Lithium-ion secondary battery negative electrode, lithium-ion secondary battery, battery module and battery pack
By controlling the porous carbon volume and deposition conditions of the silicon-carbon composite, the discharge curve of the negative electrode active material was optimized, solving the lifespan characteristics and processability problems of silicon-based active materials. This resulted in high energy density and high capacity of lithium secondary batteries, while also improving battery stability and lifespan performance.
Patent Information
- Application Number
- CN202580027889.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-10-22
- Filing Date
- 2025-08-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing silicon-based active materials for lithium secondary batteries have problems with lifespan characteristics, aqueous processability, and gas generation. In particular, when using silicon-carbon composites as anode materials, it is difficult to achieve high energy density and high capacity while improving battery life performance.
By controlling the porous carbon volume of the silicon-carbon composite, the SiH4 deposition conditions, and the coating conditions, the dQ/dV spectrum of the discharge curve of the negative electrode active material layer is kept within a specific range. This ensures that the intensity of the second peak decreases little after repeated charge-discharge cycles, thereby stably forming a stable electrolyte film and reducing particle short-circuit phenomena.
It achieves high energy density and high capacity characteristics, controls volume expansion, improves battery life performance, and ensures the aqueous processability of the negative electrode slurry and the stability of gas generation.
Smart Images

Figure CN123125692A_ABST
Abstract
Description
Technical Field
[0001] This application claims priority and benefit to Korean Patent Application No. 10-2024-0145065, filed on October 22, 2024, with the Korean Intellectual Property Office, the entire contents of which are incorporated herein by reference.
[0002] This application relates to a negative electrode for a lithium secondary battery, a lithium secondary battery, a battery module, and a battery pack. Background Technology
[0003] As the use of fossil fuels increases rapidly, the demand for alternative or clean energy sources is growing, and as part of this trend, the field of power generation and energy storage utilizing electrochemical reactions has become one of the most active areas of research.
[0004] Recently, with the rapid proliferation of battery-powered electronic devices such as mobile phones, laptops, electric vehicles, power tools, and cleaners, the demand for small, lightweight, and relatively high-capacity and / or high-output secondary batteries is increasing rapidly. In particular, lithium-ion batteries have attracted significant attention as a power source for electronic devices due to their light weight and high energy density. Therefore, research and development efforts are actively underway to improve the performance of lithium-ion batteries.
[0005] When lithium ions are inserted / deintercalated in positive and negative electrodes containing active materials capable of inserting and deintercalating lithium ions, and an organic or polymer electrolyte is filled between the positive and negative electrodes, a lithium secondary battery generates electrical energy through oxidation and reduction reactions.
[0006] Metal oxides such as LiCoO2, LiMnO2, LiMn2O4, or LiNiO2 have been used as positive electrode active materials for lithium-ion batteries. Carbon-based materials such as lithium metal, graphite, or activated carbon, and silicon oxides (SiO2) have been used as negative electrode active materials. x Materials such as lithium metal and lithium oxide are used in the early stages of the negative electrode active materials. However, with charge-discharge cycles, lithium atoms grow on the surface of the lithium metal, damaging the separator and ultimately destroying the battery. Therefore, carbon-based materials have been mainly used in recent years.
[0007] Graphite is primarily used as the negative electrode active material in lithium-ion batteries. However, graphite has a low capacity per unit mass of 372 mAh / g, making it difficult to achieve high capacity in lithium-ion batteries. Therefore, to achieve high capacity in lithium-ion batteries, non-carbon-based negative electrode materials with higher energy densities than graphite, such as silicon, tin, and their oxides, are being developed. Although these non-carbon-based negative electrode materials have high capacity, they suffer from low initial efficiency. Consequently, they exhibit high lithium consumption and significant irreversible capacity loss during the initial charge and discharge periods.
[0008] Therefore, methods are being researched to achieve high capacity and improved energy density by applying carbon-based active materials, or to ensure energy density, capacity, and lifetime performance by appropriately combining silicon-based and carbon-based active materials. However, a negative electrode for lithium-ion batteries that can solve the above problems has not yet been developed.
[0009] In particular, research is underway on silicon-carbon composites as next-generation silicon-based active materials. These materials are known to be suitable for high-energy-density lithium-ion batteries due to their high capacity and efficiency. However, silicon-carbon composites continue to be troubled by issues related to lifetime characteristics, aqueous processability, and gas generation when used in combination with aqueous binders.
[0010] Therefore, there is a need to develop a negative electrode that can effectively improve battery life characteristics and achieve fast charging performance and high energy density while using silicon-based and / or carbon-based active materials.
[0011] <List of References>
[0012] Japanese Patent Application Publication No. 2009-080971 Summary of the Invention
[0013] Technical issues
[0014] This application relates to a negative electrode for lithium-ion batteries, which addresses problems associated with silicon-based active materials in the relevant field, such as lifetime characteristics and aqueous processability and gas generation related to the use of aqueous binders. Specifically, it has been found that the aforementioned problems can be solved when the dQ / dV spectrum of the discharge curve shape of the negative electrode comprising a silicon-carbon composite used as a silicon-based active material falls within a specific range. Therefore, this application relates to a negative electrode for lithium-ion batteries, a lithium-ion battery, a battery module, and a battery pack that can ensure high energy density and high capacity as well as improved lifetime characteristics.
[0015] Technical solution
[0016] An exemplary embodiment of this specification provides a negative electrode for a lithium secondary battery, the negative electrode comprising: a negative electrode current collector layer; and a negative electrode active material layer disposed on one or both surfaces of the negative electrode current collector layer, wherein the negative electrode active material layer contains a negative electrode active material layer composition comprising a silicon-carbon composite, the negative electrode comprising a first peak in the range of 0.25 V to 0.35 V and a second peak in the range of 0.42 V to 0.48 V in the dQ / dV spectrum of the discharge curve shape, and when lithium metal is used as the counter electrode of the negative electrode for the lithium secondary battery, after N charge-discharge cycles, for the first peak (Nth cycle) and the second peak (Nth cycle), the second peak (Nth cycle) satisfies Equation 1: [Formula 1] [(Second peak (first cycle) - Second peak (second cycle)) / Second peak (first cycle)] × 100%≤ 10.
[0017] An exemplary embodiment of this application provides a lithium secondary battery comprising: a positive electrode; a negative electrode for a lithium secondary battery according to an exemplary embodiment of this application; a separator disposed between the positive electrode and the negative electrode; and an electrolyte.
[0018] An exemplary embodiment of this application provides a battery module that includes the lithium secondary battery.
[0019] Finally, a battery pack is provided, which includes the lithium secondary battery or the battery module.
[0020] Beneficial effects
[0021] In the development of automotive batteries, high energy density and high capacity are crucial for improving driving performance. To meet these performance requirements, silicon-carbon composites are used as the negative electrode active material. However, this leads to lifespan issues due to volume expansion and stability problems with the negative electrode slurry.
[0022] In the case of the negative electrode for a lithium secondary battery according to this application, the negative electrode active material comprises a silicon-carbon composite, and the negative electrode includes a first peak in the range of 0.25 V to 0.35 V and a second peak in the range of 0.42 V to 0.48 V in the dQ / dV spectrum of the discharge curve shape. When lithium metal is used as the counter electrode of the negative electrode for the lithium secondary battery, after repeating N charge-discharge cycles, for the first peak (Nth cycle) and the second peak (Nth cycle), the second peak (Nth cycle) satisfies Equation 1.
[0023] That is, when the total volume of porous carbon, SiH4 deposition conditions and coating conditions are controlled during the manufacture of the silicon-carbon composite, as described above, the dQ / dV spectrum of the discharge curve shape of the negative electrode can satisfy the range of Equation 1. In particular, the silicon-carbon composite is characterized in that the intensity of the second peak decreases slightly in the second cycle after the first cycle.
[0024] When using silicon-carbon composites with the aforementioned properties, high energy density and high capacity can be achieved, and volume expansion can be controlled to improve lifetime performance. In particular, it has the ability to control the aqueous processability of the negative electrode slurry and gas generation, thereby ensuring lifetime performance.
[0025] The silicon-carbon composite satisfying Formula 1 is the result of minimizing the amount of silicon deposited on the porous carbon surface while uniformly depositing silicon within the pores of the porous carbon, thereby ensuring lifetime performance by relatively stably forming SEI during charge and discharge and reducing electrical short-circuiting of particles. Attached Figure Description
[0026] Figure 1 This is a view showing a stacked structure of a negative electrode for a lithium secondary battery according to an exemplary embodiment of this application.
[0027] Figure 2 This is a view showing a stacked structure of a lithium secondary battery according to an exemplary embodiment of this application.
[0028] Figure 3 This is a graph showing the dQ / dV peaks according to Embodiment 1 of this application.
[0029] Figure 4 This is a graph that appears during the process of deriving the dQ / dV peaks according to Embodiment 1 of this application.
[0030] Figure 5 This is a graph showing the dQ / dV peaks of Comparative Example 1 according to this application.
[0031] <Symbol Explanation>
[0032] 10: Negative electrode current collector layer
[0033] 20: Negative electrode active material layer
[0034] 30: Diaphragm
[0035] 40: Positive electrode active material layer
[0036] 50: Positive current collector layer
[0037] 100: Negative electrode for lithium secondary batteries
[0038] 200: Positive electrode for lithium secondary batteries Detailed Implementation
[0039] Before describing the present invention, some terms will be defined.
[0040] As used herein, when a component is described as "comprising," "including," or "having" a constituent element, unless otherwise specifically described, this does not mean that other constituent elements are excluded, but rather that other constituent elements may be included.
[0041] In this specification, "p to q" refers to the range of "p and below q".
[0042] In this specification, "specific surface area" is measured by the BET method, specifically calculated by using the BELSORP-mini II, which is available from BEL Japan, based on the amount of nitrogen adsorbed at liquid nitrogen temperature (77K). That is, in this application, BET specific surface area can refer to the specific surface area measured by the above-described method.
[0043] In this specification, "Dn" refers to the particle size distribution, specifically the particle size at the n% point in the cumulative number distribution of particles according to particle size. That is, D50 is the particle size (average particle size) at the 50% point in the cumulative number distribution of particles according to particle size, D90 is the particle size at the 90% point, and D10 is the particle size at the 10% point. Note that the particle size distribution can be measured using laser diffraction. Specifically, after dispersing the powder to be tested in a dispersion medium, the resulting dispersion is introduced into a commercially available laser diffraction particle size measurement device (e.g., Microtrac S3500), where the difference in diffraction pattern according to particle size is measured as the laser beam passes through the particles, and then the particle size distribution is calculated.
[0044] As used herein, describing a polymer as containing a specific monomer as a monomeric unit means that the monomer participates in the polymerization reaction and is included in the polymer as a repeating unit. As used herein, when describing a polymer as containing a monomer, this is interpreted in the same way as when the polymer contains a monomer as a monomeric unit.
[0045] In this specification, it should be understood that, unless otherwise specified as “homogeneous polymer”, the term “polymer” is used in a broad sense, including copolymers.
[0046] As used herein, weight-average molecular weight (Mw) and number-average molecular weight (Mn) are converted molecular weights of polystyrene measured by gel permeation chromatography (GPC) using commercially available monodisperse polystyrene polymers with different degrees of polymerization (standard samples) as reference materials. Unless otherwise specified, molecular weight as used herein refers to weight-average molecular weight.
[0047] Exemplary embodiments of the present invention will be described in detail below with reference to the accompanying drawings, enabling those skilled in the art to readily implement the invention. However, the present invention can be implemented in many different forms and is not limited to the following description.
[0048] An exemplary embodiment of this specification provides a negative electrode for a lithium secondary battery, the negative electrode comprising: a negative electrode current collector layer; and a negative electrode active material layer disposed on one or both surfaces of the negative electrode current collector layer, wherein the negative electrode active material layer contains a negative electrode active material layer composition comprising a silicon-carbon composite, the negative electrode including a first peak in the range of 0.25 V to 0.35 V and a second peak in the range of 0.42 V to 0.48 V in the dQ / dV spectrum of the discharge curve shape, when lithium metal is used as the counter electrode of the negative electrode for the lithium secondary battery, after N charge-discharge cycles, for the first peak (Nth cycle) and the second peak (Nth cycle), the second peak (Nth cycle) satisfies Equation 1: [Formula 1] [(Second peak (first cycle) - Second peak (second cycle)) / Second peak (first cycle)] × 100%≤ 10.
[0049] When using silicon-carbon composites with the aforementioned properties, high energy density and high capacity can be achieved, and volume expansion can be controlled to improve lifetime performance. In particular, it has the ability to control the aqueous processability of the negative electrode slurry and gas generation, thereby ensuring lifetime performance.
[0050] Figure 1 This is a view illustrating a stacked structure of a negative electrode for a lithium secondary battery according to an exemplary embodiment of this application. Specifically, a negative electrode 100 for a lithium secondary battery is visible, which includes a negative electrode active material layer 20 on one surface of a negative electrode current collector layer 10. Figure 1 It is shown that a negative electrode active material layer is formed on one surface of the negative electrode current collector layer, but a negative electrode active material layer can be formed on both surfaces of the negative electrode current collector layer.
[0051] This will be described in more detail below.
[0052] In one exemplary embodiment of this application, the thickness of the negative electrode current collector layer is typically from 1 μm to 100 μm, specifically from 8 μm to 15 μm. There are no particular limitations on such a negative electrode current collector layer, as long as it has high conductivity without causing chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, sintered carbon, copper or stainless steel with surfaces treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloys, etc., can be used. Furthermore, the negative electrode current collector layer can have fine irregularities formed on its surface to enhance the adhesion of the negative electrode active material, and can be used in various forms, such as films, sheets, foils, meshes, porous bodies, foams, or nonwoven fabrics.
[0053] In one exemplary embodiment of this application, the thickness of the negative electrode current collector layer can be more than 1 μm and less than 100 μm.
[0054] However, the thickness can be modified in various ways depending on the type and purpose of the negative electrode used, and is not limited thereto.
[0055] According to an exemplary embodiment of this application, the negative electrode active material layer comprises a negative electrode active material layer composition including a negative electrode active material, and said negative electrode active material comprises a silicon-carbon composite.
[0056] In one exemplary embodiment of this application, the silicon-carbon composite may be represented as Si / C.
[0057] In this specification, the silicon-carbon composite is a composite of Si and C, and is distinct from silicon carbide (denoted as SiC). Silicon carbide does not undergo electrochemical reactions with lithium, therefore all properties, including lifetime, may be measured as zero.
[0058] The silicon-carbon composite can be a composite of silicon, graphite, etc., and can form a structure in which a core composed of silicon, graphite, etc., is surrounded by graphene, amorphous carbon, etc. In the silicon-carbon composite, the silicon can be nano-silicon. For example, the nano-silicon can be silicon in the range of 1 nm to 999 nm.
[0059] In one exemplary embodiment of this application, a negative electrode for a lithium secondary battery is provided, wherein the content of the negative electrode active material is 90 parts by weight or less relative to 100 parts by weight of the negative electrode active material layer composition.
[0060] In another exemplary embodiment, the content of the negative electrode active material relative to 100 parts by weight of the negative electrode active material layer composition may be 90 parts by weight or less, specifically 85 parts by weight or less, and may be 50 parts by weight or more, preferably 70 parts by weight or more.
[0061] In one exemplary embodiment of this application, a negative electrode for a lithium secondary battery is provided, wherein the content of the silicon-carbon composite is 50 parts by weight or less relative to 100 parts by weight of the negative electrode active material.
[0062] In another exemplary embodiment, the content of the silicon-carbon composite relative to 100 parts by weight of the negative electrode active material can be more than 1 part by weight and less than 50 parts by weight, specifically more than 5 parts by weight and less than 45 parts by weight, and more specifically more than 10 parts by weight and less than 35 parts by weight.
[0063] By including a negative electrode active material within this specific range, the capacity characteristics and energy density of the negative electrode can be ensured. In other words, increasing the content of the silicon-carbon composite improves energy density, but degrades lifetime characteristics due to more severe volume expansion. Conversely, if the content of the silicon-carbon composite is low, neither high energy density nor fast charging performance can be ensured. Therefore, when the content falls within this specific range, high energy density can be ensured while improving fast charging performance.
[0064] Note that the average particle size (D50 particle size) of the silicon-carbon composite of the present invention can be 1 μm or more and 10 μm or less, specifically 2 μm to 8 μm, and more specifically 3 μm to 8 μm. When the average particle size falls within this specific range, the specific surface area of the particles falls within a suitable range, resulting in a viscosity of the formed negative electrode slurry within an appropriate range. Therefore, the particles constituting the negative electrode slurry are dispersed smoothly. Furthermore, the size of the silicon-carbon composite is equal to or greater than the lower limit of this specific range. Due to the composite consisting of conductive materials and binders, the contact area between silicon particles and conductive materials in the negative electrode slurry is excellent, which increases the possibility of maintaining the conductive network and thus improves the capacity retention rate. Note that when the average particle size falls within this specific range, excessively large silicon particles are excluded, resulting in the formation of a smooth negative electrode surface. Therefore, it is possible to prevent uneven current density during charging and discharging.
[0065] Furthermore, in one exemplary embodiment of this application, the silicon-carbon composite may not contain particles with a particle size of less than 1 μm. Specifically, the silicon-carbon composite may contain particles with a particle size of 1 μm or more and 10 μm or less, and the content of particles with a particle size of less than 1 μm may be less than 1 part by weight, specifically less than 0.1 parts by weight, relative to 100 parts by weight of the silicon-carbon composite particles. That is, the silicon-carbon composite according to an exemplary embodiment of this application is characterized by not containing fine particles.
[0066] In one exemplary embodiment of this application, the silicon-carbon composite typically has a characteristic BET specific surface area. The BET specific surface area of the silicon-based active material is preferably 0.1 to 5 m².2 / g, more preferably 0.1 to 4.5 m 2 / g, particularly preferably 0.2 to 4 m 2 / g, with the most preferred value being 0.2 to 3.5 m 2 / g. BET specific surface area is measured according to DIN 66131 (using nitrogen).
[0067] In one exemplary embodiment of this application, the silicon-carbon composite may exist, for example, in crystalline or amorphous form, and is preferably not porous. The silicon particles are preferably spherical or fragmented particles. Alternatively, but less preferably, the silicon particles may also have a fibrous structure or exist in the form of a silicon-containing film or coating.
[0068] In one exemplary embodiment of this application, the silicon-carbon composite may have a non-spherical shape and its sphericity (circularity) is, for example, less than 0.9, such as 0.7 to 0.9, such as 0.8 to 0.9, such as 0.85 to 0.9.
[0069] In one exemplary embodiment of this application, the circularity is determined by the following formula 1-A, where A is the area and P is the total length of the boundary line.
[0070] [Equation 1-A]
[0071] 4πA / P 2
[0072] In one exemplary embodiment of this application, a negative electrode for a lithium secondary battery is provided, wherein the negative electrode active material further comprises a carbon-based active material.
[0073] In one exemplary embodiment of the present invention, the carbon-based active material may include artificial graphite and natural graphite.
[0074] In one exemplary embodiment of this application, the negative electrode active material is provided, wherein, based on the carbon-based active material, the weight ratio of natural graphite to artificial graphite is 5:95 or more and 50:50 or less.
[0075] In another exemplary embodiment, based on the carbon-based active material, the weight ratio of natural graphite to artificial graphite can fall within the range of 5:95 or more and 50:50 or less, preferably 7:93 to 45:55, and more preferably 10:90 to 40:60.
[0076] In one exemplary embodiment of this application, the carbon-based active material comprises graphite, and in the case of graphite, it may include both artificial and natural graphite. Artificial graphite has been confirmed to have superior battery characteristics compared to natural graphite. Therefore, the use of natural graphite is reduced while the use of artificial graphite is increased. However, from a cost perspective, artificial graphite results in high processing costs because the coke requires calcination and graphitization. In this regard, when this specific range is met, battery characteristics are improved while the cost issue is addressed.
[0077] In one exemplary embodiment of this application, natural graphite is characterized by satisfying the range of Formula 1.
[0078] In one exemplary embodiment of this application, the average particle size (D50) of natural graphite can be 10 μm or more and 30 μm or less, the tap density of natural graphite can be 0.5 g / cc or more and 2.0 g / cc or less, and the specific surface area of natural graphite can be 1 m². 2 / g or more and 5 m 2 / g or less.
[0079] In another exemplary embodiment, the average particle size (D50) of natural graphite can be 10 μm or more and 30 μm or less, specifically 12 μm or more and 27 μm or less, and more specifically 15 μm or more and 20 μm or less.
[0080] In another exemplary embodiment, the tap density of natural graphite may be 0.5 g / cc or more and 2.0 g / cc or less, specifically 0.7 g / cc or more and 1.5 g / cc or less, and more specifically 0.9 g / cc or more and 1.2 g / cc or less.
[0081] In another exemplary embodiment, the specific surface area of natural graphite can be 1 m². 2 / g or more and 5 m 2 Below / g, specifically 1 m 2 / g or more and 4 m 2 / g or less, more specifically 1 m 2 / g or more and 3 m 2 / g or less.
[0082] In one exemplary embodiment of this application, the average particle size (D50) of the artificial graphite can be 10 μm or more and 25 μm or less, the tap density of the artificial graphite can be 0.5 g / cc or more and 1.5 g / cc or less, and the specific surface area of the artificial graphite can be 0.1 m². 2 / g or more and 3.0 m 2 / g or less.
[0083] In another exemplary embodiment, the average particle size (D50) of the artificial graphite can be 10 μm or more and 25 μm or less, specifically 12 μm or more and 24 μm or less, and more specifically 14 μm or more and 23 μm or less.
[0084] In another exemplary embodiment, the tap density of the artificial graphite may be 0.5 g / cc or more and 1.5 g / cc or less, specifically 0.7 g / cc or more and 1.3 g / cc or less, and more specifically 0.9 g / cc or more and 1.1 g / cc or less.
[0085] In another exemplary embodiment, the specific surface area of the artificial graphite can be 0.1 m². 2 / g or more and 3.0 m 2 / g or less, specifically 0.2 m 2 / g or more and 2.5 m 2 / g or less, more specifically 0.2 m 2 / g or more and 2.5 m 2 / g or less.
[0086] In related technologies, graphite-based compounds are typically used as the negative electrode active material. However, in recent years, with the increasing demand for high-capacity batteries, there has been an increasing trend of using silicon-based compounds in combination to increase capacity. However, silicon-based compounds have the following limitations: their volume expands rapidly during charge and discharge, which damages the conductive paths formed in the negative electrode active material layer, thereby degrading battery performance.
[0087] Therefore, in one exemplary embodiment of this application, a negative electrode for a lithium secondary battery is provided, wherein the negative electrode active material layer composition further comprises a negative electrode conductive material and a negative electrode binder.
[0088] In one exemplary embodiment of this application, the negative electrode conductive material used can be any material commonly used in the art without limitation. Specifically, it can include one or more materials selected from the group consisting of point conductive materials, planar conductive materials and linear conductive materials.
[0089] In one exemplary embodiment of this application, the dot-shaped conductive material refers to a conductive material that can be used to improve the conductivity of the negative electrode, has conductivity without causing chemical changes, and has a dot-shaped or spherical shape. Specifically, the dot-shaped conductive material may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal cracking black, conductive fibers, fluorocarbons, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and preferably includes carbon black for high conductivity and excellent dispersibility.
[0090] In one exemplary embodiment of this application, the BET specific surface area of the dot-shaped conductive material can be 40m². 2 / g or more and 70 m 2 / g or less, preferably 45 m 2 / g or more and 65 m 2 / g or less, preferably 50 m 2 / g or more and 60m 2 / g or less.
[0091] In one exemplary embodiment of this application, the particle size of the dot-shaped conductive material can be from 10 nm to 100 nm, preferably from 20 nm to 90 nm, and more preferably from 20 nm to 60 nm.
[0092] In one exemplary embodiment of this application, the negative electrode conductive material may include a planar conductive material.
[0093] The planar conductive material can be used to improve conductivity by increasing the surface contact between silicon particles in the negative electrode, while suppressing the breakage of the conductive path caused by volume expansion, and can be represented as a plate-shaped conductive material or a block-shaped conductive material.
[0094] In one exemplary embodiment of this application, the planar conductive material may include at least one selected from the group consisting of plate graphite, graphene, graphene oxide and graphite flakes, and preferably plate graphite.
[0095] In one exemplary embodiment of this application, the average particle size (D50) of the planar conductive material can be 2 to 7 μm, specifically 3 to 6 μm, and more specifically 4 to 5 μm. When this specific range is met, sufficient particle size results in easy dispersion without causing an excessive increase in the viscosity of the negative electrode slurry. Therefore, the dispersion effect is excellent when the same equipment and time are used for dispersion.
[0096] In one exemplary embodiment of this application, the negative electrode composition is provided, wherein the planar conductive material has a D10 of 0.5 μm or more and 1.5 μm or less, a D50 of 2.5 μm or more and 3.5 μm or less, and a D90 of 7.0 μm or more and 15.0 μm or less.
[0097] In one exemplary embodiment of this application, the planar conductive material can be a high specific surface area planar conductive material with a high BET specific surface area or a low specific surface area planar conductive material.
[0098] In one exemplary embodiment of this application, the planar conductive material can be used without limitation either a high specific surface area planar conductive material or a low specific surface area planar conductive material. However, in particular, the planar conductive material according to one exemplary embodiment of this application may be affected to some extent by the dispersion effect in terms of electrode performance, thus a low specific surface area planar conductive material that does not cause dispersion problems is particularly preferred.
[0099] In one exemplary embodiment of this application, the BET specific surface area of the planar conductive material can be 5m². 2 / g or more.
[0100] In another exemplary embodiment, the BET specific surface area of the planar conductive material can be 5 m². 2 / g or more and 500 m 2 / g or less, preferably 5 m 2 / g or more and 300 m 2 / g or less, preferably 5 m 2 / g or more and 250 m 2 / g or less.
[0101] In another exemplary embodiment, the planar conductive material is a high specific surface area planar conductive material, and the BET specific surface area can fall within 50 m². 2 / g or more and 500 m 2 In the range of / g or less, 80 m is preferred. 2 / g or more and 300m 2 / g or less, more preferably 100 m 2 / g or more and 300 m 2 / g or less.
[0102] In another exemplary embodiment, the planar conductive material is a low specific surface area planar conductive material, and the BET specific surface area can fall within 5 m². 2 / g or more and 40 m 2 In the range of / g or less, 5 m is preferred. 2 / g or more and 30 m 2 / g or less, preferably 5 m 2 / g or more and 25 m 2 / g or less.
[0103] Other conductive materials may include linear conductive materials, such as carbon nanotubes. The carbon nanotubes may be bundled carbon nanotubes. A bundled carbon nanotube may comprise multiple carbon nanotube units. Specifically, unless otherwise specified, the term "bundled" herein refers to a secondary shape resembling a bundle or rope, wherein multiple carbon nanotube units are arranged side-by-side or entangled with substantially the same orientation along their longitudinal axes. The carbon nanotube units have cylindrical graphite sheets with nanometer-scale diameters and sp2 bonding structures. In this case, depending on the curl angle and structure of the graphite sheets, the properties of a conductive or semiconductor material can be exhibited. Compared to wound carbon nanotubes, bundled carbon nanotubes can be more uniformly dispersed during the fabrication of the negative electrode and can form a conductive network more smoothly in the negative electrode, thereby improving the conductivity of the negative electrode.
[0104] In particular, the linear conductive material according to an exemplary embodiment of this application may be a single-walled carbon nanotube (SWCNT).
[0105] Single-walled carbon nanotubes are tubular materials in which carbon atoms are arranged in a hexagonal pattern. Depending on their unique chirality, they exhibit non-conductor, conductor, or semiconductor properties. Because the carbon atoms are connected by strong covalent bonds, their tensile strength is more than 100 times that of steel. They also have excellent flexibility and elasticity, and are chemically stable.
[0106] The average diameter of the single-walled carbon nanotubes is 0.5 nm to 15 nm. According to an exemplary embodiment of the invention, the average diameter of the single-walled carbon nanotubes can be 1 to 10 nm, or 1 nm to 5 nm, or 1 nm to 2 nm. When the average diameter of the single-walled carbon nanotubes falls within this specific range, the conductivity of the negative electrode can be maintained even with very low concentrations of single-walled carbon nanotubes, and the desired viscosity and solids content can be obtained during the preparation of the conductive material dispersion. In the conductive material dispersion, the single-walled carbon nanotubes aggregate with each other and may therefore exist in an entangled state (aggregates). Therefore, after confirming the diameter of any entangled single-walled carbon nanotube aggregates extracted from the conductive material dispersion by SEM or TEM, the average diameter can be obtained by dividing the diameter of the aggregate by the number of single-walled carbon nanotubes constituting the aggregate.
[0107] The BET specific surface area of the aforementioned single-walled carbon nanotubes can be 500 m². 2 / g to 1,500 m 2 / g or 900 m 2 / g to 1,200 m 2 / g, specifically 250 m 2 / g to 330 m 2 / g. When the above range is met, a conductive material dispersion with a preferred solids content is obtained, and excessive increase in the viscosity of the negative electrode slurry is prevented. The BET specific surface area can be measured by the nitrogen adsorption BET method.
[0108] The aspect ratio of single-walled carbon nanotubes can range from 50 to 20,000, or the length can range from 5 to 100 μm or 5 to 50 μm. When the aspect ratio or length falls within such ranges, the specific surface area is high, allowing single-walled carbon nanotubes in the negative electrode to be adsorbed onto the active material particles by strong attraction. Therefore, the conductive network can be stably maintained even during the volume expansion of the negative electrode active material. When observing single-walled carbon nanotube powder by SEM, the aspect ratio can be confirmed by obtaining the average aspect ratio of 15 single-walled carbon nanotubes with a large aspect ratio and 15 single-walled carbon nanotubes with a small aspect ratio.
[0109] Because single-walled carbon nanotubes have a larger aspect ratio than multi-walled and double-walled carbon nanotubes, they are longer and larger in volume, thus having the advantage of being able to construct electrical networks even with only a small amount.
[0110] In one exemplary embodiment of this application, the content of the negative electrode conductive material may be more than 1 part by weight and less than 30 parts by weight relative to 100 parts by weight of the negative electrode active material layer composition.
[0111] In another exemplary embodiment, the content of the negative electrode conductive material relative to 100 parts by weight of the negative electrode active material layer composition may be more than 1 part by weight and less than 30 parts by weight, preferably more than 5 parts by weight and less than 25 parts by weight, and more preferably more than 10 parts by weight and less than 15 parts by weight.
[0112] In one exemplary embodiment of this application, the negative electrode conductive material may include dot-shaped conductive material, planar conductive material and linear conductive material, and the dot-shaped conductive material, the planar conductive material and the linear conductive material may satisfy a ratio of 1:1:0.01 to 1:1:1.
[0113] In one exemplary embodiment of this application, the content of the dot-shaped conductive material may be more than 1 part by weight and less than 60 parts by weight relative to 100 parts by weight of the negative electrode conductive material, preferably more than 5 parts by weight and less than 50 parts by weight, and more preferably more than 10 parts by weight and less than 50 parts by weight.
[0114] In one exemplary embodiment of this application, the content of the planar conductive material relative to 100 parts by weight of the negative electrode conductive material can be more than 1 part by weight and less than 60 parts by weight, preferably more than 5 parts by weight and less than 50 parts by weight, and more preferably more than 10 parts by weight and less than 50 parts by weight.
[0115] In one exemplary embodiment of this application, the content of the linear conductive material relative to 100 parts by weight of the negative electrode conductive material can be 0.01 parts by weight or more and 10 parts by weight or less, preferably 0.05 parts by weight or more and 8 parts by weight or less, and more preferably 0.1 parts by weight or more and 5 parts by weight or less.
[0116] In one exemplary embodiment of this application, the negative electrode conductive material may include linear conductive materials and planar conductive materials.
[0117] In one exemplary embodiment of this application, the negative electrode conductive material may comprise linear conductive material and planar conductive material, and the ratio of the linear conductive material to the planar conductive material may fall within the range of 0.01:1 to 0.1:1.
[0118] In an exemplary embodiment of this application, since the negative electrode conductive material specifically includes the linear conductive material and the planar conductive material, and satisfies the above composition and proportion respectively, it does not significantly affect the life characteristics of existing lithium secondary batteries, and increases the number of chargeable and dischargeable sites, thereby achieving excellent output characteristics at high C-rate.
[0119] In one exemplary embodiment of this application, the negative electrode conductive material may be composed of a linear conductive material.
[0120] In this case, the content of the linear conductive material can be 0.01 to 2 parts by weight, 0.02 to 0.7 parts by weight, or 0.02 to 0.3 parts by weight relative to 100 parts by weight of the negative electrode active material layer composition. When the content of the linear conductive material falls within this specific range, an electrical network can be sufficiently constructed in the negative electrode active material layer, which is advantageous in terms of mixing and coating processability in electrode manufacturing.
[0121] The negative electrode conductive material according to an exemplary embodiment of this application has a completely different structure from the positive electrode conductive material applied to the positive electrode. That is, the negative electrode conductive material according to an exemplary embodiment of this application is used to maintain contact between silicon-based active materials that expand significantly in electrode volume due to charging and discharging, while the positive electrode conductive material is used to impart a certain conductivity and to act as a buffer during rolling. In terms of structure and function, it is completely different from the negative electrode conductive material of this invention.
[0122] In one exemplary embodiment of this application, the negative electrode adhesive may comprise at least one selected from the group consisting of: polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, polyacrylic acid, and the above materials wherein hydrogen is replaced by Li, Na, Ca, etc., and may also comprise various copolymers thereof.
[0123] According to an exemplary embodiment of this application, the negative electrode adhesive is used to support the active material and the conductive material to prevent distortion and structural deformation of the negative electrode structure during the volume expansion and mitigation of the negative electrode active material. When the above-mentioned effects are satisfied, all common adhesives can be applied; specifically, water-based adhesives can be used, and more specifically, polyacrylamide (PAM) based adhesives can be used.
[0124] In one exemplary embodiment of this application, the content of the negative electrode adhesive may be less than 30 parts by weight, preferably less than 25 parts by weight, more preferably less than 20 parts by weight, and may be more than 5 parts by weight or more than 10 parts by weight, relative to 100 parts by weight of the negative electrode active material layer composition.
[0125] In one exemplary embodiment of this application, a negative electrode slurry is provided, the negative electrode slurry comprising the negative electrode active material layer composition and a negative electrode slurry solvent.
[0126] In one exemplary embodiment of this application, the solid content of the negative electrode slurry may fall within the range of 10% to 40%.
[0127] For the slurry solvent, any solvents used in the art can be used without limitation; specifically, water can be used.
[0128] In one exemplary embodiment of this application, the negative electrode slurry may be coated on one or both surfaces of the negative electrode current collector layer to form a negative electrode active material layer. In this case, any coating method known in the art can be used without limitation.
[0129] In one exemplary embodiment of this application, a negative electrode for a lithium secondary battery is provided, wherein the negative electrode includes a first peak in the range of 0.25 V or higher and 0.35 V or lower and a second peak in the range of 0.42 V or higher and 0.48 V or lower in the dQ / dV spectrum of the discharge curve shape. When lithium metal is used as the counter electrode of the negative electrode for the lithium secondary battery, after N charge-discharge cycles, for the first peak (Nth cycle) and the second peak (Nth cycle), the second peak (Nth cycle) satisfies Equation 1 above.
[0130] In one exemplary embodiment of this application, Equation 1 can satisfy [(second peak (first cycle) - second peak (second cycle)) / second peak (first cycle)] × 100% ≤ 10, specifically, [(second peak (first cycle) - second peak (second cycle)) / second peak (first cycle)] × 100% ≤ 9, or [(second peak (first cycle) - second peak (second cycle)) / second peak (first cycle)] × 100% ≤ 7, and can satisfy 0.1 ≤ [(second peak (first cycle) - second peak (second cycle)) / second peak (first cycle)] × 100%, specifically 1 ≤ [(second peak (first cycle) - second peak (second cycle)) / second peak (first cycle)] × 100%, more specifically 3 ≤ [(second peak (first cycle) - The upper and lower limits can be combined without restriction.
[0131] In one exemplary embodiment of this application, the first peak and the second peak correspond to the formation of Li due to lithium insertion into the silicon of the silicon-carb composite. x Si y The first peak appears during discharge after the phase transition. Typically, in silicon-carbon composites, this first peak is a natural material characteristic, while the second peak corresponds to the formation of Li during deeper charging. 15 The peak generated by Si4 during the discharge process.
[0132] However, the present application is characterized by adjusting the intensity of the first peak and the second peak.
[0133] That is, when manufacturing the silicon-carbon composite, by controlling the total volume of porous carbon, SiH4 deposition conditions, and coating conditions, as described above, the dQ / dV spectrum of the discharge curve shape of the negative electrode can be adjusted to fall within the range of Formula 1. This application is characterized in that the second peak in the second cycle shows a smaller decrease compared to the first cycle, and the deviation from the range of Formula 1 indicates that a relatively large amount of Si is deposited on the surface of the porous carbon rather than inside the pores. When a large amount of Si is deposited on the surface, it is difficult to effectively suppress expansion during charge and discharge, which may lead to side reactions and thus reduce lifetime performance. In other words, this application is characterized in that the silicon-carbon composite falls within the range of Formula 1 above and has the effect of improving lifetime performance.
[0134] In one exemplary embodiment of this application, the first and second peaks can be derived by evaluating a coin half-cell in which lithium metal is used as the counter electrode of the negative electrode of a lithium secondary battery according to an exemplary embodiment of this application. Specifically, charge and discharge are performed at a C rate of 0.1 C, charging is performed in CC / CV mode at CV 5 mV and 0.0005 C, and discharging is performed in CC mode up to 1.5 V, at which point curve data are obtained with capacity (mAh) on the x-axis and voltage (V) on the y-axis. Thereafter, only data in the range of 0 to 1.0 V from the discharge curve are selected, and the dQ / dV differential value can be obtained using the ORIGIN program.
[0135] 1. Based on the recording conditions, approximately 5,000 to 6,000 rows of raw data are extracted on average.
[0136] 2. Using the interpolate function, selectively extract 500 rows of X-axis and Y-axis data from the raw discharge data in the Y-axis range of 0 to 1.0 V.
[0137] 3. With voltage on the X-axis and capacity (mAh) on the Y-axis, perform a first-order derivative on the extracted data to obtain the dQ / dV value.
[0138] 4. Normalize the data so that the first peak in the range of 0.25 to 0.35 V is 100%, and then organize the data.
[0139] In one exemplary embodiment of this application, a negative electrode for a lithium secondary battery is provided, wherein the peak intensity ratio of the second peak (first cycle) to the first peak (first cycle) is 0.5 or more and 0.8 or less.
[0140] In another exemplary embodiment, the peak intensity ratio of the second peak (first cycle) to the first peak (first cycle) can be greater than 0.5 and less than 0.8, specifically greater than 0.55 and less than 0.75, and more specifically greater than 0.55 and less than 0.7.
[0141] In one exemplary embodiment of this application, a negative electrode for a lithium secondary battery is provided, wherein the peak intensity ratio of the second peak (second cycle) to the first peak (second cycle) is 0.55 or higher and 0.70 or lower.
[0142] In one exemplary embodiment of this application, a negative electrode for a lithium secondary battery is provided, wherein when the peak intensity ratio of the second peak (first cycle) / the first peak (first cycle) is defined as peak intensity ratio (first cycle), and the peak intensity ratio of the second peak (second cycle) / the first peak (second cycle) is defined as peak intensity ratio (second cycle), the following equation 2 is satisfied.
[0143] [Equation 2]
[0144] 10 ≤ [Peak intensity ratio (2nd cycle) / (Peak intensity ratio (1st cycle) - Peak intensity ratio (2nd cycle))] × 100%
[0145] In another exemplary embodiment, Equation 2 can satisfy 10 ≤ [peak intensity ratio (second cycle) / (peak intensity ratio (first cycle) - peak intensity ratio (second cycle))] × 100%, specifically 11 ≤ [peak intensity ratio (second cycle) / (peak intensity ratio (first cycle) - peak intensity ratio (second cycle))] × 100%, or 12 ≤ [peak intensity ratio (second cycle) / (peak intensity ratio (first cycle) - peak intensity ratio (second cycle))] × 100%, and can also satisfy [peak intensity ratio (second cycle) / (peak intensity ratio (first cycle) - peak intensity ratio (second cycle))] × 100% ≤ 80, specifically [peak intensity ratio (second cycle) / (peak intensity ratio (first cycle) - peak intensity ratio (second cycle))] × 100% ≤ 70, more specifically [peak intensity ratio (2nd cycle) / (peak intensity ratio (1st cycle) - peak intensity ratio (2nd cycle))] × 100% ≤ 60, and the upper and lower limits can be used in unlimited combinations.
[0146] That is, a negative electrode comprising a silicon-carbon composite according to an exemplary embodiment of this application is characterized in that the rate of change of the ratio of the second peak in two or more cycles relative to the ratio of the second peak in the first cycle is low. In other words, when this specific range is met, the lithium secondary battery can achieve high capacity and high energy density while ensuring lifetime performance. In this application, the specific range is met by changing the particle size, SiH4 deposition, and coating conditions during the manufacturing process of the silicon-carbon composite. Specifically, when fine particles of porous carbon (less than 1 μm) are removed and the total volume of porous carbon is adjusted to 0.6 cm³, the specific range is achieved. 3 / g to 0.9 cm 3 / g, and when the deposition conditions are controlled by depositing 45% to 51% silicon, silicon is uniformly deposited inside the pores of porous carbon, and the intensity of the second peak can be controlled, thereby controlling the range of Formulas 1 and 2 above.
[0147] In one exemplary embodiment of this application, a lithium secondary battery is provided, wherein the rolling density of the negative electrode active material layer is 0.9 g / cc or more and 1.3 g / cc or less.
[0148] An exemplary embodiment of this application provides a lithium secondary battery comprising: a positive electrode; a negative electrode for a lithium secondary battery according to an exemplary embodiment of this application; a separator disposed between the positive electrode and the negative electrode; and an electrolyte.
[0149] Figure 2 This is a view illustrating a stacked structure of a lithium secondary battery according to an exemplary embodiment of this application. Specifically, it can be seen that the negative electrode 100 of the lithium secondary battery includes a negative electrode active material layer 20 on one surface of the negative electrode current collector layer 10, and the positive electrode 200 of the lithium secondary battery includes a positive electrode active material layer 40 on one surface of the positive electrode current collector layer 50. The negative electrode 100 and the positive electrode 200 of the lithium secondary battery are formed in a stacked structure with a separator 30 inserted therebetween.
[0150] In one exemplary embodiment of this application, the lithium secondary battery may be a cylindrical battery.
[0151] A secondary battery according to an exemplary embodiment of this specification may specifically include the negative electrode for a lithium secondary battery described above. Specifically, the secondary battery may include a negative electrode, a positive electrode, a separator inserted between the positive electrode and the negative electrode, and an electrolyte, and the negative electrode is the same as the negative electrode described above. Since the negative electrode has been described above, its detailed description is omitted.
[0152] The positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and containing positive electrode active material.
[0153] In the positive electrode, there are no particular limitations on the positive electrode current collector, as long as it is conductive and does not cause chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, and aluminum or stainless steel with surfaces treated with carbon, nickel, titanium, silver, etc., can be used. Furthermore, the thickness of the positive electrode current collector is typically 3 to 500 μm, and the surface of the current collector can be formed with fine irregularities to enhance the adhesion of the positive electrode active material. For example, the positive electrode current collector can be used in various forms, such as membranes, sheets, foils, meshes, porous bodies, foams, and nonwoven fabrics.
[0154] The positive electrode active material can be a commonly used positive electrode active material. Specifically, the positive electrode active material can be a layered compound, such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2), or a compound replaced by one or more transition metals; lithium iron oxide, such as LiFe3O4; or a compound with the chemical formula Li 1+c1 Mn 2-c1 Lithium manganese oxides represented by O4 (0≤c1≤0.33), LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxides (Li2CuO2); vanadium oxides, such as LiV3O8, V2O5, and Cu2V2O7; and those represented by the chemical formula LiNi. 1-c2 M c2 O2 (where M is at least one of the following groups: Co, Mn, Al, Cu, Fe, Mg, B, and Ga, and satisfies 0.01 ≤ c2 ≤ 0.3) represents a Ni-site type lithium nickel oxide; represented by the chemical formula LiMn 2- c3 M c3 Lithium-manganese composite oxides represented by O2 (where M is selected from at least one of the following groups: Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≤c3≤0.1) or Li2Mn3MO8 (where M is selected from at least one of the following groups: Fe, Co, Ni, Cu, and Zn); LiMn2O4, etc., but not limited to these, in which a portion of the Li in the chemical formula is replaced by alkaline earth metal ions. The positive electrode may be Li metal.
[0155] The positive electrode active material layer may include a positive electrode conductive material and a positive electrode binder in addition to the above-mentioned positive electrode active material.
[0156] In this context, the positive electrode conductive material is used to impart conductivity to the electrode and can be used without particular restriction, as long as the positive electrode conductive material has electronic conductivity without causing chemical changes in the constructed battery. Specific examples may include graphite, such as natural and artificial graphite; carbon-based materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal cracking black, and carbon fiber; metal powders or metal fibers, such as copper, nickel, aluminum, and silver; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; or conductive polymers, such as polyphenylene derivatives, etc., and any one or a mixture of two or more thereof may be used.
[0157] Furthermore, the positive electrode adhesive is used to improve the bonding between positive electrode active material particles and the adhesion between the positive electrode active material and the positive electrode current collector. Specific examples may include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and any one or a mixture of two or more thereof may be used.
[0158] The separator is used to separate the negative electrode and the positive electrode and provide a path for lithium ions to move. Any separator can be used without particular limitation, as long as it is typically used in secondary batteries. In particular, separators with high electrolyte retention capacity and low resistance to electrolyte ion movement are preferred. Specifically, porous polymer membranes can be used, such as porous polymer membranes made from polyolefin polymers like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or stacked structures of two or more layers thereof. Alternatively, common porous nonwoven fabrics can be used, such as nonwoven fabrics made from high-melting-point glass fibers, polyethylene terephthalate fibers, etc. Furthermore, coated separators containing ceramic components or polymer materials can be used to ensure heat resistance or mechanical strength, and separators with single-layer or multi-layer structures can be selectively used.
[0159] Examples of the electrolyte may include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, or molten inorganic electrolytes that can be used to manufacture lithium secondary batteries.
[0160] Specifically, the electrolyte may contain a non-aqueous organic solvent and a metal salt.
[0161] As the aforementioned non-aqueous organic solvent, aprotic organic solvents such as N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butyl carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triphosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolium ketone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, or ethyl propionate can be used.
[0162] In particular, among the carbonate-based organic solvents, ethylene carbonate and propylene carbonate, as cyclic carbonates, are high-viscosity organic solvents. Due to their high dielectric constant, they readily dissociate lithium salts and are therefore preferred for use. When the cyclic carbonates are mixed and used with linear carbonates such as dimethyl carbonate and diethyl carbonate, which have low viscosity and low dielectric constant, in appropriate proportions, electrolytes with high conductivity can be prepared, and therefore, they are even more preferred for use.
[0163] As the metal salt, a lithium salt can be used, which is a material readily soluble in non-aqueous electrolytes, wherein the anion of the lithium salt can be, for example, one or more selected from the group consisting of: F - Cl - I - NO3 - N(CN)2 - BF4 - ClO4 - PF6 - (CF3)2PF4 - (CF3)3PF3 - (CF3)4PF2 - (CF3)5PF - (CF3)6P - CF3SO3 - CF3CF2SO3 - (CF3SO2)2N - (FSO2)2N - CF3CF2(CF3)2CO - (CF3SO2)2CH - (SF5)3C - (CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2 - CH3CO2 - SCN - and (CF3CF2SO2)2N - .
[0164] To improve battery life characteristics, suppress battery capacity reduction, and improve battery discharge capacity, the electrolyte may contain one or more additives in addition to the electrolyte components mentioned above, such as alkylene carbonate halide compounds like difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glycol dimethyl ether, hexamethylphosphoryltriamine, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrroles, 2-methoxyethanol, or aluminum trichloride.
[0165] An exemplary embodiment of the present invention provides a battery module comprising the secondary battery as a unit cell and a battery pack comprising the battery module. Because the battery module and the battery pack comprise the secondary battery having high capacity, high rate capability, and high cycle characteristics, the battery module and the battery pack can be used as a power source for medium to large-sized devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and energy storage systems.
[0166] [Best Mode]
[0167] Preferred embodiments will be provided below to better understand the invention. It will be apparent to those skilled in the art that the embodiments described are merely illustrative of the invention, and various modifications and variations can be made within the scope and spirit of the invention. Such modifications and variations naturally fall within the scope of the claims included herein.
[0168] <Preparation Example>
[0169] <Example 1>
[0170] <Preparation of Silicon-Carbon Composites>
[0171] Biomass-based raw materials, such as cellulose powder and coconut shells, were placed in a tube furnace. Under non-heating conditions, the furnace atmosphere was replaced with an inert gas by introducing Ar at a flow rate of 50 to 200 ml / min for 2 hours. Subsequently, the temperature was increased to 400°C at a rate of 5°C / min, followed by heating under an argon atmosphere for 2 hours. A carbonization process was then performed by increasing the tube furnace temperature to 900°C at a rate of 5°C / min and heating under an argon atmosphere for 2 hours. The resulting powder was washed 2 to 3 times with ethanol. Carbon-based particles dried at 100°C for more than 12 hours were then heated at 700°C in an argon atmosphere containing 10% to 20% CO2 as a balance gas for 3 hours to enlarge the pores. The particles were then washed with distilled water and dried at 100°C for more than 12 hours. An activation process yielded a specific surface area of approximately 1,800 m². 2After obtaining / g of porous carbon, fine particles smaller than 1 μm are removed by fractionation.
[0172] The graded porous carbon was placed as carbon-based particles in the hot zone of a CVD device, and SiH4 / H2 (=5 / 95) gas was flowed at a flow rate of 50 to 210 ml / min for 3 hours at 600°C and a low pressure of about 1 to 10 Torr to prepare a silicon-carbon composite.
[0173] Subsequently, without removing the silicon-carbon composite from the furnace, only Ar gas was allowed to flow while the furnace temperature was increased to 650°C at a rate of 5°C / min. The C2H2 / H2 / Ar (=10 / 50 / 40) gas was allowed to flow at a rate of 200 ml / min for 1 hour, and the reaction was allowed to proceed for 1 hour to form a carbon layer on the surface of the silicon-carbon composite.
[0174] <Example 2>
[0175] The silicon-carbon composite was prepared in the same manner as in Example 1, but using resin-based raw materials and a chemical activation process.
[0176] The activation process is carried out by mixing carbon-based particles dried at 100°C for more than 12 hours with KOH at a weight ratio of 1:4, and heating the mixture at 700°C under an argon atmosphere for 4 hours to enlarge the pores.
[0177] <Example 3>
[0178] The silicon-carbon composite was prepared in the same manner as in Example 2, but the graded porous carbon was placed as carbon-based particles in the hot zone of the CVD equipment, and the SiH4 / H2 (=5 / 95) gas was flowed at a flow rate of 50 to 210 ml / min for 6 hours at 600°C and a low pressure of about 1 to 10 Torr.
[0179] <Example 4>
[0180] The silicon-carbon composite was prepared in the same manner as in Example 1, but without the step of removing fine particles smaller than 1 μm after the preparation of porous carbon. The SiH4 / H2 (=5 / 95) gas was flowed to the carbon particles at a flow rate of 50 to 210 ml / min at 600°C for 6 hours, and no carbon coating was formed on the surface after the preparation of the silicon-carbon composite.
[0181] <Example 5>
[0182] The silicon-carbon composite was prepared in the same manner as in Example 2, but a spheroidization step was included in the preparation of the silicon-carbon composite. One of the following methods was selected as the spheroidization method: spray drying, rotary atomizer, and sol-gel.
[0183] <Example 6>
[0184] The silicon-carbon composite was prepared in the same manner as in Example 2, except that in Example 2, the ratio of carbon particles to KOH was 1:3 in the porous carbon activation process, fine particles were not removed in the fractionation, and the silicon-carbon composite was prepared at 650°C under SiH4 / H2 deposition conditions of SiH4 / H2 = 10 / 90 and a flow rate of 300 ml / min.
[0185] <Comparative Example 1>
[0186] The silicon-carbon composite was prepared in the same manner as in Example 1, but the graded porous carbon was placed as carbon-based particles in the hot zone of the CVD equipment, and the SiH4 / H2 (=5 / 95) gas was flowed at a flow rate of 50 to 210 ml / min for 2 hours at 600°C and a low pressure of about 1 to 10 Torr.
[0187] <Comparative Example 2>
[0188] The silicon-carbon composite was prepared in the same manner as in Example 1, but after the silicon-carbon composite was prepared, the furnace temperature was raised to 580°C while only Ar gas was flowing, and the C2H2 / H2 / Ar (=10 / 50 / 40) gas was flowed at a flow rate of 220 ml / min and reacted for 3 hours to form a carbon layer on the surface of the silicon-carbon composite.
[0189] <Comparative Example 3>
[0190] The silicon-carbon composite was prepared in the same manner as in Example 1, but after the silicon-carbon composite was prepared, the furnace temperature was raised to 750°C while only Ar gas was flowing, and the C2H2 / H2 / Ar (=10 / 50 / 40) gas was flowed at a flow rate of 220 ml / min and reacted for 3 hours to form a carbon layer on the surface of the silicon-carbon composite.
[0191] Preparation of coin half-cell
[0192] To obtain the values shown in Table 1 below, electrodes were prepared and evaluated using the following methods.
[0193] The negative electrode active material layer composition was prepared using the following components in a weight ratio of 80:9.6:0.4:10: a silicon-carbon composite (average particle size (D50): 5 μm) prepared above as the silicon-based active material, a first conductive material, a second conductive material, and polyacrylamide as a binder. A negative electrode slurry (solids concentration 28% by weight) was prepared by adding distilled water as a solvent for forming the negative electrode slurry.
[0194] The first conductive material is plate-shaped graphite (specific surface area: 17 m²). 2 / g, average particle size (D50): 3.5 μm), the second conductive material is carbon nanotubes.
[0195] As a mixing method, the first conductive material, the second conductive material, the binder and water are dispersed at 2500 rpm for 30 minutes using a homogenizer, the silicon-based active material is added to the dispersion, and the resulting mixture is dispersed at 2500 rpm for 30 minutes to prepare a negative electrode slurry.
[0196] The negative electrode slurry was prepared at 3.00 mg / cm³. 2 The loading amount was coated on both surfaces of a copper current collector (thickness: 15 μm) used as the negative electrode current collector, then rolled and dried in a vacuum oven at 130°C for 10 hours to form a negative electrode active material layer (thickness: 23 μm).
[0197] A coin half-cell was fabricated using lithium metal as the counter electrode for the negative electrode in a lithium secondary battery. Charge and discharge were performed at a C rate of 0.1 C. Charging was conducted in CC / CV mode at CV 5 mV and 0.005 C, and discharging was performed in CC mode up to 1.5 V. Curve data were extracted with the x-axis representing capacity (mAh) and the y-axis representing voltage (V). Subsequently, only data from the discharge curve within the range of 0 to 1.0 V were selected, and the dQ / dV differential values were obtained using the ORIGIN program according to the following method.
[0198] 1. Based on the recording conditions, approximately 5,000 to 6,000 rows of raw data are extracted on average.
[0199] 2. Using the interpolation function, selectively extract 500 rows of X-axis and Y-axis data from the raw discharge data in the Y-axis range of 0 to 1.0 V.
[0200] 3. With voltage on the X-axis and capacity (mAh) on the Y-axis, perform a first-order derivative on the extracted data to obtain the dQ / dV value.
[0201] 4. Normalize the data so that the first peak in the range of 0.25 to 0.35 V is 100%, and then organize the data.
[0202] The results derived using the above method are shown in Table 1 below.
[0203] [Table 1]
[0204] Figure 3 This is a graph showing the dQ / dV peaks according to Embodiment 1 of this application. For reference, Figure 4This is a graph that appears during the process of deriving the dQ / dV peaks according to Embodiment 1 of this application. Specifically, Figure 4 The diagram shows the x-axis data for capacity (mAh) and the y-axis data for voltage (V) obtained when the coin half-cell of Example 1 is charged and discharged at a C rate of 0.1 C, charged in CC / CV mode at CV 5 mV and 0.005 C, and discharged in CC mode up to 1.5 V. Figure 3 The data is shown by normalizing the data to make the first peak in the range of 0.25 to 0.35 V in the figure 100% and then sorting the data.
[0205] For reference only. Figure 5 This is a graph showing the dQ / dV peaks of Comparative Example 1 according to this application.
[0206] Experiment Example 1: Battery Performance Evaluation
[0207] The negative electrode slurry was prepared by mixing the following components in a weight ratio of 95.3:1:3.6: a negative electrode active material containing the prepared silicon-carbon composite and graphite; a conductive material containing carbon black and SWCNT; and a binder containing carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR), and adding an appropriate amount of distilled water to make the total solids content about 46% by weight.
[0208] In this case, the ratio of silicon-carbon composite to graphite in the negative electrode active material can be 8 to 12:88 to 92 by weight.
[0209] The negative electrode slurry was applied onto a copper metal film with a thickness of approximately 20 μm and then dried at a circulating air temperature of 60°C. The film was then rolled, dried in a vacuum oven at 130°C for approximately one day, and cut to a diameter of 1.4875 cm. 2 The shape is circular to prepare the negative electrode.
[0210] The batteries prepared above were charged and discharged to evaluate the discharge capacity, initial efficiency, and capacity retention, and the results are listed in Table 2 below.
[0211] In the first and second cycles, charge and discharge were performed at 0.1 C, and from the third to the 300th cycle, charge and discharge were performed at 0.5 C. In the 300th cycle, the charge and discharge was terminated in the charging state (the state where lithium ions are in the negative electrode).
[0212] Charging conditions: CC (constant current) / CV (constant voltage) (5 mV / 0.005 C current cutoff)
[0213] Discharge conditions: CC (constant current) condition 1.5 V
[0214] The discharge capacity (mAh / g) and initial efficiency (%) are derived from the results after one charge-discharge cycle. Specifically, the initial efficiency (%) is derived through the following calculations.
[0215] Initial efficiency (%) = (Discharge capacity in the first cycle / Charge capacity in the first cycle) × 100
[0216] The capacity retention rate is derived using the following calculation.
[0217] Capacity retention (%) = (Discharge capacity in cycle 299 / Discharge capacity in cycle 1) × 100
[0218] [Table 2]
[0219] As can be seen from Table 2 above, the dQ / dV spectrum of the discharge curve shape of the negative electrode in the embodiment falls within the range of Equation 1. It was confirmed that when using a silicon-carbon composite with a small decrease in the intensity of the second peak in the second cycle after the first cycle, high energy density and high capacity characteristics can be achieved, volume expansion can be controlled to improve lifetime performance, and in particular, the aqueous processability and gas generation of the negative electrode slurry can be controlled to ensure lifetime performance.
[0220] The silicon-carbon composite satisfying Formula 1 minimizes the amount of silicon deposited on the porous carbon surface while uniformly depositing silicon within the pores of the porous carbon, thereby ensuring lifetime performance by relatively stably forming the SEI during charge and discharge and reducing electrical short-circuiting of particles.
[0221] In the comparative examples, it was confirmed that, unlike the embodiments, silicon was partially deposited on the surface of porous carbon, or the temperature and time conditions of the C2H2 coating process after SiH4 deposition were not optimized, resulting in incomplete coverage of the pores or Si layer on the surface. Therefore, volume expansion or degradation of conductivity occurred during cycling, leading to poorer lifetime characteristics compared to the embodiments.
Claims
1. A negative electrode for a lithium secondary battery, comprising: Negative current collector layer; and A layer of negative electrode active material disposed on one or both surfaces of the negative electrode current collector layer, wherein The negative electrode active material layer contains a negative electrode active material layer composition comprising a negative electrode active material. The negative electrode active material comprises a silicon-carbon composite. The negative electrode exhibits a first peak in the dQ / dV spectrum of the discharge curve shape, ranging from 0.25 V to 0.35 V, and a second peak in the range of 0.42 V to 0.48 V. When lithium metal is used as the counter electrode of the negative electrode in a lithium secondary battery, after N charge-discharge cycles, for the first peak (Nth cycle) and the second peak (Nth cycle), the second peak (Nth cycle) satisfies Equation 1: [Formula 1] [(Second peak (first cycle) - Second peak (second cycle)) / Second peak (first cycle)] × 100% ≤10.
2. The negative electrode for a lithium secondary battery according to claim 1, wherein the peak intensity ratio of the second peak (first cycle) to the first peak (first cycle) is 0.5 or more and 0.8 or less.
3. The negative electrode for a lithium secondary battery according to claim 1, wherein... When the peak intensity ratio of the second peak (first cycle) / the first peak (first cycle) is defined as the peak intensity ratio (first cycle), and the peak intensity ratio of the second peak (second cycle) / the first peak (second cycle) is defined as the peak intensity ratio (second cycle), Satisfying Equation 2: [Equation 2] 10 ≤ [Peak intensity ratio (2nd cycle) / (Peak intensity ratio (1st cycle) - Peak intensity ratio (2nd cycle))] × 100%.
4. The negative electrode for a lithium secondary battery according to claim 3, wherein the peak intensity ratio of the second peak (second cycle) to the first peak (second cycle) is 0.55 or higher and 0.7 or lower.
5. The negative electrode for a lithium secondary battery according to claim 1, wherein the negative electrode active material further comprises a carbon-based active material.
6. The negative electrode for a lithium secondary battery according to claim 1, wherein the content of the silicon-carbon composite is 50 parts by weight or less relative to 100 parts by weight of the negative electrode active material.
7. The negative electrode for a lithium secondary battery according to claim 1, wherein the average particle size (D50) of the silicon-carbon composite is 1 μm or more and 10 μm or less.
8. The negative electrode for a lithium secondary battery according to claim 1, wherein the negative electrode active material layer composition further comprises a negative electrode conductive material and a negative electrode binder.
9. The negative electrode for a lithium secondary battery according to claim 1, wherein the rolling density of the negative electrode active material layer is 0.9 g / cc or more and 1.3 g / cc or less.
10. A lithium secondary battery, comprising: positive electrode; Negative electrode for lithium secondary batteries according to any one of claims 1 to 9; A membrane disposed between the positive electrode and the negative electrode; and Electrolytes.
11. The lithium secondary battery according to claim 10, wherein the lithium secondary battery is a cylindrical battery.
12. A battery module comprising a lithium secondary battery according to claim 10.
13. A battery pack comprising a lithium secondary battery according to claim 10 or a battery module according to claim 11.
Citation Information
Patent Citations
Anode for lithium ion battery
JP2009080971A
Compositions of phosphorylated tau peptides and uses thereof
KR1020240145065A