Composite substrate and method for manufacturing composite substrate

By embedding conductor patterns into recesses on the surface of an inorganic material substrate and forming steps, and then covering the steps with a dielectric film, the problem of bonding instability caused by the increase in conductor pattern thickness is solved, thus achieving a balance between conductor pattern thickness and bonding stability.

CN123126103APending Publication Date: 2026-11-17NGK CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202480088194.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In composite substrates, the increased thickness of the conductor pattern leads to unstable bonding between the inorganic material substrate and the support substrate. Existing technologies struggle to simultaneously achieve both increased conductor pattern thickness and bonding stability.

Method used

A conductor pattern is implanted by creating a recess on the surface of an inorganic material substrate, and steps are formed by grinding. The steps are then covered with a dielectric film to stabilize the substrate and ensure the thickness and bonding strength of the conductor pattern.

Benefits of technology

The thickness of the conductor pattern is sufficiently large compared to the skin depth, reducing conductor loss, and the inorganic material substrate and the support substrate can be stably bonded.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123126103A_ABST
    Figure CN123126103A_ABST
Patent Text Reader

Abstract

This invention provides a composite substrate in which a conductor pattern of desired thickness can be disposed between an inorganic material substrate and a support substrate, and the inorganic material substrate and the support substrate can be stably bonded. One embodiment of the composite substrate includes: an inorganic material substrate, a conductor pattern, a dielectric film, and a support substrate. The inorganic material substrate has a substrate surface. A recess is provided on the substrate surface. The substrate surface includes: a first portion located outside the recess, and a second portion serving as the inner surface of the recess. The conductor pattern is embedded in the recess. The conductor pattern and the first portion of the substrate surface form a step. The dielectric film is disposed on the substrate surface to cover the step. The support substrate is located on the opposite side of the inorganic material substrate relative to the dielectric film. The support substrate is bonded to the dielectric film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to composite substrates and methods for manufacturing composite substrates. Background Technology

[0002] Given: A composite substrate is formed by bonding an inorganic material substrate with a conductor pattern to a support substrate. In recent years, with the diversification of applications for composite substrates, it is sometimes required that the conductor pattern be located between the inorganic material substrate and the support substrate.

[0003] Furthermore, it is desirable to make the thickness of the conductor pattern sufficiently large compared to the skin depth, thereby reducing conductor loss within the conductor pattern. However, in composite substrates where the conductor pattern is located between the inorganic material substrate and the support substrate, there is a problem: if the thickness of the conductor pattern is increased, the bonding between the inorganic material substrate and the support substrate becomes unstable.

[0004] Existing technical documents

[0005] Patent documents

[0006] Patent Document 1: Japanese Patent Application Publication No. 2023-10103 Summary of the Invention

[0007] Therefore, it was explored that by embedding a conductor pattern in a recess on the surface of an inorganic material substrate (hereinafter referred to as the substrate surface), the thickness of the conductor pattern and the bonding stability of the inorganic material substrate and the support substrate can be simultaneously improved.

[0008] To achieve such a configuration, for example, it is conceivable that after forming a conductor pattern with sufficient thickness in the recess, the conductor pattern and the substrate surface exposed from the conductor pattern are polished.

[0009] However, if the substrate surface is polished together with the conductor pattern, the amount of polishing may differ due to the different materials of the conductor pattern and the inorganic substrate, resulting in steps between the substrate surface and the conductor pattern surface. Furthermore, depending on the proportion of conductor patterns on the substrate surface, phenomena such as dishing in the center of the conductor pattern and thinning due to over-polishing of the inorganic substrate and conductor pattern may occur, further creating complex steps on the overall surface of both the inorganic substrate and the conductor.

[0010] If such a step is created, even if the conductor pattern is embedded in the recess, it will be difficult to stably bond the inorganic material substrate and the support substrate.

[0011] The main objective of this invention is to provide a composite substrate in which a conductor pattern having a desired thickness can be disposed between an inorganic material substrate and a support substrate, and the inorganic material substrate and the support substrate can be stably bonded.

[0012] [1] One embodiment of the present invention relates to a composite substrate comprising: an inorganic material substrate, a conductor pattern, a dielectric film, and a support substrate. The inorganic material substrate has a substrate surface. A recess is provided on the substrate surface. The substrate surface includes: a first portion located outside the recess, and a second portion serving as the inner surface of the recess. The conductor pattern is embedded in the recess. The conductor pattern and the first portion of the substrate surface form a step. The dielectric film is disposed on the substrate surface such that it covers the step. The support substrate is located on the opposite side of the inorganic material substrate relative to the dielectric film. The support substrate is bonded to the dielectric film.

[0013] [2] In the composite substrate described in [1] above, the conductor pattern has a conductor surface. The conductor surface may form the aforementioned steps. The spacing between the first portion of the substrate surface and the conductor surface in the thickness direction of the inorganic material substrate may be 0.01 μm to 2.0 μm.

[0014] [3] In the composite substrate described in [2] above, the conductor surface may be located at a position closer to the supporting substrate side than the first portion of the substrate surface.

[0015] [4] In the composite substrate described in [2] above, the first portion of the substrate surface may be located at a position closer to the supporting substrate side than the conductor surface.

[0016] [5] In any of the composite substrates described in [1] to [4] above, the thickness of the conductor pattern may be 1.5 μm or more.

[0017] [6] In any of the composite substrates described in [1] to [5] above, the inorganic material substrate may be made of quartz glass.

[0018] [7] In any of the composite substrates described in [1] to [6] above, the thickness of the inorganic material substrate may be less than 100 μm.

[0019] [8] In any of the composite substrates described in [1] to [7] above, the supporting substrate may be made of Si, AlN, SiC, LTCC (low temperature co-fired ceramic), diamond or Si3N4.

[0020] [9] Another aspect of the present invention relates to a method for manufacturing a composite substrate, comprising the following steps: preparing an inorganic material substrate having a substrate surface having a recess; forming a conductor pattern embedded in the recess; grinding the conductor pattern and a first portion of the substrate surface located outside the recess, thereby forming a step through the conductor pattern and the first portion of the substrate surface; providing a dielectric film on the substrate surface in such a way as to cover the step; and bonding a support substrate on the side opposite to the inorganic material substrate relative to the dielectric film.

[0021] Invention Effects

[0022] According to embodiments of the present invention, a conductor pattern having a desired thickness can be disposed between an inorganic material substrate and a support substrate, and the inorganic material substrate and the support substrate can be stably bonded. Attached Figure Description

[0023] Figure 1 This is a schematic cross-sectional view of the composite substrate according to one embodiment of the present invention.

[0024] Figure 2 This is a schematic cross-sectional view of the composite substrate according to another embodiment of the present invention.

[0025] Figure 3 yes Figure 1 A schematic diagram of the conductor pattern of the composite substrate.

[0026] Figure 4 This is a schematic cross-sectional view of the composite substrate according to another embodiment of the present invention.

[0027] Figure 5 This is a schematic diagram illustrating a method for manufacturing a composite substrate according to another aspect of the present invention, and a schematic diagram illustrating a process for preparing an inorganic material substrate.

[0028] Figure 6 It is used to explain what follows. Figure 5 A schematic diagram illustrating the process of forming a conductor film.

[0029] Figure 7 It is used to explain what follows. Figure 6 A schematic diagram illustrating the process of grinding a conductor film to form a conductor pattern.

[0030] Figure 8 This is a schematic diagram illustrating another embodiment of the process for forming a conductor pattern.

[0031] Figure 9 It is used to explain what follows. Figure 7 and Figure 8 A schematic diagram illustrating the process of forming a dielectric film. Detailed Implementation

[0032] The embodiments of the present invention will be described below; however, the present invention is not limited to these embodiments. Furthermore, to make the description clearer, the accompanying drawings sometimes schematically represent the width, thickness, shape, etc., of each part compared to the embodiments; however, this is merely an example and does not limit the interpretation of the present invention.

[0033] A. Overview of Composite Substrates

[0034] Figure 1 This is a schematic cross-sectional view of the composite substrate according to one embodiment of the present invention.

[0035] like Figure 1 As shown, the composite substrate 100 includes: an inorganic material substrate 1, a conductor pattern 2, a dielectric film 3, and a support substrate 6. The support substrate 6 is located on the side opposite to the inorganic material substrate 1 relative to the dielectric film 3. The inorganic material substrate 1 has a first substrate surface 15 and a second substrate surface 16. The first substrate surface 15 is the surface of the inorganic material substrate 1 on the side of the support substrate 6 in the thickness direction. The second substrate surface 16 is the surface of the inorganic material substrate 1 on the side opposite to the first substrate surface 15 in the thickness direction.

[0036] A recess 11 is provided on the surface 15 of a first substrate. The surface 15 of the first substrate includes a first portion 15a located outside the recess 11 and a second portion 15b serving as the inner surface of the recess 11. The first portion 15a of the first substrate surface 15 is typically the portion of the first substrate surface 15 other than the recess 11, extending in a direction orthogonal to the thickness direction of the inorganic material substrate 1.

[0037] Conductor pattern 2 is embedded in recess 11. Conductor pattern 2 and first portion 15a of first substrate surface 15 form step 5. Dielectric film 3 is disposed on first substrate surface 15 of inorganic material substrate 1 in such a way that it covers step 5. Support substrate 6 is bonded to dielectric film 3.

[0038] With this configuration, the conductor pattern 2 is embedded in the recess 11 of the inorganic material substrate 1. Therefore, the thickness of the conductor pattern 2 can be made sufficiently large, thereby reducing conductor loss in the conductor pattern 2. Furthermore, even if the conductor pattern 2 is disposed between the inorganic material substrate 1 and the support substrate 6, and the conductor pattern 2 and the first portion 15a of the first substrate surface 15 form a step 5, since the dielectric film 3 covers the step 5 and the support substrate 6 is bonded to the dielectric film 3, the inorganic material substrate 1 and the support substrate 6 can be stably bonded.

[0039] The conductor pattern 2 typically has a conductor surface 2a. The conductor surface 2a is one face of the conductor pattern 2 in the thickness direction of the inorganic material substrate 1. The conductor surface 2a typically extends in a direction orthogonal to the thickness direction of the inorganic material substrate 1. In one embodiment, the conductor surface 2a and a first portion 15a of the first substrate surface 15 together form a step 5.

[0040] The conductor surface 2a of the conductor pattern 2 can be located on the side of the support substrate 6 closer to the first portion 15a of the first substrate surface 15 of the inorganic material substrate 1, or it can be located on the opposite side of the support substrate 6 relative to the first portion 15a of the first substrate surface 15 of the inorganic material substrate 1.

[0041] like Figure 1 As shown, when the conductor surface 2a is located on the side of the supporting substrate 6 closer to the first portion 15a of the first substrate surface 15, the conductor pattern 2 has an implanted portion 21 and a protruding portion 22 integrally in the thickness direction of the inorganic material substrate 1.

[0042] The implanted portion 21 is located within the recess 11.

[0043] The protruding portion 22 protrudes from a first portion 15a of the first substrate surface 15 in the thickness direction of the inorganic material substrate 1. The protruding portion 22 has the aforementioned conductor surface 2a and conductor side surface 2b. The conductor side surface 2b typically extends along the thickness direction of the inorganic material substrate 1. The end of the conductor side surface 2b opposite to the implanted portion 21 is connected to the conductor surface 2a.

[0044] In the example shown, a step 5 is formed by the first portion 15a of the first substrate surface 15, the conductor surface 2a, and the conductor side surface 2b.

[0045] like Figure 2 As shown, when the conductor surface 2a is located on the opposite side of the support substrate 6 relative to the first portion 15a of the first substrate surface 15, that is, when the first portion 15a of the first substrate surface 15 is located closer to the support substrate 6 than the conductor surface 2a, the entire conductor pattern 2 is located within the recess 11. In this case, the side of the recess 11 (i.e., a portion of the second portion 15b of the first substrate surface 15) has: a contact portion 11a that contacts the conductor pattern 2, and an exposed portion 11b that protrudes from the conductor pattern 2. The exposed portion 11b is located closer to the support substrate 6 than the contact portion 11a in the thickness direction of the inorganic material substrate 1.

[0046] The exposed portion 11b extends typically along the thickness direction of the inorganic material substrate 1. The end of the exposed portion 11b opposite to the contact portion 11a is connected to the first portion 15a of the first substrate surface 15.

[0047] In the example shown, the first portion 15a of the first substrate surface 15, the conductor surface 2a, and the exposed portion 11b form a step 5.

[0048] Figure 1 and Figure 2 In this process, the distance between the first portion 15a of the first substrate surface 15 in the thickness direction of the inorganic material substrate 1 and the conductor surface 2a (i.e., the height of the step 5) is, for example, 0.005 μm to 3.0 μm, preferably 0.01 μm to 2.0 μm. If the step 5 has such a height, the dielectric film 3 can stably cover the step 5, thus sufficiently improving the bonding stability between the inorganic material substrate 1 and the support substrate 6.

[0049] B. Details of the composite substrate

[0050] The following is for reference Figure 1 The details of each component of the composite substrate are explained.

[0051] B-1 Inorganic Material Substrate 1

[0052] The inorganic material substrate 1 is composed of any suitable inorganic material.

[0053] Examples of inorganic materials constituting the inorganic material substrate 1 include: single-crystal quartz, amorphous quartz, spinel, AlN, sapphire, SiC, magnesium oxide, and silicon. Inorganic materials can be used alone or in combination.

[0054] Among these inorganic materials, amorphous quartz (quartz glass) is a preferred example. If the inorganic material substrate 1 is made of quartz glass, dielectric loss in materials such as antennas and circuit boards can be reduced, and stability against changes in humidity and temperature can be improved.

[0055] The inorganic material substrate 1 is typically electrically insulating.

[0056] The resistivity of the inorganic material substrate 1 is, for example, 10. 8 kΩ·cm or higher, preferably 10 10 Above kΩ·cm. If the inorganic material substrate 1 has such a resistivity, short circuits in the conductor pattern 2 can be stably suppressed. From this point of view, the higher the resistivity of the inorganic material substrate 1, the better. The upper limit of the resistivity of the inorganic material substrate 1 is typically 10 kΩ·cm. 13 kΩ·cm.

[0057] The Young's modulus of the inorganic material substrate 1 is, for example, 30 GPa to 500 GPa, preferably 50 GPa to 400 GPa. If the Young's modulus of the inorganic material substrate 1 is in such a range, then by appropriately selecting the abrasive pad and slurry, it is possible to abrade the substrate in a manner where the step 5 is not too large.

[0058] The thickness of the inorganic material substrate 1 is, for example, 500 μm or less, preferably 200 μm or less, more preferably 100 μm or less, even more preferably 80 μm or less, and particularly preferably 60 μm or less.

[0059] If the thickness of the inorganic material substrate 1 is below such an upper limit, the composite substrate 100 can be made thinner. In addition, if such a composite substrate 100 is applied to a waveguide element, the induction of planar mode can be suppressed, and the occurrence of substrate resonance can be suppressed.

[0060] On the other hand, the thickness of the inorganic material substrate 1 is, for example, 1 μm or more, preferably 2 μm or more, more preferably 10 μm or more, even more preferably 20 μm or more, particularly preferably 30 μm or more, and particularly preferably 40 μm or more.

[0061] The inorganic material substrate 1, as described above, has a first substrate surface 15 and a second substrate surface 16.

[0062] In the example shown, the first substrate surface 15 is the lower surface of the inorganic material substrate 1, located within the composite substrate 100. The second substrate surface 16 is the upper surface of the inorganic material substrate 1.

[0063] A recess 11 is provided on the surface 15 of the first substrate.

[0064] The recess 11 has any suitable pattern shape corresponding to the conductor pattern 2.

[0065] The recess 11 has any suitable shape in the cross-section obtained by cutting the inorganic material substrate 1 along the thickness direction. Representative cross-sectional shapes of the recess 11 include approximately U-shaped and approximately V-shaped. In the example shown, the cross-section of the recess 11 is approximately U-shaped.

[0066] The inner surface (second portion 15b of the first substrate surface 15) of the recess 11, which has a generally U-shaped cross-section, includes a bottom surface, a first side surface, and a second side surface. The bottom surface of the recess 11 is substantially parallel to the first portion 15a of the first substrate surface 15. The first and second side surfaces are typically spaced apart from each other in a direction orthogonal to the thickness direction of the inorganic material substrate 1. In the example shown, the first and second side surfaces extend from the bottom surface of the recess 11 to the first portion 15a of the first substrate surface 15 in the thickness direction of the inorganic material substrate 1, respectively.

[0067] The size (depth) of the recess 11 in the thickness direction of the inorganic material substrate 1 is arbitrarily and appropriately adjusted in accordance with the thickness of the conductor pattern 2.

[0068] Regarding the depth of the recess 11, when the thickness of the inorganic material substrate 1 is set to 100%, it is, for example, 0.5% to 30%, preferably 1% to 20%. Furthermore, the depth of the recess 11 is, for example, 0.5 μm to 5.0 μm, preferably 1.0 μm to 3.0 μm. If the depth of the recess 11 is within such a range, the thickness of the conductor pattern 2 can be made sufficiently large.

[0069] B-2. Conductor Pattern 2

[0070] The conductor pattern 2 is implanted in the recess 11 as described above, and has any suitable pattern shape. There are no particular limitations on the configuration of the conductor pattern 2. The conductor pattern 2 may, for example, include electrodes, transmission lines, antennas, or substrate through-holes (conductive vias). Figure 3 As shown, in one embodiment, the conductor pattern 2 includes: a transmission line 25, a ground electrode 26, and an antenna 27.

[0071] Conductor pattern 2 is made of any suitable conductor material.

[0072] Metals can be cited as examples of conductive materials. Examples of metals include chromium (Cr), nickel (Ni), copper (Cu), gold (Au), silver (Ag), palladium (Pd), titanium (Ti), aluminum (Al), platinum (Pt), molybdenum (Mo), and their alloys.

[0073] In one embodiment, the conductor pattern 2 comprises copper and / or gold. If the conductor pattern 2 comprises copper and / or gold, it can impart excellent electrical conductivity to the conductor pattern 2.

[0074] The conductor pattern 2 can have a single-layer structure or a stacked structure consisting of two or more layers. When the conductor pattern 2 has a stacked structure, it consists of layers made of different materials or materials of the same material but with different compositions and densities.

[0075] Conductor pattern 2 is representative of electrical conductivity.

[0076] The resistivity of conductor pattern 2 is, for example, 20 μΩ·cm or less, preferably 8.0 μΩ·cm or less. On the other hand, the lower limit of the resistivity of conductor pattern 2 is typically 1.0 μΩ·cm.

[0077] The closer the coefficient of linear expansion of the conductor material constituting the conductor pattern 2 is to that of the inorganic material constituting the inorganic material substrate 1, the more ideal it is.

[0078] The coefficient of linear expansion of the conductor material constituting the conductor pattern 2 is, for example, 10 to 70 times, preferably 20 to 50 times, relative to the coefficient of linear expansion of the inorganic material constituting the inorganic material substrate 1.

[0079] The coefficient of linear expansion of the conductor material is, for example, 4 × 10⁻⁶. -6 / K~30×10 -6 / K, preferably 10×10 -6 / K~25×10 -6 / K.

[0080] If the coefficient of linear expansion of the conductor material constituting the conductor pattern 2 is in such a range, then even if the composite substrate 100 is heated, the conductor pattern 2 can be stably suppressed from peeling off from the inner surface of the recess 11.

[0081] The conductor pattern 2 can be harder or softer than the inorganic material substrate 1.

[0082] The Young's modulus of conductor pattern 2 is, for example, 20 GPa to 400 GPa, preferably 50 GPa to 150 GPa.

[0083] The absolute value of the difference between the Young's modulus of the inorganic material substrate 1 and the conductor pattern 2 is, for example, 1 GPa to 300 GPa, preferably 2 GPa to 100 GPa.

[0084] The thickness of the conductor pattern 2 is, for example, 1.0 μm or more, preferably 1.5 μm or more. If the conductor pattern 2 has such a thickness, the thickness of the conductor pattern 2 can be made sufficiently large compared to the skin depth, thereby enabling the conductor loss in the conductor pattern 2 to be stably reduced.

[0085] On the other hand, the thickness of the conductor pattern 2 is, for example, 20 μm or less, preferably 10 μm or less. If the thickness of the conductor pattern 2 is in such a range, the height of the step 5 can be stably adjusted to the range described above.

[0086] Furthermore, the thickness deviation of the conductor pattern 2 is, for example, 0.001 μm to 2.0 μm, preferably 0.05 μm to 1.0 μm, and more preferably 0.1 μm to 1.0 μm. It should be noted that the thickness deviation of the conductor pattern 2 is measured, for example, by an elevation difference meter, an atomic force microscope, or a scanning electron microscope.

[0087] like Figure 1 As shown, conductor pattern 2 has conductor surface 2a as described above.

[0088] In the example shown, conductor surface 2a is the lower surface of conductor pattern 2, located within composite substrate 100. In one embodiment, conductor surface 2a is substantially parallel to a first portion 15a of the first substrate surface 15.

[0089] An adhesive layer (not shown) may be provided on the conductor surface 2a of the conductor pattern 2. If an adhesive layer is provided on the conductor surface 2a, peeling at the interface between the conductor pattern 2 and the dielectric film 3 can be suppressed.

[0090] The sealing layer is made of any suitable metal. Examples of metals constituting the sealing layer (hereinafter sometimes referred to as the sealing layer material) include chromium (Cr), nickel (Ni), palladium (Pd), titanium (Ti), and their alloys. When conductor pattern 2 is made of metal, the sealing layer is typically made of a different metal than conductor pattern 2.

[0091] The thickness of the sealing layer is, for example, 0.01 μm to 0.3 μm, preferably 0.02 μm to 0.15 μm.

[0092] B-3. ​​Dielectric membrane 3

[0093] A dielectric film 3 is disposed between the inorganic material substrate 1 and the support substrate 6, covering the aforementioned step 5. In the example shown, the dielectric film 3 is in contact with the first substrate surface 15 of the inorganic material substrate 1 and the conductor surface 2a of the conductor pattern 2.

[0094] The dielectric film 3 is made of any suitable dielectric material.

[0095] Examples of dielectric materials include: amorphous silicon, SiO2, Ta2O5, Al2O3, TiO2, Nb2O5, Y2O3, AlN, and ZrO2. Dielectric materials can be used alone or in combination.

[0096] Among these dielectric materials, amorphous silicon is a preferred choice. If the dielectric film 3 is made of amorphous silicon, the bonding stability between the inorganic material substrate 1 and the support substrate 6 can be further improved.

[0097] The dielectric membrane 3 is typically electrically insulating.

[0098] The resistivity of the dielectric film 3 is, for example, 10 kΩ·cm or more, preferably 10 kΩ·cm. 10 Above kΩ·cm. If the dielectric film 3 has such a resistivity, short circuits in the conductor pattern 2 can be stably suppressed. From this point of view, the higher the resistivity of the dielectric film 3, the better. The upper limit of the resistivity of the dielectric film 3 is typically 10 kΩ·cm. 15 kΩ·cm.

[0099] The closer the coefficient of linear expansion of the dielectric material constituting the dielectric film 3 is to that of the materials constituting the inorganic material substrate 1 and the support substrate 6, the more ideal it is.

[0100] The coefficient of linear expansion of the dielectric material constituting the dielectric film 3 is, for example, 0.5 to 20 times, preferably 1.0 to 10 times, relative to the coefficient of linear expansion of the inorganic material constituting the inorganic material substrate 1.

[0101] Furthermore, the coefficient of linear expansion of the dielectric material constituting the dielectric film 3 is, for example, 0.01 to 10 times, preferably 0.02 to 5 times, relative to the coefficient of linear expansion of the inorganic material constituting the support substrate 6.

[0102] The coefficient of linear expansion of dielectric materials is, for example, 0.1 × 10⁻⁶. -6 / K~20×10 -6 / K, preferably 0.3×10 -6 / K~10×10 -6 / K.

[0103] If the coefficient of linear expansion of the dielectric material constituting the dielectric film 3 is in such a range, then the peeling of the dielectric film 3 from the inorganic material substrate 1 and / or the support substrate 6 can be stably suppressed.

[0104] The thermal conductivity of the dielectric film 3 is, for example, 0.5 W / km or more, preferably 1.0 W / km or more. On the other hand, the upper limit of the thermal conductivity of the dielectric film 3 is typically 50 W / km.

[0105] The thickness of the dielectric film 3 is greater than the height of the step 5. The thickness of the dielectric film 3 relative to the height of the step 5 is, for example, 1.5 times or more, preferably 2.0 times or more. If the thickness of the dielectric film 3 is at or above such a lower limit, the step 5 can be stably covered, and it is also easy to perform polishing for smoothing the dielectric film 3, which can sufficiently ensure the bonding stability between the inorganic material substrate 1 and the support substrate 6.

[0106] On the other hand, the thickness of the dielectric film 3 is, for example, 200 times or less, preferably 100 times or less, relative to the height of the step 5. If the thickness of the dielectric film 3 is below such an upper limit, the thinning of the composite substrate 100 can be sufficiently achieved.

[0107] The thickness of the dielectric film 3 is, for example, 0.05 μm to 3.0 μm, preferably 0.1 μm to 2.0 μm.

[0108] B-4. Supporting substrate 6

[0109] The support substrate 6 can impart excellent mechanical strength to the composite substrate 100. Therefore, the inorganic material substrate 1 can be thinned as described above.

[0110] The support substrate 6 is located on the opposite side of the inorganic material substrate 1 relative to the dielectric film 3. In one embodiment, the support substrate 6 is bonded to the dielectric film 3 by means of the bonding portion 4. Thus, the support substrate 6 supports the inorganic material substrate 1 through the dielectric film 3 and the bonding portion 4.

[0111] The support substrate 6 is made of any suitable inorganic material. The inorganic material constituting the support substrate 6 may be the same as or different from the inorganic material substrate 1.

[0112] Inorganic materials constituting the support substrate 6 (hereinafter sometimes referred to as support substrate materials) include, for example: silicon (Si), aluminum nitride (AlN), silicon carbide (SiC), silicon nitride (Si3N4), diamond, indium phosphide (InP), glass, silicon aluminum oxynitride ceramic (Si3N4-Al2O3), andalusite (3Al2O3·2SiO2, 2Al2O3·3SiO2), magnesium oxide (MgO), aluminum oxide (Al2O3), spinel (MgAl2O4), sapphire, quartz, crystal, gallium nitride (GaN), gallium oxide (Ga2O3), and LTCC (low-temperature co-fired ceramics). Inorganic materials can be used alone or in combination.

[0113] In one embodiment, the support substrate 6 is made of Si, AlN, SiC, LTCC, diamond, or Si3N4. If the support substrate 6 is made of such an inorganic material, the heat dissipation, mechanical strength, and thermal stability of the composite substrate 100 can be improved.

[0114] The thermal conductivity of the support substrate material is, for example, 100 W / km or more, preferably 150 W / km or more, and more preferably 200 W / km or more. Sometimes, depending on the application, an external device is connected to the composite substrate 100. In this case, if the inorganic material substrate 1 is heated by the external device, the heat from the inorganic material substrate 1 may adversely affect the external device. In this regard, if the support substrate material has such a thermal conductivity, the support substrate 6 can function as a heat sink, thereby effectively dissipating the heat from the inorganic material substrate 1.

[0115] The coefficient of linear expansion of the supporting substrate material is, for example, 0.1 × 10⁻⁶. -6 / K~20×10 -6 / K, preferably 0.3×10 -6 / K~10×10 -6 / K.

[0116] The thickness of the support substrate 6 is, for example, 150 μm to 1100 μm, preferably 250 μm to 600 μm.

[0117] B-5. Joint 4

[0118] In the example shown, the composite substrate 100 also includes a bonding portion 4. The bonding portion 4 is located between the dielectric film 3 and the support substrate 6, bonding them together.

[0119] The bonding strength between the dielectric film 3 and the supporting substrate 6 is, for example, 0.5 J / m.2 The above is preferably 1.0 J / m 2 That's all. On the other hand, the upper limit of the bonding strength between the dielectric film 3 and the supporting substrate 6 is typically 5.0 J / m. 2 It should be noted that the bond strength is determined, for example, using the crack opening method.

[0120] The joint 4 can be made of organic materials (typically organic adhesives) or inorganic materials. In one embodiment, the joint 4 is made of inorganic materials.

[0121] Examples of inorganic materials constituting the joint 4 (hereinafter sometimes referred to as joint materials) include, for example, the aforementioned support substrate material, the aforementioned dielectric material, and the aforementioned adhesive layer material. Joint materials may be used alone or in combination.

[0122] The joint 4 can have a single-layer structure or a stacked structure consisting of two or more layers. When the joint 4 has a stacked structure, it is composed of layers of different materials or materials of the same material but with different compositions and densities.

[0123] In one embodiment, the bonding portion 4 includes an amorphous layer 41 formed by direct bonding, as described later. In the example shown, the bonding portion 4 is composed of the amorphous layer 41.

[0124] The amorphous layer 41 is composed of the amorphous material of the bonding material described above. In one embodiment, the amorphous layer 41 includes the dielectric material described above, and / or the support substrate material described above.

[0125] If the bonding portion 4 includes an amorphous layer 41, the bonding strength between the dielectric film 3 and the support substrate 6 can be stably adjusted to the aforementioned range, and the thermal resistance of the bonding interface between the dielectric film 3 and the support substrate 6 can be significantly reduced compared to resin bonding. Therefore, even if an external device is connected to the composite substrate 100, and heat generated by the external device reaches the inorganic material substrate 1, such heat can be smoothly escaped from the inorganic material substrate 1 through the dielectric film 3 and the support substrate 6 to the package. As a result, the inorganic material substrate 1 can be efficiently cooled, thereby suppressing the degradation of the external device's characteristics.

[0126] The thickness of the joint 4 is, for example, 0.001 μm to 10 μm, preferably 0.01 μm to 3 μm.

[0127] B-6. First perforation 8a

[0128] One embodiment of the composite substrate 100 also includes a first through hole 8a.

[0129] The first through-hole 8a is typically electrically connected to the second conductor pattern 7, which will be described later. The number and arrangement of the first through-holes 8a are arbitrarily and appropriately designed according to the application of the composite substrate 100.

[0130] The first perforation 8a is made of any suitable conductive material. For example, the same material as the conductor material constituting conductor pattern 2 can be used as a conductor material, and metal is preferred.

[0131] The first through hole 8a is disposed within the through hole 12 formed in the inorganic material substrate 1. That is, the inorganic material substrate 1 has a through hole 12 corresponding to the first through hole 8a. The through hole 12 typically penetrates the inorganic material substrate 1 along the thickness direction.

[0132] The first through-hole 8a can have any suitable shape. Examples of shapes for the first through-hole 8a include: a pillar shape through which the inorganic material substrate 1 extends in the thickness direction, and a film shape formed on the entire inner surface of the through-hole 12. Alternatively, a conductive material can be further filled inside the conductive film formed on the entire inner surface of the through-hole 12, thereby forming a first through-hole 8a with a pillar shape.

[0133] In the example shown, the first perforation 8a has a column shape extending along the thickness direction of the inorganic material substrate 1. The first perforation 8a has a first end located on the side of the first substrate surface 15 of the inorganic material substrate 1, and a second end located on the side of the second substrate surface 16 of the inorganic material substrate 1.

[0134] The first end of the first perforation 8a may be flush with the first portion 15a of the first substrate surface 15, or it may protrude from the first portion 15a of the first substrate surface 15, or it may be located on the opposite side of the supporting substrate 6 relative to the first portion 15a of the first substrate surface 15. In the example shown, the first end of the first perforation 8a protrudes from the first portion 15a of the first substrate surface 15 to form a step 5.

[0135] The second end of the first through hole 8a may be flush with the surface 16 of the second substrate, or it may protrude from the surface 16 of the second substrate, or it may be located on the side of the supporting substrate 6 relative to the surface 16 of the second substrate. In the example shown, the second end of the first through hole 8a is flush with the surface 16 of the second substrate.

[0136] B-7. Second conductor pattern 7

[0137] like Figure 4 As shown, in one embodiment, the composite substrate 100 further includes a second conductor pattern 7. It should be noted that, hereinafter, the conductor pattern 2 located between the inorganic material substrate 1 and the support substrate 6 is sometimes referred to as the first conductor pattern 2.

[0138] The second conductor pattern 7 is located on the opposite side of the first conductor pattern 2 relative to the inorganic material substrate 1. The second conductor pattern 7 is typically disposed on the second substrate surface 16 of the inorganic material substrate 1. In the example shown, the second conductor pattern 7 is electrically connected to the first through-hole 8a.

[0139] The second conductor pattern 7 will be described in the same manner as the first conductor pattern 2, except for its placement in the composite substrate 100. Therefore, a detailed description of the second conductor pattern 7 is omitted.

[0140] B-8. Third conductor pattern 9 and second perforation 8b

[0141] In addition, the composite substrate 100 may further have a third conductor pattern 9 and a second through hole 8b.

[0142] The third conductor pattern 9 is located on the opposite side of the first conductor pattern 2 relative to the support substrate 6. The third conductor pattern 9 is typically disposed on the surface of the support substrate 6 on the opposite side of the first conductor pattern 2.

[0143] Regarding the third conductor pattern 9, except for its placement in the composite substrate 100, it will be described in the same manner as the first conductor pattern 2. Therefore, a detailed description of the third conductor pattern 9 will be omitted.

[0144] In one embodiment, the second through-hole 8b typically electrically connects the first conductor pattern 2, the second conductor pattern 7, and the third conductor pattern 9. The number and arrangement of the second through-holes 8b are arbitrarily and appropriately designed according to the application of the composite substrate 100.

[0145] The second perforation 8b is made of any suitable conductive material. For example, the same material as the conductor material constituting conductor pattern 2 can be used as a conductor material, and metal is preferred.

[0146] The second through-hole 8b is disposed within the second through-hole 13 formed in the composite substrate 100. That is, the composite substrate 100 has a second through-hole 13 corresponding to the second through-hole 8b. In the example shown, the second through-hole 13 passes through the second conductor pattern 7, the inorganic material substrate 1, the first conductor pattern 2, the dielectric film 3, the bonding portion 4, the support substrate 6, and the third conductor pattern 9.

[0147] The second through-hole 8b can have any suitable shape. Examples of the shape of the second through-hole 8b include: a pillar shape through which the composite substrate 100 extends in the thickness direction, and a film shape formed on the entire inner surface of the second through-hole 13. Alternatively, a second through-hole 8b with a pillar shape can be formed by further filling the inside of the conductive film formed on the entire inner surface of the second through-hole 13 with conductive material.

[0148] In the example shown, the second perforation 8b is a conductive film formed on the entire inner surface of the second perforation via 13.

[0149] B-9. Cavity 10

[0150] The composite substrate 100 may further include a void portion 10. The void portion 10 is located on the opposite side of the inorganic material substrate 1 relative to the conductor pattern 2. In the example shown, the void portion 10 is located on the opposite side of the first conductor pattern 2 relative to the dielectric film 3. The support substrate 6 may have a recess corresponding to the void portion 10.

[0151] C. Manufacturing method of composite substrate

[0152] Next, refer to Figures 5 to 9 The manufacturing method of the composite substrate according to another aspect of the present invention will be described.

[0153] In one embodiment, the method for manufacturing a composite substrate includes: a preparation step of an inorganic material substrate 1 having a recess 11, a conductor pattern 2 formation step, a dielectric film 3 formation step, and a bonding step of the dielectric film 3 and a support substrate 6.

[0154] like Figure 5 As shown, in the preparation process of the inorganic material substrate 1 with the recess 11, firstly, an etching mask (not shown) with a predetermined pattern shape is formed on the first substrate surface 15 of the inorganic material substrate 1, which has a generally flat shape.

[0155] The etching mask exposes the portion corresponding to the recess 11 in the inorganic material substrate 1, while covering the remaining portion. Additionally, the etching mask may, as needed, expose the portion corresponding to the first through-hole 12.

[0156] Subsequently, the inorganic material substrate 1 is etched using any suitable etching method with the aid of an etching mask. For example, reactive ion etching (RIE) can be cited as an etching method.

[0157] Thus, a recess 11 with a patterned shape is formed on the inorganic material substrate 1, and through holes 12 are formed as needed.

[0158] Next, in the process of forming conductor pattern 2, conductor pattern 2 is formed by embedding it into recess 11. In addition, in the process of forming conductor pattern 2, conductor pattern 2 and first through hole 8a are formed as needed.

[0159] In one implementation, such as Figure 6As shown, the aforementioned etch mask is removed, and the aforementioned conductor material is deposited on the entire surface 15 of the first substrate (first portion 15a and second portion 15b (inner surface of recess 11)) using any suitable film-forming method. Thus, a conductor film 20 is formed. If the inorganic material substrate 1 has a first through-hole 12, a first through-hole 8a can be formed inside the first through-hole 12 simultaneously with the formation of the conductor film 20.

[0160] Examples of film-forming methods include electroplating and electroless plating, with electroplating being a preferred method.

[0161] Next, the conductor film 20 is polished from the side opposite to the inorganic material substrate 1 using any appropriate polishing method.

[0162] Examples of grinding methods include: grinding (grinding apparatus), fine grinding, and chemical mechanical polishing (CMP). Grinding methods can be performed individually or in combination of two or more.

[0163] The grinding process is performed until a first portion 15a of the first substrate surface 15 of the inorganic material substrate 1 is exposed. Accordingly, a portion of the conductor film 20 embedded in the recess 11 becomes the conductor pattern 2, and the conductor pattern 2 and the first portion 15a of the first substrate surface 15 exposed from the conductor pattern 2 are ground together.

[0164] Therefore, as Figure 7 As shown, the aforementioned step 5 is formed through the conductor surface 2a of the conductor pattern 2 and the first portion 15a of the first substrate surface 15.

[0165] When the conductor material constituting the conductor pattern 2 is harder than the inorganic material constituting the inorganic material substrate 1, the inorganic material substrate 1 is easier to grind than the conductor pattern 2. Therefore, the conductor surface 2a of the conductor pattern 2 is located on the opposite side of the second substrate surface 16 relative to the first portion 15a of the first substrate surface 15.

[0166] In addition, such as Figure 8 As shown, when the conductor material constituting the conductor pattern 2 is softer than the inorganic material constituting the inorganic material substrate 1, the conductor pattern 2 is easier to grind than the inorganic material substrate 1. In this case, the conductor surface 2a of the conductor pattern 2 is located on the side of the second substrate surface 16 relative to the first portion 15a of the first substrate surface 15.

[0167] It should be noted that the shape of step 5 can be changed not only according to the hardness difference between conductor pattern 2 and inorganic material substrate 1, but also according to the chemical reactivity in CMP.

[0168] The formation process of such a conductor pattern 2 is not limited to the method described above. For example, the conductor material can be formed using the film-forming method described above without removing the etching mask described above. Thus, a conductor pattern 2 embedded in the recess 11 is formed. In this case, after removing the etching mask, the conductor pattern 2 and the first portion 15a of the first substrate surface 15 are polished using the polishing method described above to form a step 5.

[0169] Next, as Figure 9 As shown, in the process of forming the dielectric film 3, the dielectric film 3 is formed on the surface 15 of the first substrate by covering the steps 5. In one embodiment, the dielectric material is formed by covering the first substrate surface 15 of the inorganic material substrate 1 and the conductor surface 2a of the conductor pattern 2. Thus, a dielectric film 3 covering the steps 5 is formed.

[0170] Any suitable film-forming method can be used. Examples of film-forming methods include sputtering, chemical vapor deposition (CVD), evaporation, sol-gel method, and aerosol deposition (AD method), with sputtering being a preferred example.

[0171] Next, as Figure 1 As shown, in the bonding process of dielectric film 3 and support substrate 6, support substrate 6 is bonded to the side opposite to inorganic material substrate 1 relative to dielectric film 3 using any appropriate bonding method.

[0172] Examples of bonding methods include resin bonding using organic materials (representatively organic adhesives) and direct bonding.

[0173] In one embodiment, the dielectric film 3 and the support substrate 6 are directly bonded. In this specification, "direct bonding" means that two layers or substrates are joined without any organic material (typically an organic adhesive). The form of direct bonding can be appropriately determined according to the composition of the layers or substrates being bonded.

[0174] Direct bonding can be implemented, for example, in the following order.

[0175] First, as needed, the aforementioned bonding material is deposited on the surface of the dielectric film 3 and / or the support substrate 6 using the aforementioned film-forming method (preferably sputtering).

[0176] Then, in a high vacuum chamber (e.g., 1×10⁻⁶), -6 (Approximately Pa) irradiation of the bonding surfaces of the constituent elements (layers or substrates) to be bonded with a neutral beam. It should be noted that the bonding surfaces are planarized beforehand using grinding, as needed. Chemical mechanical polishing (CMP) is an example of such a polishing method.

[0177] The arithmetic mean roughness Ra of the mating surface that has been flattened by grinding is, for example, 0.0001 μm to 0.005 μm, preferably 0.0005 μm to 0.001 μm.

[0178] In one embodiment, during surface activation using a neutral beam, an inert gas is introduced into a chamber, and a high voltage is applied from a DC power supply to electrodes disposed within the chamber. With this configuration, electrons move due to the electric field generated between the electrodes (positive electrode) and the chamber (negative electrode), generating a beam of atoms and ions based on the inert gas. The ion beam reaching the grid is neutralized at the grid, thus the beam of neutral atoms is emitted from a high-speed atomic beam source. The atomic species constituting the beam are preferably inert gas elements (e.g., argon (Ar), nitrogen (N)). The voltage used for activation by beam irradiation is, for example, 0.5 kV to 2.0 kV, and the current is, for example, 50 mA to 200 mA. The irradiation time of the neutral beam is, for example, 10 seconds to 300 seconds, preferably 30 seconds to 120 seconds. Thus, each junction surface, more specifically the beam-irradiated surface, is activated.

[0179] Next, the activated mating surfaces are brought into contact with each other in a vacuum atmosphere at room temperature (23°C). The load at this contact can be, for example, 100N to 20000N.

[0180] Thus, a bonding portion 4 including an amorphous layer 41 is formed, and the dielectric film 3 and the support substrate 6 are bonded together by means of the bonding portion 4.

[0181] By directly bonding the inorganic material substrate 1 and the support substrate 6 without the aid of resin, the heat resistance and chemical resistance of subsequent manufacturing processes can be improved, thereby increasing the freedom of choice in the processing technology of the composite substrate 100. Furthermore, compared to the case where the bonding portion 4 contains organic material, the thermal expansion rate and water absorption rate of the bonding portion 4 can be reduced. As a result, the connection reliability between the inorganic material substrate 1 and the support substrate 6 can be improved, thereby enhancing the reliability of the composite substrate 100 exposed to the external environment.

[0182] Through the above operations, a laminate with the structure of inorganic material substrate 1 / conductor pattern 2 / dielectric film 3 / junction 4 / support substrate 6 can be obtained.

[0183] It should be noted that the direct bonding method is not limited to this; surface activation based on FAB (Fast Atom Beam) or ion gun, atomic diffusion, plasma bonding, etc., can also be applied.

[0184] The laminate is subjected to heat treatment as needed. This improves the bonding strength between the inorganic material substrate 1 and the support substrate 6. The heating temperature is, for example, 60°C to 140°C, preferably 80°C to 120°C. The heating time is, for example, 10 minutes to 5 hours, preferably 30 minutes to 3 hours.

[0185] In addition, other bonding methods can be used as a direct bonding method.

[0186] For example, into a high vacuum chamber (e.g., 1×10⁻⁶). -6 A high-speed atomic beam, using an inert gas such as Ar as the atomic species, is introduced into the bonding surface of one of the constituent elements (layers or substrates) at approximately 23°C. The bonding surface of this first constituent element is then irradiated with this high-speed atomic beam. The material of the first constituent element is then sputtered from this bonding surface onto the bonding surface of the other second constituent element as a sputtered layer. This sputtered layer is composed of the atoms constituting the first constituent element and can be a material mixed with inert gases or atoms contained in the device or fixture used. In this case, the sputtered layer can be an amorphous layer. Thus, a bonding layer composed of the material of the first constituent element is formed on the bonding surface of the second constituent element. Next, in a vacuum atmosphere at room temperature (23°C), the surface irradiated by the beam of the first constituent element and the surface of the bonding layer formed on the second constituent element are brought into contact and pressurized.

[0187] Thus, the first and second constituent elements can be joined together by means of a joint.

[0188] After bonding, amorphous layers of the first constituent element and the bonding layer and / or the second constituent element and the bonding layer may be formed respectively.

[0189] By employing this bonding method, the thickness of the bonding portion 4 can be reduced, thereby improving the bonding strength. Therefore, the heat dissipation and reliability of the composite substrate 100 as a device can be improved.

[0190] Through the above operations, composite substrate 100 is manufactured.

[0191] After that, as Figure 4 As shown, the second conductor pattern 7 and / or the third conductor pattern 9 can be formed using any suitable method as needed. Furthermore, the second through-hole 13 and the second through-hole 8b can also be formed using any suitable method.

[0192] Industrial availability

[0193] The composite substrates described in the embodiments of the present invention can be used in various industrial products, and are particularly preferred for use in multilayer substrates with electronic circuits.

[0194] Explanation of reference numerals in the attached figures

[0195] 1 Inorganic material substrate

[0196] 15 First substrate surface

[0197] 15a Part 1

[0198] 15b Part Two

[0199] 11 recess

[0200] 2. Conductor Pattern

[0201] 2a Conductor surface

[0202] 3. Dielectric membrane

[0203] 5 steps

[0204] 6 Supporting substrate

[0205] 100 composite substrate

Claims

1. A composite substrate comprising: An inorganic material substrate having a substrate surface with a recess, the substrate surface including a first portion located outside the recess and a second portion serving as the inner surface of the recess; A conductor pattern is embedded in the recess, and the conductor pattern together with the first portion of the substrate surface forms a step; A dielectric film disposed on the surface of the substrate in such a manner as to cover the steps; as well as A support substrate is located on the opposite side of the inorganic material substrate relative to the dielectric film, and the support substrate is bonded to the dielectric film.

2. The composite substrate according to claim 1, wherein, The conductor pattern has conductor surfaces that form the steps. The distance between the first portion of the substrate surface and the conductor surface in the thickness direction of the inorganic material substrate is 0.01 μm to 2.0 μm.

3. The composite substrate according to claim 2, wherein, The conductor surface is located on the side of the supporting substrate that is closer to the first portion of the substrate surface.

4. The composite substrate according to claim 2, wherein, The first portion of the substrate surface is located on the side of the supporting substrate that is closer to the conductor surface.

5. The composite substrate according to any one of claims 1 to 4, wherein, The thickness of the conductor pattern is 1.5 μm or more.

6. The composite substrate according to any one of claims 1 to 4, wherein, The inorganic material substrate is made of quartz glass.

7. The composite substrate according to any one of claims 1 to 4, wherein, The thickness of the inorganic material substrate is less than 100 μm.

8. The composite substrate according to any one of claims 1 to 4, wherein, The supporting substrate is made of Si, AlN, SiC, low-temperature co-fired ceramic, diamond, or Si3N4.

9. A method for manufacturing a composite substrate, comprising the following steps: Prepare an inorganic material substrate with a substrate surface having recesses; A conductor pattern is formed and implanted into the recess; The conductor pattern and the first portion of the substrate surface located outside the recess are ground to form a step through the conductor pattern and the first portion of the substrate surface; An dielectric film is disposed on the substrate surface in such a way that the steps are covered; as well as A support substrate is bonded to the side opposite to the inorganic material substrate, relative to the dielectric film.

Citation Information

Patent Citations

  • Semiconductor device

    JP2023010103A