Electrode composite materials and batteries

By adding organic compounds with more than two benzene rings to the electrode composite material, the degradation problem of sulfide solid electrolytes caused by charging and discharging in the battery was solved, and the increase in resistance and the improvement of chemical stability were achieved.

CN123125686APending Publication Date: 2026-11-17TOYOTA JIDOSHA KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580028220.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-11-06
Filing Date
2025-03-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Sulfide solid electrolytes deteriorate in batteries due to repeated charging and discharging, leading to increased resistance.

Method used

A sulfide solid electrolyte containing lithium, sulfur, and phosphorus is used, and an organic compound with two or more benzene rings is added between the electrode active material and the sulfide solid electrolyte as an electrode composite material to suppress the deterioration of the sulfide solid electrolyte.

Benefits of technology

It effectively suppressed the increase in battery resistance, improved chemical stability and electronic conductivity, and slowed down the deterioration of conductive additives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125686A_ABST
    Figure CN123125686A_ABST
Patent Text Reader

Abstract

The present invention aims to provide an electrode composite material capable of suppressing the increase in battery resistance. In this invention, the above-mentioned problem is solved by providing an electrode composite material containing an electrode active material, a sulfide solid electrolyte, and an organic compound. The sulfide solid electrolyte contains lithium, sulfur, and phosphorus, and the organic compound has two or more benzene rings, with at least a portion of the organic compound present between the electrode active material and the sulfide solid electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to electrode composite materials and batteries. Background Technology

[0002] In recent years, battery development has been booming. For example, in the automotive industry, various research and development efforts are underway regarding batteries for electric vehicles (BEVs), plug-in hybrid electric vehicles (PHEVs), or hybrid electric vehicles (HEVs).

[0003] For example, Patent Document 1 discloses a modified sulfide solid electrolyte for use in batteries. The BET specific surface area of ​​the aforementioned modified sulfide solid electrolyte is 10 m². 2 It contains sulfide solid electrolytes and epoxy compounds, and its infrared absorption spectrum obtained by FT-IR analysis (ATR method) is in the range of 2800–3000 cm⁻¹. -1 It has a peak.

[0004] Existing technical documents

[0005] Patent documents

[0006] Patent Document 1: International Publication No. 2022 / 158458 Summary of the Invention

[0007] The problem that the invention aims to solve

[0008] Sulfide solid electrolytes have attracted attention as battery materials, particularly electrode layers, due to their excellent ionic conductivity. However, batteries using sulfide solid electrolytes pose the risk that repeated charge-discharge cycles can lead to degradation (oxidation or reduction) of the electrolyte, resulting in increased resistance.

[0009] The present invention was made in view of the above-mentioned actual situation, with the main objective of providing an electrode composite material capable of suppressing the increase of battery resistance.

[0010] Methods for solving problems

[0011] [1] An electrode composite material comprising an electrode active material, a sulfide solid electrolyte, and an organic compound, wherein the sulfide solid electrolyte contains lithium, sulfur, and phosphorus. The organic compound has two or more benzene rings. At least a portion of the organic compound is present between the electrode active material and the sulfide solid electrolyte.

[0012] [2] The electrode composite material according to [1] contains at least one of the compounds represented by the following general formula (1) or the following general formula (2) as the organic compound.

[0013]

[0014] (where R is in the formula) 1 and R 2 Each is an independent organic group, R 3 ~R 10 Each atom can be independently a hydrogen atom or a substituent, where n is an integer from 0 to 4.

[0015] [3] According to the electrode composite material described in [2], wherein the R 1 and the R 2 At least one of them is an organic group represented by the following general formula (3).

[0016]

[0017] (In the formula, X is an organic group) (This represents a bond.)

[0018] [4] The electrode composite material according to [3], wherein the X has an epoxy group.

[0019] [5] The electrode composite material according to any one of [1] to [4] contains 9,9-bis(4-glycidoxyphenyl)fluorene as the organic compound represented by the following chemical formula (1).

[0020]

[0021] [6] The electrode composite material according to any one of [1] to [5], wherein the organic compound contains a compound represented by the following general formula (4).

[0022]

[0023] (In the formula, S is an organic group, n is 0 or 1, R) 11 ~R 20 Each can be an independent hydrogen atom or a substituent.

[0024] [7] The electrode composite material according to [6], wherein the S has an epoxy group.

[0025] [8] The electrode composite material according to [6] or [7], wherein the S is an organic group represented by the following general formula (5).

[0026]

[0027] (In the formula, T and U are each an organic group, n) 1 and n 2 Each is independently either 0 or 1. (This represents a bond.)

[0028] [9] The electrode composite material according to any one of [1] to [8], wherein 1,3-diphenyl-2,3-epoxy-1-propanone as the organic compound is represented by the following chemical formula (2).

[0029]

[0030]

[10] The electrode composite material according to [1], wherein the organic compound has a sulfonyl group.

[0031]

[11] The electrode composite material according to

[10] contains a compound represented by the following general formula (6) as the organic compound.

[0032]

[0033] (where R is in the formula) 21 ~R 30 Each can be independently a hydrogen atom, a substituent, or an organic group.

[0034]

[12] According to the electrode composite material described in

[11] , wherein the R 21 ~The R mentioned 30 At least one of them is an organic group represented by the following general formula (7) or the following general formula (8).

[0035]

[0036] (In the formula, α and β are each an organic group, n) 1 and n 2 Each is independently either 0 or 1. (This represents a bond.)

[0037]

[13] The electrode composite material according to any one of [1] to

[12] , wherein the organic compound contains tetraglycidyl-3,3'-diaminodiphenyl sulfone as shown in the following chemical formula (3).

[0038]

[0039]

[14] According to the electrode composite material of

[11] , wherein the R 21 ~The R mentioned 30 At least one of them is an organic group represented by the following general formula (9).

[0040]

[0041] (In the formula, γ is an organic group, and n is 0 or 1) (This represents a bond.)

[0042]

[15] The electrode composite material according to any one of [1] to

[14] , wherein the organic compound contains a diglycidyl ether sulfone compound represented by the following chemical formula (4).

[0043]

[0044]

[16] According to the electrode composite material of [1], wherein the organic compound has the structure shown in the following structural formula (1), the structure shown in the following structural formula (2), the structure in which at least one hydrogen atom bonded to the benzene ring of the following structural formula (1) is replaced by a group with a molecular weight of 50 or less, or the structure in which at least one hydrogen atom bonded to the benzene ring of the following structural formula (2) is replaced by a group with a molecular weight of 50 or less.

[0045]

[0046] (in the formula, (This represents a bond, where n is an integer from 0 to 4.)

[0047]

[17] According to the electrode composite material of [1], wherein the organic compound has the structure shown in the following structural formula (3-1), the structure shown in the following structural formula (3-2), the structure in which at least one hydrogen atom bonded to the benzene ring of the following structural formula (3-1) is replaced by a group with a molecular weight of 50 or less, or the structure in which at least one hydrogen atom bonded to the benzene ring of the following structural formula (3-2) is replaced by a group with a molecular weight of 50 or less.

[0048]

[0049] (in the formula, (This represents a bond.)

[0050]

[18] According to the electrode composite material of [1], wherein the organic compound has the structure shown in the following structural formula (4-1), the structure shown in the following structural formula (4-2), the structure shown in the following structural formula (4-3), the structure in which at least one hydrogen atom bonded to the benzene ring of the following structural formula (4-1) is replaced by a group with a molecular weight of 50 or less, the structure in which at least one hydrogen atom bonded to the benzene ring of the following structural formula (4-2) is replaced by a group with a molecular weight of 50 or less, or the structure in which at least one hydrogen atom bonded to the benzene ring of the following structural formula (4-3) is replaced by a group with a molecular weight of 50 or less.

[0051]

[0052] (in the formula, (This represents a bond.)

[0053]

[19] The electrode composite material according to any one of [1] to

[18] , wherein the Hansen solubility parameter of the organic compound is 8.0 MPa. 0.5 above.

[0054]

[20] The electrode composite material according to any one of [1] to

[19] , wherein the proportion of the organic compound relative to the sulfide solid electrolyte is greater than 0.50% by mass and less than 14.0% by mass.

[0055]

[21] The electrode composite material according to any one of [1] to

[20] , wherein the electrode composite material is a negative electrode composite material.

[0056]

[22] According to the electrode composite material described in

[21] , wherein the electrode active material is a Si-based active material.

[0057]

[23] The electrode composite material according to any one of [1] to

[20] , wherein the electrode composite material is a positive electrode composite material.

[0058]

[24] According to the electrode composite material of

[22] , wherein the electrode active material is an oxide active material containing at least Ni and Co elements.

[0059]

[25] A battery having a positive active material layer, a negative active material layer, and an electrolyte layer disposed between the positive active material layer and the negative active material layer, wherein at least one of the positive active material layer and the negative active material layer contains an electrode composite material as described in any one of [1] to

[24] .

[0060] Invention Effects

[0061] In this invention, the effect of suppressing the increase in battery resistance is achieved. Attached Figure Description

[0062] Figure 1 This is a schematic cross-sectional view illustrating the electrode composite material of the present invention.

[0063] Figure 2 This is a schematic cross-sectional view illustrating the battery of the present invention.

[0064] Figure 3 This is a graph showing the results of a representative rate of increase in resistance.

[0065] Figure 4This is a graph showing the results of a representative rate of increase in resistance.

[0066] Figure 5 This is a graph showing representative XPS measurement results.

[0067] Figure 6 This is a graph showing representative XPS measurement results.

[0068] Figure 7 This is a graph showing representative XPS measurement results.

[0069] Figure 8 This is a graph showing the results of the resistance increase rate for each embodiment and each comparative example.

[0070] Figure 9 This is a graph showing the results of the resistance increase rate for each embodiment and each comparative example. Detailed Implementation

[0071] The electrode composite material and battery of the present invention will now be described in detail. It should be noted that the figures shown below are schematic illustrations, and the dimensions and shapes of the parts have been appropriately exaggerated for ease of understanding.

[0072] A. Electrode composite materials

[0073] The electrode composite material of the present invention contains an electrode active material, a sulfide solid electrolyte, and an organic compound. The sulfide solid electrolyte contains lithium, sulfur, and phosphorus. Furthermore, the organic compound has two or more benzene rings. Additionally, as... Figure 1 As shown, in the electrode composite material 10, at least a portion of the organic compound 3 exists between the electrode active material 1 and the sulfide solid electrolyte 2.

[0074] According to the present invention, since the electrode composite material contains an organic compound having two or more benzene rings, and at least a portion of the organic compound exists between the electrode active material and the sulfide solid electrolyte, the degradation of the sulfide solid electrolyte (oxidation or reduction of the sulfide solid electrolyte) can be suppressed.

[0075] As described above, sulfide solid electrolytes are at risk of deterioration during battery charging and discharging. For example, in the positive electrode active material layer, there is a risk that oxygen atoms released from the positive electrode active material may oxidize the sulfide solid electrolyte. On the other hand, the electrode composite material of the present invention has two or more benzene rings, and at least a portion of them are present between the electrode active material (positive electrode active material) and the sulfide solid electrolyte, thus it is presumed that the organic compound acts as a barrier. Similarly, it is presumed that in the negative electrode active material layer, the organic compound also acts as a barrier, suppressing side reactions of the sulfide solid electrolyte (improving reduction resistance). Here, the benzene ring has a conjugated structure formed by alternating double and single bonds, possessing a π electron cloud. Therefore, it is presumed that in organic compounds with multiple benzene rings, the π electron cloud extends over a wider region, resulting in better chemical stability (oxidation resistance, reduction resistance). As a result, the chemical stability of the sulfide solid electrolyte located near such organic compounds is also improved. Based on these mechanisms, it is presumed that the increase in resistance is suppressed in batteries using the electrode composite material of the present invention.

[0076] Furthermore, in the electrode layer, excessively high electronic conductivity poses a risk of promoting the degradation of conductive additives. To address this, the organic compounds of the present invention can appropriately suppress electronic conductivity. As a result, it is presumably possible to suppress the degradation of conductive additives, thereby inhibiting the increase in resistance.

[0077] 1. Organic compounds

[0078] The organic compound of the present invention is a compound having two or more benzene rings. The number of benzene rings can be three or more, four or more, or five or more. Alternatively, the number of benzene rings can be, for example, eight or less. Furthermore, the number of benzene rings in the organic compound can be any one of 2, 3, 4, 5, 6, 7, or 8.

[0079] Examples of organic compounds having multiple benzene rings include: fused polycyclic hydrocarbons such as naphthalene, anthracene, fluorene, phenalene, tetraphenylene, and pentaphenylene; derivatives of fused polycyclic hydrocarbons; biphenyl and its derivatives; and compounds in which multiple benzene rings are linked by organic groups.

[0080] Furthermore, in the organic compounds of the present invention, it is preferable that the conjugation inside the benzene ring extends to the outside of the benzene ring. For example, in the compounds shown in general formulas (1) and (2) described later, since the two benzene rings are connected by a single bond, the conjugation inside one benzene ring extends to the outside of that benzene ring (the other benzene ring). It is speculated that by expanding the conjugation range, the conductivity of carrier ions such as lithium ions is improved.

[0081] Examples of organic compounds of the present invention include compounds (fluorene derivatives) represented by the following general formula (1) or the following general formula (2).

[0082]

[0083] In the above general formulas (1) and (2), R 1 and R 2 Each is an organic group independently. Here, in this invention, an "organic group" refers to a group having at least hydrogen and carbon atoms. An organic group can be a group consisting only of hydrogen and carbon atoms, or it can be a group containing other atoms. Examples of other atoms include at least one of oxygen, nitrogen, phosphorus, sulfur, and halogen atoms. Furthermore, an organic group can be a group consisting only of hydrogen, carbon, and oxygen atoms, or it can be a group consisting only of hydrogen, carbon, oxygen, and nitrogen atoms.

[0084] The number of carbon atoms in the organic group is not particularly limited; for example, it can be 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, or 6 or more. Alternatively, it can be 20 or less, 18 or less, or 16 or less. Furthermore, the number of carbon atoms in the organic group can be any range from 1 to 20. Additionally, the organic group can be linear, branched, or cyclic. It should be noted that the organic group can partially possess a cyclic structure such as a benzene ring. Furthermore, the organic group can have a specified functional group or may not have a functional group. Examples of functional groups include hydroxyl, ether, epoxy, carbonyl, amino, cyano, nitro, sulfonyl, sulfonyl, allyl, and halogen elements (halogen groups) such as Cl and Br. The organic group preferably has an epoxy group at the end or inside the molecular structure. Furthermore, the organic group can be an alkyl group with 5 or fewer carbon atoms. The number of carbon atoms in the alkyl group can be 3 or less, or 1 or 2. Furthermore, the organic group can have only one of the above-mentioned functional groups or more than two. In addition, the organic group may have only one of the above-mentioned functional groups, or it may have two or more of them.

[0085] As mentioned above, R 1 And the above R 2 For example, the organic groups represented by the general formula (3) below can be listed. R 1 and R 2 One of them can be an organic group represented by the following general formula (3), or both can be organic groups represented by the following general formula (3). Additionally, R 1 and R 2 It can be an organic group with the same structure. In particular, R 1 and R 2 It can be an organic group with the same structure as the general formula (3) below.

[0086]

[0087] In the above general formula (3), X is an organic group. This indicates a bonded bond. That is, the organic group represented by general formula (3) in... The bond is bonded to other atoms (e.g., carbon) that constitute the organic compound. The meaning of the bond is the same in the following examples. In addition, the organic group is the same as that described in general formulas (1) and (2). In particular, X preferably has an epoxy group. In addition, X preferably has an epoxy group at the end. Furthermore, X preferably has an epoxy group and has an ether group (ether bond) between the epoxy group and the benzene ring shown in the above general formula (3). The oxygen atom in the ether group (ether bond) can be directly bonded to the carbon atom in the benzene ring shown in the above general formula (3). In addition, the oxygen atom in the ether group (ether bond) can be directly bonded to the carbon atom in the epoxy group, or it can be bonded via an alkyl group having 1 or more and 3 or less carbon atoms. In addition, in the above general formula (3), the positional relationship between the bond and X can be ortho, meta, or para.

[0088] Furthermore, in the above general formulas (1) and (2), R 3 ~R 10 Each is independently a hydrogen atom or a substituent (of a hydrogen atom). Examples of substituents include the functional groups described above and alkyl groups having 1 to 10 carbon atoms. The alkyl groups described above can have 1 or more but less than 5 carbon atoms, or 1 or more but less than 3 carbon atoms, or 1 or 2 carbon atoms. Furthermore, in R... 3 ~R 10 Of the six R atoms, there is no particular limitation on the number of R atoms that are hydrogen atoms; there can be more than four, more than five, or even six.

[0089] Furthermore, in the above general formula (2), n is an integer from 0 to 4. When n is 0, (CH2) in general formula (2) n Some are single bonds. That is, the carbon atom of the 5-membered ring in general formula (2) is bonded to CHR. 1 R 2 The "C (carbon atom)" in the structure is directly bonded.

[0090] As a specific example of the organic compound represented by the above general formula (1), 9,9-bis(4-glycidyloxyphenyl)fluorene, represented by the following chemical formula (1), can be cited.

[0091]

[0092] In addition, as organic compounds of the present invention, compounds represented by the following general formula (4) can be listed as examples.

[0093]

[0094] In the above general formula (4), S is an organic group. Additionally, n is 0 or 1. Furthermore, R... 11 ~R 20 Each is independently a hydrogen atom or a substituent (of a hydrogen atom). The organic groups and substituents (functional groups) are the same as those described in general formulas (1) and (2). The S mentioned above preferably has an epoxy group. Additionally, in R... 11 ~R 20 Of the 10 R's, the number of R's that are hydrogen atoms is not particularly limited; it can be 6 or more, 8 or more, 9 or more, or 10. Furthermore, in the above general formula (4), when n is 0, it includes R's. 11 ~R 15 The carbon atom in the benzene ring and the R 16 ~R 20 The carbon atoms in the benzene ring are directly bonded (biphenyl structure).

[0095] Here, as S above, the organic groups represented by the following general formula (5) can be listed. As shown in general formula (5), the organic groups of the present invention may include epoxy groups and carbonyl groups.

[0096]

[0097] In general formula (5), T and U are each an independent organic group, and n 1 and n 2 Each is independently either 0 or 1. This indicates a bonded bond. Regarding organic groups, as described above. When n 1 When n is 0, the carbon atom in the epoxy group is directly bonded to other atoms that make up the organic compound (e.g., the carbon atom in the benzene ring). On the other hand, when n... 2 When the number is 0, the carbon atom in the epoxy group is directly bonded to the carbon atom in the carbonyl group. T and U can consist only of carbon and hydrogen atoms. The number of carbon atoms in T can be, for example, 5 or less, 3 or less, or 1 or 2. Similarly, the number of carbon atoms in U can be, for example, 5 or less, 3 or less, or 1 or 2.

[0098] As a specific example of the organic compound represented by the above general formula (4), 1,3-diphenyl-2,3-epoxy-1-propanone, represented by the following chemical formula (2), can be cited.

[0099]

[0100] The organic compounds of the present invention, as described above, have two or more benzene rings. Preferably, the organic compounds also have a sulfonyl group. The presence of a sulfonyl group in the organic compound enhances the conductivity of metal ions such as Li ions.

[0101] As organic compounds having a sulfonyl group, examples include compounds represented by the following general formula (6).

[0102]

[0103] In the above general formula (6), R 21 ~R 30 Each is independently a hydrogen atom, a substituent (of the hydrogen atom), or an organic group. The organic group and substituent (functional group) are the same as those described in general formulas (1) and (2). In particular, the organic group preferably has an epoxy group at the end of the molecular structure. Furthermore, in R... 21 ~R 25 Of the five R atoms, the number of R atoms that are hydrogen atoms is not particularly limited; it can be more than three, more than four, or even five. Similarly, in R... 26 ~R 30 Of the five R atoms, the number of R atoms that are hydrogen atoms is not particularly limited; it can be three or more, four or more, or even five. Furthermore, in R... 21 ~R 25 Of the five Rs, the number of Rs that are organic groups is not particularly limited; it can be two or less, or even one. Similarly, in R... 26 ~R 30 Of the five Rs, the number of Rs that are organic groups is not particularly limited; it can be two or less, or even one. Furthermore, in the R... 21 ~R 25 Of the five Rs, four can be hydrogen atoms and one can be an organic group. Similarly, in R... 26 ~R 30 Of the five Rs, four can be hydrogen atoms and one can be an organic group. Furthermore, it is preferable to have R... 21 ~R 25 The structure of the benzene ring is similar to that of the R ring. 26 ~R 30 The structure of the benzene ring is symmetrical about the sulfonyl group. For example, the compounds shown in chemical formulas (3) and (4) described later have a structure symmetrical about the sulfonyl group. In addition, in one of the benzene rings of the above general formula (6), the positional relationship between the sulfonyl group and the organic group can be ortho, meta, or para.

[0104] R 21 ~R 30At least one of them can be an organic group represented by the following general formula (7) or the following general formula (8).

[0105]

[0106] In the above general formulas (7) and (8), α and β are each independently an organic group. Additionally, n 1 and n 2 Each is independently either 0 or 1. When n 1 or n 2 When the value is 0, the nitrogen atom in general formulas (7) and (8) directly bonds to the carbon atom in the epoxy group. Additionally, This indicates a bond. Regarding organic groups, the same applies as described in general formulas (1) and (2). α and β can consist only of carbon and hydrogen atoms. The number of carbon atoms in α can be, for example, 3 or less, 2 or less, or 1. Similarly, the number of carbon atoms in β can be, for example, 3 or less, 2 or less, or 1.

[0107] As a specific example of the organic compounds represented by general formulas (6) and (8), tetraglycidyl-3,3'-diaminodiphenylsulfone represented by the following chemical formula (3) can be cited.

[0108]

[0109] Additionally, R 21 ~R 30 At least one of them can be an organic group represented by the following general formula (9).

[0110]

[0111] In the above general formula (9), γ is an organic group. Additionally, n is 0 or 1. When n is 0, the oxygen atom in general formula (9) (the oxygen atom that does not constitute an epoxy group) is directly bonded to the carbon atom in the epoxy group. Furthermore, This indicates a bond. Regarding organic groups, the same applies as described in general formulas (1) and (2). γ can consist only of carbon and hydrogen atoms. The number of carbon atoms in γ can be, for example, 3 or less, 2 or less, or even 1.

[0112] As specific examples of organic compounds represented by general formulas (6) and (9), diglycidyl ether sulfone compounds represented by the following chemical formula (4) can be listed.

[0113]

[0114] The organic compounds of the present invention may have polymerizable functional groups such as epoxy groups. The organic compounds may be polymerized via these polymerizable functional groups. That is, the organic compounds may be oligomers having two or more but less than five identical structural units, or polymers having more than five identical structural units.

[0115] Organic compounds may have the structure shown in the following structural formula (1), the structure shown in the following structural formula (2), the structure in which at least one hydrogen atom bonded to the benzene ring of the following structural formula (1) is replaced by a group with a molecular weight of less than 50, or the structure in which at least one hydrogen atom bonded to the benzene ring of the following structural formula (2) is replaced by a group with a molecular weight of less than 50.

[0116]

[0117] (in the formula, (This represents a bond, where n is an integer from 0 to 4.)

[0118] In structural formula (1) or structural formula (2) It is bonded to other atoms. Furthermore, the organic compound may have one structure as shown in structural formula (1) or structural formula (2), or it may have two or more structures as shown in structural formula (1) or structural formula (2). In the structure shown in structural formula (1) or structural formula (2), the positional relationship between the carbon (C) and oxygen (O) bonded to one benzene ring can be ortho, meta, or para. Additionally, the organic compound may have the following structure: a structure in which at least one hydrogen atom bonded to the benzene ring of structural formula (1) or structural formula (2) is replaced by a group with a molecular weight of 50 or less (especially a group with a molecular weight of 30 or less). The group with a molecular weight of 50 or less is not particularly limited, and examples include methyl, ethyl, propyl, hydroxyl, and amino. The number of hydrogen atoms bonded to the benzene ring of structural formula (1) or structural formula (2) that are replaced by a group with a molecular weight of 50 or less (especially a group with a molecular weight of 30 or less) can be 1, 2, 3, 4, or more than 5.

[0119] Organic compounds may have the structure shown in the following structural formula (3-1), the structure shown in the following structural formula (3-2), the structure in the following structural formula (3-1) in which at least one hydrogen atom bonded to the benzene ring is replaced by a group with a molecular weight of less than 50, or the structure in the following structural formula (3-2) in which at least one hydrogen atom bonded to the benzene ring is replaced by a group with a molecular weight of less than 50.

[0120]

[0121] (in the formula, (This represents a bond.)

[0122] In structural formula (3-1) or structural formula (3-2) It is bonded to other atoms. Furthermore, the organic compound may have one structure as shown in structural formula (3-1) or structural formula (3-2), or it may have two or more structures as shown in structural formula (3-1) or structural formula (3-2). Additionally, the organic compound may have the following structure: in the case where at least one hydrogen atom bonded to the benzene ring of structural formula (3-1) or structural formula (3-2) is replaced by a group with a molecular weight of 50 or less (especially a group with a molecular weight of 30 or less). The same applies to groups with a molecular weight of 50 or less. The number of hydrogen atoms bonded to the benzene ring of structural formula (3-1) or structural formula (3-2) that are replaced by groups with a molecular weight of 50 or less (especially a group with a molecular weight of 30 or less) can be 1, 2, 3, 4, or more than 5.

[0123] Organic compounds may have the structure shown in structural formula (4-1), the structure shown in structural formula (4-2), the structure shown in structural formula (4-3), the structure in structural formula (4-1) in which at least one hydrogen atom bonded to the benzene ring is replaced by a group with a molecular weight of less than 50, the structure in structural formula (4-2) in which at least one hydrogen atom bonded to the benzene ring is replaced by a group with a molecular weight of less than 50, or the structure in structural formula (4-3) in which at least one hydrogen atom bonded to the benzene ring is replaced by a group with a molecular weight of less than 50.

[0124]

[0125] (in the formula, (This represents a bond.)

[0126] In structural formula (4-1), structural formula (4-2), or structural formula (4-3) It is bonded to other atoms. Furthermore, the organic compound may have one structure as shown in structural formula (4-1), structural formula (4-2), or structural formula (4-3), or it may have two or more structures as shown in structural formula (4-1), structural formula (4-2), or structural formula (4-3). In the structures shown in structural formula (4-1), structural formula (4-2), or structural formula (4-3), the positional relationship between sulfur (S) bonded to one benzene ring and nitrogen (N), oxygen (O), or carbon (C) can be ortho, meta, or para. Alternatively, it may have the following structure: at least one hydrogen atom bonded to the benzene ring in structural formula (4-1), structural formula (4-2), or structural formula (4-3) is replaced by a group with a molecular weight of 50 or less (especially a group with a molecular weight of 30 or less). The same applies to groups with a molecular weight of 50 or less. In the hydrogens bonded to the benzene ring of structural formula (4-1), structural formula (4-2) or structural formula (4-3), the number of hydrogens replaced by groups with a molecular weight of less than 50 (especially groups with a molecular weight of less than 30) can be 1, 2, 3, 4 or more.

[0127] The organic compounds of the present invention preferably have a high Hansen solubility parameter (HSP value). This is because it is particularly effective in preventing the degradation (oxidation) of the electrode active material caused by oxygen. The HSP value of the organic compound is, for example, 8.0 MPa. 0.5 The above can be 8.5 MPa 0.5 The above can be 9.0 MPa 0.5 The above can also be 9.5 MPa. 0.5 That's all. Among the compounds shown in chemical formulas (1) to (4) above, the compound shown in chemical formula (1) has an HSP value of 10.13 MPa. 0.5 The compound shown in chemical formula (2) has an HSP value of 11.04 MPa. 0.5 The compound represented by chemical formula (3) has an HSP value of 11.62 MPa. 0.5 The compound represented by chemical formula (4) has an HSP value of 9.94 MPa. 0.5 Furthermore, among the compounds represented by chemical formulas (5) and (6) used in the comparative examples described later, the compound represented by chemical formula (5) has an HSP value of 8.26 MPa. 0.5 The compound represented by chemical formula (6) has an HSP value of 7.33 MPa. 0.5 Furthermore, the electrode composite material may contain one or more organic compounds. The structures of the organic compounds in the electrode composite material can be identified, for example, by gas chromatography-mass spectrometry (GC-MS) or time-of-flight secondary ion mass spectrometry (TOF-SIMS).

[0128] Furthermore, the organic compound of the present invention is present in at least a portion between the electrode active material and the sulfide solid electrolyte in the electrode composite material. Thus, the organic compound of the present invention acts as a barrier, protecting the sulfide solid electrolyte. In the electrode composite material, "between the electrode active material and the sulfide solid electrolyte" is envisioned to be at least three locations: (1) a location in direct contact with both the electrode active material and the sulfide solid electrolyte; (2) a location in direct contact with one of the electrode active material and the sulfide solid electrolyte, and indirect contact with the other; (3) a location indirect contact with both the electrode active material and the sulfide solid electrolyte. Indirect contact refers to contact via conductive additives, etc., as described later. It should be noted that, as described later, when the electrode active material has an ion-conductive coating layer, the organic compound may also exist between the coating layer and the sulfide solid electrolyte. Here, the organic compound of the present invention is preferably present at least in the location described above (2). In particular, as described later, the organic compound preferably coats the sulfide solid electrolyte. Since the distance between the sulfide solid electrolyte and the organic compound becomes closer, a better barrier function is achieved. It should be noted that, since the proportion of conductive additives and binders is less than that of electrode active materials and sulfide solid electrolytes, even if organic compounds are present at the position mentioned above (3), the distance between the sulfide solid electrolyte and the organic compounds is close enough to perform the barrier function.

[0129] Organic compounds can coat the electrode active material. It should be noted that organic compounds can exist on the surface of the electrode active material. When the electrode active material has a coating layer as described later, the organic compound can exist on the surface of the coating layer opposite to the electrode active material. Furthermore, organic compounds can coat sulfide solid electrolytes. The coating percentage of the organic compound is, for example, 50% or more and 95% or less. The proportion of organic compound present between the electrode active material and the sulfide solid electrolyte, relative to the total amount of organic compound, is, for example, 10% by volume or more and 50% by volume or less. The location of the organic compound and the above proportions can be determined by microscopic observation using a SEM (scanning electron microscope) or similar method.

[0130] The proportion of organic compounds in the electrode composite material is not particularly limited, for example, it is 0.05% by mass or more and 3.0% by mass or less. Furthermore, the proportion of organic compounds relative to the sulfide solid electrolyte described later is not particularly limited, for example, it is greater than 0.50% by mass, can be 1.0% by mass or more, can be 3.0% by mass or more, or can be 5.0% by mass or more. On the other hand, the proportion of organic compounds relative to the sulfide solid electrolyte is, for example, less than 14.0% by mass, can be 13.0% by mass or less, can be 10.0% by mass or less, or can be 8.0% by mass or less.

[0131] 2. Sulfide solid electrolytes

[0132] The sulfide solid electrolyte of the present invention contains lithium, sulfur, and phosphorus. Preferably, the sulfide solid electrolyte contains sulfur (S) as the main anionic element.

[0133] Sulfide solid electrolytes may also contain element X (X is at least one of As, Sb, Si, Ge, Sn, B, Al, Ga, and In). Additionally, sulfide solid electrolytes may also contain element O and at least one of the halogen elements.

[0134] The preferred sulfide solid electrolyte is PS4 with an ortho group composition. 3- The structure is the main component of the anionic structure. This is because of its high chemical stability. PS4 3- The proportion of the structure relative to all anionic structures in the sulfide solid electrolyte is, for example, 70 mol% or more, or even 90 mol% or more.

[0135] Examples of sulfide solid electrolytes include Li₂S-P₂S₅, Li₂S-P₂S₅-LiI, Li₂S-P₂S₅-GeS₂, Li₂S-P₂S₅-Li₂O, Li₂S-P₂S₅-Li₂O-LiI, Li₂S-P₂S₅-LiBr, Li₂S-SiS₂-P₂S₅-LiI, and Li₂S-P₂S₅-Z. m S n (Where m and n are positive numbers. Z is any one of Ge, Zn, and Ga.) Li2S-SiS2-Li3PO4.

[0136] Sulfide solid electrolytes can be glass (amorphous), crystallized glass (glass ceramic), or crystalline sulfide solid electrolytes. Examples of crystalline sulfide solid electrolytes include the Thio-LISICON type, LGPS type, and steric sulfide-germanium type.

[0137] There is no particular limitation on the ionic conductivity of the sulfide solid electrolyte, but a higher conductivity is preferred. For example, the ionic conductivity at 25°C is 0.1 mS / cm or higher and 10 mS / cm or lower.

[0138] The shape of sulfide solid electrolytes can be exemplified by, for example, particulate form. The average particle size (D) of sulfide solid electrolytes... 50 For example, the particle size is greater than 0.1 μm and less than 50 μm. Average particle size (D) 50This refers to the cumulative 50% of the particle size in the volumetric particle size distribution measured by a laser diffraction particle size distribution measuring device. Furthermore, the proportion of sulfide solid electrolyte in the electrode composite material is not particularly limited, for example, it can be 8% by mass or more and 30% by mass or less.

[0139] 3. Electrode active materials

[0140] Electrode active materials can be either negative electrode active materials or positive electrode active materials.

[0141] Examples of anode active materials include Si-based, carbon-based, and Li-based active materials. Si-based active materials are preferred. Si-based active materials are active materials containing the element Si. Examples of Si-based active materials include elemental Si, Si alloys, and Si oxides. Additionally, Si-based active materials can also be Si-C composite active materials where Si exists on the surface of a carbon (C) support. Si alloys preferably contain Si as the main component. The proportion of Si in the Si alloy is, for example, 50 mol% or more, 70 mol% or more, or 90 mol% or more. On the other hand, the proportion of Si in the Si alloy is, for example, 99 mol% or less. Examples of Si alloys include Si-Al alloys, Si-Sn alloys, Si-In alloys, Si-Ag alloys, Si-Pb alloys, Si-Sb alloys, Si-Bi alloys, Si-Mg alloys, Si-Ca alloys, Si-Ge alloys, and Si-Pb alloys. Si alloys can be binary alloys or multi-component alloys (3 or more elements). Examples of Si oxides include SiO.

[0142] Furthermore, Si-based active materials can possess diamond-type crystal phases, clathrate type I crystal phases, and clathrate type II crystal phases. In clathrate type I or II crystal phases, multiple Si elements form polyhedra (cages) containing pentagons or hexagons. Because these polyhedra have spaces inside capable of trapping metal ions such as Li ions, they can suppress volume changes caused by charging and discharging.

[0143] Furthermore, Si-based active materials can contain voids within the primary particles. These voids suppress volume changes in the active material and inhibit cracking of the electrode layer (negative electrode active material layer). The porosity is not particularly limited, but can be, for example, between 4% and 40%. The presence of voids in the primary particles and the porosity can be confirmed by SEM (scanning electron microscopy).

[0144] Carbon-based active materials are inorganic active materials containing carbon (C), such as graphite, hard carbon, and soft carbon. Li-based active materials are active materials containing lithium (Li), such as elemental Li and Li alloys.

[0145] The shape of the negative electrode active material can be exemplified by, for example, particulate or layered structures. The average particle size (D) of the negative electrode active material... 50 For example, particles larger than 10 nm and smaller than 50 μm. Average particle size (D) 50 The definition of ) is as described above.

[0146] Examples of positive electrode active materials include oxide active materials. Examples of oxide active materials include: LiCoO2, LiMnO2, LiNiO2, LiVO2, and LiNi. 1 / 3 Co 1 / 3 Mn 1 / 3 O2 and other layered active substances in rock salt; LiMn2O4, Li4Ti5O 12 Li(Ni) 0.5 Mn 1.5 Spinel-type active materials such as O4; olivine-type active materials such as LiFePO4, LiMnPO4, LiNiPO4, and LiCoPO4. Among them, LiNi... 1 / 3 Co 1 / 3 Mn 1 / 3 Like O2, it is preferable to use oxide active materials that contain at least Ni and Co elements.

[0147] The shape of the positive electrode active material can be exemplified by particles or layers. The average particle size (D) of the positive electrode active material... 50 For example, particles larger than 10 nm and smaller than 50 μm. Average particle size (D) 50 As described above.

[0148] Here, the aforementioned electrode active material may have a coating layer with ion conductivity. The proportion of the electrode active material in the electrode composite material is not particularly limited, for example, it is 60% by mass or more and 90% by mass or less.

[0149] 4. Electrode composite materials

[0150] The electrode composite material may also contain at least one of a conductive additive and a binder, depending on the requirements.

[0151] Examples of conductive additives include carbon materials, metal particles, and conductive polymers. Examples of carbon materials include particulate carbon materials such as acetylene black (AB) and Ketjen black (KB), as well as fibrous carbon materials such as carbon fibers, carbon nanotubes (CNTs), and carbon nanofibers (CNFs). The proportion of the conductive additive in the electrode composite material is, for example, 0.01% by mass or more and 10% by mass or less.

[0152] Examples of binders include rubber-based binders such as butadiene rubber (BR), acrylate butadiene rubber (ABR), and styrene-butadiene rubber (SBR), as well as fluorinated binders such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE). The proportion of binder in the electrode composite material is, for example, 0.01% by mass or more and 5% by mass or less.

[0153] Furthermore, the electrolyte in the electrode composite material may include electrolytes other than the aforementioned sulfide solid electrolytes. Regarding electrolytes, those described in "2. Electrolyte Layer" below can be listed. Additionally, the electrode composite material can be either a negative electrode composite material or a positive electrode composite material.

[0154] B. Battery

[0155] Figure 2 This is a schematic cross-sectional view illustrating the battery of the present invention. Figure 2 The battery 20 shown has a positive electrode active material layer 11, a negative electrode active material layer 12, and an electrolyte layer 13 disposed between the positive electrode active material layer 11 and the negative electrode active material layer 12. Furthermore, the battery 20 has a positive electrode current collector 14 for collecting electrons from the positive electrode active material layer 11 and a negative electrode current collector 15 for collecting electrons from the negative electrode active material layer 12. In particular, in the battery 20 of the present invention, at least one of the positive electrode active material layer 11 and the negative electrode active material layer 12 contains the aforementioned electrode composite material.

[0156] According to the present invention, since at least one of the positive electrode active material layer and the negative electrode active material layer contains the above-mentioned electrode composite material, it becomes a battery in which the increase in resistance is suppressed.

[0157] 1. Positive electrode active material layer and negative electrode active material layer

[0158] The positive electrode active material layer is a layer containing at least a positive electrode active material, and preferably contains the aforementioned electrode composite material. By using the aforementioned electrode composite material, the oxidation of the sulfide solid electrolyte in the positive electrode active material layer can be effectively suppressed. Regarding the electrode composite material, the same information is described in "A. Electrode Composite Material". The thickness of the positive electrode active material layer is not particularly limited, for example, it is 0.1 μm or more and 1000 μm or less.

[0159] The negative electrode active material layer is a layer containing at least a negative electrode active material, preferably containing the aforementioned electrode composite material. By using the aforementioned electrode composite material, the reduction of sulfide solid electrolyte in the negative electrode active material layer can be effectively suppressed. Regarding the electrode composite material, the same information is described in "A. Electrode Composite Material". The thickness of the negative electrode active material layer is not particularly limited, for example, it is 0.1 μm or more and 1000 μm or less.

[0160] 2. Electrolyte layer

[0161] The electrolyte layer is a layer disposed between the aforementioned positive electrode active material layer and the aforementioned negative electrode active material layer, and is a layer containing at least the electrolyte. Additionally, the electrolyte layer may contain a binder as needed. Regarding the binder, the information is the same as described in "A. Electrode Composite Materials".

[0162] The electrolyte can be a liquid electrolyte (electrolyte) or a solid electrolyte. Generally speaking, an electrolyte layer containing a solid electrolyte is called a solid electrolyte layer, and a battery with a solid electrolyte layer is called a solid-state battery. It should be noted that a solid-state battery can be a semi-solid-state battery or an all-solid-state battery. When the solid electrolyte layer in a solid-state battery contains only the inorganic solid electrolyte described later, the aforementioned solid-state battery is called an all-solid-state battery.

[0163] Examples of electrolytes used in batteries include conventionally known electrolytes. Specifically, examples include electrolytes containing lithium salts such as LiPF6 and non-aqueous solvents such as ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC). When the electrolyte layer is present, it can be a layer in the separator impregnated with the electrolyte. The separator can be a conventionally known component.

[0164] Examples of solid electrolytes include inorganic solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, halide solid electrolytes, and complexed hydrides. Sulfide solid electrolytes are particularly preferred due to their high ionic conductivity. The information regarding sulfide solid electrolytes is the same as described in "A. Electrode Composite Materials". It should be noted that the electrolyte layer may contain a sulfide solid electrolyte that does not contain phosphorus (P). Examples of sulfide solid electrolytes that do not contain P include Li₂S-SiS₂, Li₂S-SiS₂-LiI, Li₂S-SiS₂-LiBr, Li₂S-SiS₂-LiCl, Li₂S-SiS₂-B₂S₃-LiI, Li₂S-B₂S₃, and Li₂S-SiS₂-Li. x MO y(Where x and y are positive numbers. M is any one of Si, Ge, B, Al, Ga, and In.) Oxide solid electrolytes, nitride solid electrolytes, and halide solid electrolytes typically contain oxygen (O), nitrogen (N), and halogen (X) as the main anionic elements, respectively.

[0165] In addition, organic solid electrolytes such as polymer electrolytes and gel electrolytes can also be cited as examples of solid electrolytes.

[0166] Here, the electrolyte layer may contain the sulfide solid electrolyte and organic compound described in "A. Electrode Composite Material". That is, in this invention, an electrolyte layer composite material may also be provided, which contains: a sulfide solid electrolyte containing lithium, sulfur, and phosphorus; and an organic compound, wherein the organic compound has two or more benzene rings. The electrolyte layer composite material is identical to that described in "A. Electrode Composite Material" except that it does not contain electrode active materials and conductive additives. It should be noted that, in the electrolyte layer composite material, preferably at least a portion of the organic compound is present on the surface of the sulfide solid electrolyte. The thickness of the electrolyte layer is not particularly limited, for example, it is 0.1 μm or more and 1000 μm or less.

[0167] 3. Other components

[0168] The battery of the present invention typically has a positive current collector and a negative current collector. Examples of materials used for the positive current collector include SUS, aluminum, nickel, iron, titanium, and carbon. On the other hand, examples of materials used for the negative current collector include SUS, copper, nickel, and carbon.

[0169] Furthermore, the battery of the present invention may include an outer casing that houses the aforementioned components. Examples of such outer casings include laminated outer casings and shell-type outer casings. Additionally, the battery of the present invention may include a constraint clamp that applies a constraint pressure in the thickness direction to the aforementioned components. Known clamps may be used as the constraint clamp. The constraint pressure may be, for example, 0.1 MPa or more and 50 MPa or less, or 1 MPa or more and 20 MPa or less.

[0170] 4. Battery

[0171] The battery of the present invention can be a liquid battery with an electrolyte layer containing an electrolyte, or a solid battery with an electrolyte layer containing a solid electrolyte. Furthermore, as described above, the solid battery can be a semi-solid battery or an all-solid battery.

[0172] The type of battery used in this invention is not particularly limited, but is typically a lithium-ion battery. Furthermore, the battery of this invention can be a primary battery or a secondary battery, with a secondary battery being preferred. This is because it can be repeatedly charged and discharged, making it useful, for example, as a vehicle battery.

[0173] The application of the battery of the present invention is not particularly limited, and examples include power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), battery electric vehicles (BEVs), gasoline vehicles, and diesel vehicles. In particular, it is preferably used as a power source for driving hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), or battery electric vehicles (BEVs). In addition, the battery of the present invention can be used as a power source for mobile bodies other than vehicles (e.g., rail vehicles, ships, aircraft), and can also be used as a power source for electrical products such as information processing devices.

[0174] It should be noted that this invention is not limited to the embodiments described above. The embodiments described above are illustrative, and any content that has substantially the same structure as the technical concept described in the claims of this invention and performs the same effect, regardless of its content, is included within the technical scope of this invention.

[0175] Example

[0176] [Example 1-1]

[0177] As described below, the electrode composite material of the present invention is used in the negative electrode active material layer to manufacture an evaluation battery (all-solid-state battery).

[0178] (Preparation of sulfide solid electrolytes)

[0179] Under a nitrogen atmosphere, 0.59 g of lithium sulfide, 0.95 g of phosphorus pentasulfide, 0.19 g of lithium bromide, and 0.28 g of lithium iodide were introduced into a 100 mL Schlenk flask equipped with a stirrer. After rotating the stirrer, 20 mL of a complexing agent (tetramethylethylenediamine: TMEDA) was added, and the mixture was stirred continuously for 12 hours to obtain a product containing a complex. The obtained product containing the complex was dried under vacuum at room temperature (23 °C) to obtain a powdered complex. The complex powder was then heated under vacuum at 120 °C for 2 hours to obtain an amorphous sulfide solid electrolyte. Further, the amorphous sulfide solid electrolyte was heated under vacuum at 140 °C for 2 hours to obtain a crystalline sulfide solid electrolyte. It should be noted that the ionic conductivity of the obtained crystalline sulfide solid electrolyte was measured by impedance spectroscopy (25 °C), and the result was 4.1 mS / cm.

[0180] (The production of the positive electrode)

[0181] The positive electrode active material (LiNi) 1 / 3 Co 1 / 3 Mn 1 / 380.0 g of O2, 9.51 g of the aforementioned sulfide solid electrolyte, and 2.5 g of conductive additive (VGCF; manufactured by Showa Denko) were collected into a Filmix container. Then, 32.21 g of binder (a solution containing styrene-butadiene rubber; the binder concentration in the solution is 5% by mass relative to the total solution) and solvent (tetrahydronaphthalene) were added to the Filmix container and mixed. This yielded a positive electrode slurry with a solid content concentration of 69% by mass. The positive electrode slurry was coated into a film on the surface of the positive electrode current collector (aluminum foil) using a doctor blade coating method and heated at 100°C for 30 minutes. This yielded a positive electrode having a positive electrode current collector and a positive electrode active material layer.

[0182] (Making the negative electrode)

[0183] 18.6 g of negative electrode active material (Si element), 8.69 g of the above-mentioned sulfide solid electrolyte, 0.05 g of the organic compound shown in the above chemical formula (1) (organic compound A: 9,9-bis(4-glycidoxyphenyl)fluorene) as an additive, binder (a solution containing styrene-butadiene rubber; the concentration of the binder in the solution is 5% by mass relative to the total solution) and solvent (diisobutyl ketone) were added to the Filmix container and mixed. A negative electrode slurry (negative electrode composite material) with a solid component concentration of 43% by mass was obtained. In the negative electrode slurry, the proportion of the organic compound relative to the sulfide solid electrolyte was 0.58% by mass. It should be noted that the mixing speed was set to a range of 5 m / s to 30 m / s. Furthermore, a high-shear PC impeller was used in the Filmix. The negative electrode slurry was coated into a film on the surface of the negative electrode current collector (nickel foil) using a doctor blade coating method and heated at 100°C for 30 minutes.

[0184] Thus, a negative electrode with a negative current collector and a negative active material layer is obtained.

[0185] (Fabrication of the solid electrolyte layer)

[0186] 40g of the above-mentioned sulfide solid electrolyte, 8.00g of a solution containing acrylate butadiene rubber and hexane (the concentration of acrylate butadiene rubber in the solution is 5% by mass relative to the total solution), 25.62g of heptane, and 8.00g of dibutyl ether were mixed and kneaded using an ultrasonic homogenizer. This yielded a slurry for the solid electrolyte layer. The slurry was then coated onto the surface of a substrate (aluminum foil) using a doctor blade coating method and heated at 100°C for 30 minutes. This resulted in a transfer part having a substrate and a solid electrolyte layer.

[0187] (Evaluation of battery manufacturing)

[0188] Using the aforementioned components, a laminate containing a negative electrode, a solid electrolyte layer, and a positive electrode is obtained. It should be noted that the solid electrolyte layer and the positive electrode are transferred using a pressure of 20 kN each. The resulting laminate is then pressed using a roller press. It should be noted that the pressing line pressure is set to 4 tons / cm, and the roller gap is set to 130 μm. Thus, an evaluation battery (all-solid-state battery) is manufactured. It should be noted that the battery's design capacity is set to 0.3 Ah.

[0189] [Examples 1-2 to 1-12 and Comparative Examples 1-1 to 1-7]

[0190] Except for changing the types and amounts of organic compounds as shown in Table 1 to produce the negative electrode, the evaluation battery was produced in the same manner as in Example 1-1. Organic compound B in Table 1 is 1,3-diphenyl-2,3-epoxy-1-propanone as shown in the above chemical formula (2). In addition, organic compound E in Table 1 is 5,12-dioxahexacyclohexadecane as shown in the following chemical formula (5).

[0191]

[0192] [Example 2-1]

[0193] As described below, the electrode composite material of the present invention is used in the positive electrode active material layer to manufacture an evaluation battery (all-solid-state battery).

[0194] (The production of the positive electrode)

[0195] A crystalline sulfide solid electrolyte was prepared in the same manner as in Examples 1-1. Using this sulfide solid electrolyte, a positive electrode was prepared as described below.

[0196] The positive electrode active material (LiNi) 1 / 3 Co 1 / 3 Mn 1 / 380.0 g of O2, 9.51 g of the above-mentioned sulfide solid electrolyte, 0.05 g of the organic compound (A: 9,9-bis(4-glycidoxyphenyl)fluorene) as an additive, and 2.5 g of conductive additive (VGCF; manufactured by Showa Denko) were collected into a Filmix container. Then, 32.21 g of binder (a solution containing styrene-butadiene rubber; the concentration of binder in the solution is 5% by mass relative to the total solution) and solvent (tetrahydronaphthalene) were added to the Filmix container and mixed. Thus, a positive electrode slurry with a solid component concentration of 69% by mass was obtained. In the positive electrode slurry (positive electrode composite material), the proportion of organic compound relative to the sulfide solid electrolyte is 0.53% by mass. The positive electrode slurry was coated into a film on the surface of the positive electrode current collector (aluminum foil) by a doctor blade coating method using a coater and heated at 100°C for 30 minutes. Thus, a positive electrode with a positive current collector and a positive active material layer is obtained.

[0197] (Making the negative electrode)

[0198] 18.6 g of negative electrode active material (Si elemental), 8.69 g of the aforementioned sulfide solid electrolyte, binder (a solution containing styrene-butadiene rubber; the concentration of the binder in the solution is 5% by mass relative to the total solution), and solvent (diisobutyl ketone) were added to a Filmix container and mixed. This yielded a negative electrode slurry with a solid content concentration of 43% by mass. It should be noted that the mixing speed was set to a range of 5 m / s to 30 m / s. Furthermore, a high-shear PC impeller was used in the Filmix. The negative electrode slurry was coated into a film on the surface of the negative electrode current collector (nickel foil) using a doctor blade coating method and heated at 100°C for 30 minutes. This yielded a negative electrode having a negative electrode current collector and a layer of negative electrode active material.

[0199] (Evaluation of battery manufacturing)

[0200] The evaluation battery was manufactured in the same manner as in Example 1-1, except that the positive and negative electrodes described above were used.

[0201] [Examples 2-2 to 2-12 and Comparative Examples 2-1 to 2-13]

[0202] Except for changing the type and amount of additives (organic compounds) as shown in Table 2 to produce the positive electrode, the evaluation battery was produced in the same manner as in Example 2-1. It should be noted that organic compound F in Table 2 is 2-ethylhexyl glycidyl ether as shown in the following chemical formula (6). In addition, organic compounds A, B, and E are the same as in Table 1.

[0203]

[0204] [Evaluation]

[0205] Charge-discharge tests and XPS measurements were performed on each of the all-solid-state batteries fabricated in Examples 1-1 to 1-12, Comparative Examples 1-1 to 1-7, Examples 2-1 to 2-12, and Comparative Examples 2-1 to 2-13. The details are as described below.

[0206] <Charge-Discharge Test>

[0207] Using each of the fabricated all-solid-state batteries, cycle tests were performed as described below.

[0208] First, 4 cycles of CCCV charge-discharge were performed at 0.1C with an upper limit voltage of 4.25V and a lower limit voltage of 2.87V. The resistance value after 4 cycles was measured as the initial resistance (Ω·cm 2 ). Thereafter, 100 cycles of CCCV charge-discharge were performed at 1 / 3C with an upper limit voltage of 4.25V and a lower limit voltage of 2.87V. The resistance value after 100 cycles (Ω·cm 2 ) was measured. The resistance increase rate was calculated by the following formula. The results are shown in Table 1 and Table 2. It should be noted that representative results for the evaluation cells fabricated by using the electrode composite material of the present invention in the negative electrode active material layer and the evaluation cells fabricated by using the electrode composite material in the positive electrode active material layer are summarized in Figure 3 and Figure 4 .

[0209] Resistance increase rate (%) = [(Resistance after 100 cycles - Initial resistance) / (Initial resistance)] × 100

[0210] <XPS Measurement>

[0211] XPS measurement was performed on the electrode before charge-discharge and the electrode after 100 cycles under the following conditions, and 2p spectra for S and P were acquired.

[0212] Apparatus used: Versa Probe III (manufactured by ULVAC-PHI); X-ray source used: Monochromatic Al Kα ray (hν=1486.6eV); Photoelectron emission angle: 45°; X-ray beam diameter: 100 μmΦ; Analysis position: 500 μm × 300 μm at the central portion of the sample.

[0213] For Examples 1-4, 1-9, Comparative Examples 1-1 and 1-4, the negative electrode active material layer was measured, and for each of the S element and the P element, based on PS4 3-The presence ratio was used to evaluate the degradation of sulfide solid electrolytes. Furthermore, for Examples 2-3, 2-9, 2-12, and Comparative Examples 2-4 and 2-10, the positive electrode active material layer was measured. Regarding the P element, it was based on PS4. 3- and PO x The presence ratio was used to evaluate the degradation of the sulfide solid electrolyte. The results are shown in Tables 1 and 2. Additionally, representative results for the negative electrode active material layer (results from Examples 1-4 and Comparative Examples 1-1) are summarized together with the presence ratios of other structures in... Figure 5 and Figure 6 In addition, the results for representative positive electrode active material layers (Examples 2-3 and Comparative Example 2-1) are also summarized in... Figure 7 .

[0214]

[0215] As shown in Tables 1 and 2 Figure 3 , 4 As shown, in batteries using the electrode composite material of the present invention, the rate of increase in resistance is significantly reduced. For example, as shown in Table 1, Figure 5 (a), (b) and Figure 6 As shown in (a) and (b), this is believed to be because: in the embodiments, PS4 composed of ortho-thiolated compounds... 3- Even after cycling, the proportions of Li₂S and Li₃P, as reduction products, are relatively low, thus suppressing the reduction reaction of the sulfide solid electrolyte. Similarly, as Figure 7 As shown in (a) and (b), this is believed to be because: in the embodiment, PS4 3- Even after cycling, PO2, as a product of the oxidation reaction, is adequately maintained. x The formation of sulfide solid electrolyte is suppressed, and the oxidation reaction of sulfide solid electrolyte is also suppressed. Thus, it is confirmed that as long as it is the electrode composite material of the present invention, it is possible to suppress the degradation of sulfide solid electrolyte and suppress the increase in battery resistance.

[0216] [Examples 3-1 to 3-12]

[0217] Except for changing the types and amounts of organic compounds as shown in Table 3 to produce the negative electrode, the evaluation battery was produced in the same manner as in Examples 1-1. Organic compound C in Table 3 is tetraglycidyl-3,3'-diaminodiphenyl sulfone as shown in the above chemical formula (3), and organic compound D in Table 3 is a diglycidyl ether sulfone compound as shown in the above chemical formula (4).

[0218] [Examples 4-1 to 4-12]

[0219] Except for changing the types and amounts of organic compounds as shown in Table 4 to prepare the positive electrode, the evaluation battery was prepared in the same manner as in Example 2-1. It should be noted that organic compounds C and D in Table 4 are the same as organic compounds C and D in Table 3.

[0220] [evaluate]

[0221] Charge-discharge tests and XPS measurements were performed on the all-solid-state batteries fabricated in Examples 3-1 to 3-12 and Examples 4-1 to 4-12. The specific measurement methods were the same as described above. The results are shown in Tables 3 and 4.

[0222]

[0223] As shown in Table 3 and Figure 8 As shown, the batteries prepared in Examples 3-1 to 3-12 exhibited a lower rate of increase in resistance compared to the batteries prepared in Comparative Examples 1-1 to 1-7. Furthermore, the batteries prepared in Examples 3-1 to 3-12 showed a further decrease in the rate of increase in resistance compared to the batteries prepared in Examples 1-1 to 1-12. Additionally, as shown in Table 4 and... Figure 9 As shown, the batteries prepared in Examples 4-1 to 4-12 exhibited a lower rate of increase in resistance compared to the batteries prepared in Comparative Examples 2-1 to 2-13. Furthermore, the batteries prepared in Examples 4-1 to 4-12 showed a further lower rate of increase in resistance compared to the batteries prepared in Examples 2-1 to 2-12.

[0224] Compliant with instructions

[0225] 1 …electrode active material

[0226] 2 …sulfide solid electrolytes

[0227] 3 …organic compounds

[0228] 10 …Electrode composite materials

[0229] 11 …Positive electrode active material layer

[0230] 12 …Negative electrode active material layer

[0231] 13 …electrolyte layer

[0232] 14 …Positive current collector

[0233] 15 … Negative current collector

[0234] 20 … batteries

Claims

1. An electrode composite material comprising an electrode active material, a sulfide solid electrolyte, and an organic compound, wherein the sulfide solid electrolyte contains lithium, sulfur, and phosphorus, wherein... The organic compound has two or more benzene rings. At least a portion of the organic compound is present between the electrode active material and the sulfide solid electrolyte.

2. The electrode composite material according to claim 1, wherein, The organic compound contains at least one of the compounds represented by general formula (1) or general formula (2) below. wherein R 1 and R 2 each independently is an organic group, R 3 ~R 10 each independently is a hydrogen atom or a substituent, and n is an integer of 0 to 4.

3. The electrode composite material according to claim 2, wherein, at least one of said R 1 and said R 2 is an organic group represented by the following general formula (3) In the formula, X is an organic group. Indicates a bond.

4. The electrode composite material according to claim 3, wherein, X has an epoxy group.

5. The electrode composite material according to claim 1, wherein, The organic compound contains 9,9-bis(4-glycidoxyphenyl)fluorene as shown in chemical formula (1). 。 6. The electrode composite material according to claim 1, wherein, The organic compound contains a compound represented by the following general formula (4). wherein S is an organic group, n is 0 or 1, R 11 ~R 20 each independently is a hydrogen atom or a substituent.

7. The electrode composite material according to claim 6, wherein, The S has an epoxy group.

8. The electrode composite material according to claim 7, wherein, The S is an organic group represented by the following general formula (5). In the formula, T and U are each an independent organic group, and n 1 and n 2 Each is independently either 0 or 1. Indicates a bond.

9. The electrode composite material according to claim 1, wherein, The organic compound contains 1,3-diphenyl-2,3-epoxy-1-propanone as shown in chemical formula (2). 。 10. The electrode composite material according to claim 1, wherein, The organic compound has a sulfonyl group.

11. The electrode composite material according to claim 10, wherein, The organic compound contains a compound represented by the following general formula (6). In the formula, R 21 ~R 30 Each can be an independent hydrogen atom, substituent, or organic group.

12. The electrode composite material according to claim 11, wherein, The R 21 ~The R mentioned 30 At least one of them is an organic group represented by the following general formula (7) or the following general formula (8). In the formula, α and β are each an independent organic group, and n 1 and n 2 Each is independently either 0 or 1. Indicates a bond.

13. The electrode composite material according to claim 1, wherein, The organic compound contains tetraglycidyl-3,3'-diaminodiphenyl sulfone as shown in the following chemical formula (3). 。 14. The electrode composite material according to claim 11, wherein, The R 21 ~The R mentioned 30 At least one of them is an organic group represented by the following general formula (9). In the formula, γ is an organic group, and n is 0 or 1. Indicates a bond.

15. The electrode composite material according to claim 1, wherein, The organic compound contains a diglycidyl ether sulfone compound represented by the following chemical formula (4). 。 16. The electrode composite material according to claim 1, wherein, The organic compound has the structure shown in structural formula (1), the structure shown in structural formula (2), the structure in structural formula (1) where at least one hydrogen atom bonded to the benzene ring is replaced by a group with a molecular weight of 30 or less, or the structure in structural formula (2) where at least one hydrogen atom bonded to the benzene ring is replaced by a group with a molecular weight of 30 or less. In the formula, This represents a bond, where n is an integer from 0 to 4.

17. The electrode composite material according to claim 1, wherein, The organic compound has the structure shown in structural formula (3-1), the structure shown in structural formula (3-2), the structure in structural formula (3-1) where at least one hydrogen atom bonded to the benzene ring is replaced by a group with a molecular weight of 50 or less, or the structure in structural formula (3-2) where at least one hydrogen atom bonded to the benzene ring is replaced by a group with a molecular weight of 50 or less. In the formula, Indicates a bond.

18. The electrode composite material according to claim 1, wherein, The organic compound has the structure shown in structural formula (4-1), the structure shown in structural formula (4-2), the structure shown in structural formula (4-3), the structure in structural formula (4-1) where at least one hydrogen atom bonded to the benzene ring is replaced by a group with a molecular weight of 50 or less, the structure in structural formula (4-2) where at least one hydrogen atom bonded to the benzene ring is replaced by a group with a molecular weight of 50 or less, or the structure in structural formula (4-3) where at least one hydrogen atom bonded to the benzene ring is replaced by a group with a molecular weight of 50 or less. In the formula, Indicates a bond.

19. The electrode composite material according to claim 1, wherein, The Hansen solubility parameter of the organic compound is 8.0 MPa. 0.5 above.

20. The electrode composite material according to claim 1, wherein, The proportion of the organic compound relative to the sulfide solid electrolyte is greater than 0.50% by mass and less than 14.0% by mass.

21. The electrode composite material according to claim 1, wherein, The electrode composite material is a negative electrode composite material.

22. The electrode composite material according to claim 21, wherein, The electrode active material is a Si-based active material.

23. The electrode composite material according to claim 1, wherein, The electrode composite material is a positive electrode composite material.

24. The electrode composite material according to claim 23, wherein, The electrode active material is an oxide active material containing at least Ni and Co elements.

25. A battery having a positive electrode active material layer, a negative electrode active material layer, and an electrolyte layer disposed between the positive electrode active material layer and the negative electrode active material layer, wherein, At least one of the positive electrode active material layer and the negative electrode active material layer contains the electrode composite material according to any one of claims 1 to 24.

Citation Information

Patent Citations

  • Modified sulfide solid electrolyte and method for producing same

    WO2022158458A1