Passivation contact structure with selective tunneling layer thickness and TOPCon battery

By adopting a passivation contact structure with selective tunneling layer thickness in TOPCon batteries, adjusting the tunneling silicon oxide layer thickness and the phosphorus-doped polysilicon layer, the problems of low battery efficiency and surface recombination are solved, and the battery conversion efficiency is significantly improved and performance.

CN222106728UActive Publication Date: 2024-12-03JIANGSU LINYANG SOLARFUN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323454943.5
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-19
Publication Date
2024-12-03
Estimated Expiration
2033-12-19

AI Technical Summary

Technical Problem

The actual efficiency of existing TOPCon batteries does not reach the theoretical conversion efficiency, and there are problems with surface composite and interface contact resistance, which affects battery performance.

Method used

Using a passivation contact structure with a selective tunneling layer thickness, including providing a first tunneling silicon oxide layer and a second tunneling silicon oxide layer on the silicon substrate, and adjusting its thicknesses respectively in the metal and non-metal contact areas, combined with Phosphorus doped polysilicon and silicon nitride layers form a bilayer structure to improve passivation and carrier selectivity.

Benefits of technology

By adjusting the thickness of the tunneled silicon oxide layer, the metal recombination and contact resistivity are reduced, the surface recombination is suppressed, the battery efficiency is improved, the battery performance is improved, and the biases of the prior art are overcome.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222106728U_ABST
    Figure CN222106728U_ABST
Patent Text Reader

Abstract

The utility model discloses a passivation contact structure with a selective tunneling layer thickness and a TOPCon cell, and the thickness of a tunneling silicon oxide layer in different areas is adjusted, specifically, the thickness of the tunneling silicon oxide layer corresponding to a non-metal contact area and a metal contact area is adjusted. Metal recombination and contact resistivity of the metal contact area are reduced, surface recombination of the non-metal contact area can be obviously inhibited, and especially when another tunneling silicon oxide layer is deposited in the non-metal contact area and the thickness relation of the tunneling silicon oxide layer and the non-metal contact area is controlled to be within a certain range, the surface recombination of the non-metal contact area is inhibited. The structure obtains an unexpected reduction degree in the aspect of inhibiting surface recombination, can inhibit Auger recombination, and obviously improves the surface chemical passivation effect, so that adverse factors of a system are improved on the whole, key factors influencing the battery efficiency can be regulated and controlled after the structure is applied to a battery, and the battery efficiency is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the field of solar cells, in particular to a passivation contact structure with selective tunneling layer thickness and a TOPCon cell. Background Art

[0002] The tunneling oxide passivation contact cell (TOPCon cell for short) uses a combination of an ultra-thin silicon oxide layer and a doped polysilicon layer to achieve efficient passivation of the entire back side of the cell and selective collection of carriers. Therefore, the TOPCon cell can achieve higher opening voltage and higher FF. Generally, the tunneling silicon oxide layer has the following functions: 1. Providing chemical passivation, the intervention of the tunneling silicon oxide can saturate some dangling bonds on the surface of the silicon wafer, thereby reducing the interface defect state density. 2. Carriers pass selectively, the blocking barrier of the tunneling silicon oxide for holes is 4.5eV, which is greater than the blocking barrier for electrons of 3.1eV. 3. Blocking of doped atoms, the tunneling silicon oxide layer has a certain blocking effect on the diffusion of doped atoms, thereby controlling the diffusion distribution of doped atoms on the surface of the silicon wafer, thereby playing a role in regulating the interface Auger recombination and band bending. However, in current practice, the actual efficiency of TOPCon cells has not reached the theoretical conversion efficiency, and there is still a big gap. Utility Model Content

[0003] The purpose of the utility model is to overcome one or more deficiencies in the prior art and to provide a novel passivation contact structure with a selective tunneling layer thickness, which can achieve comprehensive improvements in surface composite, metal composite, interface contact resistance and other performances, and is beneficial to improving battery conversion efficiency.

[0004] The utility model also provides a tunneling oxide layer passivation contact battery (TOPCon battery for short) comprising the above passivation contact structure with selective tunneling layer thickness.

[0005] In order to achieve the above-mentioned purpose, a technical solution adopted by the utility model is: a passivation contact structure with a selective tunneling layer thickness, the passivation contact structure comprising:

[0006] A silicon substrate, the silicon substrate comprising a back surface, wherein the back surface is composed of a metal contact area and a non-metal contact area;

[0007] A first tunneling silicon oxide layer is disposed on the back surface, wherein the thickness of the first tunneling silicon oxide layer is less than or equal to 2.0 nm;

[0008] A second tunneling silicon oxide layer, which is disposed on a portion of the first tunneling silicon oxide layer corresponding to the non-metal contact region;

[0009] The thickness of the second tunneling silicon oxide layer is less than or equal to 1.3 nm, and the sum of the thickness of the first tunneling silicon oxide layer and the thickness of the second tunneling silicon oxide layer is not greater than 2.4 nm and not less than 1.4 nm;

[0010] A phosphorus-doped polysilicon layer is arranged on the back surface, and in the metal contact area, the first tunneling silicon oxide layer and the phosphorus-doped polysilicon layer are stacked in sequence; in the non-metal contact area, the first tunneling silicon oxide layer, the second tunneling silicon oxide layer and the phosphorus-doped polysilicon layer are stacked in sequence.

[0011] According to some preferred aspects of the present invention, the thickness of the first tunneling silicon oxide layer is less than or equal to 1.4 nm.

[0012] According to some preferred aspects of the present invention, the thickness of the second tunneling silicon oxide layer is less than or equal to 1.0 nm.

[0013] According to some preferred aspects of the present invention, the thickness of the first tunneling silicon oxide layer is 0.8-1.4 nm.

[0014] According to some preferred aspects of the present invention, the thickness of the second tunneling silicon oxide layer is 0.6-1.0 nm.

[0015] In some implementation cases, the thickness of the first tunneling silicon oxide layer can be 0.8 nm, 0.85 nm, 0.9 nm, 0.95 nm, 1 nm, 1.05 nm, 1.1 nm, 1.15 nm, 1.2 nm, 1.25 nm, 1.3 nm, 1.35 nm, 1.4 nm, etc.

[0016] In some implementation cases, the thickness of the second tunneling silicon oxide layer may be 0.6 nm, 0.65 nm, 0.7 nm, 0.75 nm, 0.8 nm, 0.85 nm, 0.9 nm, 0.95 nm, 1 nm, etc.

[0017] According to some preferred aspects of the present invention, the average concentration of phosphorus doping in the phosphorus-doped polysilicon layer is 1×10 20 -6×10 20 / cm 3 .

[0018] According to some preferred aspects of the present invention, in the portion of the phosphorus-doped polysilicon layer corresponding to the non-metallic contact region, the phosphorus doping concentration from the surface to the non-metallic contact region is 1×10 17 / cm 3 The depth of the position is taken as the phosphorus doping inner diffusion depth, and the phosphorus doping inner diffusion depth is 0.05-0.1 μm;

[0019] The phosphorus-doped polysilicon layer has a phosphorus doping concentration of 1×10 17 / cm 3 The depth of the position is taken as the phosphorus doping inner diffusion depth, and the phosphorus doping inner diffusion depth is 0.15-0.2 μm.

[0020] According to some preferred aspects of the present invention, the thickness of the phosphorus-doped polysilicon layer is 60-150 nm.

[0021] According to some preferred aspects of the present invention, the silicon substrate is an N-type single crystal silicon wafer with a resistivity of 0.5-3Ω·cm and a thickness of 100-200μm.

[0022] In some embodiments of the present invention, the passivation contact structure also includes a passivation layer arranged on the surface of the phosphorus-doped polysilicon layer and a metal electrode arranged in the metal contact area, and the passivation layer is a silicon nitride layer with a refractive index of 1.9-2.3 and a thickness of 70-100nm.

[0023] Another technical solution provided by the present invention is a TOPCon battery, which includes the above-mentioned passivation contact structure with selective tunneling layer thickness.

[0024] Due to the application of the above technical solution, the utility model has the following advantages compared with the prior art:

[0025] At present, it is generally believed that the passivation contact structure needs to be combined with a uniform ultra-thin tunneling silicon oxide layer deposited once on the basis of doped polysilicon to achieve efficient passivation and selective carrier collection. However, in a large number of practical studies, the inventors of the utility model have found through intensive research that by adjusting the thickness of the tunneling silicon oxide layer in different areas, specifically adjusting the thickness of the tunneling silicon oxide layer corresponding to the non-metallic contact area and the metal contact area, not only can the metal recombination and contact resistivity of the metal contact area be reduced, but also the surface recombination of the non-metallic contact area can be significantly inhibited, especially when another layer of tunneling silicon oxide layer is deposited in the non-metallic contact area and the thickness relationship between them is controlled within a certain range, this structure has achieved an unexpected reduction in inhibiting surface recombination. The structure greatly consumes the energy to be transferred after the collision of electrons or holes, reduces the probability of electron or hole transition, and thus greatly inhibits the occurrence of Auger recombination. Moreover, the combination of the double-layer structure also significantly improves the surface chemical passivation effect, thereby improving the unfavorable factors of the system as a whole, regulating the key factors affecting the battery efficiency, greatly improving the battery efficiency, and overcoming the technical bias existing in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the utility model or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the utility model. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0027] Figure 1 This is a schematic diagram of the structure of the silicon substrate after alkali polishing in the embodiment of the utility model;

[0028] Figure 2 This is a schematic diagram of the structure after the first tunneling silicon oxide layer is deposited in an embodiment of the utility model;

[0029] Figure 3 It is a schematic diagram of the structure after depositing a local second tunneling silicon oxide layer in an embodiment of the utility model;

[0030] Figure 4 This is a schematic diagram of the structure after the amorphous silicon layer is deposited in the embodiment of the utility model;

[0031] Figure 5 This is a schematic diagram of the structure after annealing treatment in an embodiment of the utility model;

[0032] Figure 6 This is a schematic diagram of the structure after removing the back phosphosilicate glass layer and then depositing the silicon nitride layer in the embodiment of the utility model;

[0033] Figure 7 It is a schematic structural diagram of a passivation contact structure with a selective tunneling layer thickness in an embodiment of the present utility model;

[0034] Figure 8 This is a schematic diagram of the structure of the compact cover plate used in the embodiment of the utility model;

[0035] In the figure markings: 1, silicon substrate; 2, first tunneling silicon oxide layer; 3, second tunneling silicon oxide layer; 4, amorphous silicon layer; 5, phosphorus-doped polysilicon layer; 6, phosphosilicate glass layer; 7, silicon nitride layer; 8, metal electrode; 9, dense cover plate; 91, gate line; 92, gap structure. DETAILED DESCRIPTION

[0036] In order to make the above-mentioned purposes, features and advantages of the utility model more obvious and easy to understand, the utility model is described in detail below in conjunction with the accompanying drawings and specific embodiments. In the following description, many specific details are set forth to facilitate a full understanding of the utility model. However, the utility model can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the utility model, so the utility model is not limited by the specific embodiments disclosed below.

[0037] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present utility model, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0038] In the present invention, unless otherwise clearly specified and limited, the terms "install", "connect", "connect", "fix" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0039] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0040] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be an intermediate element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time.

[0041] The above scheme is further described below in conjunction with the accompanying drawings and specific embodiments; it should be understood that these embodiments are used to illustrate the basic principles, main features and advantages of the utility model, and the utility model is not limited to the scope of the following embodiments; the implementation conditions adopted in the embodiments can be further adjusted according to specific requirements, and the implementation conditions not specified are usually the conditions in conventional experiments.

[0042] Embodiment 1:

[0043] See also Figure 7As shown, this example provides a passivation contact structure with selective tunneling layer thickness, the passivation contact structure comprising: a silicon substrate 1, the silicon substrate 1 comprising a back surface, the back surface consisting of a metal contact area and a non-metal contact area; a first tunneling silicon oxide layer 2, which is arranged on the back surface, and the thickness of the first tunneling silicon oxide layer 2 is less than or equal to 2.0nm; a second tunneling silicon oxide layer 3, which is arranged on the first tunneling silicon oxide layer 2 corresponding to the non-metal contact area; the thickness of the second tunneling silicon oxide layer 3 is less than or equal to 1.3nm, and the sum of the thickness of the first tunneling silicon oxide layer 2 and the thickness of the second tunneling silicon oxide layer 3 is not greater than 2.4nm and not less than 1.4nm; a phosphorus-doped polysilicon layer 5, which is arranged on the back surface, and in the metal contact area, the first tunneling silicon oxide layer 2 and the phosphorus-doped polysilicon layer 5 are stacked in sequence; in the non-metal contact area, the first tunneling silicon oxide layer 2, the second tunneling silicon oxide layer 3 and the phosphorus-doped polysilicon layer 5 are stacked in sequence.

[0044] In this example, the thickness of the first tunneling silicon oxide layer 2 is less than or equal to 1.4 nm, and the thickness of the second tunneling silicon oxide layer 3 is less than or equal to 1.0 nm. Further, the thickness of the first tunneling silicon oxide layer 2 is 0.8-1.4 nm, and the thickness of the second tunneling silicon oxide layer 3 is 0.6-1.0 nm.

[0045] As an optional embodiment, the thickness of the first tunneling silicon oxide layer 2 can be 0.8nm, 0.85nm, 0.9nm, 0.95nm, 1nm, 1.05nm, 1.1nm, 1.15nm, 1.2nm, 1.25nm, 1.3nm, 1.35nm, 1.4nm, etc.; the thickness of the second tunneling silicon oxide layer 3 can be 0.6nm, 0.65nm, 0.7nm, 0.75nm, 0.8nm, 0.85nm, 0.9nm, 0.95nm, 1nm, etc.

[0046] In this example, the average concentration of phosphorus doping in the phosphorus-doped polysilicon layer 5 is 1×10 20 -6×10 20 / cm 3 , the thickness of the phosphorus-doped polysilicon layer 5 is 60-150 nm. In the portion of the phosphorus-doped polysilicon layer 5 corresponding to the non-metallic contact region, the phosphorus doping concentration from the surface to the 17 / cm 3 The depth of the phosphorus doping inner diffusion depth is 0.05-0.1 μm; in the portion of the phosphorus doped polysilicon layer 5 corresponding to the metal contact region, the phosphorus doping concentration is 1×10 17 / cm 3 The depth of the position is taken as the phosphorus doping inner diffusion depth, and the phosphorus doping inner diffusion depth is 0.15-0.2 μm.

[0047] In this example, the silicon substrate 1 is an N-type single crystal silicon wafer with a resistivity of 0.5-3Ω·cm and a thickness of 100-200 μm.

[0048] In this example, the passivation contact structure further includes a passivation layer disposed on the surface of the phosphorus-doped polysilicon layer and a metal electrode 8 disposed in the metal contact region. The passivation layer is a silicon nitride layer 7 with a refractive index of 1.9-2.3 and a thickness of 70-100 nm.

[0049] Embodiment 2:

[0050] This example provides a method for preparing the above-mentioned passivation contact structure with a selective tunneling layer thickness, comprising:

[0051] Depositing a first tunneling silicon oxide layer on the back surface of the silicon substrate, controlling the thickness of the first tunneling silicon oxide layer to be less than or equal to 2.0 nm;

[0052] Covering the first tunneling silicon oxide layer with a dense cover plate having a void structure, wherein the void structure corresponds to a non-metallic contact area, and a portion of the dense cover plate other than the void structure corresponds to a metal contact area;

[0053] Then, a second tunneling silicon oxide layer is deposited, wherein the gap structure allows the second tunneling silicon oxide layer to be deposited in the non-metal contact area, and the thickness of the second tunneling silicon oxide layer is controlled to be less than or equal to 1.3 nm, and the sum of the thickness of the first tunneling silicon oxide layer and the thickness of the second tunneling silicon oxide layer is not greater than 2.4 nm and not less than 1.4 nm;

[0054] After removing the dense cover plate, an amorphous silicon layer is deposited and annealed to form a phosphorus-doped polysilicon layer.

[0055] Specifically, the following Figures 1 to 8 The utility model further introduces the passivation contact structure with selective tunneling layer thickness and its preparation process. The preparation method of the passivation contact structure with selective tunneling layer thickness includes:

[0056] Step (1): providing an N-type single crystal silicon wafer with a resistivity in the range of 0.5-3Ω·cm and a thickness in the range of 100-200μm as a silicon substrate; polishing the silicon substrate with an alkaline solution to remove the damaged layer on the surface of the silicon substrate and obtain a flat surface morphology. The schematic diagram of the polished silicon substrate is as shown in Figure 1 As shown;

[0057] Specifically, the treatment temperature is 50-70°C, and the mass percentage of the alkaline substance in the alkaline solution is 0.5%-2.5%. It is also preferred to add 0.1%-1.0% of an alkaline treatment protection additive. The alkaline substance includes but is not limited to sodium hydroxide, potassium hydroxide, etc. For example, an aqueous sodium hydroxide solution can be used to control the reflectivity of the silicon substrate surface after polishing to 30%-50%.

[0058] Step (2): depositing a first tunneling silicon oxide layer on the back surface of the silicon substrate obtained after the treatment in step (1), wherein the thickness of the first tunneling silicon oxide layer is 0.8-1.4 nm, and the preparation method of the first tunneling silicon oxide layer includes thermal oxidation, light ozone oxidation, ozone water, nitric acid oxidation, plasma enhanced chemical vapor deposition (PECVD), etc., and preferably plasma enhanced chemical vapor deposition (PECVD) can be used;

[0059] The schematic diagram of the structure after depositing the first tunneling silicon oxide layer is as follows: Figure 2 As shown, a silicon substrate 1 and a first tunneling silicon oxide layer 2 are arranged in sequence.

[0060] Step (3): A dense cover plate (also called a mask plate) made of carbon fiber or graphite is covered on the first tunneling silicon oxide layer, wherein the dense cover plate has a gap structure, the gap structure corresponds to the non-metallic contact area, and the portion of the dense cover plate other than the gap structure corresponds to the metal contact area. Furthermore, the portion of the dense cover plate other than the gap structure is in the form of equally spaced grid lines, with a spacing of 0.8-1.5 mm and a grid line width of 50-200 μm. The schematic structure of the dense cover plate 9 is as follows: Figure 8 As shown, the whole is in a plate shape, and the purpose of the gap structure 92 is to facilitate the deposition of the second tunneling silicon oxide layer so that it can pass through and be deposited on the first tunneling silicon oxide layer, while the gate line 91 area without the gap structure is a dense structure, and the second tunneling silicon oxide layer is difficult to pass through and is blocked during deposition, thereby realizing the local deposition of the second tunneling silicon oxide layer;

[0061] Then, a second tunneling silicon oxide layer is deposited on the back surface of the silicon wafer covered with a mask plate using plasma enhanced chemical vapor deposition. The thickness of the second tunneling silicon oxide layer is 0.6-1.0nm. Due to the presence of the dense cover plate, the second tunneling silicon oxide layer can be deposited in the void structure corresponding to the non-metallic contact area, while the part of the dense cover plate except the void structure corresponds to the metal contact area without deposition.

[0062] Among them, plasma enhanced chemical vapor deposition can be divided into tubular deposition and plate deposition, and the reaction gas can be divided into laughing gas and oxygen. Specifically, the second tunneling silicon oxide layer adopts the plate PECVD method, preferably oxygen as the reaction gas, wherein the reaction temperature is 200-300°C, the oxygen flow rate is 300-1000sccm, the reaction RF source power is 30-120w, and the reaction pressure is 5-20Pa; the sum of the thickness of the first tunneling silicon oxide layer and the thickness of the second tunneling silicon oxide layer is controlled to be no more than 2.4nm and no less than 1.4nm;

[0063] After the reaction is completed, the dense cover is removed;

[0064] The schematic diagram of the structure after depositing the local second tunneling silicon oxide layer is shown in Figure 3 As shown, in the metal contact area, a silicon substrate 1 and a first tunneling silicon oxide layer 2 are arranged in sequence from the direction in the figure, and in the non-metal contact area, a silicon substrate 1, a first tunneling silicon oxide layer 2 and a second tunneling silicon oxide layer 3 are arranged in sequence from the direction in the figure.

[0065] Step (4): depositing an amorphous silicon layer on the back surface of the intermediate after the treatment in step (3), wherein the preparation method of the amorphous silicon layer includes a low pressure chemical vapor deposition (LPCVD) intrinsic deposition method, a plasma enhanced chemical vapor deposition (PECVD) intrinsic / in-situ doping deposition method, and a physical vapor deposition (PVD) intrinsic / in-situ doping deposition method. The thickness of the amorphous silicon layer is 60-150 nm.

[0066] Among them, the low pressure chemical vapor deposition (LPCVD) intrinsic deposition method is preferred, specifically, the above-mentioned silicon substrate to be treated is horizontally inserted into a quartz boat and sent into a quartz furnace tube, the temperature is raised to 600-620°C, the pressure is maintained at 20-50Pa, 500-1200sccm of silane is introduced, the reaction time is 700-1800s, and after the end, the temperature is lowered and the sample is taken out;

[0067] The schematic diagram of the structure after depositing the amorphous silicon layer is shown in Figure 4 As shown, in Figure 3 A layer of amorphous silicon layer is deposited on the basis of the substrate. In the metal contact area, a silicon substrate 1, a first tunneling silicon oxide layer 2, and an amorphous silicon layer 4 are arranged in sequence from the direction in the figure. In the non-metal contact area, a silicon substrate 1, a first tunneling silicon oxide layer 2, a second tunneling silicon oxide layer 3 and an amorphous silicon layer 4 are arranged in sequence from the direction in the figure.

[0068] Step (5): The intermediate obtained after the treatment in step (4) is placed in a quartz boat and sent into a quartz furnace tube for high temperature treatment.

[0069] When the amorphous silicon layer is intrinsic amorphous silicon, the high temperature treatment is phosphorus diffusion high temperature treatment; when the amorphous silicon layer is in-situ doped amorphous silicon, the high temperature treatment is high temperature annealing treatment. The high temperature treatment temperature is in the range of 750-900°C.

[0070] The phosphorus diffusion high temperature treatment process comprises: inserting the intermediate obtained after the treatment in step (4) into a quartz boat and sending it into a quartz furnace tube, heating it to 750-820°C, introducing 1000-2000sccm of phosphorus oxychloride and 1000-2000sccn of oxygen, maintaining for 10-30 minutes, then heating and keeping the temperature constant at 850-900°C, the process gas is nitrogen, the flow rate is 3000-6000sccm, maintaining for 20-30 minutes, and cooling and taking it out after completion.

[0071] After step (5), the amorphous silicon layer is transformed into polysilicon, and some phosphorus atoms are activated, become electrically active, and diffuse to a certain depth through the first tunneling silicon oxide layer and the second tunneling silicon oxide layer. At the same time, a phosphorus silicon glass (PSG) layer is formed on the surface of the phosphorus-doped polysilicon layer.

[0072] Furthermore, the phosphorus electrically activated doping concentration in the phosphorus-doped polysilicon layer is controlled to be 1×10 20 -6×10 20 / cm 3 In the phosphorus-doped polysilicon layer containing only the first tunneling silicon oxide layer, the phosphorus-doped inner diffusion depth (from the surface to the phosphorus-doping concentration of 1×10 17 / cm 3 The depth of the phosphorus doping position is 0.15-0.2 μm; in the phosphorus doped polysilicon layer corresponding to the region where the first tunneling silicon oxide layer and the second tunneling silicon oxide layer are located, the phosphorus doping inner diffusion depth (from the silicon wafer surface to the phosphorus doping concentration of 1×10 17 / cm 3 The depth of the position) is 0.05-0.1μm;

[0073] The schematic diagram of the structure after annealing treatment is as follows Figure 5 As shown, in the metal contact area, a silicon substrate 1, a first tunneling silicon oxide layer 2, a phosphorus-doped polysilicon layer 5, and a phosphosilicate glass layer 6 are arranged in sequence from the direction in the figure; in the non-metal contact area, a silicon substrate 1, a first tunneling silicon oxide layer 2, a second tunneling silicon oxide layer 3, a phosphorus-doped polysilicon layer 5, and a phosphosilicate glass layer 6 are arranged in sequence from the direction in the figure.

[0074] Step (6): using HF solution to remove the PSG layer on the back surface of the intermediate obtained in step (5), the mass percentage concentration of HF is 5%-20%. Then using PECVD method (process parameters: temperature 470-500°C, reaction pressure 180-240Pa, silane flow rate 800-1600sccm, ammonia flow rate 8000-16000sccm, power 17000W, process time 600-1200s) to form a silicon nitride layer on the back surface of the silicon wafer, the silicon nitride layer has a refractive index of 1.9-2.3 and a thickness of 70-100nm;

[0075] The schematic diagram of the structure after removing the back phosphosilicate glass layer and depositing the silicon nitride layer is shown in Figure 6 As shown, in the metal contact area, a silicon substrate 1, a first tunneling silicon oxide layer 2, a phosphorus-doped polysilicon layer 5, and a silicon nitride layer 7 are arranged in sequence from the direction in the figure; in the non-metal contact area, a silicon substrate 1, a first tunneling silicon oxide layer 2, a second tunneling silicon oxide layer 3, a phosphorus-doped polysilicon layer 5, and a silicon nitride layer 7 are arranged in sequence from the direction in the figure.

[0076] Step (7): Use screen printing technology to print equally spaced silver paste electrode lines in the metal contact area corresponding to the first tunneling silicon oxide layer and perform high temperature sintering. The spacing between the silver paste electrode lines is 0.8-1.5 mm, the width of the silver paste electrode lines is 20-40 μm, the electrode line width is smaller than the width of the line area on the dense cover plate, and the sintering temperature is 700-850°C;

[0077] The schematic diagram of the passivation contact structure with selective tunneling layer thickness is shown in FIG. Figure 7 As shown, in the metal contact area, a silicon substrate 1, a first tunneling silicon oxide layer 2, a phosphorus-doped polysilicon layer 5, a silicon nitride layer 7, and a metal electrode 8 (such as a silver paste electrode) penetrating into the phosphorus-doped polysilicon layer 5 are arranged in sequence from the direction in the figure; in the non-metal contact area, a silicon substrate 1, a first tunneling silicon oxide layer 2, a second tunneling silicon oxide layer 3, a phosphorus-doped polysilicon layer 5, and a silicon nitride layer 7 are arranged in sequence from the direction in the figure.

[0078] Example 2-1:

[0079] This example provides a combination of the above Figures 1 to 8 The structure and process shown in the figure are used to prepare a passivation contact structure with a selective tunneling layer thickness. The specific process and parameters are as follows:

[0080] Step (1): providing an N-type single crystal silicon wafer with a resistivity of 0.7 Ω·cm and a thickness of 140 μm as a silicon substrate; the treatment temperature is 65° C., the mass percentage of sodium hydroxide in the sodium hydroxide aqueous solution is 1.4%, and the protective additive is a commercially available brand PS42V08, and the addition amount is 0.5%; the reflectivity of the silicon substrate surface after polishing is 46%;

[0081] Step (2): using thermal oxidation deposition (process parameters: deposition temperature 600° C., oxygen flow rate 30000 sccm, deposition time 600 s) to deposit a first tunneling silicon oxide layer with a thickness of 1.0 nm;

[0082] Step (3): the material of the dense cover plate is graphite, the grid line spacing on the dense cover plate is 1.2 mm, and the grid line width is 80 μm;

[0083] A second tunneling silicon oxide layer is deposited by using a plate-type plasma enhanced chemical vapor deposition method (process parameters are: temperature 300° C., reaction pressure 12 Pa, oxygen flow rate 800 sccm, reaction power 60 W, process time 60 s), and the thickness of the second tunneling silicon oxide layer is 0.8 nm;

[0084] Step (4): Deposit an amorphous silicon layer using a low pressure chemical vapor deposition (LPCVD) intrinsic deposition method, raise the temperature to 610° C., maintain the pressure at 30 Pa, introduce 900 sccm of silane, the reaction time is 1500 s, and the thickness of the amorphous silicon layer is 120 nm;

[0085] Step (5): phosphorus diffusion high temperature treatment is adopted, and the process comprises: inserting the intermediate obtained after the treatment in step (4) into a quartz boat and sending it into a quartz furnace tube, heating it to 780°C, introducing 1200sccm of phosphorus oxychloride and 1000sccm of oxygen, maintaining it for 16 minutes, and then heating it and keeping it constant at 870°C, the process gas is nitrogen, the flow rate is 5000sccm, and maintaining it for 25 minutes;

[0086] The phosphorus electrically activated doping concentration in the phosphorus doped polysilicon layer is 4×10 20 / cm 3 In the phosphorus-doped polysilicon layer containing only the first tunneling silicon oxide layer, the phosphorus-doped inner diffusion depth (from the surface to the phosphorus-doping concentration of 1×10 17 / cm 3 The depth of the phosphorus doping position) is 0.185 μm; in the phosphorus doped polysilicon layer corresponding to the region where the first tunneling silicon oxide layer and the second tunneling silicon oxide layer are located, the phosphorus doping inner diffusion depth (from the silicon wafer surface to the phosphorus doping concentration of 1×10 17 / cm 3 The depth of the position) is 0.08μm;

[0087] Step (6): the mass percent concentration of HF is 15%;

[0088] A silicon nitride layer was formed on the back surface of the silicon wafer using the PECVD method (process parameters: temperature 500°C, reaction pressure 200 Pa, silane flow rate 1200 sccm, ammonia flow rate 14000 sccm, power 17000 W, process time 720 s). The silicon nitride layer had a refractive index of 2.1 and a thickness of 80 nm.

[0089] Step (7): Use screen printing technology to print equally spaced silver paste electrode lines in the metal contact area corresponding to the first tunneling silicon oxide layer and perform high-temperature sintering; specifically, the width of the silver paste electrode lines is 30 μm, the electrode line width is smaller than the width of the line area on the dense cover plate, and the sintering temperature is 740°C.

[0090] In the passivation contact structure with selective tunneling layer thickness in this example, the first tunneling silicon oxide layer has a thickness of 1.0 nm, and the second tunneling silicon oxide layer has a thickness of 0.8 nm.

[0091] Comparative Example 1

[0092] It is basically the same as Example 2-1, with the only difference being that the thickness of the second tunneling silicon oxide layer is 0.4 nm, and the thickness of the first tunneling silicon oxide layer is 0.8 nm.

[0093] Comparative Example 2

[0094] It is basically the same as Example 2-1, with the only difference being that the thickness of the second tunneling silicon oxide layer is 1.2 nm, and the thickness of the first tunneling silicon oxide layer is 1.6 nm.

[0095] Performance Testing

[0096] In order to further demonstrate the improvement of battery performance by the passivation contact structure with selective tunneling layer thickness of the utility model, the preparation process and performance test results of the N-TOPCon battery including the above-mentioned Example 2-1 and Comparative Example 1-2 are supplemented as follows:

[0097] (1): Using an N-type silicon wafer with a resistivity of 0.7Ω.cm and a thickness of 140μm, the silicon wafer was textured, the weight loss of the textured silicon wafer was 0.3g, and the textured surface reflectivity was 9.6%;

[0098] (2): Boron diffusion treatment is performed on the front side of the silicon wafer, the deposition temperature is 860°C, the push temperature is 940°C, and the square resistance after the process is 110Ω / sq;

[0099] (3): Laser scanning is performed on the boron diffusion surface of the silicon wafer to achieve local laser doping. The square resistance of the laser scanning area is 75Ω / sq;

[0100] (4): The silicon wafer is subjected to high-temperature oxidation at 1060°C. After oxidation, the square resistance of the laser-doped area is 80Ω / sq, and the square resistance of the non-laser-doped area is 220Ω / sq. After oxidation, a borosilicate glass layer (BSG) is formed on the front side;

[0101] (5): corresponding to step (1) of the embodiment or comparative example, since the BSG layer is retained on the front side, the front side is not polished;

[0102] (6): corresponding to step (2) of the embodiment or comparative example;

[0103] (7): corresponding to step (3) of the embodiment or comparative example;

[0104] (8): corresponding to step (4) of the embodiment or comparative example;

[0105] (9): corresponding to step (5) of the embodiment or comparative example;

[0106] (10): That is, the step (6) corresponding to the embodiment or comparative example, which is different from the preparation method of the structure. The battery structure has increased the details of the steps due to the requirements of the front structure. Specifically, first use a single-sided HF (concentration 15%) chain machine to remove the front PSG, then use an alkaline solution (alkali concentration 3.5%) to remove the front amorphous silicon plating, and finally use an HF solution to remove the back PSG layer, and then use the ALD method to deposit the front aluminum oxide (thickness of about 4nm), use the PECVD method to deposit the front silicon nitride (thickness of about 75nm), and finally use the PECVD method to deposit the back silicon nitride;

[0107] (11): That is, it corresponds to step 7 of the embodiment or comparative example; first print the back main grid, the number of main grids is 16, the width of the main grid is 60μm, and then print the back fine grid after drying. After drying, print the front main grid, the number of main grids is 16, the width of the main grid is 50μm, and after drying, print the front fine grid lines, the fine grid line spacing is 1.2mm, the grid line width is 20μm, and finally sintering is performed.

[0108] The test method is: use an IV tester to test the cell photoelectric conversion efficiency and related electrical performance parameters under standard light power under simulated solar light source.

[0109] The specific test results are shown in Table 1 (Eta: conversion efficiency, Voc: open circuit voltage, Jsc: short circuit current, FF: fill factor).

[0110] Table 1

[0111]

[0112] It can be seen from Table 1 above that the conversion efficiency of the battery prepared by the method of the utility model has been significantly improved. Compared with Comparative Examples 1 and 2, Example 2-1 increases the conversion efficiency of the battery by 0.43% and 0.58% respectively by adjusting the thickness of the tunneling silicon oxide layer in different areas and controlling the total thickness of the tunneling silicon oxide layer in the non-metallic contact area to 1.4-2.4nm. For crystalline silicon solar cells, a change of 0.1% is usually a huge improvement. It can be seen that the passivation contact structure with selective tunneling layer thickness of the utility model can achieve comprehensive improvement in surface composite, metal composite, interface contact resistance and other properties, which is beneficial to the qualitative improvement of battery conversion efficiency.

[0113] The above embodiments are only for illustrating the technical concept and features of the utility model, and their purpose is to enable people familiar with the technology to understand the content of the utility model and implement it accordingly, and they cannot be used to limit the protection scope of the utility model. Any equivalent changes or modifications made according to the spirit of the utility model should be included in the protection scope of the utility model.

[0114] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. A passivation contact structure with a selective tunneling layer thickness, It is characterized in that The passivation contact structure comprises: A silicon substrate, the silicon substrate comprising a back surface, wherein the back surface is composed of a metal contact area and a non-metal contact area; A first tunneling silicon oxide layer is disposed on the back surface, wherein the thickness of the first tunneling silicon oxide layer is less than or equal to 2.0 nm; A second tunneling silicon oxide layer, which is disposed on a portion of the first tunneling silicon oxide layer corresponding to the non-metal contact region; The thickness of the second tunneling silicon oxide layer is less than or equal to 1.3 nm, and the sum of the thickness of the first tunneling silicon oxide layer and the thickness of the second tunneling silicon oxide layer is not greater than 2.4 nm and not less than 1.4 nm; A phosphorus-doped polysilicon layer is arranged on the back surface, and in the metal contact area, the first tunneling silicon oxide layer and the phosphorus-doped polysilicon layer are stacked in sequence; in the non-metal contact area, the first tunneling silicon oxide layer, the second tunneling silicon oxide layer and the phosphorus-doped polysilicon layer are stacked in sequence.

2. The passivation contact structure with selective tunneling layer thickness according to claim 1, It is characterized in that The thickness of the first tunneling silicon oxide layer is less than or equal to 1.4 nm.

3. The passivation contact structure with selective tunneling layer thickness according to claim 1 or 2, It is characterized in that The thickness of the second tunneling silicon oxide layer is less than or equal to 1.0 nm.

4. The passivation contact structure with selective tunneling layer thickness according to claim 1, It is characterized in that The thickness of the first tunneling silicon oxide layer is 0.8-1.4 nm.

5. The passivation contact structure with selective tunneling layer thickness according to claim 1 or 4, It is characterized in that The thickness of the second tunneling silicon oxide layer is 0.6-1.0 nm.

6. The passivation contact structure with selective tunneling layer thickness according to claim 1, It is characterized in that The thickness of the phosphorus-doped polysilicon layer is 60-150 nm.

7. The passivation contact structure with selective tunneling layer thickness according to claim 1, It is characterized in that The silicon substrate adopts an N-type single crystal silicon wafer with a resistivity of 0.5-3Ω·cm and a thickness of 100-200μm.

8. The passivation contact structure with selective tunneling layer thickness according to claim 1, It is characterized in that The passivation contact structure further includes a passivation layer arranged on the surface of the phosphorus-doped polysilicon layer and a metal electrode arranged in the metal contact area. The passivation layer is a silicon nitride layer with a refractive index of 1.9-2.3 and a thickness of 70-100 nm.

9. A TOPCon battery, It is characterized in that The TOPCon cell comprises the passivation contact structure having a selective tunneling layer thickness as claimed in any one of claims 1 to 8.