Sequential self-alignment method in complementary field-effect transistor devices
By replacing the sacrificial layer of CFET devices through a sequential self-aligned process, the problems of material degradation and deposition difficulty in high-temperature processes of CFET devices are solved, improving production efficiency and yield, and supporting the application of GAA to replace metal gates.
Patent Information
- Application Number
- CN202580029393.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-22
- Filing Date
- 2025-03-28
- Publication Date
- 2026-11-17
AI Technical Summary
The vertical orientation of existing CFET devices faces challenges in high-temperature processes, including material degradation and difficulty in depositing high aspect ratio features, leading to low production efficiency and reduced yield.
By employing a sequential self-aligned process, complementary field-effect transistors (CFETs) are formed by replacing the sacrificial layers in the top and bottom element structures, and insulators are inserted between the nanosheet stacks to reduce the feature height and avoid the need for high-temperature thermally stable materials.
It effectively solves the problem of material damage caused by high-temperature processes, reduces the difficulty of deposition of aspect ratio features, improves production efficiency and yield, and supports the application of current gate all-around (GAA) replacement of metal gate (RMG) and epitaxial processes.
Smart Images

Figure CN123126052A_ABST
Abstract
Description
Technical Field
[0001] The embodiments described herein generally relate to the fabrication of semiconductor devices, and in particular to methods for forming complementary field-effect transistor (CFET) devices. Background Technology
[0002] To continue scaling beyond the physical limits of planar metal-oxide-semiconductor field-effect transistors (MOSFETs), as well as quasi-planar devices such as FinFETs, and traditional nanosheet or forked gate fully surrounded FETs (GAAFETs), complementary FET (CFET) devices have been proposed. CFETs are attractive for technology node shrinking due to their vertically stacked N-type metal-oxide-semiconductor (NMOS) and P-type metal-oxide-semiconductor (PMOS) structures, offering significant advantages over other transistor types, including reduced area requirements and lower power consumption.
[0003] However, the vertical orientation of CFET devices presents numerous manufacturing challenges. For example, in the currently proposed process flow, the contact trenches in the bottom element are filled with silicide and metal contact slots before the top element is formed. Therefore, silicides and contact slots formed from currently known materials, such as titanium silicides, cobalt, or tungsten, may not withstand the high-temperature processes required to form the top element and may degrade during these processes. High-temperature processes also cause problems for the front-side copper wiring when forming the back-side contacts. In another instance, the vertical orientation of the CFET architecture creates a very high aspect ratio, making it difficult to create and uniformly deposit materials within it. Therefore, new methods for forming CFET devices are urgently needed. Summary of the Invention
[0004] Embodiments of this disclosure provide a method for forming a semiconductor device structure, and more specifically, a method for forming complementary field-effect transistor (CFET) devices or other vertically aligned semiconductor structures using a sequential self-aligned process.
[0005] In one embodiment, a method for forming a complementary field-effect transistor (CFET) is provided. The method includes replacing a top sacrificial layer between channel layers in a top superlattice of a top element structure disposed on a bottom element structure, the top element structure being disposed on a first substrate layer, with a top replacement metal gate layer; securing a second substrate layer to the top element structure; removing the first substrate layer from the bottom element structure; and replacing a bottom sacrificial layer between channel layers in a bottom superlattice of the bottom element structure with a bottom replacement metal gate layer.
[0006] In another embodiment, a method of forming a CFET includes sequentially forming a CFET element from a nanosheet stack disposed on a first substrate layer, wherein the nanosheet stack includes a bottom element structure and a top element structure disposed above the bottom element structure, the bottom element structure and the top element structure each including: (a) a sacrificial superlattice layer, and (b) a superlattice disposed above the sacrificial superlattice layer, the superlattice including a plurality of channel layers extending through a dummy gate layer, wherein the plurality of channel layers are separated by a plurality of sacrificial layers, wherein the dummy gate layer includes a top dummy gate layer in the top element structure and a bottom dummy gate layer in the bottom element structure. The sequential formation of a CFET device further includes forming a portion of a bottom field-effect transistor (FET) from a bottom device structure and a portion of a top FET from a top device structure; replacing the sacrificial superlattice layer of the bottom device structure with an isolation structure and replacing the sacrificial superlattice layer of the top device structure with an isolation structure; forming a second portion of the bottom FET from the bottom device structure and disposing a first dielectric fill layer on the bottom device structure; forming a second portion of the top FET; bonding a second substrate layer to the top FET; removing the first substrate layer; removing the first dielectric fill layer; forming a second portion of the bottom FET; forming a bottom FET device contact; bonding a third substrate layer to the bottom FET; and forming a top FET device contact. Attached Figure Description
[0007] To enable a detailed understanding of the features of this disclosure described above, more specific descriptions of the disclosure briefly summarized above may be found in the embodiments, some of which are illustrated in the accompanying drawings. However, it should be noted that the drawings illustrate exemplary embodiments only and should not be construed as limiting the scope thereof, and other equally effective embodiments may be recognized.
[0008] Figure 1 A schematic top view of a multi-chamber processing system is illustrated according to the embodiments described herein.
[0009] Figures 2A to 2C A process flow diagram of a method for forming a semiconductor structure is illustrated according to the embodiments described herein.
[0010] Figures 3A to 3Z A cross-sectional view of a portion of a semiconductor element substrate is illustrated during the method according to the embodiments described herein.
[0011] Figure 4 A cross-sectional view of a portion of a semiconductor device structure is illustrated according to the embodiments described herein.
[0012] For ease of understanding, the same reference numerals have been used to identify the same elements in the figures where feasible. It is foreseeable that elements and features of one embodiment may be beneficially integrated into other embodiments without further explanation.
[0013] This disclosure contains at least one page of drawings executed in color. A copy of this disclosure, with a color appendix, will be provided to the Patent Office upon request and payment of the necessary fees. Since the color drawings are submitted electronically via EFS-Web, only one set of drawings is submitted. Detailed Implementation
[0014] Integrated circuits have evolved into complex components that can contain billions of transistors, capacitors, and resistors on a single chip. In the course of the evolution of integrated circuits, functional density (i.e., the number of interconnects per chip area) has generally increased, while geometry (i.e., the smallest element (or line) that can be created using manufacturing processes) has decreased.
[0015] To continue scaling beyond the physical limits of planar metal-oxide-semiconductor field-effect transistors (MOSFETs), as well as quasi-planar devices such as FinFETs and nanosheet and fork-gate fully enclosed FETs (GAAFETs), complementary FET (CFET) devices have been proposed. CFETs are attractive for technology node shrinking due to their vertically stacked NMOS and PMOS structures, which offer significant advantages over other types of transistors, including reduced area requirements and lower power consumption.
[0016] However, the vertical orientation of CFET devices presents numerous manufacturing challenges. For example, in the currently proposed process flow, the contact trenches in the bottom element are filled with silicide and metal contact slots before the top element is formed. Therefore, silicides and contact slots made of currently known materials, such as titanium silicide, cobalt, or tungsten, may not withstand the high-temperature processes required to form the top element and may degrade during these processes. High-temperature processes also cause problems for the front-side copper traces when forming the back-side contacts. In another instance, the vertical orientation of the CFET architecture creates a very high aspect ratio, making it difficult to create and uniformly deposit materials within it.
[0017] Compared to traditional monolithic approaches, which rely on complex alignment and device bonding methods that degrade device performance and yield, certain aspects of this disclosure include methods that allow for the creation of CFETs or other vertically aligned semiconductor structures using sequential self-aligned processes in a more efficient manner. By reducing feature height and eliminating several high aspect ratio modules, the methods described herein reduce the problems associated with traditional high aspect ratio features. Furthermore, by inserting another insulator between nanosheet stacks, the methods described herein reduce or eliminate the need for high-temperature thermally stable silicides, contact pads, and gap fill materials, thereby allowing the current Gate All-Around (GAA) replacement of Metal Gate (RMG) and epitaxial processes to be utilized without requiring lower thermal budgets. For example, the methods described herein also allow the front copper wires to remain unexposed to the thermal budget of the back-side contact formation at temperatures exceeding 4000°C (approximately 800–850°C).
[0018] Processing System Instances
[0019] Figure 1 A schematic representation of a processing system 100 used in conjunction with one or more embodiments of this disclosure is illustrated. In one or more embodiments, the processing system 100 may be used to perform all or part of the method 200.
[0020] As detailed below, substrates in processing system 100 can be processed and transferred within individual chambers without exposing them to the surrounding environment outside processing system 100 (e.g., the atmosphere that may exist in a semiconductor foundry). For example, substrates can be processed and transferred within individual chambers maintaining low pressure (e.g., less than or equal to about 300 Torr) or subatmospheric pressure, such as in a vacuum environment, without disrupting the reduced relative pressure or vacuum environment in the various processes performed on the substrates within processing system 100. Therefore, processing system 100 can provide some integrated solutions for substrate processing.
[0021] Examples of processing systems that can be appropriately modified based on the provided teachings include Endura. ® Integrated processing systems or other suitable commercially available processing systems are provided by Applied Materials, Inc., located in Santa Clara, California, USA. It is conceivable that other processing systems, including those from other manufacturers, can be adapted to benefit from the described aspects.
[0022] Figure 1This is a schematic top view of a processing system 100 (also referred to as a “processing platform”) according to embodiments described herein. The processing system 100 typically includes a device front-end module (EFEM) 102 for loading substrates into the processing system 100, a first load-locking chamber 104 coupled to the EFEM 102, a transfer chamber 108 coupled to the first load-locking chamber 104, and a plurality of other chambers coupled to the transfer chamber 108 as described in detail below. The EFEM 102 typically includes one or more robots 105 configured to transfer substrates from a front-opening wafer transfer cassette (FOUP) 103 to at least one of the first load-locking chamber 104 or a second load-locking chamber 106. Starting from the buffer portion 108A of the first load-locking chamber 104, and proceeding counterclockwise along the transfer chamber 108, the processing system 100 includes a first dedicated degassing chamber 109, a first pre-cleaning chamber 110, a first passage chamber 112, a second passage chamber 113, a second pre-cleaning chamber 114, a second degassing chamber 116, and a second load-locking chamber 106. The buffer portion 108A of the transfer chamber 108 includes a first robot 115 configured to transfer the substrate to each of the load-locking chambers 104 and 106, the degassing chambers 109 and 116, the pre-cleaning chambers 110 and 114, and the passage chambers 112 and 113.
[0023] The rear end portion 108B of the transfer chamber 108 includes a second robot 135 configured to transfer a substrate to each of the processing chambers connected to the rear end portion 108B of the processing system 100 via chambers 112, 113. The processing chambers may include a first processing chamber 132, a second processing chamber 134, a third processing chamber 136, a fourth processing chamber 138, and a fifth processing chamber 140. Generally, processing chambers 132, 134, 136, 138, and 140 may include at least one of the following: atomic layer deposition (ALD) chamber, chemical vapor deposition (CVD) chamber, physical vapor deposition (PVD) chamber, etching chamber, degassing chamber, annealing chamber, and other types of semiconductor substrate processing chambers. In some embodiments, one or more of processing chambers 132, 134, 136, 138, and 140 are PVD chambers. In some instances, processing chamber 110 may be capable of performing etching processes, processing chamber 114 may be capable of performing cleaning or annealing processes, and processing chambers 132, 134, 136, 138, and 140 may be capable of performing their respective CVD or ALD deposition processes. In one instance, processing chamber 110 or 114 may be a SELECTRA from Applied Materials in Santa Clara, California. ®Etching chamber. In one example, processing chamber 110 or 114 might be SICONI from Applied Materials, Santa Clara, California. ® Pre-cleaning chambers. In one example, processing chambers 132, 134, 136, 138, or 140 might be from the Volta system of Applied Materials, Inc., Santa Clara, California. ® CVD / ALD chamber, or SIP ENCORE ® PVD chamber.
[0024] The buffer portion 108A and the rear end portion 108B of the transfer chamber 108, as well as each chamber coupled to the transfer chamber 108, can be maintained in a vacuum state. As used herein, the term "vacuum" can refer to a pressure below 760 Torr and will typically be maintained at a pressure close to 10. -5 Torr (that is, about 10) -3 The pressure is approximately 10 Pa. However, some high vacuum systems may experience pressures close to 10 Pa. -7 Torr (that is, about 10) -5 The following operation is performed (Pa). In some embodiments, the vacuum is created using a rough pump and / or turbomolecular pump coupled to each of the delivery chamber 108 and one or more processing chambers (e.g., processing chambers 109-140). However, other types of vacuum pumps are also considered.
[0025] A system controller 126, such as a programmable computer, is coupled to the processing system 100 for controlling one or more of its components. For example, the system controller 126 may control the operation of one or more processing chambers, such as processing chambers 132, 134, 136, 138, and 140. In operation, the system controller 126 enables data acquisition and feedback from the respective components to coordinate processing within the processing system 100.
[0026] System controller 126 includes a programmable central processing unit (CPU) 126A, which can operate together with memory 126B (e.g., non-volatile memory) and support circuitry 126C. Support circuitry 126C (e.g., cache, clock circuitry, input / output subsystem, power supply, etc., and combinations thereof) is conventionally coupled to CPU 126A and to various components within processing system 100.
[0027] In some implementations, CPU 126A is any form of general-purpose computer processor used in an industrial setting, such as a programmable logic controller (PLC), for controlling various monitoring system components and subprocessors. Memory 126B coupled to CPU 126A is non-transient and is typically one or more readily available memory types, such as random access memory (RAM), read-only memory (ROM), disk drives, hard disks, or any other form of digital storage, whether local or remote.
[0028] Here, memory 126B exists in the form of a computer-readable storage medium containing instructions (e.g., non-volatile memory) that, when executed by CPU 126A, facilitate the operation of processing system 100. The instructions in memory 126B exist in the form of a program product, such as a program implementing the methods of this disclosure (e.g., middleware application, device software application, etc.). The program code may conform to any of a variety of different programming languages. In one instance, this disclosure may be implemented as a program product stored on a computer-readable storage medium used with a computer system. The program of the program product defines the functionality of the implementation (including the methods described herein). Exemplary computer-readable storage media include, but are not limited to: (i) non-writable storage media (e.g., read-only memory elements within a computer, such as CD-ROM discs readable by a CD-ROM drive, flash memory, ROM chips, or any type of solid-state non-volatile semiconductor memory) on which information is permanently stored; and (ii) writable storage media (e.g., a disk located within a floppy disk drive or hard disk drive, or any type of solid-state random access semiconductor memory) on which variable information is stored. Such computer-readable storage media, when carrying computer-readable instructions to guide the functions described herein, constitute embodiments of this disclosure. The various methods disclosed herein are typically implemented, for example, as a software routine by CPU 126A executing computer instruction codes stored in memory 126B (or memory of a specific processing chamber) under the control of CPU 126A. When the computer instruction codes are executed by CPU 126A, CPU 126A controls the chamber to perform the process according to the various methods.
[0029] Examples of semiconductor devices
[0030] Figure 4A simplified cross-sectional view of a portion of a semiconductor device structure according to one or more embodiments described herein is illustrated. More specifically, the semiconductor device structure shown is a CFET 400. Compared to current transistor architectures, which are primarily planar or quasi-planar, the CFET employs a vertically stacked layout, including an insulator 402, a bottom device structure 304B (e.g., a bottom FET) disposed above the insulator 402, a top device structure 304A (e.g., a top FET) disposed above the bottom device structure 304B, and a common gate 404 disposed through the bottom device structure 304B and the top device structure 304A. In this embodiment, the bottom device structure 304B is a PMOS device, including source / drain regions 406 formed by several layers of p-type material 352. The top device structure 304A is an NMOS device, including source / drain regions 408 formed by several layers of n-type material 338. In other embodiments, the top device structure 304A may be a PMOS device, while the bottom device structure 304B may be an NMOS device.
[0031] Processing sequence instances
[0032] Based on processing system 100 and Figure 1 , Figure 4 and Figures 3A to 3C Based on the information provided in section C, embodiments of this disclosure include a method 200 for forming a CFET semiconductor device. A process flow diagram of method 200 is shown below. Figures 2A to 2C As shown. Although method 200 is described using a portion of a CFET as an example, method 200 is not limited to a specific transistor type or construction. Furthermore, Figures 3A to 3C C only shows a portion of the component substrate 300. In practice, additional layers and structures may be placed on it. Figures 3A to 3C C refers to the layer above, below, or inside the layer.
[0033] In operation 202 of method 200, the component substrate 300 is transferred to the processing chamber. Figure 3A A cross-sectional view of a portion of a component substrate 300 is shown. The component substrate 300 includes a first substrate layer 302, a bottom component structure 304B disposed above the first substrate layer 302, and a top component structure 304A disposed above the bottom component structure 304B. The first substrate layer 302 is a temporary substrate because it will be removed in a subsequent manufacturing sequence.
[0034] The component substrate 300 includes a first substrate layer 302. As used herein, the term "substrate" refers to a layer of material that serves as the basis for subsequent processing operations and includes the surface to be cleaned. The first substrate layer 302 may be a silicon-based material, or any suitable insulating or conductive material as required. The first substrate layer 302 may contain, but is not limited to, crystalline silicon (e.g., Si). <100> or Si <111> Materials including: silicon oxide, strained silicon, silicon germanium, doped or undoped polycrystalline silicon, doped or undoped silicon wafers and patterned or unpatterned wafers, silicon on insulator (SOI), carbon-doped silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass or sapphire.
[0035] The component substrate 300 includes a dual bottom component structure 304B disposed above a first substrate layer 302, and a top component structure 304A disposed above the bottom component structure 304B. Both the top component structure 304A and the bottom component structure 304B include a sacrificial superlattice layer 306, on which a superlattice is disposed. The top superlattice 305A of the top component structure 304A and the superlattice 305B of the bottom component structure 304B each include alternating layers of channel layers 308 and sacrificial layers 310, stacked in the Z direction and disposed above their respective sacrificial superlattice layers 306. The top superlattice 305A of the top component structure 304A and the superlattice 305B of the bottom component structure 304B may each have approximately 2 to approximately 10 pairs of channel layers 308 and sacrificial layers 310. The top superlattice 305A of the top element structure 304A and the superlattice 305B of the bottom element structure 304B may each optionally have more than 10 pairs of channel layers 308 and sacrificial layers 310.
[0036] The channel layer 308 may be formed of a first material. The sacrificial layer 310 may be formed of a second material. The sacrificial superlattice layer 306 may be formed of a third material. The sacrificial superlattice layer 306 may be formed of a single layer of material, or alternatively, of a multilayer material. The etch selectivity of the second material (i.e., the ratio of the etch rate of the second material to the etch rate of the first material) is between about 10:1 and about 500:1. Examples of the first material include, but are not limited to, pure silicon (Si), germanium (Ge), and silicon-germanium (SiGe). Examples of the second material include, but are not limited to, SiGe having a Ge concentration of about 10% to about 30%. The third material may be formed of a material whose etch selectivity to the first and second materials is between about 10:1 and about 200:1. Examples of the third material include, but are not limited to, SiGe with a higher Ge concentration, between about 35% and about 60%.
[0037] Each channel layer 308 has a thickness between about 5 nm and about 40 nm. Each sacrificial layer 310 has a thickness between about 5 nm and about 40 nm. The superlattice sacrificial layer 306 may have a thickness between about 20 nm and about 100 nm.
[0038] The sacrificial superlattice layer 306, channel layer 308, and sacrificial layer 310 of the bottom element structure 304B and the top element structure 304A can be formed by any suitable deposition process, including but not limited to PVD, CVD, and ALD. For example, they can be formed by epitaxy. Epitaxial formation of the sacrificial superlattice layer 306 of the bottom element structure 304B, and the alternating pattern of the channel layer 308 and the sacrificial layer 310, typically involves positioning the element substrate 300 on a substrate support within a processing volume of a processing chamber, heating the first substrate layer 302 to a target temperature, and introducing one or more precursor gases into the processing volume. The choice of precursor gas depends on the specific materials and processes involved. In one embodiment, the precursor gas may comprise silane (SiH4) and germanane (GeH4). Upon heating, the precursor gas decomposes and first deposits onto the substrate surface via nucleation, followed by lattice structure growth. By controlling the growth conditions, including temperature, pressure, and precursor gas composition, the characteristics of the resulting epitaxial layer can be controlled.
[0039] The top element structure 304A includes a sacrificial superlattice layer 306 formed over the bottom element structure 304B. The top element structure 304A includes an alternating layer pattern comprising a channel layer 308 and a sacrificial layer 310 formed over the sacrificial superlattice layer 306 of the top element structure 304A. The top element structure 304A can be formed by any suitable process as described above.
[0040] In operation 204 of method 200, the top element structure 304A and the bottom element structure 304B are etched to form a shallow trench isolation (STI) feature 312. Figure 3B The element substrate 300 after operation 204 of method 200 is depicted. In operation 204 of method 200, etching the element substrate 300 includes first forming and patterning a resist layer over the top element structure 304A.
[0041] The formation of the resist layer can be performed using any suitable lithographic printing process. For example, the resist layer can be formed using optical lithography, extreme ultraviolet (EUV) lithography, X-ray lithography, electron beam lithography, nanoimprint lithography, step-and-flash lithography, maskless lithography, or similar processes. The area of the component substrate 300 covered by the developed resist layer will be protected from subsequent etching operations.
[0042] As the resist layer is formed and patterned, the component substrate 300 undergoes an etching process. In one embodiment, the etching process is a reactive ion etching (RIE) process. During the RIE process, the processing chamber operates under vacuum pressure. This vacuum pressure is between about 2 Torr and about 10⁻⁶ Torr. A non-reactive gas (e.g., argon) and an etching gas (e.g., a reactive gas typically containing chlorine (Cl) or fluorine (F)) are introduced into the processing chamber. An electromagnetic field ionizes these gases, creating a plasma composed of ions, electrons, and neutral particles. Positively charged ions are accelerated toward the substrate and collide with the surface of the component substrate 300, thereby physically sputtering material from the component substrate 300. Simultaneously, reactive gas molecules chemically react with the exposed material, forming removed byproducts. Both sputtering and chemical reactions enable the precise removal of material not protected by the resist layer. In other embodiments, different dry etching processes, wet etching processes, or combinations of processes may be used.
[0043] Following the etching process, the remaining resist layer is removed. Removal of the remaining resist layer can be achieved using either a dry stripping process or a wet stripping process. A dry stripping process may involve etching the resist layer. A plasma of reactive gases is used to react with and remove the resist layer. High-energy ions and free radicals in the plasma decompose the resist material into pumped-out volatile byproducts. Dry stripping processes can be highly selective, removing only the resist layer, or less selective to additionally remove the underlying layer. Wet stripping processes may involve the use of chemical solvents or combinations of solvents, depending on the type of resist material used. Examples of solvents include, but are not limited to, acetone, N-methyl-2-pyrrolidone (NMP), γ-butyrolactone (GBL), and other suitable solvents.
[0044] STI feature 312 can be formed by any suitable process. STI feature 312 can be formed before or after the etching process described above. STI feature 312 reduces interference by decreasing parasitic capacitance and crosstalk between adjacent transistors. This allows for higher placement density and improved performance. STI feature 312 is formed from any suitable dielectric material. For example, STI feature 312 may include, but is not limited to, silicon dioxide, silicon nitride, silicon oxynitride, high dielectric constant materials, polycrystalline silicon, spin-coated glass, borosilicate glass, or combinations thereof.
[0045] When operation 204 ends, as follows Figure 3B As shown, the remaining structures are the first structure 314A and the second structure 314B, each containing a top element structure 304A and a bottom element structure 304B, separated by the STI feature 312.
[0046] In operation 206 of method 200, a first oxide layer 316 and a bottom dummy gate layer 318 are formed. Figure 3C The image depicts a component substrate 300 after operation 206 of method 200. A first oxide layer 316 is disposed over STI feature 312, over first structure 314A and second structure 314B, and over the sidewall surfaces of first structure 314A and second structure 314B. The first oxide layer 316 serves as a sacrifice or "dummy" oxide layer for subsequent operations. The first oxide layer 316 can be formed from any suitable dielectric material. For example, the first oxide layer 316 can comprise, but is not limited to, silicon dioxide, silicon nitride, silicon oxynitride, high dielectric constant materials, polysilicon, spin-coated glass, borosilicate glass, or combinations thereof. The first oxide layer 316 can be formed by any suitable deposition process, including, but not limited to, physical vapor deposition (PVD), chemical vapor deposition (CVD), atomic layer deposition (ALD), or any combination thereof. The deposition process may include intermediate steps such as cleaning, degassing, lithography, etching, chemical mechanical polishing (CMP), or other processes common in semiconductor device manufacturing.
[0047] The device substrate 300 includes a bottom dummy gate layer 318 disposed over a first oxide layer 316. The bottom dummy gate layer 318 extends from the first oxide layer 316 disposed over the STI feature 312 to approximately between the top device structure 304A and the bottom device structure 304B on both the first structure 314A and the second structure 314B. The bottom dummy gate layer 318 may comprise, but is not limited to, polysilicon. The bottom dummy gate layer 318 may be formed by any suitable deposition process, including, but not limited to, PVD, CVD, ALD, or combinations thereof. The deposition process may include intermediate steps such as cleaning, degassing, lithography, etching, CMP, or other processes common in semiconductor device manufacturing.
[0048] like Figure 3D As shown, in operation 208 of method 200, a silicon nitride layer 320 is disposed on the exposed portion of the device substrate 300. The silicon nitride layer 320 may comprise, but is not limited to, silicon nitride (Si3N4). The silicon nitride layer 320 may be formed by any suitable deposition process, including, but not limited to, PVD, CVD, ALD, or combinations thereof. The deposition process may include intermediate steps such as cleaning, degassing, lithography, etching, CMP, or other processes common in semiconductor device manufacturing.
[0049] like Figure 3EAs shown, in operation 210 of method 200, a top dummy gate layer 322 and a hard mold layer 324 are formed. The device substrate 300 includes the top dummy gate layer 322 disposed over the silicon nitride layer 320. The top dummy gate layer 322 extends from the silicon nitride layer 320 to or beyond the silicon nitride layer disposed over the top device structure 304A disposed on both the first structure 314A and the second structure 314B. The top dummy gate layer 322 may comprise, but is not limited to, polysilicon. The top dummy gate layer 322 may be formed by any suitable deposition process, including, but not limited to, PVD, CVD, ALD, or combinations thereof. The deposition process may include intermediate steps such as cleaning, degassing, lithography, etching, CMP, or other processes common in semiconductor device manufacturing.
[0050] The device substrate 300 includes a hard stencil layer 324 disposed above the top dummy gate layer 322. The hard stencil layer 324 can be formed by any suitable deposition process, such as PVD, CVD, ALD, or combinations thereof. Once deposition is complete, the hard stencil layer 324 is patterned to form a “dummy gate hard stencil” or “dummy gate hard stencil feature.” For example, the hard stencil layer 324 can be patterned using optical lithography, extreme ultraviolet (EUV) lithography, X-ray lithography, electron beam lithography, nanoimprint lithography, step and flash lithography, maskless lithography, or similar processes. The area of the device substrate 300 covered by the patterned hard stencil layer 324 is protected from subsequent etching operations. The process of forming the patterned hard stencil layer 324 may include intermediate steps such as cleaning, degassing, lithography, etching, CMP, or other processes common in semiconductor device manufacturing.
[0051] In operation 212 of method 200, the component substrate 300 is subjected to an etching process to remove portions of the component substrate 300 that are not protected by the patterned hard mold layer 324. In this embodiment, the removed portions of the component substrate 300 include portions of the top dummy gate layer 322, the silicon nitride layer 320, and the bottom dummy gate layer 318, thereby terminating at the first oxide layer 316.
[0052] The removal of portions of the top dummy gate layer 322, silicon nitride layer 320, and bottom dummy gate layer 318 can be accomplished by a dry etching process, a wet etching process, or a CMP process. A dry etching process may involve plasma etching of the component substrate 300. During a dry etching process, a plasma of reactive gas is used to react with and remove portions of the top dummy gate layer 322, silicon nitride layer 320, and bottom dummy gate layer 318. The reactive gas used in a dry etching process typically contains fluorine-based compounds. High-energy ions and free radicals in the plasma decompose the top dummy gate layer 322, silicon nitride layer 320, and bottom dummy gate layer 318 into pumped-out volatile byproducts. Dry etching processes can be highly selective, removing only a small portion of the top dummy gate layer 322, silicon nitride layer 320, and bottom dummy gate layer 318, or less selective to remove additional material. Dry etching processes can include reactive ion etching (RIE), inductively coupled plasma (ICP), capacitively coupled plasma (CCP), or other suitable dry etching processes. Figure 3F The component substrate 300 is depicted after operation 212 of method 200. The etching process of operation 212 of method 200 leaves vertical structures 326, which are separated by trenches with high aspect ratios, extending perpendicular to the first structure 314A and the second structure 314B.
[0053] In operation 214 of method 200, the component substrate 300 is exposed to an etching process to remove the exposed first oxide layer 316 disposed between the vertical structures 326, followed by the formation of a spacer layer 328. The etching of the first oxide layer 316 of the component substrate 300 can be performed using either a dry etching process or a wet etching process. A dry etching process may involve plasma etching of the component substrate 300. During the dry etching process, a plasma using a reactive gas reacts with and removes the first oxide layer 316 above the STI feature 312, the first structure 314A, the second structure 314B, and the exposed portions on the sides of the first structure 314A and the second structure 314B. The reactive gas used in the dry etching process typically contains a fluorine-based compound. High-energy ions and free radicals in the plasma decompose the first oxide layer 316 into pumped-out volatile byproducts. The dry etching process can be highly selective, removing only a small portion of the first oxide layer 316, or less selective to remove additional portions. Dry etching processes may include reactive ion etching (RIE), inductively coupled plasma (ICP), capacitively coupled plasma (CCP), or other suitable dry etching processes.
[0054] Following the etching process, operation 214 of method 200 includes depositing a conformal spacer layer 328 on the exposed side of the vertical structure 326. The spacer layer can be formed of any suitable material, including but not limited to silicon dioxide (SiO2), silicon nitride (Si3N4), organosilicon glass (OSG), fluorinated silicate glass (FSG), Black Diamond®, organic dielectrics, low-dielectric-constant dielectrics, or combinations thereof. The deposition of the spacer layer 328 can be performed by any suitable deposition process, including but not limited to PVD, CVD, ALD, or combinations thereof. The deposition process may include intermediate steps such as cleaning, degassing, lithography, etching, CMP, or other processes common in semiconductor device fabrication. After depositing the conformal spacer layer 328, high-energy RIE etching is performed to form the spacer structure, such as... Figure 3G The description.
[0055] In operation 216 of method 200, the source-drain regions (i.e., channel layer 308) of the top element structure 304A and the bottom element structure 304B are recessed. The recess is formed by a superlattice material stack consisting of channel layer 308, layer 306, and layer 310, as shown in the figure. Figure 3A The 304A and 304B described in the text form a structure like Figure 3H The depicted source-drain trench. By recessing the source-drain region, transistor performance can be improved, particularly in controlling charge carrier flow. The performance improvement may be due to reduced short-channel effects and lower parasitic capacitance. The source-drain region of the recessed device substrate 300 involves modifying the configuration of the channel layer 308 by selectively removing a portion of the first material in the channel layer 308. The process for creating the source-drain trench involves selectively etching a portion of the channel layer 308 using any suitable dry etching process, wet etching process, or any combination thereof as described above. Figure 3H The component substrate 300 is depicted after operation 216 is performed in method 200.
[0056] In operation 218 of method 200, the component substrate 300 is exposed to an etching process to remove the sacrificial superlattice layer 306. Etching of the sacrificial superlattice layer 306 of the component substrate 300 can be performed by a dry etching process, a wet etching process, or a combination of processes. A dry etching process may involve plasma etching of the component substrate 300. During a dry etching process, a plasma using a reactive gas reacts with and removes the SiGe layer 306 from the top component structure 304A and the bottom component structure 304B. The reactive gas used in a dry etching process typically contains a fluorine-based compound. High-energy ions and radicals in the plasma decompose the sacrificial superlattice layer 306 into pumped-away volatile byproducts. The dry etching process can be highly selective, removing only a small portion of the sacrificial superlattice layer 306, or less selective to remove an additional portion. Dry etching processes may include reactive ion etching (RIE), inductively coupled plasma (ICP), capacitively coupled plasma (CCP), or other suitable dry etching processes. A wet etching process may involve cleaning the component substrate 300, masking portions of the component substrate 300, immersing it in an etchant, and cleaning and removing the mask. Examples of etchants used in a wet etching process include, but are not limited to, potassium hydroxide (KOH), tetramethylaminohydroxide (TMAH), hydrofluoric acid (HF), buffered oxide etchants such as a mixture of ammonium fluoride (NH4F) and HF, phosphoric acid (H3PO4), nitric acid (HNO3), acetic acid (CH3COOH), hydrochloric acid (HCl), ammonium persulfate (NH4S2O8), ferric chloride (FeCl3), copper chloride (CuCl2), acetone, hydrogen peroxide (H2O2), deionized water, or any combination thereof. The specific etchant used in a wet etching process will depend on the material to be etched. When the material is exposed to the etchant, it dissolves in the solution and is subsequently removed, leaving the etched pattern. Figure 3I The component substrate 300 is depicted after operation 216 of method 200.
[0057] In operation 220 of method 200, such as Figure 3J The depicted configuration includes forming an isolation structure 330 within the pores left by removing the sacrificial superlattice layer 306 in operation 218. The isolation structure 330 can be formed from any suitable dielectric material, including but not limited to silicon dioxide, silicon nitride, silicon oxynitride, high dielectric constant materials, polycrystalline silicon, spin-coated glass, borosilicate glass, or combinations thereof. The deposition of the isolation structure 330 can be performed by any suitable deposition process, including but not limited to PVD, CVD, ALD, or combinations thereof. The deposition process may include intermediate steps such as cleaning, degassing, lithography, etching, CMP, or other processes common in semiconductor device fabrication. Figure 3J The component substrate 300 is depicted after operation 224 of method 200.
[0058] In operation 222 of method 200, the component substrate 300 is exposed to an etching process to remove the sacrificial layer 310. Etching of the sacrificial layer 310 of the component substrate 300 can be performed using either a dry etching process or a wet etching process. A dry etching process may involve plasma etching of the component substrate 300. During the dry etching process, a plasma using a reactive gas reacts with and removes the sacrificial layer 310 from the top component structure 304A and the bottom component structure 304B. The reactive gas used in the dry etching process typically contains a fluorine-based compound. High-energy ions and radicals in the plasma decompose the sacrificial layer 310 into pumped-out volatile byproducts. The dry etching process can be highly selective, removing only a small portion of the sacrificial layer 310, or less selective to remove additional components. Dry etching processes may include reactive ion etching (RIE), inductively coupled plasma (ICP), capacitively coupled plasma (CCP), or other suitable dry etching processes. A wet etching process may involve cleaning the component substrate 300, masking portions of the component substrate 300, immersing it in an etchant, cleaning, and removing the mask. Examples of etchants used in a wet etching process may include, but are not limited to, potassium hydroxide (KOH), tetramethylaminohydroxide (TMAH), hydrofluoric acid (HF), buffered oxide etchants such as a mixture of ammonium fluoride (NH4F) and HF, phosphoric acid (H3PO4), nitric acid (HNO3), acetic acid (CH3COOH), hydrochloric acid (HCl), ammonium persulfate (NH4S2O8), ferric chloride (FeCl3), copper chloride (CuCl2), acetone, hydrogen peroxide (H2O2), deionized water, or any combination thereof. The specific etchant used in a wet etching process will depend on the material to be etched. When the material is exposed to the etchant, it dissolves in the solution and is then removed, leaving the etched pattern. Figure 3K The image depicts the component substrate 300 after operation 222 of method 200.
[0059] In operation 224 of method 200, such as Figure 3LThe illustration shows the formation of a second oxide layer 332 in the pores left by removing the sacrificial layer 310 in operation 222. The second oxide layer 332 serves as a sacrificial layer or a "dummy" oxide layer for subsequent operations. The second oxide layer 332 can be formed from any suitable dielectric material. For example, the second oxide layer 332 can comprise, but is not limited to, silicon dioxide, silicon nitride, silicon oxynitride, high dielectric constant materials, polycrystalline silicon, spin-coated glass, borosilicate glass, or combinations thereof. The second oxide layer 332 can be formed by any suitable deposition process, including but not limited to physical vapor deposition (PVD), chemical vapor deposition (CVD), atomic layer deposition (ALD), or any combination thereof. The deposition process may include intermediate steps such as cleaning, degassing, lithography, etching, chemical mechanical polishing (CMP), or other processes common in semiconductor device manufacturing.
[0060] In operation 226 of method 200, internal spacers 334 are formed. Forming internal spacers 334 includes other processes such as etching and deposition. The etching process includes removing a portion of the second oxide layer 332. Etching a portion of the second oxide layer 332 can be performed using a dry etching process or a wet etching process. The dry etching process may involve plasma etching of the component substrate 300. During the dry etching process, a plasma using a reactive gas reacts with and removes a portion of the second oxide layer 332. The reactive gas used in the dry etching process typically contains fluorine-based compounds. High-energy ions and free radicals in the plasma decompose a portion of the second oxide layer 332 into pumped-out volatile byproducts. The dry etching process can be highly selective, removing only a small portion of the second oxide layer 332, or less selective to remove an additional portion. The dry etching process may include reactive ion etching (RIE), inductively coupled plasma (ICP), capacitively coupled plasma (CCP), or other suitable dry etching processes. A wet etching process may involve cleaning the component substrate 300, masking portions of the component substrate 300, immersing it in an etchant, cleaning and removing the mask. Examples of etchants used in a wet etching process may include, but are not limited to, potassium hydroxide (KOH), tetramethylaminohydroxide (TMAH), hydrofluoric acid (HF), buffered oxide etchants such as a mixture of ammonium fluoride (NH4F) and HF, phosphoric acid (H3PO4), nitric acid (HNO3), acetic acid (CH3COOH), hydrochloric acid (HCl), ammonium persulfate (NH4S2O8), ferric chloride (FeCl3), copper chloride (CuCl2), acetone, hydrogen peroxide (H2O2), deionized water, or any combination thereof. The specific etchant used in a wet etching process will depend on the material to be etched. When the material is exposed to the etchant, it dissolves and becomes part of the solution, and is then removed, leaving the etched pattern.
[0061] After a portion of the second oxide layer 332 is removed, an internal spacer 334 is disposed within the pores left by the removal of the portion of the second oxide layer 332. The internal spacer 334 can be formed by any suitable deposition process, including but not limited to physical vapor deposition (PVD), chemical vapor deposition (CVD), atomic layer deposition (ALD), or any combination thereof. The deposition process may include intermediate steps such as cleaning, degassing, lithography, etching, chemical mechanical polishing (CMP), or other processes common in semiconductor device manufacturing. Figure 3M The component substrate 300 is depicted after operation 226 of method 200.
[0062] In operation 228 of method 200, a first dielectric fill layer 336 is disposed between vertical structures 326 in high aspect ratio trenches extending perpendicularly to the first structure 314A and the second structure 314B, thereby covering the bottom element structure 304B. The first dielectric fill layer 336 can be formed from any suitable dielectric material. For example, the first dielectric fill layer 336 can comprise, but is not limited to, silicon dioxide, silicon nitride, silicon oxynitride, high dielectric materials, polysilicon, spin-coated glass, borosilicate glass, or combinations thereof. The first dielectric fill layer 336 can be formed from any suitable deposition process, including, but not limited to, physical vapor deposition (PVD), chemical vapor deposition (CVD), atomic layer deposition (ALD), or any combination thereof. The deposition process may include intermediate steps such as cleaning, degassing, lithography, etching, chemical mechanical polishing (CMP), or other processes common in semiconductor device manufacturing. Figure 3N The component substrate 300 is depicted after operation 228 of method 200.
[0063] In operation 230 of method 200, an n-type material 338 is formed on the top element structure 304A. This n-type material 338 is formed by an epitaxial process. Epitaxy typically involves positioning the element substrate 300 on a substrate support within a processing volume of a processing chamber, heating the element substrate 300 to a target temperature, and introducing one or more precursor gases into the processing volume. The choice of precursor gas depends on the specific materials and processes involved. In one embodiment, the precursor gas may include, but is not limited to, silane (SiH4), bissilane (Si2H6), and tetrasilane (Si4H6). 10 Germanane (GeH4), bisgermanane (Ge2H6), germanium tetrachloride (GeCl4), trimethylgallium (Ga(CH3)3), phosphine (PH3), phosphorus trichloride (PCl3), triisobutylphosphine ([(CH3)3C]3P), arsenic trichloride (AsCl3), tert-butylarsenic (AsC4H) 11 The precursor gas can be antimony trichloride (SbCl3), or Sb(C2H5)5, arsine (AsH3), diborane (B2H6), trimethylphosphorus (TMP), or any dopant or precursor commonly used in semiconductor device fabrication. When heated, the precursor gas decomposes and first deposits onto the substrate surface via nucleation, followed by lattice structure growth. The characteristics of the resulting epitaxial layer can be controlled by regulating the growth conditions, including temperature, pressure, and precursor gas composition. In some embodiments with p-type elements on top, a p-type semiconductor can be formed at the location of the n-type material 338, instead of an n-type semiconductor. Figure 3O The component substrate 300 is depicted after operation 230 of method 200.
[0064] In operation 232 of method 200, a first contact etch-stop liner (CESL) 340 is formed, and a second dielectric fill layer 342 is disposed. After the deposition of the second dielectric fill layer 342, a chemical mechanical polishing process is performed to remove excess deposited material, planarize the surface, and expose the dummy gate material of the vertical structure 326. Figure 3P The device substrate 300 is depicted after operation 232 of method 200. A first CESL 340 is disposed on the exposed surface of the device substrate 300, including the side surface of the vertical structure 326, the top surface of the first dielectric filling layer 336, the exposed surface of the first oxide layer 316, and the outer surface of the n-type material 338. The first CESL 340 is a thin layer of material designed to serve as a termination layer during subsequent etching processes. The first CESL 340 can be formed from any suitable material, including but not limited to silicon nitride, silicon-rich silicon nitride, or any combination thereof. The formation of the first CESL 340 can be performed by any suitable deposition process, including but not limited to CVD, PVD, ALD, or any combination thereof. The deposition process may include intermediate steps such as cleaning, degassing, lithography, etching, CMP, or other processes common in semiconductor device manufacturing.
[0065] Following the first CESL 340, a second dielectric fill layer 342 is disposed on the device substrate 300, filling the remaining area between the vertical structures 326, thereby covering the n-type material 338 of the top device structure 304A. The second dielectric fill layer 342 can be formed of any suitable dielectric material. For example, the second dielectric fill layer 342 may comprise, but is not limited to, silicon dioxide, silicon nitride, silicon oxynitride, high dielectric constant materials, polysilicon, spin-coated glass, borosilicate glass, or combinations thereof. The second dielectric fill layer 342 can be formed by any suitable deposition process, including but not limited to PVD, CVD, ALD, or combinations thereof. The deposition process may include intermediate steps such as cleaning, degassing, lithography, etching, CMP, or other processes common in semiconductor device manufacturing. Figure 3P The component substrate 300 is depicted after operation 232 of method 200.
[0066] In operation 234 of method 200, the dummy gate material of the vertical structure 326 and the second oxide layer 332 are removed and replaced with a replacement metal gate (RMG) 344. The process of forming the RMG 344 in operation 234 typically involves depositing a channel dielectric material, which is typically a chemical oxide selectively deposited on a silicon channel, and a conformal high-dielectric-constant dielectric material, such as HfO2. Following these processes, processes for RMG metal pads and metal filling are performed. At the end of operation 234, a metal chemical mechanical polishing process is performed to remove excess deposited material, thereby forming a separate metal gate. Furthermore, prior to the dielectric layer deposition step, the high-dielectric-constant dielectric material is doped with an appropriate dipole material (typically Al for p-type and La for n-type). RMG 344 can contain any suitable conductive material, including but not limited to cobalt (Co), tungsten (W), platinum (Ru), copper (Cu), molybdenum (Mo), titanium (Ti), nickel (Ni), silver (Ag), gold (Au), bismuth (Ir), tantalum (Ta), platinum (Pt), their conductive oxides or nitrides, or any combination thereof. RMG 344 can be separated from other structures / regions of the component substrate 300 by one or more insulating layers. In some embodiments, RMG 344 can contain multiple layers of the same or different conductive materials. Forming RMG 344 includes several sub-processes, such as selectively etching the second oxide layer 332 and depositing RMG 344.
[0067] Selectively etching the second oxide layer 332 of the element substrate 300 can be accomplished by a dry etching process, a wet etching process, or a combination of these processes. This selective etching process provides selective removal of the dummy gate (polysilicon). A dry etching process may involve plasma etching of the element substrate 300. During the dry etching process, a plasma using a reactive gas reacts with the second oxide layer 332 from the top element structure 304A and removes the top element structure. The reactive gas used in the dry etching process typically contains fluorine-based compounds. High-energy ions and radicals in the plasma decompose the second oxide layer 332 into pumped-out volatile byproducts. In one embodiment, the dry etching process may be highly selective, removing only a small portion of the second oxide layer 332. In other embodiments, the dry etching process may be less selective to remove additional material. The dry etching process may include reactive ion etching (RIE), inductively coupled plasma (ICP), capacitively coupled plasma (CCP), or other suitable dry etching processes. A wet etching process may involve cleaning the component substrate 300, masking portions of the component substrate 300, immersing it in an etchant, and cleaning and removing the mask. Examples of etchants used in a wet etching process may include, but are not limited to, potassium hydroxide (KOH), tetramethylaminobutanol (TMAH), hydrogen fluoride (HF), buffered oxide etchants such as a mixture of ammonium fluoride (NH4F) and HF, phosphoric acid (H3PO4), nitric acid (HNO3), acetic acid (CH3COOH), hydrochloric acid (HCl), ammonium persulfate (NH4S2O8), ferric chloride (FeCl3), copper chloride (CuCl2), acetone, hydrogen peroxide (H2O2), deionized water, or any combination thereof. The specific etchant used in a wet etching process will depend on the material to be etched. When the second oxide layer 332 is exposed to the etchant, the layer is dissolved and becomes part of the soluble solution, and then removed, leaving the etched pattern.
[0068] RMG 344 can be formed by any suitable deposition process, including but not limited to CVD, PVD, ALD, or any combination thereof. The process for depositing RMG 344 may include intermediate steps such as cleaning, degassing, lithography, etching, CMP, or other processes common in semiconductor device manufacturing. Figure 3Q The component substrate 300 is depicted after operation 234 of method 200.
[0069] In operation 236 of method 200, a second substrate layer 350 (e.g., a carrier substrate) is bonded to the top surface of the component substrate 300, and then the component substrate 300 is inverted such that the first substrate layer 302 becomes the uppermost portion of the component substrate. The second substrate layer 350 is also a temporary substrate because it will be removed later in the manufacturing sequence. The second substrate layer 350 can be bonded to the component substrate 300 by any suitable method and process, including but not limited to adhesive bonding, thermoforming bonding, anodic bonding, direct bonding (e.g., cold / contact soldering), wafer / fusion bonding, solder bonding, plasma-activated bonding, or any combination thereof. Figure 3R The component substrate 300 is depicted after operation 236 of method 200.
[0070] In operation 238 of method 200, portions of the first substrate layer 302 and STI feature 312 are removed down to the isolation structure 330 of the bottom component structure 304B, thereby exposing portions of the bottom component structure 304B. Removal of portions of the first substrate layer 302 and STI feature 312 can be performed by any suitable dry etching process, wet etching process, CMP, ion milling, or any combination thereof, as described above. Figure 3S The component substrate 300 is depicted after operation 238 of method 200.
[0071] In operation 240 of method 200, a first dielectric fill layer 336 is removed between vertical structures 326 disposed in high aspect ratio trenches extending perpendicular to the second structure 314B. The removal of the first dielectric fill layer 336 is selective for the isolation structure 330. After removing the first dielectric fill layer 336, an oriented dielectric material 337 is deposited, preferably on top of the vertical structures 326 and at the bottom of the space formed by removing the first dielectric fill layer 336. This protects the dummy gate vertical features during subsequent epitaxial deposition processes. The removal of the first dielectric fill layer 336 can be accomplished by any suitable dry etching process, wet etching process, CMP, or any combination thereof as described above. Figure 3T The component substrate 300 is depicted after operation 240 of method 200.
[0072] In operation 242 of method 200, a p-type material 352 is formed on the bottom element structure 304B. This p-type material 352 is formed by an epitaxial process. Epitaxy typically involves positioning the element substrate 300 on a substrate support within the processing volume of a processing chamber, heating the element substrate 300 to a target temperature, and introducing one or more precursor gases into the processing chamber. The choice of precursor gas depends on the specific materials and processes involved. In one embodiment, the precursor gas may include, but is not limited to, silane (SiH4), bissilane (Si2H6), and tetrasilane (Si4H6).10 Germanane (GeH4), bisgermanane (Ge2H6), germanium tetrachloride (GeCl4), trimethylgallium (Ga(CH3)3), phosphine (PH3), phosphorus trichloride (PCl3), triisobutylphosphine ([(CH3)3C]3P), arsenic trichloride (AsCl3), tert-butylarsenic (AsC4H) 11 The precursor gas can be antimony trichloride (SbCl3) or Sb(C2H5)5, arsine (AsH3), diborane (B2H6), trimethylphosphorus (TMP), or any other dopant or precursor commonly used in semiconductor device fabrication. When heated, the precursor gas decomposes and first deposits onto the substrate surface via nucleation, followed by lattice structure growth. The characteristics of the resulting epitaxial layer can be controlled by adjusting the growth conditions, including temperature, pressure, and precursor gas composition. In some embodiments with p-type elements on top, an n-type semiconductor, instead of a p-type semiconductor, can be formed at the location of the p-type material 352. Figure 3U The component substrate 300 is depicted after operation 242 is completed.
[0073] In operation 244 of method 200, a second contact etch stop pad (CESL) 354 is formed and a third dielectric fill layer 356 is disposed. Figure 3V The device substrate 300 is depicted after operation 244 of method 200. A second CESL 354 is disposed on the exposed surface of the device substrate 300, including the side surface of the vertical structure 326, the top surface of the first dielectric filling layer 336, the exposed surface of the silicon nitride layer 320, and the outer surface of the p-type material 352. The second CESL 354 is a thin layer of material designed to serve as a termination layer during subsequent etching processes. The second CESL 354 can be made of any suitable material, including but not limited to silicon nitride, silicon-rich silicon nitride, or any combination thereof. The formation of the second CESL 354 can be performed by any suitable deposition process, including but not limited to CVD, PVD, ALD, or any combination thereof. The deposition process may include intermediate steps such as cleaning, degassing, lithography, etching, CMP, or other processes common in semiconductor device fabrication.
[0074] Following the second CESL 354, a third dielectric fill layer 356 is disposed on the device substrate 300, filling the remaining area between the vertical structures 326, thereby covering the p-type material 352 of the bottom device structure 304B. The third dielectric fill layer 356 can be formed of any suitable dielectric material. For example, the third dielectric fill layer 356 may comprise, but is not limited to, silicon dioxide, silicon nitride, silicon oxynitride, high dielectric constant materials, polysilicon, spin-coated glass, borosilicate glass, or combinations thereof. The third dielectric fill layer 356 can be formed by any suitable deposition process, including but not limited to PVD, CVD, ALD, or any combination thereof. The deposition process may include intermediate steps such as cleaning, degassing, lithography, etching, CMP, or other processes common in semiconductor device manufacturing. For example, after forming the second dielectric fill layer 356, a chemical mechanical polishing process is performed to remove excess deposited material and expose the dummy gate material of the vertical structure 326. Figure 3V The component substrate 300 is depicted after operation 244 of method 200.
[0075] In operation 246 of method 200, the dummy gate material of the vertical structure 326, as well as the second oxide layer 332 and bottom isolation structure 330 in the bottom element structure 304B, are removed and replaced with a replacement metal gate (RMG) 358. The RMG 358 formation process in operation 246 typically involves depositing a channel dielectric material, which is typically a chemical oxide selectively deposited on a silicon channel, and a conformal high-k dielectric material, such as HfO2. Following these processes, an RMG metal pad and metal fill process is performed. At the end of operation 234, a metal chemical mechanical polishing process is performed to remove excess deposited material, thereby forming a separate metal gate. Furthermore, prior to dielectric layer deposition, the high-k dielectric material is doped with an appropriate dipole material (typically Al for p-type and La for n-type). RMG 358 may contain any suitable conductive material, including but not limited to cobalt (Co), tungsten (W), platinum (Ru), copper (Cu), molybdenum (Mo), titanium (Ti), nickel (Ni), silver (Ag), gold (Au), bismuth (Ir), tantalum (Ta), platinum (Pt), their conductive oxides or nitrides, or any combination thereof. RMG 358 may be separated from other structures / regions of the component substrate 300 by one or more insulating layers. In some embodiments, RMG 358 may contain multiple layers of the same or different conductive materials. Forming RMG 358 involves several sub-processes, such as selectively etching the second oxide layer 332 and depositing RMG 358.
[0076] The selective etching of the second oxide layer 332 of the element substrate 300 can be accomplished by a dry etching process, a wet etching process, or a combination of these processes as described above. This selective etching process provides selective removal of the dummy gate (polysilicon) and the bottom isolation structure 330. The replacement metal gate (RMG) 358 can be formed by any suitable deposition process, including but not limited to CVD, PVD, ALD, or any combination thereof. The deposition of the RMG 344 may include intermediate steps such as cleaning, degassing, lithography, etching, CMP, or other processes common in semiconductor device manufacturing. Figure 3W The component substrate 300 is depicted after operation 246 of method 200.
[0077] In operation 248 of method 200, a back-side element contact 360B is formed. Operation 248 can be any suitable contact formation sequence, and in one embodiment typically includes: a patterning step to pattern the contact in a lithographic manner; an etching step to remove material and open contacts leading to the structure (source-drain or gate); a silicide step to form ohmic contacts leading to the source-drain; a metal pad deposition and metal filling step; followed by a chemical mechanical polishing step to remove excess deposited material and planarize the structure. The back-side element contact 360B may include the deposition of one or more of the following: a passivation layer, a metal layer, a back-side interconnect, and similar structures, or any combination thereof. The back-side element contact 360B can be formed by any of the suitable processes described above. Figure 3X The component substrate 300 is depicted after operation 248 of method 200.
[0078] In operation 250 of method 200 ( Figure 3Y In this process, the component substrate 300 is bonded to the third substrate layer 362 (e.g., a back-side interconnect substrate assembly). The third substrate layer 362 can be fabricated independently to provide wiring interconnects suitable for the design purpose using any suitable technology. The third substrate layer 362 may include deposited one or more of the following: passivation layer, back-side metal layer, back-side partial wiring, back-side interconnect, back-side interposer window, component, structure, or any combination thereof (e.g., bottom component contact). The third substrate layer 362 can be formed by any of the suitable processes described above. Figure 3Y The component substrate 300 is depicted after operation 250 of method 200.
[0079] In operation 252 of method 200 ( Figure 3ZIn the process, the second substrate layer 350 is removed, the component substrate 300 is flipped, and a top component contact 360A is deposited. The top component contact 360A may include one or more of the following deposited: a passivation layer, a metal layer, a front-side interconnect, and similar structures, or any combination thereof. The top component contact 360A can be formed by any of the suitable processes described above. In one example, the top component contact 360A can be formed using a conventional or other suitable MOL contact sequence, followed by a BEOL interconnect fabrication sequence (…). Figure 3Z Only one BEOL interconnect layer is depicted in the image. The MOL contact sequence typically includes: a patterning step to pattern the contacts using a lithographic printing method; an etching step to remove material and open contacts leading to the structure (source-drain or gate); a silicide step to form ohmic contacts leading to the source-drain; metal pad deposition and metal filling steps; followed by a chemical mechanical polishing process to remove excess deposited material and planarize the structure. Several such process sequences are used to form... Figure 3X All MOL contacts are depicted in the diagram. The BEOL sequence is similar to the MOL sequence (except for siliconization) and is also a standard process sequence used in current manufacturing. Figure 3Z The component substrate 300 is depicted after operation 252 of method 200.
[0080] Compared to monolithic approaches that rely on complex alignment and device bonding methods, various aspects of this disclosure include methods that allow for the creation of CFETs or other vertically aligned semiconductor structures in a more efficient manner using sequential self-aligned processes. By reducing feature height and eliminating several high aspect ratio modules, the methods described herein reduce the problems associated with conventional high aspect ratio features. Furthermore, by inserting another insulator between nanosheet stacks, the methods described herein reduce or eliminate the need for high-temperature thermally stable silicides, contact pads, and gap fill materials, thereby allowing the current Gate All-Around (GAA) replacement of Metal Gate (RMG) and epitaxial processes to be utilized without requiring lower thermal budgets. For example, the methods described herein also allow the front copper traces not to be exposed to the back-side contact formation thermal budget (approximately 800-850°C).
[0081] Additional considerations
[0082] Although this specification contains many specific details of implementation, these should not be construed as limiting the scope of possible requests, but rather as descriptions of features that may be specific to certain implementations. Some features described in the context of independent implementations may also be implemented in combination in a single implementation. Conversely, various features described in the context of a single implementation may also be implemented separately in multiple implementations, or in any suitable sub-combinations. Furthermore, although previously described features may be described as operating in certain combinations, or even initially requested in this manner, in some cases one or more features from the requested combination may be excluded, and the requested combination may be for a sub-combination or a variation of a sub-combination.
[0083] Specific implementations of the objective have been described. Other implementations, variations, and modifications of the described implementations are within the scope of the following claims, which will be apparent to those skilled in the art. Although operations are depicted in a specific order in the drawings or claims, this is not to be construed as requiring such operations to be performed in the specific order or sequence shown, or that all illustrated operations must be completed (some operations may be considered optional) to achieve the desired result. In some cases, multitasking or parallel processing (or a combination of multitasking and parallel processing) may be advantageous and may be performed as needed. Although the various steps of the method or process in the implementation are presented and described in a sequential manner, those with ordinary knowledge in the art will understand that some or all of the steps may be performed in a different order, may be combined or omitted, and some or all of the steps may be performed in parallel. These steps may be performed in an active or passive manner. The method or process may be repeated or extended to support multiple components or multiple users within a field environment. Therefore, its scope should not be considered limited to the specific arrangement of steps shown in the flowcharts or illustrations.
[0084] Furthermore, any of the claimed implementations are considered applicable to at least one computer-implemented method; a non-transitory computer-readable medium for storing computer-readable instructions for performing the computer-implemented method; and a computer system including computer memory interoperably coupled to a hardware processor configured to perform the computer-implemented method or instructions stored on the non-transitory computer-readable medium.
[0085] As used herein, “CPU,” “controller,” “processor,” “at least one processor,” or “one or more processors” generally refers to a single processor configured to perform one or more operations, or multiple processors configured to collectively perform one or more operations. In the case of multiple processors, the execution of one or more operations can be assigned to different processors; while a single processor can perform multiple operations, multiple processors can also collectively perform a single operation. Similarly, “memory,” “at least one memory,” or “one or more memory” generally refers to a single memory configured to store data and / or instructions, or multiple memory modules configured to collectively store data and / or instructions.
[0086] As used in this article, the terms "gas" and "fluid" can be used interchangeably. These two terms generally refer to elements, compounds, materials, etc., that have the properties of a gas, a fluid, or both.
[0087] Unless otherwise defined, all technical and scientific terms used have the same meaning as commonly understood by one of ordinary skill in the art to which these systems, apparatuses, methods, processes and ingredients pertain.
[0088] In this disclosure, the terms "top," "bottom," "side," "above," "below," "up," "down," "upward," "downward," "horizontal," "vertical," and the like do not refer to absolute directions, but rather to directions relative to a non-specific reference plane. This non-specific reference plane can be vertical, horizontal, or other angular orientations.
[0089] The singular forms “a,” “an,” and “the” include plural references unless the context clearly indicates otherwise. In the claims, unless specifically stated otherwise, a reference to a single element is not intended to mean “only one,” but rather “one or more.” Unless specifically stated otherwise, the term “some” refers to one or more.
[0090] Embodiments of this disclosure may suitably include, consist of, or substantially consist of the limiting features disclosed, and may be practiced without the undisclosed limiting features. As used herein and in the appended claims, the words “comprising,” “having,” and “including,” and all grammatical variations thereof, are intended to have an open-ended and non-limiting meaning and do not exclude additional elements or steps.
[0091] "Optional" and "optionally" mean that the material, event, or situation described below may or may not exist or occur. The description includes both the possibility that the material, event, or situation will occur and the possibility that it will not occur.
[0092] "Coupled" and "phase-coupled" mean that the material described subsequently is connected to the material described previously. The connection can be direct or indirect and may or may not include intermediate elements such as pipes, wiring, fasteners, mechanical power transmission, electrical communication, wired and / or wireless transmission, which may be suitable to affect the operation of the components.
[0093] As used, the term "determine" encompasses a wide variety of actions. For example, "determine" can include calculation, operation, processing, derivation, investigation, searching (e.g., looking in a table, database, or other data structure), and confirmation. Furthermore, "determine" can include receiving (e.g., receiving information) and accessing (e.g., accessing data in memory). Additionally, "determine" can include parsing, selecting, picking, and building.
[0094] When the terms “approximately” or “about” are used, the term may mean that the value may vary by up to ±10%, up to 5%, up to 2%, up to 1%, up to 0.5%, up to 0.1%, or up to 0.01%.
[0095] A range can be expressed as from about one specific value to about another specific value (inclusive of the two specific values). When such a range is expressed, it should be understood that another implementation is from one specific value to another specific value, together with all specific values within that range and their combinations.
[0096] As used, terms such as “first” and “second” are arbitrarily assigned and are intended only to distinguish two or more parts of a system, apparatus, or component. It should be understood that the terms “first” and “second” serve no other purpose and are not part of the names or descriptions of components, nor do they necessarily define the relative positions or orientations of components. Furthermore, it should be understood that the use of the terms “first” and “second” does not require the existence of any “third” component, although this is conceivable within the scope of the various embodiments described.
[0097] Although only a few exemplary embodiments have been described in detail, those skilled in the art will readily recognize that numerous modifications to these exemplary embodiments are possible without substantially departing from the scope of the disclosure. Therefore, all such modifications are intended to be included within the scope of this disclosure as defined in the following claims. In the claims, the use of the term "means function" is intended to encompass structures described as performing said function, and not merely structural equivalents, but including equivalent structures. The applicant's explicit intention is that any limitation on any aspect of the claims shall not invoke patent law unless the claim expressly uses the phrase "means, for…" followed by a description of the relevant function.
[0098] By reducing feature height and eliminating several high aspect ratio modules, the method described in this paper reduces the problems associated with traditional high aspect ratio features. Furthermore, by inserting another insulator between nanosheet stacks, the method reduces or eliminates the need for high-temperature thermally stable silicides, contact pads, and gap-filling materials, thereby allowing current gate-all-around (GAA) replacements for metal gates (RMGs) and epitaxial processes to be utilized without requiring lower thermal budgets.
[0099] The techniques described above can be expressed as follows (non-limiting examples).
[0100] Implementation 1: A method for forming a complementary field-effect transistor (CFET) includes: replacing a top sacrificial layer between channel layers in a top superlattice of a top element structure with a top replacement metal gate layer, the top element structure being disposed on a bottom element structure, the bottom element structure being disposed on a first substrate layer; securing a second substrate layer to the top element structure and removing the first substrate layer from the bottom element structure; and replacing a bottom sacrificial layer between channel layers in a bottom superlattice of the bottom element structure with a bottom replacement metal gate layer.
[0101] Implementation Method 2: The method of Implementation Method 1 further includes forming a back-side element contact on the side of the bottom element structure opposite to the top element structure.
[0102] Implementation 3: The method of Implementation 2 further includes: fastening the third substrate layer to the back-side component contact formed on the bottom component structure, and removing the second substrate layer from the top component structure.
[0103] Implementation 4: The method of Implementation 3 further includes: forming a front element contact on the side of the top element structure opposite to the bottom element structure.
[0104] Implementation 5: The method of Implementation 1, wherein replacing the top sacrificial layer between the channel layers interleaved in the top superlattice further comprises: etching the material of the top sacrificial layer and the material of the channel layers at an etch rate ratio of about 10:1 to about 500:1.
[0105] Implementation method 6: The method of implementation method 5, wherein the material of the top sacrificial layer comprises a germanium (Ge) concentration between about 10% and about 30%.
[0106] Implementation Method 7: The method of Implementation Method 6, wherein the material of the channel layer is one of pure silicon (Si), germanium (Ge), or silicon-germanium (SiGe).
[0107] Implementation method 8: The method of implementation method 1 further includes: forming a vertical structure through the top element structure and the bottom element structure.
[0108] Implementation 9: The method of Implementation 8 further includes: depositing n-type material between the vertical structures formed in the top element structure.
[0109] Implementation 10: The method of Implementation 8 further includes: depositing p-type material between vertical structures formed in the bottom element structure.
[0110] Implementation method 11: The method of implementation method 8, wherein forming a vertical structure through the top element structure and the bottom element structure is performed using a self-alignment process.
[0111] Implementation 12: The method of Implementation 1, wherein the replacement of the bottom sacrificial layer between the channel layers in the bottom superlattice of the bottom element structure is performed at a temperature below about 900 degrees Celsius.
[0112] Implementation 13: A method of forming a complementary field-effect transistor (CFET), comprising: forming a bottom device structure on a device substrate, wherein the device substrate includes a first substrate layer, wherein the bottom device structure is disposed above the first substrate layer; the bottom device structure includes: a sacrificial superlattice layer; a plurality of channel layers disposed above the sacrificial superlattice layer, wherein the plurality of channel layers extend through a dummy gate layer, and the plurality of channel layers are separated by a plurality of sacrificial layers; forming a top device structure, wherein the top device structure is disposed above the bottom device structure; the top device structure includes: a sacrificial superlattice layer; a plurality of channel layers disposed above the sacrificial superlattice layer, wherein the plurality of channel layers extend through a dummy gate layer, and the plurality of channel layers are separated by a plurality of sacrificial layers; replacing the sacrificial superlattice layer of the bottom device structure with an isolation structure, and replacing the sacrificial superlattice layer of the top device structure with an isolation structure; disposing a first dielectric filling layer above the bottom device structure; forming an N-channel metal-oxide-semiconductor (NMOS) device from the top device structure, wherein forming the NMOS device includes: removing a plurality of The process involves: a sacrificial layer; performing an epitaxial (epi) process to form an n-type source / drain region on at least one exposed surface of a plurality of channel layers of a top device structure; performing a replacement metal gate (RMG) process to replace a dummy gate layer of the top device structure with a metal gate; and placing a second dielectric fill layer over the NMOS device; bonding a second substrate layer over the NMOS device; removing a first substrate layer; removing the first dielectric fill layer; forming a P-channel metal-oxide-semiconductor (PMOS) device from a bottom device structure, wherein forming the PMOS device includes: removing a plurality of sacrificial layers from the bottom device structure; performing an epitaxial process to form a p-type source / drain region on at least one exposed surface of a plurality of channel layers of the bottom device structure; performing an RMG process to replace a dummy gate layer of the bottom device structure with a metal gate; placing a third dielectric fill layer over the PMOS device; forming a back-side device contact over the PMOS device; bonding a third substrate layer over the back-side device contact; removing a second substrate layer; and forming a front-side device contact over the NMOS device.
[0113] Implementation 14: The method of Implementation 13, wherein the sequential formation of CFET elements includes a self-aligned process.
[0114] Implementation method 15: The method of implementation method 13, wherein the sequential formation of PMOS elements occurs at a temperature below about 900°C.
[0115] Implementation 16: The method of Implementation 13, wherein: a plurality of channel layers include a first material; a plurality of sacrificial layers include a second material, wherein: the ratio of the etch rate of the second material to the etch rate of the first material is between about 10:1 and about 500:1, and the second material contains a germanium (Ge) concentration between about 10% and about 30%; and the sacrificial superlattice layer includes a third material, wherein: the ratio of the etch rate of the third material to the etch rate of the second material and the etch rate of the first material is between about 10:1 and about 200:1, and the third material contains a germanium (Ge) concentration between about 35% and about 60%.
[0116] Implementation 17: A method of forming a complementary field-effect transistor (CFET) includes: forming a bottom device structure on a device substrate, wherein the device substrate includes a first substrate layer, and the bottom device structure is disposed above the first substrate layer; the bottom device structure includes: a sacrificial superlattice layer; a plurality of channel layers disposed above the sacrificial superlattice layer, wherein the plurality of channel layers extend through a dummy gate layer and the plurality of channel layers are separated by a plurality of sacrificial layers; forming a top device structure, wherein the top device structure is disposed above the bottom device structure; the top device structure includes: a sacrificial superlattice layer; a plurality of channel layers disposed above the sacrificial superlattice layer, wherein the plurality of channel layers extend through a dummy gate layer and the plurality of channel layers are separated by a plurality of sacrificial layers; replacing the sacrificial superlattice layer of the bottom device structure with an isolation structure, and replacing the sacrificial superlattice layer of the top device structure with an isolation structure; disposing a first dielectric filling layer on the bottom device structure; forming a P-channel metal-oxide-semiconductor (PMOS) device from the top device structure, wherein forming the PMOS device includes: removing a plurality of The process involves: a sacrificial layer; performing an epitaxial (epi) process to form a P-type source / drain region on at least one exposed surface of a plurality of channel layers of a top device structure; performing a replacement metal gate (RMG) process to replace a dummy gate layer of the top device structure with a metal gate; placing a second dielectric fill layer over the PMOS device; bonding a second substrate layer over the PMOS device; removing a first substrate layer; removing the first dielectric fill layer; forming an N-channel metal-oxide-semiconductor (NMOS) device from a bottom device structure, wherein forming the NMOS device includes: removing a plurality of sacrificial layers from the bottom device structure; performing an epitaxial process to form an n-type source / drain region on at least one exposed surface of a plurality of channel layers of the bottom device structure; performing an RMG process to replace a dummy gate layer of the bottom device structure with a metal gate; placing a third dielectric fill layer over the NMOS device; forming a back-side device contact over the NMOS device; bonding a third substrate layer over the back-side device contact; removing a second substrate layer; and forming a front-side device contact over the PMOS device.
[0117] Implementation 18: The method of Implementation 17, wherein the sequential formation of CFET elements includes a self-aligned process.
[0118] Implementation method 19: The method of implementation method 17, wherein the sequential formation of NMOS devices occurs at a temperature below about 900°C.
[0119] Implementation 20: The method of Implementation 17, wherein: a plurality of channel layers include a first material; a plurality of sacrificial layers include a second material, wherein: the ratio of the etch rate of the second material to the etch rate of the first material is between about 10:1 and about 500:1, and the second material contains a germanium (Ge) concentration between about 10% and 30%; and the sacrificial superlattice layer includes a third material, wherein: the ratio of the etch rate of the third material to the etch rate of the second material and the etch rate of the first material is between about 10:1 and about 200:1, and the third material contains a germanium (Ge) concentration between about 35% and 60%.
[0120] Implementation 21: A method of forming a complementary field-effect transistor (CFET), comprising: sequentially forming CFET elements from a nanosheet stack disposed on a first substrate layer, wherein the nanosheet stack includes a bottom element structure and a top element structure disposed above the bottom element structure, the bottom element structure and the top element structure each including: a sacrificial superlattice layer, and a superlattice disposed above the sacrificial superlattice layer, the superlattice including a plurality of channel layers extending through a dummy gate layer, wherein the plurality of channel layers are separated by a plurality of sacrificial layers, wherein the dummy gate layer includes a top dummy gate layer in the top element structure and a bottom dummy gate layer in the bottom element structure, and wherein sequentially forming the CFET elements further includes The process involves: forming a portion of a bottom field-effect transistor (FET) from a bottom element structure, and forming a portion of a top FET from a top element structure; replacing the sacrificial superlattice layer of the bottom element structure with an isolation structure, and replacing the sacrificial superlattice layer of the top element structure with an isolation structure; forming a second portion of the bottom FET from the bottom element structure and disposing a first dielectric fill layer on top of the bottom element structure; forming a second portion of the top FET; bonding a second substrate layer to the top FET; removing the first substrate layer; removing the first dielectric fill layer; forming a second portion of the bottom FET; forming a bottom FET element contact; bonding a third substrate layer to the bottom FET; and forming a top FET element contact.
[0121] Implementation 22: The method of Implementation 21, wherein the sequential formation of CFET elements includes a self-aligned process.
[0122] Implementation 23: The method of Implementation 21, wherein the bottom FET of the second part is formed at a temperature below about 900°C.
[0123] Implementation 24: The method of Implementation 21, wherein: a plurality of channel layers include a first material; a plurality of sacrificial layers include a second material, wherein: the ratio of the etch rate of the second material to the etch rate of the first material is between about 10:1 and about 500:1, and the second material contains a germanium (Ge) concentration between about 10% and about 30%; and the sacrificial superlattice layer includes a third material, wherein: the ratio of the etch rate of the third material to the etch rate of the second material and the etch rate of the first material is between about 10:1 and about 200:1, and the third material contains a germanium (Ge) concentration between about 35% and about 60%.
[0124] Implementation 25: The method of Implementation 21, wherein the top FET is an N-channel metal-oxide-semiconductor (NMOS) FET and the bottom FET is a P-channel metal-oxide-semiconductor (PMOS) FET.
[0125] Implementation 26: The method of Implementation 21, wherein the top FET is a P-channel metal-oxide-semiconductor (PMOS) FET and the bottom FET is an N-channel metal-oxide-semiconductor (NMOS) FET.
[0126] Implementation 27: The method of Implementation 21, wherein forming the first portion of the bottom FET and the first portion of the top FET further comprises: forming one or more first structures, wherein: each of the one or more first structures includes a portion of a top element structure disposed on a portion of the bottom element structure, each of the one or more first structures being independent of each other, and each of the one or more first structures being oriented in a first direction; forming shallow trench isolation (STI) features between each of the one or more first structures in a first substrate layer; disposing a first oxide layer on the one or more first structures and the STI features; disposing a bottom dummy gate layer above the first oxide layer as a dummy gate, located between each of the one or more first structures, up to the approximately sacrificial superlattice layer of the top element structure; and disposing a silicon nitride layer on the bottom dummy gate. The method comprises: placing a gate layer and one or more exposed surfaces of a first oxide layer above the gate layer; placing a top dummy gate layer above the silicon nitride layer, extending above the top element structure; forming one or more vertical features, wherein: each of the one or more vertical features includes a portion of the top element structure disposed above a portion of the bottom element structure, each of the one or more vertical features being independent of each other, and each of the one or more vertical features being oriented perpendicular to a first direction; placing a spacer layer on one or more exposed side surfaces of the one or more vertical features; recessing a plurality of channel layers, wherein recessing the plurality of channel layers removes a portion of each of the plurality of channel layers, creating a plurality of channel layer pores; selectively etching a sacrificial layer, leaving a plurality of sacrificial layer pores; placing a second oxide layer in the plurality of sacrificial layer pores; and placing internal spacers in the plurality of channel layer pores.
[0127] Implementation 28: The method of Implementation 21, wherein replacing the sacrificial superlattice layer of the bottom element structure with an isolation structure and replacing the sacrificial superlattice layer of the top element structure with an isolation structure comprises: selectively etching the sacrificial superlattice layer to leave one or more pores; and placing the isolation structure in one or more pores.
[0128] Implementation 29: The method of Implementation 21, wherein the second portion of forming the top FET further comprises: performing an epitaxial (epi) process to form a source / drain (S / D) region on at least one exposed surface of a plurality of channel layers of the top device structure; disposing a first contact etch-stop liner (CESL) on the exposed surface of the first dielectric fill layer, the side surface of each of one or more vertical features, and the S / D region, wherein: each of the one or more vertical features comprises a portion of the top device structure disposed above a portion of the bottom device structure, and each of the one or more vertical features is isolated from each other; disposing a second dielectric fill layer over the first CESL and between the one or more vertical features; and forming a replacement metal gate (RMG) from the top dummy gate layer.
[0129] Implementation 30: The method of Implementation 21, wherein the second portion of forming the bottom FET further comprises: performing an epitaxial (epi) process to form a source / drain (S / D) region on at least one exposed surface of a plurality of channel layers of the bottom device structure; disposing a second contact etch-stop liner (CESL) over the exposed surface of the top device structure, the side surface of each of one or more vertical features, and the S / D region, wherein: each of the one or more vertical features comprises a portion of the bottom device structure disposed over a portion of the bottom device structure, and each of the one or more vertical features is isolated from each other; disposing a third dielectric fill layer over the first CESL and between the one or more vertical features; and forming a replacement metal gate (RMG) from the bottom dummy gate layer.
[0130] The claims above are not intended to limit the provided embodiments, but rather to provide a full scope consistent with the language of the claims.
Claims
1. A method for forming a complementary field-effect transistor (CFET), the method comprising: The top sacrificial layer between the channel layers in the top superlattice interleaved in the top element structure is replaced by a top replacement metal gate layer, the top element structure being disposed on the bottom element structure, and the bottom element structure being disposed on the first substrate layer; Secure the second substrate layer to the top element structure and remove the first substrate layer from the bottom element structure; as well as The bottom sacrificial layer between the channel layers in the bottom superlattice of the bottom element structure is replaced with a bottom replacement metal gate layer.
2. The method of claim 1, further comprising: A back-side element contact is formed on the side of the bottom element structure opposite to the top element structure.
3. The method of claim 2, further comprising: The third substrate layer is fastened to the back-side element contact formed on the bottom element structure, and the second substrate layer is removed from the top element structure.
4. The method of claim 3, further comprising: A front element contact is formed on the side of the top element structure opposite to the bottom element structure.
5. The method of claim 1, wherein replacing the top sacrificial layer interlaced between the channel layers in the top superlattice further comprises: The material of the top sacrificial layer is etched at an etch rate ratio of approximately 10:1 to approximately 500:1 relative to the material of the channel layer.
6. The method of claim 5, wherein the material of the top sacrificial layer comprises a germanium (Ge) concentration between about 10% and about 30%.
7. The method of claim 6, wherein the material of the channel layer is one of pure silicon (Si), germanium (Ge), or silicon-germanium (SiGe).
8. The method of claim 1, further comprising: A vertical structure is formed by passing through the top element structure and the bottom element structure.
9. The method of claim 8, further comprising: n-type material is deposited between the vertical structures formed in the top element structure.
10. The method of claim 8, further comprising: p-type material is deposited between the vertical structures formed in the bottom element structure.
11. The method of claim 8, wherein forming the vertical structure through the top element structure and the bottom element structure is performed using a self-aligned process.
12. The method of claim 1, wherein replacing the bottom sacrificial layer between the channel layers interleaved in the bottom superlattice of the bottom element structure is performed at a temperature below about 900 degrees Celsius.
13. A method for forming a complementary field-effect transistor (CFET), the method comprising: A bottom component structure is formed on a component substrate, wherein the component substrate includes a first substrate layer, and the bottom component structure is disposed above the first substrate layer; The bottom component structure includes: Sacrifice superlattice layer; Multiple channel layers are disposed on the sacrificial superlattice layer, wherein the multiple channel layers extend through the dummy gate layer and are separated by multiple sacrificial layers; A top element structure is formed, wherein the top element structure is disposed above the bottom element structure; the top element structure includes: Sacrifice superlattice layer; Multiple channel layers are disposed on the sacrificial superlattice layer, wherein the multiple channel layers extend through the dummy gate layer and are separated by multiple sacrificial layers; The sacrificial superlattice layer of the bottom element structure is replaced with an isolation structure, and the sacrificial superlattice layer of the top element structure is replaced with an isolation structure. The first dielectric filling layer is placed on top of the bottom component structure; An N-channel metal-oxide-semiconductor (NMOS) device is formed from the top element structure, wherein forming the NMOS device includes: Remove the plurality of sacrificial layers from the top component structure; An epitaxial (epi) process is performed to form an n-type source-drain region on at least one exposed surface of the plurality of channel layers in the top element structure; Perform a replacement metal gate (RMG) process to replace the dummy gate layer of the top element structure with a metal gate; and A second dielectric filling layer is placed on top of the NMOS device; A second substrate layer is bonded on top of the NMOS element; Remove the first substrate layer; Remove the first dielectric fill layer; A P-channel metal-oxide-semiconductor (PMOS) device is formed from the bottom element structure, wherein forming the PMOS device includes: Remove the plurality of sacrificial layers from the bottom component structure; Perform an epitaxial process to form a p-type source / drain region on at least one exposed surface of the plurality of channel layers of the bottom element structure; Perform the RMG process to replace the dummy gate layer of the bottom element structure with a metal gate; and A third dielectric filling layer is placed on the PMOS element; A back-side element contact is formed on the PMOS element; A third substrate layer is bonded over the back-side component contact; Remove the second substrate layer; and A front-side element contact is formed on the NMOS element.
14. The method of claim 13, wherein sequentially forming the CFET element includes a self-aligned process.
15. The method of claim 13, wherein the sequential formation of the PMOS element occurs at a temperature below about 900°C.
16. The method of claim 13, wherein: The plurality of channel layers include a first material; The plurality of sacrificial layers include a second material, wherein: The ratio of the etching rate of the second material to the etching rate of the first material is between approximately 10:1 and approximately 500:
1. The second material contains a germanium (Ge) concentration between about 10% and about 30%; and The sacrificial superlattice layer comprises a third material, wherein: The ratio of the etching rate of the third material to the etching rate of the second material and the etching rate of the first material is between approximately 10:1 and approximately 200:
1. The third material contains a germanium (Ge) concentration ranging from about 35% to about 60%.
17. A method for forming a complementary field-effect transistor (CFET), the method comprising: A bottom component structure is formed on a component substrate, wherein the component substrate includes a first substrate layer, and the bottom component structure is disposed above the first substrate layer; The bottom component structure includes: Sacrifice superlattice layer; Multiple channel layers are disposed on the sacrificial superlattice layer, wherein the multiple channel layers extend through the dummy gate layer and are separated by multiple sacrificial layers; A top element structure is formed, wherein the top element structure is disposed above the bottom element structure; the top element structure includes: Sacrifice superlattice layer; Multiple channel layers are disposed on the sacrificial superlattice layer, wherein the multiple channel layers extend through the dummy gate layer and are separated by multiple sacrificial layers; The sacrificial superlattice layer of the bottom element structure is replaced with an isolation structure, and the sacrificial superlattice layer of the top element structure is replaced with an isolation structure. The first dielectric filling layer is placed on top of the bottom component structure; A P-channel metal-oxide-semiconductor (PMOS) element is formed from the top element structure, wherein forming the PMOS element includes: Remove the plurality of sacrificial layers from the top component structure; An epitaxial (epi) process is performed to form a p-type source / drain region on at least one exposed surface of the plurality of channel layers in the top element structure; Perform a replacement metal gate (RMG) process to replace the dummy gate layer of the top element structure with a metal gate; and A second dielectric filling layer is disposed on the PMOS element; A second substrate layer is bonded on top of the PMOS element; Remove the first substrate layer; Remove the first dielectric fill layer; An N-channel metal-oxide-semiconductor (NMOS) device is formed from the bottom element structure, wherein forming the NMOS device includes: Remove the plurality of sacrificial layers from the bottom component structure; Perform an epitaxial process to form an n-type source / drain region on at least one exposed surface of the plurality of channel layers of the bottom element structure; Perform the RMG process to replace the dummy gate layer of the bottom element structure with a metal gate; and A third dielectric filling layer is placed on top of the NMOS device; A back-side element contact is formed on the NMOS element; A third substrate layer is bonded over the back-side component contact; Remove the second substrate layer; and A front-side element contact is formed on the PMOS element.
18. The method of claim 17, wherein sequentially forming the CFET element includes a self-aligned process.
19. The method of claim 17, wherein the sequential formation of the NMOS element occurs at a temperature below about 900°C.
20. The method of claim 17, wherein: The plurality of channel layers include a first material; The plurality of sacrificial layers include a second material, wherein: The ratio of the etching rate of the second material to the etching rate of the first material is between approximately 10:1 and approximately 500:
1. The second material contains a germanium (Ge) concentration between about 10% and about 30%; and The sacrificial superlattice layer comprises a third material, wherein: The ratio of the etching rate of the third material to the etching rates of the second and first materials is between approximately 10:1 and approximately 200:
1. The third material contains a germanium (Ge) concentration ranging from about 35% to about 60%.