Crushing, sorting and recycling system for waste lithium ion batteries
The lithium-ion battery recycling system with multiple screening and separation devices solves the problems of electrolyte volatilization, separator adhesion and adhesive in lithium battery recycling, achieves efficient recovery and classification of black powder, and reduces the risk of explosion and recycling The problem of low rates.
Patent Information
- Application Number
- CN202323311868.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-05
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2033-12-05
AI Technical Summary
In the recycling process of existing lithium batteries, there are problems such as electrolyte not being treated, resulting in a high risk of volatilization, black powder adhering to the wet separator shell during the sorting process, resulting in a low recovery rate, and the adhesive in the positive and negative electrode sheets not being removed, resulting in incomplete shedding of black powder. problem.
A waste lithium-ion battery crushing, sorting and recycling system is designed to achieve effective collection and graded recovery of black powder through multiple screening and separation devices, including a crushing unit, heating device, separation device, pyrolysis device and multiple screenings The device removes the battery casing, separator and adhesive to improve the collection and purity of black powder.
It achieves efficient recovery and classification of black powder, reduces the risk of explosion, improves the recovery rate, and recovers solvent through the heating device, avoiding the accumulation of black powder and the impact of adhesives.
Smart Images

Figure CN221827947U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the field of chemical industry, and in particular to a waste lithium-ion battery crushing, sorting and recycling system. Background Art
[0002] 2021 is the early stage of power battery retirement, and the scale of power battery retirement will continue to increase in the future. According to the previous sales of new energy vehicles in my country, the life of new energy passenger vehicles is about 4-6 years. If it is assumed that the retirement period of my country's lithium battery recycling industry is 5 years, the retirement level of power batteries in 2021 will be 252,000 tons. By 2030, the retirement level of power batteries in my country is expected to be 2.373 million tons. The content of valuable metals in waste lithium-ion batteries is much greater than that of primary ore lithium-ion batteries. It can be seen that the resource recycling of waste lithium-ion batteries can effectively alleviate the shortage of metal resources in my country; at the same time, the recycling of waste lithium-ion batteries can obtain a variety of metals and their salts. According to the current market conditions of such products, huge economic benefits will be obtained, which is also the main driving force for the development of the waste lithium-ion battery recycling industry.
[0003] Regarding lithium battery recycling, most of the current industry directly sorts after crushing, and finally obtains lithium-containing black powder after separating the components. This generally leads to the following problems: first, the electrolyte is not treated, which will cause volatilization during the sorting process, with a high risk of explosion and harm to human health after inhalation; second, a small amount of black powder will adhere to the wet diaphragm, shell, etc. during the sorting process, resulting in a low black powder recovery rate; third, the adhesive in the positive and negative electrodes is not removed, resulting in incomplete black powder shedding during the crushing and sorting process, further reducing the black powder recovery rate.
[0004] Therefore, the technical problems solved in this case are: how to effectively recycle black powder and how to recycle black powder in grades. Utility Model Content
[0005] The main purpose of the utility model is to provide a waste lithium-ion battery crushing, sorting and recycling system, which realizes the first black powder collection through the first screening device of the system, the second black powder collection through the second screening device, and the third black powder collection through the third screening device, thereby realizing effective recovery of the black powder; there is a difference in purity between the black powder collected for the second time and the black powder collected for the third time, thereby realizing graded recovery of black powders of different purities.
[0006] In order to achieve the above purpose, the utility model provides the following technical solutions:
[0007] A waste lithium-ion battery crushing, sorting and recycling system comprises a first crushing unit, a heating device, a first separation device, a first screening device, a second separation device, a pyrolysis device, a second screening device, a second crushing unit and a third screening device;
[0008] The first crushing unit is used to crush the lithium-ion battery to obtain a first crushed product;
[0009] A heating device, used for heating the first crushed product to volatilize at least part of the solvent in the crushed product to obtain a first solid;
[0010] A first separation device, used to remove the battery casing from the first solid to obtain a second solid;
[0011] A first screening device, used for screening the second solid to obtain a first oversize material and a first undersize material;
[0012] a second separation device for removing the membrane from the first screen material to obtain a third solid;
[0013] A pyrolysis device, used for heating the first undersize material and the third solid to pyrolyze organic matter in the first undersize material and the third solid to obtain a fourth solid;
[0014] a second screening device, used for screening the fourth solid to obtain a second oversize material and a second undersize material;
[0015] A second crushing unit is used to crush the second screen material to obtain a second crushed product;
[0016] The third screening device is used to screen the second crushed product to obtain a third oversize material and a third undersize material.
[0017] The beneficial effects of the technical solution of the utility model are:
[0018] 1. The system collects black powder for the first time through the first screening device, collects black powder for the second time through the second screening device, and collects black powder for the third time through the third screening device, thereby realizing effective recovery of black powder; there is a difference in purity between the second collected black powder and the third collected black powder, thereby realizing graded recovery of black powder of different purities;
[0019] 2. The first separation device is arranged before the first screening device. By removing the battery shell, black powder can be prevented from accumulating in the shell during the first screening, thereby improving the yield of the black powder collected for the first time. At the same time, the first separation device can also reduce the difficulty of removing the diaphragm of the second separation device;
[0020] 3. Arranging a second crushing unit after the second screening device can achieve black powder grading and black powder recovery rate. Specifically, on the one hand, the second crushing unit can crush the electrode piece and make the black powder on the electrode piece fall off through the impact force, thereby improving the black powder recovery rate of the third screening device; however, in this process, metal debris will be generated, so this part of the black powder has a relatively high impurity content. Screening in the second screening device can prevent the free black powder from entering the subsequent crushing step and being contaminated, thereby achieving black powder grading.
[0021] 4. The solvent is evaporated by a heating device to achieve solvent recovery. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a pipeline flow chart of Example 1 of the utility model;
[0023] Figure 2 This is a pipeline flow chart of Example 2 of the utility model;
[0024] Figure 3 This is a pipeline flow chart of Example 3 of the utility model;
[0025] Figure 4 This is a pipeline flow chart of Example 4 of the utility model. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the utility model to clearly and completely describe the technical solution of the utility model. Obviously, the described embodiments are only part of the embodiments of the utility model, not all of the embodiments. Based on the embodiments of the utility model, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model.
[0027] Example 1
[0028] refer to Figure 1 , a waste lithium-ion battery crushing and sorting recycling system, comprising a first crushing unit, a heating device 2, a first separation device 3, a first screening device 4, a second separation device 5, a pyrolysis device 6, a second screening device 7, a second crushing unit 8, and a third screening device 9;
[0029] A first crushing unit is used to crush the lithium-ion battery to obtain a first crushed product;
[0030] A heating device 2, used for heating the first crushed product to volatilize at least part of the solvent in the crushed product to obtain a first solid;
[0031] A first separation device 3, used to remove the battery shell in the first solid to obtain a second solid;
[0032] A first screening device 4, used for screening the second solid to obtain a first oversize material and a first undersize material;
[0033] A second separation device 5, used to remove the diaphragm in the first screen material to obtain a third solid;
[0034] A pyrolysis device 6, used for heating the first undersize material and the third solid to pyrolyze organic matter in the first undersize material and the third solid to obtain a fourth solid;
[0035] A second screening device 7, used for screening the fourth solid to obtain a second oversize material and a second undersize material;
[0036] The second crushing unit 8 is used to crush the second screen material to obtain a second crushed product;
[0037] The third screening device 9 is used to screen the second crushed product to obtain a third oversize material and a third undersize material.
[0038] As a preferred embodiment of this embodiment, the first crushing unit includes:
[0039] Cutting device 1: used to cut off the complete lithium-ion battery;
[0040] Crushing device 11: used for crushing the lithium-ion batteries cut by the cutting device 1;
[0041] The first separation device 3 and the second separation device 5 are both airflow separators; the first screening device 4 and the second screening device 7 are both drum screens.
[0042] The specific production process of this embodiment is:
[0043] Step 1: crushing 1 ton of cylindrical waste lithium iron phosphate batteries using a first crushing unit under nitrogen protection to obtain a first crushed product, and heating the first crushed product to a solvent volatilization temperature of the electrolyte under inert gas protection to obtain a first solid;
[0044] The battery is broken by the cutting device 1 and the breaking device 11. The cutting device 1 is used to cut the battery into two parts, and then the battery is broken by the blade-type breaking device 11. The size of the broken parts is 10-30 mm. At this time, a mixture of the shell, the diaphragm, the electrode, the electrolyte and the black powder is obtained, which is the first broken product.
[0045] The first crushed product is heated to the volatilization temperature of the electrolyte (100-150°C, 1h) by a heating device 2 to fully volatilize part of the solvent with a lower boiling point in the electrolyte; the remaining shell, diaphragm, electrode, lithium salt, some non-volatile additives and solvent with a higher boiling point after volatilization are the first solid; the solvent and additive with a higher boiling point mainly exist in the form of attachment to the diaphragm and electrode.
[0046] When cutting and crushing, nitrogen is introduced to control the oxygen content to <2.0% to avoid the risk of combustion and explosion.
[0047] Nitrogen is introduced into the heating device 2 throughout the entire process to facilitate solvent volatilization and ensure process safety.
[0048] Step 2: The first solid is fed into the first separation device 3, which is a wind separator to remove the battery shells in the first solid; the material extracted by the wind separator is the second solid;
[0049] The diaphragm, pole piece, lithium salt, black powder, some non-volatile additives, high boiling point organic solvents, etc. in the first solid are sucked into the first screening device 4 by negative pressure extraction to obtain the second solid;
[0050] By removing the outer shell in this step, black powder can be prevented from accumulating in the outer shell during screening in step 3; at the same time, it is beneficial to the airflow sorting operation of the diaphragm in step 4, and the outer shell can be prevented from squeezing the diaphragm, which makes it difficult to remove the diaphragm;
[0051] Step 3: Screening the second solid to obtain a first undersize and a first oversize, wherein the first undersize contains free black powder in the second solid, and the first undersize is sent to a pyrolysis device 6;
[0052] This step is performed in the first screening device 4, and the screening aperture can be selected to be 2 to 50 meshes, for example, 2, 5, 10, 15, 20, 25, 30, 40 or 50 meshes, preferably 10 meshes;
[0053] It should be noted that in this step, the aperture should be set larger, that is, the mesh number should be smaller. In actual production, more than 50% of the black powder needs to be screened in this step. If the free black powder cannot be screened, the black powder will be pumped away in step 4. At the same time, if a large amount of black powder cannot be screened in this step, it will be difficult to pump away the diaphragm in step 4.
[0054] The first screening device 4 in this step is a drum screen;
[0055] Step 4: The first screen material is separated by airflow through the second separation device 5 to remove the diaphragm, so as to obtain a third solid; the third solid is sent to the pyrolysis device 6 after the magnetic metal powder is removed through the magnetic separation device 10;
[0056] The second separation device 5 in this step is an airflow separator, the membrane is sucked away by the airflow separator, and the remaining material is the third solid; more specifically, the first screen material is placed on a 80-100 mesh screen conveyor belt, above which is the airflow separator;
[0057] Step 5: pyrolyzing the first undersize and the third solid, the pyrolysis is performed by a pyrolysis device 6 to decompose the lithium salt and carbonize organic matter such as a binder in the electrode to obtain a fourth solid;
[0058] The pyrolysis temperature of the pyrolysis device 6 is 500° C., and the time is 1.5 h. During the pyrolysis process, nitrogen protection is introduced, and the oxygen content is controlled to be less than 2.0%.
[0059] Step 6: Screening the fourth solid to obtain a second undersize material and a second oversize material; the second undersize material is the first black powder;
[0060] This step is performed by the second screening device 7, which is a drum screen with a mesh size of 80 to 150. The first black powder collected has a low metal content, so it is easier to extract lithium, fluorine and other metal elements of the positive electrode material from the black powder.
[0061] Step 7: Crush the second oversize material through the second crushing unit 8 to obtain a second crushed product, and screen the second crushed product through the third screening device 9 to obtain a third undersize material and a third oversize material; the third undersize material is the second black powder, and the third oversize material is the metal substrate particles of the electrode.
[0062] In this step, the size of the crushed particles is 1 to 3 mm;
[0063] It should be noted that in this step, crushing is very important. After repeated experiments, if crushing is not performed, the electrode pieces are relatively large. Although there is no binder in the positive electrode material, it is still difficult for the black powder to separate from the electrode pieces. By crushing, on the one hand, the size of the electrode pieces is reduced, and on the other hand, the black powder on the positive and negative electrode pieces can be easily fallen off and crushed into powder, which is conducive to a more thorough separation of black powder and copper and aluminum particles in the subsequent screening process.
[0064] Therefore, crushing before screening is very important.
[0065] It should also be further noted that the second black powder obtained in this step should not be mixed with the first black powder. After crushing, more metal powder will be produced. These metal powders will cause certain difficulties in the recovery of the black powder. It is necessary to set up special recovery steps for aluminum and copper elements. This part of black powder accounts for about 15% of the total black powder. Therefore, the above operation is worthwhile for fully recovering the black powder.
[0066] At the same time, it should be noted that if the crushing size in step 1 is adjusted to the size in step 7, although it can reduce the size of the pole piece from the source, it will also cause the diaphragm to be crushed. Over-crushed diaphragms will increase the difficulty of diaphragm sorting in step 4, and some small-sized diaphragms will be buried by pole pieces or other solids, making it difficult to extract. At the same time, excessive crushing in step 1 causes the screened material obtained by large-aperture screening in step 3 to contain small-sized pole pieces and diaphragms, making subsequent processes more complicated.
[0067] It should be noted that the system and process of this embodiment can also be used to perform black powder recovery operations on square aluminum shell ternary batteries and other types of batteries.
[0068] Example 2
[0069] refer to Figure 2 On the basis of Example 1, the evaporated solvent of the heating device 2 is recovered and the tail gas of the pyrolysis device 6 is treated;
[0070] Specifically, the present embodiment further comprises a first condensing unit connected to the exhaust port of the heating device 2; the first condensing unit comprises a primary condensing device 22 for condensing the solvent in the gas generated in the heating device 2; the primary condensing device 22 can recover most of the solvent, which is mainly a solvent with a boiling point lower than 150°C;
[0071] As a further preferred embodiment of the present invention, the present embodiment further comprises a tail gas combustion device 13, a heat exchanger 14, a flue gas quenching tower 15, a semi-dry reactor 16, a dust collector 17, an induced draft fan 18, a primary alkali spray tower 19, a secondary alkali spray tower 20, and a chimney 21 connected in sequence; the tail gas combustion device is connected to the tail gas discharge port of the pyrolysis device 6;
[0072] In actual production, it is found that the tail gas discharged from the pyrolysis device 6 contains a relatively large amount of oil, which is mostly high-boiling solvents and binder cracking products. In order to reduce the frequency of pipeline cleaning, an oil removal device 12 is also provided between the tail gas discharge port of the pyrolysis device 6 and the tail gas combustion device; the oil removal device can be selected from a filter, an electrostatic oil remover containing an electrostatic plate electric field, etc.
[0073] The tail gas treatment process of the pyrolysis device 6 of this embodiment is as follows: first, the tail gas is degreased by the degreasing device, and then enters the tail gas combustion device for aerobic combustion. The flue gas from the combustion is cooled by the heat exchanger and then enters the flue gas quenching tower for quenching. This process is to avoid the generation of dioxins. The tail gas from the flue gas quenching tower enters the semi-dry reactor for reaction and then enters the primary alkali spray tower and the secondary alkali spray tower for alkali solution spraying through the induced draft fan, and is finally discharged through the chimney.
[0074] Example 3
[0075] refer to Figure 3 On the basis of Example 1, the evaporated solvent of the heating device 2 is recovered, and the tail gas of the pyrolysis device 6 is treated, providing a completely different solution from Example 2. Specifically, it also includes a first condensation unit and a second condensation unit. The gas generated in the heating device 2 is transported to the first condensation unit through a pipeline; the gas generated in the pyrolysis device 6 is transported to the second condensation unit through a pipeline, and the second condensation unit is formed by a plurality of condensers connected in series in sequence;
[0076] Preferably, the first condensation unit includes a primary condensation device 22 for condensing the solvent in the gas generated in the thermal device, and a post-condensation device 27 for separating the fluorine-containing compounds in the primary condensation device 22; the second condensation unit includes a pre-condensation device 23, a primary condensation device 24, a secondary condensation device 25, and a tertiary condensation device 26 connected in series in sequence; the fluorine-containing compounds separated by the post-condensation device 27 are introduced into the secondary condensation device 25.
[0077] A pump or fan 28 for extracting gas is provided between the heating device 2 and the primary condensing device 22 , and a pump or fan for extracting gas is also provided between the pyrolysis device 6 and the pre-condensing device 23 .
[0078] The above preferred solution is a further refinement of step 1 and step 5, and its specific process is as follows:
[0079] Step 11: The organic solvent (first gas) evaporated in the heating device 2 of the above step 1 is extracted and condensed through a water-cooled tubular condenser (primary condensing device 22) to recover the organic solvent, and the solvent in the heating device 2 is fully evaporated to obtain a first solid; the primary condensing device 22 discharges uncondensed gas, and the uncondensed gas is introduced into a cold trap (post-condensing device 27) using -20°C supercooled brine as a refrigerant to obtain a second gas, which contains relatively pure fluorine-containing gas (PF5) and nitrogen; cooling water at about 5°C is introduced into the primary condensing device 22;
[0080] Most of the first gas is an organic solvent, but at the evaporation temperature, such as 100° C., a small amount of cracking of the lithium salt will occur, and this part of the cracking gas is worth recovering.
[0081] Step 12: The cracked gas obtained in the above step 5 is the third gas; the third gas contains organic solvent, N2, water, PF5, HF, POF3; most of the organic solvent in the third gas is oligomers after the decomposition of the binder and high boiling solvents with a boiling point higher than 150°C in the electrolyte;
[0082] Step 13: Send the third gas into the pre-condensing device 23 to remove the high-boiling solvent in the third gas; the pre-condensing device 23 is a water-cooled tubular condenser (pre-condensing device 23), and cooling water of about 5°C is passed into the pre-condensing device 23. The uncondensed gas discharged from the pre-condensing device 23 is the fourth gas.
[0083] Step 14: The fourth gas is sent to a tubular condenser (a primary condensing device 24), the refrigerant of the primary condensing device 24 is frozen brine, the temperature of the frozen brine is -5°C to 0°C, HF and water are completely condensed to obtain a fifth gas, the fifth gas contains only N2, PF5, POF3 and trace amounts of unidentified impurities;
[0084] Generally speaking, the refrigerant temperature in the tubular condenser should be significantly lower than the boiling point of the desired condensation object, and can even be close to the freezing point of the condensation object. The reason is that the amount of nitrogen in the fourth gas is relatively large and the gas flow rate is relatively fast. If the condensation temperature is too high, the condensation object to be condensed will not be fully condensed.
[0085] Step 15: Mix the fifth gas and the second gas and send them into a tubular condenser (secondary condensation device 25) for condensation to obtain a sixth gas; the refrigerant used in the secondary condensation device 25 is liquid nitrogen, and the condensation temperature is -60 to -50°C;
[0086] Step 16: Send the sixth gas to the tubular condenser (three-stage condensing device 26) for condensation, and collect liquid PF5. The refrigerant used in the three-stage condensing device 26 is liquid nitrogen, and the condensation temperature is -120 to -110°C.
[0087] Comprehensive analysis:
[0088] Through the introduction of the above three processes, it can be clearly seen that the system of this embodiment 3 can not only recycle the pole pieces, but also recycle the solvent of the electrolyte of the lithium-ion battery, LiF and PF5 after the decomposition of the lithium salt, thereby realizing the full recovery of useful substances in the lithium-ion battery.
[0089] Example 4
[0090] refer to Figure 4 , which is substantially the same as Example 1, except that:
[0091] The first screen undersize does not directly enter the pyrolysis device, but is combined with the third solid to undergo magnetic separation;
[0092] Specific process reference Figure 4 , the first screen material is sent to the magnetic separation device 10; in the magnetic separation device 10, the first screen material and the third solid are magnetically separated together, and after the magnetic separation, they enter the depyrolysis device for pyrolysis operation.
[0093] The advantage of this embodiment over the first embodiment is that it can reduce the content of magnetic metal in the black powder and improve the purity of the first black powder.
[0094] Although the embodiments of the present invention have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.
Claims
1. A waste lithium-ion battery crushing, sorting and recycling system. It is characterized in that It includes a first crushing unit, a heating device, a first separation device, a first screening device, a second separation device, a pyrolysis device, a second screening device, a second crushing unit, and a third screening device; A first crushing unit is used to crush the lithium-ion battery to obtain a first crushed product; A heating device, used for heating the first crushed product to volatilize at least part of the solvent in the crushed product to obtain a first solid; A first separation device, used to remove the battery casing from the first solid to obtain a second solid; A first screening device, used for screening the second solid to obtain a first oversize material and a first undersize material; a second separation device for removing the membrane from the first screen material to obtain a third solid; A pyrolysis device, used for heating the first undersize material and the third solid to pyrolyze organic matter in the first undersize material and the third solid to obtain a fourth solid; a second screening device, used for screening the fourth solid to obtain a second oversize material and a second undersize material; A second crushing unit is used to crush the second screen material to obtain a second crushed product; The third screening device is used to screen the second crushed product to obtain a third oversize material and a third undersize material.
2. The system according to claim 1, It is characterized in that A magnetic separation device is also provided between the second separation device and the pyrolysis device.
3. The system according to claim 1, It is characterized in that The first crushing unit comprises: Cutting device: used to cut off the complete lithium-ion battery; Crushing device: used for crushing the lithium-ion batteries cut by the cutting device.
4. The system according to claim 1, It is characterized in that The first separation device and the second separation device are both airflow separators; the first screening device and the second screening device are both drum screens.
5. The system according to claim 1, It is characterized in that It also includes a first condensation unit and a second condensation unit. The gas generated in the heating device is transported to the first condensation unit through a pipeline; the gas generated in the pyrolysis device is transported to the second condensation unit through a pipeline.
6. The system according to claim 5, It is characterized in that The second condensing unit is formed by connecting a plurality of condensers in series.
7. The system according to claim 6, It is characterized in that The first condensing unit comprises: Primary condensation device: used to condense the solvent in the gas generated in the thermal device; Post-condensation device: used to separate the fluorine-containing compounds in the tail gas produced by the primary condensation device; The second condensation unit comprises a pre-condensation device, a primary condensation device, a secondary condensation device, and a tertiary condensation device connected in series in sequence; the fluorine-containing compound separated by the post-condensation device is introduced into the secondary condensation device.
8. The system according to claim 1, It is characterized in that It also includes a tail gas combustion device, a heat exchanger, a flue gas quenching tower, a semi-dry reactor, a dust collector, an induced draft fan, a primary alkali spray tower, a secondary alkali spray tower, a chimney, and a tail gas discharge port connection between the tail gas combustion device and the pyrolysis device.
9. The system according to claim 8, It is characterized in that An oil removal device is provided between the tail gas discharge port of the pyrolysis device and the tail gas combustion device.
10. The system according to claim 1, It is characterized in that The mesh number of the first screening device is 2 to 50 meshes, and the mesh number of the second screening device is 80 to 150 meshes.