Cathode Frame for Solid State Batteries
By using a combination of frame structure and adhesive layer in solid-state lithium batteries, the problem of difficult deformation of solid materials during assembly was solved, achieving stable assembly of electrochemical stacks and improving the structural integrity of batteries.
Patent Information
- Application Number
- CN202580028495.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-19
- Filing Date
- 2025-04-18
- Publication Date
- 2026-11-17
AI Technical Summary
Maintaining the structural integrity of battery components during the assembly of electrochemical stacks for solid-state lithium batteries presents challenges, especially due to the difficult-to-deform properties of solid materials.
The system employs a frame structure, which surrounds the four subsurfaces of the solid cathode, contacts the cathode current collector and the solid diaphragm, and is connected by an adhesive layer. Combined with pressure and temperature treatment, the structural stability during assembly is ensured.
It effectively maintains the structural integrity of the electrochemical stack, improving the assembly efficiency and reliability of solid-state lithium batteries.
Smart Images

Figure CN123125702A_ABST
Abstract
Description
Cross-references to related applications
[0001] This application claims priority and benefit to U.S. Provisional Patent Application No. 63 / 636,655 (filed April 19, 2024), the entire contents of which are incorporated herein by reference for all purposes. Technical Field
[0002] This application relates to an electrochemical stack having a frame for a solid cathode, and a method for assembling an electrochemical stack having a frame for a solid-state battery. Background Technology
[0003] Solid-state lithium batteries offer several advantages over conventional lithium-ion batteries that rely solely on liquid-based electrolytes. However, solids are inherently more difficult to deform than liquids, making stack assembly more challenging. One such challenge is maintaining the structural integrity of the battery components during assembly.
[0004] Therefore, there is a need for electrochemical stacks having a frame for a solid cathode, and methods for assembling such electrochemical stacks with the frame. This application describes such electrochemical stacks and methods. Summary of the Invention
[0005] In a first aspect, this application provides an electrochemical stack comprising: a) a solid cathode having two main surfaces, four subsurfaces, a first width, and a first length, said solid cathode comprising a solid cathode electrolyte; b) a solid membrane having a second width and a second length; c) a cathode current collector; d) an adhesive layer; and e) a frame surrounding the four subsurfaces of said solid cathode; wherein the frame is located between and in contact with the cathode current collector and the solid membrane; the adhesive layer is located between and in contact with the solid cathode and the solid membrane; the first width is less than the second width; and the first length is less than the second length.
[0006] In a second aspect, this application provides an electrochemical stack comprising: a) a solid cathode having two primary surfaces and four secondary surfaces, the solid cathode comprising a solid cathode electrolyte; b) a solid membrane; c) a cathode current collector; d) an adhesive layer; and e) a frame surrounding the four secondary surfaces of the solid cathode; wherein the frame is located between and in contact with the cathode current collector and the solid membrane; wherein the adhesive layer is located between and in contact with the solid cathode and the solid membrane.
[0007] In a third aspect, this application provides a method for assembling an electrochemical stack, the method comprising: (1) providing an electrochemical stack; the electrochemical stack comprising: the frame, solid cathode, bonding layer and solid membrane described in this application; and (2) applying a pressure of about 70 kPa to about 700 kPa to the electrochemical stack.
[0008] In a fourth aspect, this application provides a method for assembling an electrochemical stack, the method comprising: (1) Provide the framework described in this application; (2) Provide a solid cathode with an adhesive layer on a main surface; (3) The solid cathode is placed within the frame, which surrounds all four subsurfaces of the solid cathode, thereby forming a sub-pile; (4) Apply a pressure of about 70 kPa to about 700 kPa to the sub-piles at a temperature of about 65 °C to about 75 °C; (5) Placing a solid membrane on the adhesive layer, thereby forming an electrochemical stack; and (6) Apply a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 80 °C to about 160 °C.
[0009] In a fifth aspect, this application provides a method for assembling an electrochemical stack, the method comprising: (1) Provide the framework described in this application; (2) A solid cathode is placed within the frame, wherein the frame surrounds all four subsurfaces of the solid cathode, thereby forming a sub-pile. (3) Apply a pressure of about 70 kPa to about 700 kPa to the sub-piles at a temperature of about 65 °C to about 75 °C; (4) Provide a solid membrane with an adhesive layer; (5) A framed solid cathode is placed on the adhesive layer, thereby forming an electrochemical stack; and (6) Apply a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 80 °C to about 160 °C.
[0010] In a sixth aspect, this application provides a method for assembling an electrochemical stack, the method comprising: (1) Provide the framework described in this application; (2) The frame is placed on a solid diaphragm, thereby forming a sub-pile; (3) Apply a pressure of about 70 kPa to about 700 kPa to the sub-piles at a temperature of about 65 °C to about 75 °C; (4) Provide a solid cathode with an adhesive layer on a main surface; (5) A solid cathode with an adhesive layer is placed on a framed solid membrane, the frame surrounding the four subsurfaces of the solid cathode, and the adhesive layer is in contact with the solid membrane, thereby forming an electrochemical stack; and (6) Apply a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 80 °C to about 160 °C.
[0011] In a seventh aspect, this application provides a method for assembling an electrochemical stack, the method comprising: (1) Provide the framework described in this application; (2) Provide a solid membrane with an adhesive layer; (3) Place the frame on the solid membrane; (4) Apply a pressure of about 70 kPa to about 700 kPa at a temperature of about 65 °C to about 75 °C; (5) A solid cathode is placed on a framed solid diaphragm, the frame surrounding the four subsurfaces of the solid cathode, and the adhesive layer is in contact with the solid cathode, thereby forming an electrochemical stack; and (6) Apply a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 80 °C to about 160 °C.
[0012] In an eighth aspect, this application provides a method for assembling an electrochemical stack, the method comprising: (1) Provide the framework described in this application; (2) Provide a solid cathode with an adhesive layer on a main surface; (3) The solid cathode is placed in the frame surrounding the four subsurfaces of the solid cathode, and a solid diaphragm is placed on the adhesive layer, thereby forming an electrochemical stack; (4) Applying a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 65 °C to about 75 °C; and (5) Apply a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 80 °C to about 160 °C.
[0013] In a ninth aspect, this application provides a method for assembling an electrochemical stack, the method comprising: (1) Provide the framework described in this application; (2) Provide a solid membrane with an adhesive layer; (3) A solid cathode is placed inside the frame, the frame surrounding the four subsurfaces of the solid cathode, and a solid diaphragm with an adhesive layer is placed on the framed solid cathode, the adhesive layer being in contact with the solid cathode, thereby forming an electrochemical stack; (4) Apply a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 65 °C to about 75 °C; (5) Apply a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 80 °C to about 160 °C. Attached Figure Description
[0014] Figure 1 is a cross-sectional view of an electrochemical stack, which includes a frame surrounding a solid cathode and in contact with a solid diaphragm and a cathode current collector.
[0015] Figure 2 is a vertical stacking diagram of an electrochemical stack, which includes a frame located between a solid membrane and a cathode current collector.
[0016] Figure 3A is a cross-sectional view of a three-layer frame, each layer having a thickness.
[0017] Figure 3B is a cross-sectional view of a two-layer frame, each layer having a thickness.
[0018] Figure 4 is a top view of the frame surrounding the solid cathode.
[0019] Figure 5 is a three-dimensional view of a solid cathode with four subsurfaces and two primary surfaces.
[0020] Figure 6 shows the effect of compressing electrochemical stacks with and without a frame.
[0021] Figure 7 is a cross-sectional view of the electrochemical stack, which includes a two-layer frame that surrounds the solid cathode and contacts the solid membrane and the cathode current collector.
[0022] Figure 8 is a cross-sectional view of the electrochemical stack, which includes a three-layer frame surrounding a solid cathode and contacting a solid membrane and a cathode current collector.
[0023] Figure 9 is a top view of the framework disclosed in this application.
[0024] Figure 10 is a top view of the open frame disclosed in this application.
[0025] Figure 11 is a cross-sectional view of a three-story frame, one of which has an opening.
[0026] Figure 12 is a cross-sectional view of a two-layer frame, one of which has an opening. Detailed Implementation I. Definition
[0027] In this application, the term "about" when modifying a numerical value (e.g., 15 wt% (w / w)) refers to the modified numerical value, and optionally includes values within a range of ±10% of the modified numerical value. For example, about 15 wt% (w / w) includes 15 wt% (w / w), as well as 13.5 wt% (w / w), 14 wt% (w / w), 14.5 wt% (w / w), 15.5 wt% (w / w), 16 wt% (w / w), or 16.5 wt% (w / w). For example, "about 75 °C" includes 75 °C, as well as 68 °C, 69 °C, 70 °C, 71 °C, 72 °C, 73 °C, 74 °C, 75 °C, 76 °C, 77 °C, 78 °C, 79 °C, 80 °C, 81 °C, 82 °C, or 83 °C. For example, evaporating a solvent at about 80 °C includes evaporating a solvent at 79 °C, 80 °C, or 81 °C.
[0028] In this application, "selected from a group consisting of..." means selected from one member of that group, multiple members of that group, or a combination of members of that group. Members selected from a group consisting of A, B, and C include, for example, only A, only B, or only C, as well as A and B, A and C, B and C, and A, B, and C.
[0029] In this application, the phrase "electrochemical cell" or "cell" refers to a single cell comprising a cathode and an anode, which are ionically connected by an electrolyte. In some embodiments, the same cell may comprise multiple cathodes and / or multiple anodes encapsulated in the same container.
[0030] In this application, the term "surface" refers to material at the interface between two different phases, chemical substances, or states of matter. For example, a solid electrolyte membrane, when exposed to air, has a surface described by the periphery or outer portion of the membrane in contact with air. For a rectangular thin-film membrane, there are a top surface and a bottom surface (or main surface), each with a surface area greater than the surface area of each of the four side surfaces (or secondary surfaces). In this example of a rectangular membrane, there are four side surfaces, each with a surface area smaller than the surface area of either or both of the top and bottom surfaces. For a disk-shaped thin-film membrane, there are a top surface and a bottom surface, each with a surface area greater than the surface area of the circumferential side surfaces of the disk. When used as an electrolyte membrane in an electrochemical cell, the top or bottom surface is the side or portion of the membrane in contact with the anode (i.e., Li metal), the cathode, or the cathode electrolyte, and / or a layer or adhesive disposed between the electrolyte membrane and the cathode. The physical dimensions of the surface in the x-axis and y-axis directions are greater than its physical dimensions in the z-axis direction, where the z-axis is the axis perpendicular to the surface. The depth or thickness of the surface can be on the molecular scale or up to 1 micrometer. The membrane surface may include dangling bonds, excess hydroxyl groups, bridged oxides, or a variety of other components that result in a chemical composition on the membrane surface that may differ stoichiometrically from the bulk. In this application, the term "bulk" refers to a portion of the membrane extending at least 1 micrometer in three dimensions in space. Bulk refers to the portion of the material excluding its surface (as defined above).
[0031] In this application, the terms "cathode" and "anode" refer to the electrodes of the battery. During the charging cycle of a lithium secondary battery, Li ions leave the cathode, pass through the electrolyte, and reach the anode. During the charging cycle, electrons leave the cathode and reach the anode through the external circuit. During the discharging cycle of a lithium secondary battery, Li ions migrate from the anode to the cathode through the electrolyte. During the discharging cycle, electrons leave the anode and reach the cathode through the external circuit. The cathode active material of this application is not particularly limited, and known cathode active materials used in all-solid-state batteries can be used. Specific examples of such cathode active materials include the following: manganese oxide (MnO), iron oxide, copper oxide, nickel oxide, lithium-manganese composite oxides (e.g., LiMn2O4 or LiMnO2), lithium-nickel composite oxides (e.g., LiNiO2), lithium-cobalt composite oxides (e.g., LiCoO2), and lithium-cobalt-nickel oxides (LiNiO2). 1-y Co y O2), lithium-manganese-cobalt composite oxides (e.g., LiMn) y Co 1-y O2), lithium-nickel-manganese-cobalt oxides (e.g., LiNi) x Mn y Co 1-x-y O2), lithium-nickel-cobalt-aluminum oxides (e.g., LiNi)x Al y Co 1-x-y O₂), spinel-phase lithium-manganese-nickel composite oxides (e.g., LiMn 1.5 Ni 0.5 O₄), lithium phosphates with an olivine structure (e.g., LiFePO₄, which is also referred to as LFP, and LiCoPO₄), lithium iron manganese phosphates (e.g., LiFeMnPO₄, also referred to as LMFP), lithium phosphates with a NASICON-type structure (e.g., Li₇V₂(PO₄)₃), iron(III) sulfate (Fe₂(SO₄)₃) and vanadium oxides (e.g., V₂O₅). One type thereof may be used alone, or two or more types thereof may be used in combination. Preferably, x and y in these chemical formulas fall within the ranges of 0<x<1 and 0<y<1.
[0032] In the present application, "catholyte" refers to an ionic conductor that is intimately mixed with, surrounds, or is in contact with the cathode active material. Catholytes suitable for the embodiments described herein include, but are not limited to, catholytes with the generic names LPS, LXPS, LXPSO (where X is Si, Ge, Sn, As, Al), LATS, or lithium-filled garnets, or combinations thereof, etc. The catholytes include those set forth in U.S. Patent Application Publication No. 2015-0171465 (published on June 18, 2015, entitled SOLID STATE CATHOLYTE OR ELECTROLYTE FOR BATTERY USING Li A MP B S C (M = Si, Ge, AND / OR Sn)), the entire content of which is incorporated herein by reference in its entirety.
[0033] In the present application, the phrase "solid-state cathode" refers to a cathode that does not include a liquid-phase electrolyte.
[0034] In the present application, the phrase "double-sided solid-state cathode" refers to two solid-state cathode layers, with one or two cathode current collectors disposed between the two solid-state cathode layers to separate the two solid-state cathode layers.
[0035] In the present application, the phrases "solid-state catholyte", "solid catholyte" or the term "catholyte" refer to an ionic conductor that is intimately mixed with or surrounded by the solid cathode active material.
[0036] In this application, the phrase "current collector" refers to a component or layer in a secondary battery that is in direct contact with the electrodes, through which electrons are conducted to or from the electrodes to form an external circuit loop. In some embodiments, the current collector is a layer of metal (e.g., Al, Cu, or Ni, steel, alloys thereof, or combinations thereof) laminated to the cathode or anode. In some embodiments, the current collector is Al. In some embodiments, the current collector is Cu. In some embodiments, the current collector is Ni. In some embodiments, the current collector is steel. In some embodiments, the current collector is an alloy of Al. In some embodiments, the current collector is an alloy of Cu. In some embodiments, the current collector is an alloy of steel. In some embodiments, the current collector is Al. In some embodiments, the current collector is coated with carbon. In some embodiments, the current collector comprises a combination of the above metals. During charging and discharging, electrons move in the opposite direction to the flow of Li ions, passing through the current collector as they enter or leave the electrodes.
[0037] In this application, the phrase "adhesive layer" refers to a layer containing a borohydride compound that adheres a lithium-filled garnet layer to a sulfide electrolyte layer or a sulfide-containing buffer layer. The borohydride can be any compound described in WO2018 / 075972 (published April 26, 2018, filed as international PCT patent application PCT / US2017 / 057735, entitled "ELECTROLYTE SEPARATORS INCLUDING LITHIUM BOROHYDRIDE AND COMPOSITE ELECTROLYTE SEPARATORS OF LITHIUM-STUFFED GARNET AND LITHIUMBOROHYDRIDE"), the entire contents of which are incorporated herein by reference for all purposes. The borohydride may be any compound described in WO2019078897A1 (published on April 25, 2019, filed on October 20, 2017 as international PCT patent application PCT / US2017 / 057739, entitled "BOROHYDRIDE-SULFIDE INTERFACIAL LAYER IN ALL SOLID STATE BATTERY"), the entire contents of which are incorporated herein by reference for all purposes.
[0038] In this application, the term "electrolyte" refers to a permissible ion (e.g., Li) +A material through which electrons can conduct electricity, but not electrons. The electrolyte electrically isolates the cathode and anode of a secondary battery while allowing ions (e.g., Li) to conduct electricity. + The ion passes through the electrolyte. The electrolyte is a material that can conduct ions while being electrically insulating. Electrolytes are used to electrically insulate the cathode and anode of a secondary battery, while allowing ions (such as Li) to pass through. + Conduction occurs through the electrolyte.
[0039] In this application, the terms "solid-state membrane," "thin-film solid-state membrane," "thin solid-state membrane," "solid electrolyte membrane," "solid membrane," or "membrane" are used interchangeably, referring to membranes capable of conducting Li. + Ions are essentially insulating to electrons (e.g., lithium-ion conductivity is at least 10 times that of electron conductivity). 3 Times, often 10 6 The membrane is a material that acts as a physical barrier or spacer between the cathode and anode electrodes in an electrochemical or rechargeable battery. In one embodiment, the membrane is a thin-film garnet membrane, such as a lithium-filled garnet film. In another embodiment, the membrane is a bare membrane or a membrane on a foil.
[0040] In this application, "thin" in the context of modifying solid membranes refers to a thickness of less than 200 µm, sometimes less than 100 µm, in some cases between 0.1 µm and 60 µm, and in others between about 10 nm and about 100 µm; in still others, the thickness is about 1 µm, 10 µm, or 50 µm.
[0041] In this application, the "thickness" of the membrane refers to the shortest vertical distance between the top and bottom surfaces of the membrane, or the median of the measured shortest vertical distances. In this application, the top and bottom surfaces refer to the sides of the membrane with the largest surface area. In this application, the thickness of the electrolyte membrane or membrane is measured using cross-sectional scanning electron microscopy.
[0042] In this application, the phrase "active electrode material" or "active material" refers to a material suitable for use in rechargeable lithium batteries and that undergoes a chemical reaction during charge and discharge cycles.
[0043] In this application, the term "manufacturing" refers to the process or procedure that forms or causes the object to be manufactured. For example, manufacturing an energy storage electrode includes processes, steps, or procedures that cause the formation of an electrode for an energy storage device. The end result of these steps constituting the manufacture of an energy storage electrode is the production of material that can be used as an electrode.
[0044] In this application, the phrase "electrochemical device" refers to an energy storage device, such as, but not limited to, a secondary lithium battery that operates or generates electricity or current through an electrochemical reaction.
[0045] In this application, the phrase "provide" refers to supplying, generating, presenting or delivering the thing being provided.
[0046] In this application, the phrase "lithium-filled garnet" refers to a membrane characterized by a crystal structure related to the garnet crystal structure. Lithium-filled garnets include those of the formula Li A La B M' c M" D Zr E O F , Li A La B M' C M" D Ta E O F or Li A La B M' C M" D Nb E O F compounds, wherein 4<A<8.5, 1.5<B<4, 0≤C≤2, 0≤D≤2, 0≤E<2, 10<F<13, and M' and M" are each independently selected in each case from Al, Mo, W, Nb, Sb, Ca, Ba, Sr, Ce, Hf, Rb or Ta; or of the formula Li a La b Zr c Al d Me" e O f compounds, wherein 5<a<7.7, 2<b<4, 0<c≤2.5, 0≤d<2, 0≤e<2, 10<f<13, and Me'' is a metal selected from Nb, V, W, Mo, Ta, Ga or Sb, as described in this application. The garnets in this application also include the aforementioned garnets doped with Al2O3. The garnets in this application also include those aforementioned garnets doped such that Al 3+ substitutes for Li + as described above. The lithium-filled garnets and garnets in this application generally include, but are not limited to, Li 7.0 La3(Zr t1 + Nb t2 + Ta t3 )O 12 + 0.35Al2O3; wherein (t1+t2+t3 = subscript 2), such that the La:(Zr / Nb / Ta) ratio is 3:2. Furthermore, the garnets used in this application include, but are not limited to, Li x La3Zr2O 12+ yAl₂O₃, where x is in the range of 5.5 to 9 and y is in the range of 0 to 1. In some examples, x is 7 and y is 1.0. In some examples, x is 7 and y is 0.35. In some examples, x is 7 and y is 0.7. In some examples, x is 7 and y is 0.4. Furthermore, the garnet in this application includes, but is not limited to, Li. x La3Zr2O 12 + yAl2O3.
[0047] In this application, garnet does not include YAG-garnet (i.e., yttrium aluminum garnet, or, for example, Y3Al5O). 12 In this application, garnet does not include silicate-based garnets such as pyrope, almandine, spessartine, grossular, hessonite or cinnamonstone, tsavorite, uvarovite, and andradite, as well as solid solutions of pyrope-almandine-spessartine and uvarovite-grossular-andradite. Garnet in this application does not include island silicates having the general formula X3Y2(SiO4)3, where X is Ca, Mg, Fe, and / or Mn, and Y is Al, Fe, and / or Cr.
[0048] In this application, the terms "LZO" or "LLZO" refer to Li2ZrO3, ZrO2, or a combination thereof.
[0049] The term "double layer" in this application includes a ceramic layer deposited on a metal layer. The sintered double layer may have a ceramic layer thickness of 10 µm to 50 µm and a metal layer thickness of 2 µm to 20 µm. Alternatively, the double layer may have a ceramic layer thickness of 20 µm to 30 µm and a metal layer thickness of 3 µm to 10 µm.
[0050] In this application, the "Gurley number" refers to the time (in seconds) required for 100 cubic centimeters (cc) of air to pass through a one-square-inch material sample under a pressure difference of 1.21 kPa. The Gurley number depends on the thickness of the sample being tested. The thickness of the samples measured in this application is between approximately 50 µm and 150 µm.
[0051] In this application, "Poisson's ratio" refers to the deformation of a material under applied force. It is the ratio of the strain experienced by the material in the direction perpendicular to the applied force (i.e., transverse strain) to the strain experienced by the material in the direction of the applied force (i.e., longitudinal strain). Transverse strain is a measure of the change in diameter of a cylindrical material relative to its original diameter under longitudinal force, while longitudinal strain is a measure of the change in thickness of the cylinder. The Poisson's ratio measured in this application was obtained by applying a pressure of approximately 250 kPa to approximately 700 kPa at a temperature of approximately 110 °C to approximately 150 °C. II. Electrochemical Stack
[0052] In a first aspect, this application provides an electrochemical stack comprising: a) a solid cathode having two main surfaces, four subsurfaces, a first width, and a first length, the solid cathode comprising a solid cathode electrolyte; b) a solid membrane having a second width and a second length; c) a cathode current collector; d) an adhesive layer; and e) a frame surrounding the four subsurfaces of the solid cathode; the frame being located between and in contact with the cathode current collector and the solid membrane; the adhesive layer being located between and in contact with the solid cathode and the solid membrane; the first width being less than the second width; and the first length being less than the second length.
[0053] In some embodiments, including any of the above embodiments, the electrochemical stack includes a second solid cathode, a second solid membrane, a second bonding layer, and a second frame. In some embodiments, the electrochemical stack includes a double-sided solid cathode.
[0054] In some embodiments, including any of the above embodiments, the frame is attached to the solid-state diaphragm and the cathode current collector. In other embodiments, the frame is attached to the solid-state diaphragm. In still other embodiments, the frame is attached to the current collector.
[0055] In some embodiments, including any of the above embodiments, the frame surrounds and contacts all four subsurfaces of the solid-state cathode. In some embodiments, the frame surrounds and contacts at least one of the four subsurfaces of the solid-state cathode. In other embodiments, the frame surrounds the four subsurfaces of the solid-state cathode but does not contact any one of the four subsurfaces. In some embodiments, a gap exists between at least one of the four subsurfaces of the solid-state cathode and the frame. In some embodiments, gaps exist between all four subsurfaces of the solid-state cathode and the frame.
[0056] In some implementations, the framework comprises a thermoplastic polymer.
[0057] In some embodiments, including any of the above embodiments, the framework includes a modified thermoplastic polymer. In some embodiments, the modified thermoplastic polymer is a copolymer. In other embodiments, the modified thermoplastic polymer is a homopolymer of a modified monomer. In other embodiments, the modified thermoplastic polymer is a thermoplastic polymer with additives that alter the properties of the native polymer. In other embodiments, the modified thermoplastic polymer is a crosslinked polymer. In other embodiments, the modified thermoplastic polymer is a polymer functionalized with functional groups. In some embodiments, the functional groups are selected from vinyl acetate, vinyl alcohol, halides (e.g., chlorides or fluorides), terephthalates, alkyl groups, propyl groups, acrylic acid, maleic anhydride, or combinations thereof.
[0058] In some embodiments, the thermoplastic polymer is selected from polyethylene polymers, polypropylene polymers, polybutene polymers, polypentene polymers, polystyrene polymers, polyaryletherketone polymers, polyimide polymers, polyaryletherimide polymers, polysulfone polymers, acrylate polymers, polycarbonate polymers, or combinations thereof.
[0059] In some embodiments, the polyimide polymer is a porous polyimide polymer. In some embodiments, the porosity of the porous polyimide polymer is about 60% to 80% by volume. In some embodiments, the pore size of the porous polyimide polymer is about 0.01 µm to about 2 µm, or about 0.01 µm to about 1 µm.
[0060] In some embodiments, the thermoplastic polymer is selected from modified polyethylene polymers, modified polypropylene polymers, modified polybutene polymers, modified polypentene polymers, modified polystyrene polymers, modified polyaryletherketone polymers, modified polyaryletherimide polymers, modified polysulfone polymers, modified acrylate polymers, modified perfluoroelastomer polymers, modified polycarbonate polymers, or combinations thereof.
[0061] In some embodiments, the thermoplastic polymer is selected from acrylonitrile-butadiene-styrene (ABS), ethylene-propylene rubber (EPM), ethylene propylene diene monomer (EPDM), fluorinated ethylene propylene (FEP), perfluoroelastomer (FFKM), polybutene-1 (PB-1), polycarbonate (PC), polyetheretherketone (PEEK), polyetherimide (PEI), polyethersulfone (PES), polyethylene terephthalate (PET), polyisobutylene (PIB), polyisoprene, poly(methyl methacrylate) (PMMA), polymethylpentene (PMP), polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-co-fluorinated ethylene propylene (PVDF-co-FEP), poly(styrene-isoprene-styrene) (SIS), poly(styrene-butadiene-styrene) (SBS), ultra-high molecular weight polyethylene (UHWPE), or combinations thereof. In some embodiments, the thermoplastic polymer is acrylonitrile-butadiene-styrene (ABS). In some embodiments, the thermoplastic polymer is ethylene-propylene rubber (EPM). In some embodiments, the thermoplastic polymer is ethylene propylene diene monomer (EPDM). In some embodiments, the thermoplastic polymer is fluorinated ethylene propylene (FEP). In some embodiments, the thermoplastic polymer is a perfluoroelastomer (FFKM). In some embodiments, the thermoplastic polymer is polybutene-1 (PB-1). In some embodiments, the thermoplastic polymer is polycarbonate (PC). In some embodiments, the thermoplastic polymer is polyetheretherketone (PEEK). In some embodiments, the thermoplastic polymer is polyetherimide (PEI). In some embodiments, the thermoplastic polymer is polyethersulfone (PES). In some embodiments, the thermoplastic polymer is polyethylene terephthalate (PET). In some embodiments, the thermoplastic polymer is polyisobutylene (PIB). In some embodiments, the thermoplastic polymer is polyisoprene. In some embodiments, the thermoplastic polymer is poly(methyl methacrylate) (PMMA). In some embodiments, the thermoplastic polymer is polymethylpentene (PMP). In some embodiments, the thermoplastic polymer is polytetrafluoroethylene (PTFE). In some embodiments, the thermoplastic polymer is polyvinylidene fluoride-co-fluorinated ethylene propylene (PVDF-co-FEP). In some embodiments, the thermoplastic polymer is poly(styrene-isoprene-styrene) (SIS). In some embodiments, the thermoplastic polymer is poly(styrene-butadiene-styrene) (SBS). In some embodiments, the thermoplastic polymer is ultra-high molecular weight polyethylene (UHWPE).
[0062] In some embodiments, including any of the above embodiments, the melting point of the modified thermoplastic polymer is in the range of about 50 °C to about 350 °C. In some embodiments, the melting point of the modified thermoplastic polymer is about 80 °C to about 300 °C. In some embodiments, the melting point of the modified thermoplastic polymer is about 80 °C to about 250 °C. In some embodiments, the melting point of the modified thermoplastic polymer is about 100 °C to about 200 °C. In some embodiments, the melting point of the modified thermoplastic polymer is about 110 °C to about 180 °C. In some embodiments, the melting point of the modified thermoplastic polymer is about 120 °C to about 170 °C. In some embodiments, the melting point of the modified thermoplastic polymer is about 130 °C to about 170 °C. In some embodiments, the melting point of the modified thermoplastic polymer is about 140 °C to about 170 °C. In some embodiments, the modified thermoplastic polymer has a melting point of about 150 °C to about 170 °C. In some embodiments, the modified thermoplastic polymer has a melting point of about 150 °C to about 160 °C.
[0063] In some embodiments, the modified thermoplastic polymer has a melting point above 160 °C.
[0064] In some embodiments, the melting point of the modified thermoplastic polymer is in the range of about 160 °C to about 350 °C. In some embodiments, the melting point of the modified thermoplastic polymer is in the range of about 160 °C to about 300 °C. In some embodiments, the melting point of the modified thermoplastic polymer is in the range of about 160 °C to about 250 °C. In some embodiments, the melting point of the modified thermoplastic polymer is in the range of about 160 °C to about 200 °C. In some embodiments, the melting point of the modified thermoplastic polymer is in the range of about 160 °C to about 180 °C. In some embodiments, the melting point of the modified thermoplastic polymer is in the range of about 160 °C to about 170 °C.
[0065] In some embodiments, the glyph of the thermoplastic polymer is from about 1 second / 100 cubic centimeters (1 sec / 100 cc) to about 50 sec / 100 cc (based on samples with a thickness of 50 µm to 150 µm).
[0066] In some embodiments, the modified thermoplastic polymer has a weight-average molecular weight (M). w In some embodiments, the modified thermoplastic polymer has a weight-average molecular weight (M) after crosslinking. w ).
[0067] In some embodiments, the weight-average molecular weight (M) of the modified thermoplastic polymer is... w The weight-average molecular weight (M) of the modified thermoplastic polymer is approximately 10,000 g / mol to approximately 500,000 g / mol. In some embodiments, the weight-average molecular weight (M) of the modified thermoplastic polymer is... w The weight-average molecular weight (M) of the modified thermoplastic polymer is approximately 10,000 g / mol to approximately 450,000 g / mol. In some embodiments, the weight-average molecular weight (M) of the modified thermoplastic polymer is... w The weight-average molecular weight (M) of the modified thermoplastic polymer is approximately 10,000 g / mol to approximately 400,000 g / mol. In some embodiments, the weight-average molecular weight (M) of the modified thermoplastic polymer is... w The weight-average molecular weight (M) of the modified thermoplastic polymer is approximately 10,000 g / mol to approximately 350,000 g / mol. In some embodiments, the weight-average molecular weight (M) of the modified thermoplastic polymer is... w The weight-average molecular weight (M) of the modified thermoplastic polymer is approximately 10,000 g / mol to approximately 300,000 g / mol. In some embodiments, the weight-average molecular weight (M) of the modified thermoplastic polymer is... w The weight-average molecular weight (M) of the modified thermoplastic polymer is approximately 10,000 g / mol to approximately 250,000 g / mol. In some embodiments, the weight-average molecular weight (M) of the modified thermoplastic polymer is... w The weight-average molecular weight (M) of the modified thermoplastic polymer is approximately 10,000 g / mol to approximately 200,000 g / mol. In some embodiments, the weight-average molecular weight (M) of the modified thermoplastic polymer is... w The weight-average molecular weight (M) of the modified thermoplastic polymer is approximately 30,000 g / mol to approximately 200,000 g / mol. In some embodiments, the weight-average molecular weight (M) of the modified thermoplastic polymer is... w The weight-average molecular weight (M) of the modified thermoplastic polymer is approximately 50,000 g / mol to approximately 200,000 g / mol. In some embodiments, the weight-average molecular weight (M) of the modified thermoplastic polymer is... w The concentration is approximately 100,000 g / mol to approximately 200,000 g / mol.
[0068] In some embodiments, the modified thermoplastic polymer has a weight-average molecular weight (M) after crosslinking. w The concentration is approximately 20,000 g / mol to approximately 1,000,000 g / mol.
[0069] In some embodiments, the modified polyethylene polymer is a vinyl acetate-modified polyethylene polymer. In some embodiments, the modified polyethylene polymer is a vinyl alcohol-modified polyethylene polymer. In some embodiments, the modified polyethylene polymer is a halogen-modified polyethylene polymer. In some embodiments, the modified polyethylene polymer is a chloride-modified polyethylene polymer. In some embodiments, the modified polyethylene polymer is a fluoride-modified polyethylene polymer. In some embodiments, the modified polyethylene polymer is an amide-modified polyethylene polymer. In some embodiments, the modified polyethylene polymer is a phthalate-modified polyethylene polymer. In some embodiments, the modified polyethylene polymer is an alkyl-modified polyethylene polymer. In some embodiments, the modified polyethylene polymer is a propyl-modified polyethylene polymer. In some embodiments, the modified polyethylene polymer is an acrylic acid-modified polyethylene polymer. In some embodiments, the modified polyethylene polymer is a maleic anhydride-modified polyethylene polymer. In some embodiments, the modified polyethylene polymer is crosslinked. In other embodiments, the modified polyethylene polymer is not crosslinked.
[0070] In some embodiments, the modified polyethylene polymer is a maleic anhydride polyethylene copolymer.
[0071] In some embodiments, the modified polyethylene polymer is a cross-linked maleic anhydride polyethylene copolymer.
[0072] In some embodiments, the melting point of the modified polyethylene polymer is in the range of about 80 °C to about 300 °C. In some embodiments, the melting point of the modified polyethylene polymer is about 80 °C to about 250 °C. In some embodiments, the melting point of the modified polyethylene polymer is about 100 °C to about 200 °C. In some embodiments, the melting point of the modified polyethylene polymer is about 110 °C to about 180 °C. In some embodiments, the melting point of the modified polyethylene polymer is about 120 °C to about 170 °C. In some embodiments, the melting point of the modified polyethylene polymer is about 130 °C to about 170 °C. In some embodiments, the melting point of the modified polyethylene polymer is about 140 °C to about 170 °C. In some embodiments, the melting point of the modified polyethylene polymer is about 150 °C to about 170 °C. In some embodiments, the melting point of the modified polyethylene polymer is about 150 °C to about 160 °C.
[0073] In some embodiments, the modified polyethylene polymer has a melting point above 160 °C.
[0074] In some embodiments, the melting point of the modified polyethylene polymer is in the range of about 160 °C to about 350 °C. In some embodiments, the melting point of the modified polyethylene polymer is in the range of about 160 °C to about 300 °C. In some embodiments, the melting point of the modified polyethylene polymer is in the range of about 160 °C to about 250 °C. In some embodiments, the melting point of the modified polyethylene polymer is in the range of about 160 °C to about 200 °C. In some embodiments, the melting point of the modified polyethylene polymer is in the range of about 160 °C to about 180 °C. In some embodiments, the melting point of the modified polyethylene polymer is in the range of about 160 °C to about 170 °C.
[0075] In some embodiments, the crosslinked maleic anhydride polyethylene copolymer has a melting point above about 160 °C.
[0076] In some embodiments, the melting point of the crosslinked maleic anhydride polyethylene copolymer is in the range of about 160 °C to about 350 °C. In some embodiments, the melting point of the crosslinked maleic anhydride polyethylene copolymer is in the range of about 160 °C to about 300 °C. In some embodiments, the melting point of the crosslinked maleic anhydride polyethylene copolymer is in the range of about 160 °C to about 250 °C. In some embodiments, the melting point of the crosslinked maleic anhydride polyethylene copolymer is in the range of about 160 °C to about 200 °C. In some embodiments, the melting point of the crosslinked maleic anhydride polyethylene copolymer is in the range of about 160 °C to about 180 °C. In some embodiments, the melting point of the crosslinked maleic anhydride polyethylene copolymer is in the range of about 160 °C to about 170 °C.
[0077] In some embodiments, the modified polypropylene polymer is a halide-modified polypropylene polymer. In some embodiments, the modified polypropylene polymer is a chloride-modified polypropylene polymer. In some embodiments, the modified polypropylene polymer is a fluoride-modified polypropylene polymer. In some embodiments, the modified polypropylene polymer is an alkyl-modified polypropylene polymer. In some embodiments, the modified polypropylene polymer is an ethylene-modified polypropylene polymer. In other embodiments, the modified polypropylene polymer is a maleic anhydride-modified polypropylene polymer.
[0078] In some embodiments, the framework includes a first thermoplastic polymer and a second thermoplastic polymer. In some embodiments, the first thermoplastic polymer and the second thermoplastic polymer are different thermoplastic polymers.
[0079] In some embodiments, the first thermoplastic polymer is a modified polyethylene polymer. In some embodiments, the first thermoplastic polymer is a weight-average molecular weight polymer (M). w The first thermoplastic polymer is a modified polyethylene polymer with a molecular weight ratio of about 100,000 g / mol to about 200,000 g / mol. In some embodiments, the first thermoplastic polymer is a maleic anhydride-modified polyethylene polymer. In some embodiments, the first thermoplastic polymer is a weight-average molecular weight (M... w The first thermoplastic polymer is a maleic anhydride-modified polyethylene polymer ranging from about 100,000 g / mol to about 200,000 g / mol. In some embodiments, the first thermoplastic polymer is a crosslinked maleic anhydride-polyethylene copolymer.
[0080] In some embodiments, the second thermoplastic polymer is PTFE. In other embodiments, the second thermoplastic polymer is PEEK. In other embodiments, the second thermoplastic polymer is a polyimide polymer. In other embodiments, the second thermoplastic polymer is a porous polyimide polymer.
[0081] In some embodiments, the frame comprises one or more layers. In some embodiments, the frame comprises two or more layers. In some embodiments, the frame comprises three or more layers. In some embodiments, the frame comprises one or more layers, each layer comprising a thermoplastic polymer. In some embodiments, the frame comprises two or more layers, each layer comprising a thermoplastic polymer. In some embodiments, the frame comprises three or more layers, each layer comprising a thermoplastic polymer.
[0082] In some embodiments, the frame comprises a first layer and a second layer. In some embodiments, the first layer and the second layer of the frame comprise the same thermoplastic polymer. In other embodiments, the first layer and the second layer of the frame comprise different thermoplastic polymers.
[0083] In some embodiments, the framework includes a first layer and a second layer, wherein the first layer comprises a modified polyethylene polymer.
[0084] In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a weight-average molecular weight (M) layer. w The first layer comprises a modified polyethylene polymer with a molecular weight of about 100,000 g / mol to about 200,000 g / mol. In some embodiments, the first layer comprises a maleic anhydride-modified polyethylene polymer. In some embodiments, the first layer comprises a maleic anhydride-modified polyethylene copolymer. In other embodiments, the first layer comprises a weight-average molecular weight (M... wThe first layer comprises a maleic anhydride polyethylene copolymer at a concentration of about 100,000 g / mol to about 200,000 g / mol. In other embodiments, the first layer comprises a crosslinked maleic anhydride polyethylene copolymer.
[0085] In some embodiments, the framework includes a first layer and a second layer, the second layer comprising a thermoplastic polymer with a glycemic index of about 1 sec / 100cc to about 50 sec / 100cc (based on a sample thickness of 50 µm to 150 µm).
[0086] In some embodiments, the frame includes a first layer and a second layer, the second layer comprising PEEK. In other embodiments, the second layer comprises PTFE. In other embodiments, the second layer comprises a polyimide polymer. In other embodiments, the second layer comprises a porous polyimide polymer.
[0087] In some embodiments, the framework includes a first layer and a second layer, the second layer comprising PEEK with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In other embodiments, the second layer comprises PTFE with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In other embodiments, the second layer comprises a polyimide polymer with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In other embodiments, the second layer comprises a porous polyimide polymer with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample).
[0088] In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a maleic anhydride polyethylene copolymer, and the second layer comprising a thermoplastic polymer with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer, and the second layer comprising a thermoplastic polymer with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample).
[0089] In some embodiments, including any of the above embodiments, the framework includes a first layer and a second layer, the first layer comprising a maleic anhydride polyethylene copolymer, and the second layer comprising PEEK, PTFE, a polyimide polymer, or a porous polyimide polymer. In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer, and the second layer comprising PEEK, PTFE, a polyimide polymer, or a porous polyimide polymer.
[0090] In some embodiments, including any of the above embodiments, the framework includes a first layer and a second layer, the first layer comprising a maleic anhydride polyethylene copolymer and the second layer comprising PEEK. In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer and the second layer comprising PEEK. In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a maleic anhydride polyethylene copolymer and the second layer comprising PTFE. In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer and the second layer comprising PTFE. In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a maleic anhydride polyethylene copolymer and the second layer comprising a polyimide polymer. In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer and the second layer comprising a polyimide polymer. In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a maleic anhydride polyethylene copolymer and the second layer comprising a porous polyimide polymer. In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a cross-linked maleic anhydride polyethylene copolymer and the second layer comprising a porous polyimide polymer.
[0091] In some embodiments, including any of the above embodiments, the framework comprises a first layer and a second layer, the first layer comprising a maleic anhydride polyethylene copolymer, and the second layer comprising PEEK with a Glyph value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework comprises a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer, and the second layer comprising PEEK with a Glyph value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework comprises a first layer and a second layer, the first layer comprising a maleic anhydride polyethylene copolymer, and the second layer comprising PTFE with a Glyph value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework comprises a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer, and the second layer comprising PTFE with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework comprises a first layer and a second layer, the first layer comprising a maleic anhydride polyethylene copolymer, and the second layer comprising a polyimide polymer with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework comprises a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer, and the second layer comprising a polyimide polymer with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework comprises a first layer and a second layer, the first layer comprising a maleic anhydride polyethylene copolymer, and the second layer comprising a porous polyimide polymer with a Glyph value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework comprises a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer, and the second layer comprising a porous polyimide polymer with a Glyph value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample).
[0092] In some embodiments, the frame includes a first layer and a second layer, the first layer contacting the cathode current collector. In some embodiments, the frame includes a first layer and a second layer, the second layer contacting the solid-state membrane. In some embodiments, the frame includes a first layer and a second layer, the first layer contacting the cathode current collector and the second layer contacting the solid-state membrane.
[0093] In some embodiments, the frame includes a first layer and a second layer, the first layer comprising a cross-linked maleic anhydride polyethylene copolymer in contact with the cathode current collector.
[0094] In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer in contact with the cathode current collector, and the second layer comprising PEEK in contact with the solid membrane. In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer in contact with the cathode current collector, and the second layer comprising PTFE in contact with the solid membrane. In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer in contact with the cathode current collector, and the second layer comprising a polyimide polymer in contact with the solid membrane. In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer in contact with the cathode current collector, and the second layer comprising a porous polyimide polymer in contact with the solid membrane.
[0095] In some embodiments, the framework includes a first layer and a second layer, the second layer comprising a thermoplastic polymer in contact with the solid separator having a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework includes a first layer and a second layer, the first layer comprising a crosslinked maleic anhydride polyethylene copolymer in contact with the cathode current collector, and the second layer comprising a thermoplastic polymer in contact with the solid separator having a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample).
[0096] In some embodiments, the frame includes a first layer, a second layer, and a third layer. In some embodiments, the first, second, and third layers each comprise a thermoplastic polymer. In some embodiments, the first and third layers of the frame comprise the same thermoplastic polymer. In some embodiments, the first and third layers of the frame comprise different thermoplastic polymers. In some embodiments, the second layer comprises a thermoplastic polymer different from the first and third layers. In some embodiments, the second layer comprises the same thermoplastic polymer as the first and third layers. In some embodiments, the second layer comprises the same thermoplastic polymer as the first layer and also comprises a thermoplastic polymer different from the third layer. In some embodiments, the second layer comprises the same thermoplastic polymer as the third layer and also comprises a thermoplastic polymer different from the first layer.
[0097] In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the first layer comprises a modified polyethylene polymer. In some embodiments, the third layer comprises a modified polyethylene polymer. In some embodiments, the first layer and the third layer each comprise a modified polyethylene polymer, wherein the modified polyethylene polymer of the first layer is the same as that of the third layer. In some embodiments, the first layer and the third layer each comprise a modified polyethylene polymer, wherein the modified polyethylene polymer of the first layer is different from that of the third layer.
[0098] In some embodiments, the framework includes a first layer, a second layer, and a third layer, wherein the first layer includes a weight-average molecular weight (M) layer. w The first layer comprises a modified polyethylene polymer with a molecular weight ratio of about 100,000 g / mol to about 200,000 g / mol. In some embodiments, the first layer comprises a maleic anhydride-modified polyethylene polymer. In other embodiments, the first layer comprises a weight-average molecular weight (M...) w The first layer comprises a maleic anhydride-modified polyethylene polymer with a molecular weight ratio of about 100,000 g / mol to about 200,000 g / mol. In other embodiments, the first layer comprises a maleic anhydride-modified polyethylene copolymer. In other embodiments, the first layer comprises a weight-average molecular weight (M... w The first layer comprises a maleic anhydride polyethylene copolymer with a molecular weight of about 100,000 g / mol to about 200,000 g / mol. In other embodiments, the first layer comprises a crosslinked maleic anhydride polyethylene copolymer. In some embodiments, the third layer comprises a weight-average molecular weight (M... wThe third layer comprises a modified polyethylene polymer with a molecular weight ratio of about 100,000 g / mol to about 200,000 g / mol. In some embodiments, the third layer comprises a maleic anhydride-modified polyethylene polymer. In other embodiments, the third layer comprises a weight-average molecular weight (M...) w The third layer comprises a maleic anhydride-modified polyethylene polymer of about 100,000 g / mol to about 100,000 g / mol. In other embodiments, the third layer comprises a maleic anhydride-modified polyethylene copolymer. In other embodiments, the third layer comprises a weight-average molecular weight (M... w The first layer comprises a maleic anhydride-modified polyethylene copolymer with a molecular weight of about 100,000 g / mol to about 200,000 g / mol. In other embodiments, the third layer comprises a crosslinked maleic anhydride-modified polyethylene copolymer. In other embodiments, both the first and third layers comprise a maleic anhydride-modified polyethylene polymer. In other embodiments, both the first and third layers comprise a weight-average molecular weight (M...) w The first layer is a maleic anhydride-modified polyethylene polymer with a molecular weight ratio of about 100,000 g / mol to about 200,000 g / mol. In other embodiments, the first layer and the third layer each comprise a maleic anhydride-modified polyethylene copolymer. In other embodiments, the first layer and the third layer each comprise a weight-average molecular weight (M...) w The first layer is a maleic anhydride polyethylene copolymer with a concentration of about 100,000 g / mol to about 200,000 g / mol. In other embodiments, the first layer and the third layer each comprise a crosslinked maleic anhydride polyethylene copolymer.
[0099] In some embodiments, the framework includes a first layer, a second layer, and a third layer, wherein the second layer comprises a thermoplastic polymer with a glycemic index of about 1 sec / 100cc to about 50 sec / 100cc (based on a sample thickness of 50 µm to 150 µm).
[0100] In some embodiments, the framework includes a first layer, a second layer, and a third layer, wherein the second layer comprises PEEK. In other embodiments, the second layer comprises PTFE. In other embodiments, the second layer comprises a polyimide polymer. In other embodiments, the second layer comprises a porous polyimide polymer.
[0101] In some embodiments, the framework includes a first layer, a second layer, and a third layer, the second layer comprising PEEK with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework includes a first layer, a second layer, and a third layer, the second layer comprising PTFE with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In other embodiments, the second layer comprises a polyimide polymer with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In other embodiments, the second layer comprises a porous polyimide polymer with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample).
[0102] In some embodiments, the framework includes a first layer, a second layer, and a third layer, wherein the first layer and the third layer each comprise a weight-average molecular weight (M). w The first layer is a modified polyethylene polymer of about 100,000 g / mol to about 200,000 g / mol, and the second layer comprises PEEK. In some embodiments, the framework comprises a first layer, a second layer, and a third layer, the first layer and the third layer each comprising a weight-average molecular weight (M). w The first layer comprises a modified polyethylene polymer of about 100,000 g / mol to about 200,000 g / mol, and the second layer comprises PTFE. In some embodiments, the framework comprises a first layer, a second layer, and a third layer, the first layer and the third layer each comprising a maleic anhydride-modified polyethylene polymer, and the second layer comprising PEEK. In some embodiments, the framework comprises a first layer, a second layer, and a third layer, the first layer and the third layer each comprising a maleic anhydride-modified polyethylene polymer, and the second layer comprising PTFE. In some embodiments, the framework comprises a first layer, a second layer, and a third layer, the first layer and the third layer each comprising a weight-average molecular weight (M... w The first layer is a maleic anhydride-modified polyethylene polymer with a concentration of about 100,000 g / mol to about 200,000 g / mol, and the second layer comprises PEEK. In some embodiments, the framework comprises a first layer, a second layer, and a third layer, wherein the first layer and the third layer each comprise a weight-average molecular weight (M). wThe framework comprises a maleic anhydride-modified polyethylene polymer at a concentration of about 100,000 g / mol to about 200,000 g / mol, wherein the second layer comprises PTFE. In some embodiments, the framework comprises a first layer, a second layer, and a third layer, wherein the first layer and the third layer each comprise a maleic anhydride polyethylene copolymer, and the second layer comprises PEEK. In some embodiments, the framework comprises a first layer, a second layer, and a third layer, wherein the first layer and the third layer each comprise a crosslinked maleic anhydride polyethylene copolymer, and the second layer comprises PEEK. In some embodiments, the framework comprises a first layer, a second layer, and a third layer, wherein the first layer and the third layer each comprise a maleic anhydride polyethylene copolymer, and the second layer comprises PTFE. In some embodiments, the framework comprises a first layer, a second layer, and a third layer, wherein the first layer and the third layer each comprise a maleic anhydride polyethylene copolymer, and the second layer comprises a polyimide polymer. In some embodiments, the framework includes a first layer, a second layer, and a third layer, wherein the first layer and the third layer each comprise a crosslinked maleic anhydride polyethylene copolymer, and the second layer comprises a polyimide polymer.
[0103] In some embodiments, the framework includes a first layer, a second layer, and a third layer, wherein the first layer and the third layer each comprise a maleic anhydride polyethylene copolymer, and the second layer comprises PEEK, PTFE, a polyimide polymer, or a porous polyimide polymer. In some embodiments, the framework includes a first layer, a second layer, and a third layer, wherein the first layer and the third layer each comprise a crosslinked maleic anhydride polyethylene copolymer, and the second layer comprises PEEK, PTFE, a polyimide polymer, or a porous polyimide polymer.
[0104] In some embodiments, including any of the above embodiments, the framework comprises a first layer, a second layer, and a third layer, the first layer and the third layer each comprising a maleic anhydride polyethylene copolymer, and the second layer comprising PEEK with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework comprises a first layer, a second layer, and a third layer, the first layer and the third layer each comprising a crosslinked maleic anhydride polyethylene copolymer, and the second layer comprising PEEK with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework comprises a first layer, a second layer, and a third layer, the first layer and the third layer each comprising a maleic anhydride polyethylene copolymer, and the second layer comprising PTFE with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework includes a first layer, a second layer, and a third layer, the first layer and the third layer each comprising a crosslinked maleic anhydride polyethylene copolymer, and the second layer comprising PTFE with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework includes a first layer, a second layer, and a third layer, the first layer and the third layer each comprising a maleic anhydride polyethylene copolymer, and the second layer comprising a polyimide polymer with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework includes a first layer, a second layer, and a third layer, the first layer and the third layer each comprising a crosslinked maleic anhydride polyethylene copolymer, and the second layer comprising a polyimide polymer with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample). In some embodiments, the framework includes a first layer, a second layer, and a third layer, the first layer and the third layer each comprising a maleic anhydride polyethylene copolymer, and the second layer comprising a porous polyimide polymer with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample).In some embodiments, the framework includes a first layer, a second layer, and a third layer, the first layer and the third layer each comprising a crosslinked maleic anhydride polyethylene copolymer, and the second layer comprising a porous polyimide polymer with a Glycol value of about 1 sec / 100cc to about 50 sec / 100cc (based on a 50 µm to 150 µm thick sample).
[0105] In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the first layer or the third layer contacts the cathode current collector, and the remaining layers contact the solid membrane.
[0106] In some embodiments, the frame includes a first layer, a second layer, and a third layer, the first layer and the third layer each comprising a crosslinked maleic anhydride polyethylene copolymer, the first layer or the third layer contacting the cathode current collector, and the remaining layers contacting the solid membrane.
[0107] In some embodiments, the thermoplastic polymer has initial dimensions (i.e., initial length, initial width, initial height) before heating or applying pressure. In some embodiments, the thermoplastic polymer has initial dimensions before heating and applying pressure. In some embodiments, the thermoplastic polymer has final dimensions (i.e., final length, final width, final height) after heating or applying pressure. In some embodiments, the thermoplastic polymer has final dimensions after heating and applying pressure.
[0108] In some embodiments, the Poisson's ratio of the thermoplastic polymer is about 0.2 to 0.3. In some embodiments, the Poisson's ratio of the thermoplastic polymer is about 0.2 to 0.3 at a temperature of about 110 °C to about 150 °C. In some embodiments, the Poisson's ratio of the thermoplastic polymer is about 0.2 to 0.3 at an applied pressure of about 250 kPa to about 700 kPa. In some embodiments, the Poisson's ratio of the thermoplastic polymer is about 0.2 to 0.3 at a temperature of about 110 °C to about 150 °C and an applied pressure of about 250 kPa to about 700 kPa.
[0109] In some embodiments, the thermoplastic polymer exhibits a transverse strain of less than about 1.5% at a temperature of about 110 °C to about 150 °C and an applied pressure of about 250 kPa to about 700 kPa.
[0110] In some embodiments, after heating to a temperature of about 80°C to about 160°C, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 10%. In some embodiments, after heating to a temperature of about 80°C to about 160°C, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 9%. In some embodiments, after heating to a temperature of about 80°C to about 160°C, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 8%. In some embodiments, after heating to a temperature of about 80°C to about 160°C, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 7%. In some embodiments, after heating to a temperature of about 80°C to about 160°C, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 6%. In some embodiments, after heating to a temperature of about 80°C to about 160°C, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 5%. In some embodiments, after heating to a temperature of about 80°C to about 160°C, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 4%. In some embodiments, after heating to a temperature of about 80°C to about 160°C, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 3%. In some embodiments, after heating to a temperature of about 80°C to about 160°C, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 2%. In some embodiments, after heating to a temperature of about 80°C to about 160°C, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 1.5%. In some embodiments, after heating to a temperature of about 80°C to about 160°C, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 1%. In some embodiments, after heating to a temperature of about 80°C to about 160°C, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 0.5%.
[0111] In some embodiments, after pressure is applied, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 10%. In some embodiments, after pressure is applied, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 9%. In some embodiments, after pressure is applied, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 8%. In some embodiments, after pressure is applied, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 7%. In some embodiments, after pressure is applied, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 6%. In some embodiments, after pressure is applied, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 5%. In some embodiments, after pressure is applied, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 4%. In some embodiments, after pressure is applied, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 3%. In some embodiments, after pressure is applied, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 2%. In some embodiments, after pressure is applied, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 1.5%. In some embodiments, after pressure is applied, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 1%. In some embodiments, after pressure is applied, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 0.5%.
[0112] In some embodiments, after heating to a temperature of about 80°C to about 160°C and applying pressure, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 10%. In some embodiments, after heating to a temperature of about 80°C to about 160°C and applying pressure, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 9%. In some embodiments, after heating to a temperature of about 80°C to about 160°C and applying pressure, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 8%. In some embodiments, after heating to a temperature of about 80°C to about 160°C and applying pressure, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 7%. In some embodiments, after heating to a temperature of about 80°C to about 160°C and applying pressure, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 6%. In some embodiments, after heating to a temperature of about 80°C to about 160°C and applying pressure, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 5%. In some embodiments, after heating to a temperature of about 80°C to about 160°C and applying pressure, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 4%. In some embodiments, after heating to a temperature of about 80°C to about 160°C and applying pressure, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 3%. In some embodiments, after heating to a temperature of about 80°C to about 160°C and applying pressure, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 2%. In some embodiments, after heating to a temperature of about 80°C to about 160°C and applying pressure, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 1.5%. In some embodiments, after heating to a temperature of about 80°C to about 160°C and applying pressure, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 1%. In some embodiments, after heating to a temperature of about 80°C to about 160°C and applying pressure, the thermoplastic polymer shrinks or expands relative to its initial size by no more than 0.5%.
[0113] In some embodiments, including any of the above embodiments, the frame comprises one or more layers, each of the one or more independent layers of the frame having a thickness, the sum of the thicknesses of all layers being the total thickness of the frame. In some embodiments, the frame comprises two or more layers, each of the two or more independent layers of the frame having a thickness, the sum of the thicknesses of all layers being the total thickness of the frame. In some embodiments, the frame comprises three or more layers, each of the three or more independent layers of the frame having a thickness, the sum of the thicknesses of all layers being the total thickness of the frame.
[0114] In some embodiments, the total thickness of the frame is from about 80 µm to about 200 µm. In some embodiments, the total thickness of the frame is from about 80 µm to about 180 µm. In some embodiments, the total thickness of the frame is from about 90 µm to about 160 µm. In some embodiments, the total thickness of the frame is from about 100 µm to about 140 µm. In some embodiments, the total thickness of the frame is from about 100 µm to about 130 µm. In some embodiments, the total thickness of the frame is from about 110 µm to about 130 µm.
[0115] In some implementations, the total thickness of the frame is greater than the thickness of the solid cathode.
[0116] In some embodiments, the thickness of the solid-state cathode is from about 80 µm to about 180 µm. In some embodiments, the thickness of the solid-state cathode is from about 80 µm to about 170 µm. In some embodiments, the thickness of the solid-state cathode is from about 90 µm to about 170 µm. In some embodiments, the thickness of the solid-state cathode is from about 100 µm to about 170 µm. In some embodiments, the thickness of the solid-state cathode is from about 100 µm to about 160 µm.
[0117] In some embodiments, the frame includes a first layer and a second layer, the first layer and the second layer having different thicknesses. In some embodiments, the thickness of the first layer is from about 10 µm to about 60 µm. In some embodiments, the thickness of the first layer is from about 10 µm to about 50 µm. In some embodiments, the thickness of the first layer is from about 20 µm to about 50 µm.
[0118] In some implementations, the frame includes a first layer and a second layer, wherein the thickness of the second layer is greater than the thickness of the first layer.
[0119] In some embodiments, the frame includes a first layer and a second layer, the thickness of the second layer being about 50% to about 90% of the total thickness of the frame. In some embodiments, the frame includes a first layer and a second layer, the thickness of the second layer being about 50% to about 85% of the total thickness of the frame. In some embodiments, the frame includes a first layer and a second layer, the thickness of the second layer being about 50% to about 80% of the total thickness of the frame. In some embodiments, the frame includes a first layer and a second layer, the thickness of the second layer being about 55% to about 80% of the total thickness of the frame. In some embodiments, the frame includes a first layer and a second layer, the thickness of the second layer being about 55% to about 75% of the total thickness of the frame. In some embodiments, the frame includes a first layer and a second layer, the thickness of the second layer being about 60% to about 75% of the total thickness of the frame. In some embodiments, the frame includes a first layer and a second layer, the thickness of the second layer being about 60% to about 70% of the total thickness of the frame.
[0120] In some embodiments, the frame includes a first layer and a second layer, the second layer having a thickness of about 20 µm to about 140 µm. In some embodiments, the frame includes a first layer and a second layer, the second layer having a thickness of about 20 µm to about 130 µm. In some embodiments, the frame includes a first layer and a second layer, the second layer having a thickness of about 20 µm to about 120 µm. In some embodiments, the frame includes a first layer and a second layer, the second layer having a thickness of about 20 µm to about 110 µm. In some embodiments, the frame includes a first layer and a second layer, the second layer having a thickness of about 30 µm to about 110 µm. In some embodiments, the frame includes a first layer and a second layer, the second layer having a thickness of about 30 µm to about 100 µm. In some embodiments, the frame includes a first layer and a second layer, the second layer having a thickness of about 30 µm to about 90 µm. In some embodiments, the frame includes a first layer and a second layer, the second layer having a thickness of about 40 µm to about 80 µm. In some implementations, the frame includes a first layer and a second layer, the second layer having a thickness of about 60 µm to about 80 µm.
[0121] In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the first layer and the third layer have different thicknesses. In some embodiments, the thickness of the first layer is from about 10 µm to about 50 µm. In some embodiments, the thickness of the first layer is from about 20 µm to about 40 µm. In some embodiments, the thickness of the third layer is from about 20 µm to about 60 µm. In some embodiments, the thickness of the third layer is from about 20 µm to about 50 µm.
[0122] In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the first layer and the third layer have the same thickness. In some embodiments, the thickness of each of the first layer and the third layer is from about 10 µm to about 60 µm. In some embodiments, the thickness of each of the first layer and the third layer is from about 10 µm to about 50 µm. In some embodiments, the thickness of each of the first layer and the third layer is from about 20 µm to about 40 µm.
[0123] In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is greater than the thickness of either the first layer or the third layer. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is greater than both the thickness of the first layer and the thickness of the third layer.
[0124] In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is about 30% to about 70% of the total thickness of the frame. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is about 35% to about 65% of the total thickness of the frame. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is about 35% to about 60% of the total thickness of the frame. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is about 35% to about 55% of the total thickness of the frame. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is about 40% to about 55% of the total thickness of the frame. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is about 45% to about 50% of the total thickness of the frame.
[0125] In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is from about 20 µm to about 140 µm. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is from about 20 µm to about 130 µm. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is from about 20 µm to about 120 µm. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is from about 20 µm to about 110 µm. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is from about 30 µm to about 110 µm. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is from about 30 µm to about 90 µm. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is from about 40 µm to about 80 µm. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is from about 60 µm to about 80 µm. In some embodiments, the frame includes a first layer, a second layer, and a third layer, wherein the thickness of the second layer is from about 50 µm to about 70 µm.
[0126] In some embodiments, the frame is permeable to gas. In some embodiments, the frame is impermeable to moisture. In some embodiments, the frame is permeable to gas but impermeable to moisture. In some embodiments, the frame is permeable to H2S, SO2, NH3, Ar, N2, O2, H2, or combinations thereof.
[0127] In some embodiments, the frame has an outer length and an outer width. In some embodiments, the frame also has an inner length and an inner width.
[0128] In some embodiments, the outer length of the frame is from about 70 mm to about 95 mm. In some embodiments, the outer length of the frame is from about 70 mm to about 90 mm. In some embodiments, the outer length of the frame is from about 70 mm to about 85 mm. In some embodiments, the outer length of the frame is from about 70 mm to about 80 mm.
[0129] In some embodiments, the outer width of the frame is from about 55 mm to about 80 mm. In some embodiments, the outer width of the frame is from about 55 mm to about 75 mm. In some embodiments, the outer width of the frame is from about 55 mm to about 70 mm. In some embodiments, the outer width of the frame is from about 55 mm to about 65 mm.
[0130] In some embodiments, the internal length of the frame is from about 60 mm to about 85 mm. In some embodiments, the internal length of the frame is from about 60 mm to about 80 mm. In some embodiments, the internal length of the frame is from about 60 mm to about 75 mm. In some embodiments, the internal length of the frame is from about 60 mm to about 70 mm.
[0131] In some embodiments, the inner width of the frame is from about 45 mm to about 70 mm. In some embodiments, the inner width of the frame is from about 45 mm to about 65 mm. In some embodiments, the inner width of the frame is from about 45 mm to about 60 mm. In some embodiments, the inner width of the frame is from about 45 mm to about 55 mm.
[0132] In some embodiments, the difference between the outer length and the inner length of the frame is about 5 mm to about 35 mm. In some embodiments, the difference is about 5 mm to about 30 mm. In some embodiments, the difference is about 5 mm to about 25 mm. In some embodiments, the difference is about 5 mm to about 20 mm. In some embodiments, the difference is about 5 mm to about 15 mm.
[0133] In some embodiments, the difference between the outer width of the frame and the inner width of the frame is from about 5 mm to about 35 mm. In some embodiments, the difference is from about 5 mm to about 30 mm. In some embodiments, the difference is from about 5 mm to about 25 mm. In some embodiments, the difference is from about 5 mm to about 20 mm. In some embodiments, the difference is from about 5 mm to about 15 mm.
[0134] In some embodiments, the width of the solid-state cathode is from about 45 mm to about 65 mm. In some embodiments, the width of the solid-state cathode is from about 50 mm to about 65 mm. In some embodiments, the width of the solid-state cathode is from about 50 mm to about 60 mm.
[0135] In some embodiments, the solid-state cathode has a length of about 60 mm to about 80 mm. In some embodiments, the solid-state cathode has a length of about 60 mm to about 75 mm. In some embodiments, the solid-state cathode has a length of about 65 mm to about 75 mm.
[0136] In some embodiments, the inner width of the frame is at least about 20 µm, at least about 100 µm, at least about 500 µm, at least about 1 mm, or at least about 2 mm wider than the solid-state cathode. In some embodiments, the inner width of the frame is about 20 µm to about 5 mm wider than the solid-state cathode. In some embodiments, the inner width of the frame is about 20 µm to about 2.5 mm wider than the solid-state cathode. In some embodiments, the inner width of the frame is about 20 µm to about 2 mm wider than the solid-state cathode. In some embodiments, the inner width of the frame is about 50 µm to about 2 mm wider than the solid-state cathode. In some embodiments, the inner width of the frame is about 100 µm to about 2 mm wider than the solid-state cathode. In some embodiments, the inner width of the frame is about 200 µm to about 1.5 mm wider than the solid-state cathode. In some embodiments, the inner width of the frame is about 300 µm to about 1.5 mm wider than the solid-state cathode. In some embodiments, the width within the frame is approximately 400 µm to approximately 1.2 µm wider than the width of the solid cathode.
[0137] In some embodiments, the inner length of the frame is at least about 20 µm, at least about 100 µm, at least about 500 µm, at least about 1 mm, or at least about 2 mm greater than the length of the solid-state cathode. In some embodiments, the inner length of the frame is about 20 µm to about 5 mm greater than the length of the solid-state cathode. In some embodiments, the inner length of the frame is about 20 µm to about 2.5 mm greater than the length of the solid-state cathode. In some embodiments, the inner length of the frame is about 20 µm to about 2 mm greater than the length of the solid-state cathode. In some embodiments, the inner length of the frame is about 50 µm to about 2 mm greater than the length of the solid-state cathode. In some embodiments, the inner length of the frame is about 100 µm to about 2 mm greater than the length of the solid-state cathode. In some embodiments, the inner length of the frame is about 200 µm to about 1.5 mm greater than the length of the solid-state cathode. In some embodiments, the inner length of the frame is about 300 µm to about 1.5 mm greater than the length of the solid-state cathode. In some embodiments, the inner length of the frame is about 400 µm to about 1.2 µm greater than the length of the solid-state cathode.
[0138] In some embodiments, the solid-state separator comprises lithium-filled garnet. In some embodiments, the solid-state separator consists essentially of lithium-filled garnet.
[0139] In some embodiments, the solid-state separator is represented by the formula Li A La B Zr C O F , Li A La B M' C M" D Ta E O F or Li A La B M' C M" D Nb E O F , where 4<A<8.5, 1.5<B<4, 0<C≤2, 0<D<2, 0<E<2.5, 10<F<13, and M' and M" are each independently selected at each occurrence from Al, Mo, W, Nb, Ga, Sb, Ca, Ba, Sr, Ce, Hf, Rb, and Ta; or is represented by the formula Li a La b Zr c Al d Me" e O fwherein 5<a<7.7, 2<b<4, 0<c≤2.5, 0<d<2, 0<e<2, 10<f<13, and Me" is a metal selected from Nb, V, W, Mo, Ta, Ga and Sb.
[0140] In some embodiments, the solid-state separator has a thickness of about 10 µm to 50 µm.
[0141] In a second aspect, the present application provides an electrochemical stack, comprising: a) a solid-state cathode having two major surfaces and four minor surfaces, wherein the solid-state cathode comprises a solid cathode electrolyte; b) a solid-state separator; c) a cathode current collector; d) an adhesive layer; and e) a frame surrounding the four minor surfaces of the solid-state cathode; the frame is located between and in contact with both the cathode current collector and the solid-state separator; the adhesive layer is located between and in contact with both the solid-state cathode and the solid-state separator.
[0142] In some embodiments, the electrochemical stack is substantially as shown in Figure 1. Figure 1 is not drawn to scale. In Figure 1 , the electrochemical stack 100 is shown in a cross-sectional view. The electrochemical stack 100 includes a solid-state cathode 102, which is disposed over the cathode current collector 104 on both sides of the stack. The electrochemical stack 100 further includes an adhesive layer 105 disposed over the solid-state cathode; and a solid-state separator 101 disposed over the adhesive layer 105 and in contact with the adhesive layer on both sides of the stack. The electrochemical stack 100 further includes a frame 103 surrounding the four minor surfaces of each solid-state cathode layer, and disposed between the solid-state separator 101 and the cathode current collector 104 on both sides of the stack. The electrochemical stack 100 further includes a void 107 located between the minor surface of the solid-state cathode and the frame. In some embodiments, the solid-state separator 101 includes any solid-state separator set forth in the present application. In some embodiments, the solid-state cathode 102 includes any cathode active material set forth in the present application. Within the solid-state cathode 102 is a solid cathode electrolyte, which in some embodiments may include any solid cathode electrolyte material set forth in the present application. The frame 103 is in contact with the solid-state separator 101 and the cathode current collector 104. In some non-limiting embodiments, the frame 103 is attached to the solid-state separator 101 and the cathode current collector 104.
[0143] In some embodiments, the electrochemical stack is substantially as shown in Figure 2. Figure 2 is not drawn to scale. In Figure 2In the diagram, an electrochemical stack 200 is shown in a vertical stacked view. The electrochemical stack 200 includes a double-sided solid cathode 202 with adhesive layers on both sides, and a cathode current collector 204 disposed between the double-sided solid cathodes. The electrochemical stack 200 also includes a solid membrane 201 located on both sides of the stack above the double-sided solid cathodes 202 and in contact with the adhesive layers on the double-sided solid cathodes. The electrochemical stack 200 also includes a frame 203 located on both sides of the stack between the solid membrane 201 and the cathode current collector 204, ultimately coplanar with and surrounding each layer of the double-sided solid cathode 202. The electrochemical stack 200 also includes an anode current collector 206 located on both sides of the stack above the solid membrane 201. In some embodiments, the solid membrane 201 includes any solid membrane described herein. In some embodiments, the solid cathode 202 includes any cathode active material described herein. The solid cathode 202 contains a solid cathode electrolyte, which in some embodiments includes any solid cathode electrolyte material described herein. When assembly is complete, the frame 203 contacts the solid diaphragm 201 and the cathode current collector 204. In some non-limiting embodiments, the frame 203 is attached to the solid diaphragm 201 and the cathode current collector 204.
[0144] Figure 3A is not drawn to scale. Figure 3A is a cross-sectional view of a frame including multiple layers 301A-303A. In some embodiments, the frame includes one or more layers. In some embodiments, the frame includes two or more layers. In some embodiments, the frame includes three or more layers. The cross-sectional thickness of the frame is shown as H. 框架 The cross-sectional thickness of the first layer 301A of the frame is shown as H. 301A The cross-sectional thickness of the second layer 302A of the frame is shown as H. 302A The cross-sectional thickness of the third layer 303A of the frame is shown as H. 303A The cross-sectional thickness H of each layer 301A H 302A and H 303A The sum equals the cross-sectional thickness H of the frame. 框架 In some non-limiting embodiments, the cross-sectional thickness H of the first layer 301A With the cross-sectional thickness H of the third layer 303A The same. In some non-limiting embodiments, the cross-sectional thickness H of the first layer is... 301A With the cross-sectional thickness H of the third layer 303A Different. In some non-limiting embodiments, the cross-sectional thickness H of the second layer is... 302A The cross-sectional thickness H is greater than that of the first layer 301A It is also greater than the cross-sectional thickness H of the third layer.303A .
[0145] Figure 3B is not drawn to scale. Figure 3B is a cross-sectional view of a frame including multiple layers 301B-302B. In some embodiments, the frame includes one or more layers. In some embodiments, the frame includes two or more layers. The cross-sectional thickness of the frame is shown as H. 框架 The cross-sectional thickness of the first layer 301B of the frame is shown as H. 301B The cross-sectional thickness of the second layer 302B of the frame is shown as H. 302B The cross-sectional thickness H of each layer 301B and H 302B The sum equals the cross-sectional thickness H of the frame. 框架 In some non-limiting embodiments, the cross-sectional thickness H of the first layer 301B With the cross-sectional thickness H of the second layer 302B Different. In some non-limiting embodiments, the cross-sectional thickness H of the second layer is... 302B The cross-sectional thickness H is greater than that of the first layer 301B .
[0146] Figure 4 is not drawn to scale. Figure 4 is a top view of the frame 402 surrounding the solid cathode 401. The outer width and length of the frame 402 are shown as W. 402 外 and L 402 外 The internal width and length of frame 402 are shown as W. 402 内 and L 402 内 The width and length of the solid cathode 401 are shown as W. 401 and L 401 In some implementations, the internal width W of the frame... 402 内 Width W greater than that of the solid cathode 401 In some implementations, the internal length L of the frame... 402 内 The length L greater than that of the solid cathode 401 .
[0147] Figure 5 is not drawn to scale. Figure 5 is a three-dimensional view of a solid-state cathode with secondary and primary surfaces. The primary surfaces are labeled as the two surfaces along the top and bottom of the solid-state cathode. The secondary surfaces are labeled as the four surfaces along the four sides of the solid-state cathode. The surface area of each primary surface is greater than the surface area of each of the four side surfaces.
[0148] Figure 6 is not drawn to scale. Figure 6 illustrates the effects of compressing framed and frameless electrochemical stacks. The upper electrochemical stack includes a solid separator 601 situated above a binder layer 605, which in turn is situated above a solid cathode 602, which is situated above a cathode current collector 604. The lower electrochemical stack includes a solid separator 601 situated above a binder layer 605, which in turn is situated above a solid cathode 602, which is situated above a cathode current collector 604, and also includes a frame 603 situated between the solid separator 601 and the cathode current collector 604. In the frameless stack, compression or stress on the stack (e.g., during assembly) can cause cracks 606 to appear in the solid separator 601 of the upper electrochemical stack. In a battery stack with frame 603, compression or pressure applied to the battery stack will not cause severe cracking or defects in any electrochemical stack component below the frame 603. The use of a frame in the battery stack is important for reducing crack formation in the solid separator during and after stack formation.
[0149] In some embodiments, the electrochemical stack is essentially as shown in Figure 7. Figure 7 is not drawn to scale. Figure 7The electrochemical stack 700 is shown in cross-sectional view. The electrochemical stack 700 includes a solid cathode 702 situated on both sides of the stack above a cathode current collector 704. The electrochemical stack 700 also includes an adhesive layer 705 situated above the solid cathode; and a solid diaphragm 701 situated above the adhesive layer 705 and contacting the adhesive layer on both sides of the stack. The electrochemical stack 700 also includes two frames, each surrounding four subsurfaces of each solid cathode layer, situated on both sides of the stack between the solid diaphragm 701 and the cathode current collector 704. Each frame includes two layers (703A / 708A or 703B / 708B), each layer comprising a thermoplastic polymer. In some embodiments, layers 708A and 703B comprise the same thermoplastic polymer. In some embodiments, layers 703A and 708B comprise the same thermoplastic polymer, while in other embodiments, layers 703A and 708B comprise different thermoplastic polymers. The electrochemical stack 700 also includes a void 707 located between the subsurface of the solid cathode and each frame. In some embodiments, the solid diaphragm 701 includes any solid diaphragm described herein. In some embodiments, the solid cathode 702 includes any cathode active material described herein. The solid cathode 702 contains a solid cathode electrolyte, which in some embodiments may include any solid cathode electrolyte material described herein. Frames on each side of the stack contact the solid diaphragm 701 and the cathode current collector 704. In some non-limiting embodiments, frames on each side of the stack are connected to the solid diaphragm 701 and the cathode current collector 704. In other non-limiting embodiments, frames on each side of the stack contact the solid diaphragm 701 and are connected to the cathode current collector 704.
[0150] In some embodiments, the electrochemical stack is substantially as shown in Figure 8. Figure 8 is not drawn to scale. Figure 8In the diagram, an electrochemical stack 800 is shown in cross-sectional view. The electrochemical stack 800 includes a solid cathode 802 situated on both sides of the stack above a cathode current collector 804. The electrochemical stack 800 also includes an adhesive layer 805 situated above the solid cathode; and a solid diaphragm 801 situated above the adhesive layer 805 and contacting the adhesive layer on both sides of the stack. The electrochemical stack 800 also includes two frames, each surrounding four subsurfaces of each solid cathode layer, situated on both sides of the stack between the solid diaphragm 801 and the cathode current collector 804. Each frame includes three layers (803A / 808A / 809A or 803B / 808B / 809B), each layer comprising a thermoplastic polymer. In some embodiments, layers 803A and 809A, layers 803B and 809B, or layers 803A, 809A, 803B, and 809B comprise the same thermoplastic polymer. In other embodiments, layer 808A comprises a different thermoplastic polymer than layers 803A and 809A. In still other embodiments, layer 808B comprises a different thermoplastic polymer than layers 803B and 809B. In some embodiments, layers 808A and 808B comprise the same thermoplastic polymer, while in other embodiments, layers 808A and 808B comprise different thermoplastic polymers. The electrochemical stack 800 also includes voids 807 located between the subsurface of the solid cathode and each frame. In some embodiments, the solid diaphragm 801 comprises any solid diaphragm described herein. In some embodiments, the solid cathode 802 comprises any cathode active material described herein. Solid cathode 802 contains a solid cathode electrolyte, which in some embodiments comprises any solid cathode electrolyte material described herein. Frames on each side of the stack contact the solid diaphragm 801 and the cathode current collector 804. In some non-limiting embodiments, the frames on each side of the stack are connected to the solid diaphragm 801 and the cathode current collector 804. In other non-limiting embodiments, the frames on each side of the stack contact the solid diaphragm 801 and are connected to the cathode current collector 804.
[0151] Figure 9 is not drawn to scale. Figure 9 is a top view of frame 900. The external width and length of frame 900 are shown as 902 and 901, respectively. The internal width and length of frame 900 are shown as 904 and 903, respectively.
[0152] Figure 10 is not drawn to scale. Figure 10 is a top view of the frame 1000 with an opening. The outer width and length of the frame 1000 are shown as 1002 and 1001, respectively. The inner width and length of the frame 1000 are shown as 1004 and 1003, respectively. The length of the opening of the frame 1000 is shown as 1005. In some embodiments, the length of the opening is sufficient to accommodate the tab. III. Methods for assembling electrochemical stacks
[0153] In a third aspect, this application provides a method for assembling an electrochemical stack, comprising: (1) Provide an electrochemical stack; the electrochemical stack includes: the frame, solid cathode, adhesive layer and solid membrane described in this application; (2) Apply a pressure of about 70 kPa to about 700 kPa to the electrochemical stack.
[0154] In some embodiments, the pressure applied in step (2) is from about 70 kPa to about 620 kPa. In some embodiments, the pressure applied in step (2) is from about 130 kPa to about 620 kPa. In some embodiments, the pressure applied in step (2) is from about 130 kPa to about 550 kPa. In some embodiments, the pressure applied in step (2) is from about 200 kPa to about 550 kPa. In some embodiments, the pressure applied in step (2) is from about 200 kPa to about 480 kPa. In some embodiments, the pressure applied in step (2) is from about 270 kPa to about 480 kPa. In some embodiments, the pressure applied in step (2) is from about 270 kPa to about 420 kPa.
[0155] In some embodiments, step (2) is performed at a temperature of about 80°C to about 160°C. In some embodiments, step (2) is performed at a temperature of about 90°C to about 160°C. In some embodiments, step (2) is performed at a temperature of about 100°C to about 160°C. In some embodiments, step (2) is performed at a temperature of about 110°C to about 160°C. In some embodiments, step (2) is performed at a temperature of about 120°C to about 160°C. In some embodiments, step (2) is performed at a temperature of about 130°C to about 160°C. In some embodiments, step (2) is performed at a temperature of about 140°C to about 160°C.
[0156] In some embodiments, step (2) is performed at a temperature of about 65°C to about 75°C, followed by a temperature of 80°C to about 160°C. In some embodiments, step (2) is performed at a temperature of about 65°C to about 75°C, followed by a temperature of 90°C to about 160°C. In some embodiments, step (2) is performed at a temperature of about 65°C to about 75°C, followed by a temperature of 100°C to about 160°C. In some embodiments, step (2) is performed at a temperature of about 65°C to about 75°C, followed by a temperature of 110°C to about 160°C. In some embodiments, step (2) is performed at a temperature of about 65°C to about 75°C, followed by a temperature of 120°C to about 160°C. In some embodiments, step (2) is performed at a temperature of about 65°C to about 75°C, followed by a temperature of 130°C to about 160°C. In some embodiments, step (2) is performed at a temperature of about 65°C to about 75°C, followed by a temperature of 140°C to about 160°C.
[0157] In some embodiments, the pressure applied in step (2) is from about 70 kPa to about 700 kPa, and step (2) is performed at a temperature from about 80 °C to about 160 °C. In some embodiments, the pressure applied in step (2) is from about 70 kPa to about 700 kPa, and step (2) is performed at a temperature from about 65 °C to about 75 °C, followed by a temperature from 80 °C to about 160 °C.
[0158] In some implementations, step (2) is performed for about 20 minutes, about 15 minutes, about 10 minutes, or about 5 minutes.
[0159] In some implementations, step (2) is performed for less than about 20 minutes, less than about 15 minutes, less than about 10 minutes, or less than about 5 minutes.
[0160] In some implementations, step (2) is performed for approximately 5 minutes to approximately 20 minutes. In some implementations, step (2) is performed for approximately 10 minutes to approximately 20 minutes. In some implementations, step (2) is performed for approximately 15 minutes to approximately 20 minutes.
[0161] In some embodiments, the electrochemical stack also includes an additional solid cathode, an additional solid membrane, an additional bonding layer, and an additional frame.
[0162] In some embodiments, the frame is connected to the solid-state diaphragm and the cathode current collector. In other embodiments, the frame is connected to the solid-state diaphragm and contacts the cathode current collector. In still other embodiments, the frame contacts the solid-state diaphragm and is connected to the current collector.
[0163] In some embodiments, an electrode stacking device is used to assemble the electrochemical stack. In some embodiments, the assembly of the electrochemical stack is carried out manually.
[0164] Non-restrictive implementation scheme
[0165] This application provides at least the following non-restrictive implementation schemes: (a) An electrochemical stack comprising: A solid cathode having two main surfaces, four secondary surfaces, a first width, and a first length, wherein the solid cathode comprises a solid cathode electrolyte; A solid diaphragm having a second width and a second length; Cathode current collector; Adhesive layer; and frame; The frame surrounds the four subsurfaces of the solid cathode; The frame is located between the cathode current collector and the solid membrane, and is in contact with both the cathode current collector and the solid membrane. The adhesive layer is located between the solid cathode and the solid membrane, and is in contact with both the solid cathode and the solid membrane; The first width is smaller than the second width, and the first length is smaller than the second length. (b) The electrochemical stack as described in (a), wherein the frame is connected to the solid membrane and the cathode current collector. (c) The electrochemical stack as described in (a), wherein the frame is connected to the cathode current collector. (d) An electrochemical stack as described in any one of (a)-(c), wherein the framework comprises a thermoplastic polymer. (e) The electrochemical stack as described in (d), wherein the thermoplastic polymer is selected from polyethylene polymers, polypropylene polymers, polybutene polymers, polypentene polymers, polystyrene polymers, polyaryletherketone polymers, polyaryletherimide polymers, polysulfone polymers, acrylate polymers, polycarbonate polymers, or combinations thereof. (f) An electrochemical stack as described in any one of (d)-(e), wherein the thermoplastic polymer is selected from modified polyethylene polymers, modified polypropylene polymers, modified polybutene polymers, modified polypentene polymers, modified polystyrene polymers, modified polyaryletherketone polymers, modified polyaryletherimide polymers, modified polysulfone polymers, modified acrylate polymers, modified perfluoroelastomer polymers, modified polycarbonate polymers, or combinations thereof. (g) The electrochemical stack as described in any one of (d)-(f), wherein the thermoplastic polymer is selected from acrylonitrile-butadiene-styrene copolymer (ABS), ethylene propylene rubber (EPM), ethylene propylene diene monomer (EPDM), fluorinated ethylene propylene copolymer (FEP), perfluoroelastomer (FFKM), polybutene-1 (PB-1), polycarbonate (PC), polyetheretherketone (PEEK), polyetherimide (PEI), polyethersulfone (PES), polyethylene terephthalate (PET), polyisobutylene (PIB), polyisoprene, polymethyl methacrylate (PMMA), polymethylpentene (PMP), polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-co-fluorinated ethylene propylene (PVDF-co-FEP), poly(styrene-isoprene-styrene) (SIS), poly(styrene-butadiene-styrene) (SBS), ultra-high molecular weight polyethylene (UHWPE), or combinations thereof. (h) An electrochemical stack as described in any one of (f)-(g), wherein the modified polyethylene polymer is a maleic anhydride polyethylene copolymer. (i) The electrochemical stack as described in (h), wherein the maleic anhydride polyethylene copolymer is cross-linked. (j) An electrochemical stack as described in any one of (a)-(i), wherein the framework comprises one or more layers. (k) An electrochemical stack as described in any one of (a)-(j), wherein the frame comprises two or more layers. (l) An electrochemical stack as described in any one of (a)-(k), wherein the frame comprises three or more layers. (m) An electrochemical stack as described in any one of (j)-(l), each layer comprising a thermoplastic polymer. (n) An electrochemical stack as described in any one of (a)-(m), wherein the frame comprises a first layer and a second layer, the first layer and the second layer of the frame comprising the same thermoplastic polymer. (o) An electrochemical stack as described in any one of (a)-(m), wherein the frame comprises a first layer and a second layer, the first layer and the second layer comprising different thermoplastic polymers. (p) The electrochemical stack as described in (o), wherein the first layer of the framework comprises a cross-linked maleic anhydride polyethylene copolymer. (q) An electrochemical stack as described in any one of (a)-(m), wherein the frame comprises a first layer, a second layer and a third layer, wherein the first layer and the third layer of the frame comprise the same thermoplastic polymer. (r) An electrochemical stack as described in any one of (a)-(m), wherein the frame comprises a first layer, a second layer and a third layer, the first layer and the third layer of the frame comprising different thermoplastic polymers. (s) An electrochemical stack as described in any one of (q)-(s), wherein the second layer of the framework comprises a thermoplastic polymer different from the first layer and the third layer. (t) An electrochemical stack as described in any one of (q) or (s), wherein the first and third layers of the frame comprise cross-linked maleic anhydride polyethylene copolymer. (u) An electrochemical stack as described in any one of (n)-(t), wherein the second layer of the framework comprises PEEK. (v) An electrochemical stack as described in any one of (n)-(t), wherein the second layer of the framework comprises PTFE. (w) An electrochemical stack as described in any one of (n)-(t), wherein the second layer of the framework comprises a polyimide polymer. (x) An electrochemical stack as described in any one of (n)-(t), wherein the second layer of the framework comprises a porous polyimide polymer. (y) An electrochemical stack as described in any one of (a)-(x), wherein the thermoplastic polymer has an initial size before heating or applying pressure, or heating and applying pressure, and a final size after heating or applying pressure, and the thermoplastic polymer shrinks or expands relative to the initial size by no more than about 5% after being heated to a temperature of about 80 °C to about 160 °C. (z) The electrochemical stack as described in any one of (a)-(y) wherein the thermoplastic polymer shrinks or expands relative to the initial size by no more than about 5% after pressure is applied. (aa) The electrochemical stack as described in any one of (a)-(z) wherein the thermoplastic polymer, after being heated to a temperature of about 80°C to about 160°C and subjected to pressure, shrinks or expands relative to the initial size by no more than about 5%. (bb) The electrochemical stack as described in any one of (a)-(aa), wherein the thermoplastic polymer has a Poisson's ratio of about 0.2 to about 0.3 at a temperature of about 110 °C to about 150 °C and a pressure of about 250 kPa to about 700 kPa. (cc) An electrochemical stack as described in any one of (a)-(bb), wherein each of the one or more independent layers of the frame has a thickness, the sum of the thicknesses of all layers being the total thickness of the frame, the total thickness of the frame being about 80 µm to about 200 µm. (dd) An electrochemical stack as described in any one of (n)-(p), wherein the thickness of the first layer is from about 10 µm to about 60 µm. (ee) An electrochemical stack as described in any one of (n)-(p), wherein the thickness of the second layer is about 50% to about 90% of the total thickness of the frame. (ff) An electrochemical stack as described in any one of (n)-(p), wherein the thickness of the second layer is from about 20 µm to about 140 µm. (gg) An electrochemical stack as described in any one of (q)-(t), wherein the first layer and the third layer have different thicknesses. (hh) As described in (gg), the thickness of the first layer is from about 10 µm to about 50 µm. (ii) The electrochemical stack as described in (gg), wherein the thickness of the third layer is from about 20 µm to about 60 µm. (jj) An electrochemical stack as described in any one of (q)-(t), wherein the first layer and the third layer have the same thickness. (kk) As described in (jj), the electrochemical stack has a thickness of approximately 10 µm to approximately 60 µm for the first and third layers, respectively. (ll) The electrochemical stack as described in any one of (q)-(t), wherein the thickness of the second layer is about 30% to about 70% of the total thickness of the frame. (mm) As in any one of (q)-(t) of the electrochemical stack, the thickness of the second layer is from about 20 µm to about 140 µm. (nn) An electrochemical stack as described in any one of (a)-(mm), wherein the frame has an inner frame length and an outer frame length, the inner frame length being about 60 mm to about 85 mm. (oo) The electrochemical stack as described in (nn) has an outer frame length of about 70 mm to about 95 mm. (pp) The electrochemical stack according to any one of (a) to (oo), wherein the frame has an inner frame width and an outer frame width, and the inner frame width is about 45 mm to about 70 mm. (qq) The electrochemical stack according to (pp), wherein the outer frame width is about 55 mm to 80 mm. (rr) The electrochemical stack according to any one of (a) to (qq), wherein the difference between the outer frame length and the inner frame length is about 5 mm to about 35 mm. (ss) The electrochemical stack according to any one of (a) to (qq), wherein the difference between the outer frame width and the inner frame width is about 5 mm to about 35 mm. (tt) The electrochemical stack according to any one of (a) to (ss), wherein the inner frame width and the inner frame length are each at least about 20 µm greater than the width and the length of the solid-state cathode, respectively. (uu) The electrochemical stack according to any one of (a) to (tt), wherein the solid-state separator comprises lithium-filled garnet. (vv) The electrochemical stack according to any one of (a) to (uu), wherein the solid-state separator consists essentially of lithium-filled garnet. (ww) The electrochemical stack according to any one of (a) to (vv), wherein the lithium-filled garnet separator is represented by the formula Li A La B Zr C O F , Li A La B M' C M" D Ta E O F or Li A La B M' C M" D Nb E O F , wherein 4<A<8.5, 1.5<B<4, 0<C≤2, 0<D<2, 0<E<2.5, 10<F<13, and M' and M" are each independently selected in each case from Al, Mo, W, Nb, Ga, Sb, Ca, Ba, Sr, Ce, Hf, Rb and Ta; or represented by the formula Li a La b Zr c Al d Me" e O fwhere 5<a<7.7, 2<b<4, 0<c≤2.5, 0<d<2, 0<e<2, 10<f<13, and Me" is a metal selected from Nb, V, W, Mo, Ta, Ga and Sb. (xx) The electrochemical stack according to any one of (a)-(ww), further comprising a second solid-state cathode, a second solid-state separator, a second adhesive layer and a second frame. (yy) An electrochemical stack, comprising: a solid-state cathode having two main surfaces and four secondary surfaces, wherein the solid-state cathode comprises a solid cathode electrolyte; a solid-state separator; a cathode current collector; an adhesive layer; and a frame surrounding the four secondary surfaces of the solid-state cathode; the frame being located between the cathode current collector and the solid-state separator and in contact with the cathode current collector and the solid-state separator; the adhesive layer being located between the solid-state cathode and the solid-state separator and in contact with the solid-state cathode and the solid-state separator. (zz) A method of assembling an electrochemical stack, comprising: i. providing an electrochemical stack, wherein the electrochemical stack comprises: the frame in the electrochemical stack according to any one of (a)-(ww); a solid-state cathode, an adhesive layer and a solid-state separator; and ii. applying a pressure of about 70 kPa to about 700 kPa to the electrochemical stack. (aaa) The method according to (zz), wherein step (ii) is performed at a temperature of about 80°C to about 160°C. (bbb) The method according to any one of (zz)-(aaa), wherein the electrochemical stack comprises a second solid-state cathode, a second solid-state separator, a second adhesive layer and a second frame. (ccc) The method according to any one of (zz)-(bbb), wherein the frame is connected to the solid-state separator and the cathode current collector. (ddd) The method according to any one of (zz)-(bbb), wherein the frame is connected to the cathode current collector and in contact with the solid-state separator. (eee) The method according to any one of (zz)-(ddd), wherein the frame comprises a thermoplastic polymer. (fff) The method according to any one of (zz)-(eee), wherein the frame comprises one or more layers. (ggg) The method of any one of (zz)-(fff) wherein the solid membrane comprises lithium-filled garnet. (hhh) A method for assembling an electrochemical stack includes: i. Provide a framework for an electrochemical stack as described in any one of (a)-(ww); ii. Provide a solid cathode with an adhesive layer on a main surface; iii. The solid cathode is placed within the frame, the frame surrounding all four subsurfaces of the solid cathode, thereby forming a sub-pile; iv. Apply a pressure of about 70 kPa to about 700 kPa to the sub-stacking at a temperature of about 65 °C to about 75 °C; v. Placing a solid diaphragm on the adhesive layer to form an electrochemical stack; and vi. Apply a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 80 °C to about 160 °C. (iii) A method for assembling an electrochemical stack, comprising: i. Provide a framework as described in any one of (a)-(ww); ii. A solid cathode is placed within the frame, the frame surrounding all four subsurfaces of the solid cathode, thereby forming a sub-pile; iii. Apply a pressure of about 70 kPa to about 700 kPa to the sub-stacking at a temperature of about 65 °C to about 75 °C; iv. Provide a solid diaphragm with an adhesive layer; v. Placing a solid cathode with a frame on the adhesive layer to form an electrochemical stack; and vi. Apply a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 80 °C to about 160 °C. (jjj) A method for assembling an electrochemical stack, comprising: i. Provide a framework as described in any one of (a)-(ww); ii. The frame is placed on a solid diaphragm to form a sub-pile; iii. Apply a pressure of about 70 kPa to about 700 kPa to the sub-stacking at a temperature of about 65 °C to about 75 °C; iv. Provide a solid cathode with an adhesive layer on a main surface; v. Placing a solid cathode with an adhesive layer on a solid membrane with a frame surrounding four subsurfaces of the solid cathode, the adhesive layer contacting the solid membrane, thereby forming an electrochemical stack; and vi. Apply a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 80 °C to about 160 °C. (kkk) A method for assembling an electrochemical stack, comprising: i. Provide a framework as described in any one of (a)-(ww); ii. Provide a solid diaphragm with an adhesive layer; iii. The frame is placed on the solid diaphragm to form a sub-pile; iv. Apply a pressure of about 70 kPa to about 700 kPa to the sub-stacking at a temperature of about 65 °C to about 75 °C; v. Placing a solid cathode on a solid diaphragm with a frame surrounding four subsurfaces of the solid cathode, the adhesive layer contacting the solid cathode to form an electrochemical stack; and vi. Apply a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 80 °C to about 160 °C. (lll) A method for assembling an electrochemical stack, comprising: i. Provide a framework as described in any one of (a)-(ww); ii. Provide a solid cathode with an adhesive layer on a main surface; iii. The solid cathode is placed within the frame surrounding the four subsurfaces of the solid cathode, and a solid diaphragm is placed on the adhesive layer to form an electrochemical stack; iv. Applying a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 65 °C to about 75 °C; and v. Applying a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 80 °C to about 160 °C. (mmm) A method for assembling an electrochemical stack, comprising: i. Provide a framework as described in any one of (a)-(ww); ii. Provide a solid diaphragm with an adhesive layer; iii. A solid cathode is placed within the frame surrounding the four subsurfaces of the solid cathode, and a solid diaphragm with an adhesive layer is placed on the solid cathode with the frame, the adhesive layer contacting the solid cathode, thereby forming an electrochemical stack; iv. Apply a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 65 °C to about 75 °C; v. Applying a pressure of about 70 kPa to about 700 kPa to the electrochemical stack at a temperature of about 80 °C to about 160 °C. Example
[0166] Unless otherwise stated, all reagents, chemicals and materials disclosed in this application are commercially available.
[0167] Unless otherwise specified, lithium-filled garnet films are prepared as follows: A slurry of lithium-filled garnet precursor material is deposited onto an aluminum substrate using a doctor blade method and sintered at 1000 °C to 1300 °C to produce a lithium-filled garnet film with a thickness of approximately 20 to 50 micrometers (µm).
[0168] Unless otherwise specified, the bilayer (film on metal foil) is prepared as follows: A slurry of lithium-filled garnet precursor material is cast onto a metal foil and dried to form a green tape. The bilayer is sintered at 1000 °C to 1300 °C. The sintered film is then cut to appropriate dimensions using a laser cutter. The bilayer film of this application is prepared according to, for example, WO / 2022 / 192464 published on September 15, 2022, the entire contents of which are incorporated herein by reference.
[0169] Unless otherwise specified, the external dimensions (i.e., the length and width of the main surfaces) of lithium-filled garnet films and bilayer films used for electrochemical assembly are larger than the corresponding external dimensions of the bi-sided solid cathodes used in each cell. Example 1 – Method 1: Assembly method of electrochemical stack including solid cathode frame
[0170] A PTFE liner is placed on a stainless steel substrate to prevent static electricity generation and adhesion of any electrochemical stack components during assembly. Next, a first frame is placed on the PTFE liner. This frame has three layers, each with a thermoplastic polymer. Additionally, a lithium borohydride adhesive layer is deposited on both layers of the double-sided solid cathode, with a cathode current collector positioned between the two solid cathode layers. The double-sided solid cathode is placed within the frame, centered relative to the frame center and one of the cathode layers. Next, a second frame, identical to the first frame, is placed, centered relative to the frame center and the second cathode layer of the double-sided cathode. The inner frame length, inner frame width, and total frame thickness are all greater than the corresponding length, width, and thickness of any solid cathode layer of the double-sided solid cathode. A second PTFE liner, followed by a second stainless steel substrate, is placed on top of the assembly. High-temperature silicone foam is added to the top stainless steel plate to provide uniform pressure distribution.
[0171] The component was heated for 2 minutes at a temperature of approximately 65 °C to approximately 75 °C and a pressure of approximately 70 kPa to approximately 700 kPa. The component was then removed and cooled to room temperature.
[0172] Additionally, an anode current collector is applied onto a lithium-filled garnet solid membrane. This lithium-filled garnet solid membrane is then placed on top of the frames on both sides of the assembly, forming a stack. Finally, the stack is heated for several minutes at a temperature of approximately 80 °C to approximately 160 °C and a pressure of approximately 70 kPa to approximately 700 kPa. Example 2 – Method 2: Electrochemical Cell Assembly Method Including Solid Cathode Frame
[0173] A lithium borohydride binder layer is deposited on both layers of a double-sided solid cathode, and a cathode current collector is disposed between the two solid cathode layers. The anode current collector is placed on one side of the lithium-filled garnet solid membrane.
[0174] An electrochemical stack was assembled using an electrode stacking device. A frame was automatically stacked on top of the lithium-filled garnet solid separator, opposite the anode current collector, and aligned relative to the frame center. The frame had three layers, each containing a thermoplastic polymer. The assembly was heated for 2 minutes at a temperature of approximately 65°C to approximately 75°C and a pressure of approximately 70 kPa to approximately 700 kPa. The assembly was then removed and cooled to room temperature. A double-sided solid cathode with an adhesive layer was placed within the frame, centered relative to the frame center and one cathode layer of the double-sided cathode. Next, a second frame identical to the first frame was placed, centered relative to the frame center and the second cathode layer of the double-sided cathode. The double-sided solid cathode was automatically aligned relative to the frame center of each frame, such that each frame surrounds each cathode layer of the double-sided solid cathode. The internal frame length, internal frame width, and total frame thickness of both frames were greater than the corresponding length, width, and thickness of any solid cathode layer of the double-sided solid cathode. Then, another lithium-filled garnet solid separator was placed on top of the top frame, in contact with both the top adhesive layer and the frame.
[0175] Finally, the pile was heated for several minutes at a temperature of about 80 °C to about 160 °C and a pressure of about 70 kPa to about 700 kPa. Example 3 – Method 3: Electrochemical Cell Assembly Method Including Solid Cathode Frame
[0176] A PTFE liner is placed on a stainless steel substrate to prevent static electricity generation and adhesion of any electrochemical stack components during assembly. Next, a first frame is placed on the PTFE liner. This frame has two layers, each containing a thermoplastic polymer. One of the thermoplastic polymers is a cross-linked maleic anhydride polyethylene copolymer. A double-sided solid cathode is placed within the frame, centered relative to the frame center and one cathode layer of the double-sided cathode, with a cathode current collector positioned between the two solid cathode layers. The cross-linked maleic anhydride polyethylene copolymer layer of this frame faces the cathode current collector. Next, a second frame identical to the first frame is placed, centered relative to the frame center and the second cathode layer of the double-sided cathode, with the cross-linked maleic anhydride polyethylene copolymer layer of this frame facing the cathode current collector. The inner frame length, inner frame width, and total frame thickness are all greater than the corresponding length, width, and thickness of any solid cathode layer of the double-sided solid cathode. A second PTFE liner, followed by a second stainless steel substrate, is placed on top of the assembly. High-temperature silicone foam is added to the top stainless steel plate to provide uniform pressure distribution.
[0177] The component was heated for 2 minutes at a temperature of approximately 65 °C to approximately 75 °C and a pressure of approximately 70 kPa to approximately 700 kPa. The component was then removed and cooled to room temperature.
[0178] Next, lithium borohydride binder layers are deposited on both layers of the double-sided cathode.
[0179] Alternatively, an anode current collector is placed on a lithium-filled garnet solid membrane. The lithium-filled garnet solid membrane is then placed on top of the frames on both sides of the assembly, forming a stack.
[0180] Finally, the pile was heated for several minutes at a temperature of about 80 °C to about 160 °C and a pressure of about 70 kPa to about 700 kPa. Example 4 – Method 4: Electrochemical Cell Assembly Method Including Solid Cathode Frame
[0181] A lithium borohydride binder layer is deposited on one side of a lithium-filled garnet solid membrane. Then, an anode current collector is applied to the other side of the membrane to form a lithium-filled garnet solid membrane assembly.
[0182] An electrochemical stack is assembled using an electrode stacking device. A double-sided solid cathode is automatically stacked on top of a frame, aligned with the frame center and one cathode layer of the double-sided cathode, with a cathode current collector positioned between the two solid cathode layers. The frame has two layers, each containing a thermoplastic polymer. One of the thermoplastic polymers is a cross-linked maleic anhydride polyethylene copolymer, facing the cathode current collector. Next, a second frame identical to the first frame is placed, centered with respect to the frame center and the second cathode layer of the double-sided cathode. The cross-linked maleic anhydride polyethylene copolymer layer of the second frame faces the cathode current collector. The inner frame length, inner frame width, and total frame thickness are all greater than the corresponding length, width, and thickness of any solid cathode layer of the double-sided solid cathode.
[0183] The bifacial cathode assembly was then heated for 2 minutes at a temperature of approximately 65 °C to approximately 75 °C and a pressure of approximately 70 kPa to approximately 700 kPa. The assembly was then removed and allowed to cool to room temperature.
[0184] Next, the double-sided cathode assembly is automatically stacked on top of the lithium-filled garnet solid membrane assembly from above, relative to the center of the separator. The adhesive layer contacts one cathode layer of the double-sided cathode, and the separator contacts the frame. Then, a second lithium-filled garnet solid membrane assembly is automatically stacked on top of the double-sided cathode assembly, with the adhesive layer facing the second layer of the double-sided cathode, forming a stack.
[0185] Finally, the pile was heated for several minutes at a temperature of about 80 °C to about 160 °C and a pressure of about 70 kPa to about 700 kPa. Example 5 – Battery Performance Study
[0186] Electrochemical cells were assembled according to Examples 1-4, with varying numbers of frame layers and thermoplastic polymers. The electrochemical cells were tested using 1C CC-CV (constant current-constant voltage) charging – 1C CC (constant current) discharging at 30 °C. Cycle count was defined as the number of cycles with a capacity retention greater than 80%. The results are shown in Table 1. A indicates more than 1000 cycles, B indicates 200-1000 cycles, and C indicates less than 200 cycles.
[0187] PEX refers to cross-linked maleic anhydride polyethylene copolymer, PI refers to polyimide polymer, PEEK refers to polyether ether ketone polymer, PIB refers to polyisobutylene polymer, and PTFE refers to polytetrafluoroethylene polymer. Example 6 – X-ray crosslinking and thermal deformation
[0188] Maleic anhydride polyethylene copolymer was modified by irradiating it with X-rays to initiate crosslinking in the polymer.
[0189] The heat distortion as a function of temperature (room temperature to 200 °C) was measured for both cross-linked and uncross-linked maleic anhydride polyethylene copolymers. The uncross-linked polymer began to deform around 100 °C, exhibiting up to 100% deformation at approximately 160 °C. In contrast, the cross-linked polymer only began to deform above 115 °C, producing less than 10% deformation at temperatures up to 200 °C. Example 7 – X-ray crosslinking and tensile strength
[0190] Alternatively, the maleic anhydride polyethylene copolymer was modified by irradiating it with X-rays at intensities of 25 kGy, 50 kGy, or 100 kGy to initiate crosslinking.
[0191] For each crosslinked polymer and the uncrosslinked maleic anhydride polyethylene copolymer (0 kGy), tensile strength was measured as a function of temperature (room temperature to 200 °C). The unirradiated sample (0 kGy) exhibited a sharp decrease in tensile strength at 110 °C, corresponding to a decrease in tensile modulus of nearly five orders of magnitude. The tensile moduli measured at 110 °C were: 1 kPa for the uncrosslinked polymer (0 kGy), 600 kPa for the sample irradiated with 25 kGy, 600 kPa for the sample irradiated with 50 kGy, and 1440 kPa for the sample irradiated with 100 kGy. Relative to the initial tensile modulus, the corresponding tensile moduli for each crosslinked sample did not decrease by more than three orders of magnitude at temperatures up to 200 °C.
[0192] The above embodiments and examples are intended to be illustrative rather than restrictive. Those skilled in the art will recognize, or be able to, numerous equivalents for determining a particular compound, material, and procedure using no more than conventional experiments. All such equivalents are considered to fall within the scope of this application and are covered by the appended claims.
Claims
1. An electrochemical stack comprising: A solid cathode having two main surfaces, four secondary surfaces, a first width, and a first length, the solid cathode comprising a solid cathode electrolyte; A solid diaphragm having a second width and a second length; Cathode current collector; bonding layer; and frame; The frame surrounds the four subsurfaces of the solid cathode; The frame is located between the cathode current collector and the solid membrane and is in contact with both the cathode current collector and the solid membrane. The adhesive layer is located between the solid cathode and the solid membrane and is in contact with both the solid cathode and the solid membrane; the first width is less than the second width, and the first length is less than the second length.
2. The electrochemical stack according to claim 1, wherein the frame is connected to the cathode current collector.
3. The electrochemical stack according to claim 1, wherein the frame is connected to the solid membrane and the cathode current collector.
4. The electrochemical stack according to any one of claims 1-3, wherein the framework comprises a thermoplastic polymer.
5. The electrochemical stack according to claim 4, wherein the thermoplastic polymer is selected from polyethylene polymers, polypropylene polymers, polybutene polymers, polypentene polymers, polystyrene polymers, polyaryletherketone polymers, polyaryletherimide polymers, polysulfone polymers, acrylate polymers, polycarbonate polymers, or combinations thereof.
6. The electrochemical stack according to any one of claims 4-5, wherein the thermoplastic polymer is selected from modified polyethylene polymers, modified polypropylene polymers, modified polybutene polymers, modified polypentene polymers, modified polystyrene polymers, modified polyaryletherketone polymers, modified polyaryletherimide polymers, modified polysulfone polymers, modified acrylate polymers, modified perfluoroelastomer polymers, modified polycarbonate polymers, or combinations thereof.
7. The electrochemical stack according to any one of claims 4-6, wherein the thermoplastic polymer is selected from acrylonitrile-butadiene-styrene copolymer (ABS), ethylene propylene rubber (EPM), ethylene propylene diene monomer (EPDM), fluorinated ethylene propylene copolymer (FEP), perfluoroelastomer (FFKM), polybutene-1 (PB-1), polycarbonate (PC), polyetheretherketone (PEEK), polyetherimide (PEI), polyethersulfone (PES), polyethylene terephthalate (PET), polyisobutylene (PIB), polyisoprene, polymethyl methacrylate (PMMA), polymethylpentene (PMP), polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-co-fluorinated ethylene propylene (PVDF-co-FEP), poly(styrene-isoprene-styrene) (SIS), poly(styrene-butadiene-styrene) (SBS), ultra-high molecular weight polyethylene (UHWPE), or combinations thereof.
8. The electrochemical stack according to any one of claims 6-7, wherein the modified polyethylene polymer is a maleic anhydride polyethylene copolymer.
9. The electrochemical stack according to claim 8, wherein the maleic anhydride polyethylene copolymer is cross-linked.
10. The electrochemical stack according to any one of claims 1-9, wherein the framework comprises one or more layers.
11. The electrochemical stack according to any one of claims 1-10, wherein the frame comprises two or more layers.
12. The electrochemical stack according to any one of claims 1-11, wherein the frame comprises three or more layers.
13. The electrochemical stack according to any one of claims 10-12, wherein each layer comprises a thermoplastic polymer.
14. The electrochemical stack according to any one of claims 1-13, wherein the frame comprises a first layer and a second layer, the first layer and the second layer of the frame comprising the same thermoplastic polymer.
15. The electrochemical stack according to any one of claims 1-13, wherein the frame comprises a first layer and a second layer, the first layer and the second layer of the frame comprising different thermoplastic polymers.
16. The electrochemical stack of claim 15, wherein the first layer of the framework comprises a cross-linked maleic anhydride polyethylene copolymer.
17. The electrochemical stack according to any one of claims 1-13, wherein the frame comprises a first layer, a second layer, and a third layer, wherein the first layer and the third layer of the frame comprise the same thermoplastic polymer.
18. The electrochemical stack according to any one of claims 1-13, wherein the frame comprises a first layer, a second layer, and a third layer, wherein the first layer and the third layer of the frame comprise different thermoplastic polymers.
19. The electrochemical stack according to any one of claims 17-18, wherein the second layer of the frame comprises a thermoplastic polymer different from the first layer and the third layer.
20. The electrochemical stack according to claim 17 or 19, wherein the first and third layers of the frame comprise cross-linked maleic anhydride polyethylene copolymer.
Citation Information
Patent Citations
SOLID STATE CATHOLYTE OR ELECTROLYTE FOR BATTERY USING LiaMPbSc (M=Si, Ge, and / or Sn)
US20150171465A1
Electrolyte separators including lithium borohydride and composite electrolyte separators of lithium-stuffed garnet and lithium borohydride
WO2018075972A1
Borohydride-sulfide interfacial layer in all solid-state battery
WO2019078897A1
Rapid ceramic processing techniques and equipment