Airtight device shell based on parallel seam welding assembly
Through split design and parallel seam welding assembly technology, the problems of high-temperature welding deformation and inconvenient design of traditional device shells are solved, and a miniaturized, lightweight and highly reliable airtight shell is achieved, which is suitable for aerospace, aviation and other fields. .
Patent Information
- Application Number
- CN202420150587.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2034-01-22
AI Technical Summary
The all-metal airtight device shell assembled by traditional parallel seam welding is easily deformed during high-temperature sintering and vacuum brazing processes, and the integrated design is inconvenient for internal assembly, replacement, and repair, making it difficult to achieve miniaturization and lightweight.
The split design of the base plate, frame and cover is adopted, and the device shell is realized through parallel seam welding assembly process. There are sintering holes and welding holes on the base plate or cover plate, and the signal pins and grounding pins are sintered and soldered respectively. Fixed to avoid deformation of the frame during high temperature, and to achieve flexible combination of multiple pin-in methods.
It has achieved a miniaturized and lightweight shell design with good air tightness and excellent full electromagnetic shielding performance, which facilitates internal assembly, replacement and repair, reduces the risk of high-temperature welding deformation, and meets high reliability requirements in aerospace, aviation and other fields.
Smart Images

Figure CN221805807U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the field of device manufacturing, in particular to an airtight device housing assembled based on parallel seam welding. Background Art
[0002] As switching power converters develop towards miniaturization, high frequency, and high power density, electronic equipment urgently requires LC filters (Lumped Component Fitler), EMI filters (Electromagnetic Fitler) and other devices to be miniaturized, lightweight, and have high electromagnetic shielding capabilities. High-reliability projects such as aerospace and aviation also require devices to have good airtightness and high reliability.
[0003] The traditional all-metal, airtight packaged device housing assembled by parallel seam welding is generally realized by the shell and cover plate, or the cap and base. If the shell is realized by the shell and cover plate, the pins can be distributed at the bottom and side walls. If the shell is realized by the cap and base, the pins are distributed at the bottom. The signal pins are assembled by insulator sintering, and the ground pins are assembled by vacuum brazing. Both assembly processes need to be completed under very high temperature conditions. In order to avoid deformation of the shell or base during the sintering of the signal pins and the vacuum brazing of the ground pins, it needs to be designed to be thick enough. In addition, this integrated design is not convenient for internal assembly, replacement, debugging, and subsequent rework and repair of devices. In addition, it is not convenient to realize a shell with pins coming out from the top.
[0004] Therefore, it is proposed that the shell adopts a split design scheme of a base plate, a frame, and a cover plate, and adopts parallel seam welding assembly process packaging technology to realize the device shell, that is, the base plate and the frame, the frame and the cover plate are assembled together by parallel seam welding, which can not only meet the requirements of high reliability, good airtightness, good full electromagnetic shielding performance, and miniaturization and light weight, but also avoid the various shortcomings of the traditional parallel seam welding assembly of the all-metal, airtight packaging device shell integrated design, and also facilitate internal assembly, replacement, debugging and subsequent rework and repair. If the bottom pin is used, the bottom plate is locally thickened at the sintered insulator, and only the bottom plate participates in the high-temperature sintering of the signal pin and the vacuum brazing process of the ground pin, reducing the risk of deformation of the frame during high-temperature sintering and brazing. The frame and the cover plate can be as thin as possible on the premise of meeting the strength requirements to meet the needs of miniaturization and light weight. If the pin is inserted at the top, the cover plate is partially thickened at the sintered insulator, and only the cover plate participates in the high-temperature sintering of the signal pin and the vacuum brazing process of the ground pin, reducing the risk of deformation of the frame during high-temperature sintering and brazing. The frame and the bottom plate can be thinned as much as possible on the premise of meeting the strength requirements to meet the needs of miniaturization and lightweight. If the pin is inserted at the side, the cover plate is partially thickened at the sintered insulator, and only the frame participates in the high-temperature sintering of the signal pin and the vacuum brazing process of the ground pin, avoiding the problem of deformation of the bottom plate during high-temperature sintering and brazing. The bottom plate and the cover plate can be thinned as much as possible on the premise of meeting the strength requirements to meet the needs of miniaturization and lightweight. Taking the side pin insertion device shell of the split solution as an example, if the subsequent device product fails and needs to be repaired, first analyze and determine that if the components on the front of the PCB board fail, then open the cover plate for repair, and if the components on the bottom of the PCB board fail, then open the bottom plate for repair, which is very convenient. In addition, the shell adopts a split design of base plate, frame and cover plate, which makes it easy to realize a shell with lead pins at the bottom, side and top. The three lead pin methods can be flexibly combined as needed to better meet application requirements. Utility Model Content
[0005] The technical problem to be solved by the utility model is to provide an airtight device housing assembled based on parallel seam welding, which effectively overcomes the defects of the prior art.
[0006] The technical solution of the utility model to solve the above technical problems is as follows:
[0007] A hermetic device housing assembled based on parallel seam welding, comprising an annular frame and a cover plate and a bottom plate horizontally arranged in the frame with upper and lower intervals, the edges of the bottom plate and the cover plate are assembled and fixed to the inner wall of the frame along the direction of the gap by parallel seam welding; the bottom plate or the cover plate is provided with a first sintering hole passing through it from top to bottom, and an annular insulator embryo is sintered and fixed in the first sintering hole, and a signal lead pin sintered and fixed to it is penetrated in the insulator embryo, or the side wall of the frame is provided with a second sintering hole passing through it horizontally, and an annular insulator embryo is sintered and fixed in the second sintering hole.
[0008] On the basis of the above technical solution, the present invention can also be improved as follows.
[0009] Furthermore, the upper surface of the base plate is provided with a first groove for accommodating tall components, and the lower surface of the cover plate is provided with a second groove for accommodating tall components.
[0010] Furthermore, the above-mentioned base plate and cover plate are rectangular, square, circular or elliptical. If they are rectangular or square, the four right angles of the above-mentioned base plate and cover plate are rounded or set to right angles; the corresponding above-mentioned frame is rectangular, square, circular or elliptical. If it is rectangular or square, the four right angles of the outer wall of the above-mentioned frame are rounded or set to right angles, and the four corners of the inner wall are rounded; the above-mentioned insulator blank is circular or elliptical, and the above-mentioned insulator blank is provided with a single or multiple matching signal pins, and the cross-section of the above-mentioned signal pin is circular, elliptical, square, rectangular or trapezoidal.
[0011] Further, when the thickness of the above-mentioned bottom plate is greater than 0.15mm, the above-mentioned bottom plate is surrounded by a first edge with a thickness less than its thickness, and the above-mentioned first edge is assembled and fixed by seam welding in parallel to the inner wall of the above-mentioned frame, otherwise the edge on the bottom plate is directly assembled and fixed by seam welding in parallel to the bottom end of the side wall of the frame; when the thickness of the above-mentioned cover plate is greater than 0.15mm, the above-mentioned cover plate is surrounded by a second edge with a thickness less than its thickness, and the above-mentioned second edge is assembled and fixed by seam welding in parallel to the inner wall of the above-mentioned frame, otherwise the edge of the cover plate is directly assembled and fixed by seam welding in parallel to the top end of the side wall of the frame.
[0012] Furthermore, the above-mentioned bottom plate, cover plate and surrounding frame are all metal plates, and their material and surface treatment meet the requirements of parallel welding process.
[0013] Furthermore, the bottom plate, the cover plate, or the side wall of the surrounding frame may be provided with grounding pins according to the use requirements, and the grounding pins may be machined into one piece or assembled by brazing.
[0014] Further, if the grounding pin is assembled by a brazing process, the above-mentioned base plate or cover plate is provided with a first welding hole, which is a through hole that penetrates from top to bottom, or a non-penetrating half hole, and a double-sided pin-type grounding pin that is welded and fixed to the through hole is vertically penetrated through the through hole that penetrates from top to bottom, and a single-sided pin-type grounding pin that is welded and fixed to the through hole is vertically inserted into the non-penetrating half hole; or the side wall of the above-mentioned frame is provided with a second welding hole, which is a horizontally penetrating through hole, and a double-sided pin-type grounding pin that is welded and fixed to the through hole is horizontally penetrated through the second welding hole, or the second welding hole is a non-penetrating half hole, and a single-sided pin-type grounding pin that is welded and fixed to the through hole is horizontally inserted into the second welding hole.
[0015] Furthermore, the signal pins are distributed on the side walls of the bottom plate or the surrounding frame; the ground pins are distributed on the side walls of the bottom plate, the cover plate, or the surrounding frame.
[0016] Furthermore, the upper surface of the bottom plate corresponding to the first sintering hole and the first welding hole is provided with a first structural reinforcement portion; or the inner wall of the frame corresponding to the second sintering hole and the second welding hole is provided with a second structural reinforcement portion.
[0017] The beneficial effects of the utility model are as follows: the split design is easy to process; the shell of this split design can have three pin-in methods, namely, pin-in at the bottom, top and side of the shell, and multiple surfaces are very convenient for extending the pins, that is, the three pin-in methods can be flexibly combined according to needs, which can better meet application requirements; the risk of deformation caused by high temperature during sintering of insulators or soldering of pins can be reduced; the bottom plate and the cover plate are easy to disassemble and assemble, which is convenient for the assembly, replacement and debugging of components; it is conducive to the later rework and repair of the device; it has good air tightness and can meet the high reliability requirements of aerospace and aviation. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a cross-sectional view of a bottom plate of a bottom pin-leading method in a gas-tight device housing assembled based on parallel seam welding of the utility model;
[0019] Figure 2 It is a top view of the bottom plate of the bottom pin-leading method in the airtight device housing assembled based on parallel seam welding of the utility model;
[0020] Figure 3 It is a cross-sectional view of a surrounding frame without lead pins in the airtight device housing assembled based on parallel seam welding of the utility model;
[0021] Figure 4 It is a top view of a surrounding frame without lead pins in the airtight device housing assembled based on parallel seam welding of the utility model;
[0022] Figure 5It is a cross-sectional view of a surrounding frame of side lead pins in a gas-tight device housing assembled based on parallel seam welding of the utility model;
[0023] Figure 6 It is a top view of a surrounding frame of side lead pins in a gas-tight device housing assembled based on parallel seam welding of the utility model;
[0024] Figure 7 It is a cross-sectional view of a bottom plate without lead pins in a gas-tight device housing assembled based on parallel seam welding of the utility model;
[0025] Figure 8 It is a top view of a bottom plate without lead pins in a gas-tight device housing assembled based on parallel seam welding of the utility model;
[0026] Fig. 9 It is a cross-sectional view of a cover plate in a gas-tight device housing assembled based on parallel seam welding of the utility model;
[0027] Fig.10 A bottom view of a cover plate in an airtight device housing assembled based on parallel seam welding according to the utility model;
[0028] Fig.11 It is a cross-sectional view of the first lead pin sintered graphite tooling in the airtight device housing assembled based on parallel seam welding of the utility model;
[0029] Fig.12 It is a top view of the first lead pin sintered graphite tooling in the airtight device housing assembled based on parallel seam welding of the utility model;
[0030] Fig.13 It is a cross-sectional view of the second lead pin sintered graphite tooling in the airtight device housing assembled based on parallel seam welding of the utility model;
[0031] Fig.14 It is a top view of the second lead pin sintered graphite tooling in the airtight device housing assembled based on parallel seam welding of the utility model;
[0032] Fig.15 It is a finished cross-sectional view of the bottom plate of the bottom lead pin in the airtight device housing assembled based on parallel seam welding of the utility model;
[0033] Fig.16 It is a sectional view of a finished product of a surrounding frame for side lead pins in a gas-tight device housing assembled based on parallel seam welding of the utility model;
[0034] Fig.17 This is a structural diagram of an insulator stamping die involved in the airtight device housing assembled based on parallel seam welding of the utility model;
[0035] Fig.18This is a structural diagram of an insulator in an airtight device housing assembled based on parallel seam welding according to the utility model;
[0036] Fig.19 The present invention is a flow chart of the preparation process of an airtight device housing based on parallel seam welding assembly.
[0037] In the accompanying drawings, the components represented by the reference numerals are listed as follows:
[0038] 1. Base plate; 2. Cover plate; 3. Frame; 4. Insulator blank; 5. Signal pin; 6. Ground pin; 11. First groove; 12. First sintering hole; 13. First welding hole; 21. Second groove; 31. Second sintering hole; 32. Second welding hole; 111. First edge; 113. First structural reinforcement; 211. Second edge; 311. Second structural reinforcement. DETAILED DESCRIPTION
[0039] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0040] Example
[0041] like Figures 1 to 18 As shown, the airtight device housing based on parallel seam welding assembly of this embodiment includes an annular frame 3 and a cover plate 2 and a base plate 1 horizontally arranged at both ends of the frame 3 with upper and lower intervals, and the edges of the base plate 1 and the cover plate 2 are assembled and fixed to the inner wall of the frame 3 along the direction of the gap by parallel seam welding; the base plate 1 or the cover plate 2 is provided with a first sintering hole 12 passing through it from top to bottom, and the first sintering hole 12 is sintered and fixed with an annular insulator blank 4, and the insulator blank 4 is penetrated with a signal lead pin 5 sintered and fixed thereto, or the side wall of the frame 3 is provided with a second sintering hole 31 passing through it horizontally, and the second sintering hole 31 is sintered and fixed with an annular insulator blank 4.
[0042] In this embodiment, the base plate 1, the cover plate 2 or the surrounding frame 3 are provided with a grounding pin 6 (wherein the grounding pin 6 can be provided as a single-sided or double-sided pin according to the use requirements; the grounding pin 6 can be directly machined into one piece or assembled by brazing process, but the former is more expensive and is also limited by factors such as the diameter and length of the pin).
[0043] There are two types of grounding pin 6, one is a double-sided pin-type grounding pin. If brazing is used for assembly, a first welding hole 13 (for assembly of double-sided pins) is provided on the bottom plate 1 or the cover plate 2, which is a through hole that penetrates from top to bottom. The other is a single-sided pin-type grounding pin. If brazing is used for assembly, a half hole that does not penetrate from top to bottom is provided on the bottom plate 1, namely, a first welding hole 13 (for assembly of single-sided pins). A grounding pin 6 is vertically penetrated or inserted in the first welding hole 13 and is welded and fixed thereto. Similarly, the grounding pin 6 can be arranged on the side wall of the enclosure. If brazing is used for assembly, a through hole (second welding hole 32) that penetrates thereto horizontally is provided on the side wall of the enclosure 3, which is used to install the double-sided pin-type grounding pin. A half hole (second welding hole 32) that does not penetrate thereto horizontally is provided on the side wall of the enclosure 3, which is used to install the single-sided pin-type grounding pin. A grounding pin 6 is penetrated or inserted in the second welding hole 32 and is welded and fixed thereto.
[0044] Specifically, Fig.19 As shown, the preparation process of the airtight device housing based on parallel seam welding assembly includes the following steps:
[0045] Step 1: Manufacturing insulator blanks:
[0046] S1. Put glass powder or ceramic powder into an insulator stamping die to punch out an insulator green body;
[0047] More specifically, (1) taking the use of glass powder to manufacture insulator blanks as an example, first select a glass powder formula, for example, granulate the glass powder with a 4% polyvinyl alcohol solution, select glass powder with a diameter of 35-80 microns for drying, mix the glass powder: paraffin wax: oleic acid in a ratio of 50:10:1, wherein the paraffin wax is a binder and the oleic acid is a release agent, and heat and fully stir to make a glass powder rough blank; (2) Fig.17 As shown, the rough glass powder blank is placed in the groove 102 of the lower die 10 of the insulator stamping die (a stamping seat 101 is arranged at the bottom of the groove 102), and the groove 102 is required to be filled and compacted with the rough glass powder blank, and then the punch 91 of the upper die 9 of the insulator stamping die is used to punch out the green blank of the insulator;
[0048] S2, put the insulator green body into the sintering furnace for sintering, and obtain the insulator cooked body D (such as Fig.18 shown);
[0049] Step 2: Pin assembly:
[0050] For the bottom pin method, the assembly method is: first pre-treat the surface of the bottom plate 1, install the bottom plate 1 into the first pin sintered graphite tooling ( Fig.11 , Fig.12A in the figure indicates that the upper end of the tooling is provided with a first accommodating groove a1 for accommodating the base plate 1, and the bottom of the groove is provided with a first slot a2 adapted to the signal lead pin 5 and the ground lead pin 6). If the sintering assembly temperature of the insulator embryo and the base plate is higher than the vacuum brazing temperature of the ground lead pin, the insulator embryo is loaded into the corresponding first sintering hole 12 of the base plate 1, and the signal lead pin 5 is inserted into the insulator embryo, and the insulator embryo is put into the sintering furnace for the second sintering to complete the assembly of the signal lead pin 5; thereafter, if the first welding hole 13 on the base plate is a through hole that penetrates from top to bottom, the base plate 1 is loaded into the first lead pin sintering graphite tooling, and a silver-copper welding ring is placed in the first welding hole 13 on the base plate 1; if the first welding hole 13 on the base plate is a half hole that does not penetrate from top to bottom, a silver-copper welding ring is placed in the first welding hole 13 on the base plate or silver-copper solder is coated, the base plate is loaded into the first lead pin sintering graphite tooling, and then the ground lead pin 6 is penetrated or inserted into the first welding hole 13, and the assembly of the ground lead pin 6 is completed by vacuum brazing (such as Figure 2 The first welding hole 13 shown in the figure has a through hole that penetrates from top to bottom and a half hole that does not penetrate from top to bottom. The through hole welding hole is used to assemble the double-sided lead-in type grounding lead-in pin, and the half hole welding hole is used to assemble the single-sided lead-in type grounding lead-in pin; the assembled single-sided lead-in type grounding pin is as shown in FIG. Fig.15 6); if the sintering assembly temperature of the insulator embryo and the bottom plate is lower than the vacuum brazing temperature of the ground pin 6, the ground pin 6 is first assembled by vacuum brazing, and then the sintering assembly of the insulator embryo, the signal pin and the bottom plate is completed; wherein, the assembly sequence of the surrounding frame 3 and the bottom plate 1, and the surrounding frame 3 and the cover plate 2 can be adjusted according to the characteristics of the device production process;
[0051] For the top pin-in method, the pins are assembled on the cover plate 2 in accordance with the above bottom pin-in method;
[0052] For the side lead-in method, the assembly method is: first pre-treat the surface of the frame 3, and then install the frame 3 into the second lead-in sintered graphite tooling ( Fig.13 , 14B indicates that the upper end of the tooling is provided with a second receiving groove b1 for accommodating the enclosure 3, and the side walls of the second receiving groove b1 are respectively provided with second slots b2 adapted to the signal lead pin 5 and the ground lead pin 6). If the sintering assembly temperature of the insulator embryo and the enclosure is higher than the vacuum brazing temperature of the ground lead pin, the insulator embryo is installed into the corresponding second sintering hole 31 of the enclosure 3, and the signal lead pin 5 is inserted into the insulator embryo, and the insulator embryo is placed in the sintering furnace for the second sintering to complete the assembly of the signal lead pin 5; thereafter, the enclosure 3 is installed in the second lead pin sintering graphite tooling, if the second welding hole 32 on the enclosure is a horizontal through hole, a silver-copper soldering ring is placed in the second welding hole 32 on the enclosure 3, if the second welding hole on the enclosure is a horizontal non-penetrating half hole, a silver-copper soldering ring is placed in the second welding hole of the enclosure or silver-copper solder is applied, and then the ground lead pin 6 is inserted or inserted into the second welding hole 32, and the ground lead pin 6 is assembled by vacuum brazing (the assembled double-sided lead pin type ground pin is as shown in FIG. Fig.16 6); if the sintering assembly temperature of the insulator embryo and the surrounding frame is lower than the vacuum brazing temperature of the ground pin 6, the ground pin 6 is assembled by vacuum brazing first, and then the insulator embryo, the signal pin 5 and the surrounding frame 3 are assembled by sintering; wherein, the assembly sequence of the surrounding frame 3 and the bottom plate 1, and the surrounding frame 3 and the cover plate 2 can be adjusted according to the characteristics of the device production process;
[0053] Step 3: Use a leak detector to test the air tightness of the sintering of the insulator and the brazing of the grounding pin:
[0054] Step 4: Complete the final surface treatment of the bottom plate, cover plate and frame. If the surface treatment method of the lead pins is different from that of the shell, the lead pins (ground lead pin 6 and signal lead pin 5) need to be surface treated separately after the shell is surface treated.
[0055] Step 5: Assembly of internal components and PCB boards:
[0056] For the bottom pin-in method: Method 1 is to assemble the bottom plate 1 and the surrounding frame 3 together by parallel welding, and then assemble the internal components and PCB boards, and then debug, clean, test, and perform internal three-proofing, and perform internal potting or gluing when necessary; Method 2 is to complete the assembly of internal components and PCB boards on the bottom plate, and then debug, clean, test, perform internal three-proofing, and properly glue the inside when necessary, and then assemble the bottom plate and the surrounding frame together by parallel welding, and perform internal potting when necessary;
[0057] For the top pin-in method: refer to the above bottom pin-in method for assembly;
[0058] For the side lead method: after completing the assembly of components, PCB boards, etc. in the enclosure 3, debugging, cleaning, testing, internal three-proofing, potting or bonding when necessary, the enclosure 3 and the base plate 1 are assembled together by parallel welding (the assembly sequence can be adjusted according to the characteristics of the device production process);
[0059] Step 6: Assemble the frame 3 and the cover plate 2 or the bottom plate 1 together by parallel welding, use laser marking equipment to set a mark on the surface of the packaged device product (specifically, use laser to set the mark), and finally apply a protective agent to the outer surface (specifically, use a thin film protective agent or a three-conformal paint, or a combination of thin film protective agent coating and three-conformal paint coating according to the application of the device);
[0060] Step 7: Final test.
[0061] In this embodiment, the bottom plate 1, the cover plate 2 and the surrounding frame 3 are designed to be split, and then assembled by parallel seam welding, which has the following advantages:
[0062] First, the front and back sides of the PCB board inside the shell are convenient for assembly, replacement and debugging of components; second, it is conducive to the later rework and repair of the device, because the cover plate 2 and the bottom plate 1 assembled by parallel seam welding can be reworked and repaired. Taking the device shell with side pin insertion as an example, if the component on the front of the PCB board fails, the cover plate 2 is opened for rework and repair, and if the component on the bottom of the PCB board fails, the bottom plate 1 is opened for rework and repair, which is very convenient. Third, the shell of this split design can have three pin-in methods, namely, pin-in at the bottom, top and side of the shell, and it is very convenient to extend the pins from all six sides, that is, the three pin-in methods can be flexibly combined according to needs, which can better meet application requirements; Fourth, the shell adopts a split design of base plate 1, frame 3, and cover plate 2. The sintering of signal pin 5 adopts the high-temperature sintering process of insulator, and the ground pin 6 is assembled by vacuum brazing process. Compared with the ground pin formed by one-piece machining, the brazing process assembly is not limited to the diameter and length of the ground pin 6, and has strong versatility and low cost. If the bottom lead pin method is adopted, the assembly place of the insulator signal pin and the ground pin of the bottom plate is locally thickened, and the bottom plate participates in the high temperature sintering of the signal lead pin and the vacuum brazing process of the ground lead pin, so as to avoid the deformation of the frame during the warm sintering and brazing process. If the side lead pin method is adopted, the assembly place of the insulator signal pin and the ground pin of the frame is locally thickened, and the frame participates in the high temperature sintering of the signal lead pin and the vacuum brazing process of the ground lead pin, so as to avoid the deformation of the bottom plate during the high temperature sintering and brazing process. If the size and length of the ground lead pin 6 meet the process requirements of mechanical processing, it can also be directly machined into one piece, so as to further avoid the deformation risk caused by the brazing process. The frame 3 and the bottom plate 1, the frame 3 and the cover plate 2 are assembled together by a parallel seam welding process, which adopts a method combining a variety of commonly used mature processes, and realizes the design and preparation method of the airtight device housing based on parallel seam welding assembly. The method has the characteristics of being simple and easy to operate, low cost, high yield rate, good sealing performance, high reliability, strong versatility, etc., and can meet the high reliability requirements of aerospace and aviation. In addition, there is more operating space when assembling internal components, and it is convenient for subsequent rework and repair of finished products.
[0063] As a preferred embodiment, the upper surface of the base plate 1 is provided with a first groove 11 for accommodating tall components, and the lower surface of the cover plate 2 is provided with a second groove 21 for accommodating tall components.
[0064] In the above embodiment, by respectively providing the first groove 11 and the second groove 21 on the base plate 1 and the cover plate 2, it is convenient to install high components such as chokes and inductors in the grooves, effectively utilize the internal space, and at the same time, reduce the overall height and weight of the device package.
[0065] In this embodiment, the above-mentioned base plate 1 and cover plate 2 are rectangular, square, circular or elliptical. If they are rectangular or square, the four right angles of the above-mentioned base plate 1 and cover plate 2 are chamfered or set to right angles; the corresponding above-mentioned frame 3 is rectangular, square, circular or elliptical. If it is rectangular or square, the four right angles of the outer wall of the above-mentioned frame 3 are chamfered or set to right angles, and the four corners of the inner wall are all rounded; the above-mentioned insulator blank 4 is circular or elliptical, and the above-mentioned insulator blank 4 is provided with a single or multiple matching signal pins 5, and the cross-section of the above-mentioned signal pin 5 is circular, elliptical, square, rectangular or trapezoidal.
[0066] It should be noted that the shapes of the base plate 1, cover plate 2, frame 3, insulator 4, and the cross-sectional profile shapes of the signal pin 5 and ground pin 6 can be set to other shapes according to actual needs in addition to the above shapes.
[0067] As a preferred embodiment, when the thickness of the above-mentioned base plate 1 is greater than 0.15mm, the above-mentioned base plate 1 needs to be provided with a first edge 111 with a thickness less than its thickness all around, and the above-mentioned first edge 111 is assembled and fixed by seam welding in parallel with the bottom end of the side wall of the above-mentioned frame 3, otherwise the edge of the base plate 1 is directly assembled and fixed by seam welding in parallel with the bottom end of the side wall of the frame 3; when the thickness of the above-mentioned cover plate 2 is greater than 0.15mm, the above-mentioned cover plate 2 needs to be provided with a second edge 211 with a thickness less than its thickness all around, and the above-mentioned second edge 211 is assembled and fixed by seam welding in parallel with the top end of the side wall of the above-mentioned frame 3, otherwise the edge of the cover plate 1 is directly assembled and fixed by seam welding in parallel with the top end of the side wall of the above-mentioned frame 3.
[0068] In the above implementation scheme, the design of the first edge 111 and the second edge 211 is mainly intended to make the device meet the strength requirements of use, and to meet the requirements of the parallel seam welding assembly process so that the finished product has good airtightness. In addition, the edges of the cover plate 2 and the bottom plate 1 adopt a convex edge design. The design of the first edge 111 and the second edge 211 meets the requirements of the parallel seam welding assembly process so that the finished product has good airtightness, ensuring that the sealing performance of the finished product meets the high reliability requirements of aerospace and aviation. At the same time, it can avoid deviation during parallel seam welding assembly. If the cover plate 2 and the bottom plate 1 are already very thin (for example, 0.10mm to 0.15mm), there is no need to adopt a convex edge design.
[0069] In this embodiment, the bottom plate 1, cover plate 2 and surrounding frame 3 are all metal plates. After being assembled together by parallel seam welding, the full electromagnetic shielding performance and air tightness are good.
[0070] In this embodiment, the ground pins 6 and the signal pins 5 are distributed at both ends of the bottom plate 1, or the ground pins 6 and the signal pins 5 are distributed on the side walls of the surrounding frame 3. The layout is relatively reasonable.
[0071] In this embodiment, one or more signal pins 5 can be provided according to the use requirements. Multiple settings can be arranged in one row or multiple rows and can be distributed on the above-mentioned base plate 1, frame 3, and cover plate 2. The layout position can be determined according to actual needs.
[0072] In this embodiment, the insulator blank 4 can be circular, elliptical or set to other shapes according to actual needs. A single insulator can be provided with a single or multiple matching lead pins, and the cross-section of the lead pin can be circular, elliptical, square, rectangular, trapezoidal or set to other shapes according to actual needs.
[0073] In the embodiment, one or more ground pins 6 may be provided according to the use requirements, and may be distributed on the bottom plate 1, the surrounding frame 3, and the cover plate 2. The layout position may be determined according to actual needs.
[0074] In the embodiment, the ground pin 6 can be configured as a single-side pin or a double-side pin according to usage requirements.
[0075] In the embodiment, the ground pin 6 can be directly machined into one piece or assembled by brazing.
[0076] In this embodiment, the upper surface of the base plate 1 corresponding to the first sintering hole 12 and the first welding hole 13 are both protrudingly provided with a first structural reinforcement portion 113. The first structural reinforcement portion 113 makes the base plate 1 thickened at the first sintering hole 12 and the first welding hole 13, and the structure is strengthened to avoid weakening the local structural strength due to the opening. The thickness of the remaining parts can be as thin as possible while meeting the strength requirements, thereby reducing the volume and weight of the shell; or the inner wall of the frame 3 corresponding to the second sintering hole 31 and the second welding hole 32 are both protrudingly provided with a second structural reinforcement portion 311. Similarly, the second structural reinforcement portion 311 makes the frame 3 thickened at the second sintering hole 31 and the second welding hole 32, and the structure is strengthened to avoid weakening the local structural strength due to the opening. The thickness of the remaining walls can be as thin as possible while meeting the strength requirements, thereby reducing the overall volume and weight of the shell.
[0077] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0078] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present utility model, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0079] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0080] In the present utility model, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0081] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the utility model. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0082] Although the embodiments of the present invention have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations of the present invention. Ordinary technicians in the field can change, modify, replace and modify the above embodiments within the scope of the present invention.
Claims
1. A hermetic device housing assembled based on parallel seam welding, characterized in that: The invention comprises an annular enclosure (3) and a cover plate (2) and a bottom plate (1) which are horizontally arranged at both ends of the enclosure (3) with an interval between the upper and lower parts, wherein the edges of the bottom plate (1) and the cover plate (2) are assembled and fixed to the inner wall of the enclosure (3) along the direction of the gap by means of parallel seam welding; the bottom plate (1) or the cover plate (2) is provided with a first sintering hole (12) which passes through it from top to bottom, and an annular insulator blank (4) is sintered and fixed in the first sintering hole (12), and a signal lead pin (5) which is sintered and fixed in the insulator blank (4) is passed through the side wall of the enclosure (3), or a second sintering hole (31) which passes through it horizontally, and an annular insulator blank (4) is sintered and fixed in the second sintering hole (31).
2. The airtight device housing assembled based on parallel seam welding according to claim 1, characterized in that: The upper surface of the base plate (1) is provided with a first groove (11) for accommodating tall components, and the lower surface of the cover plate (2) is provided with a second groove (21) for accommodating tall components.
3. The airtight device housing assembled based on parallel seam welding according to claim 1, characterized in that: The base plate (1) and the cover plate (2) are rectangular, square, circular or elliptical. If they are rectangular or square, the four right angles of the base plate (1) and the cover plate (2) are rounded or set as right angles; the corresponding enclosure (3) is rectangular, square, circular or elliptical. If they are rectangular or square, the four right angles of the outer wall of the enclosure (3) are rounded or set as right angles, and the four corners of the inner wall are rounded; the insulator blank (4) is circular or elliptical, and the insulator blank (4) is provided with a single or multiple matching signal lead pins (5), and the cross-section of the signal lead pin (5) is circular, elliptical, square, rectangular or trapezoidal.
4. The airtight device housing assembled based on parallel seam welding according to claim 1, characterized in that: When the thickness of the bottom plate (1) is greater than 0.15 mm, the bottom plate (1) is surrounded by a first edge (111) having a thickness less than the bottom plate's thickness, and the first edge (111) is parallel to the bottom end of the side wall of the surrounding frame (3) and assembled and fixed by seam welding; otherwise, the edge of the bottom plate (1) is directly parallel to the bottom end of the side wall of the surrounding frame (3) and assembled and fixed by seam welding; when the thickness of the cover plate (2) is greater than 0.15 mm, the cover plate (2) is surrounded by a second edge (211) having a thickness less than the bottom plate's thickness, and the second edge (211) is parallel to the top end of the side wall of the surrounding frame (3) and assembled and fixed by seam welding; otherwise, the edge of the cover plate (2) is directly parallel to the top end of the side wall of the surrounding frame (3) and assembled and fixed by seam welding.
5. The airtight device housing assembled based on parallel seam welding according to claim 1, characterized in that: The bottom plate (1), the cover plate (2) and the surrounding frame (3) are all metal plates.
6. The airtight device housing assembled based on parallel seam welding according to claim 1, characterized in that: A grounding pin (6) is provided on the bottom plate (1), or the cover plate (2), or the side wall of the surrounding frame (3); the grounding pin (6) is machined into one piece or assembled using a brazing process.
7. The airtight device housing assembled based on parallel seam welding according to claim 6, characterized in that: The grounding pin (6) is assembled by a brazing process. A first welding hole (13) is provided on the bottom plate (1) or the cover plate (2). The first welding hole (13) is a through hole that penetrates vertically, or a half hole that does not penetrate vertically. A double-sided lead-in-type grounding pin (6) is vertically inserted through the through hole that penetrates vertically and is fixed to the through hole by welding. A single-sided lead-in-type grounding pin (6) is vertically inserted into the half hole that does not penetrate vertically. Alternatively, a second welding hole (32) is provided on the side wall of the enclosure (3). The second welding hole (32) is a through hole that penetrates horizontally. A double-sided lead-in-type grounding pin (6) is horizontally inserted through the second welding hole (32) and is fixed to the through hole by welding. Alternatively, the second welding hole (32) is a half hole that does not penetrate vertically. A single-sided lead-in-type grounding pin (6) is horizontally inserted into the second welding hole (32) and is fixed to the through hole by welding.
8. The airtight device housing assembled based on parallel seam welding according to claim 7, characterized in that: The signal pins (5) and / or the ground pins (6) are distributed on the side walls of the base plate (1) or the cover plate (2) or the surrounding frame (3).
9. The airtight device housing assembled based on parallel seam welding according to claim 7, characterized in that: A first structural reinforcement portion (113) is protrudingly provided at the portion of the upper surface of the bottom plate (1) corresponding to the first sintering hole (12) and the first welding hole (13); or a second structural reinforcement portion (311) is protrudingly provided at the portion of the inner wall of the surrounding frame (3) corresponding to the second sintering hole (31) and the second welding hole (32).