Microwave pultrusion system for resin matrix fiber reinforced composite material

By arranging a contoured cavity of absorbing material in the inner cavity of the microwave heating device, the problems of uneven temperature and high energy consumption in the production of resin-based fiber-reinforced composite materials are solved, achieving more efficient production and more stable production. Performance improvements.

CN221819552UActive Publication Date: 2024-10-11JIANGSU HENGRUI CARBON NEUTRALITY TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202420120288.5
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-01-18
Publication Date
2024-10-11
Estimated Expiration
2034-01-18

AI Technical Summary

Technical Problem

In the production process of existing resin-based fiber-reinforced composite materials, mold heating and oven heating have problems such as slow production speed, high energy consumption, large internal stress caused by uneven internal and external temperatures, and product quality problems. Microwave heating causes large temperature differences in the horizontal direction, resulting in poor product quality. Overheated or unshaped.

Method used

Design a microwave pultrusion system for resin-based fiber-reinforced composite materials, which uses a contoured cavity of absorbing material in the inner cavity of the microwave heating device to ensure that the temperature of the composite preform is maintained in the radial direction and the direction of the fiber bundle. Uniform and stable, the silicon carbide inner cavity wall plate absorbs microwaves to form a stable temperature area for curing.

Benefits of technology

The tensile strength, tensile modulus and double shear strength of the product are improved, the performance is more stable and uniform, the production speed is increased by 40-70%, the energy consumption is reduced, and the temperature fluctuation is controlled within 15°C, avoiding product overburning and Unformed problem.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221819552U_ABST
    Figure CN221819552U_ABST
Patent Text Reader

Abstract

The utility model discloses a microwave pultrusion system for a resin matrix fiber reinforced composite material, which comprises a creel, a gum dipping device, a preforming device, at least one group of microwave heating devices, a traction device and a cutting device which are arranged in sequence. An inner cavity is formed in a microwave cavity of the microwave heating device and comprises wall plates and a cavity defined by the wall plates. The wall plate is made of a silicon carbide material; the section size of the cavity is larger than that of a composite material product so that it can be guaranteed that the composite material can horizontally pass through the wallboard without making contact with the composite material product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of resin-based fiber-reinforced composite materials, in particular to a microwave pultrusion system for resin-based fiber-reinforced composite materials. Background Art

[0002] Reinforced concrete is the main material for infrastructure, and its durability is related to the quality and safety of infrastructure. For coastal infrastructure, chloride salts will cause steel corrosion, and the high temperature, high salt, and high humidity island and reef environment will also accelerate the corrosion and damage of steel. Therefore, durable marine engineering concrete is of great significance to the safety of coastal and island and reef infrastructure. Since fiber reinforced composite materials (FRP) have the advantages of light weight, high strength, good corrosion resistance in marine engineering, and good electromagnetic insulation, it has become a development trend to use fiber reinforced composite materials to replace steel bars.

[0003] At present, for this type of reinforcement, or other profiles with cross-sections of rods, tubes, grooves, squares, etc., the pultrusion process that is generally used is mold heating or oven heating for curing. Mold heating is limited by mold length and mold cost. A mold with a length of 0.9-1.2m is generally used. The production speed of different resins is generally 0.15-1m / min, and the production speed is often low. In addition, heating is used to heat the mold, and the mold then conducts heat to the resin in the mold cavity to cure the resin. This process has a large heat loss and high energy consumption. In addition, this heat transfer method from outside to inside has different internal and external temperatures, resulting in different resin curing and shrinkage, resulting in large internal stress, uneven internal and external interface bonding, and other product quality problems. Oven heating is also limited by the length of the production line, the number of ovens and the cost. The production speed is also low. The production speed of different resins is generally 0.3-1m / min. Electric heating wires are used to heat the air, and then the air is transmitted to the product to cause curing. This process has a greater heat loss and higher energy consumption. There is also heat conduction from the outside to the inside, and the temperature inside and outside is uneven, which causes the curing and shrinkage of the resin inside and outside to be different. The internal stress is large, the bonding of the internal and external interfaces is uneven, and the tensile strength and tensile modulus of the product are unstable.

[0004] CN107839295A discloses a microwave-heated fiber pultrusion production system and production method, including a yarn rack, a resin dipping tank, a microwave heating device, a curing device and a traction device arranged in sequence. The invention first pre-treats the resin on the fiber through a microwave heating device to perform preliminary gel molding, but subsequently an electric heating curing device is still required to further heat and cure the composite material.

[0005] In addition, the inventors also found that although microwave heating can heat the composite material uniformly inside and outside, there will be a temperature difference of more than 100 degrees in different areas at different times in the horizontal direction, which can easily cause the product to overburn or fail to reach the molding temperature, resulting in a decrease in the performance of the pultruded product or the product cannot be formed. Utility Model Content

[0006] In view of the above-mentioned problems existing in the prior art, the purpose of the utility model is to provide a resin-based fiber-reinforced composite microwave pultrusion system, which can be adapted to the preparation of high-performance plates, reinforcement materials, etc., and is particularly suitable for the production of reinforcement materials for marine engineering. On the one hand, the system can increase the production speed and reduce energy consumption, and on the other hand, it can improve product performance, so that the tensile strength, tensile modulus, and double shear strength of the product are increased by at least 3-14% on the existing basis, and the performance is more stable and uniform.

[0007] To achieve this purpose, the utility model provides a resin-based fiber-reinforced composite microwave pultrusion system, and the specific technical scheme is as follows:

[0008] A resin-based fiber-reinforced composite microwave pultrusion system comprises a yarn frame, a dipping device, a preforming device, a microwave heating device, a traction device, and a cutting device which are arranged in sequence. The microwave heating device is provided with at least one group. An inner cavity is also provided in the microwave cavity of the microwave heating device. The inner cavity comprises a wall panel and a cavity surrounded by the wall panel. The wall panel is made of an absorbing material, such as silicon carbide. The cross-sectional size of the cavity is larger than the cross-sectional size of the composite product to ensure that the composite product can pass horizontally without contacting the inner wall of the wall panel.

[0009] The creel is used to fix the yarn ball; the dipping device can use a dipping tank or a glue injection box to fully soak or coat the yarn or fiber led out of the creel with resin to form a composite material embryo; the preforming device has a mold cavity that does not need to be heated, which is used to preliminarily shape the composite material embryo into a product shape to obtain a composite material preform; the microwave heating device solidifies and shapes the composite material preform. When the composite material preform enters the microwave cavity, it immediately enters the inner cavity, and the surface of the composite material preform does not contact the inner wall of the inner cavity, and uniform curing is completed in the inner cavity.

[0010] By adopting the above technical scheme, the curing method in the traditional pultrusion system is designed to be microwave heating curing, so as to improve the heating efficiency, and by arranging an internal cavity with absorbing performance in the microwave cavity, the internal cavity is utilized to absorb microwaves, and a microwave-stable and temperature-stable area is formed in the internal cavity, so that when the composite material preform passes through the area, it can stably and evenly absorb microwaves and heat, thereby achieving uniform and stable temperature of the composite material preform in the radial direction and the direction of fiber bundle travel, achieving uniform curing of the composite material, and avoiding the problem of product overburning or failure to form caused by temperature difference in microwave heating in the prior art.

[0011] In another embodiment, the cavity of the inner cavity of the microwave heating device is a profiled cavity, and its cross-sectional shape is adapted to the cross-sectional shape of the product, for example, when the product is a round bar, the cross-sectional shape of the profiled cavity of the inner cavity is round; when the product is a square plate, the cross-sectional shape of the profiled cavity of the inner cavity is rectangular. The outer contour of the profiled cavity cross-section is 3-30 mm larger than the outer contour of the composite product.

[0012] By adopting the above technical solution, the cross-sectional shape of the contoured cavity of the inner cavity is imitated to the cross-sectional shape of the product, so that the distance between each point on the surface of the product and the inner wall of the inner cavity is equal, which can better control the overall shape of the composite material blank to be heated evenly and solidified consistently.

[0013] In another embodiment, the wall thickness of the inner cavity should be greater than 1 mm.

[0014] In another embodiment, the thickness of the inner cavity wall is 3-10 mm.

[0015] In another embodiment, the microwave heating device comprises a first microwave heating device, a second microwave heating device, and a third microwave heating device which are arranged in sequence.

[0016] In another embodiment, the pultrusion system further comprises a shaping device, which is arranged between the preforming device and the microwave heating device, and plays a role in maintaining the shape of the composite material preform output from the preforming device. The form of the shaping device can be reasonably selected according to the shape of the product. For example, when the product is a reinforcing material, the shaping device can be a winding device, which is arranged between the preforming device and the first microwave heating device. The fiber bundle output from the preforming device is spirally wound on the strapping tape through the winding device. After the product is formed, the strapping tape is removed; when the product is a plate, the shaping device can be a shaping mold, which has a mold cavity with the same cross-sectional shape as the product. The shaping mold can be set at the head and tail ends of the first microwave heating device, and then the product is shaped through appropriate tension control.

[0017] In another embodiment, the length of the inner cavity is 10-20 cm shorter than the length of the microwave cavity, and the inner cavity is centrally disposed in the microwave cavity.

[0018] Beneficial effects:

[0019] (1) The mechanical properties of the product obtained by the microwave pultrusion system are improved. Since an inner cavity is set in the cavity of the microwave heating device, the wall material of the inner cavity is made of silicon carbide. After the material absorbs microwaves, a microwave-stable and temperature-stable area is formed in the cavity. When the composite material preform passes through the inner cavity, it can absorb microwaves and heat more stably and evenly, so that the temperature fluctuation from the inside to the outside and in the direction of travel is controlled within 15°C, so that the interface between the fiber and the resin in the product is more uniform, the product curing consistency is more uniform, and the performance is more stable;

[0020] (2) The microwave pultrusion of the present invention improves the heating and curing efficiency, and the production speed can be increased by 40-70% compared with mold heating or oven heating;

[0021] (3) Energy consumption is reduced. Taking the curing temperature of 120° as an example, microwave heating only requires about 200W to achieve the desired effect. Mold heating usually requires three 2000W heating plates, while oven heating usually requires three 2000W ovens to complete. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Attached Figure 1 This is a schematic diagram of a composite material microwave pultrusion system of the present invention;

[0023] Attached Figure 2 It is a schematic diagram of the structure of a microwave heating device;

[0024] Attached Figure 3 The temperature stability curve of the cavity with different wall thickness in the microwave heating device;

[0025] Attached Figure 4 This is the thermal imaging distribution diagram of the microwave cavity (without the inner cavity);

[0026] Attached Figure 5 It is the thermal imaging distribution map of the microwave cavity (with inner cavity);

[0027] Among them: 1-yarn ball; 2-yarn rack; 3-impregnation device; 4-preforming device; 5-winding device; 6-microwave heating device; 61-microwave cavity; 62-inner cavity, 621-wall panel, 622-profile cavity; 7-traction machine; 8-cutting device, 9-composite material preform. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0029] A resin-based fiber-reinforced composite microwave pultrusion system comprises a yarn rack, a dipping device, a preforming device, a microwave heating device, a traction device, and a cutting device which are arranged in sequence. An inner cavity is also arranged in the microwave cavity of the microwave heating device, and the wall panels constituting the inner cavity are made of silicon carbide.

[0030] The creel is used to fix the yarn ball; the dipping device can use a dipping tank or a glue injection box to fully soak or coat the yarn or fiber led out of the creel with resin to form a composite material embryo; the preforming device has a mold cavity, which is used to preliminarily shape the composite material embryo into a product shape to obtain a composite material preform; the microwave heating device solidifies and shapes the composite material preform. When the composite material preform enters the microwave cavity, it immediately enters the inner cavity, and the surface of the composite material preform does not contact the inner wall of the inner cavity, and uniform curing is completed in the inner cavity.

[0031] An inner cavity is arranged in the microwave cavity of the microwave heating device, and the inner cavity includes a wall plate and a contoured cavity surrounded by the wall plate, and the contoured cavity is adapted to the outer contour of the product cross section. For example, when the product is a round bar, the cross section of the contoured cavity of the inner cavity is round; when the product is a square plate, the cross section of the contoured cavity of the inner cavity is rectangular.

[0032] The wall thickness of the inner cavity should be greater than 1 mm, and the preferred thickness range is 3-10 mm.

[0033] The microwave heating device comprises a first microwave heating device, a second microwave heating device, and a third microwave heating device which are arranged in sequence.

[0034] The pultrusion system also includes a shaping device, which is arranged between the preforming device and the microwave heating device, and plays a role in maintaining the shape of the composite material preform output from the preforming device. The form of the shaping device can be reasonably selected according to the shape of the product. For example, when the product is a rib material, the shaping device can be a winding device, which is arranged between the preforming device and the first microwave heating device; when the product is a plate material, the shaping device can be a mold, which is arranged at the first and last ends of the first microwave heating device.

[0035] The length of the inner cavity is 10-20 cm shorter than the length of the microwave cavity, and the inner cavity is centrally arranged in the microwave cavity.

[0036] Example 1

[0037] One of the resin-based fiber-reinforced composite microwave pultrusion systems covered by the present invention is shown in the attached Figure 1 and attached Figure 2As shown, it includes a yarn rack 2, a dipping device 3, a preforming device 4, a winding device 5, three sets of microwave heating devices 6, a traction machine 7, and a cutting device 8, which are arranged in sequence. The yarn rack 2 is used to fix the yarn ball 1; the dipping device 3 is a dipping tank, which performs resin infiltration on the fibers or yarns passing through it; the preforming device 4 has a mold cavity that does not need to be heated, which performs preliminary preforming of the fibers or yarns; the microwave cavity 61 of the microwave heating device 6 is also provided with an inner cavity 62, the inner cavity 62 includes a wall plate 621 and a contoured cavity 622 surrounded by the wall plate 621, the cross section of the contoured cavity 622 is circular, the wall plate 621 is made of silicon carbide; the length of the microwave cavity 61 is 600mm; the inner cavity 62 is centrally arranged in the microwave cavity 61, and its length is 200mm shorter than the length of the microwave cavity 61, the inner diameter of the inner cavity 62 is 25mm, the outer diameter is 35mm, and the thickness of the wall plate 621 is 5mm. The pultrusion system in this embodiment can be used to prepare rods, ribs, etc.

[0038] Example 2

[0039] The difference between this embodiment and the embodiment 1 is that the outer diameter of the inner cavity 62 of the microwave heating device 6 is 30 mm, and the thickness of the wall plate is 2.5 mm.

[0040] Example 3

[0041] The difference between this embodiment and the embodiment 1 is that the outer diameter of the inner cavity 62 of the microwave heating device 6 is 40 mm, and the thickness of the wall plate is 7.5 mm.

[0042] Example 4

[0043] The difference between this embodiment and the embodiment 1 is that the inner diameter of the inner cavity 62 of the microwave heating device 6 is 20 mm, and the outer diameter is 30 mm.

[0044] Example 5

[0045] The difference between this embodiment and the embodiment 1 is that the inner diameter of the inner cavity 62 of the microwave heating device 6 is 30 mm, and the outer diameter is 40 mm.

[0046] Example 6

[0047] The difference from Example 1 is that the cross-sectional shape of the inner cavity 62 is rectangular, with dimensions of 115 mm × 15 mm, and the thickness of the inner cavity wall is 5 mm; the shaping device is a mold having a cavity suitable for the product, which is specifically arranged at each end of the first microwave heating device. In this embodiment, the pultrusion system can be used to prepare the plate.

[0048] Example 7

[0049] Based on the microwave pultrusion system of Example 1, taking the preparation of reinforcement material as an example, the reinforcement material design specification is 10 mm in diameter, the fiber used is glass fiber, the resin used is thermoplastic acrylic resin for pultrusion, the required curing temperature is 100-130 degrees Celsius, and the microwave heating device used uses a microwave power of 200W.

[0050] The preparation steps include:

[0051] S1, dipping, drawing the glass fiber from the creel through a traction device, and then passing through a dipping device to fully infiltrate the glass fiber with resin to form a composite material blank;

[0052] S2, preforming, passing the composite material embryo through a preforming device having a circular cavity, so that the composite material embryo is formed into a cylindrical shape, thereby obtaining a composite material preform;

[0053] S3, microwave heating curing and molding, the composite material preform passes through the inner cavity of three groups of microwave heating devices in sequence, and is heated and cured in the inner cavity to obtain a resin-based fiber-reinforced composite material product; when the composite material preform passes through the inner cavity, the distance between its surface and the inner wall of the inner cavity is controlled to be 6.5-8.5 mm;

[0054] S4, cutting, cutting the microwave pultruded reinforcement output from the microwave heating device according to size requirements.

[0055] Example 8

[0056] The difference between this embodiment and embodiment 7 is that the reinforcement is prepared based on the microwave pultrusion system of embodiment 2, and the wall thickness of the inner cavity of the microwave heating device is 2.5 mm.

[0057] Example 9

[0058] The difference between this embodiment and embodiment 7 is that the reinforcement is prepared based on the microwave pultrusion system of embodiment 3, and the inner cavity wall thickness of the microwave heating device is 7.5 mm.

[0059] Based on Examples 7-9, microwave pultrusion systems with different wall thickness inner cavities were used to prepare microwave pultruded composite materials, and the effects of different wall thicknesses on the temperature of each point in the length direction of the composite materials were tested and recorded. Specifically, during the test, the temperature of different positions in the horizontal direction of the composite material in the third microwave heating device was tested, and the position of the composite material preform just entering the microwave cavity of the microwave heating device was recorded as 0cm, and the temperature test points were set at intervals of 5cm, and the position when it was about to leave the microwave cavity was recorded as 60cm. Then the three situations were compared with those without the inner cavity (recorded as a comparative example), and the temperature changes were specifically shown in Table 1 and the attached Figure 3 .

[0060] Table 1

[0061]

[0062] Combined with Table 1 and Appendix Figure 3 It can be seen that within the first 5 cm range entering the microwave cavity and within the range of 55-60 cm about to leave the microwave cavity, the temperature changes in the four cases are basically the same; within the range of 5-10 cm and 50-55 cm, the heating and cooling trends of the composite materials in Examples 7-9 are faster than those in the comparative example; within the range of 10-50 cm, the temperature range when no inner cavity is set is 32-187°C, and the temperature difference is very large, while when the inner cavity is set, the temperature fluctuation is greatly reduced, when the wall thickness of the inner cavity is 2.5 mm, the temperature range is 94-110°C, and when the wall thickness of the inner cavity is 5 mm, the temperature range is 100-120°C, and the overall temperature fluctuation is the most stable; when the wall thickness of the inner cavity is 7.5 mm, the temperature range is between 85-95°C, the overall temperature is slightly lower, but the temperature fluctuation is also very stable, which can be adapted to products that match the pultrusion curing temperature. From this, it can be seen that after setting up the inner cavity, the temperature of the composite material in the microwave cavity is more uniform and stable, which can avoid quality problems such as product failure due to insufficient curing temperature or product overburning due to excessive curing temperature during microwave heating curing in the prior art.

[0063] The performance of the reinforcement prepared in Example 7 was compared with reinforcements of the same specification prepared in two forms: a mold and an oven. The tensile strength comparison is shown in Table 2, the tensile modulus comparison is shown in Table 3, and the double shear strength comparison is shown in Table 4.

[0064] Table 2

[0065]

[0066] Table 3

[0067]

[0068] Table 4

[0069]

[0070]

[0071] It can be seen from Tables 2-4 that, in the microwave pultrusion of the present application, the tensile strength of the reinforcement is increased by 5% and 8% respectively compared with mold heating and oven heating, and the tensile modulus is increased by 3% and 7% respectively compared with mold heating and oven heating; the shear strength is increased by 12% and 14% respectively compared with mold heating and oven heating, and the CV values ​​of various properties are greatly reduced, and the product performance is very stable and uniform.

[0072] Example 10

[0073] This embodiment is based on the preparation system of Example 6, and prepares a plate with a width of 105 mm and a thickness of 5 mm. The resin used is an acrylic thermoplastic resin, glass fiber is used, and the required curing temperature is 100-130°C. The microwave power of the microwave heating device used is 300-800W, and the specific power setting is adjusted in combination with the pultrusion speed.

[0074] The preparation steps specifically include:

[0075] S1, yarn guide, pulls the glass fiber on the yarn rack through the pulling device;

[0076] S2, dipping, the glass fiber drawn out from the creel passes through a dipping device, the dipping device has a dipping tank, after the continuous fiber passes through the dipping tank, it is fully infiltrated by the resin solution to form a composite material embryo;

[0077] S3, preforming, the composite material embryo passes through a preforming device, and is initially formed into a flat plate structure in the preforming device to obtain a composite material preform;

[0078] S4, microwave heating curing and molding, the composite material preform passes through the shaping device and enters the inner cavity of the first microwave heating device, then enters the shaping device at the tail end of the first microwave heating device, and then passes through the second microwave heating device and the third microwave heating device in sequence to complete the curing and molding to obtain a composite material; the distance between the surface of the composite material preform and the inner wall of the inner cavity is controlled to be 4.5-5.5mm;

[0079] S5, cutting the composite material output from the microwave heating device as needed.

[0080] The temperature of the composite material in the third microwave heating device is detected by using a thermal imager. When the microwave heating device does not have an inner cavity, the temperature distribution diagram of the composite material is shown in FIG. Figure 4 When the inner cavity is set, the temperature distribution diagram of the composite material is shown in Figure 5 .contrast Figure 4 and Figure 5 It can be clearly seen that when the inner cavity is not set, the temperature distribution in the horizontal direction of the composite material is extremely uneven, and the temperature difference is large; after the inner cavity is set, the composite material is heated more evenly in the horizontal direction, which is conducive to the uniform curing of the composite material and avoids incomplete curing or overburning.

[0081] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes can be made based on the above description. It is not necessary to list all implementation methods here, and obvious changes derived therefrom are still within the scope of protection of the present invention.

Claims

1. A microwave pultrusion system for resin matrix fiber reinforced composite materials, comprising a creel, a dipping device, a preforming device, a microwave heating device, a traction device and a cutting device arranged in sequence, wherein the microwave heating device is provided with at least one group, characterized in that: An inner cavity is arranged in the microwave cavity of the microwave heating device, and the inner cavity includes a wall panel and a cavity surrounded by the wall panel; the wall panel is made of absorbing material; the cross-sectional size of the cavity is larger than the cross-sectional size of the composite material product to ensure that the composite material can pass through the cavity without contacting the wall panel.

2. The microwave pultrusion system of a resin matrix fiber reinforced composite material according to claim 1, characterized in that: The cavity of the inner cavity of the microwave heating device is a contoured cavity, the cross-sectional shape of the contoured cavity is the same as the cross-sectional shape of the composite product, and the cross-sectional outer contour of the contoured cavity is 3-30 mm larger than the cross-sectional outer contour of the composite product.

3. The microwave pultrusion system of a resin matrix fiber reinforced composite material according to claim 1, characterized in that: The wall thickness of the inner cavity is greater than 1 mm.

4. The microwave pultrusion system of a resin matrix fiber reinforced composite material according to claim 3, characterized in that: The wall thickness of the inner cavity is 3-10 mm.

5. The microwave pultrusion system for resin matrix fiber reinforced composite materials according to claim 1, characterized in that: The inner cavity is centrally arranged in the microwave cavity, and its length is 10-20 cm shorter than that of the microwave cavity.

6. The microwave pultrusion system of a resin matrix fiber reinforced composite material according to claim 1, characterized in that: The microwave heating devices are arranged in 2-3 groups in sequence.

7. A composite material microwave pultrusion system according to claim 1, characterized in that: The system further comprises a shaping device, which is arranged after the preforming device.

Citation Information

Cited By

  • Pultrusion system and method for resin matrix fiber reinforced composite material

    CN117863601A