Plating layer structure of barrel plating white gun color tin-nickel alloy
By sequentially preparing a polymeric thiocyanate copper plating layer, a bright nickel plating layer, and a white gunmetal tin-nickel alloy plating layer on a steel substrate, the problem of insufficient adhesion between the plating layer and the substrate in the cyanide-free copper plating process is solved, achieving high corrosion resistance and good adhesion.
Patent Information
- Application Number
- CN202323359751.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-11
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2033-12-11
AI Technical Summary
In existing technologies, the problem of adhesion between the plating layer and the substrate in cyanide-free copper plating processes for steel parts has not been completely solved, resulting in reduced corrosion resistance of the plated parts. Furthermore, direct plating of bright nickel presents the problem of galvanic corrosion.
The structure involves sequentially preparing a polymeric thiocyanate copper plating layer, a bright nickel plating layer, and a white gunmetal tin-nickel alloy plating layer on a steel substrate. The copper plating layer is anodic, with an electrode potential positive than that of the nickel plating layer, providing electrochemical protection and enhancing adhesion and corrosion resistance.
It effectively solves the problem of adhesion between the coating and the substrate, improves the corrosion resistance of the coated parts, avoids galvanic corrosion, and meets the requirements of high corrosion resistance and good adhesion.
Smart Images

Figure CN221877205U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the technical field of metal surface treatment, and in particular relates to a coating structure of a barrel-plated white gunmetal-colored tin-nickel alloy. Background Art
[0002] Electroplating white gunmetal tin-nickel alloy is used to prepare a bright tin-nickel alloy coating, which is dark white and has a uniform alloy content. Due to its unique alloy ratio, the coating has low contact resistance, strong weldability, and extremely high corrosion resistance. It is an ideal anti-corrosion coating and functional coating, and is widely used in industries such as electronics and daily hardware. The traditional technology for rolling white gunmetal tin-nickel alloy on steel parts is usually to perform cyanide copper plating, bright nickel plating, and white gunmetal tin-nickel alloy plating on the steel substrate in sequence.
[0003] In recent years, the industry is actively developing cyanide-free copper plating processes to replace cyanide copper plating, but the problem of bonding strength between the coating and the substrate has not been completely solved. [1] At present, many electroplating plants have to adopt the process of directly plating bright nickel on the steel surface to avoid cyanide copper plating. However, the nickel plating layer is a cathodic coating relative to the steel substrate, which has the problem of galvanic corrosion, greatly reducing the corrosion resistance of the plated parts.
[0004] The newly developed polythiocyanate copper plating process uses polycuprous thiocyanate as the main salt and polysodium thiocyanate as the coordination agent. Its process performance is close to that of cyanide copper plating and is a cyanide-free copper plating process that is expected to replace cyanide copper plating. At present, the polythiocyanate copper plating process is still in the development and trial stage, and the process stability needs to be tested in practice.
[0005] References: [1] Qin Zuzu, Li Jiansan, Xu Jinlai, Research progress of cyanide-free copper plating technology at home and abroad [J], Electroplating and Finishing, 2015, 34(3): 149-152. Summary of the invention
[0006] In order to solve the high pollution problem of using cyanide copper plating to prepare the bottom plating layer of steel parts, the utility model provides a coating structure of barrel plating white gun-colored tin-nickel alloy. In order to achieve the above purpose, the utility model adopts the following technical solutions:
[0007] A coating structure of a barrel-plated white gunmetal tin-nickel alloy comprises a steel substrate, and a polymerized thiocyanate copper coating, a bright nickel coating, and a white gunmetal tin-nickel alloy coating, which are sequentially prepared from inside to outside on the steel substrate;
[0008] The thickness of the polymerized thiocyanate copper plating layer is 3-8 μm.
[0009] Preferably, the thickness of the bright nickel plating layer is 5 to 13 μm.
[0010] Preferably, the thickness of the white gunmetal tin-nickel alloy plating layer is 1 to 5 μm.
[0011] Copper is first plated on the surface of steel parts and then nickel is plated. The nickel-plated layer is an anodic layer relative to the copper-plated layer, and the electrode potential of the copper-plated layer is significantly more positive than that of the nickel-plated layer. This coating structure has an electrochemical protective effect on the steel substrate and can effectively prevent the corrosion of the steel substrate by the corrosive medium. A white gunmetal tin-nickel alloy coating is plated on the nickel-plated layer. The white gunmetal tin-nickel alloy coating has high corrosion resistance and can effectively slow down the corrosion rate of the corrosive medium on the nickel-plated layer.
[0012] Compared with the prior art, the utility model has the following beneficial effects:
[0013] 1. The utility model discloses a coating structure of a barrel-plated white gun-colored tin-nickel alloy, in which a bottom copper coating is prepared by a polysulfate cyanide copper plating process, thereby overcoming the high pollution problem of cyanide pre-plating of copper on steel parts;
[0014] 2. The coating structure of the white gunmetal-colored tin-nickel alloy by roller plating disclosed in the utility model is a coating structure of cyanide-free copper plating + bright nickel plating + white gunmetal-colored tin-nickel alloy plating on the steel surface, which overcomes the technical defect that the direct bright nickel plating + white gunmetal-colored tin-nickel alloy plating on the steel substrate does not have an electrochemical protective effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The drawings described herein are used to provide a further understanding of the present invention, constitute a part of the present application, and do not constitute an improper limitation of the present invention. In the drawings:
[0016] Figure 1 It is a schematic diagram of the coating structure of Example 1 and Example 2 of the utility model. Implementation
[0017] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The schematic embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.
[0018] A coating structure of a barrel-plated white gunmetal-tin-nickel alloy comprises a steel substrate, and a polymerized thiocyanate copper coating, a bright nickel coating and a white gunmetal-tin-nickel alloy coating which are sequentially prepared from inside to outside on the steel substrate.
[0019] The existing pre-treatment process is used to remove oil, rust and activate the steel substrate.
[0020] A polythiocyanate copper plating layer is prepared on a pre-treated steel part by using a polythiocyanate copper rolling plating process.
[0021] Preferably, the thickness of the polymerized thiocyanate copper plating layer is 3 to 8 μm.
[0022] Preferably, the polymerized thiocyanate copper plating layer is prepared by using the HT-810 polymerized thiocyanate copper roller plating process of Zunyi Huitong:
[0023] Polymeric cuprous thiocyanate 17-23 g / L, polymeric sodium thiocyanate 100-160 g / L, potassium sodium tartrate 8-12 g / L, HT-810 brightener 1-2 mL / L, HT-810 moving agent 2-4 mL / L, plating tank temperature 45°C-55°C, plating solution pH range 12-13, plating voltage 5-8 V, drum speed 8-12 r / min, anode current density ≤ 0.5 A / dm 2 , using oxygen-free electrolytic copper particles as anode.
[0024] The bright nickel coating is prepared on the steel parts after copper coating by polymerized thiocyanate barrel plating by using the existing bright nickel barrel plating process.
[0025] Preferably, the thickness of the bright nickel plating layer is 5 to 13 μm.
[0026] The white gunmetal tin-nickel alloy coating is prepared by adopting the existing barrel plating white gunmetal tin-nickel alloy process on the steel parts after barrel plating of bright nickel.
[0027] Preferably, the thickness of the white gunmetal tin-nickel alloy plating layer is 1 to 5 μm.
[0028] Preferably, the white gunmetal tin-nickel alloy coating is prepared by using the PGA-215 barrel plating white gunmetal tin-nickel alloy process of Chaobang Chemical:
[0029] Nickel chloride hexahydrate 135 ~ 175g / L, PGA-215A additive 450 ~ 500mL / L, PGA-215B additive 30 ~ 60mL / L, PGA-215C additive 10 ~ 30mL / L, plating solution pH range 3.5 ~ 4.5, plating tank temperature 63 ℃ ~ 73 ℃, plating voltage 5 ~ 8V.
[0030] Steel parts are barrel plated with white gunmetal tin-nickel alloy and then passivated and dried:
[0031] The specific process is "oxidation with 5% volume fraction hydrogen peroxide → water washing → pure water washing → centrifuge dehydration → drying". Example 1
[0032] like Figure 1 As shown, a coating structure of a barrel-plated white gunmetal tin-nickel alloy comprises a steel substrate 1, and a polymerized thiocyanate copper plating layer 2, a bright nickel plating layer 3, and a white gunmetal tin-nickel alloy plating layer 4 sequentially prepared from inside to outside on the steel substrate 1.
[0033] 1. Pre-treatment:
[0034] According to the current pre-treatment process, the steel substrate 1 is subjected to "alkaline chemical degreasing → water washing → acid washing → water washing → alkaline ultrasonic degreasing → water washing → activation → water washing".
[0035] 2. Polythiocyanate barrel copper plating:
[0036] After pretreatment of the steel parts, the polythiocyanate copper plating layer 2 was prepared by using the HT-810 polythiocyanate copper barrel plating process of Zunyi Huitong, and the coating thickness was 4 μm.
[0037] Polythiocyanate cuprous acid 19g / L, polythiocyanate sodium 120g / L, potassium sodium tartrate 10g / L, HT-810 brightener 1.5mL / L, HT-810 moving agent 3mL / L, plating tank temperature 50℃, plating solution pH 12.8, plating voltage 6V, drum speed 10r / min, anode current density 0.4A / dm 2 , use oxygen-free electrolytic copper corner as anode.
[0038] 3. Barrel plating bright nickel:
[0039] After the steel parts are subjected to polymerized thiocyanate barrel plating of copper, a bright nickel plating layer 3 is prepared by using the existing barrel plating bright nickel process, and the plating thickness is 10 μm.
[0040] 4. Barrel plating of white gunmetal tin-nickel alloy:
[0041] After the steel parts are roll-plated with bright nickel, the white gunmetal tin-nickel alloy coating 4 is prepared by the PGA-215 roll-plating white gunmetal tin-nickel alloy process of Chaobang Chemical, and the coating thickness is 3 μm.
[0042] Nickel chloride hexahydrate 140g / L, PGA-215A additive 460mL / L, PGA-215B additive 40mL / L, PGA-215C additive 15mL / L, plating solution pH 4.2, plating tank temperature 70℃, plating voltage 6V.
[0043] 5. Passivation and drying:
[0044] After the steel parts are roll-plated with white gunmetal tin-nickel alloy, they are "oxidized with 5% volume fraction hydrogen peroxide → washed with water → washed with pure water → dehydrated in a centrifuge → dried". Example 2
[0045] like Figure 1 As shown, a coating structure of a barrel-plated white gunmetal tin-nickel alloy comprises a steel substrate 1, and a polymerized thiocyanate copper plating layer 2, a bright nickel plating layer 3, and a white gunmetal tin-nickel alloy plating layer 4 sequentially prepared from inside to outside on the steel substrate 1.
[0046] 1. Pre-treatment:
[0047] According to the current pre-treatment process, the steel substrate 1 is subjected to "alkaline chemical degreasing → water washing → acid washing → water washing → alkaline ultrasonic degreasing → water washing → activation → water washing".
[0048] 2. Polythiocyanate barrel copper plating:
[0049] After pretreatment of the steel parts, the polythiocyanate copper plating layer 2 was prepared by using the HT-810 polythiocyanate copper barrel plating process of Zunyi Huitong, and the coating thickness was 6 μm.
[0050] Polymerized cuprous thiocyanate 22g / L, polymerized sodium thiocyanate 150g / L, potassium sodium tartrate 10g / L, HT-810 brightener 1.5mL / L, HT-810 moving agent 3mL / L, plating tank temperature 53℃, plating solution pH 12.5, plating voltage 7V, drum speed 10r / min, anode current density 0.4A / dm 2 , using oxygen-free electrolytic copper particles as anode.
[0051] 3. Barrel plating bright nickel:
[0052] After the steel parts are subjected to polymerized thiocyanate barrel plating of copper, a bright nickel plating layer 3 is prepared by using the existing barrel plating bright nickel process, and the plating thickness is 8 μm.
[0053] 4. Barrel plating of white gunmetal tin-nickel alloy:
[0054] After the steel parts are roll-plated with bright nickel, the white gunmetal tin-nickel alloy coating 4 is prepared by the PGA-215 roll-plating white gunmetal tin-nickel alloy process of Chaobang Chemical, and the coating thickness is 3 μm.
[0055] Nickel chloride hexahydrate 170g / L, PGA-215A additive 480mL / L, PGA-215B additive 50mL / L, PGA-215C additive 25mL / L, plating solution pH 3.8, plating tank temperature 66℃, plating voltage 7V.
[0056] 5. Passivation and drying:
[0057] After the steel parts are roll-plated with white gunmetal tin-nickel alloy, they are "oxidized with 5% volume fraction hydrogen peroxide → washed with water → washed with pure water → dehydrated in a centrifuge → dried".
[0058] Test Example 1:
[0059] According to Example 1 and Example 2, a barrel-plated white gunmetal tin-nickel alloy sample was prepared, and the bonding strength of the coating was tested by the thermal shock method according to GB / T 5270-2005 "Review of Test Methods for Adhesion Strength of Electrodeposited and Chemically Deposited Metal Coatings on Metal Substrates". The plated piece was placed in a heating furnace and heated to 220°C for 30 minutes, then taken out and suddenly cooled in water at room temperature. The coating did not blister or fall off. The test showed that the coating structure prepared in this example had good bonding strength.
[0060] Test Example 2:
[0061] According to Example 1 and Example 2, a white gunmetal-colored tin-nickel alloy sample was prepared for roller plating. According to GB / T 10125-2021 "Artificial atmosphere corrosion test salt spray test", an acetic acid salt spray test was carried out for 72 hours. There was no red rust on the surface of the plated part, which met the requirements of GB / T 9797-2005 "Metallic coating nickel + chromium and copper + nickel + chromium electroplating layer" standard.
[0062] The technical solutions provided by the embodiments of the present utility model are described in detail above. The principles and implementation methods of the embodiments of the present utility model are described in detail in this article using specific examples. The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present utility model. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present utility model, which all belong to the protection scope of the present utility model.
Claims
1. A coating structure of barrel-plated white gunmetal tin-nickel alloy, Features: It comprises a steel substrate, and a polymerized thiocyanate copper plating layer, a bright nickel plating layer, and a white gun-colored tin-nickel alloy plating layer which are sequentially prepared from the inside to the outside on the steel substrate; The thickness of the polymerized thiocyanate copper plating layer is 3-8 μm.
2. The coating structure of barrel-plated white gunmetal tin-nickel alloy as claimed in claim 1, Features: The thickness of the bright nickel plating layer is 5 to 13 μm.
3. The coating structure of barrel-plated white gunmetal tin-nickel alloy as claimed in claim 1, Features: The thickness of the white gunmetal tin-nickel alloy plating layer is 1-5 μm.