Welded structure, top cover assembly, individual battery cells and battery pack

By optimizing the welding trajectory and material selection of the terminals and tabs, the problems of welding defects and insufficient interface mixing were solved, improving the energy density and welding reliability of the battery, preventing stress concentration, and achieving the battery's stability and high energy density requirements.

CN224986578UActive Publication Date: 2026-11-17HUIZHOU EVE POWER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202522380649.7
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2025-11-07
Publication Date
2026-11-17
Estimated Expiration
2035-11-07

AI Technical Summary

Technical Problem

In existing technologies, the welding trajectory planning of the terminals and tabs is not perfect, resulting in welding defects and insufficient mixing at the welding interface, which affects the stability and energy density of the battery.

Method used

Design a welding structure in which the welding trajectory area between the pole and the tab accounts for 30% to 60% of the welding area, and set recessed units on the surface of the pole to form a ring or spiral welding trajectory. Use laser welding and form a metal compound through metal layers with different melting points to improve hardness and tensile strength.

Benefits of technology

It improves the energy density of the battery, prevents welding defects and insufficient interface mixing, enhances the reliability and mechanical properties of the weld, and avoids the decline in fatigue life caused by stress concentration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN224986578U_ABST
    Figure CN224986578U_ABST
Patent Text Reader

Abstract

This utility model relates to the field of battery technology, providing a welding structure, a top cover assembly, a single battery cell, and a battery pack. The welding structure includes tabs and terminals, with the terminals welded to the tabs. A welding trajectory is defined on the surface of the terminals, and each terminal has a welding area. The welding trajectory is located within the welding area, where the area of ​​the welding trajectory is S1, and the area of ​​the welding area is S2, satisfying: 30% ≤ S1 / S2 ≤ 60%. This prevents welding defects caused by excessive heat input during welding and also avoids insufficient mixing at the welding interface due to insufficient heat input.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This utility model relates to the field of battery technology, specifically to a welding structure, a top cover assembly, a single battery cell, and a battery pack. Background Technology

[0002] In related technologies, the market demands supercharging and high energy density for power batteries, requiring batteries to maintain stability under high current and minimize structural space to meet these requirements. For battery terminals and tabs, they are typically connected by connecting tabs, usually through welding. However, current planning for the welding paths of terminals and tabs is not yet perfect, leading to welding defects after welding. Utility Model Content

[0003] The embodiments of this utility model provide a welding structure, a top cover assembly, a single battery cell, and a battery pack, which can improve the technical problem of poor welding.

[0004] In a first aspect, embodiments of the present invention provide a welding structure, comprising: Extreme ear; A pole post is welded to the tab and a welding trajectory is defined on the surface of the pole post. The pole post has a welding area and the welding trajectory is located within the welding area. The area of ​​the welding trajectory is S1 and the area of ​​the welding area is S2, satisfying: 30%≤S1 / S2≤60%.

[0005] Therefore, it can prevent welding defects caused by excessive heat input during the welding process, and also avoid insufficient mixing of the welding interface caused by insufficient heat input during the welding process.

[0006] In one embodiment, the welding trajectory is recessed on the surface of the pole, and the depth of the recess is H, satisfying: 20 micrometers ≤ H ≤ 50 micrometers.

[0007] Therefore, on the one hand, it can prevent stress concentration from causing a decrease in fatigue life, and on the other hand, it can avoid the mechanical properties after welding not meeting the standards.

[0008] In one embodiment, the welding trajectory includes at least two sequentially connected recessed units, which are connected to form a ring-shaped or spiral-shaped welding trajectory.

[0009] This ensures the welding area of ​​the welding trajectory, so that the pole and the tab can form a reliable connection.

[0010] In one embodiment, the recessed unit includes a first bottom edge and a second bottom edge that are opposite to and spaced apart. For two adjacent recessed units, the first bottom edge of one recessed unit is connected to the second bottom edge of the other recessed unit.

[0011] This creates a welding trajectory.

[0012] In one embodiment, the length of the first base side is greater than the length of the second base side, wherein the length of the first base side is L, satisfying: 50 micrometers ≤ L ≤ 200 micrometers.

[0013] Therefore, on the one hand, it can prevent stress concentration from causing a decrease in fatigue life, and on the other hand, it can avoid the mechanical properties after welding not meeting the standards.

[0014] In one embodiment, the electrode post is laser-welded to the electrode tab, and the outer diameter of the laser spot is D1, which satisfies: 1.2L≤D1≤1.5L.

[0015] Therefore, on the one hand, it prevents the laser spot from being too large, which would result in an excessively wide heat-affected zone during the welding process and cause weld explosion; on the other hand, it prevents the laser spot from being too small, which would result in insufficient preheating of the welding interface and cause the mechanical properties after welding to fail to meet the standards.

[0016] In one embodiment, the distance between the first bottom edge and the second bottom edge is D2, which satisfies: 30 micrometers ≤ D2 ≤ 50 micrometers.

[0017] Therefore, on the one hand, it can prevent stress concentration from causing a decrease in fatigue life, and on the other hand, it can avoid the mechanical properties after welding not meeting the standards.

[0018] In one embodiment, the recessed unit includes a connecting segment and a bending segment, the bending segment being connected to the outer periphery of the connecting segment, and the connecting segments of every two adjacent recessed units being interconnected.

[0019] This ensures that the welding trajectory has a sufficient welding area, and that the bending segments of each recessed unit of the welding trajectory have a certain spacing to prevent the bending segments of two adjacent recessed units from connecting and causing excessive concentration of welding heat.

[0020] In one embodiment, the electrode post includes a first metal layer and a second metal layer, wherein the first metal layer, the second metal layer and the electrode tab are stacked sequentially; Wherein, the first metal layer and the second metal layer have different melting points, and / or the second metal layer and the tab have the same melting point.

[0021] This allows the formation of metallic compounds after welding, increasing hardness and tensile strength.

[0022] In one embodiment, a groove is formed on the side of the first metal layer away from the second metal layer, and the bottom surface of the groove serves as the welding area.

[0023] This allows for a reduction in the thickness of the electrode laser welding zone and a decrease in laser power, thereby reducing welding costs and difficulty.

[0024] Secondly, embodiments of the present invention provide a top cover assembly, including the welding structure as described above.

[0025] Therefore, it can prevent welding defects caused by excessive heat input during the welding process, and also avoid insufficient mixing of the welding interface caused by insufficient heat input during the welding process.

[0026] Thirdly, embodiments of this utility model provide a single battery cell, including the top cover assembly as described above.

[0027] Therefore, it can prevent welding defects caused by excessive heat input during the welding process, and also avoid insufficient mixing of the welding interface caused by insufficient heat input during the welding process.

[0028] Fourthly, embodiments of the present invention provide a battery pack, including the single battery cell as described above.

[0029] Therefore, it can prevent welding defects caused by excessive heat input during the welding process, and also avoid insufficient mixing of the welding interface caused by insufficient heat input during the welding process.

[0030] The beneficial effects of the embodiments of this utility model are as follows: In embodiments of this invention, by directly welding the tabs to the terminals, the use of connecting pieces can be eliminated, thereby increasing the utilization rate of internal space and improving the energy density of the battery. The area of ​​the welding trajectory between the terminals and the tabs accounts for 30% to 60% of the welding area, which can prevent excessive heat input during the welding process from causing welding defects, and can also avoid insufficient heat input during the welding process from causing insufficient mixing at the welding interface. Attached Figure Description

[0031] To more clearly illustrate the technical solutions in the embodiments of this utility model, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this utility model. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0032] Figure 1 This is a schematic diagram of the structure of a single battery cell provided in an embodiment of this utility model; Figure 2 yes Figure 1 Top view; Figure 3 yes Figure 1 A sectional view; Figure 4 yes Figure 3A magnified view of part A in the middle; Figure 5 This is one of the structural schematic diagrams of the welding trajectory provided in the embodiments of this utility model; Figure 6 This is the second schematic diagram of the welding trajectory provided in the embodiment of this utility model.

[0033] Explanation of reference numerals in the attached figures: 1. Electrode; 2. Pole post; 21. Welding area; 22. First metal layer; 23. Second metal layer; 24. Groove; 3. Welding trajectory; 31. Recessed unit; 311. First bottom edge; 312. Second bottom edge; 313. First inclined edge; 314. Second inclined edge; 32. Connecting section; 33. Bending section; 4. Molten pool; 5. Individual battery cell. Detailed Implementation

[0034] The technical solutions of the present utility model will be clearly and completely described below with reference to the accompanying drawings of the embodiments. Obviously, the described embodiments are only some embodiments of the present utility model, and not all embodiments. Based on the embodiments of the present utility model, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present utility model. In addition, it should be understood that the specific embodiments described herein are only for illustration and explanation of the present utility model and are not intended to limit the present utility model. In the present utility model, unless otherwise stated, directional terms such as "upper" and "lower" generally refer to the upper and lower positions of the device in actual use or operation, specifically the drawing directions in the accompanying drawings; while "inner" and "outer" refer to the outline of the device.

[0035] This application provides a battery pack. The battery pack includes a battery box and battery modules disposed within the battery box. The battery modules include multiple individual battery cells 5. The battery box provides a space for accommodating the individual battery cells 5, and the battery box can adopt various structures. In some embodiments, the battery box includes a box body and a box cover that overlap each other. The box body and the box cover together define an accommodating space for accommodating the individual battery cells 5. The box body can be a hollow structure, and the box cover can be a plate-like structure, with the box cover closing onto the opening side of the box body so that the box cover and the box body together define the accommodating space. Both the box body and the box cover can be hollow structures with an opening on one side, with the opening of the box cover closing onto the opening side of the box body. Of course, the battery box formed by the box cover and the box body can be of various shapes, such as a cylinder, a cuboid, etc.

[0036] In a battery pack, multiple individual cells 5 can be configured. These individual cells 5 can be connected in series, parallel, or in a hybrid configuration. A hybrid configuration means that multiple individual cells 5 are connected in both series and parallel configurations. Multiple individual cells 5 can be directly connected in series, parallel, or in a hybrid configuration, and then the entire assembly of these individual cells 5 is housed within a battery box. Alternatively, the battery pack can consist of multiple individual cells 5 first connected in series, parallel, or in a hybrid configuration to form battery modules, and then these battery modules are connected in series, parallel, or in a hybrid configuration to form a whole, which is then housed within a battery box. The battery pack may also include other structures; for example, it may include a busbar component for electrical connection between the multiple individual cells 5.

[0037] Each individual cell 5 can be a secondary battery or a primary battery; it can also be a lithium-sulfur battery, a sodium-ion battery, or a magnesium-ion battery, but is not limited to these. The individual cell 5 can be cylindrical, flat, cuboid, or other shapes.

[0038] This application also provides a single battery cell 5. The single battery cell 5 includes a housing, a top cover assembly, and electrode assemblies and other functional components located within the housing.

[0039] This application also provides a top cover assembly. The top cover assembly includes a top cover, a pole post 2 and a tab 1 disposed on the top cover. The pole post 2 and the tab 1 are laser welded.

[0040] like Figures 1 to 6 As shown in the embodiment of this application, a welding structure is also provided. This welding structure includes a tab 1 and a post 2. The post 2 is welded to the tab 1, and a welding trajectory 3 is defined on the surface of the post 2. The post 2 has a welding area 21. The welding trajectory 3 is located within the welding area 21. The area of ​​the welding trajectory 3 is S1, and the area of ​​the welding area 21 is S2, satisfying: 30% ≤ S1 / S2 ≤ 60%.

[0041] In this embodiment, by directly welding the tab 1 to the post 2, the use of a connecting piece can be eliminated, thereby increasing the utilization rate of internal space and improving the energy density of the battery. The area of ​​the welding trajectory 3 between the post 2 and the tab 1 accounts for 30% to 60% of the area of ​​the welding area 21, which can prevent excessive heat input during the welding process from causing welding defects, and can also avoid insufficient heat input during the welding process from causing insufficient mixing at the welding interface. Insufficient mixing at the welding interface between the post 2 and the tab 1 will lead to insufficient welding strength and easy cracking, causing premature fatigue fracture. At the same time, insufficient flow of the molten pool during the welding process is not conducive to the rise and escape of the gas and / or slag generated during welding, causing the gas to be trapped at the interface and forming pores, and / or causing the slag to be trapped at the interface and forming inclusions. Furthermore, it will also increase the resistance between the post 2 and the tab 1, which is not conducive to the charging and discharging of the battery.

[0042] It is understandable that the electrode post 2 and the electrode tab 1 are directly welded together without the need for a connecting piece. Since the connecting piece has a certain thickness, removing the connecting piece can free up that thickness space, thereby increasing the utilization rate of the internal space and thus improving the energy density of the battery.

[0043] In some embodiments, the terminal post 2 and the tab 1 are laser welded, with the terminal post 2 being some distance away from the tab 1 as the welding surface. This allows the terminal post 2 and the tab 1 to be welded on the outside of the battery, preventing metal spatter generated during welding from contacting the battery pack and potentially causing a short circuit.

[0044] During laser welding of the electrode post 2 and the electrode tab 1, the welding surface of the electrode post 2 has a welding area 21. The electrode post 2 and the electrode tab 1 are laser welded at positions corresponding to the welding area 21, and a welding trajectory 3 is formed on the surface of the electrode post 2. In this embodiment, the area of ​​the welding trajectory 3 accounts for 30% to 60% of the area of ​​the welding area 21. This can prevent excessive heat input during the welding process from causing welding defects, and can also avoid insufficient heat input during the welding process from causing insufficient mixing of the welding interface.

[0045] If the area of ​​welding trajectory 3 is greater than 60% of the area of ​​welding zone 21, it will result in excessive welding heat input and cause welding defects.

[0046] If the area of ​​welding trajectory 3 is less than 30% of the area of ​​welding zone 21, it will result in insufficient welding heat input and insufficient mixing of the welding interface.

[0047] In some embodiments, the area of ​​the welding trajectory 3 accounts for 30%, 40%, 50%, 60% of the area of ​​the welding area 21, or any value between the two.

[0048] It should be noted that tab 1 is a structural component formed by ultrasonic welding of all positive electrode tabs, or by ultrasonic welding of all negative electrode tabs. After forming the tabs through ultrasonic welding, laser penetration welding is then used to weld the tabs to the electrode post 2.

[0049] In some embodiments, the welding trajectory 3 is recessed on the surface of the pole post 2, and the recess depth of the welding trajectory 3 is H, satisfying: 20 micrometers ≤ H ≤ 50 micrometers.

[0050] Understandably, after laser welding is performed on the side of electrode 2 away from electrode 1, a pit is formed on the outer surface of electrode 2. This pit defines the welding trajectory 3, thus making the welding trajectory 3 recessed on the surface of electrode 2. Setting the recess depth of the welding trajectory 3 in the range of 20 micrometers to 50 micrometers can prevent stress concentration from reducing fatigue life and avoid substandard mechanical properties after welding.

[0051] If the depth of the depression in the welding trajectory 3 is less than 20 micrometers, the laser energy is insufficient, and the mechanical properties of the welded structure formed by the pole post 2 and the tab 1 will not meet the standards after welding.

[0052] If the depth of the depression in welding trajectory 3 is greater than 50 micrometers, the laser energy is relatively high, which will cause stress concentration during the welding process and lead to a decrease in fatigue life.

[0053] In some embodiments, the depth of the indentation of the welding trajectory 3 is set to 20 micrometers, 30 micrometers, 40 micrometers, 50 micrometers, or any value between the two.

[0054] like Figure 5 and Figure 6 As shown, in some embodiments, the welding trajectory 3 includes at least two sequentially connected recessed units 31, and the at least two recessed units 31 are connected to form a ring-shaped or spiral-shaped welding trajectory 3.

[0055] It is understandable that the welding trajectory 3 is formed by connecting multiple micro-pit units in sequence to form a ring or spiral structure, thereby ensuring the welding area of ​​the welding trajectory 3 so that the pole post 2 and the tab 1 can form a reliable connection.

[0056] In some embodiments, the welding trajectory 3 is configured as a ring. For example, the welding trajectory 3 is a circular ring, an elliptical ring, or any closed ring structure. Multiple welding trajectories 3 may be configured, and these multiple welding trajectories 3 are spaced apart. For example, multiple welding trajectories 3 may be configured, and each welding trajectory 3 is configured as a ring, wherein the diameters of the multiple welding trajectories 3 decrease progressively, and the multiple welding trajectories 3 share a common center.

[0057] In some embodiments, the welding trajectory 3 is set to a spiral shape.

[0058] like Figure 5 As shown, in some embodiments, the recessed unit 31 includes a first bottom edge 311 and a second bottom edge 312 that are opposite to and spaced apart. For two adjacent recessed units 31, the first bottom edge 311 of one recessed unit 31 is connected to the second bottom edge 312 of the other recessed unit 31.

[0059] It is understood that the first bottom edge 311 of one recessed unit 31 is connected to the second bottom edge 312 of the other recessed unit 31 between two adjacent recessed units 31, so that at least two recessed units 31 can be connected sequentially to form a welding trajectory 3. The recessed unit 31 also includes a first inclined side 313 and a second inclined side 314. The opposite ends of the first inclined side 313 are respectively connected to the first end of the first bottom edge 311 and the first end of the second bottom edge 312, and the opposite ends of the second inclined side 314 are respectively connected to the second end of the first bottom edge 311 and the second end of the second bottom edge 312.

[0060] It should be noted that the welding equipment forms equilateral triangular micro-pits on the surface of the pole post 2. When two adjacent equilateral triangular micro-pits are connected, their parts overlap, thereby forming a recessed unit 31 with a first base 311, a second base 312, a first hypotenuse 313, and a second hypotenuse 314.

[0061] Please continue reading. Figure 5 In some embodiments, the length of the first bottom edge 311 is greater than the length of the second bottom edge 312, wherein the length of the first bottom edge 311 is L, which satisfies: 50 micrometers ≤ L ≤ 200 micrometers.

[0062] Understandably, setting the length of the longer first bottom edge 311 within the range of 50 micrometers to 200 micrometers can, on the one hand, prevent stress concentration from causing a decrease in fatigue life, and on the other hand, avoid substandard mechanical properties after welding.

[0063] If the length of the first bottom edge 311 is less than 50 micrometers, the laser energy will be insufficient, and the mechanical properties of the welded structure formed by the pole post 2 and the tab 1 will not meet the standards after welding.

[0064] If the length of the first bottom edge 311 is greater than 200 micrometers, the laser energy will be too high, which will cause stress concentration during the welding process and lead to a decrease in fatigue life.

[0065] It should be noted that, since the welding equipment forms an equilateral triangular micro-pit on the surface of the pole post 2, the length of the first base 311 is the side length of the formed equilateral triangular micro-pit.

[0066] In some embodiments, the length of the first bottom edge 311 is set to 50 micrometers, 80 micrometers, 100 micrometers, 120 micrometers, 150 micrometers, 180 micrometers, 200 micrometers, or any value between any two.

[0067] Please continue reading. Figure 5 In some embodiments, the electrode post 2 is laser welded to the electrode tab 1, and the outer diameter of the laser spot is D1, which satisfies: 1.2L≤D1≤1.5L.

[0068] Understandably, making the outer diameter of the laser spot 1.2 to 1.5 times the length of the first bottom edge 311 serves two purposes: firstly, to prevent the laser spot from being too large, which would result in an excessively wide heat-affected zone during welding and cause weld explosion; and secondly, to prevent the laser spot from being too small, which would result in insufficient preheating of the welding interface and thus substandard mechanical properties after welding.

[0069] If the diameter of the laser spot is less than 1.2 times the length of the first bottom edge 311, the laser spot is too small, resulting in insufficient preheating of the welding interface and failure to meet the mechanical properties after welding.

[0070] If the diameter of the laser spot is greater than 1.5 times the length of the first bottom edge 311, the laser spot is too large, resulting in an excessively wide heat-affected zone during the welding process, which can lead to weld explosion.

[0071] In some embodiments, the diameter of the laser spot is 1.2 times, 1.3 times, 1.4 times, or 1.5 times the length of the first base 311, or any value between the two.

[0072] In some embodiments, the distance between the first bottom edge 311 and the second bottom edge 312 is D2, which satisfies: 30 micrometers ≤ D2 ≤ 50 micrometers.

[0073] It is understandable that the distance between the first bottom edge 311 and the second bottom edge 312 is the distance between the first bottom edges 311 of two adjacent recessed units 31. Setting the distance between the first bottom edge 311 and the second bottom edge 312 in the range of 30 micrometers to 50 micrometers can prevent stress concentration from causing a decrease in fatigue life, and can also avoid substandard mechanical properties after welding.

[0074] If the distance between the first bottom edge 311 and the second bottom edge 312 is less than 30 micrometers, the mechanical properties of the welded structure formed by the pole post 2 and the pole lug 1 will not meet the standards after welding.

[0075] If the distance between the first bottom edge 311 and the second bottom edge 312 is greater than 50 micrometers, it will cause stress concentration during the welding process, resulting in a decrease in fatigue life.

[0076] In some embodiments, the depth of the indentation of the welding trajectory 3 is set to 30 micrometers, 40 micrometers, 50 micrometers, or any value between the two.

[0077] like Figure 6 As shown, in some embodiments, the recessed unit 31 includes a connecting segment 32 and a bending segment 33, the bending segment 33 being connected to the outer periphery of the connecting segment 32, and the connecting segments 32 of each two adjacent recessed units 31 being connected to each other.

[0078] It is understandable that the unit with connecting segment 32 and bending segment 33 can make the welding trajectory 3 have a sufficient welding area, and the bending segments 33 of each recessed unit 31 of the welding trajectory 3 have a certain spacing to prevent the bending segments 33 of two adjacent recessed units 31 from being connected, which would cause the welding heat to be too concentrated.

[0079] In some embodiments, the bend 33 may be configured as a V-shape.

[0080] like Figures 2 to 4As shown, in some embodiments, the electrode post 2 includes a first metal layer 22 and a second metal layer 23, and the first metal layer 22, the second metal layer 23 and the electrode tab 1 are stacked in sequence; wherein the first metal layer 22 and the second metal layer 23 have different melting points, and / or the second metal layer 23 and the electrode tab 1 have the same melting point.

[0081] When electrode 2 is the negative electrode, it is made of a composite material of a first metal layer 22 and a second metal layer 23. Typically, the individual battery cell 5 is placed vertically, with the first metal layer 22 positioned above the second metal layer 23. The first metal layer 22 and the second metal layer 23 have different melting points. During laser welding, it is necessary to penetrate metal layers with different melting points to form a metal compound after welding, thereby increasing hardness and tensile strength.

[0082] In some embodiments, the first metal layer 22 is an aluminum layer and the second metal layer 23 is a copper layer.

[0083] In some embodiments, the melting point of the first metal layer 22 is lower than the melting point of the second metal layer 23, and / or the melting point of the second metal layer 23 is the same as the melting point of the tab 1.

[0084] Understandably, the melting point of the first metal layer 22 is lower than that of the second metal layer 23. During laser welding, this interface needs to penetrate metal layers with different melting points. The melting point of the second metal layer 23 is the same as that of the tab 1, so this interface does not need to penetrate metal layers with different melting points during laser welding. Because the melting point of the first metal layer 22 is lower than that of the second metal layer 23, laser welding requires a higher power density to penetrate the second metal layer 23.

[0085] In some embodiments, a groove 24 is formed on the side of the first metal layer 22 away from the second metal layer 23, and the bottom surface of the groove 24 serves as the welding area 21.

[0086] It is understandable that forming a groove 24 on the upper surface of the first metal layer 22 and using the bottom surface of the groove 24 as the welding area 21 can reduce the thickness of the laser welding area 21 of the electrode 2 and reduce the laser power, thereby reducing welding costs and welding difficulty. At the same time, the groove 24 can also facilitate the positioning of the electrode 2 by the welding equipment, enabling the welding equipment to quickly and accurately identify the welding area 21, which is beneficial to improving welding efficiency and welding accuracy.

[0087] like Figure 3 and Figure 4 As shown, in some embodiments, the pole post 2 is welded to the tab 1 and a molten pool 4 is formed inside them. The molten pool 4 defines a welding trajectory 3 on the surface of the pole post 2, wherein the end of the molten pool 4 away from the welding area 21 extends into the tab 1.

[0088] Understandably, after laser welding, a molten pool 4 can be formed within the electrode post 2 and the tab 1, and the molten pool 4 can define the welding trajectory 3 from the surface of the electrode post 2. The molten pool 4 extends from the surface of the electrode post 2 into the tab 1 to ensure reliable welding between the electrode post 2 and the tab 1.

[0089] The embodiments of this utility model have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this utility model. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of this utility model. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this utility model. Therefore, the content of this specification should not be construed as a limitation of this utility model.

Claims

1. A welded structure, characterized in that, include: Polar ear (1); A pole post (2) is welded to the tab (1), and a welding trajectory (3) is defined on the surface of the pole post (2). The pole post (2) has a welding area (21), and the welding trajectory (3) is located within the welding area (21). The area of ​​the welding trajectory (3) is S1, and the area of ​​the welding area (21) is S2, satisfying: 30%≤S1 / S2≤60%.

2. The welded structure according to claim 1, characterized in that, The welding trajectory (3) is recessed on the surface of the pole post (2), and the depth of the recess of the welding trajectory (3) is H, which satisfies: 20 micrometers ≤ H ≤ 50 micrometers.

3. The welded structure according to claim 2, characterized in that, The welding trajectory (3) includes at least two sequentially connected recessed units (31), which are connected to form a ring-shaped or spiral-shaped welding trajectory (3).

4. The welded structure according to claim 3, characterized in that, The recessed unit (31) includes a first bottom edge (311) and a second bottom edge (312) that are opposite to each other and spaced apart. For two adjacent recessed units (31), the first bottom edge (311) of one recessed unit (31) is connected to the second bottom edge (312) of the other recessed unit (31).

5. The welded structure according to claim 4, characterized in that, The length of the first bottom edge (311) is greater than the length of the second bottom edge (312), wherein the length of the first bottom edge (311) is L, which satisfies: 50 micrometers ≤ L ≤ 200 micrometers.

6. The welded structure according to claim 5, characterized in that, The electrode post (2) is laser welded to the electrode tab (1), and the outer diameter of the laser spot is D1, which satisfies: 1.2L≤D1≤1.5L.

7. The welded structure according to claim 4, characterized in that, The distance between the first bottom edge (311) and the second bottom edge (312) is D2, which satisfies: 30 micrometers ≤ D2 ≤ 50 micrometers.

8. The welded structure according to claim 3, characterized in that, The recessed unit (31) includes a connecting section (32) and a bending section (33), the bending section (33) being connected to the outer periphery of the connecting section (32), and the connecting sections (32) of each two adjacent recessed units (31) being connected to each other.

9. The welded structure according to any one of claims 1 to 8, characterized in that, The pole post (2) includes a first metal layer (22) and a second metal layer (23), and the first metal layer (22), the second metal layer (23) and the tab (1) are stacked in sequence; Wherein, the first metal layer (22) and the second metal layer (23) have different melting points, and / or the second metal layer (23) has the same melting point as the tab (1).

10. The welded structure according to claim 9, characterized in that, A groove (24) is formed on the side of the first metal layer (22) away from the second metal layer (23), and the bottom surface of the groove (24) serves as the welding area (21).

11. A top cover assembly, characterized in that, Includes the welded structure as described in any one of claims 1 to 10.

12. A single-cell battery cell (5), characterized in that, Includes the top cover assembly as described in claim 11.

13. A battery pack, characterized in that, Includes the single cell (5) as described in claim 12.