV of the fitted circle CCV based on the maximum protrusion point CV1, the productivity decreases. Therefore, the upper limit is preferably set to 150 m.

[0060] The embodiments and comparative examples of the present invention will be described next.

[0061] (Example)

[0062] First, a glass plate made of alkali-free aluminosilicate glass manufactured by the overflow-pull method is prepared, and annular glass blanks are cut out according to the manufacturing method described above. Then, edge surface grinding, edge surface polishing, main surface grinding, first polishing, and second polishing processes are performed to manufacture multiple disk glass substrates with different maximum indentation point positions (radial distance from the center of the disk substrate), as shown in Table 1 below. Each disk substrate has a thickness of 0.5 mm, a diameter (outer diameter) of 97 mm (radius of 48.5 mm), a diameter of 25 mm for the circular hole, and a chamfer length of 80 μm (angle of 45 degrees) in the radial direction. Furthermore, when the surface roughness of the main surface is measured by AFM, the arithmetic mean roughness (Ra) is 0.11 nm. Under the same conditions, a magnetic film, etc., is formed on the surface of each disk glass substrate to obtain a disk for perpendicular magnetic recording. Since the magnetic film, etc., is extremely thin relative to the thickness of the disk substrate and is uniformly formed on the main surface, the surface morphology of the disk can be considered the same as that of the disk substrate.

[0063] Based on the above trends, the first and second polishing processes will be carried out simultaneously with appropriate adjustments within the following conditions.

[0064] (First polishing process) Polishing pad: Polyurethane polishing pad (Asker C hardness 80 to 100, with grid-like grooves formed and pre-impregnated with zirconium oxide and cerium oxide) Polishing slurry: A polishing slurry containing cerium oxide (D50: 1.0 μm) as loose abrasive particles. Amount of material removed per surface by polishing: 10 μm to 20 μm Load applied to the substrate: 20 g / cm 2 Up to 100 g / cm 2

[0065] (Second polishing process) Polishing pad: Suede-type polishing pad containing polyurethane foam (Asker C hardness 60 to 80). Polishing slurry: A polishing slurry containing silica (D50: 30 nm) as loose abrasive particles. The amount of material removed from each surface by polishing: 0.5 μm to 2.0 μm Load applied to the substrate: 20 g / cm 2Up to 100 g / cm 2

[0066] (Comparative Example)

[0067] For the comparative example, the disk substrate was obtained in the same manner as in the embodiment, except that the first and second polishing processes were performed under the following conditions.

[0068] (First polishing process) Polishing pad: Suede-type polishing pad containing polyurethane foam (Asker C hardness 90). Amount of material removed per surface by polishing: 15 μm Load applied to the substrate: 100 g / cm 2

[0069] (Second polishing process) Polishing pad: Suede-type polishing pad containing polyurethane foam (Asker C hardness 75). Polishing slurry: A polishing slurry containing silica (D50: 30 nm) as loose abrasive particles. Amount of material removed per surface by polishing: 1.0 μm Load applied to the substrate: 100 g / cm 2

[0070] Then, the disk was rotated using a spinstand tester, keeping the circumferential velocity of the disk at the radial position of the head (i.e., the relative velocity between the head and the disk) constant (33.9 m / sec), regardless of the radial position of the head. While the head, employing thermally controlled flight altitude, was reading from and / or writing to the disk (hereinafter referred to as "R / W"), the flight position of the head was varied from the central radial region of the disk to the outer radial region, and the location (radial distance from the center of the disk) where R / W errors occurred (or suddenly increased) was measured. The width of the head used was approximately 0.5 mm, and the R / W element was located at the center of its rear end in the width direction. Furthermore, during R / W, the flight altitude of the head slider body above the disk surface was maintained at 10 nm, and the flight altitude of the R / W element above the disk surface was set as follows: 0.6 nm for the read element and 0.8 nm for the write element. The further outward the location of the R / W error, the greater the extent to which the magnetic recording area can expand radially outward. As shown in Examples 1 to 3, as the location of the maximum indentation point shifts towards the inner periphery of the disk, that is, as the radial distance from the center of the disk to the maximum indentation point decreases, the location of the R / W error occurs closer to the outer periphery of the disk. Conversely, in Comparative Example 1, where the location of the maximum indentation point is closer to the outer periphery than in Example 1, the location of the R / W error occurs closer to the inner periphery than in Example 1.

[0071] [Table 1]

[0072] Furthermore, based on the manufacturing conditions of Example 2, the conditions of the first and second polishing processes were further adjusted according to the aforementioned trend to prepare multiple disk substrates such that the radii of the fitted circles based on their respective maximum depression points are different from each other, as shown in Table 2 below. The thickness, diameter (radius), and chamfer length of each disk substrate are the same as those in Table 1 above. In addition, in each disk substrate, the radial position of the maximum depression point is within the range of 42.5 ± 1 mm. As in Table 1 above, the magnetic film and the like are extremely thin relative to the thickness of the disk substrate and are uniformly formed on the main surface. Therefore, it can be considered that the surface morphology of the disk is the same as the surface morphology of the disk substrate.

[0073] Then, using a helium-filled hard disk drive (HDD), the disk was rotated at a constant speed (7200 rpm), and 100,000 high-speed continuous seek operations were performed on the disk from the central radial region to the outer radial region while the read and / or write operations (hereinafter referred to as "R / W") were performed on the disk using a thermally controlled flight altitude head. The number of R / W errors occurring during the operation was measured. The number of errors occurring when the radius of the fitted circle based on the maximum indentation point was 80 m was used as the baseline value (1.00), and the number of errors occurring in other cases was expressed relative to the baseline value. During R / W, the flight altitude of the head slider body above the disk surface was maintained at 10 nm, and the flight altitude of the R / W elements above the disk surface was set as follows: 0.6 nm for read elements and 0.8 nm for write elements.

[0074] [Table 2]

[0075] Even with a fitted circle radius of 60 m, there are no practical problems; however, it has been found that seek operation errors decrease when the radius is set to 80 m or higher. Furthermore, seek operation errors decrease further when the radius is set to 100 m, 120 m, and 140 m or higher, with the error reaching its minimum at 162 m; however, at 260 m, the result is comparable to that at 100 m.

[0076] Furthermore, the disk substrate was manufactured in the same manner as in the embodiments described above, except that the substrate thickness was set to 0.43 mm. As a result, there was almost no effect from the thickness, and substantially the same outer peripheral edge shape was obtained. Disks for perpendicular magnetic recording were manufactured using these substrates, and the evaluations shown in Tables 1 and 2 were performed, yielding substantially the same results. That is, even when the thickness is reduced from 0.5 mm to below 0.45 mm, the disk glass substrate of the present invention does not exhibit any particular disadvantages in its R / W characteristics, and the number of disks mounted in HDDs can be increased while expanding the magnetic recording area.

[0077] List of reference numerals

[0078] 1. Disk substrate

[0079] 11a, 11b Main surfaces

[0080] 12. Outer peripheral edge surface

[0081] 12a, 12b Chamfered surfaces

[0082] 13 Inner peripheral edge surface

[0083] 13a, 13b Chamfered surfaces

[0084] CC recess

[0085] CV protrusion

[0086] CC1 Maximum Indentation Point

[0087] CCC Fitting Circle

[0088] RCC is the radius of circle CCC.

[0089] CV1 maximum protrusion point

[0090] CCV Fitting Circle

[0091] RCV (Radius of Circular CCV)

Claims

1. A disk substrate, comprising: A pair of annular main surfaces; as well as outer peripheral edge surface, In a cross-section taken along the radial and thickness directions of the substrate, at least one of the pair of main surfaces has a protrusion extending upward in the thickness direction and a recess located radially inward relative to the protrusion and extending downward in the thickness direction. The radial distance from the center of the substrate to the maximum depression point is less than 0.90R. At the maximum depression point, the depression depth of the depression in the downward direction of the thickness direction is the largest, where R represents the radius of the substrate.

2. The disk substrate according to claim 1, in, The radius of the fitted circle based on the maximum depression point is 80 m or more.

3. The disk substrate according to claim 1, in, The absolute value of the radial distance between the maximum depression point and the center of the fitted circle based on the maximum depression point is less than 1.00 mm.

4. The disk substrate according to claim 1, in, The radial distance from the center of the glass substrate to the maximum protrusion point is less than 0.98R, and at the maximum protrusion point, the protrusion height in the upward direction of the thickness direction is the maximum.

5. The disk substrate according to claim 4, in, The radius of the fitted circle based on the maximum protrusion point is 15 m or more.

Citation Information

Patent Citations

  • Substrate for magnetic disk and magnetic disk

    JP2010073289A