Nitrogen-containing cationic polymers, binders for metal-ion secondary batteries, and electrolytes for metal-ion secondary batteries

By using nitrogen-containing cationic polymers and fumaric acid-based polymers as binders for lithium-ion secondary batteries, the problem of insufficient adhesion and bonding properties of polyacrylic acid binders was solved, resulting in higher coulombic efficiency and durability.

CN123125698APending Publication Date: 2026-11-17JAPAN ADVANCED INST OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202580028335.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-05-01
Filing Date
2025-03-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing lithium-ion secondary battery negative electrode binders, polyacrylic acid has insufficient adhesion and bonding with the current collector, resulting in electrolyte decomposition and low coulombic efficiency.

Method used

Using nitrogen-containing cationic polymers as binders, including nitrogen-containing cationic polymers and fumaric acid-based polymers containing specific repeating units, improves adhesion and bonding with active materials and current collectors, and inhibits electrolyte decomposition.

Benefits of technology

It improves the coulombic efficiency and durability of lithium-ion secondary batteries, enhances the adhesion and bonding of the negative electrode, and inhibits the decomposition of the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125698A_ABST
    Figure CN123125698A_ABST
Patent Text Reader

Abstract

A kind of formula (I) (where X + Indicates containing N + The invention relates to a nitrogen-containing cationic polymer (with a cyclic structure of cations), a binder for a metal-ion secondary battery containing the nitrogen-containing cationic polymer, a negative electrode for a metal-ion secondary battery containing the binder, a metal-ion secondary battery having the negative electrode, and an electrolyte for a metal-ion secondary battery containing the nitrogen-containing cationic polymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to binders for metal-ion secondary batteries. More specifically, this invention relates to a nitrogen-containing cationic polymer, a binder for metal-ion secondary batteries comprising the nitrogen-containing cationic polymer, an electrolyte for metal-ion secondary batteries comprising the nitrogen-containing cationic polymer, a negative electrode comprising the binder for metal-ion secondary batteries, and a metal-ion secondary battery having the negative electrode. Background Technology

[0002] Polyacrylic acid and polyvinylidene fluoride are commonly used as negative electrode binders in metal-ion secondary batteries such as lithium-ion batteries. Polyacrylic acid has better performance than polyvinylidene fluoride in negative electrode binders and is therefore widely used (see, for example, Patent Documents 1-3).

[0003] However, polyacrylic acid has carbon chains between its functional groups, so it is impossible to introduce functional groups into the polyacrylic acid molecule at a high density. Therefore, in the use of polyacrylic acid as a negative electrode binder, there are limitations on the adhesion to the active material and the adhesion to the current collector.

[0004] Existing technical documents

[0005] Patent documents

[0006] Patent Document 1: Japanese Patent Application Publication No. 2017-152123

[0007] Patent Document 2: Japanese Patent Application Publication No. 2019-175629

[0008] Patent Document 1: International Publication No. 2019 / 212040 Summary of the Invention

[0009] The problem that the invention aims to solve

[0010] This invention was made in view of the above-mentioned prior art. The objective of this invention is to provide a binder for metal-ion secondary batteries and an electrolyte for metal-ion secondary batteries, a negative electrode comprising the aforementioned binder for metal-ion secondary batteries, a metal-ion secondary battery having the negative electrode, and a nitrogen-containing cationic polymer useful for the binder and electrolyte for metal-ion secondary batteries. Compared to conventional binders using polyacrylic acid, the binder for metal-ion secondary batteries exhibits superior adhesion to active materials and to current collectors, and can improve coulombic efficiency while suppressing electrolyte decomposition.

[0011] Methods for solving problems

[0012] This invention relates to the following: (1) A nitrogen-containing cationic polymer having repeating units as shown in formula (I), [Chemistry 1]

[0013] (where X) + Indicates containing N + (Cations with cyclic structures).

[0014] (2) A binder for metal-ion secondary batteries, comprising a nitrogen-containing cationic polymer having repeating units as shown in formula (I) as the binder polymer. [Chemistry 2]

[0015] (where X) + Indicates containing N + (Cations with cyclic structures).

[0016] (3) A negative electrode for a metal-ion secondary battery, comprising the binder for a metal-ion secondary battery described in (2) above.

[0017] (4) A metal-ion secondary battery having a positive electrode, a negative electrode, and a separator disposed between the positive and negative electrodes, wherein the negative electrode is the negative electrode for the metal-ion secondary battery described in (3) above.

[0018] (5) An electrolyte for a metal-ion secondary battery, comprising a nitrogen-containing cationic polymer having repeating units as shown in formula (I) as the electrolyte. [Chemistry 3]

[0019] (where X) + Indicates containing N + (Cations with cyclic structures).

[0020] Invention Effects

[0021] According to the present invention, a binder for a metal-ion secondary battery and an electrolyte for a metal-ion secondary battery are provided, a negative electrode comprising the aforementioned binder for a metal-ion secondary battery, a metal-ion secondary battery having the negative electrode, and a nitrogen-containing cationic polymer useful for the binder for a metal-ion secondary battery and the electrolyte for a metal-ion secondary battery, wherein the binder for a metal-ion secondary battery has superior adhesion to active materials and adhesion to current collectors compared to conventional binders using polyacrylic acid, and can improve coulombic efficiency while suppressing electrolyte decomposition. Attached Figure Description

[0022] Figure 1 This illustrates the fumaric acid homopolymer obtained in Example 1. 1 H-NMR spectra and 13A graph of C-NMR spectra.

[0023] Figure 2 This is a graph showing the FT-IR spectrum of the fumaric acid homopolymer obtained in Example 1.

[0024] Figure 3 This is a graph showing the results of mass spectrometry analysis of the fumaric acid homopolymer obtained in Example 1.

[0025] Figure 4 It is a graph showing the adhesive strength of fumaric acid homopolymer, the adhesive strength of polyacrylic acid, and the adhesive strength of polyvinylidene fluoride.

[0026] Figure 5 It is a cyclic voltammogram of a half-cell using fumaric acid homopolymer, polyacrylic acid, and polyvinylidene fluoride as binders.

[0027] Figure 6 This is a graph showing the Nyquist plots before and after cyclic voltammetry for half-cells using fumaric acid homopolymer, polyacrylic acid, or polyvinylidene fluoride as binders.

[0028] Figure 7 It is a graph showing the Arrhenius plot of a half-cell using fumaric acid homopolymer, polyacrylic acid, or polyvinylidene fluoride as a binder.

[0029] Figure 8 It is a graph showing the change in specific capacity of half-cells using fumaric acid homopolymer, polyacrylic acid, or polyvinylidene fluoride as binders.

[0030] Figure 9 It is a graph showing the internal resistance of a half-cell during lithiation and delithiation when using fumarate homopolymer, polyacrylic acid, or polyvinylidene fluoride as a binder.

[0031] Figure 10 It is a cyclic voltammogram of a half-cell using fumaric acid homopolymer, polyacrylic acid, or polyvinylidene fluoride as a binder.

[0032] Figure 11 This is a graph showing the Nyquist plots before and after cyclic voltammetry for half-cells using fumaric acid homopolymer, polyacrylic acid, or polyvinylidene fluoride as binders.

[0033] Figure 12 It is a graph showing the Arrhenius plot of a half-cell using fumaric acid homopolymer, polyacrylic acid, or polyvinylidene fluoride as a binder.

[0034] Figure 13 It is a graph showing the change in specific capacity of half-cells using fumaric acid homopolymer, polyacrylic acid, or polyvinylidene fluoride as binders.

[0035] Figure 14 The graph shows the internal resistance of a half-cell when sodium-treated and desodium-treated, using a half-cell with fumarate homopolymer, polyacrylic acid, or polyvinylidene fluoride as a binder.

[0036] Figure 15 This shows the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer. 13 A graph of C-NMR spectra.

[0037] Figure 16 This is a graph showing the FT-IR spectrum of the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer.

[0038] Figure 17 This is the cyclic voltammogram of a half-cell using an oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer as a binder.

[0039] Figure 18 This is a graph showing the Nyquist plot of a half-cell before cyclic voltammetry, used to investigate half-cells employing oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer or polyvinylidene fluoride as binders.

[0040] Figure 19 The graph is an Arrhenius plot showing a half-cell using an oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer or polyvinylidene fluoride as a binder.

[0041] Figure 20 The graph shows the results of investigating the specific capacity stepwise from 0.1C to 2C using a half-cell with oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer as a binder and a half-cell with polyvinylidene fluoride as a binder.

[0042] Figure 21 This is a graph showing the results of investigating the changes in specific capacity of half-cells using oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer or polyvinylidene fluoride as binders.

[0043] Figure 22 The graph shows the internal resistance of a half-cell during lithiation and delithiation, using an oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer or polyvinylidene fluoride as a binder. Detailed Implementation

[0044] The present invention will now be described in detail, but the present invention is not limited to the embodiments described below. Those skilled in the art can make various changes and modifications within the scope of the technical concept described in this specification.

[0045] 1. Adhesive for metal-ion secondary batteries

[0046] The binder for metal-ion secondary batteries of the present invention comprises a nitrogen-containing cationic polymer having repeating units as shown in formula (I). [Chemistry 4]

[0047] (where X) + Indicates containing N + (Cations with cyclic structures).

[0048] The metal-ion secondary battery binder of the present invention contains a nitrogen-containing cationic polymer having repeating units as shown in Formula (I). Therefore, compared with conventional binders using polyacrylic acid, it has excellent adhesion to active materials and adhesion to current collectors, and can improve coulombic efficiency while suppressing electrolyte decomposition.

[0049] The binder for metal-ion secondary batteries of the present invention can be used as either a positive electrode binder or a negative electrode binder. The binder for metal-ion secondary batteries of the present invention is preferably used as a negative electrode binder.

[0050] In this invention, in addition to nitrogen-containing cationic polymers having repeating units as shown in formula (I), fumaric acid-based polymers having repeating units as shown in formula (II) can also be used as polymers for adhesives. [Chemistry 5]

[0051] (where R is in the formula) 1 and R 2 Each can be represented independently as a hydrogen atom or an alkali metal atom.

[0052] Among nitrogen-containing cationic polymers having repeating units as shown in Formula (I) and fumaric acid-based polymers having repeating units as shown in Formula (II), the nitrogen-containing cationic polymer having repeating units as shown in Formula (I) is preferred from the aspects of excellent thermal stability, improved adhesion to active materials and current collectors, improved coulombic efficiency while suppressing electrolyte decomposition, and usefulness as an electrolyte. The fumaric acid-based polymer having repeating units as shown in Formula (I) can also be used in combination with the nitrogen-containing cationic polymer having repeating units as shown in Formula (II).

[0053] (1) Nitrogen-containing cationic polymers

[0054] The nitrogen-containing cationic polymer has repeating units as shown in formula (I). In formula (I), X + Indicates containing N + A cyclic cation. As a cation containing N...+ Cations with cyclic structures, for example, include imidazolium-containing cyclic cations as shown in formula (Ia). [Chemistry 6]

[0055] (where R is in the formula) 3 and R 4 Each can independently represent an alkyl or allyl group having 1 to 4 carbon atoms; The piperidine-containing ring cation represented by formula (Ib) [Chemistry 7]

[0056] (where R is in the formula) 5 and R 6 Each alkyl group independently represents an alkyl group with 1 to 4 carbon atoms; The pyrrolidine-containing ring cation shown in formula (Ic) [Chemistry 8]

[0057] (where R is in the formula) 5 and R 6 (Same as above); etc., but the invention is not limited to this example. These include N + The cyclic cations can be used individually or in combination of two or more.

[0058] Nitrogen-containing cationic polymers having repeating units as shown in formula (II) can use N + It is prepared from cyclic compounds as raw materials. As a compound containing N... + Cyclic compounds, such as imidazolium compounds, pyrrolidineium compounds, piperidinium compounds, etc., are included, but the invention is not limited to these examples. These contain N + The cyclic compounds can be used individually or in combination of two or more.

[0059] Representative examples of imidazolium compounds include 1-allyl-3-methylimidazolium and 1-allyl-3-methylimidazolium hydroxide, but the present invention is not limited to these examples. 1-allyl-3-methylimidazolium hydroxide can be readily prepared, for example, by ion exchange of 1-allyl-3-methylimidazolium using a column filled with an ion exchange resin [manufactured by Organo Corporation, trade name: Amberlite IRN78, etc.].

[0060] Representative examples of pyrrolidine-onium compounds include dialkylpyrrolidine-onium compounds with 1 to 4 carbon atoms in the alkyl group, but the present invention is not limited to these examples.

[0061] Examples of piperidinium compounds include alkylpiperidinium compounds with 1 to 4 carbon atoms in the alkyl group, but the present invention is not limited to these examples.

[0062] Next, the above-mentioned fumaric acid homopolymer and N-containing + The cyclic compound dissolves in a solution capable of dissolving the above-mentioned fumaric acid homopolymer and containing N + In a solvent containing a cyclic compound, the resulting solution is stirred thoroughly, then the solvent is removed, and the resulting product is washed with an organic solvent such as acetone and dried, thereby obtaining a nitrogen-containing cationic polymer having repeating units as shown in formula (I).

[0063] The number-average molecular weight of the aforementioned nitrogen-containing cationic polymer is not particularly limited. From the viewpoints of improving adhesion to active materials and current collectors, suppressing electrolyte decomposition, improving coulombic efficiency, enhancing charge-discharge durability when used as a negative electrode binder in metal-ion secondary batteries, and increasing discharge capacity, the number-average molecular weight of the aforementioned nitrogen-containing cationic polymer is preferably 1000 to 100000, more preferably 2000 to 50000. It should be noted that the number-average molecular weight of the nitrogen-containing cationic polymer is a value determined based on the method described in the following examples.

[0064] Without prejudice to the purpose of the invention, the nitrogen-containing cationic polymer may contain repeating units other than those shown in formula (I).

[0065] (2) Fumaric acid polymers

[0066] As described above, fumaric acid polymers are represented by formula (II). Fumaric acid polymers possess the following properties: they prevent electrode cracking when used in metal-ion secondary batteries, inhibit electrolyte decomposition, and improve the electrochemical performance of metal-ion secondary batteries.

[0067] In equation (II), R 1 and R 2 Each atom can be independently either a hydrogen atom or an alkali metal atom. Examples of alkali metal atoms include lithium, sodium, and potassium atoms. Among these, lithium and sodium atoms are preferred. 1 and R 2 From the perspective of improving adhesion to active materials and current collectors, and improving coulombic efficiency while suppressing electrolyte decomposition, hydrogen atoms are preferred.

[0068] In equation (II), R 1 and R 2When all atoms are hydrogen atoms, the fumaric acid polymer shown in formula (II) is a fumaric acid homopolymer. From the viewpoint of improving adhesion to active materials and current collectors, and improving coulombic efficiency while suppressing electrolyte decomposition, fumaric acid homopolymers can be suitably used in this invention.

[0069] Fumaric acid homopolymers can be easily prepared using fumaric acid as a raw material.

[0070] Fumaric acid is a white crystalline powder used in food additives, pharmaceutical raw materials, bath preparations, and oral treatments for psoriasis. It is a commercially available compound. Fumaric acid is an intermediate product of the tricarboxylic acid cycle, a cellular process for energy production in mitochondria, and can be produced or isolated from plants (Vigna) and filamentous fungi (Rhizopus). Fumaric acid produced or isolated from plants and filamentous fungi has the advantage of being environmentally friendly.

[0071] Fumaric acid homopolymers can be prepared using fumaric acid derived from or isolated from plants and filamentous fungi, making them environmentally friendly bio-based polymers. Fumaric acid homopolymers can be readily prepared, for example, by preparing fumarate diesters such as diethyl fumarate from fumaric acid, polymerizing these diesters, and then subjecting the resulting fumarate diester polymer to alkali treatment.

[0072] The aforementioned fumarate diester can be prepared, for example, by reacting fumaric acid with an aliphatic monohydric alcohol. Examples of aliphatic monohydric alcohols include methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butanol, and other aliphatic monohydric alcohols with 1 to 4 carbon atoms, but the present invention is not limited to these examples.

[0073] The aforementioned fumarate diester polymer can be prepared by polymerizing fumarate diester. Examples of polymerization methods for fumarate diester polymers include bulk polymerization, solution polymerization, emulsion polymerization, and suspension polymerization, but the present invention is not limited to these examples. Among these polymerization methods, bulk polymerization and solution polymerization are preferred from the perspective of easily carrying out the polymerization of fumarate diester, and bulk polymerization is more preferred from the perspective of not using solvents.

[0074] It should be noted that when polymerizing fumarate diester by solution polymerization, for example, fumarate diester can be dissolved in an organic solvent, and a polymerization initiator can be added to the solution while stirring, thereby polymerizing fumarate diester. Alternatively, fumarate diester can be added to a solution obtained by pre-dissolving a polymerization initiator in an organic solvent while stirring, thereby polymerizing fumarate diester.

[0075] Examples of organic solvents mentioned above include ethyl acetate, butyl acetate, toluene, tetrahydrofuran, cyclopentane, ethyl acetoacetate, and propylene glycol monomethyl ether acetate, but the present invention is not limited to these examples. These organic solvents can be used individually or in combination of two or more. Among the aforementioned organic solvents, ethyl acetate, butyl acetate, toluene, and tetrahydrofuran are preferred. The amount of organic solvent is not particularly limited. The amount of organic solvent relative to 100 parts by weight of difumarate is preferably 50 to 400 parts by weight, more preferably 100 to 350 parts by weight.

[0076] When polymerizing fumarate diester, a polymerization initiator is preferably used. Examples of polymerization initiators include 2,2'-azobisisobutyronitrile, azobis(dimethyl)valerate, methyl azoisobutyrate, benzoyl peroxide, potassium persulfate, ammonium persulfate, benzophenone derivatives, phosphine oxide derivatives, benzoquinone derivatives, phenyl sulfide derivatives, azide derivatives, diazo derivatives, and disulfide derivatives, but the present invention is not limited to these examples. These polymerization initiators can be used individually or in combination of two or more. It is preferable to select a polymerization initiator suitable for the polymerization method of fumarate diester polymers from these initiators. The amount of polymerization initiator is not particularly limited. The amount of polymerization initiator relative to 100 parts by weight of fumarate diester is preferably 0.05 to 20 parts by weight.

[0077] In the polymerization of fumarate diester, chain transfer agents can be used to control the molecular weight. Chain transfer agents are typically used by mixing with fumarate diester. Examples of chain transfer agents include, for instance, thiol-containing compounds such as lauryl thiol and dodecyl thioglycerol, inorganic salts such as sodium hypophosphite and sodium bisulfite, but the present invention is not limited to these examples. These chain transfer agents can be used individually or in combination of two or more. The amount of chain transfer agent is not particularly limited. The amount of chain transfer agent is typically 0.01 to 10 parts by mass relative to 100 parts by mass of fumarate diester.

[0078] There are no particular limitations on the polymerization temperature and atmosphere for fumarate diester polymerization. The polymerization temperature is typically between 60 and 120°C. From the viewpoint of avoiding the influence of oxygen contained in the air, the atmosphere for the polymerization reaction is preferably an inert gas atmosphere such as nitrogen or argon. Furthermore, the polymerization reaction time of fumarate diester varies depending on the polymerization temperature, etc., and therefore cannot be generalized; it is typically between 3 and 20 hours.

[0079] Fumarate diester polymers can be obtained by polymerizing fumarate diester as described above.

[0080] Next, the fumarate diester polymer obtained above is dissolved in a monoaliphatic alcohol such as ethanol, and an aqueous solution of an alkali metal hydroxide such as potassium hydroxide is added to the resulting solution, thereby obtaining a reaction mixture containing fumarate polymers.

[0081] After acidifying the reaction mixture containing fumaric acid polymers using acids such as hydrochloric acid, dialysis is performed to obtain R in formula (II). 1 and R 2 Fumaric acid homopolymers with hydrogen atoms are considered fumaric acid-based polymers. R in formula (II) 1 and R 2 Fumaric acid polymers containing alkali metal atoms can be obtained by adding an aqueous solution of the alkali metal hydroxide to an aqueous solution of a fumaric acid homopolymer.

[0082] The number-average molecular weight of the fumaric acid-based polymer obtained as described above is not particularly limited. From the viewpoints of excellent adhesion to active materials and current collectors, suppression of electrolyte decomposition, improved coulombic efficiency, improved charge-discharge durability when used as a negative electrode binder in metal-ion secondary batteries, and increased discharge capacity, the number-average molecular weight of the fumaric acid-based polymer is preferably 1000 to 100000, more preferably 2000 to 50000. It should be noted that the number-average molecular weight of the fumaric acid-based polymer is a value determined based on the method described in the following examples.

[0083] Without prejudice to the purpose of the invention, the fumaric acid polymer may contain repeating units other than those shown in formula (II).

[0084] [Binder for Metal-Ion Secondary Batteries]

[0085] As described above, the binder for metal-ion secondary batteries of the present invention contains a nitrogen-containing cationic polymer having repeating units as shown in formula (I).

[0086] The binder for metal-ion secondary batteries of the present invention contains a nitrogen-containing cationic polymer having repeating units as shown in Formula (I), thus exhibiting excellent adhesion to active materials and current collectors. It can suppress electrolyte decomposition, improve coulombic efficiency, and enhance charge-discharge durability and discharge capacity when used as a negative electrode binder for metal-ion secondary batteries.

[0087] The binder for metal-ion secondary batteries of the present invention can be dissolved in a non-polar solvent for use. Examples of non-polar solvents include saturated hydrocarbon compounds such as hexane, cyclohexane, heptane, octane, nonane, decane, and 2-ethylhexane; aromatic compounds such as toluene and xylene; and halogenated hydrocarbon compounds such as dichloromethane, chloroform, and dichloroethane, but the present invention is not limited to these examples. It is preferable to select a suitable non-polar solvent from these non-polar solvents for use as the binder for metal-ion secondary batteries. The amount of non-polar solvent is not particularly limited, but it is preferable to use an appropriate amount.

[0088] The binder for metal-ion secondary batteries of the present invention may be composed solely of the polymers described above for binders, or, without prejudice to the purpose of the present invention, may include other binders for negative electrodes such as polyacrylic acid, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, and ethylene propylene diene rubber.

[0089] From the viewpoints of excellent adhesion to active materials and current collectors, suppression of electrolyte decomposition, improvement of coulombic efficiency, improved charge-discharge durability and increased discharge capacity when used as a negative electrode binder for metal-ion secondary batteries, the content of the aforementioned binder polymer in the binder for metal-ion secondary batteries of the present invention is preferably 80% by mass or more, more preferably 90% by mass or more.

[0090] 2. Metal-ion secondary battery

[0091] The metal-ion secondary battery of the present invention is a metal-ion secondary battery having a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode. One feature of the metal-ion secondary battery of the present invention is that the negative electrode comprises the aforementioned binder for metal-ion secondary batteries.

[0092] The metal-ion secondary battery of the present invention has a negative electrode containing the above-mentioned binder for metal-ion secondary batteries, thus exhibiting excellent adhesion to the active material and to the current collector, thereby suppressing electrolyte decomposition and improving coulombic efficiency.

[0093] The metal-ion secondary battery of the present invention has the same structure as conventionally used metal-ion secondary batteries. Representative examples of metal-ion secondary batteries include lithium-ion and sodium-ion secondary batteries, both of which can be suitably used in the present invention.

[0094] The metal-ion secondary battery of the present invention typically includes a positive electrode, a negative electrode, a separator, and an electrolyte. Examples of shapes for metal-ion secondary batteries include cylindrical and stacked types, but the present invention is not limited to these examples.

[0095] In the case of a metal-ion secondary battery of the present invention, such as a CR2025 type button cell, the negative electrode, separator, and electrolyte are housed within the casing. Hereinafter, an embodiment in the case of a CR2025 type button cell will be described, but the present invention is not limited to this embodiment.

[0096] The CR2025 button cell casing is hollow with an opening that also serves as the positive electrode container. A cover is located at the opening, which also functions as the negative electrode cover. A gasket is placed between the casing and the cover to maintain insulation and a seal. The electrodes and electrolyte are housed in the space between the casing and the cover.

[0097] (1) Electrode

[0098] The electrode has a positive electrode, a diaphragm, and a negative electrode, arranged in that order. The positive electrode is in contact with the inner surface of the housing, and the negative electrode is in contact with the inner surface of the cover.

[0099] [positive electrode]

[0100] The positive electrode can be the same as the positive electrode used in commonly used metal-ion secondary batteries; the present invention is not limited by the composition and structure of the positive electrode.

[0101] The positive electrode can be made as follows: the positive electrode active material, conductive material and binder are mixed in a specified ratio, an appropriate amount of solvent, activated carbon as needed, viscosity adjuster additives, etc. are added to the resulting mixture, the resulting mixture is kneaded, a positive electrode composite paste is prepared, and then coated on the surface of the current collector. It is then pressed and shaped as needed and dried to produce the positive electrode.

[0102] Examples of positive electrode active materials include lithium and lithium-manganese composite oxides, but the present invention is not limited to these examples. Examples of conductive materials include carbon black such as acetylene black, natural graphite, artificial graphite, and expanded graphite, but the present invention is not limited to these examples. Examples of binders, exemplified by the binder for metal-ion secondary batteries of the present invention, include polyacrylic acid, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, and ethylene propylene diene rubber, but the present invention is not limited to these examples. Among these binders, the binder for metal-ion secondary batteries of the present invention is preferred. Examples of solvents include N-methyl-2-pyrrolidone, but the present invention is not limited to these examples. Examples of current collectors include copper, aluminum, nickel, silver, tin, indium, magnesium, iron, chromium, molybdenum, and their alloys, but the present invention is not limited to these examples.

[0103] [Septum]

[0104] A separator is used between the positive and negative electrodes. The separator separates the positive and negative electrodes, retains the electrolyte, and forms a pathway for lithium ions to move between them. The separator can be made of polyolefin resins such as polyethylene and polypropylene, thin films such as cellulose and glass. Preferably, multiple micropores are formed on the thin film.

[0105] [negative electrode]

[0106] The negative electrode uses the negative electrode for metal-ion secondary batteries of the present invention. The binder for metal-ion secondary batteries of the present invention is used in the negative electrode for metal-ion secondary batteries.

[0107] For example, the negative electrode for a metal-ion secondary battery can be made as follows: a negative electrode active material, the binder for a metal-ion secondary battery of the present invention, and a conductive additive as needed are mixed, and the resulting mixture is added to a solvent to prepare a paste-like negative electrode composite material. The negative electrode composite material is coated on the surface of a metal foil current collector such as a copper foil, dried, and shaped using a roller press as needed, and then dried to produce the negative electrode for a metal-ion secondary battery.

[0108] The negative electrode active material can be any active material capable of inserting and deintercalating lithium ions, and the present invention is not limited to the type of negative electrode active material. Examples of negative electrode active materials include carbon-based materials such as graphite, silicon, lithium metal, lithium alloys, sodium metal, sodium alloys, silicon-containing compounds, silicon-containing alloys, tin, tin-containing alloys, metal oxides, metal sulfides, metal nitrides, etc., but the present invention is not limited to these examples.

[0109] From the viewpoint of improving the capacity of metal-ion secondary batteries, silicon, which exhibits large expansion and contraction during charging and discharging, is preferably used as the negative electrode active material. The silicon can be amorphous silicon or silicon microcrystals. Alternatively, silicon nanoparticles can be used as silicon. Silicon nanoparticles are readily available commercially, but can be prepared as described below.

[0110] Alkoxysilane compounds can be used as raw materials for silicon nanoparticles. Examples of alkoxysilane compounds include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropyldimethylethoxysilane, and N-(2-aminoethyl)aminomethyltrimethoxysilane, but the present invention is not limited to these examples. These alkoxysilane compounds can be used individually or in combination of two or more. Alkoxysilane compounds can be used in the form of a mixture with water.

[0111] The alkoxysilane compound is preferably pre-reduced. Reduction of the alkoxysilane compound can be achieved, for example, by adding a reducing agent to a mixture of the alkoxysilane compound and water. The temperature for reducing the alkoxysilane compound is not particularly limited, and is typically between 5 and 80°C. The atmosphere for reducing the alkoxysilane compound is not particularly limited; it can be atmospheric gas or an inert gas such as nitrogen or argon.

[0112] Examples of reducing agents include ascorbic acid, sodium ascorbate, potassium ascorbate, and their salts; sodium sulfite, potassium sulfite, sodium bisulfite, sodium aldehyde bisulfite, potassium bisulfite, and other sulfites; and sodium metabisulfite, potassium metabisulfite, sodium metabisulfite, potassium metabisulfite, and other metabisulfite salts. However, the present invention is not limited to these examples. These reducing agents can be used individually or in combination of two or more.

[0113] The amount of reducing agent varies depending on the type of reducing agent, and therefore cannot be generalized. The reducing agent is generally preferred to be used in the amount required to neutralize the alkoxysilane compound.

[0114] The temperature at which the reducing agent is added to the mixture of alkoxysilane compound and water is not particularly limited, and is generally in the range of 5 to 80°C. After adding the reducing agent to the mixture of alkoxysilane compound and water, from the viewpoint of obtaining silicon nanoparticles with uniform particle size, it is preferable to stir the mixture until it becomes a homogeneous composition.

[0115] As described above, an aqueous dispersion of silicon nanoparticles can be obtained by reducing alkoxysilane compounds using a reducing agent.

[0116] From the viewpoint of improving dispersion stability and the durability of metal-ion secondary batteries during charge and discharge, and increasing discharge capacity, the average particle size of the silicon nanoparticles obtained above is preferably 1–300 nm, more preferably 2–250 nm, and even more preferably 3–200 nm. It should be noted that the average particle size of the silicon nanoparticles refers to the value obtained by randomly selecting 100 silicon nanoparticles from an image taken with a scanning electron microscope, calculating the average value of the vertical and horizontal axes of each silicon nanoparticle, summing this average value for all 100 silicon nanoparticles, and then dividing this sum by 100.

[0117] As a solvent, water is a representative example. Examples of organic solvents that can be used as solvents include N-methylpyrrolidone, dimethylformamide, dimethylacetamide, methyl ethyl ketone, cyclohexanone, methyl acetate, diethyltriamine, N,N-dimethylaminopropylamine, ethylene oxide, and tetrahydrofuran. However, the present invention is not limited to this example.

[0118] The negative electrode composite may contain conductive additives as needed. Examples of conductive additives include acetylene black, Ketjen black (conductive carbon black), channel black, furnace black, lampblack, thermal cracking black, and other carbon blacks; conductive fibers such as carbon fibers and metal fibers; fluorinated carbon; metal powders such as copper and nickel; and organic conductive materials such as polyphenylene derivatives. However, the present invention is not limited to these examples. The content of conductive additives in the negative electrode composite is generally preferably 10% by mass or less.

[0119] Furthermore, the negative electrode compound may contain an appropriate amount of inclusion compounds as needed. These inclusion compounds have the property of absorbing gases generated within the battery. Examples of inclusion compounds include cyclodextrins such as α-cyclodextrin, β-cyclodextrin, and γ-cyclodextrin, as well as crown ethers such as 12-crown-4, 15-crown-5, and 18-crown-6, but the present invention is not limited to these examples. The content of inclusion compounds in the negative electrode compound is generally preferably between 3 and 10% by mass.

[0120] Examples of current collectors include copper, aluminum, nickel, silver, tin, indium, magnesium, iron, chromium, molybdenum and their alloys, but the present invention is not limited to these examples.

[0121] (2) Electrolytes

[0122] Examples of electrolytes include cyclic carbonates such as nitrogen-containing cationic polymers having repeating units as shown in Formula (I), ethylene carbonate, diethyl carbonate, propylene carbonate, butyl carbonate, and trifluoropropylene carbonate; chain carbonates such as dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, and dipropyl carbonate; and ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran, and dimethoxyethane, but the present invention is not limited to these examples. These electrolytes can be used individually or in combination of two or more. Nitrogen-containing cationic polymers having repeating units as shown in Formula (I) have the same properties as the binder for metal-ion secondary batteries of the present invention, and are therefore useful as electrolytes.

[0123] As explained above, since the metal-ion secondary battery of the present invention uses the binder of the present invention, the metal-ion secondary battery of the present invention has superior adhesion to the active material and adhesion to the current collector compared with the conventional case using a binder made of polyacrylic acid, thus suppressing the decomposition of the electrolyte and improving the coulombic efficiency.

[0124] Next, the present invention will be described in detail based on embodiments, but the present invention is not limited to these embodiments.

[0125] 1.Raw materials

[0126] As raw materials, diethyl fumarate (purity: 98%), hydrochloric acid (12N), 2,2'-azobis(isobutyronitrile) (AIBN) as a free radical polymerization initiator, poly(vinylidene fluoride) (PVDF) binder (average molecular weight: 540,000), polyacrylic acid, 1.0M LiPF6 in ethylene carbonate / diethyl carbonate (capacity ratio: 50 / 50), electrolyte and graphite for batteries were obtained from Sigma-Aldrich.

[0127] In addition, potassium hydroxide, ethanol (purity: 99.5%), and N-methylpyrrolidone (NMP) were obtained as raw materials from Fujifilm and Kojun Pharmaceutical Co., Ltd., and conductive carbon black (Super P conductive carbon black) as a conductive additive was obtained from Alfa Aesar Co., Ltd. Regenerated cellulose dialysis tubing was used as the dialysis tubing.

[0128] 2.Physical properties

[0129] (1) Number-average molecular weight of polymers (MALDI-TOF mass spectrometry analysis)

[0130] The number-average molecular weight of the polymer was determined using a mass spectrometer [Bruker Daltonics, trade name: microflex LRF], with 2,5-dihydroxybenzoic acid (DHB) as the matrix and sodium iodide as the cation reagent.

[0131] (2) Nuclear magnetic resonance spectroscopy

[0132] Nuclear magnetic resonance of polymers 1 H-NMR and 13 C-NMR was performed using a nuclear magnetic resonance spectrometer [Bruker, trade name: AVANCE II NMR Spectrometer 400MHz], with D2O as the solvent.

[0133] (3) Fourier transform infrared absorption spectroscopy (FT-IR spectroscopy)

[0134] The Fourier transform infrared absorption spectra of the polymers were investigated using a Fourier transform infrared spectrometer [manufactured by PerkinElmer].

[0135] (4) Thermogravimetric analysis

[0136] Thermogravimetric analysis of the polymer was performed using a thermal analysis system [Hitachi High-Tech Science Corporation, model: STA7200] at a heating rate of 10°C / min and a nitrogen flow rate of 200 mL / min.

[0137] 3. Battery performance

[0138] (1) Cyclic Voltammetry (CV)

[0139] Cyclic voltammetry was performed at room temperature using a potentiostat (Biological, model: VSM) with the aforementioned button cell. It should be noted that the potential range for cyclic voltammetry measurements is 0.01–2.1 V, with the scan rate adjusted to 0.1 mV / s, 0.2 mV / s, 0.4 mV / s, 0.6 mV / s, or 0.8 mV / s.

[0140] (2) Electrochemical impedance spectroscopy (EIS)

[0141] Electrochemical impedance spectroscopy was performed before and after the cyclic voltammetry measurement at a frequency of 1.0 MHz to 0.1 Hz and an AC voltage of 10 mV.

[0142] (3) Dynamic electrochemical impedance spectroscopy (EIS)

[0143] Dynamic electrochemical impedance spectroscopy was performed after 700 charge-discharge cycles at a frequency of 1.0 MHz to 0.1 Hz and an AC voltage of 10 mV.

[0144] (4) Measurement of constant current cycling

[0145] The constant current cyclic automatic battery evaluation device [Electrofield, trade name: ABE 1024] was used to investigate the battery at a constant current of 0.01 to 2.1V.

[0146] (5) Activation energy

[0147] After cycling, the potential of the half-cell was set to 0.2V, the value of lithium intercalation in graphite, and then calculated using electrochemical impedance spectroscopy. It should be noted that the potential was maintained, and the electrochemical impedance spectra were investigated within different temperature ranges.

[0148] (6) Rheological properties of slurry and electrodes

[0149] The rheological properties of the slurry and electrodes were evaluated by performing viscosity and peel tests, respectively. It should be noted that viscosity was measured using a viscometer [Toki Sangyo Co., Ltd., model: TV-35] at 25°C. The peel test was performed as follows: For electrodes with a length of 40 mm, a universal testing machine [Instron Co., Ltd., model: 3342] was used to roll the electrodes in an atmosphere at 25°C. Cellophane adhesive tape [NICHIBAN Co., Ltd., trade name: Cellotape (registered trademark), width: 15 mm] was applied to the coated surface of the resulting electrode. The cellophane adhesive tape was peeled off at a constant speed of 1 mm / min at a 90° angle, and the peel test was conducted to investigate the adhesive strength.

[0150] (7) Analysis after long-term cyclic test

[0151] X-ray photoelectron spectroscopy (XPS) analysis was performed after long-term cyclic testing. XPS analysis was conducted using an XPS analyzer (Fisons Instruments, S-PROBE 2803). Furthermore, the morphology of the electrodes after long-term cyclic testing was investigated using a field emission scanning electron microscope (Hitachi High-Tech, S-4500) at an accelerating voltage of 1.0 kV.

[0152] Example 1

[0153] (1) Preparation of fumaric acid homopolymer

[0154] The reaction shown in the following reaction equation will proceed.

[0155] [Chemistry 9]

[0156] More specifically, in the presence of 38 mg (0.23 mmol) of 2,2'-azobisisobutyronitrile (AIBN), 2 g (11.6 mmol) of diethyl fumarate was polymerized at 70 °C under a nitrogen atmosphere for 24 hours. The resulting polymer was added to 50 mL of hexane under stirring, and the polymer was dried under reduced pressure for about 10 hours. The hexane was then removed by distillation.

[0157] Next, the polymer obtained above was hydrolyzed in a mixed solvent of ethanol:water (2:1) with excess potassium hydroxide under reflux for 24 hours. The resulting reaction mixture was concentrated and acidified with 1N hydrochloric acid (pH: 4.6). Then, the reaction mixture was dialyzed through a cellulose acetate tube and dried to obtain R in formula (II). 1 and R 2 1.1 g of fumaric acid homopolymer containing hydrogen atoms (yield: 82%).

[0158] (2) 1 H-NMR and 13 C-NMR

[0159] The fumaric acid homopolymer obtained above 1 H-NMR spectra and 13 The C-NMR spectra are shown in the figures. Figure 1 (a) and (b).

[0160] Confirmed: In Figure 1 (a) shows 1In the H-NMR spectrum, the peak p at 3.25 ppm is based on the CH of the methylene group present in the main chain of the fumaric acid homopolymer. Figure 1 (b) shows 13 In the C-NMR spectrum, the characteristic peaks q and r at 170.8 ppm and 62.4 ppm are based on the carbonyl and methylene carbon of the fumaric acid homopolymer, respectively.

[0161] (3) FT-IR spectroscopy

[0162] The FT-IR spectrum of the obtained fumaric acid homopolymer is shown in... Figure 2 .exist Figure 2 In the FT-IR spectrum shown, the wavenumber is 3500 cm⁻¹. -1 The peak at 2977 cm⁻¹ is due to the stretching of the OH groups of the carboxyl groups in the fumaric acid homopolymer. -1 The characteristic absorption peak at this point is based on the stretching of the -CH- group in the main chain of the fumaric acid homopolymer, with a wavenumber of 1715 cm⁻¹. -1 and 1090cm -1 The peak at that point is based on the carbonyl and ether bonds of the fumaric acid homopolymer.

[0163] (4) Number-average molecular weight

[0164] The results of the MALDI-TOF mass spectrometry analysis of the obtained fumaric acid homopolymer are shown below. Figure 3 The mass spectrometry analysis of the fumaric acid homopolymer confirmed that its number-average molecular weight was 3000 (m / z).

[0165] (5) Thermogravimetric analysis

[0166] Thermogravimetric analysis of the fumaric acid homopolymer revealed an initial weight loss at approximately 100°C. This weight loss is attributed to the evaporation of adsorbed water from the carboxyl groups of the fumaric acid homopolymer. The thermal stability of the fumaric acid homopolymer is approximately 235°C; above this temperature, rapid decomposition due to dehydration, believed to be caused by the formation of intramolecular bonds or anhydride bonds, is observed.

[0167] Based on the above, fumaric acid homopolymers exhibit excellent thermal stability, making them suitable as binders for metal-ion secondary batteries used at high temperatures.

[0168] (Example 2)

[0169] Electrodes and half-cells were fabricated using the fumaric acid homopolymer obtained in Example 1 as follows.

[0170] Graphite, conductive carbon black, and fumaric acid homopolymer were added to water in a mass ratio of 80:10:10, and the resulting mixture was uniformly dispersed using a homogenizer to prepare a slurry (negative electrode material).

[0171] The slurry obtained above is applied to copper foil (vertical: 20 mm, horizontal: 100 mm, thickness: 20 μm) with a coating thickness of about 100 μm using a doctor blade. After drying under reduced pressure at 80°C for 12 hours, it is then passed through rollers with a gap of 70 μm at 80°C to perform rolling pressing, thereby producing an electrode with a coating thickness of about 50 μm.

[0172] The electrodes obtained above are compressed using a hot rolling mill and cut into discs with a diameter of 13 mm, thus obtaining disc-shaped electrodes.

[0173] The disc-shaped electrode obtained above was inserted into a button cell (CR2025). The button cell was placed in a glove box filled with argon gas and the oxygen and water vapor concentrations were both below 0.5 ppm. A lithium disk was used as the counter electrode, polypropylene CELGARD was used as the separator, and a 1.0 M LiPF6 ethylene carbonate / diethyl carbonate (capacity ratio: 50 / 50) solution was used as the electrolyte to make a button cell (half cell).

[0174] For comparison of battery performance, polyacrylic acid or polyvinylidene fluoride was used instead of fumarate homopolymer as a binder, and button cells (half-cells) were manufactured in the same manner as described above. It should be noted that when using polyvinylidene fluoride, N-methyl-2-pyrrolidone was used instead of water as a solvent.

[0175] (1) Adhesive bonding strength

[0176] The adhesive strength was evaluated based on the stress upon peeling off cellophane adhesive tape [manufactured by NICHIBAN Co., Ltd., trade name: Cellotape, width: 15 mm]. The results of adhesive strength measurements using fumaric acid homopolymer, polyacrylic acid, or polyvinylidene fluoride as adhesives are shown below. Figure 4 .

[0177] exist Figure 4 In the diagram, symbol A represents the adhesive strength of the fumaric acid homopolymer, symbol B represents the adhesive strength of the polyacrylic acid, and symbol C represents the adhesive strength of the polyvinylidene fluoride.

[0178] like Figure 4 As shown, the adhesive strength A of the fumaric acid homopolymer is significantly higher than that of polyacrylic acid (B) and polyvinylidene fluoride (C). Therefore, the high adhesive strength of the fumaric acid homopolymer to the current collector of the electrode is considered useful for addressing volume expansion during lithiation and preventing electrode assembly disintegration during delithiation.

[0179] (2) Viscosity of the adhesive

[0180] The viscosities of slurries containing fumaric acid homopolymer, polyacrylic acid, and polyvinylidene fluoride were measured at 25°C. The results showed that for a shear rate of 3.75 s⁻¹... -1 The viscosity of the slurry at that time was 4.9 Pa·s in the slurry containing fumaric acid homopolymer, 4.2 Pa·s in the slurry containing polyacrylic acid, and 2.9 Pa·s in the slurry containing polyvinylidene fluoride.

[0181] Generally speaking, it is believed that a uniform film is formed on the electrode as the viscosity of the slurry increases. Therefore, it is known that slurries containing fumaric acid homopolymers have moderate viscosity and are superior in forming a uniform film compared to slurries containing polyacrylic acid and polyvinylidene fluoride.

[0182] (3) Electrochemical characteristics

[0183] [Electrochemical Stability]

[0184] The electrochemical stability of the binder within the electrode was evaluated using cyclic voltammetry.

[0185] Cyclic voltammograms were investigated using half-cells with fumaric acid homopolymer, polyacrylic acid, or polyvinylidene fluoride as binders at scan rates of 0.1 mV / sec, 0.2 mV / sec, 0.4 mV / sec, 0.6 mV / sec, or 0.8 mV / sec. The results are presented in... Figure 5 .

[0186] exist Figure 5 In the figure, (a) is the cyclic voltammogram of the half-cell using fumaric acid homopolymer, (b) is the cyclic voltammogram of the half-cell using polyacrylic acid, and (c) is the cyclic voltammogram of the half-cell using polyvinylidene fluoride.

[0187] like Figure 5 As shown, a reduction peak of 0.7V accompanied by electrolyte decomposition is present when any binder is used, indicating that electrolyte decomposition is suppressed. Furthermore, when polyacrylic acid is used as the binder, the overpotential difference of the delithiation peak is 0.129V; when polyvinylidene fluoride is used as the binder, the overpotential difference is 0.132V; and when fumarate homopolymer is used as the binder, the overpotential difference is 0.117V. Therefore, it can be concluded that the overpotential difference of the delithiation peak is small between scan rates of 0.1mV / sec and 1.0mV / sec.

[0188] Based on the above results, it is believed that the fumaric acid homopolymer has excellent adhesion to the active material. Even at high scanning speeds, lithium ions can easily penetrate into the SEI layer, inducing lithium ion diffusion.

[0189] [Lithium-ion diffusion coefficient]

[0190] The lithium-ion diffusion coefficient is investigated based on the following formula. Randles-Sevcik formula: Ip = 2.69 × 10 5 n 3 / 2 AD Li C Li V 1 / 2 [In the formula, Ip represents the peak current (A), n represents the number of electrons participating in the reaction, and A represents the electrode area (cm²).] 2 D represents the diffusion coefficient of lithium ions (cm). 2 / sec), C represents molar concentration (mol / cm³) 3 (V represents the scan rate (V / sec)). As a result, the lithium-ion diffusion coefficient in the fumaric acid homopolymer is 3.57 × 10⁻⁶. -8 cm 2 / sec, which is 2.11 × 10 in polyacrylic acid. -8 cm 2 / sec, which is 6.59 × 10 in polyvinylidene fluoride. -9 cm 2 / sec.

[0191] The results above show that the fumaric acid homopolymer exhibits a weak interaction with lithium ions, promoting lithium diffusion within the electrode.

[0192] [Nyquist plot]

[0193] The Nyquist plots before and after cyclic voltammetry were investigated using half-cells with fumaric acid homopolymer, polyacrylic acid, or polyvinylidene fluoride as binders. The results are presented in... Figure 6 .

[0194] exist Figure 6 In the diagram, symbol A represents the Nyquist plot before cyclic voltammetry using a half-cell containing a fumaric acid homopolymer; symbol B represents the Nyquist plot after cyclic voltammetry using a half-cell containing a fumaric acid homopolymer; symbol C represents the Nyquist plot before cyclic voltammetry using a half-cell containing polyacrylic acid; symbol D represents the Nyquist plot after cyclic voltammetry using a half-cell containing polyacrylic acid; symbol E represents the Nyquist plot before cyclic voltammetry using a half-cell containing polyvinylidene fluoride; and symbol F represents the Nyquist plot after cyclic voltammetry using a half-cell containing polyvinylidene fluoride.

[0195] The charge movement process within the electrode is correlated with the concave portion of the Nyquist plot generated at high frequencies and the straight line of the Nyquist plot in the subsequent low-frequency region, i.e., the diffusion-controlled Warburg impedance. The smaller the value in the concave portion of the Nyquist plot, the smaller the charge movement resistance (RCT).

[0196] The Nyquist plot B obtained by cyclic voltammetry using fumaric acid homopolymer is smaller than the Nyquist plots D and F obtained using polyacrylic acid and polyvinylidene fluoride, indicating that the charge-moving resistance (RCT) is smaller.

[0197] The charge-moving resistance (RCT) is related to the concentration of lithium ions on the electrode surface where the SEI layer is formed, which has an adverse effect on cycle life. However, when using fumarate homopolymer, the charge-moving resistance (RCT) is small, thus improving cycle life.

[0198] [activation energy]

[0199] Arrhenius diagrams were investigated using half-cells with various binders. The results are presented below. Figure 7 .exist Figure 7 In the diagram, symbol A is the Arrhenius plot determined using a half-cell using a fumaric acid homopolymer, symbol B is the Arrhenius plot determined using a half-cell using polyacrylic acid, and symbol C is the Arrhenius plot determined using a half-cell using polyvinylidene fluoride.

[0200] The activation energies of each binder were determined from the slope of the Arrhenius plot. The results showed that the activation energies were 36.4 kJ / mol for the fumaric acid homopolymer, 48.9 kJ / mol for polyacrylic acid, and 52.8 kJ / mol for polyvinylidene fluoride. This indicates that the fumaric acid homopolymer has a lower activation energy compared to polyacrylic acid and polyvinylidene fluoride, thus facilitating the smooth transport of lithium ions within the electrode.

[0201] [Initial charge / discharge capacity]

[0202] The initial charge-discharge capacity was investigated using half-cells with various binders. The results are shown in Table 1.

[0203] [Table 1]

[0204] As shown in Table 1, the initial discharge capacity is exceptionally high when using fumaric acid homopolymer as a binder, compared to the case where polyacrylic acid or polyvinylidene fluoride is used as a binder. Therefore, the coulombic efficiency of fumaric acid homopolymer is excellent.

[0205] [The Influence of Binders on Constant Current Charge-Discharge Cycling]

[0206] To evaluate its practical applicability to lithium-ion batteries, the effect of the binder on constant current charge-discharge cycling was investigated using a half-cell at a charge capacity of 5C. The results are presented below. Figure 8 .exist Figure 8 In the diagram, symbol A represents the change in specific capacity measured using a half-cell using a fumaric acid homopolymer, symbol B represents the change in specific capacity measured using a half-cell using polyacrylic acid, and symbol C represents the change in specific capacity measured using a half-cell using polyvinylidene fluoride.

[0207] Depend on Figure 8 The results show that, in half-cells using fumaric acid homopolymer as a binder, compared with half-cells using polyacrylic acid or polyvinylidene fluoride as a binder, the half-cells can maintain a high charge capacity even after 1000 charge-discharge cycles. Therefore, the coulombic efficiency of fumaric acid homopolymer is excellent, and the long-term cycle durability of the electrode is excellent.

[0208] [Battery internal resistance]

[0209] The internal resistance of half-cells under lithiation and delithiation was investigated using half-cells with various binders. The results are presented in... Figure 9 .exist Figure 9 In the diagram, (a) represents the internal resistance during lithiation, and (b) represents the internal resistance during delithiation. Additionally, in... Figure 9 In the diagram, symbol A represents data when using fumaric acid homopolymer, symbol B represents data when using polyacrylic acid, and symbol C represents data when using polyvinylidene fluoride.

[0210] Depend on Figure 9 The results shown in (a) indicate that, for the internal resistance during lithiation, the internal resistance decreases similarly to that of polyvinylidene fluoride when using fumarate homopolymer. Figure 9 As shown in (b), the internal resistance during delithiation is lowest when using fumaric acid homopolymer. This indicates that fumaric acid homopolymer exhibits excellent lithium-ion conductivity and low activation energies during lithiation and delithiation.

[0211] [Observation of the electrodes after cyclic testing]

[0212] After 1000 cycles of 5C charge-discharge cycling using half-cells with various binders, the electrode surfaces were observed using a scanning electron microscope. The results showed that no cracks were detected in the electrode using the fumaric acid homopolymer, while cracks were observed on the electrode surfaces using polyacrylic acid and polyvinylidene fluoride. This indicates that the electrode using the fumaric acid homopolymer exhibits excellent charge-discharge cycle characteristics.

[0213] (Example 3)

[0214] Electrodes and half-cells were fabricated using the fumaric acid homopolymer obtained in Example 1 as follows.

[0215] Hard carbon, conductive carbon black, and fumaric acid homopolymer were mixed in water at a mass ratio of 80:10:10 to prepare a slurry (negative electrode material).

[0216] The slurry obtained above is applied to copper foil (vertical: 20 mm, horizontal: 100 mm, thickness: 20 μm) with a coating thickness of about 100 μm using a doctor blade. After drying under reduced pressure at 80°C for 12 hours, it is then passed through rollers with a gap of 70 μm at 80°C to perform rolling pressing, thereby producing an electrode with a coating thickness of about 50 μm.

[0217] The electrodes obtained above are compressed using a hot rolling mill and cut into discs with a diameter of 13 mm, thus obtaining disc-shaped electrodes.

[0218] The disc-shaped electrode obtained above was inserted into a button cell (CR2025). The button cell was placed in a glove box filled with argon gas and the oxygen and water vapor concentrations were both below 0.5 ppm. A sodium disc was used as the counter electrode, polypropylene CELGARD was used as the separator, and a 1.0 M NaClO4 solution of ethylene carbonate / propylene carbonate (capacity ratio: 50 / 50) was used as the electrolyte to make a button cell (half cell).

[0219] For comparison of battery performance, polyacrylic acid or polyvinylidene fluoride was used instead of fumarate homopolymer as a binder, and button cells (half-cells) were manufactured in the same manner as described above. It should be noted that when using polyvinylidene fluoride, N-methyl-2-pyrrolidone was used instead of water as a solvent.

[0220] Cyclic voltammograms were investigated using half-cells with fumarate homopolymer, polyacrylic acid, or polyvinylidene fluoride as binders at scan rates of 0.1 mV / sec, 0.2 mV / sec, 0.4 mV / sec, 0.6 mV / sec, 0.8 mV / sec, or 1.08 mV / sec. The results are presented in... Figure 10 .

[0221] exist Figure 10 In the diagram, (a) is a cyclic voltammogram using fumaric acid homopolymer, (b) is a cyclic voltammogram using polyacrylic acid, and (c) is a cyclic voltammogram using polyvinylidene fluoride.

[0222] like Figure 10As shown, a reduction peak of 0.3V accompanied by electrolyte decomposition is present when any binder is used, indicating that electrolyte decomposition is suppressed. Furthermore, it is found that the overpotential difference of the desodiumization peak is 0.200V when polyacrylic acid is used as the binder, and 0.237V when polyvinylidene fluoride is used. In contrast, the overpotential difference of the desodiumization peak is 0.200V when fumarate homopolymer is used as the binder. Therefore, it is concluded that when fumarate homopolymer is used as the binder, sodium ions easily penetrate into the SEI layer, inducing sodium ion diffusion.

[0223] [Nyquist plot]

[0224] The Nyquist plots before and after cyclic voltammetry were determined using half-cells employing fumaric acid homopolymer, polyacrylic acid, or polyvinylidene fluoride as binders in the half-cell. The results are presented in… Figure 11 .

[0225] exist Figure 11 In the diagram, symbol A represents the Nyquist plot before cyclic voltammetry using a half-cell of fumaric acid homopolymer, symbol B represents the Nyquist plot after cyclic voltammetry using a half-cell of fumaric acid homopolymer, symbol C represents the Nyquist plot before cyclic voltammetry using a half-cell of polyacrylic acid, symbol D represents the Nyquist plot after cyclic voltammetry using a half-cell of polyacrylic acid, symbol E represents the Nyquist plot before cyclic voltammetry using a half-cell of polyvinylidene fluoride, and symbol F represents the Nyquist plot after cyclic voltammetry using a half-cell of polyvinylidene fluoride.

[0226] The charge movement process within the electrode is correlated with the concave portion of the Nyquist plot generated at high frequencies and the straight line of the Nyquist plot in the subsequent low-frequency region, i.e., the diffusion-controlled Warburg impedance. The smaller the value in the concave portion of the Nyquist plot, the smaller the charge movement resistance (RCT).

[0227] The Nyquist plot obtained from cyclic voltammetry using a half-cell with fumaric acid homopolymer shows a smaller value in the concave portion compared to those obtained using a half-cell with polyacrylic acid and a half-cell with polyvinylidene fluoride. This indicates a smaller charge-moving resistance (RCT). The RCT is related to the sodium ion concentration on the electrode surface where the SEI layer forms and negatively impacts cycle life. However, the smaller RCT when using fumaric acid homopolymer indicates an improved cycle life.

[0228] [activation energy]

[0229] Arrhenius diagrams were investigated using half-cells with various binders. The results are presented below. Figure 12 .exist Figure 12 In the diagram, symbol A is the Arrhenius diagram using a half-cell with fumaric acid homopolymer, symbol B is the Arrhenius diagram using a half-cell with polyacrylic acid, and symbol C is the Arrhenius diagram using a half-cell with polyvinylidene fluoride.

[0230] When the activation energy of each binder was determined from the slope of the Arrhenius plot, it was 50.7 kJ / mol for fumaric acid homopolymer, 52.9 kJ / mol for polyacrylic acid, and 58.6 kJ / mol for polyvinylidene fluoride. This indicates that the activation energy of the fumaric acid homopolymer is low, thus allowing for the smooth transport of sodium ions within the electrode.

[0231] [Initial discharge capacity]

[0232] The initial discharge capacity at a charge of 0.25C was investigated using half-cells with various binders. The results are shown in Table 2.

[0233] [Table 2]

[0234] As shown in Table 2, the initial discharge capacity of the half-cell using fumaric acid homopolymer as a binder is significantly better than that of the half-cell using polyacrylic acid or polyvinylidene fluoride as a binder.

[0235] [The Influence of Binders on Constant Current Charge-Discharge Cycling]

[0236] To evaluate its practical applicability to sodium-ion batteries, the effect of the binder on constant current charge-discharge cycling was investigated using a half-cell method with a charge capacity of 30 mA / g. The results are presented below. Figure 13 .exist Figure 13 In the diagram, symbol A represents the change in specific capacity when using fumaric acid homopolymer, symbol B represents the change in specific capacity when using polyacrylic acid, and symbol C represents the change in specific capacity when using polyvinylidene fluoride.

[0237] Depend on Figure 13 The results show that, in half-cells using fumaric acid homopolymer as a binder, compared with half-cells using polyacrylic acid or polyvinylidene fluoride as binders, the half-cells can maintain a high charge capacity even after 200 charge-discharge cycles. Therefore, the coulombic efficiency of fumaric acid homopolymer is excellent, and the long-term cycle durability of the electrode is excellent.

[0238] [Battery internal resistance]

[0239] The internal resistance of cells under sodium- and desodium-conditioning was investigated using half-cells with various binders. The results are presented below.Figure 14 .exist Figure 14 In the diagram, (a) represents the internal resistance of the half-cell during sodium formation, and (b) represents the internal resistance of the half-cell during desodium formation. Additionally, in... Figure 14 In the diagram, symbol A represents the internal resistance of a half-cell using fumaric acid homopolymer, symbol B represents the internal resistance of a half-cell using polyacrylic acid, and symbol C represents the internal resistance of a half-cell using polyvinylidene fluoride.

[0240] Depend on Figure 14 As shown in (a), for the internal resistance during sodium treatment, the internal resistance decreases similarly to that of polyvinylidene fluoride when using fumaric acid homopolymer. Figure 14 As shown in (b), the internal resistance during desodiumization is lowest when using fumaric acid homopolymer. This indicates that fumaric acid homopolymer exhibits excellent sodium ion conductivity and low activation energies during sodiumization and desodiumization.

[0241] [Observation of the electrodes after cyclic testing]

[0242] After 1000 cycles of 5C charge-discharge cycling using half-cells with various binders, the electrode surfaces were observed using a scanning electron microscope. The results showed that no cracks were detected in the electrode using the fumaric acid homopolymer, while cracks were observed on the electrode surfaces using polyacrylic acid and polyvinylidene fluoride. This indicates that the electrode using the fumaric acid homopolymer exhibits excellent charge-discharge cycle characteristics.

[0243] (Example 4)

[0244] In a 100 mL round-bottom flask, 2 g of the fumaric acid homopolymer prepared in the same manner as in Example 1 was dissolved in 50 mL of distilled water. At room temperature, 0.1 M of lithium hydroxide aqueous solution was added dropwise to the aqueous solution to adjust the pH of the aqueous solution to 7.0, thereby obtaining the reaction mixture.

[0245] By removing water from the reaction mixture obtained above, a lithium salt of fumaric acid homopolymer is obtained. The number average molecular weight of the obtained lithium salt of fumaric acid homopolymer is 4000 (m / z).

[0246] Next, using the lithium salt of the obtained fumaric acid homopolymer, half-cells were prepared in the same manner as in Examples 2 and 3, and the performance evaluation of the obtained half-cells was investigated in the same manner as in Examples 2 and 3. As a result, it was confirmed that the above-mentioned half-cells have the same performance as the half-cells obtained in Examples 2 and 3.

[0247] Example 5

[0248] (1) Preparation of imidazolium polymer (nitrogen-containing cationic polymer)

[0249] 2 g of 1-allyl-3-methylimidazolium chloride was dissolved in 100 mL of water. The resulting aqueous solution of 1-allyl-3-methylimidazolium was introduced into a column packed with ion exchange resin [manufactured by Organo Corporation, trade name: Amberlite IRN78, etc.] to allow ion exchange of 1-allyl-3-methylimidazolium, thereby obtaining an aqueous solution of 1-allyl-3-methylimidazolium hydroxide.

[0250] Next, water was evaporated from the aqueous solution of 1-allyl-3-methylimidazolium hydroxide, and dried at 60°C under reduced pressure for about 10 hours, thereby recovering 1-allyl-3-methylimidazolium hydroxide.

[0251] 200 mg of fumaric acid homopolymer and 482 mg of 1-allyl-3-methylimidazolium hydroxide, prepared in the same manner as in Example 1, were dissolved in 100 mL of water. The resulting aqueous solution was stirred at room temperature for about 10 hours, and then the water was evaporated. The resulting product was washed with acetone and then dried under reduced pressure to obtain an imidazolium polymer (1-allyl-3-methylimidazolium polymer) having repeating units as shown in Formula (III) (yield: 78%). [Chemistry 10]

[0252] (where R is in the formula) 7 (Indicates methylene).

[0253] (2) 13 C-NMR

[0254] The above-obtained oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer 13 C-NMR spectra are shown in Figure 15 .

[0255] exist Figure 15 shown 13 In the C-NMR spectrum, characteristic peaks a and c at 62.4 ppm and 30 ppm were confirmed, respectively, based on the methylene and methylene carbons of the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer.

[0256] (3) FT-IR spectroscopy

[0257] The FT-IR spectrum of the above-obtained oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer is shown in... Figure 16 .

[0258] exist Figure 16In the FT-IR spectrum shown, the wavenumber is 3500 cm⁻¹. -1 The peak at that location is based on the CO of the carboxyl group of the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer. - wavenumber 1725cm -1 The characteristic absorption peak at this point is based on the C=O group of the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer, due to a wavenumber of 1582 cm⁻¹. -1 CN stretching vibration at 1157 cm⁻¹ -1 asymmetric bending vibration and wavenumber 3151 cm at CH at the location -1 The presence of C=CH at the point confirms that it has a structure based on imidazolium.

[0259] (4) Number-average molecular weight

[0260] The MALDI-TOF mass spectrometry analysis of the obtained oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer confirmed that the number-average molecular weight of the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer was 4000 (m / z).

[0261] (5) Thermogravimetric analysis

[0262] Thermogravimetric analysis (TGA) was performed on the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer. The results showed that the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer experienced an initial weight loss at approximately 150 °C. This initial weight loss was higher than that of the fumaric acid homopolymer, indicating that the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer exhibits superior heat resistance (thermal stability) compared to the fumaric acid homopolymer. Therefore, the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer demonstrates excellent thermal stability and is suitable as a binder for metal-ion secondary batteries used at high temperatures.

[0263] Example 6

[0264] Electrodes were fabricated using the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer obtained in Example 4, as follows.

[0265] A slurry (negative electrode material) was prepared by mixing battery-grade graphite [Sigma-Aldrich], conductive carbon [Alfa Aesar], and an oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer as a binder in water at a mass ratio of 80:10:10.

[0266] The slurry obtained above was coated onto copper foil (vertical: 20 mm, horizontal: 100 mm, thickness: 20 μm) with a coating thickness of approximately 100 μm using a doctor blade. The coating was then dried under reduced pressure at 80 °C for 24 hours to fabricate an electrode. The electrode obtained above was then cut into a disc with a diameter of 13 mm to obtain a disc-shaped electrode.

[0267] In the case of sodium-ion secondary batteries, the disc-shaped electrode obtained above is inserted into a button cell (CR2025). The button cell is placed in a glove box filled with argon gas, and the oxygen and water vapor concentrations are both below 0.5 ppm. A sodium disc is used as the counter electrode, glass fiber [manufactured by Whatman Corporation] is used as the separator, and a 1.0 M NaClO4 solution of ethylene carbonate / diethyl carbonate (capacity ratio: 50 / 50) is used as the electrolyte to make a button cell (half cell).

[0268] In the case of lithium-ion secondary batteries, the disc-shaped electrode obtained above is inserted into a button cell (CR2025). The button cell is placed in a glove box filled with argon gas and the oxygen and water vapor concentrations are both below 0.5 ppm. A lithium disc is used as the counter electrode, polypropylene CELGARD is used as the separator, and a 1.0 M LiPF6 ethylene carbonate / diethyl carbonate (capacity ratio: 50 / 50) solution is used as the electrolyte to make a button cell (half cell).

[0269] (1) Adhesive bonding strength

[0270] The adhesive strength of the binder was evaluated based on the stress during peeling of the adhesive tape. The adhesive strength of the binder using oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer as the binder was approximately 11 N, indicating high adhesive strength. Therefore, oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer is considered useful for addressing volume expansion during lithiation in electrodes and preventing electrode assembly disintegration during delithiation.

[0271] (2) Electrochemical characteristics

[0272] [Electrochemical Stability]

[0273] The electrochemical stability of the binder within the electrode was evaluated using cyclic voltammetry. Cyclic voltammetry was investigated using a half-cell of the lithium-ion secondary battery obtained above at scan rates of 0.1 mV / sec or 0.2 mV / sec. The results are presented below. Figure 17 .

[0274] When using the aforementioned half-cell, by Figure 17As shown in the cyclic voltammogram, a reduction peak exists at approximately 0.6 V, accompanying electrolyte decomposition. Furthermore, in the aforementioned cyclic voltammogram, the overpotential difference of the delithiation peak is 0.150 V between scan rates of 0.1 mV / sec and 1.0 mV / sec, which is lower than the overpotential difference of 0.196 V when using polyvinylidene fluoride as a binder. This indicates that the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer promotes lithium-ion transport, thereby reducing the battery's internal impedance.

[0275] [Nyquist plot]

[0276] The Nyquist plots before cyclic voltammetry were investigated for half-cells of lithium-ion secondary batteries using oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer or polyvinylidene fluoride as binders in the half-cell. The results are presented in… Figure 18 .

[0277] exist Figure 18 In the diagram, symbol A represents the Nyquist plot using a half-cell with an oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer, and symbol B represents the Nyquist plot using a half-cell with polyvinylidene fluoride.

[0278] The charge movement process within the electrode is correlated with the concave portion of the Nyquist plot generated at high frequencies and the straight line of the Nyquist plot in the subsequent low-frequency region, i.e., the diffusion-controlled Warburg impedance. The smaller the value in the concave portion of the Nyquist plot, the smaller the charge movement resistance (RCT).

[0279] The Nyquist plot obtained by cyclic voltammetry using a half-cell of oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer is smaller than that obtained by cyclic voltammetry using a half-cell of polyvinylidene fluoride, indicating that the charge-moving resistance (RCT) is smaller.

[0280] The charge-moving resistance (RCT) is related to the concentration of lithium ions on the electrode surface where the SEI layer is formed, which has an adverse effect on cycle life. However, when using the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer, the charge-moving resistance (RCT) is small, thus improving cycle life.

[0281] [activation energy]

[0282] Arrhenius plots were investigated using half-cells of lithium-ion secondary batteries employing oxycarbonylmethylene-1-allyl-3-methylimidazolium polymers or polyvinylidene fluoride as binders. The results are presented in… Figure 19 .

[0283] exist Figure 19In the diagram, symbol A is the Arrhenius diagram using a half-cell with oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer, and symbol B is the Arrhenius diagram using a half-cell with polyvinylidene fluoride.

[0284] When determining the activation energy of each binder using the slope of the Arrhenius plot, the activation energy was 36.2 kJ / mol in the half-cell using the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer, and 62.1 kJ / mol in the half-cell using polyvinylidene fluoride. This indicates that the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer has a lower desolvation activation energy compared to polyvinylidene fluoride, thus ions are transported smoothly in the electrode. Furthermore, this suggests that the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer (a nitrogen-containing cationic polymer) is also useful as an electrolyte.

[0285] [Specific Capacity]

[0286] The specific capacity of lithium-ion secondary batteries was investigated stepwise from 0.1C to 2C using half-cells of lithium-ion secondary batteries employing oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer or polyvinylidene fluoride as binders. The results are presented below. Figure 20 .

[0287] like Figure 20 As shown, in the half-cell using the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer, the specific capacity from 0.1C to 2C is 355 mAh / g, 348 mAh / g, 308 mAh / g, 260 mAh / g, and 110 mAh / g, respectively. In contrast, in the half-cell using polyvinylidene fluoride (PVDF), the specific capacity from 0.1C to 2C is 326 mAh / g, 226 mAh / g, 184 mAh / g, 150 mAh / g, and 64 mAh / g, respectively. This indicates that the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer, compared to PVDF, promotes lithium-ion transport in the electrode and exhibits a high specific capacity over a wide range of applied current densities. Furthermore, this suggests that the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer (a nitrogen-containing cationic polymer) is also useful as an electrolyte.

[0288] [The Influence of Binders on Constant Current Charge-Discharge Cycling]

[0289] To evaluate its practical applicability to lithium-ion batteries, the effect of the binder on constant current charge-discharge cycling was investigated using a half-cell of a lithium-ion secondary battery at a charge capacity of 5C. The results are presented below. Figure 21 .

[0290] exist Figure 21In the diagram, symbol A represents the change in specific capacity using a half-cell with an oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer, and symbol B represents the change in specific capacity using a half-cell with polyvinylidene fluoride.

[0291] Depend on Figure 21 The results show that in half-cells using oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer as a binder, a high specific capacity of approximately 85 mAh / g can be maintained even after 1000 charge-discharge cycles. Therefore, oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer exhibits excellent coulombic efficiency and excellent long-term cycling durability of the electrode.

[0292] [Battery internal resistance]

[0293] The internal resistance of a lithium-ion secondary battery half-cell under lithiation and delithiation was investigated using either an oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer or polyvinylidene fluoride as a binder. The results are presented in… Figure 22 .

[0294] exist Figure 22 In the diagram, (a) represents the internal resistance during lithiation, and (b) represents the internal resistance during delithiation. Additionally, in... Figure 22 In the diagram, symbol A represents the internal resistance when using a half-cell with an oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer, and symbol B represents the internal resistance when using a half-cell with polyvinylidene fluoride.

[0295] Depend on Figure 22 The results show that the half-cell using the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer exhibits lower internal resistance during lithiation and delithiation compared to the half-cell using polyvinylidene fluoride. This indicates that the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer possesses excellent lithium-ion conductivity and low activation energies during lithiation and delithiation. Furthermore, this suggests that the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer (a nitrogen-containing cationic polymer) is also useful as an electrolyte.

[0296] [Observation of the electrodes after cyclic testing]

[0297] After 1000 cycles of 5C charge-discharge cycling using a half-cell employing an oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer and a half-cell employing polyvinylidene fluoride (PVDF), the surface of the electrodes was observed using a scanning electron microscope. The results showed that no cracks were detected in the electrode using the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer, while surface cracks were observed in the PVDF electrode. This indicates that the electrode using the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer exhibits excellent charge-discharge cycling characteristics. Furthermore, this suggests that the oxycarbonylmethylene-1-allyl-3-methylimidazolium polymer (a nitrogen-containing cationic polymer) is also useful as an electrolyte.

[0298] The results above demonstrate that the binder for metal-ion secondary batteries of the present invention exhibits excellent adhesion to the active material and to the current collector, thereby improving coulombic efficiency while suppressing electrolyte decomposition. Furthermore, the binder for metal-ion secondary batteries of the present invention demonstrates excellent long-term cycling performance, enabling the realization of high-speed charging and high-load charge-discharge electrochemical performance in metal-ion secondary batteries.

[0299] The adhesive for metal-ion secondary batteries of the present invention not only has excellent adhesion to metal substrates and excellent charge-discharge cycle characteristics, but also maintains the shape of the electrodes without cracking even after repeated charge-discharge cycles. Therefore, it is suitable as an adhesive for metal-ion secondary batteries, and it is expected to open the door to applications in rechargeable high-energy batteries.

[0300] Furthermore, the electrolyte of the present invention contains a nitrogen-containing cationic polymer used in the binder for metal-ion secondary batteries, thus exhibiting excellent charge-discharge cycle characteristics, and is therefore expected to be used as an electrolyte for metal-ion secondary batteries.

[0301] Industrial applicability

[0302] The binder for metal-ion secondary batteries of the present invention is expected to be used as a binder in pigment-sensitized solar cells, capacitors, and light-emitting devices, represented by metal-ion secondary batteries. Furthermore, metal-ion secondary batteries using the above-mentioned binder exhibit high discharge capacity and excellent charge-discharge durability, thus promising wide applications from small portable devices to transportation systems, such as smartphones, tablet PCs, hybrid vehicles, and electric vehicles.

Claims

1. A nitrogen-containing cationic polymer having repeating units as shown in formula (I), [Chemistry 1] In the formula, X + Indicates containing N + A cyclic cation.

2. A binder for metal-ion secondary batteries, comprising a nitrogen-containing cationic polymer having repeating units as shown in formula (I) as the binder polymer. [Chemistry 2] In the formula, X + Indicates containing N + A cyclic cation.

3. A negative electrode for a metal-ion secondary battery, comprising the binder for a metal-ion secondary battery as described in claim 2.

4. A metal-ion secondary battery, comprising a positive electrode, a negative electrode, and a separator disposed between the positive and negative electrodes, wherein, The negative electrode is the negative electrode for the metal-ion secondary battery according to claim 3.

5. An electrolyte for a metal-ion secondary battery, comprising a nitrogen-containing cationic polymer having repeating units as shown in formula (I) as the electrolyte. [Chemistry 3] In the formula, X + Indicates containing N + A cyclic cation.

Citation Information

Patent Citations

  • Negative electrode for lithium ion secondary battery and lithium ion secondary battery using the same

    JP2017152123A

  • Negative electrode binder for lithium ion secondary battery, negative electrode for lithium ion secondary battery using the same, and lithium ion secondary battery

    JP2019175629A

  • Lithium ion secondary battery

    WO2019212040A1